Method for producing porous ceramic
The method addresses non-uniform pore formation and physical property issues in porous ceramics by a calcination, pulverization, classification, and firing process, resulting in controlled pore size and improved strength.
Patent Information
- Application Number
- JP2023051944
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Existing methods for manufacturing porous ceramics face challenges in controlling pore size and ratio, leading to non-uniform pore formation, poor dispersibility of pore-forming agents, and adverse effects on physical properties such as strength and chemical resistance.
A method involving a calcination process to remove moisture and organic impurities, followed by pulverization, classification, forming, and main firing to control pore size and ratio, using ceramic raw materials with optional organic binders to enhance strength and shape.
Achieves a porous structure with excellent physical properties and controlled pore size and ratio, improving strength and reducing manufacturing costs through simplified processes using existing ceramic equipment.
Smart Images

Figure 2024140673000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing porous ceramics. More specifically, the present invention relates to a method for producing porous ceramics that is simple, yet capable of producing a porous structure with excellent physical properties, and that allows control of the size and ratio of pores between raw material particles. [Background technology]
[0002] In recent years, various products have been developed that take advantage of the excellent functions of porous materials.
[0003] The functions of porous materials include, for example, low specific gravity and light weight, thermal insulation, sound absorption and sound deadening, substance retention and adsorption, large specific surface area, selective separation of substances, and adjustment of the passage of substances.
[0004] In addition, applications based on their various functions include building materials, insulating bricks, sound-absorbing materials for buildings and roads, humidity-regulating tiles, catalyst carriers used in the chemical industry, adsorbents for water and air purification, and molecular sieve materials for substance purification or chromatography, and the like, allowing for a wide range of uses.
[0005] In the field of ceramics, too, there is technology to manufacture porous ceramics, and products are being made that take advantage of the properties of porcelain porcelain.
[0006] Here, for example, one technique for producing porous ceramics has been proposed in which an organic pore-forming agent is added to the raw materials to produce porous ceramics (see, for example, Patent Document 1).
[0007] In the method of adding an organic pore-forming agent, the pore-forming agent disappears upon firing, and pores are formed in the places where the pore-forming agent was previously present, resulting in a porous ceramic.
[0008] Another method for producing porous ceramics is to add glass to already sintered raw materials such as ceramic ware, and then fire the material. In this method, the molten glass acts as a binder, and the areas where the particles of the sintered raw materials are not bonded together become pores between the particles, producing porous ceramics. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Publication No. 64-87584 Summary of the Invention [Problem to be solved by the invention]
[0010] Here, in the method using an organic pore-forming agent, including that described in Patent Document 1, various pore-forming agents are commercially available, but the size of the pores formed depends on the raw material, and it is difficult to control the desired pore size and pore ratio.
[0011] Furthermore, even when attempts were made to control the pores by mixing multiple pore-forming agents, the pores could not be formed well, or areas with a high concentration of pores and areas without any pores were mixed, making it impossible to form pores uniformly in the ceramic.
[0012] In addition, there are problems such as poor dispersibility of the pore-forming agent, which does not mix with the raw material and results in poor quality, organic matter remaining as a black residue that adversely affects the appearance, and when cellulose is used as the pore-forming agent, a bad odor is emitted when heated.
[0013] Furthermore, in the manufacturing method in which glass is added, the glass causes defects in the physical properties of the porous ceramic, such as a decrease in strength of the glass-containing parts, a decrease in heat resistance, and a decrease in chemical resistance, such as dissolution when exposed to strong alkali.
[0014] However, if porous materials could be produced using ceramic manufacturing techniques that have been accumulated over many years, it would be possible to develop multifunctional and useful products using ceramic raw materials and manufacturing equipment, so there is a desire to utilize ceramic manufacturing techniques.
[0015] The present invention has been devised in consideration of the above points, and aims to provide a method for producing porous ceramics which is simple yet produces a porous structure with excellent physical properties and enables control of the size and proportion of pores between raw material particles. [Means for solving the problem]
[0016] In order to achieve the above-mentioned object, the manufacturing method of porous ceramics of the present invention comprises a calcination process in which ceramic raw materials are heated and baked to a state before sintering is completed, a crushing process in which the product produced through the calcination process is crushed to obtain raw material particles with different particle sizes, a classification process in which the raw material particles are divided into a plurality of sections according to particle size, a molding process in which at least one section is selected from the plurality of sections and the raw material particles of the selected section are molded, and a main firing process in which the molded product that has undergone the molding process is heated at a temperature higher than the heating temperature of the calcination to complete sintering.
[0017] In addition, the expression "▲ka▼" in this specification and claims is actually an external character that is not included in JIS Level 1 and Level 2, and is the character shown in the external character below. Also, the external character for the expression "▲ka▼" is a character whose on-reading in Japanese is "ka" or "ke".
