Submerged arc welding method for high-tensile strength steel
Patent Information
- Application Number
- JP2023051557
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-28
AI Technical Summary
【0012】 本発明を適用した高張力鋼のサブマージアーク溶接方法によれば、安定した溶接金属の強度及び低温靭性が得られ、かつ、溶接金属の拡散性水素量が低く、溶接欠陥が無く、溶接作業性が得られるなど、高能率に高品質な溶接部を提供することが可能となる。
Smart Images

Figure 2024140424000001 
Figure 2024140424000002 
Figure 2024140424000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a submerged arc welding method for 780 MPa class high tensile steel, which provides stable weld metal strength and low temperature toughness, has a low diffusible hydrogen content in the weld metal, is free of welding defects, and has good welding workability. [Background technology]
[0002] Submerged arc welding is highly efficient and produces weld metal with good welding workability and excellent mechanical properties, and is therefore used in a wide range of fields, such as shipbuilding, steel frame construction, pipe construction, bridges, and vehicles.
[0003] In recent years, with the development of the energy industry, the strength and toughness of steel materials, and the thickness of plates are being increased due to the enlargement of structures, are being considered, and the application rate of submerged arc welding is increasing year by year from the viewpoint of quality and productivity. In such submerged arc welding of high tensile steel, further quality improvement is required to improve productivity in welding work and ensure safety and durability, and among them, high welding efficiency and strength and toughness of the weld metal that match the steel characteristics are required. Since submerged arc welding has a large welding heat input and a large base metal dilution rate compared to covered metal arc welding and gas shielded arc welding, the welding workability and performance of the weld metal are mostly determined by the composition of the flux and wire. In submerged arc welding of high tensile steel, bonded fluxes that can freely adjust the chemical composition of the weld metal are used to ensure the strength and toughness of the weld metal that match the steel. However, in the welding of high tensile steel, the strength and toughness of the weld metal cannot be obtained by simply adding alloying components to the bonded flux. Therefore, in order to obtain the appropriate strength and toughness of the weld metal, it is necessary to select the optimal combination by including alloying elements such as Si and Mn in the solid wire to be combined and by taking into consideration the chemical components of the flux and solid wire.
[0004] Considering these points, various technological developments have been made so far regarding submerged arc welding methods for high tensile steels that can provide good welding workability and weld metal mechanical properties.
[0005] For example, Patent Document 1 discloses a bond flux and wire for submerged arc welding that can obtain a weld metal having high strength and excellent low-temperature toughness down to -60°C by optimizing the components of the bond flux and wire. However, the bond flux described in Patent Document 1 is CaF 2 Since only a small amount of Si is added, the basicity of the slag is low, and the Si and Ti contents in the solid wire are not adequate, so there was a problem that a weld metal with stable low-temperature toughness could not be obtained at temperatures above -60°C.
[0006] Patent Document 2 discloses a weld metal that has high strength and excellent toughness down to -20°C by optimizing the composition of the weld metal obtained by combining a solid wire and a bond flux. However, the CaF 2 However, since the Si and Ti contents of the solid wire are not appropriate, there has been a problem that a weld metal having good low-temperature toughness at temperatures of -60°C or higher cannot be obtained.
[0007] Furthermore, Patent Document 3 discloses a weld metal that has excellent toughness down to -30°C in both as-welded and PWHT by specifying the components of the bond flux and the carbon equivalent of the solid wire in a submerged arc welding method for high-tensile steel. However, since the Ni and Ti of the solid wire described in Patent Document 3 are not appropriate, there is a problem that a weld metal having good low-temperature toughness at -60°C or higher cannot be obtained.
