Two-pack aqueous coating composition
The two-component water-based coating composition addresses the adhesion and anticorrosion limitations of epoxy resin-based paints by optimizing elastic modulus and gel fraction, resulting in a film with superior adhesion and corrosion resistance for diverse substrates.
Patent Information
- Application Number
- JP2023051278
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Epoxy resin-based water-based paints do not fully demonstrate adhesion and anticorrosion properties compared to solvent-based paints.
A two-component water-based coating composition containing an epoxy resin, a resin that reacts with the epoxy resin, a pigment, and water, with specific formulations to achieve an elastic modulus of 600 to 2400 N/mm² and a gel fraction of 80% or more, ensuring excellent adhesion and anticorrosion properties.
The composition forms a coating film with enhanced adhesion and corrosion resistance, suitable for various substrates including metals and plastics, even under harsh conditions.
Smart Images

Figure 2024140236000001 
Figure 2024140236000002 
Figure 2024140236000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a two-pack water-based coating composition, and in particular to a two-pack water-based coating composition capable of forming a coating film having excellent adhesion and corrosion prevention properties. [Background technology]
[0002] Traditionally, in the field of coatings for architectural and civil engineering structures, there has been a shift from solvent-based to water-based paints to reduce the health hazards to painters and residents and to reduce odors. For metal coating materials, room temperature curing two-component water-based epoxy resin paints with excellent film strength, adhesion, and rust prevention properties have been developed.
[0003] JP 2021-1314 A (Patent Document 1) describes an invention of an aqueous coating material containing a film-forming component and a powder component, wherein the film-forming component contains an aqueous epoxy resin emulsion as a resin component, and the gel fraction of the formed coating is 10% or more, the powder component contains an anti-rust pigment, and calcium carbonate, and the powder component contains 50 to 300 parts by weight per 100 parts by weight of the resin component, and the powder component contains 30 to 90% by weight of the calcium carbonate. This aqueous coating material is said to have excellent coating film strength, adhesion, rust prevention, etc. In addition, JP 2021-1315 A (Patent Document 2) describes an invention in which a coloring pigment containing titanium oxide and a red iron oxide pigment is blended into the aqueous coating material described in Patent Document 1.
[0004] JP 2009-149791 A (Patent Document 3) describes an invention of a two-component water-based anticorrosive paint that is composed of a combination of (I) a base agent containing an epoxy resin emulsion and a pigment, and (II) an amine curing agent, and that is mixed and applied immediately before use, characterized in that the pigment in the base agent (I) contains a phosphate-based rust-preventive pigment as part of its components, and the amine curing agent (II) contains, as part of its components, a polyamine (IIa) having a cyclic structure and an active hydrogen equivalent in the range of 80 or more and less than 1000. This two-component water-based anticorrosive paint has good curing properties even under conditions of drying at room temperature, and can form an anticorrosive coating film with excellent corrosion resistance against substrates such as steel materials such as iron and zinc plating, and non-ferrous materials, so that the beauty of the coated object can be maintained for a long time even under harsh environments.
[0005] JP 2019-515991 A (Patent Document 4) describes a two-component epoxy resin paint comprising (a) an epoxy resin component and (b) an amine component for curing the epoxy resin component, the amine component comprising (i) at least one polyamide curing agent and (ii) at least one Mannich base curing agent, at least one of the polyamide curing agent and the Mannich base curing agent being derived from one or more polyfunctional amines including at least one alicyclic polyfunctional amine, the alicyclic polyfunctional amine being present in an amount of 30% by weight or more relative to the total amount of the polyfunctional amine, and the weight ratio of the epoxy resin component (a) to the amine component (b) being 100:8 to 100:20. The invention describes a two-component epoxy resin paint, which provides a two-component epoxy resin paint having a good balance between a long pot life and a fast drying speed.
[0006] JP 2018-53028 A (Patent Document 5) describes an invention of a two-component reactive curing water-based coating composition for undercoat paint that contains an epoxy resin and an amine resin, in which the weight ratio of an epoxy resin having an epoxy equivalent of 400 to 1000 g / eq to an epoxy resin having an epoxy equivalent of 150 to 300 g / eq is 90:10 to 60:40, and describes that this makes it possible to provide a two-component reactive curing water-based coating composition for undercoat paint that gives an undercoat coating film with excellent chemical resistance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent Publication No. 2021-1314 [Patent Document 2] Patent Publication No. 2021-1315 [Patent Document 3] JP 2009-149791 A [Patent Document 4] JP 2019-515991 A [Patent Document 5] JP 2018-53028 A Summary of the Invention [Problem to be solved by the invention]
[0008] As described above, epoxy resin-based water-based paint compositions have been proposed. However, while epoxy resins are generally known as resins with excellent adhesive properties, it was thought that the adhesive properties of epoxy resins cannot be fully exhibited when used in water-based paints, compared with when used in organic solvent-based paints.
[0009] Therefore, an object of the present invention is to provide a two-pack water-based paint composition capable of forming a coating film having excellent adhesion and corrosion resistance. [Means for solving the problem]
[0010] In order to achieve the above object, the present inventors have conducted research and have found that the elastic modulus of a coating film formed from an epoxy resin-based two-liquid water-based coating composition is 600 to 2400 N / mm 2 It was found that by adjusting the viscosity of the coating material to the above range, a coating film having excellent adhesion could be formed even though it was a water-based coating material, and this led to the completion of the present invention.
[0011] The coating composition of the present invention is therefore a two-liquid water-based coating composition containing (A) an epoxy resin, (B) a resin that reacts with the epoxy resin, (C) a pigment, and (D) water, and when the coating composition is applied and dried for 7 days under conditions of 23°C and 50% humidity, the coating film has an elastic modulus of 600 to 2400 N / mm 2 It is a coating composition.
