Method for covering metal component with insulation coating and solid lubrication coating

By employing multiple layers of insulating film coating and natural drying with a solid lubricant film, the method significantly enhances voltage resistance performance in metal parts, achieving high withstand voltages across various thickness ranges.

JP2024140311APending Publication Date: 2024-10-10PARKER NETSUSHORI KOGYO CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023051399
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Conventional methods for coating metal parts with insulating and solid lubricating films fail to achieve superior voltage resistance performance.

Method used

A method involving multiple layers of insulating film coating and natural drying steps, followed by a firing process with a solid lubricant film application, enhances the voltage resistance performance.

Benefits of technology

The method achieves significantly improved voltage resistance performance, with withstand voltages exceeding 1200V for an insulating film thickness of 10 μm or less, 1400V for 10-15 μm, and 1800V for 15-20 μm, while maintaining a total film thickness of 30 μm or less.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140311000001_ABST
    Figure 2024140311000001_ABST
Patent Text Reader

Abstract

To provide a method for covering a metal component with an insulation coating and a solid lubrication coating, the method being capable of realizing an excellent voltage resistance performance compared to conventional ones.SOLUTION: A method for covering a metal component with an insulation coating and a solid lubrication coating includes: a first applying step of applying a first layer of the insulation coating onto a surface of the metal component; a first drying step of drying the first layer applied in the first applying step; a second applying step of applying a second layer of the insulation coating onto a surface of the first layer dried in the first drying step; a second drying step of drying the second layer applied in the second applying step; a solid lubrication coating applying step of applying the solid lubrication coating after the second drying step; and a calcination step of calcining the metal component accompanied with the first layer and the second layer of the insulation coating and the solid lubrication coating after the solid lubrication coating applying step.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for coating a metal part with an insulating coating and a solid lubricant coating, and also to a metal part coated with an insulating coating and a solid lubricant coating. [Background technology]

[0002] Patent Document 1 describes that by coating a metal part (rolling bearing) with an insulating film (insulating coating) and a solid lubricant coating (creep-resistant coating), it is possible to simultaneously achieve both insulating performance and wear resistance (creep-resistant coating). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2022-42162 Summary of the Invention [Problem to be solved by the invention]

[0004] The present inventors, through repeated intensive research and experimentation into specific aspects of the method for coating an insulating coating and a solid lubricating coating, have found that carrying out the painting (application) and drying of the insulating coating multiple times (multiple layers) significantly improves the voltage resistance performance provided by the insulating coating.

[0005] The present invention has been devised based on the above findings. An object of the present invention is to provide a method for coating a metal part with an insulating coating and a solid lubricant coating, which is capable of achieving superior voltage resistance performance compared to conventional methods. Another object of the present invention is to provide a metal part that can be produced by the method and has superior voltage resistance performance compared to conventional methods. [Means for solving the problem]

[0006] The present invention is a method for coating a metal part with an insulating coating and a solid lubricant coating, comprising: a first coating step of coating a first layer of insulating coating on a surface of the metal part; a first drying step of drying the first layer coated in the first coating step; a second coating step of coating a second layer of insulating coating on the surface of the first layer dried in the first drying step; a second drying step of drying the second layer coated in the second coating step; a solid lubricant coating coating step of coating a solid lubricant coating after the second drying step; and a firing step of firing the metal part with the first and second layers of insulating coating and the solid lubricant coating after the solid lubricant coating coating step.

[0007] According to the present invention, by dividing the insulating coating into a first layer and a second layer, i.e., by separating the coating and drying of the first layer from the coating and drying of the second layer, it is possible to achieve voltage resistance performance that is significantly superior to conventional techniques, as will be clearly demonstrated in the examples described below.

[0008] According to the findings of the present inventors, the first drying step is preferably a natural drying step carried out for a period of 5 minutes or more.

