Fine-fineness fluorine-based unfired fiber and producing method thereof
Fine-grained fluorine-based unsintered fibers with controlled characteristics and processing methods address interfiber fusion issues, enabling thin papermaking with uniform texture and high productivity.
Patent Information
- Application Number
- JP2023050853
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing fluorine-based fibers, such as polytetrafluoroethylene (PTFE) and perfluoroalkoxyalkane (PFA) fibers, face issues with interfiber fusion during the firing process, leading to uneven thickness and texture in papermaking applications, limiting their application to PTFE and making it difficult to achieve fineness and productivity for thin papermaking.
Production of fine-grained fluorine-based unsintered fibers with specific characteristics: single fiber fineness of 1.0 dtex to 15.0 dtex, carbon content of 5.0% to 25.0%, crystal orientation of 0.60 to 0.80, and minimal single yarn adhesion, using a matrix spinning method with controlled spinning parameters and processing conditions.
The solution results in fibers suitable for thin papermaking with low single filament adhesion and high productivity, maintaining excellent heat resistance, chemical resistance, and electrical insulation properties.
Smart Images

Figure 2024139910000001
Abstract
Description
[Technical field]
[0001] The present invention relates to fine fluorine-based unsintered fibers and a method for producing the same. [Background technology]
[0002] Fluororesin fibers, such as polytetrafluoroethylene (PTFE) and perfluoroalkoxyalkane (PFA) fibers, are widely used, primarily for industrial material applications, due to their excellent heat resistance, chemical resistance, electrical insulation, and low friction coefficient and excellent sliding properties. In recent years in particular, it is expected that its insulating properties will be utilized to make insulating sheets for communication components such as printed circuit boards, and research into this material is currently being conducted because the large number of voids gives it excellent breathability and low dielectric properties. When considering use in communication components such as smartphones, thinning is essential, but uniform texture is also an important factor in stabilizing paper thickness and properties. In order to make thinner paper, it is necessary to use finer fluorine-based fibers as a raw material. For example, Patent Document 1 proposes fine polytetrafluoroethylene fibers that can be produced with good productivity by adjusting the hole diameter and hole length of a spinneret, spinning draft, and baking conditions. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2022-85088 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the polytetrafluoroethylene fiber described in Patent Document 1 has some inter-fiber fusion during the baking process, and the occurrence of fused parts tends to increase when the total fineness of the multifilament is increased in order to balance fineness and productivity, which causes problems such as an increase in the thickness of the fused parts and non-uniform texture when used in papermaking applications. In addition, the manufacturing method is limited to PTFE, and there is a problem that it is difficult to apply to other fluororesins such as PFA.
[0005] Therefore, an object of the present invention is to provide a fine fluorine-based fiber which maintains the characteristics of a fluorine-based fiber as a material, such as excellent heat resistance, chemical resistance and electrical insulation, is finer, is suitable for thin papermaking applications, has less single filament adhesion and has good productivity, and a method for producing the same. [Means for solving the problem]
[0006] In order to solve the above problems, the present invention is configured as follows. [1] A fluorine-based unburned fiber having a single fiber fineness of 1.0 dtex or more and 15.0 dtex or less, and a carbon content of 5.0% or more and 25.0% or less by weight of the fiber. [2] The above fluorine-based unsintered fiber, characterized in that the number of fiber adhesion parts in a single yarn adhesion evaluation is 1 part / 0.2 g or less. [3] The above fluorine-based unsintered fiber, characterized in that the degree of crystal orientation is 0.60 to 0.80. [4] The above fluorine-based unsintered fiber, characterized in that the fluorine-based resin used is polytetrafluoroethylene or perfluoroalkoxyalkane. [5] A method for producing a fluorine-based unsintered fiber, comprising: mixing an aqueous dispersion of viscose and a fluororesin in a cellulose:fluororesin weight ratio of 5:95 to 25:75; discharging the resulting mixture into a coagulation bath of an aqueous solution of 7 to 13% sulfuric acid and 7 to 15% sodium sulfate through a spinning nozzle having a hole diameter of 40 μm to 80 μm and a hole length / hole diameter ratio of 1.0 to 3.0, at a take-up speed / discharge linear speed of 1.5 to 4.0, as a multifilament having a total fineness of 4,000 dtex or more; and washing the resulting mixture with warm water and an alkaline aqueous solution. Effect of the Invention
[0007] According to the present invention, it is possible to obtain fine fluorine-based fibers suitable for thin papermaking applications, which have low filament adhesion and good productivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] <Fluorine-based unburned fiber> As the fluorine-based unsintered fiber of the present invention, any fiber can be used as long as it is made of a polymer (fluororesin) composed of a monomer in which 90% or more of the repeating structural units contain one or more fluorine atoms in the main chain or side chain, but the fiber composed of a monomer with a larger number of fluorine atoms is more preferable, and in addition to PTFE, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene polymer (FEP), tetrafluoroethylene olefin copolymer (ETFE), etc. can be used. Among them, PTFE or PFA is preferable from the viewpoints of heat resistance, chemical resistance, and dielectric properties.