[0012] In a preferred embodiment of the coating composition of the present invention, when the coating composition is applied and dried under conditions of 23° C. and 50% humidity for 7 days, the coating film has a gel fraction of 80% or more.
[0013] In another preferred embodiment of the coating composition of the present invention, when the coating composition is applied and dried for 7 days under conditions of 23° C. and 50% humidity, the amount of solvent remaining in the coating film is less than 8.0%.
[0014] In another preferred embodiment of the coating composition of the present invention, the (B) resin that reacts with the epoxy resin contains at least a modified polyamine having a cyclic structure.
[0015] In another preferred embodiment of the coating composition of the present invention, the resin that reacts with the epoxy resin (B) contains at least a modified polyamine having a cyclic structure, and the content of the modified polyamine having a cyclic structure in the resin that reacts with the epoxy resin (B) is 50 to 100 mass %. Effect of the Invention
[0016] According to the present invention, it is possible to provide a two-pack water-based coating composition capable of forming a coating film having excellent adhesion and corrosion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present invention will be described in detail below. The present invention relates to a two-component water-based coating composition containing an epoxy resin, a resin that reacts with the epoxy resin, a pigment, and water. In this specification, this coating composition is also referred to as "the two-component water-based coating composition of the present invention" or "the coating composition of the present invention". Furthermore, "epoxy resin" is the (A) component, and is also referred to as "(A) epoxy resin". "Resin that reacts with the epoxy resin" is the (B) component, and is also referred to as "(B) resin that reacts with the epoxy resin". "Pigment" is the (C) component, and is also referred to as "(C) pigment". "Water" is the (D) component, and is also referred to as "(D) water".
[0018] In this specification, the water-based coating composition is a coating composition containing water as a main solvent. The water used in the coating composition of the present invention is not particularly limited, but preferred examples include tap water, ion-exchanged water, distilled water, and other pure water. When the coating composition is to be stored for a long period of time, water sterilized by ultraviolet irradiation or the like may be used to prevent the growth of mold and bacteria. In the coating composition of the present invention, the amount of water is preferably 20 to 60% by mass, more preferably 30 to 50% by mass.
[0019] In the coating composition of the present invention, the amount of non-volatile content is preferably 40 to 80 mass %, more preferably 50 to 70 mass %. In this specification, the non-volatile content refers to the components excluding volatile components such as solvents, and is the components that will ultimately form a coating film, but in the present invention, the components remaining when the coating composition is dried in an oven at 110°C for 3 hours are treated as the non-volatile content.
[0020] In this specification, a two-liquid type coating composition is a coating composition consisting of a base agent and a curing agent. A two-liquid type coating composition can be prepared by mixing a base agent, a curing agent, and additives selected as necessary at the time of coating. In the present invention, (A) an agent containing an epoxy resin is the base agent, and (B) an agent containing a resin that reacts with an epoxy resin is the curing agent. (C) A pigment may be blended in either the base agent or the curing agent, but is usually included in the base agent. (D) Water is usually included in the base agent and the curing agent, but may be used only in the base agent. Also, a part of (D) Water may be used as an additive when mixing the base agent and the curing agent.
[0021] Epoxy resin is a resin having an epoxy group in the molecule, and can be cured by the reaction of the epoxy group. Epoxy resin is generally known as a resin having excellent anticorrosive properties because it has high adhesion to substrates, particularly metal substrates, and also has an effect of shielding the substrate from environmental factors (e.g., water, oxygen, etc.) that affect the corrosion of substrates, particularly metal substrates (shielding effect). On the other hand, when used in a water-based paint composition, it has not been possible to say that the effect of improving adhesion and anticorrosive properties by this epoxy resin has been fully exerted. However, according to the present invention, by adjusting the elastic modulus and gel fraction of the coating film formed, it is possible to fully improve adhesion and anticorrosive properties even in a water-based paint composition.
[0022] The epoxy resin is preferably a resin having at least two epoxy groups in one molecule, and is obtained, for example, by reacting a polyhydric alcohol or a polyhydric phenol with a halohydrin, and specific examples include bisphenol A type epoxy resin, halogenated bisphenol A type epoxy resin, novolac type epoxy resin, polyglycol type epoxy resin, bisphenol F type epoxy resin, epoxidized oil, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, etc. Furthermore, from the viewpoint of increasing the elastic modulus of the resulting coating film, the epoxy resin is preferably one having a rigid structure such as an aromatic ring.
[0023] The epoxy resin is preferably blended in any one of the forms of an epoxy resin emulsion, an epoxy resin dispersion, and an aqueous epoxy resin solution. In this specification, the resin emulsion means an emulsion in which a resin is dispersed in an aqueous medium mainly composed of water, the resin dispersion means a dispersion in which a resin is dispersed in an aqueous medium mainly composed of water, and the aqueous resin solution means a solution in which a resin is dissolved in an aqueous medium mainly composed of water. The epoxy resin emulsion is not particularly limited, but is prepared by emulsifying an epoxy resin in an aqueous medium mainly composed of water by a normal forced emulsification method (a method using an emulsifier and a high-speed stirrer, etc.). Here, examples of the emulsifier include polyethers such as polyoxyethylene alkylphenol ether-based nonionic surfactants and polyoxyethylene-polyoxypropylene block copolymers; and adducts of at least one of the nonionic surfactants and the polyethers with a diisocyanate compound. The emulsifier may be used alone or as a blend of two or more types. Commercially available epoxy resin emulsions include, for example, Epolsion EA-1, 2, 3, 7, 12, 20, 55, and HD2 (manufactured by Henkel Japan Co., Ltd.); Yuka Resin KE-002, KE-116, E-1022, and KE-301C (manufactured by Yoshimura Oil Chemicals Co., Ltd.); Adeka Resin EM-101-50 (manufactured by Adeka Corporation); jER W1155R55, jER W3435R67, and jER W2821R70 (manufactured by Mitsubishi Chemical Corporation). Commercially available epoxy resin dispersions include, for example, Beckpox EP2381 (manufactured by Allnex Co., Ltd.); and EPI-REZ6530-WH-53 (manufactured by Momentive Co., Ltd.).