[0009] The insulating coating may be applied and dried in three separate layers (a first layer, a second layer, and a third layer). That is, the present invention may further include a third coating step of applying a third layer of the insulating coating onto the surface of the second layer dried in the second drying step, and a third drying step of drying the third layer applied in the third coating step, in which case the solid lubricant coating step is carried out after the third drying step.

[0010] In this case, according to the findings of the present inventors, the second drying step is preferably a natural drying step carried out for 5 minutes or more.

[0011] Similarly, the insulating coating may be applied and dried in four or more layers.

[0012] According to the method of the present invention, in a metal component coated with an insulating coating and a solid lubricant coating, an insulating coating having a thickness (only) of 10 μm or less can provide a withstand voltage performance of 1,200 V or more when the leakage current threshold is 10 mA.

[0013] Furthermore, according to the method of the present invention, in a metal component coated with an insulating coating and a solid lubricant coating, an insulating coating having a thickness (only) of 10 μm to 15 μm can provide a withstand voltage performance of 1,400 V or more when the leakage current threshold is 10 mA.

[0014] Furthermore, according to the method of the present invention, in a metal component coated with an insulating coating and a solid lubricant coating, an insulating coating having a thickness (only) of 15 μm to 20 μm can provide a withstand voltage performance of 1800 V or more when the leakage current threshold is 10 mA.

[0015] As described above, while still providing extremely high voltage resistance, the sum of the thicknesses of the insulating film and the solid lubricating film can be kept to, for example, 30 μm or less. Effect of the Invention

[0016] According to the present invention, by dividing the insulating coating into multiple layers, i.e., by separating the painting and drying of a first layer from the painting and drying of a second layer (...., the painting and drying of an n-th layer), it is possible to achieve voltage resistance performance that is significantly superior to conventional techniques, as will be clearly shown in the examples described below. [Brief description of the drawings]

[0017] [Figure 1] 1 is a flowchart showing a method for coating a metal component with an insulating coating and a solid lubricant coating according to a first embodiment of the present invention. [Diagram 2] 1 is a table showing the withstand voltages of Examples 1 to 6 obtained according to the first embodiment of the present invention, together with the withstand voltages of the corresponding Comparative Examples 1 to 6. [Diagram 3]5 is a flowchart showing a method for coating a metal component with an insulating coating and a solid lubricant coating according to a second embodiment of the present invention. [Figure 4] 11 is a table showing the withstand voltages of Examples 7 to 9 obtained in the second embodiment of the present invention. [Diagram 5] 1 is a photograph of the front side of a ring test piece used in each of the examples and comparative examples. [Figure 6] 6 is a photograph of the back side of the ring specimen of FIG. 5. [Figure 7] 6 is a photograph of the ring specimen of FIG. 5 taken from the side. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described.

[0019] (First embodiment: flow chart) 1 is a flow chart showing a method for coating a metal component with an insulating coating and a solid lubricant coating according to a first embodiment of the present invention, in which the insulating coating is applied and dried in a first layer and a second layer.

[0020] That is, as shown in Fig. 1, first, a first coating step is performed in which a first layer of an insulating coating is coated (generally spray-coated) on the surface of a metal part (STEP 1). Then, a first drying step is performed in which the first layer coated in the first coating step is dried (STEP 2). Then, a second coating step is performed in which a second layer of an insulating coating is coated (generally spray-coated) on the surface of the first layer dried in the first drying step (STEP 3). Then, a second drying step is performed in which the second layer coated in the second coating step is dried (STEP 4).

[0021] After the second drying step, a solid lubricant coating coating step is carried out in which a solid lubricant coating is applied (STEP 5), and after the solid lubricant coating coating step, a firing step is carried out in which the metal part with the first and second layers of the insulating coating and the solid lubricant coating is fired (STEP 6).

[0022] In this embodiment, the first drying step (STEP 2) and the second drying step (STEP 4) are natural drying steps, each of which is carried out for 5 minutes.

[0023] In this embodiment, the baking step (STEP 6) is carried out at 120° C. for 90 minutes.