[0009] Since the viscosity of the heated melt of fluororesin polymer is extremely high, a matrix spinning method is known in which a fluororesin polymer is mixed with a matrix polymer to form an emulsion, and the emulsion is extruded from a spinneret into a coagulation bath to form fibers. The fibers obtained by matrix spinning are generally subjected to a baking process in which the fibers are baked at a temperature equal to or higher than the melting point of the polymer, thereby removing most of the matrix polymer and fusing the particles of the fluororesin polymer together to form baked yarns. The fluorine-based unbaked fibers of the present invention refer to those that have not been subjected to the baking process.
[0010] The single fiber fineness of the fluorine-based unsintered fiber of the present invention is preferably 1.0 dtex or more and 15.0 dtex or less. If the single fiber fineness is less than 1.0 dtex, the spinnability is significantly deteriorated, making industrial production difficult. If the single fiber fineness is more than 15.0 dtex, the effect of fineness reduction is reduced, making it unsuitable for thin papermaking applications.
[0011] It is important that the carbon content of the fluorine-based unsintered fiber of the present invention is 5.0% or more and 25.0% or less based on the fiber weight. If the carbon content is less than 5.0%, the matrix component is small, resulting in poor spinnability, and there is a high incidence of broken yarns and defective yarns. If the carbon content exceeds 25.0%, the processing time for sintering and bleaching after papermaking becomes longer, which affects productivity. The fluorine-based unsintered fiber of the present invention does not pass through the sintering process, so that adhesion between single filaments due to fusion of the fluororesin does not occur. In addition, by setting the take-up speed / discharge linear speed from the spinning nozzle within an appropriate range, the single filaments do not come into contact with each other during spinning, so that adhesion between single filaments does not occur. Therefore, it is preferable that the number of fiber adhesion parts in the single filament adhesion evaluation is 1 / 0.2g or less. If it is 2 / 0.2g or more, the thickness of the paper increases, the texture becomes non-uniform, and the performance as a thin paper decreases. The single filament adhesion evaluation was performed by the following method. First, the fiber is cut to 6 mm, and 200 mL of an aqueous dispersion of the fiber is prepared using a dispersant at a dispersant concentration of 0.05% and a fiber amount of 1 g / L, and then the mixture is stirred at 25°C, 500 rpm, and 3 minutes. The obtained aqueous dispersion of the fiber is suction-filtered using filter paper, and the fiber morphology after suction filtration is visually measured for the part (fiber adhesion part) where the fiber bundles are bonded to each other and formed into a bundle.
[0012] The fluorine-based unsintered fiber of the present invention preferably has a crystal orientation degree of 0.60 or more and 0.80 or less. If the crystal orientation degree is less than 0.60, the fiber properties are low and quality and operability are deteriorated due to yarn breakage, inclusion of defective yarns, etc. If the crystal orientation degree exceeds 0.80, the quality and operability are deteriorated due to yarn breakage, inclusion of defective yarns, etc. due to excessive drawing during the spinning process.