[0024] The epoxy resin may be a modified epoxy resin, such as a urethane-modified epoxy resin, an amine-modified epoxy resin, an isocyanate-modified epoxy resin, an acrylic-modified epoxy resin, a polyester-modified epoxy resin, or a dimer acid-modified epoxy resin.
[0025] The epoxy equivalent of the epoxy resin is preferably 100 to 1,000 g / eq, more preferably 200 to 700 g / eq, and even more preferably 300 to 600 g / eq. When the epoxy equivalent is 100 g / eq or more, sufficient coating film properties are easily obtained. On the other hand, when the epoxy equivalent is 1,000 g / eq or less, the leveling property is not easily deteriorated and a uniform coating film is easily obtained. When multiple epoxy resins are used in combination, it is preferable that the average epoxy equivalent of each epoxy resin mixture is within the above specified range. The epoxy equivalent of the epoxy resin can be determined according to JIS K 7236:2001 "Determination of epoxy equivalent of epoxy resin".
[0026] In the coating composition of the present invention, the amount of the epoxy resin in the non-volatile matter is preferably 30 to 70 mass %. The epoxy resin may be used alone or in combination of two or more kinds.
[0027] The resin that reacts with epoxy resin is a resin that reacts with epoxy resin, particularly with its epoxy group, and is used to promote or control the curing reaction. As the resin that reacts with epoxy resin, a resin having active hydrogen that reacts with epoxy group is preferable, and a polyamine resin is more preferable. The polyamine resin is a resin having at least two amino groups in one molecule. For example, the polyamine resin includes resins made by condensation polymerization of amines and aldehydes, etherification of amines with alcohols, ring-opening polymerization of amines having a heterocyclic structure (such as ethyleneimine), condensation of amines and carboxylic acids, or Mannich reaction of amines, formaldehyde, and ketones or phenols. Here, a polyamine resin that also has an amide bond in the molecule, such as a resin made by condensation of amines and carboxylic acids, is also called a "polyamidoamine resin" or "polyamidoamine". In addition, ring-opening polymerization of alkylene oxides such as ethylene oxide and propylene oxide can be used for etherification of amines with alcohols.
[0028] Examples of amines that can be used in producing the polyamine resin include aliphatic polyamines such as ethylenediamine, trimethylenediamine, tetramethylenediamine, pentamethylenediamine, triaminopropane, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, isophoronediamine, and 1,3-bisaminomethylcyclohexane; aromatic polyamines such as phenylenediamine, metaxylylenediamine, paraxylylenediamine, and diaminodiphenylmethane; and amines having a heterocyclic structure such as ethyleneimine.
[0029] The polyamine resin may be a modified polyamine resin. The modified polyamine resin is a polyamine resin in which a portion of the amino group is modified. The amino group can be modified by a known method, such as amidation of the amino group, Mannich reaction of the amino group with a carbonyl compound, or addition reaction of the amino group with an epoxy group.
[0030] The resin that reacts with the epoxy resin preferably contains at least a modified polyamine having a cyclic structure. By using a modified polyamine having a cyclic structure as the resin that reacts with the epoxy resin, the elastic modulus of the resulting coating film can be increased. The modified polyamine is a polyamine resin in which a part of the amino group is modified, and the modification can be, for example, amidation of the amino group, Mannich reaction of the amino group with a carbonyl compound, addition reaction of the amino group with an epoxy group, etc. The modified polyamine is preferably a Mannich modified polyamidoamine.
[0031] The content of the modified polyamine having a cyclic structure in the resin that reacts with the epoxy resin is preferably from 50 to 100% by mass, and more preferably from 60 to 90% by mass.
[0032] It is more preferable that the resin reacting with the epoxy resin contains at least a modified polyamine having a cyclic structure. The effect of increasing the elastic modulus can be enhanced by using a modified polyamine having a cyclic structure. The modified polyamine having a cyclic structure can be obtained by using a substance having a cyclic structure during its production. Examples of amines having a cyclic structure that can be used in the production of polyamine resins include piperazines such as N-aminoethylpiperazine, 1,3-bisaminoethylcyclohexane, isophoronediamine, 1-cyclohexylamino-3-aminopropane, 1,4-diaminocyclohexane, di(aminocyclohexyl)methane, 1,3-di-(aminocyclohexyl)propane, 2,4-diamino-cyclohexane N,N'-diethyl-1,4-diaminocyclohexane, and 3,3'-dimethyl-4,4'-diaminocyclohexylmethane; and aromatic polyamines such as phenylenediamine, metaxylylenediamine, paraxylylenediamine, and diaminodiphenylmethane. In addition, an aliphatic polyamine having a cyclic structure may be referred to as an alicyclic polyamine. In addition, examples of alcohols having a cyclic structure that can be used in the production of a polyamine resin include phenol and its derivatives. Examples of phenol derivatives include phenols in which the benzene ring is substituted with a hydrocarbon group, particularly phenols substituted with a linear or branched hydrocarbon group that may have one or more unsaturated bonds. Here, the hydrocarbon group is preferably a long-chain hydrocarbon group having 10 to 20 carbon atoms, particularly an alkyl group. Specific examples of phenol derivatives include cardanol. In addition, the resin to be reacted with the epoxy resin is preferably one having a cyclic structure, and more preferably one having a rigid structure such as an aromatic ring from the viewpoint of increasing the elastic modulus of the resulting coating film.