[0024] (First embodiment: Examples and comparative examples) According to the flow chart of the first embodiment shown in Fig. 1, the films shown in Examples 1 to 6 were formed on metal parts, and the withstand voltage performance was evaluated. Meanwhile, the withstand voltage performance was also evaluated for Comparative Examples 1 to 6 (STEP 3 and STEP 4 were not performed) in which the insulating film was applied and dried only once. Furthermore, for reference, in the case where the insulating film was not applied and dried, a manganese phosphate layer (thickness 5 µm) was formed as a base instead of the insulating film, and the withstand voltage performance was evaluated for Comparative Example 7 (the result of Comparative Example 7 shows that the withstand voltage performance is dominated by the effect of the insulating film).

[0025] As an example of a metal part, a ring test piece made of hot forged sintered alloy (AISI4620) with an outer diameter of 35 mm and a thickness of 8.8 mm was used. The surface hardness before coating was 60HRC. Photographs of the cut surface of the ring piece (approximately divided into two) are shown in Figures 5 to 7. The target surface on which each coating is formed is the cylindrical outer surface of the ring piece. The inner hole of the ring piece has a tapered surface for mounting to the wear tester described later, but no coating is formed on the surface of the inner hole.

[0026] As an example of the insulating coating, PAI resin (polyamide-imide resin) was used for both the first and second layers. The weight molecular weight was about 17,500 (for example, it can be measured by a general GPC method). The coating amount of each layer was adjusted so that the thickness after drying was about half of the "insulating coating thickness" shown in the table of Figure 2 (i.e., it was roughly divided into two in terms of volume and / or weight).

[0027] As an example of a solid lubricant film, "HMB-2" manufactured by Kawamura Laboratory Co., Ltd. was used (the ingredients listed in the SDS are lubricant ingredients: molybdenum disulfide 5%, antimony trioxide 5%, solvent: 1,4 dioxane 45%, N-methylpyrrolidone 25-35%, xylene 1.8%, ethylbenzene 1.8%).

[0028] The withstand voltage was evaluated using a withstand voltage tester (TOS5301) manufactured by Kikusui Electronics Co., Ltd. Specifically, the withstand voltage was measured by increasing the voltage from 0V to 6200V over a period of 10 seconds, with the leakage current threshold set at 10mA.

[0029] As shown in the table of Fig. 2, Examples 1 and 2 are examples in which the thickness of the insulating coating (total thickness of the first layer and the second layer) is 10 µm or less. The thickness of the insulating coating and the thickness of the solid lubricating coating can be evaluated (measured) using a micrometer after each drying step, or by microscopic observation or component analysis of the cross section of the coating after firing. The withstand voltages of Examples 1 and 2 are significantly higher than those of the corresponding Comparative Examples 1 and 2 (in which the insulating coating is 10 µm thick).

[0030] Even if an error of about 10% is taken into account, according to this embodiment, in a case where the insulating coating is made of PAI resin having a thickness of 10 μm or less, a withstand voltage of 1200 V or more can be achieved when the leakage current threshold is set to 10 mA.

[0031] 2, Examples 2, 3, 4, and 5 are examples in which the thickness of the insulating coating (total thickness of the first and second layers) is 10 μm to 15 μm. The withstand voltages of Examples 2, 3, 4, and 5 are significantly higher than the withstand voltages of the corresponding Comparative Examples 2, 3, 4, and 5 (in which the insulating coating has a thickness of 10 μm to 15 μm).

[0032] Even if an error of about 10% is taken into account, according to this embodiment, when the insulating coating is made of PAI resin having a thickness of 10 μm to 15 μm, a withstand voltage of 1400 V or more can be achieved when the leakage current threshold is 10 mA.

[0033] 2, Examples 5 and 6 are examples in which the thickness of the insulating coating (total thickness of the first and second layers) is 15 μm to 20 μm. The withstand voltages of Examples 5 and 6 are significantly higher than the withstand voltages of the corresponding Comparative Examples 5 and 6 (in which the insulating coating has a thickness of 15 μm to 20 μm).