[0008] Furthermore, Patent Document 4 discloses a technology for submerged arc welding of high tensile steel, in which the composition of the bond flux is optimized and the Si content of the solid wire is reduced to bring the carbon equivalent into an appropriate range, thereby obtaining a weld metal having high strength and good low-temperature toughness. However, the bond flux described in Patent Document 4 contains CaF2 Since the Si content in the wire is low, the oxygen content in the weld metal is high, and there was a problem that good and stable low-temperature toughness could not be obtained even at -60°C. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2013-39604 A [Patent Document 2] JP 2007-260696 A [Patent Document 3] Japanese Patent Application Publication No. 8-257789 [Patent Document 4] Japanese Patent Application Publication No. 5-212583 Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been devised in view of the above-mentioned problems, and an object of the present invention is to provide a submerged arc welding method for 780 MPa class high tensile steel, which can obtain stable weld metal strength and low temperature toughness, has a low diffusible hydrogen content in the weld metal, is free of welding defects, and has good welding workability. [Means for solving the problem]
[0011] The gist of the present invention is a method for submerged arc welding of high tensile steel, comprising the steps of: 2 :5~20%, CaO:5~20%, MgO:25~35%, Al 2 O 3 : 10-20%, CaF 2 : 23-35%, CaCO 3 and MgCO 3 CO 2 Conversion value: 2-7%, Si: 0.3-2.0%, Na 2 O and K 2 Total of one or more of O: 1 to 5%, TiO2 The present invention relates to a submerged arc welding method for high tensile steel, comprising the steps of: combining and welding a bond flux containing, in mass % relative to the total mass of the solid wire, 0.08-0.15% C, 0.1-0.3% Si, 1.5-2.5% Mn, 2.0-3.0% Ni, 0.5-1.5% Mo, 0.02-0.08% Ti, 0.05% or less Al, 0.015% or less P, and 0.015% or less S, with the balance being Fe, Cu from the copper plating on the wire surface, and unavoidable impurities. Effect of the Invention
[0012] According to the submerged arc welding method for high tensile steel to which the present invention is applied, stable strength and low temperature toughness of the weld metal can be obtained, and the amount of diffusible hydrogen in the weld metal is low, there are no welding defects, and welding workability is obtained, making it possible to provide a high-quality weld with high efficiency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] In order to solve the above-mentioned problems in performing submerged arc welding of 780 MPa class high tensile steel, the inventors have produced and examined various chemical compositions of bonded flux for submerged arc welding (hereinafter referred to as bonded flux) and the chemical components of solid wires to be combined with the bonded flux. As a result, it was found that the CaO, MgO, CaF 2 It was discovered that by adding an appropriate amount of Si to increase the basicity of the slag, and by combining it with a solid wire containing C, Si, Mn, Ni, Mo, and Ti in appropriate ranges, the strength and oxygen content of the weld metal can be optimized, resulting in stable low-temperature toughness. It was also discovered that the amount of diffusible hydrogen can be reduced by optimizing the amount of metal carbonate in the flux. Furthermore, Na is important for arc stability. 2 O and K 2 O and Al 2 O 3 Optimization of the amount of SiO for slag removal 2 It has been found that the welding workability of these materials can be improved by adding an appropriate amount of
[0014] First, the reasons for limiting the composition of the bonded flux used in the submerged arc welding method according to the present invention will be described below. In the following, the percentage of each component indicates the mass percentage relative to the total mass of the bonded flux.
[0015] [SiO 2 :5~20%] SiO 2 SiO is an important component for adjusting the viscosity of the slag and forming a good weld bead. 2 By adding SiO, the slag becomes vitreous, resulting in a slag that is easy to break and has good peelability. 2 If the content of SiO is less than 5%, the slag removability is deteriorated and undercuts are likely to occur. 2 If SiO exceeds 20%, the oxygen content of the weld metal increases and the low-temperature toughness deteriorates. 2 The content of SiO is 5 to 20%. 2 can be added from raw materials such as silica sand, water glass, etc.
[0016] [CaO: 5-20%] CaO has the effect of improving low-temperature toughness by increasing the basicity of the slag and reducing the oxygen content of the weld metal. If the CaO content is less than 5%, this effect is not obtained and the low-temperature toughness of the weld metal decreases. On the other hand, if the CaO content exceeds 20%, the basicity of the slag increases, the arc becomes unstable, and the slag removability deteriorates. Therefore, the CaO content is set to 5 to 20%. CaO can be added from raw materials such as wollastonite and calcium oxide.