[0033] From the viewpoint of increasing the elastic modulus of the coating film, the modified polyamine having a cyclic structure is preferably a polyamine resin obtained by the Mannich reaction of amines, formaldehyde, and a phenol derivative. Here, the cyclic structure is derived from a phenol derivative, and the amines are preferably a chain compound (or acyclic compound) such as ethylenediamine. The phenol derivative is as described above, and cardanol is particularly preferred. Such modified polyamine resins are also called phenalkamine-based curing agents.
[0034] As described above, the use of modified polyamines, particularly modified polyamines having a cyclic structure, can increase the elastic modulus of the coating film. On the other hand, modified polyamines, particularly modified polyamines having a cyclic structure, tend to have low reactivity with epoxy resins. Therefore, it is preferable to use modified polyamines, particularly modified polyamines having a cyclic structure, in combination with resins that do not fall under the category of modified polyamines, as resins that react with epoxy resins. This ensures the reactivity of the resins that react with epoxy resins. Here, the resins that can be used in combination with modified polyamines are not particularly limited, and for example, polyoxyethylene amines (also called polyether amines) such as polyoxyethylene diamines and polyoxypropylene diamines can be used.
[0035] When the resin that reacts with the epoxy resin contains a modified polyamine and a resin that does not fall under the category of modified polyamine, it is preferable that the proportion of the modified polyamine in the entire resin that reacts with the epoxy resin is 50 to 99 mass %, and the proportion of the resin that does not fall under the category of modified polyamine is 1 to 50 mass %.
[0036] The resin that reacts with the epoxy resin is preferably blended in the form of an emulsion, a dispersion, or an aqueous solution.
[0037] The active hydrogen equivalent of the resin that reacts with the epoxy resin is preferably 80 to 350 g / eq, more preferably 100 to 250 g / eq. The active hydrogen equivalent of the resin that reacts with the epoxy resin is the number of grams [g / eq] of the resin containing 1 equivalent of active hydrogen, and is the value obtained by dividing the molecular weight of the resin that reacts with the epoxy resin by the number of hydrogen atoms of the amino group per molecule.
[0038] In the coating composition of the present invention, the amount of the resin reactive with the epoxy resin in the non-volatile matter is preferably 5 to 20 mass %. The resin reactive with the epoxy resin may be used alone or in combination of two or more kinds.
[0039] The pigment is not particularly limited, and pigments that are commonly used in the paint industry, such as anti-rust pigments, extender pigments, coloring pigments, etc. The pigments may be used alone or in combination of two or more.
[0040] Examples of the rust-preventive pigment include zinc powder, zinc oxide, barium metaborate, calcium silicate, aluminum phosphate, condensed aluminum phosphate, aluminum tripolyphosphate, zinc phosphate, zinc phosphite, potassium phosphite, calcium phosphite, aluminum phosphite, calcium zinc phosphate, zinc aluminum phosphate, zinc phosphomolybdate, aluminum phosphomolybdate, magnesium phosphate, vanadate / phosphoric acid mixed pigment, etc. Among these, from the viewpoint of corrosion prevention, phosphoric acid-based rust-preventive pigments are preferred. Examples of the phosphoric acid-based rust-preventive pigments include salts of phosphoric acid compounds such as phosphoric acid, phosphorous acid, and polyphosphoric acid (magnesium salts, calcium salts, zinc salts, aluminum salts, phosphomolybdate salts, etc.). In the coating composition of the present invention, the amount of the rust-preventive pigment in the non-volatile content is, for example, 1 to 20 mass%.
[0041] Examples of the extender pigment include silica, talc, mica, calcium carbonate, barium sulfate, etc. Among these, calcium carbonate is preferred from the viewpoint of chemical resistance. In the coating composition of the present invention, the amount of the extender pigment in the nonvolatile matter is, for example, 10 to 50 mass %.
[0042] Examples of color pigments include titanium oxide, iron oxide, carbon black, yellow lead, molybdate orange, ultramarine, Prussian blue, phthalocyanine blue, phthalocyanine green, quinacridone red, naphthol red, benzimidazolone yellow, Hansa yellow, benzimidazolone orange, dioxazine violet, etc. In the coating composition of the present invention, the amount of color pigment in the nonvolatile content is, for example, 1 to 20 mass %.
[0043] The pigment may be at least partially a scaly pigment. The scaly pigment has the effect of inhibiting the intrusion of corrosive factors such as water, oxygen, and chlorides, and the effect of reducing the internal stress of the coating film, based on its scaly shape. By reducing the internal stress of the coating film, the adhesion of the coating film can be further improved, and a thick coating film can be advantageously formed. Examples of the scaly pigment include talc, mica, kaolin clay, glass flake, micaceous iron oxide, aluminum, and other metal pigments. Some of the scaly pigments are classified into the above-mentioned rust-preventive pigments, extender pigments, or coloring pigments. In the coating composition of the present invention, the amount of the scaly pigment in the nonvolatile content is, for example, 0 to 50% by mass.
[0044] In the present invention, from the viewpoint of increasing the elastic modulus of the resulting coating film, it is preferable to use a scaly pigment having an aspect ratio of more than 1 and less than 120. From the viewpoint of increasing the elastic modulus, scaly pigments having an aspect ratio of more than 30 are preferable, but since such pigments have poor dispersibility, it is preferable that the average aspect ratio is from 1 to 30.