[0034] Even if an error of about 10% is taken into account, according to this embodiment, when the insulating coating is made of PAI resin having a thickness of 15 μm to 20 μm, a withstand voltage of 1800 V or more can be achieved when the leakage current threshold is 10 mA.

[0035] (First embodiment: function and effect) As described above, according to the present embodiment, by dividing the insulating coating into a first layer and a second layer, i.e., by separating the coating and drying of the first layer from the coating and drying of the second layer, it is possible to achieve significantly superior voltage resistance performance compared to Comparative Examples 1 to 6, as clearly shown by Examples 1 to 6.

[0036] More specifically, as shown in Examples 1 and 2, in a metal component coated with an insulating film and a solid lubricant film, an insulating film having a thickness (only) of 10 μm or less can provide a withstand voltage performance of 1200 V or more when the leakage current threshold is set to 10 mA.

[0037] Furthermore, as shown in Examples 2, 3, 4, and 5, according to the method of the present invention, in a metal component coated with an insulating coating and a solid lubricant coating, an insulating coating having a thickness of 10 μm to 15 μm (only) can provide a withstand voltage performance of 1400 V or more when the leakage current threshold is 10 mA.

[0038] Furthermore, as shown in Examples 5 and 6, in a metal component coated with an insulating coating and a solid lubricant coating, an insulating coating having a thickness (only) of 15 μm to 20 μm can provide a withstand voltage performance of 1800 V or more when the leakage current threshold is 10 mA.

[0039] As shown in Examples 1 to 6, the sum of the thicknesses of the insulating coating and the solid lubricating coating (total thickness) can be kept to 30 μm or less while still providing extremely high voltage resistance.

[0040] The thickness ratio of the insulating film to the solid lubricant film can be divided into the following five categories, and improvements in voltage resistance performance can be confirmed in all five categories. (i) Insulating film / solid lubricant film≦1 / 2 (Example 1, Comparative Example 1) (ii) 1 / 2≦insulating film / solid lubricant film≦2 / 3 (Examples 1 to 3, Comparative Examples 2 to 4) (iii) 2 / 3≦insulating film / solid lubricant film≦3 / 2 (Examples 3 to 5, Comparative Examples 4 to 5) (iv) 3 / 2≦insulating film / solid lubricant film≦2 (Examples 5 to 6, Comparative Examples 5 to 6) (v) 2≦Insulating film / solid lubricant film

[0041] (Second embodiment: flow chart) 3 is a flow chart showing a method for coating a metal component with an insulating coating and a solid lubricant coating according to a second embodiment of the present invention. In this embodiment, the insulating coating is applied and dried in a first layer, a second layer, and a third layer.

[0042] That is, first, as shown in FIG. 3, a first coating step is performed in which a first layer of an insulating film is coated (generally spray-coated) on the surface of a metal part (STEP 21). Then, a first drying step is performed in which the first layer coated in the first coating step is dried (STEP 22). Then, a second coating step is performed in which a second layer of an insulating film is coated (generally spray-coated) on the surface of the first layer dried in the first drying step (STEP 23). Then, a second drying step is performed in which the second layer coated in the second coating step is dried (STEP 24). Then, a third coating step is performed in which a third layer of an insulating film is coated (generally spray-coated) on the surface of the second layer dried in the second drying step (STEP 25). Then, a third drying step is performed in which the third layer coated in the third coating step is dried (STEP 26).

[0043] After the third drying step, a solid lubricant coating coating step is carried out in which a solid lubricant coating is applied (STEP 27), and after the solid lubricant coating coating step, a firing step is carried out in which the metal part with the first, second and third layers of the insulating coating and the solid lubricant coating is fired (STEP 28).

[0044] In this embodiment, the first drying step (STEP 22), the second drying step (STEP 24), and the third drying step (STEP 26) are also natural drying steps, and each of them takes 5 minutes.

