Solar battery and method for manufacturing solar battery
The solar cell design with a phase-separated active layer and controlled formation conditions addresses inefficiencies in existing cells by optimizing interfacial length, enhancing power generation efficiency through reduced exciton loss and charge recombination.
Patent Information
- Application Number
- JP2023051314
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing solar cells face challenges in improving power generation efficiency due to suboptimal phase-separated structures in their active layers, which can lead to exciton deactivation or charge recombination.
A solar cell design with a phase-separated active layer containing organic donor and acceptor materials, controlled by specific solvents and formation conditions, achieving an interfacial length of 70-100 μm, optimized by using a second solvent with lower solubility and forming at temperatures between 25°C and 40°C in a nitrogen atmosphere.
Enhances power generation efficiency by maintaining optimal phase separation, preventing exciton deactivation and charge recombination, thereby improving overall solar cell performance.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a solar cell and a method for manufacturing a solar cell. [Background technology]
[0002] In recent years, research and development into solar cells has been conducted to contribute to energy efficiency, ensuring that many people have access to affordable, reliable, sustainable and advanced energy.
[0003] 2. Description of the Related Art Solar cells are known in which a cathode, an electron transport layer, an active layer, a hole transport layer and an anode are laminated in this order, and the active layer contains an organic donor material and an organic acceptor material (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-13879 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, there is a demand for improving the power generation efficiency of solar cells.
[0006] An object of the present invention is to provide a solar cell capable of improving power generation efficiency. [Means for solving the problem]
[0007] (1) A cathode, an electron transport layer, an active layer, a hole transport layer and an anode are laminated in this order, and the active layer contains an organic donor material and an organic acceptor material, and has a thickness of 1 μm 2 A solar cell having a phase separation structure in which the interfacial length per unit area is 70 μm or more and 100 μm or less.
[0008] (2) The organic donor material has the chemical formula [ka] and the organic acceptor material is a compound represented by the chemical formula [ka] The solar cell according to (1), wherein the compound is a compound represented by the formula:
[0009] (3) A method for producing the solar cell according to (1) or (2), comprising the step of forming the active layer by applying a coating liquid containing the organic donor material, the organic acceptor material, a first solvent, and a second solvent, wherein the second solvent has a lower solubility for the organic donor material and the organic acceptor material than the first solvent.
[0010] (4) The method for producing a solar cell according to (3), wherein the first solvent is a halogen-based solvent, the second solvent is one or more solvents selected from the group consisting of diiodooctane, chloronaphthalene, dimethylformamide, dimethylbenzylamine, dichlorooctane, and octanediol, and the content of the second solvent is 1.0 volume % or less.
[0011] (5) The method for producing a solar cell according to (3) or (4), wherein the temperature of the environment in which the active layer is formed is 25° C. or higher and 40° C. or lower. Effect of the Invention
[0012] According to the present invention, it is possible to provide a solar cell capable of improving power generation efficiency. [Brief description of the drawings]
[0013] [Figure 1] 1 is a cross-sectional view showing an example of a solar cell according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a top view showing a phase-separated structure of the active layer in FIG. [Diagram 3]1 is a graph showing the relationship between the interface length per 1 μm 2 in the phase-separated structure of the active layer and power generation efficiency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0015] FIG. 1 shows an example of the solar cell of this embodiment.
[0016] The solar cell 10 has a cathode 11, an electron transport layer 12, an active layer 13, a hole transport layer 14, and an anode 15 laminated in this order.
[0017] As shown in FIG. 2, the active layer 13 contains an organic donor material D and an organic acceptor material A, and has a phase-separated structure. 2 The interface length per unit area is 70 μm or more and 100 μm or less, and preferably 75 μm or more and 90 μm or less. 2 If the interface length per unit area is less than 70 μm, the phase separation structure becomes coarse, and excitons generated by absorbing sunlight are easily deactivated, resulting in a decrease in the power generation efficiency of the solar cell 10. 2 If the interface length per unit area exceeds 100 μm, the phase separation structure becomes dense and separated charges tend to recombine, resulting in a decrease in the power generation efficiency of the solar cell 10.