[0045] In this specification, the average aspect ratio of a scaly pigment refers to the ratio (D / T) of the average particle diameter (D) to the average thickness (T) of the scaly pigment. Here, the average particle diameter refers to the 50% particle diameter (D 50) and is determined from the particle size distribution measured using a laser diffraction / scattering particle size distribution analyzer. The particle size of a scaly pigment is expressed as the sphere equivalent diameter measured by the laser diffraction / scattering method. The average thickness is the average value of the thicknesses measured using a SEM (scanning electron microscope) for 100 or more scaly pigment particles.
[0046] The average particle size of the scaly pigment is preferably 3 to 40 μm, and more preferably 3 to 20 μm.
[0047] The coating composition of the present invention preferably has a pigment volume concentration (PVC) of 10 to 40%, more preferably 25 to 35%. In the present invention, from the viewpoint of increasing the elastic modulus of the resulting coating film, it is preferable that the PVC is high, and from this viewpoint, the PVC is preferably 28% or more.
[0048] In this specification, pigment volume concentration (PVC) is the ratio of the total volume of pigments to the total volume of non-volatile matter in a coating composition, and can be calculated from the composition and specific gravity of the components that make up the non-volatile matter.
[0049] The coating composition of the present invention has a coating film having an elastic modulus of 600 to 2400 N / mm when the coating composition is applied and dried for 7 days under conditions of 23°C and 50% humidity. 2 900~2400N / mm 2 It is preferable that the strength is 1300 to 2400 N / mm 2 The present inventors have set the elastic modulus of the coating film to 600 N / mm 2 It was found that the adhesion of the coating film can be improved by setting the modulus of elasticity at 2400N / mm or more. The modulus of elasticity is a physical property that indicates resistance to deformation. Therefore, it is believed that the higher the modulus of elasticity, the higher the resistance to deformation, which improves the adhesion of the coating film. In addition, when the modulus of elasticity of the coating film is 2400N / mm 2 If the content is less than this, the coating film will have excellent adhesion and exhibit excellent corrosion prevention properties without causing poor film formation.
[0050] (How to determine the elastic modulus of a coating film) The coating composition is applied to a substrate (e.g., a polypropylene plate) using an applicator so that the dry film thickness is 50 to 70 μm, and then dried for 7 days under conditions of 23°C and 50% humidity. A 50 mm x 10 mm rectangular test piece is cut out from the resulting coating film to prepare a measurement sample. A tensile test is performed at a speed of 5 mm / min in an environment of 23°C and 50% humidity, and the stress-strain ratio is calculated from the slope (proportionality constant) within the range in which the stress and strain are proportional.
[0051] Conventional epoxy resin-based water-based paint compositions have a coating film elastic modulus of 600 N / mm 2 However, the present inventors have found that by using a modified polyamine, particularly a modified polyamine having a cyclic structure, as a resin that reacts with the epoxy resin, the elastic modulus of the resulting coating film can be increased to 600 N / mm 2 It has been found that it is possible to form a coating film having an elastic modulus of 2400 N / mm or more. However, when the coating film is dried at a high temperature (for example, at a temperature of 50°C or more) or when the pigment volume concentration (PVC) exceeds 40%, the elastic modulus of the formed coating film is 2400 N / mm 2 It is expected that the elastic modulus will exceed 2400N / mm 2 A coating film exceeding this temperature tends to become hard and brittle, loses toughness, and may result in poor coating formation or cracks.
[0052] The coating composition of the present invention preferably has a gel fraction of 80% or more, preferably 90% or more, when the coating composition is applied and dried for 7 days under conditions of 23°C and 50% humidity. The gel fraction is an index of the reactivity of the epoxy resin and the resin that reacts with the epoxy resin. In the present invention, if the gel fraction of the coating film is less than 80%, the reactivity between these resins cannot be said to be sufficient, and problems such as re-dissolution occurring when a paint is applied over the coating film, insufficient water resistance and corrosion resistance being exhibited, etc. may occur.
[0053] For example, when a modified polyamine, especially a modified polyamine having a cyclic structure, is used as a resin that reacts with an epoxy resin, the effect of increasing the elastic modulus is obtained, but the reactivity with the epoxy resin tends to be low, and the gel fraction of the coating film may fall below 80%. In such a case, it is preferable to use a resin that does not fall under the category of modified polyamine having a cyclic structure as a resin that reacts with the epoxy resin in combination. This allows the elastic modulus of the coating film to be 600 to 2400 N / mm 2 It is also possible to achieve a gel fraction of 90% or more while still being within this range.
[0054] (How to determine the gel fraction of a coating film) The coating composition is applied to a substrate (e.g., a polypropylene plate) using an applicator so that the dry film thickness is 50 to 70 μm, and after drying for 7 days under conditions of 23°C and 50% humidity, it is peeled off from the substrate and the mass of the resulting coating film is measured and this mass is designated as W0. Next, the coating film is immersed in tetrahydrofuran (THF) at 23°C for 1 day. After immersion, the coating film is taken out of the THF and completely dried, and its mass is measured. The mass of the coating film at this time is designated as Wd. The mass loss rate is calculated by dividing the mass loss amount ΔW (=W0-Wd) by W0 and converting the value into a percentage. The gel fraction is a value calculated from the difference between 100% and the mass loss rate. Calculation formula: Gel fraction = 100-(W0-Wd) / W0 x 100
[0055] The coating composition of the present invention has a residual solvent content of less than 8.0%, preferably 7.0% or less, and more preferably 6.5% or less, when the coating composition is applied and dried for 7 days under conditions of 23°C and 50% humidity. If a large amount of solvent remains, problems such as a decrease in elastic modulus due to plasticization effect and insufficient adhesion may occur. The residual solvent content can be kept low by reducing the proportion of volatile components such as water and film-forming aids used in the coating composition.