[0045] In this embodiment, the baking step (STEP 26) is also carried out at 120° C. for 90 minutes.

[0046] (Second embodiment: Example) According to the flow chart of the second embodiment shown in FIG. 2, the films shown in Examples 7 to 9 were formed on metal parts, and the voltage resistance performance was evaluated.

[0047] As in the first embodiment, a ring test piece made of hot forged sintered alloy (AISI4620) with an outer diameter of 35 mm and a thickness of 8.8 mm was used as an example of a metal part (see Figs. 5 to 7). The surface hardness before coating was 60HRC.

[0048] As in the first embodiment, PAI resin (polyamide-imide resin) was used as an example of the insulating coating for the first, second and third layers. The weight molecular weight was about 17,500. The coating amount of each layer was adjusted so that the thickness after drying was about 1 / 3 of the "insulating coating thickness" shown in the table of FIG. 2 (i.e., the coating amount was roughly divided into three equal parts in terms of volume and / or weight).

[0049] As in the first embodiment, "HMB-2" manufactured by Kawamura Laboratory Co., Ltd. was used as an example of the solid lubricant film.

[0050] As in the first embodiment, the withstand voltage was evaluated using a withstand voltage tester (TOS5301) manufactured by Kikusui Electronics Co., Ltd. Specifically, the withstand voltage was determined by setting the leakage current threshold to 10 mA during the process of increasing the voltage from 0 V to 6200 V over 10 seconds.

[0051] 2, Examples 7, 8, and 9 are examples in which the insulating coating has a thickness (total thickness of the first, second, and third layers) of 15 to 20 μm. The withstand voltages of Examples 7, 8, and 9 are significantly higher than the withstand voltages of the corresponding Comparative Examples 5 and 6 (in which the insulating coating has a thickness of 15 to 20 μm).

[0052] Even if an error of about 10% is taken into account, according to this embodiment, a withstand voltage of 2200 V or more can be achieved when the insulating coating is made of PAI resin and has a thickness of 15 to 20 μm.

[0053] (Second embodiment: action and effect) As described above, according to the present embodiment, by dividing the insulating coating into a first layer, a second layer, and a third layer, i.e., by separating the coating and drying of the first layer from the coating and drying of the second layer and the coating and drying of the third layer, it is possible to achieve significantly superior voltage resistance performance compared to Comparative Examples 5 and 6, as clearly shown by Examples 7 to 9.

[0054] More specifically, as shown in Examples 7, 8, and 9, according to the method of the present invention, in a metal component coated with an insulating film and a solid lubricant film, an insulating film having a thickness (only) of 15 μm to 20 μm can provide a withstand voltage performance of 2200 V or more with a leakage current threshold of 10 mA.

[0055] Furthermore, as shown in Examples 7 to 9, the sum of the thicknesses of the insulating coating and the solid lubricating coating (total thickness) can be kept to 30 μm or less while still providing extremely high voltage resistance.

[0056] (Additional information about the insulating film) In each of the above examples and comparative examples, a PAI resin having a weight molecular weight of about 17,500 was used as the insulating coating, but the present invention is applicable in substantially the same manner even if the weight molecular weight is changed.

[0057] In fact, additional examples 1 and 2 having thickness distributions roughly similar to those of examples 1 and 6 (categories (i) and (v)) were manufactured using a PAI resin with a weight molecular weight of about 9000, and the withstand voltages were evaluated. The values ​​were 1455 V and 2480 V, respectively, within ±10% of the values ​​of examples 1 and 6.

[0058] Furthermore, additional examples 3 and 4 having thickness distributions roughly similar to those of examples 1 and 6 (categories (i) and (v)) were manufactured using a PAI resin with a weight molecular weight of about 32,000, and the withstand voltages were evaluated to be 1,382 V and 2,539 V, respectively, which were values ​​within ±10% of the values ​​of examples 1 and 6.