[0018] The organic donor material D is not particularly limited as long as it is a p-type semiconductor material, and examples thereof include oligothiophene, polythiophene, polypyrrole, polyaniline, polyphenylene, polyphenylenevinylene, polythienylenevinylene, polyacetylene, polydiacetylene, tetrathiafulvalene, quinone, and tetracyanoquinodimethane. Among these, from the viewpoint of the power generation efficiency of the solar cell 10, the organic donor material represented by the chemical formula [ka] An example of the compound represented by the formula: PBDB-T-2F(PM6) (manufactured by Ossila) is mentioned.
[0019] The organic acceptor material A is not particularly limited as long as it is an n-type semiconductor material, and examples thereof include perfluoropentacene, perfluorophthalocyanine, naphthalene tetracarboxylic anhydride, perylene tetracarboxylic anhydride, naphthalene tetracarboxylic diimide, and perylene tetracarboxylic diimide. Among these, from the viewpoint of the power generation efficiency of the solar cell 10, the organic acceptor material represented by the chemical formula [ka] Examples of the organic acceptor material A other than the above include compound Y6 (manufactured by Sigma-Aldrich) represented by the formula: BTP-eC9 (manufactured by Ossila), BTP-4Cl-12 (manufactured by Ossila), BTP-4F-12 (manufactured by Ossila), compound Y7 (manufactured by Sigma-Aldrich) in which F in Y6 is replaced with Cl, and BTO (manufactured by Brilliant Matters).
[0020] The thickness of the active layer 13 is not particularly limited, but is, for example, not less than 90 nm and not more than 110 nm.
[0021] The active layer 13 is formed by applying a coating liquid containing an organic donor material D, an organic acceptor material A, a first solvent, and a second solvent. Here, the second solvent has a lower solubility in the organic donor material D and the organic acceptor material A than the first solvent. This reduces the solubility of the organic donor material D and the organic acceptor material A in the phase-separated structure of the active layer 13 by 1 μm. 2 The contact interface length can be adjusted.
[0022] The first solvent is not particularly limited, but examples thereof include halogen-based solvents such as chlorobenzene and chloroform.
[0023] The second solvent is a solvent having a thickness of 1 μm in the phase-separated structure of the active layer 13. 2As long as it is possible to adjust the contact interface length, the solvent is not particularly limited, and examples thereof include diiodooctane, chloronaphthalene, dimethylformamide, dimethylbenzylamine, dichlorooctane, and octanediol, and two or more of them may be used in combination.
[0024] The content of the second solvent in the coating liquid is 1.0% by volume or less, and preferably 0.1% by volume or more and 0.6% by volume or less. When the content of the additive in the coating liquid is 1.0% by volume or less, the power generation efficiency of the solar cell 10 is increased.
[0025] The temperature of the environment in which the active layer 13 is formed is preferably 25° C. or higher and 40° C. or lower. When the temperature of the environment in which the active layer 13 is formed is 25° C. or higher and 40° C. or lower, the power generation efficiency of the solar cell 10 is increased.
[0026] The active layer 13 may be formed in air, but is preferably formed in a nitrogen atmosphere, which increases the power generation efficiency of the solar cell 10.
[0027] The oxygen concentration in the nitrogen atmosphere is not particularly limited, but is, for example, 1 ppm or less. The dew point of the nitrogen atmosphere is not particularly limited, but is, for example, -70°C or more and -50°C or less.
[0028] The cathode 11 is a metal electrode. The metal constituting the metal electrode is not particularly limited, but examples thereof include aluminum, silver, and gold.
[0029] The thickness of the cathode 11 is not particularly limited, but is, for example, not less than 150 nm and not more than 200 nm.
[0030] The cathode 11 can be formed by, for example, a vacuum deposition method or a solution coating method.
[0031] The cathode 11 may be a transparent electrode.