[0013] The tensile strength is preferably 0.03 cN / dtex or more and 1.0 cN / dtex or less. If it is less than 0.03 cN / dtex, the tensile strength will be too weak, leading to poor operability, such as an increase in yarn breakage during the fiber manufacturing process. Fibers with a tensile strength of more than 1.0 cN / dtex can be manufactured by increasing the ratio of the matrix component, but the processing time for sintering and bleaching after papermaking will be longer, which will affect productivity.
[0014] <Production method of fluorine-based unburned fiber> The fine fluorine-based unsintered fibers of the present invention are preferably produced by a matrix spinning method in which an aqueous dispersion of a fluororesin and a matrix material are mixed and spun.
[0015] The matrix material is not particularly limited as long as it is a viscose that is commonly used in the production of rayon. A preferred example is viscose with a cellulose concentration of 5.0 to 11.0 wt%, an alkali concentration of 4.0 to 10.0 wt%, and carbon disulfide concentration of 27.0 to 32.0 wt% (relative to cellulose).
[0016] The spinning dope is preferably a mixture of viscose and an aqueous dispersion of fluororesin in a weight ratio of cellulose:fluororesin = 5:95 to 25:75. If the weight ratio of cellulose is less than 5%, spinnability decreases, making it difficult to produce fine fibers. If the weight ratio of cellulose exceeds 75%, the processing time for sintering and bleaching after papermaking becomes longer, affecting productivity.
[0017] These spinning dope solutions are subjected to the spinning process after being degassed, but if the temperature during degassing is too high, there is a concern that the viscose will solidify, and there is also a concern that the water will evaporate and the PTFE will aggregate. Therefore, it is preferable to control the temperature during degassing to a low temperature of 15°C or less. The degree of vacuum during this process is preferably about 10 Torr or less.
[0018] Next, these spinning dope solutions are discharged from a die immersed in a coagulating bath and are coagulated in the coagulating bath.
[0019] As the coagulation bath, an aqueous solution of an inorganic mineral acid or an inorganic salt is used, but in the present invention, it is preferable to use a mixed aqueous solution containing sulfuric acid and sodium sulfate.
[0020] In this case, the sulfuric acid concentration is preferably 7.0 to 13.0 wt%. If the sulfuric acid concentration is less than 7.0 wt%, the speed at which the yarn coagulates in the coagulation bath becomes very slow, which is undesirable as it reduces production capacity or requires a longer immersion line. On the other hand, if the sulfuric acid concentration exceeds 13.0 wt%, it becomes difficult to deoxidize the sulfuric acid attached to the fiber surface.
[0021] The sodium sulfate concentration is preferably adjusted to 7.0 to 15.0 wt%. Sodium sulfate inhibits rapid coagulation of cellulose. If the sodium sulfate concentration is less than 7.0 wt%, the rate at which the threads coagulate in the coagulation bath becomes very fast, which is undesirable as it makes it difficult to control the fiber cross section. On the other hand, if the sodium sulfate concentration exceeds 15.0 wt%, the rate at which the threads coagulate in the coagulation bath becomes very slow, which is undesirable as it makes it difficult to control the fiber cross section. Using a mixed aqueous solution containing both sulfuric acid and sodium sulfate concentrations within the above-mentioned specific ranges as the coagulation bath is effective for producing uniform fluorine-based fibers.
[0022] The hole diameter of the nozzle hole used is preferably 40 μm or more and 80 μm or less, and the hole length / hole diameter ratio is 1.0 or more and 3.0 or less. When the hole diameter of the nozzle hole is in this range, an appropriate extrusion linear velocity is obtained, and good stretchability is imparted. In addition, by making the hole length / hole diameter ratio 1.0 or more, the back pressure of the nozzle hole can be ensured, and the spinning dope is evenly distributed to each hole of the nozzle hole, which leads to stable productivity of fine fluorine-based fibers, and by making it 3.0 or less, clogging of the holes with particles can be suppressed. From the viewpoint of fineness, the take-up speed / discharge linear speed when discharging the spinning dope from the spinning nozzle is preferably 1.5 to 4.0. When this value is 1.5 or more, the spun yarn can maintain an appropriate tension and can be spun without adjacent single yarns adhering to each other, and when it is 4.0 or less, single yarn breakage due to excessive tension can be suppressed.