[0018] (External characters) TIFF2024140673000002.tif4346
[0019] In the calcination process, the ceramic raw materials are heated and baked to a state before sintering is completed, which removes moisture and impurities derived from organic matter in the ceramic raw materials, and the ceramic raw materials are baked to harden them, forming a bulk product that can improve its strength. In addition, the improved strength makes it possible to obtain a particle group (powder) in the subsequent crushing process that contains a mixture of raw material particles of various particle sizes in an agglomerate structure formed by the aggregation of primary particles of multiple ceramic raw materials.
[0020] On the other hand, if the calcination process is not performed, the ceramic raw material will remain at a low strength, and the granular structure formed by the aggregation of multiple primary particles of the ceramic raw material will not be able to be maintained. Even if the subsequent crushing process is performed, only raw material particles with a fine particle size similar to that of the original ceramic raw material will be obtained, and a particle group (powder) containing a mixture of raw material particles of various particle sizes will not be obtained.
[0021] The state before sintering is completed here means the state before the raw material particles are heated at a temperature lower than the melting point, the raw material particles bond together, the gaps between the particles become smaller, and the whole shrinks and solidifies into a dense object. Before sintering is completed, the density is low, and after sintering, the density increases. Also, before sintering is completed, there are pores in the raw material particle structure, but after sintering is completed, the material is sintered and the pores in the raw material particle structure almost disappear, and pores are formed between the raw material particles.
[0022] In addition, in the pulverization process, the product produced through the calcination process is pulverized to obtain raw material particles with different particle sizes, thereby obtaining a particle group (powder) containing raw material particles with a variety of particle sizes. In other words, the calcined bulk product is crushed to obtain a powdered raw material particle group with a wide particle size distribution.
[0023] In addition, by dividing the raw material particles into multiple compartments according to particle size in the classification process, the raw material particle group, which is a mixture of particles with various particle sizes, can be aligned according to the target particle size within a certain range.
[0024] In addition, in the molding process, at least one section is selected from the multiple sections, and the raw material particles in the selected section are molded, so that raw material particles in a desired particle size range can be adjusted to the shape of the final product. That is, the shape of the porous ceramic can be formed according to the application or shape of the final product.
[0025] In the main firing process, the molded product that has been through the molding process is heated at a temperature higher than the heating temperature of the calcination process to complete the sintering, and the contact points between the raw material particles in the molded product are bonded by sintering, resulting in a lumpy fired product. In addition, between the raw material particles, pores of a size corresponding to the particle size of the raw material particles in the section selected in the molding process can be formed. In other words, by heating at a temperature higher than the heating temperature of the calcination process, the molded product can be sufficiently sintered to promote sintering. In this main firing process, the contact points between the adjacent raw material particles gradually bond, the gaps between the raw material particles become smaller, and at the same time, the entire product shrinks, forming a hard final product. The gaps here are the pores between the final raw material particles, that is, the main pores of the porous ceramics.
[0026] In addition, when the heating temperature for calcination is 300°C or higher and 1000°C or lower, it is possible to calcinate various types of ceramic raw materials to produce bulk products and improve their strength so that they can withstand the subsequent crushing and classification processes.
[0027] On the other hand, if the calcination temperature is less than 300 degrees, the removal of moisture and organic impurities from the raw materials may be insufficient, and the strength of the ceramic raw materials may not be improved sufficiently. As a result, the ceramic raw materials may not have a strength sufficient to withstand the subsequent crushing process, and a particle group (powder) containing raw material particles of various particle sizes may not be obtained in the crushing process. Also, if the calcination temperature is more than 1000 degrees, sintering may be completed even for ceramic raw materials with a relatively high appropriate firing temperature, and the raw material particles may not be able to be used in the subsequent crushing process and subsequent processes.
[0028] In addition, when the ceramic raw material is one selected from the group consisting of porcelain raw material, pottery raw material, and fine ceramics, or a combination of one selected from the group consisting of porcelain raw material, pottery raw material, and fine ceramics with an organic binder, a porous ceramic can be formed that is composed of a single structure of any one of the raw materials, porcelain raw material, pottery raw material, or fine ceramics. Note that the organic binder is an auxiliary agent that binds raw material particles together, and by adding it, plasticity and shape retention can be imparted or improved, but it is fired in the main firing process, and after the main firing process, the porous ceramic is composed only of a structure derived from any one of the raw materials, porcelain raw material, pottery raw material, or fine ceramics.