[0059] In addition, the material of the insulating film is generally a mixture of PAI resin as the main component and epoxy resin. Examples of epoxy resin include bisphenol A type, bisphenol F type, novolac type, aliphatic type, and glycidylamine type epoxy resins. The epoxy resin content can be about 0 to 50% relative to the PAI resin. If the resin does not harden at 120°C or less, a curing agent or a curing accelerator can be added. Examples of the curing agent include aliphatic polyamines, aromatic amines, polyamidoamines, amine salts, acid anhydrides, imidazole compounds, and BF3 complexes. The curing agent content can be about 80 to 110% of the stoichiometric amount relative to the epoxy resin. In addition, an insulating solid lubricant can be mixed to improve the sliding properties of the insulating film. For example, polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, fluorinated ethylene propylene resin, boron nitride, melamine cyanurate, mica, etc. The content of the solid lubricant is permissible at about 0 to 30% of the dry PAI resin.

[0060] (Additional information on solid lubricant films) For the above Examples 1 to 9 and Additional Examples 1 to 4, the wear resistance based on the solid lubricant film was evaluated by a friction wear test using a block-on-ring type LFWA-1 friction wear tester manufactured by FALEX Corporation, and good results equivalent to or better than existing solid lubricant films were obtained. Specifically, the lubricant was ATF, and each Example (test piece) was rotated at 55 RPM and pressed against a block of ADC12 (a type of aluminum alloy) at 100 LBS for 24 hours, and the cross-sectional curves of the test piece and the block were measured to determine the amount of wear. In Comparative Example 7, the friction coefficient rose sharply during the test, so the test was interrupted after 8 hours, but in Examples 1 to 9 and Additional Examples 1 to 4, the test was continued for 24 hours, and the wear amount of the test piece was 25 μm or less, and the wear amount of the block was 5 μm or less, which was a good result.

Claims

1. A method for coating a metal part with an insulating coating and a solid lubricating coating, comprising the steps of: a first coating step of coating a first layer of an insulating coating on a surface of the metal part; a first drying step for drying the first layer applied in the first coating step; a second coating step of coating a second layer of the insulating coating on the surface of the first layer dried in the first drying step; a second drying step for drying the second layer applied in the second coating step; a solid lubricant coating coating step of coating a solid lubricant coating after the second drying step; a firing step of firing the metal part together with the first layer and the second layer of the insulating coating and the solid lubricant coating after the solid lubricant coating coating step; A method comprising:

2. The first drying step is a natural drying step carried out for 5 minutes or more.

2. The method of claim 1 .

3. a third coating step of coating a third layer of the insulating coating on the surface of the second layer dried in the second drying step; a third drying step for drying the third layer applied in the third coating step; The solid lubricant coating step is carried out after the third drying step.

3. The method according to claim 1 or 2.

4. The second drying step is a natural drying step carried out for 5 minutes or more.

4. The method according to claim 3 .

5. A metal part coated with an insulating coating and a solid lubricating coating, The insulating coating is at least mainly composed of a PAI resin and has a thickness of 10 μm or less, The withstand voltage of the metal part is 1200V or more when the leakage current threshold is 10mA. A metal part characterized by:

6. A metal part coated with an insulating coating and a solid lubricating coating, The insulating coating is at least mainly composed of PAI resin and has a thickness of 10 μm to 15 μm, The withstand voltage of the metal part is 1400V or more when the leakage current threshold is 10mA. A metal part characterized by:

7. A metal part coated with an insulating coating and a solid lubricating coating, The insulating coating is at least mainly composed of PAI resin and has a thickness of 15 μm to 20 μm, The withstand voltage of the metal part is 1800V or more when the leakage current threshold is 10mA. A metal part characterized by:

8. The sum of the thicknesses of the insulating film and the solid lubricating film is 30 μm or less.

8. The metal part according to claim 5, wherein the metal part is made of a non-magnetic material.

Citation Information

Patent Citations

  • Roller bearing

    JP2022042162A