[0023] From the viewpoint of industrial productivity, it is preferable that the total fineness of the spun multifilaments is 4000 dtex or more.
[0024] The solidified fibers are then deacidified in hot water, washed in an alkaline washing step, and then stored in a tow can.
[0025] For deoxidation with hot water, washing with hot water in a tray-type bath is preferred. The temperature of the hot water is preferably 60°C or higher and 90°C or lower. If the temperature is lower than 60°C, the washing efficiency decreases. On the other hand, if the temperature is higher than 90°C, the bath liquid becomes more turbulent, causing interference with adjacent yarns and yarn breakage due to increased resistance of the counterflow.
[0026] In the alkaline washing step, washing with an alkaline aqueous solution containing an alkaline salt is preferable. In such an alkaline washing bath, an aqueous solution of a compound selected from hydroxides, carbonates, and bicarbonates of an alkaline metal or an alkaline earth metal is used, but generally, an aqueous solution of an alkaline metal salt, especially an aqueous solution of caustic soda, is preferably used. The concentration of these alkaline salts is preferably 0.08 wt% or more and 0.18 wt% or less. More preferably, it is 0.10 wt% or more and 0.16 wt% or less. If it is less than 0.08 wt%, deoxidation is insufficient, leading to poor sintering after papermaking. On the other hand, if it exceeds 0.18 wt%, cellulose will dissolve during alkaline washing, and residue will easily accumulate in the alkaline bath and guides. In addition, the strength of the undrawn yarn will decrease, and process passing troubles such as winding in the process will easily occur, which is not preferable.
[0027] Furthermore, the temperature of the alkaline bath is preferably 20° C. or less, and more preferably 15° C. or less. If the temperature of the alkaline bath exceeds 20° C., like the case where the alkali concentration is too high, cellulose dissolves in the alkaline washing, and residue tends to accumulate in the alkaline bath or on the guide, and troubles during the process such as winding in the process tend to occur, which is undesirable.
[0028] The fibers obtained by the production method of the present invention can be cut to a desired length as required to produce fluorine-based short fibers.
[0029] The fibers obtained by the manufacturing method of the present invention can be made into paper without being calcined after being shortened, and sintered after papermaking. This allows papermaking to be performed with little adhesion of the single filaments, thereby suppressing thickness increase and uneven texture. EXAMPLES
[0030] Next, the present invention will be specifically described based on examples. However, the present invention is not limited to these examples. Various modifications and corrections are possible within the scope of the technical scope of the present invention. The methods for measuring various properties used in the examples are as follows.
[0031] [Measurement and evaluation method] (1) Single fiber size A multifilament sample exactly 1 m long was taken by applying an initial load (a load (g) that is 6% of the fineness). After heat treatment at a temperature of 140°C in an air atmosphere for 1 hour, the mass of the sample was measured to the nearest 1 / 10,000 g and calculated using the following formula: Single fiber fineness (dtex) = sample mass / (sample length x number of holes in spinning nozzle) x 10,000 The average value of three measurements was taken as the single fiber fineness (dtex).
[0032] (2) Coal content After 3 g of fiber was heat-treated at 300°C for 72 hours in an air atmosphere, the fiber mass change was measured and calculated using the following formula: Carbon content (%) = (fiber mass before heat treatment - fiber mass after heat treatment) / fiber mass before heat treatment × 100 The carbon content (%) was calculated.
[0033] (3) Production stability When the average number of times that yarn bundle breakage occurred in each spinning and drawing process per 100 kg of fiber produced was determined to be less than 10 times / 100 kg production, it was given an "A" rating; when it was 10 to 30 times / 100 kg production, it was given an "B" rating; and when it was 30 or more times / 100 kg production, it was given an "C" rating. Cases that fell between A and B were judged to have excellent production stability.