[0056] (How to determine the amount of solvent remaining in a coating film) The coating composition is applied to a substrate (e.g., a polypropylene plate) using an applicator so that the dry film thickness is 50 to 70 μm. The mass of the coating composition used for coating is designated as the coating mass W0. Next, after coating, the coating is dried for 7 days under conditions of 23°C and 50% humidity, and the mass of the resulting coating film is measured, which is designated as the actual coating film mass W. In addition, the theoretical value of the final dry coating film mass is calculated from the mass of the non-volatile content in the coating composition used for coating, which is designated as the theoretical coating film mass Wz. The difference between the actual and theoretical coating film masses (W-Wz) is divided by the coating mass W0 to convert the value into a percentage to calculate the remaining amount of solvent. Calculation formula: remaining amount of solvent = (W-Wz) / W0 x 100
[0057]
[0043] The coating composition of the present invention may contain, as other components, appropriate blends according to the purpose, such as resins not corresponding to component (A) or component (B), crosslinking agents not corresponding to component (B), film-forming aids, antifreeze agents, surface conditioners (also called wetting agents), dispersants, defoamers, viscosity adjusters, thickeners, rust inhibitors not corresponding to anti-rust pigments, flash rust prevention agents, anti-settling agents, anti-skinning agents, anti-sagging agents, color separation prevention agents, matting agents, adhesion imparting agents, leveling agents, drying agents, catalysts, plasticizers, mildew inhibitors, antibacterial agents, antiviral agents, preservatives, insecticides, antistatic agents, and conductivity imparting agents.
[0058] The coating composition of the present invention can be prepared by preparing the base agent and the curing agent in advance, and then mixing the base agent, the curing agent, and, if necessary, the additives at the time of coating. The base agent and the curing agent can be prepared by mixing various components appropriately selected as necessary.
[0059] The coating composition of the present invention has a viscosity of 1 to 1000 (Pa·s, 23°C) at a shear rate of 0.1 (1 / s), and preferably has a viscosity of 0.05 to 10 (Pa·s, 23°C) at a shear rate of 1000 (1 / s).
[0060] In this specification, the viscosity is measured using a rheometer (for example, ARES rheometer manufactured by TA Instruments) after adjusting the liquid temperature to 23°C.
[0061] The means for applying the coating composition of the present invention is not particularly limited, and known coating means such as brush coating, roller coating, trowel coating, spatula coating, flow coater coating, and spray coating (e.g., air spray coating, airless spray coating), can be used.
[0062] The means for drying the coating composition of the present invention is not particularly limited, and may be either natural drying at ambient temperature or forced drying using a dryer or the like.
[0063] The coating composition of the present invention is capable of forming a coating film having excellent adhesion and preferably also having improved corrosion resistance, and therefore is suitable as an undercoat coating.
[0064] Examples of substrates to be coated with the coating composition of the present invention include plastic substrates such as epoxy resins, ABS resins, polycarbonates, polyvinyl chloride, polystyrene, acrylic resins, such as polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), polyolefins, such as polypropylene (PP), metal substrates such as steel, galvanized steel, tinned steel, stainless steel, magnesium alloys, aluminum, aluminum alloys, titanium, titanium alloys, and other metal substrates such as cement, mortar, concrete, slate, gypsum, calcium silicate, glass, ceramics, calcium carbonate, marble, and artificial marble, and other inorganic substrates other than metals, wood substrates such as wood, paper substrates, and composite substrates such as a combination of two or more of these substrates. Examples of composite substrates include composite substrates such as wood fiber reinforced cement boards, fiber reinforced cement boards, and fiber reinforced cement-calcium silicate boards, metal substrates that have been subjected to various surface treatments, such as oxidation treatments, and plastic substrates whose surfaces are coated with inorganic substances (for example, plastic substrates coated with glass).
[0065] Since the coating composition of the present invention is capable of forming a coating film that has excellent adhesion and preferably also excellent corrosion resistance, the substrate to be coated is preferably a metal substrate or a composite substrate made of a metal and another material.
[0066] The substrate may have various shapes, for example, a two-dimensional substrate such as a film, sheet, or plate, or a three-dimensional substrate that is a complex three-dimensional object, etc. The surface of the substrate may be smooth or may have irregularities.
[0067] The surface of the substrate may be subjected to pretreatment such as degreasing, chemical conversion treatment, polishing, etc., painting with a sealer, primer, zinc-rich paint, etc., plating, metal spraying, etc.
[0068] The substrate may have an old coating film on its surface. The old coating film may cover a part or the whole of the substrate surface. In this specification, the old coating film means a coating film that is already present on the substrate when painting, particularly repair, is performed.
[0069] When a substrate has an old coating film on its surface, the substrate surface including the old coating film can be coated with the coating composition of the present invention. If the old coating film is sound, the coating composition of the present invention can be applied onto the old coating film without peeling or removing the old coating film on the substrate surface. Since contaminants such as dust and dirt are attached to the old coating film, the adhesion of a new coating film to the old coating film can be improved by removing the contaminants. Methods for removing contaminants include high-pressure water washing, alkaline washing with caustic soda, etc., acid washing with inorganic or organic acids, washing with bleaching agents such as perchloric acid, and washing with scraping and cloth wiping.