[0029] In addition, in the molding process, when two or more sections are selected from a plurality of sections and the raw material particles of the selected sections are molded, raw material particles of a plurality of particle size ranges can be combined to diversify the size of the pores that are finally formed and the combination of the sizes of the plurality of pores. In addition, when raw material particles of a plurality of particle size ranges are combined, the ratio of the pores formed can be adjusted by adjusting the blending amount of each section. That is, for example, in the case of only a single section, only pores of a size corresponding to the particle size range of that section are formed, but by combining particle size ranges of a plurality of sections, the size of the pores formed changes, and the variation in the size of the pores can be increased.
[0030] Furthermore, when the formed body that has undergone the firing process is formed only from the structure derived from the ceramic raw material, the strength, heat resistance, or chemical resistance according to the type of ceramic raw material can be imparted to the porous ceramic. Also, since the types of raw materials are simplified, the manufacturing cost can be reduced.
[0031] In addition, when the ceramic raw material is a porcelain raw material or a combination of a porcelain raw material and an organic binder, and the heating temperature for calcination is 500 degrees or higher and 900 degrees or lower, impurities such as moisture and organic matter in the raw material are efficiently removed while maintaining the porcelain raw material in a state before sintering is completed, making it possible to improve the strength.
[0032] Furthermore, when the ceramic raw materials are pottery raw materials or a combination of pottery raw materials and an organic binder, and the heating temperature for calcination is between 400°C and 800°C, impurities such as moisture and organic matter in the raw materials can be efficiently removed while maintaining the pottery raw materials in a state before sintering is completed, thereby making it possible to improve strength.
[0033] In addition, when the ceramic raw materials are fine ceramics or a combination of fine ceramics and an organic binder, and the heating temperature for calcination is between 900°C and 1000°C, impurities such as moisture and organic matter in the raw materials are efficiently removed while keeping the fine ceramics in the state before sintering is completed, making it possible to improve the strength. Effect of the Invention
[0034] The method for manufacturing porous ceramics according to the present invention is a simple method that can produce porous structures with excellent physical properties and that can control the size and proportion of pores between raw material particles. [Brief description of the drawings]
[0035] [Figure 1]1 is a schematic process diagram showing the flow of each step in a manufacturing method according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a photograph showing the appearance of the molded body of Example 1. [Diagram 3] FIG. 2 is a photograph showing an enlarged image of the molded body of Example 1 taken with a digital microscope. [Figure 4] FIG. 4 is a photograph showing the appearance of the molded body of Example 2. [Diagram 5] FIG. 1 is a photograph showing the appearance of the molded body of Example 3. [Figure 6] FIG. 1 is a photograph showing the appearance of the molded body of Example 4. [Figure 7] FIG. 11 is a photograph showing the appearance of the molded body of Example 5. [Figure 8] FIG. 11 is a photograph showing the appearance of the molded body of Example 6. [Figure 9] FIG. 11 is a photograph showing the appearance of the molded body of Example 7. [Figure 10] FIG. 1 is a photograph showing the results of a comparative alkali resistance test of Example 8 and Comparative Example 1. [Figure 11] 1 is a graph showing the results of pore size distribution measurement by mercury porosimetry. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0036] An example of a method for producing porous ceramic ware to which the present invention is applied (an embodiment of the present invention) will be described below.
[0037] [Embodiment Mode] As shown in FIG. 1, manufacturing method A according to an embodiment of the present invention includes a calcination step (S1), a pulverization step (S2), a classification step (S3), a molding step (S4), and a main sintering step (S5).
[0038] Here, manufacturing method A is a method for manufacturing porous ceramics with pores of a desired size and ratio from various ceramic raw materials. Furthermore, manufacturing method A is a method that can form pores with a higher porosity than porous ceramics manufactured by conventional methods that use organic pore-forming agents.
[0039] The calcination step (reference symbol S1) is a step in which the ceramic raw material is heated and baked to a state before sintering is completed.
[0040] By carrying out this calcination process (reference symbol S1), the moisture in the ceramic raw material is removed, and the impurities derived from organic matter in the ceramic raw material are also removed. In addition, by removing the moisture and impurities from the ceramic raw material, the ceramic raw material is slightly fired and the strength can be improved.
[0041] The pulverization step (reference symbol S2) is a step of pulverizing the raw material aggregate (bulk raw material) that has been lightly sintered and compacted through the calcination step (reference symbol S1).
[0042] By carrying out this crushing step (symbol S2), the bulk ceramic raw material produced in the calcination step (symbol S1) can be crushed to obtain a raw material particle group containing a mixture of raw material particles of various particle sizes.
[0043] The classification step (reference symbol S3) is a step of fractionating the raw material particle group obtained in the pulverization step (reference symbol S2), which is a mixture of raw material particles of various particle sizes, into a certain range of sizes using a sieve or the like.
[0044] By carrying out this classification step (reference symbol S3), a group of raw material particles having various particle sizes can be aligned according to the target particle size within a certain range.