[0017] [MgO: 25~35%] MgO has the effect of improving low-temperature toughness by increasing the basicity of the slag and reducing the oxygen content of the weld metal. If the MgO content is less than 25%, this effect cannot be obtained, and the low-temperature toughness of the weld metal deteriorates. On the other hand, if the MgO content exceeds 35%, the melting point of the slag increases, slag removability and bead appearance deteriorate, and welding defects such as slag inclusion become more likely to occur. Therefore, the MgO content is set to 25 to 35%. Note that MgO can be added from magnesia clinker or the like as a raw material.
[0018] [Al 2 O 3 :10~20%] Al 2 O 3 Al acts as a slag former and also has the effect of improving the arc stability. 2 O 3 If the content of Al is less than 10%, the arc becomes unstable, and the slag removability and bead appearance deteriorate. 2 O 3 If Al exceeds 20%, the oxygen content of the weld metal increases, and the low-temperature toughness of the weld metal deteriorates. 2 O 3 The content of Al is 10 to 20%. 2 O 3 can be added from a raw material such as alumina.
[0019] [CaF 2 :23~35%] CaF 2 CaF has the effect of improving low-temperature toughness by increasing the basicity of the slag and reducing the oxygen content of the weld metal. 2 If the content of CaF is less than 23%, this effect cannot be obtained and the low temperature toughness of the weld metal decreases. 2 If the content of CaF exceeds 35%, the arc becomes unstable, and the slag removability and bead appearance deteriorate. 2 The content is 23 to 35%. 2 can be added from a raw material such as fluorite.
[0020] [CaCO 3 and MgCO 3CO 2 Conversion rate: 2~7% CaCO 3 or MgCO 3 CO from 2 The conversion value is CaCO 3 or MgCO 3 is decomposed to CO or CO 2 The gas reduces the hydrogen partial pressure in the arc atmosphere, which has the effect of reducing the amount of diffusible hydrogen in the weld metal. CaCO 3 and MgCO 3 CO 2 If the conversion value is less than 2%, the effect of reducing the amount of diffusible hydrogen cannot be obtained. 3 and MgCO 3 CO 2 If the converted value exceeds 7%, pockmarks are likely to occur on the bead surface, and the oxygen content of the weld metal increases, deteriorating the low-temperature toughness of the weld metal. 3 and MgCO 3 CO 2 The conversion value shall be 2 to 7%.
[0021] [Si: 0.3-2.0%] Silicon is a deoxidizing element and has the effect of improving the bead appearance by reducing the amount of oxygen in the weld metal. If the silicon content is less than 0.3%, the deoxidizing effect is not obtained and pockmarks are likely to occur on the bead surface. On the other hand, if the silicon content exceeds 2.0%, the strength of the weld metal increases and the low-temperature toughness deteriorates. Therefore, the silicon content is set to 0.3 to 2.0%. Silicon can be added from raw materials such as metal silicon, Fe-Si, and Fe-Si-Mn.
[0022] [Na 2 O and K 2 O 1 or 2 types in total: 1-5%] Na 2 O and K 2 O has the effect of improving the stability of the arc. 2 O and K 2 If the total of one or both types of O is less than 1%, this effect cannot be obtained and the arc becomes unstable.2 O and K 2 If the total of one or both of the O elements exceeds 5%, pockmarks are likely to occur and the bead appearance deteriorates. 2 O and K 2 The total of one or two types of O is 1 to 5%. 2 O and K 2 O can be added from raw materials such as sodium carbonate and potassium carbonate.
[0023] [TiO 2 :0.1% or less] TiO 2 Since TiO deteriorates the slag removability, it is desirable to avoid its inclusion as much as possible. 2 If TiO exceeds 0.1%, the deterioration of slag removability becomes significant. 2 The content of TiO is 0.1% or less. 2 is added from calcium titanate, ilmenite, etc.
[0024] The remainder of the bond flux other than the above-mentioned components is the Fe content from the iron alloy, and unavoidable impurities such as MnO, P, and S. Both P and S form compounds with low melting points and reduce toughness, so it is preferable that the content be as low as possible.