[0070] The old coating film preferably contains a resin, and examples thereof include acrylic resin, silicone resin, acrylic silicone resin, styrene acrylic copolymer resin, polyester resin, fluororesin, rosin resin, petroleum resin, coumarone resin, phenolic resin, urethane resin, melamine resin, urea resin, epoxy resin, cellulose resin, xylene resin, alkyd resin, aliphatic hydrocarbon resin, butyral resin, maleic acid resin, fumaric acid resin, vinyl resin, amine resin, ketimine resin, and resins obtained by modifying these resins (modified resins), etc. The resins may be used alone or in combination of two or more.
[0071] The old coating film may contain various additives as other components, such as pigments, dispersants, surface conditioners, antioxidants, plasticizers, rust inhibitors, solvents, antibacterial agents, antiviral agents, viscosity adjusters, fillers, defoamers, charge control agents, stress relaxation agents, penetrating agents, light-guiding materials, glittering materials, magnetic materials, phosphors, ultraviolet absorbers, and radical scavengers.
[0072] The coating composition of the present invention has a coating film elastic modulus of 600 to 2400 N / mm when dried for 7 days under conditions of 23°C and 50% humidity. 2 Therefore, resistance to external stress is increased, and as a result, it is possible to form a coating film that is excellent in adhesion to the substrate and old coating film, and preferably also excellent in corrosion prevention. In addition, by selecting an appropriate undercoat or topcoat paint according to the external environment, it is possible to create a coating film that has properties adapted to the environment, such as antifouling properties, water repellency, weather resistance, environmental barrier properties, etc., in addition to imparting adhesion and corrosion prevention to the substrate and old coating film.
[0073] When the coating composition of the present invention is used as an undercoat coating, a topcoat coating film can be formed on the undercoat coating film, or an intermediate coating film and a topcoat coating film can be formed in that order.
[0074] The coating material for forming the intermediate coating film or the top coating film is preferably a water-based coating material composition, similar to the coating material composition of the present invention.These coating materials can be appropriately mixed with resins, crosslinking agents, pigments, water, film-forming aids, antifreezing agents, surface conditioners (also called wetting agents), dispersants, defoamers, viscosity adjusters, thickeners, rust inhibitors, antisettling agents, antiskinning agents, antisagging agents, color separation inhibitors, matting agents, adhesion agents, leveling agents, drying agents, catalysts, plasticizers, antifungal agents, antibacterial agents, antiviral agents, preservatives, insecticides, ultraviolet absorbers, radical scavengers, antistatic agents, and conductivity imparting agents, etc., according to the purpose. EXAMPLES
[0075] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0076] <Preparation example of coating composition> The base material and the curing agent were prepared by mixing the raw materials according to the formulation shown in Tables 1 and 2. The obtained base material and the curing agent were mixed with water for dilution in the mixing ratio shown in Table 3 to prepare a coating composition, which was then evaluated. The formulations and mixing ratios shown in Tables 1 to 3 are based on mass.
[0077] Details of the materials used in preparing the coating compositions are provided below. Epoxy resin 1: ADEKA Resin EM101-50 (ADEKA epoxy resin emulsion: non-volatile content 47% by mass, epoxy equivalent 1075 g / eq) Epoxy resin 2: jER W2821R70 (epoxy resin emulsion manufactured by Mitsubishi Chemical Corporation: non-volatile content 70% by mass, epoxy equivalent 220 to 240 g / eq) Anti-rust pigment: Aluminum tripolyphosphate K-WHITE#84S (manufactured by Teika Co., Ltd.) Extender pigment 1: Calcium carbonate (average particle size 6 μm) Extender pigment 2: Talc (average particle size 13 μm, aspect ratio less than 20) Color pigment 1: Titanium dioxide (white pigment) Color pigment 2: Carbon black (black pigment) Color pigment 3: Iron oxide (Oukatsu color pigment) Color pigment 4: Iron oxide (rust pigment) Dispersant: FLORENE GW-1640 (Kyoeisha Chemical Co., Ltd.) Film forming agent: Dipropylene glycol n-butyl ether Defoamer: SN DEFOAMER 1312 (San Nopco) Thickener: SN Thickener 665T (San Nopco, urethane modified polyether compound, non-volatile content 30%) Polyamine resin 1: Cardolite NX-8401 (amine resin emulsion manufactured by Cardolite; non-volatile content 57% by mass, active hydrogen equivalent 290 g / eq) Polyamine resin 2: Daitoclar X-7024 (amine resin emulsion manufactured by Daito Sangyo Co., Ltd.: non-volatile content 50%, active hydrogen equivalent 392 g / eq) Polyamine resin 3: JEFFAMINE T-403 (polyetheramine manufactured by HUNTSUMAN; non-volatile content 100% by mass, active hydrogen equivalent 81 g / eq) Polyamine resin 4: BECKOPOX EH623W (water-soluble amine resin manufactured by ALLNEX; non-volatile content 80% by mass, active hydrogen equivalent 200 g / eq) Rust inhibitor 1: HALOX650 (organic rust inhibitor manufactured by ICL Phosphate Specialty, non-volatile content 100% by mass) Rust inhibitor 2: Sodium nitrite
[0078] <Coating film preparation method 1> The paint prepared in the above <Preparation Example of Paint Composition> was applied to a polypropylene plate (2.0 x 70 x 150 mm) using an applicator so that the dry film thickness was 50 to 70 μm, and the plate was dried in an environment of 23°C and 50% relative humidity for 7 days to obtain a coated plate.