[0032] The material constituting the electron transport layer 12 is not particularly limited, but examples thereof include 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP) and bis-3,6-(3,5-di-4-pyridylphenyl)-2-methylpyrimidine (B4PyMPM). Among these, poly(9,9-bis(3'-(N,N-dimethyl)-N-ethylammonium-propyl-2,7-fluorene)-alt-2,7-(9,9-dioctylfluorene))dibromide (PFN-Br) is preferred.
[0033] The thickness of the electron transport layer 12 is not particularly limited, but is, for example, not less than 5 nm and not more than 30 nm.
[0034] The electron transport layer 12 can be formed by, for example, a vacuum deposition method or a solution coating method.
[0035] The material constituting the hole transport layer 14 is not particularly limited, but examples thereof include polythiophene, poly(3,4-ethylenedioxythiophene) (PEDOT), polyaniline, N,N'-di(1-naphthyl)-N,N'-diphenyl-(1,1'-biphenyl)-4,4'-diamine (NPB), hexaazatriphenylene-hexacarbonitrile (HAT-CN), and tetraphenyldibenzoperiflanthene (DBP). Among these, poly(3,4-ethylenedioxythiophene) / polystyrenesulfonic acid (PEDOT / PSS) is preferred.
[0036] The thickness of the hole transport layer 14 is not particularly limited, but is, for example, not less than 8 nm and not more than 15 nm.
[0037] The hole transport layer 14 can be formed by, for example, a vacuum deposition method or a solution coating method.
[0038] The anode 15 is a transparent electrode. The material constituting the transparent electrode is not particularly limited, but examples thereof include indium tin oxide (ITO), indium zinc oxide (IZO), aluminum doped zinc oxide (AZO), gallium doped zinc oxide (GZO), zinc oxide (ZnO), and fluorine doped tin oxide (SnO2:F). Among these, ITO is preferable from the viewpoint of availability.
[0039] The thickness of the anode 15 is not particularly limited, but is, for example, not less than 100 nm and not more than 300 nm.
[0040] The anode 15 may be formed on a transparent substrate.
[0041] The material constituting the transparent substrate is not particularly limited, but examples thereof include glass and resin.
[0042] The thickness of the transparent substrate is not particularly limited, but is, for example, 0.5 mm or more and 1 mm or less.
[0043] A cathode buffer layer may be formed between the cathode 11 and the electron transport layer 12, and an anode buffer layer may be formed between the anode 15 and the hole transport layer 14. A hole collecting layer may be formed between the electron transport layer 12 and the active layer 13, and an electron collecting layer may be formed between the hole transport layer 14 and the active layer 13.
[0044] Alternatively, the cathode 11 may be a transparent electrode and the anode 15 may be a metal electrode.
[0045] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and the above embodiment may be modified as appropriate within the scope of the spirit of the present invention. EXAMPLES
[0046] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0047] [Example 1] (Preparation of coating solution for active layer) Compound PM6 (organic donor material) and compound Y6 (organic acceptor material) were weighed out in a mass ratio of 1:1.2, and then dissolved in chloroform (first solvent) to a concentration of 8 mg / ml. Next, chloronaphthalene (second solvent) was added to a content of 0.5% by volume to obtain a coating solution for the active layer.
[0048] (Fabrication of solar cells) On the ITO film of the glass substrate on which the ITO film (anode) of 150 nm thick was formed, a PEDOT / PSS film (hole transport layer) of 15 nm thick was formed by spin coating in the atmosphere. Next, an active layer coating liquid was applied on the PEDOT / PSS film by spin coating in a nitrogen atmosphere to form an active layer of 100 nm thick. Here, the nitrogen atmosphere had a temperature of 24.5°C, an oxygen concentration of 1 ppm, and a dew point of -40°C. Next, a PFN-Br film (electron transport layer) of 5 nm thick was formed on the active layer by spin coating in a nitrogen atmosphere. Next, an Al film (cathode) was formed on the PFN-Br film by vacuum deposition. Next, the solar cell was obtained by sealing with a glass cap using an ultraviolet curing adhesive in a nitrogen atmosphere. 2 The interface length per unit area was 70 μm.