[0025] Next, the components of the solid wire to be combined with the bond flux will be described. In the following, the percentage of each component indicates the mass percentage relative to the total mass of the solid wire.
[0026] [C:0.08~0.15%] C is an important element that ensures the strength of the weld metal through solid solution strengthening, and also has the effect of improving low-temperature toughness by reacting with oxygen in the arc to reduce the amount of oxygen in the arc atmosphere and weld metal. If C is less than 0.08%, the deoxidizing effect is not obtained, pockmarks are likely to occur, and the low-temperature toughness of the weld metal is also reduced. On the other hand, if C exceeds 0.15%, the strength of the weld metal becomes excessively high and the low-temperature toughness is deteriorated. Therefore, C is set to 0.08 to 0.15%.
[0027] [Si: 0.1-0.3%] Silicon has the effect of reducing the oxygen content in the weld metal and improving the bead appearance and low-temperature toughness. If the silicon content is less than 0.1%, the deoxidizing effect is not obtained and the low-temperature toughness of the weld metal decreases. On the other hand, if the silicon content exceeds 0.3%, the matrix of the weld metal is solid-solution strengthened, but the grains become coarse, resulting in a significant decrease in low-temperature toughness. Therefore, the silicon content is set to 0.1 to 0.3%.
[0028] [Mn: 1.5-2.5%] Mn has the effect of improving the strength of the weld metal. If the Mn content is less than 1.5%, this effect is not obtained and the strength of the weld metal decreases. On the other hand, if the Mn content exceeds 2.5%, the strength of the weld metal becomes excessively high and the low-temperature toughness deteriorates. Therefore, the Mn content is set to 1.5 to 2.5%.
[0029] [Ni: 2.0~3.0%] Ni has the effect of stabilizing the low-temperature toughness of the weld metal. If Ni is less than 2.0%, this effect is not obtained and the low-temperature toughness of the weld metal decreases. On the other hand, if Ni exceeds 3.0%, the austenite grain size of the weld metal becomes coarse, decreasing the low-temperature toughness. Therefore, Ni is set to 2.0 to 3.0%.
[0030] [Mo: 0.5-1.5%] Mo has the effect of improving the strength of the weld metal. If Mo is less than 0.5%, this effect is not obtained and the strength of the weld metal decreases. On the other hand, if Mo exceeds 1.5%, an intermetallic compound is generated in the weld metal, which makes the strength of the weld metal excessively high and reduces the low-temperature toughness. Therefore, Mo is set to 0.5 to 1.5%.
[0031] [Ti: 0.02~0.08%] Ti has the effect of improving low-temperature toughness by reacting with oxygen in the arc and reducing the amount of oxygen in the arc atmosphere and weld metal. If Ti is less than 0.02%, this effect is not obtained and the low-temperature toughness of the weld metal decreases. On the other hand, if Ti exceeds 0.08%, the amount of solid-solubilized Ti in the weld metal increases, decreasing the low-temperature toughness. Therefore, Ti is set to 0.02 to 0.08%.
[0032] [Al: 0.05% or less, P: 0.015% or less, S: 0.015% or less] It is desirable to minimize the content of Al, P, and S, since they all form compounds with low melting points and reduce low-temperature toughness. Therefore, the content of Al is limited to 0.05% or less, P to 0.015% or less, and S to 0.015% or less.
[0033] The remainder of the solid wire other than the above-mentioned components is Fe, Cu from the copper plating on the wire surface, and unavoidable impurities such as W, V, P, and S. Both P and S form compounds with low melting points and reduce toughness, so it is preferable that their contents are as low as possible. EXAMPLES
[0034] The effects of the present invention will now be described in more detail with reference to examples.
[0035] Bond fluxes with the various compositions shown in Table 1 and solid wires shown in Table 2 were prototyped, and these were combined to evaluate the welding workability and mechanical performance. 780 MPa class steel plate with a thickness of 25 mm and the chemical composition shown in Table 3 was machined into a groove shape with a groove angle of 30° and a root spacing of 13 mm. A backing metal was applied and a multi-layer welding test was performed under the welding conditions shown in Table 4.