[0034] (4) Single yarn adhesion The fibers were cut into 6 mm pieces, and 200 mL of an aqueous dispersion of the fibers was prepared using Woopol (Matsumoto Yushi Seiyaku Co., Ltd.) as a dispersant at a dispersant concentration of 0.05% and a fiber amount of 1 g / L. The dispersion was then stirred at 25°C, 500 rpm, and 3 minutes using a magnetic stirrer. The resulting aqueous dispersion of the fibers was then transferred to a tube with a diameter of 11 cm and a fiber weight of 118 g / m 2 The fiber bundles were filtered by suction using filter paper, and the number of fiber bundles (fiber adhesion parts) in the fiber configuration after suction filtration was visually counted. When the number of fiber adhesion parts was 1 or less per 0.2 g, it was judged as "good", and when it was 2 or more per 0.2 g, it was judged as "poor". When it was good, it was judged as having excellent single yarn adhesion.
[0035] (5) Degree of crystal orientation The crystal orientation was calculated from the half-width (H) of the intensity distribution obtained by scanning the sample in the equatorial direction and then scanning each peak in the circumferential direction. The calculation formula is as follows: Crystal orientation = (180-H) / 180 The measurements were carried out using an apparatus manufactured by Rigaku Corporation.
[0036] [Example 1] After mixing 46% by mass of viscose (cellulose concentration 9.0 wt%, alkali concentration 6.0 wt%) and 54% of PTFE aqueous dispersion with a concentration of 60%, the mixture was degassed under a reduced pressure of 10 Torr to obtain a spinning mixture with a cellulose:PTFE weight ratio of 11:89 in the mixture. The spinning solution was wet-spun into a spinning bath solution with a sulfuric acid concentration of 9.0%, a sodium sulfate concentration of 10.0%, and a temperature of 15 ° C. using a round hole die with a hole diameter of 50 μm and a hole length of 80 μm, so that the spinning take-up speed / discharge linear speed was 3.8 and the total fineness was 6000 dtex. The solidified unsintered yarn was then washed with warm water at a temperature of 70 ° C., and then refined by being introduced into an alkali bath containing a caustic soda aqueous solution with a concentration of 0.12%, and the acid components were completely removed. After that, the unsintered yarn introduced from the alkali bath was squeezed with a nip roller and then stored in a tow can to obtain PTFE unsintered fiber. The obtained PTFE unsintered fiber had a single fiber fineness of 2.2 dtex, a carbon content of 15.5%, and a crystal orientation of 0.72. The average number of times that the yarn bundle broke during the spinning process in the production of the PTFE unsintered fiber was 3 times / 100 kg production, and the single fiber adhesiveness of this PTFE unsintered fiber was evaluated to be 1 piece / 0.2 g.
[0037] [Example 2] A PTFE unsintered fiber was obtained in the same manner as in Example 1, except that the hole diameter of the spinneret discharge hole was changed to 80 μm, the hole length was changed to 80 μm, the spinning take-up speed / discharge linear speed was changed to 1.5, and the total fineness was changed to 40,000 dtex. The obtained PTFE unsintered fiber had a single fiber fineness of 14.5 dtex, a carbon content of 15.2%, and a crystal orientation degree of 0.73. In addition, the number of times that the yarn bundle broke during the spinning process in the production of the PTFE unsintered fiber was 1 time / 100 kg production, and the single yarn adhesiveness of this PTFE unsintered fiber was evaluated and found to be 0 pieces / 0.2 g.
[0038] [Example 3] After mixing 41% by mass of viscose (cellulose concentration 9.0 wt%, alkali concentration 6.0 wt%) and 59% of PTFE aqueous dispersion with a concentration of 50%, the mixture was degassed under a reduced pressure of 10 Torr to obtain a spinning mixture with a cellulose:PFA weight ratio of 11:89 in the mixture. After spinning, PFA unsintered fibers were obtained in the same manner as in Example 1, except that the total fineness was changed to 7700 dtex. The obtained PFA unsintered fibers had a single fiber fineness of 2.8 dtex, a carbon content of 15.3%, and a crystal orientation degree of 0.69. In addition, the average number of times that yarn bundle breakage occurred during the spinning process during the production of PFA unsintered fibers was 4 times / 100 kg production, and the single yarn adhesiveness of this PFA unsintered fiber was evaluated to be 1 piece / 0.2 g.