[0049] [Example 2] A solar cell was obtained in the same manner as in Example 1, except that the temperature of the nitrogen atmosphere during the formation of the active layer was changed to 30° C. 2 The average interface length was 100 μm.
[0050] [Example 3] A solar cell was obtained in the same manner as in Example 1, except that the temperature of the nitrogen atmosphere during the formation of the active layer was changed to 29.5° C. 2 The interface length per unit area was 83 μm.
[0051] [Comparative Example 1] A solar cell was obtained in the same manner as in Example 1, except that the content of the second solvent was changed to 1 volume % when preparing the coating solution for the active layer. 2 The interface length per unit area was 52 μm.
[0052] [Comparative Example 2] A solar cell was obtained in the same manner as in Comparative Example 1, except that the temperature of the nitrogen atmosphere during the formation of the active layer was changed to 25° C. 2 The interface length per unit area was 52 μm.
[0053] [Comparative Example 3] A solar cell was obtained in the same manner as in Comparative Example 1, except that the temperature of the nitrogen atmosphere during the formation of the active layer was changed to 30° C. 2 The interface length per unit area was 62 μm.
[0054] [1μm in the phase-separated structure of the active layer 2 Peripheral length] Using an atomic force microscope (AFM), a phase image of the active layer formed during the fabrication of the solar cell was obtained, and the phase image was then binarized. Next, the length of the boundary between the organic donor material and the organic acceptor material was calculated from the binarized phase image, and then divided by the area of the phase image to obtain the 1 μm 2 In the binarization process of the phase image, the threshold value was set to the position where the mass ratio of the organic donor material and the organic acceptor material in the coating liquid for the active layer was equal to the area ratio of the phase image.
[0055] [Power generation efficiency of solar cells] The power generation efficiency of the solar cell was measured in accordance with IEC 61215 and 61836 (JIS C61215 MQT06, JIS C8904). At this time, the irradiance of the light source was set to 1000 W / m2 in accordance with JIS C8904-3. 2 The temperature of the solar cell (module temperature) was set to 25°C.
[0056] Table 1 shows the evaluation results of the power generation efficiency of the solar cells. [Table 1]
[0057] In addition, Fig. 3 shows the 1 μm 2 The relationship between the permeable interface length and power generation efficiency is shown.
[0058] 3, it can be seen that the solar cells of Examples 1 to 3 have high power generation efficiency. In contrast, the solar cells of Comparative Examples 1 to 3 have a 1 μm 2 The interface lengths per unit area are 55 μm, 66 μm, and 105 μm, respectively, resulting in low power generation efficiency. [Explanation of symbols]
[0059] 10. Solar Cells 11 Cathode 12 Electron transport layer 13 Active layer 14 Hole transport layer 15 Anode D Organic donor material A Organic Acceptor Material
Claims
1. A cathode, an electron transport layer, an active layer, a hole transport layer, and an anode are sequentially stacked, The active layer includes an organic donor material and an organic acceptor material, and has a thickness of 1 μm 2 A solar cell having a phase separation structure in which the interface length per unit area is 70 μm or more and 100 μm or less.
2. The organic donor material has the formula [Formula 1] A compound represented by the formula: The organic acceptor material has the formula [chemical 2] The solar cell according to claim 1 , wherein the compound is represented by the formula:
3. A method for producing the solar cell according to claim 1 or 2, comprising the steps of: forming the active layer by applying a coating liquid containing the organic donor material, the organic acceptor material, a first solvent, and a second solvent; The second solvent has a lower solubility for the organic donor material and the organic acceptor material than the first solvent.
4. the first solvent is a halogen-based solvent, the second solvent is one or more solvents selected from the group consisting of diiodooctane, chloronaphthalene, dimethylformamide, dimethylbenzylamine, dichlorooctane, and octanediol; The method for producing a solar cell according to claim 3 , wherein the content of the second solvent is 1.0% by volume or less.
5. The method for manufacturing a solar cell according to claim 3 , wherein the temperature of the environment in which the active layer is formed is 25° C. or higher and 40° C. or lower.