[0036] The bond flux shown in Table 1 was made by compounding and mixing various mineral raw materials, granulating them with water glass as a binder, and then sintering them at 400 to 550°C for 2 hours to granulate them to 1.4 x 0.15 mm. The wires shown in Table 2 were made by reducing, annealing, and plating the original wires to make strands, which were then drawn to a diameter of 4.0 mm.
[0037] [Table 1]
[0038] [Table 2]
[0039] [Table 3]
[0040] [Table 4]
[0041] The combinations of various prototype bond fluxes and various prototype solid wires are shown in Table 5. The evaluation of each test was carried out by investigating the arc stability during multi-pass welding, bead appearance, slag removability, and the presence or absence of welding defects by X-ray examination, and also by investigating the mechanical performance of the weld metal.
[0042] (Arc Stability) The welding voltage was judged to be stable when it was constant and had little fluctuation during welding.
[0043] (Bead appearance) Bead width, excess height, waviness and surface condition were uniform and there were no undercuts or pockmarks, etc., and the weld was rated as good.
[0044] (Slag removability) After welding, the condition was judged to be good if the slag naturally peeled off or if, when the solidified slag was struck with a chipping hammer, the slag cracked and could then be easily removed.
[0045] (Welding defects) In the X-ray test, the test was conducted based on the radiographic test for steel welded joints shown in JIS Z 3104:1995, and cases where no slag inclusion or the like occurred were regarded as non-existent.
[0046] (Machine performance evaluation) The mechanical performance of the weld metal was evaluated by mechanical testing tensile test pieces and impact test pieces taken in accordance with AWS A5.23. For the tensile test, a tensile strength of 780MPa to 880MPa was considered good. For the impact test, a Charpy impact test was performed at -74°C, and an average of 80J or more for three out of five repetitions, excluding the minimum and maximum values, was considered good. The amount of diffusible hydrogen in the weld metal was measured in accordance with JIS Z3118:2007. A diffusible hydrogen amount in the weld metal of 5ml / 100g or less was considered good. The results of these investigations are also summarized in Table 5.
[0047] [Table 5]
[0048] In Table 5, test codes T1 to T16 are examples of the present invention, and test codes T17 to T38 are comparative examples. In the test codes T1 to T16, which are examples of the present invention, the flux codes F1 to F16 and the combined wire codes W1 to W14 satisfy the constituent requirements of the present invention, so the arc was stable, and welding workability such as bead appearance and slag removability was good, there were no welding defects, the tensile strength and absorbed energy of the weld metal were good, and the amount of diffusible hydrogen in the weld metal was low, resulting in extremely satisfactory results.
[0049] In the comparative example, the test code T17 is SiO with the flux code F17. 2 The amount of Mo in the wire W15 was so small that the slag removability was poor and undercut occurred. Also, the amount of Mo in the wire W15 was so large that the tensile strength of the weld metal was high and the absorbed energy was low.
[0050] Test code T18 is SiO with flux code F18 2 Therefore, the absorbed energy of the weld metal was low.
[0051] Test code T19 had a low CaO content in the flux code F19, so the absorbed energy of the weld metal was low.
[0052] Test code T20 had an unstable arc and poor slag removability due to the flux code F20 containing a large amount of CaO. Also, wire code W16 contained a small amount of C, which caused pockmarks to form and the absorbed energy of the deposited metal to be low.
[0053] Test code T21 has a low MgO content compared to flux code F21, so the absorbed energy of the weld metal was low. 2 O and K 2 Pockmarks occurred because there was a high total of one or two types of O.
[0054] Test code T22 is Al with flux code F22 2 O 3 The arc was unstable, and the slag removability and bead appearance were poor. Also, the wire W17 had a low amount of silicon, so the absorbed energy of the weld metal was low.