[0039] [Comparative Example 1] The PTFE unsintered fibers obtained by the same method as in Example 1 were not stored in a tow can, but were semi-sintered at a temperature of 320°C while being relaxed by 2% with a total fineness / width of 30 ktex / m, and then sintered at a temperature of 345°C. After being wound up once, the fibers were hot-drawn at a temperature of 340°C to a ratio of 7.6 to obtain PTFE fibers. The obtained PTFE fibers had a single fiber fineness of 0.3 dtex, a carbon content of 2.9%, and a crystal orientation of 0.96. The average number of times that the yarn bundle broke in each process of spinning and drawing during the production of the PTFE fibers was 6 times / 100 kg production, and the single yarn adhesiveness of the PTFE fibers was evaluated to be 3 pieces / 0.2 g.
[0040] [Comparative Example 2] A PTFE unsintered fiber was obtained in the same manner as in Example 1, except that the spinning take-up speed / discharge linear speed was changed to 5.0. The obtained PTFE unsintered fiber had a single fiber fineness of 2.2 dtex, a carbon content of 15.1%, and a crystal orientation degree of 0.85. The number of times that the yarn bundle broke during the spinning process in the production of the PTFE unsintered fiber was 20 times / 100 kg production, and the single yarn adhesiveness of this PTFE unsintered fiber was evaluated to be 0 pieces / 0.2 g.
[0041] [Comparative Example 3] The PFA unburned fibers obtained by the same method as in Example 3 were not stored in a tow can, but were semi-burned at a temperature of 300°C while being relaxed by 2% with a total fineness / width of 30 ktex / m, and then were burned at a temperature of 325°C. After being wound up once, the fibers were hot-drawn at a ratio of 7.6 times at a temperature of 320°C to obtain PFA fibers. The obtained PFA fibers had a single fiber fineness of 0.4 dtex and a carbon content of 3.8%. The average number of times that the yarn bundle broke in each process of spinning and drawing during the production of the PFA fibers was 150 times / 100 kg production, and the single yarn adhesiveness of the PFA fibers was evaluated to be 50 pieces / 0.2 g.
[0042] [Table 1]
[0043] The fluorine-based unburned fibers produced in Examples 1 to 3 and Comparative Examples 1 to 3 were evaluated for the above-mentioned (1) single fiber fineness, (2) carbon content, (3) production stability, (4) single fiber adhesion, and (5) crystal orientation, and the results are shown in Table 1. As a result, it was clear that the fluorine-based unburned fibers of the present invention are suitable for papermaking applications because they have low single fiber adhesion despite their fineness, and that a method for producing fine fluorine-based unburned fibers with high productivity can be provided.
Claims
1. A fluorine-based unburned fiber having a single fiber fineness of 1.0 dtex or more and 15.0 dtex or less, and a carbon content of 5.0% or more and 25.0% or less based on the fiber weight.
2. 2. The fluorine-based unburned fiber according to claim 1, characterized in that the number of fiber adhesion parts in a single filament adhesion evaluation is 1 / 0.2 g or less.
3. 3. The fluorine-based unburned fiber according to claim 1, characterized in that the degree of crystal orientation is 0.60 to 0.
80.
4. 3. The fluorine-based unsintered fiber according to claim 1, wherein the fluorine-based resin is polytetrafluoroethylene or perfluoroalkoxyalkane.
5. 3. A method for producing a fluorine-based unsintered fiber according to claim 1 or 2, characterized in that a mixed solution obtained by mixing an aqueous dispersion of viscose and a fluororesin in a ratio of cellulose:fluororesin (weight ratio) of 5:95 to 25:75 is discharged into a coagulation bath of an aqueous solution having a sulfuric acid concentration of 7 to 13% and a sodium sulfate concentration of 7 to 15% from a spinning nozzle having a discharge hole diameter of 40 μm to 80 μm and a hole length / hole diameter ratio of 1.0 to 3.0, at a take-up speed / discharge linear speed of 1.5 to 4.0, as a multifilament having a total fineness of 4,000 dtex or more, and then washed with warm water and an alkaline aqueous solution.
Citation Information
Patent Citations
Thin fineness polytetrafluoroethylene fiber and method for producing the same
JP2022085088A