[0079] <Coating film preparation method 2> A sandblasted board (3.2 x 70 x 150 mm) was air-sprayed with a modified epoxy resin paint weak solvent type (manufactured by Dai Nippon Toryo Co., Ltd., "Epool Smile") to a dry film thickness of 55-65 μm, dried for one day in a 23°C, 50% relative humidity environment, and then forced dried for 7 days in a 50°C environment to obtain a base. The paint prepared in the above <Preparation Example of Paint Composition> was applied to the obtained base using an applicator to a dry film thickness of 50-70 μm, and dried for 7 days in a 23°C, 50% relative humidity environment to obtain a coated board.
[0080] <Coating film preparation method 3> The paint prepared in the above <Preparation Example of Paint Composition> was air spray painted onto a sandblasted board (3.2 x 70 x 150 mm) so that the dry film thickness was 55 to 65 μm, and then dried in a 23°C, 50% relative humidity environment for 7 days to obtain a painted board. The back side and periphery of the painted board were painted with the same paint and sealed.
[0081] <Elasticity modulus> From the coated plate prepared by coating method 1, a 50mm x 10mm strip of coating was cut out as a test piece, and a tensile test was carried out on the test piece at 23°C and 50% humidity at a speed of 5mm / min. The elastic modulus (N / mm 2 The results are shown in Table 3.
[0082] <Gel fraction> A 20 mm x 50 mm strip of coating film was cut out as a test piece from the coated plate prepared by coating film preparation method 1. The mass (W0) of the obtained coating film (test piece) was measured, and then the coating film (test piece) was immersed in tetrahydrofuran (THF) at 23°C for one day. After immersion, the coating film (test piece) was taken out of the THF, washed with THF, and then completely dried, and its mass (Wd) was measured, and the gel fraction was calculated using the following calculation formula and evaluated based on the following criteria. The results are shown in Table 3. Calculation formula: Gel fraction = 100-(W0-Wd) / W0 x 100 (standard) 〇: 85% or more △: 80% or more, less than 85% ×: Less than 80%
[0083] <Solvent Residual Rate> The mass (W) of the coating on the coated plate prepared by coating method 1 and the mass (W0) of the paint used to prepare the coating were measured, and the theoretical coating mass (Wz) when completely dried was calculated from the mass of the non-volatile matter in the paint. The remaining amount of solvent was calculated according to the following formula, and evaluated based on the following criteria. The results are shown in Table 3. Calculation formula: remaining amount of solvent = (W-Wz) / W0 x 100 (standard) ○: Less than 6.0% △: 6.0% or more, less than 8.0% ×: 8.0% or more
[0084] <Adhesion> In an environment of 23°C and 50% RH, nine grids were created by cutting four lines at 5 mm intervals vertically and horizontally with a cutter knife on the coating surface (test surface) on a coated plate prepared by coating preparation method 2 so as to reach the base material. Cellophane tape with creases on one side was firmly pressed against the grid surface and forcefully peeled off at an angle of 60 to 90°, and the adhesion of the coating was evaluated according to the following criteria based on the area of the remaining coating. The results are shown in Table 3. If the area of the remaining coating corresponds to four or more squares, the coating has excellent adhesion. (standard) ◎: The area of the remaining coating film corresponds to 8 or more squares. ○: The area of the remaining coating film corresponds to 6 or more but less than 8 squares. △: The area of the remaining coating film corresponds to 4 or more but less than 7 squares. ×: The area of the remaining coating film corresponds to less than 4 squares.
[0085] <Corrosion resistance> Test pieces were prepared by cutting a notch with a utility knife into the lower half of the coating on the coated plate prepared using coating method 3 so as to reach the sandblasted plate (base material). The condition of rust and blisters after 336 hours of neutral salt spray testing according to JIS Z 2371 was evaluated. The evaluation criteria are as follows, and the results are shown in Table 3. If the rust and blister width in the cut area is within 3 mm, the coating has excellent corrosion protection. (standard) ○: Rust and swelling width of cut area is less than 2mm △: Rust / bulge width of cut area is greater than 2mm and less than 3mm ×: Rust or blister width in cut area is 3mm or more, or abnormality is found in general area
[0086] [Table 1]
[0087] [Table 2]
[0088] [Table 3]
Claims
1. A two-liquid water-based coating composition comprising (A) an epoxy resin, (B) a resin that reacts with the epoxy resin, (C) a pigment, and (D) water, the coating composition being applied and dried for 7 days under conditions of 23°C and 50% humidity, and having a coating film with an elastic modulus of 600 to 2400 N / mm 2 The coating composition.
2. 2. The coating composition according to claim 1, wherein the coating film has a gel fraction of 80% or more when the coating composition is applied and dried for 7 days under conditions of 23°C and 50% humidity.
3. 3. A coating composition according to claim 1 or 2, characterized in that when the coating composition is applied and dried for 7 days under conditions of 23°C and 50% humidity, the amount of solvent remaining in the coating film is less than 8.0%.
4. 3. The coating composition according to claim 1, wherein the resin (B) that reacts with the epoxy resin contains at least a modified polyamine having a cyclic structure.
5. 3. The coating composition according to claim 1, wherein the resin that reacts with the epoxy resin (B) contains at least a modified polyamine having a cyclic structure, and the content of the modified polyamine having a cyclic structure in the resin that reacts with the epoxy resin (B) is 50 to 100 mass %.
Citation Information
Patent Citations
Aqueous epoxy resin composition and cured product of same
WO2020110601A1
Water-based anticorrosive coating composition
WO2021261071A1
Material for two-part aqueous Anti-corrosive coating and method for Anti-corrosive coating
JP2009149791A
Two liquid reaction-curable aqueous coating composition for primer, and multilayer film forming method using the same and coated body
JP2018053028A
Two-component epoxy resin paint
JP2019515991A
Cited By
Method for forming multilayer film