[0055] Test code T23 is Al with flux code F23 2 O 3 The absorbed energy of the weld metal was low because of the large amount of Mn in the wire W18. Also, the tensile strength of the weld metal was low because of the small amount of Mn in the wire W18.
[0056] Test code T24 is CaF with flux code F24 2 The absorbed energy of the weld metal was low because of the low Na content. 2 O and K 2 The arc was unstable because the total of one or two types of O was low.
[0057] Test code T25 is CaF with flux code F25 2 The arc was unstable, and the slag removability and bead appearance were poor. Also, the wire W19 had a high Mn content, so the tensile strength of the weld metal was high and the absorbed energy was low.
[0058] Test code T26 contains a lot of MgO in flux code F26, which resulted in poor slag removability and poor bead appearance, and slag inclusion in the weld metal. 3 and MgCO 3 CO 2 The converted value was low, so the amount of diffusible hydrogen in the weld metal was high. Furthermore, the amount of Mo in the wire symbol W20 was low, so the tensile strength of the weld metal was low.
[0059] Test code T27 is CaCO with flux code F27 3 and MgCO 3 CO 2 Because the conversion value was high, pockmarks occurred and the absorbed energy of the weld metal was low.
[0060] Test code T28 had pockmarks due to the flux code F28 having a low Si content, and wire code W21 had a high C content, resulting in high tensile strength of the weld metal and low absorbed energy.
[0061] Test code T29 had a high Si content in wire code W22, so the absorbed energy of the weld metal was low.
[0062] The test code T30 had a low absorbed energy in the weld metal because the wire code W23 contained less Ni.
[0063] Test code T31 had a low absorbed energy in the weld metal because the wire code W24 contained a large amount of Ni.
[0064] Test code T32 has a high Si content in flux code F29, so the tensile strength of the weld metal was high and the absorbed energy was low.
[0065] Test code T33 had a high Ti content in wire code W25, so the absorbed energy of the weld metal was low.
[0066] The test code T34 had a low Ti content compared to the wire code W26, so the absorbed energy of the weld metal was low.
[0067] Test code T35 is TiO with flux code F30 2 The amount of slag was so large that the slag removability was poor.
[0068] Test code T36 had a low absorbed energy in the weld metal of wire code W27, which contained a large amount of Al.
[0069] Test code T37 had a low absorbed energy in the weld metal due to the high P content of wire code W28.
[0070] Test code T38 had a low absorbed energy in the weld metal due to the high S content of wire code W29.
Claims
[Claim 1] In a submerged arc welding method for high tensile steel, the method comprises, in mass % based on the total mass of the bond flux for submerged arc welding, Yes 2 :5~20%、 CaO: 5-20%, MgO: 25-35%, <h2 style=";text-align:left;direction:ltr">Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> :15~250%、 CaF 2 :23~35%、 CaCO 3 and MgCO 3 One or two of the following CO 2 Conversion rate: 2-7%, Si: 0.3-2.0%, Na 2 O and K 2 One or more of O in total: 1 to 5%; TiO 2 : 0.1% or less, The balance is a bond flux for submerged arc welding, which is composed of Fe from the iron alloy and inevitable impurities; Mass % relative to the total mass of the solid wire C: 0.08-0.15%, Si: 0.1 to 0.3%, Mn: 1.5-2.5%, Ni: 2.0 to 3.0%, Mo: 0.5-1.5%, Ti: 0.02 to 0.08%; Al: 0.05% or less, P: 0.015% or less, S: 0.015% or less; A submerged arc welding method for high tensile steel, comprising welding in combination with a solid wire consisting essentially of Fe, Cu from the copper plating on the wire surface, and unavoidable impurities.
Citation Information
Patent Citations
Submerged arc welding
JP1996257789A
Electroslag welding method
JP2005246398A
SUBMERGED ARC WELD METAL FOR 1.25%Cr-0.5%Mo STEEL, COKE DRUM AND BONDED FLUX
JP2010110819A
Bonded flux and solid wire for submerged arc welding, and method for submerged arc welding of steel for low temperature service
JP2012176435A
Welded metal superior in hydrogen embrittlement resistance sensitivity
JP2014133258A