[0045] The molding process (symbol S4) is a process of selecting a section of raw material particles in which pores of the desired size can be formed from the multiple sections of raw material particles that have undergone the classification process (symbol S3), and shaping the raw material particles into the shape of the final product.
[0046] By carrying out this molding step (reference symbol S4), it is possible to form a porous structure according to the application and shape of the final product.
[0047] The sintering process (S5) is a process in which the porous structure formed in the molding process (S4) is heated at a temperature higher than that in the calcination process (S1) and lower than the melting point to complete the sintering and bond the raw material particles at their contact points to form a rice-cake-like object.
[0048] By carrying out this final firing step (reference symbol S5), the molded product is sufficiently fired and sintered to form a hard final product, i.e., porous ceramics, with pores of the desired size formed between the raw material particles.
[0049] In addition, in the manufacturing method A, a porcelain raw material, a pottery raw material, or a fine ceramic can be used as the ceramic raw material. In addition, the ceramic raw material can be a raw material in which a porcelain raw material, a pottery raw material, or a fine ceramic is combined with an organic binder.
[0050] The porcelain raw materials may be mainly made of pottery stone mined in each production area, and examples include Amakusa pottery clay, Tobe pottery clay, etc. The porcelain raw materials may be blended pottery clay, and examples include pottery clay (porcelain clay) uniquely blended in each production area, Mino porcelain clay, Seto porcelain clay, various types of ▲Sessyo clay, heat-resistant pottery clay (cordierite), and reinforced porcelain clay.
[0051] As the pottery raw materials, for example, china clay such as white clay, red clay, black clay, etc., which are mined and prepared in each production area, and heat-resistant china clay (petalite, chamotte), etc. can be used.
[0052] Moreover, as the fine ceramics, for example, alumina ceramics and the like can be adopted.
[0053] In addition, in the manufacturing method A to which the present invention is applied, known ceramic raw materials can be used in addition to the raw materials listed above.
[0054] In the calcination step (reference symbol S1), the ceramic raw material is preferably heated at a temperature of 300 degrees or more and 1000 degrees or less.
[0055] If the heating temperature in the calcination step (reference symbol S1) is less than 300 degrees, the removal of moisture and organic impurities in the raw materials will be insufficient, the ceramic raw materials will not be densified sufficiently, and the strength may not be improved sufficiently. As a result, the raw material aggregate will not have enough strength in the next crushing step (reference symbol S2), and only raw material particles with a relatively small particle size will be obtained after crushing.
[0056] Furthermore, if the heating temperature in the calcination process (symbol S1) exceeds 1000 degrees, there is a risk that sintering will be completed even if the ceramic raw material has a relatively high appropriate firing temperature, and the raw material particles will not be able to be subjected to the subsequent crushing process (symbol S2) and subsequent processes.
[0057] In the calcination step (reference symbol S1), it is more preferable to set the heating temperature as follows according to the type of ceramic raw material.
[0058] For example, for porcelain raw materials, it is more preferable that the heating temperature in the calcination step (symbol S1) be set to a temperature of 500° C. or more and 900° C. or less. For earthenware raw materials, it is more preferable that the heating temperature in the calcination step (symbol S1) be set to a temperature of 400° C. or more and 800° C. or less. For fine ceramics, it is more preferable that the heating temperature in the calcination step (symbol S1) be set to a temperature of 900° C. or more and 1000° C. or less.
[0059] In this way, by setting the heating temperature in the calcination process (symbol S1) to a more preferable temperature depending on the type of ceramic raw material, it is possible to efficiently remove impurities such as moisture and organic matter in the raw materials while maintaining the state before sintering is completed, thereby improving strength.
[0060] In the pulverizing step (reference symbol S2), a dry or wet pulverizing method can be used.
[0061] In the pulverization step (reference symbol S2), for example, a jaw crusher (coarse pulverization), a roll crusher (medium pulverization), and a stamp mill (coarse to fine pulverization) can be used if it is a dry process, and for example, a ball mill (thoron mill) (fine pulverization) can be used if it is a wet process.
[0062] In addition, in the manufacturing method A to which the present invention is applied, in addition to the methods listed above, known crushing techniques can be used as appropriate depending on the type of ceramic raw material and the size and proportion of the pores to be formed.
[0063] In the classification step (reference symbol S3), a dry or wet fractionation method can be used.
[0064] In the classification step (reference symbol S3), for example, a dry method may be used, such as sieving (wire screen, etc.) (large to small particle size), air classification (zigzag classifier, cyclone classifier, vortex classifier, etc.) (small to fine particle size), etc. In addition, for example, a wet method may be used, such as wet sieving (wire screen, etc.) (large to small particle size), elutriation (small to fine particle size), wet cyclone classifier (small to fine particle size), etc.
[0065] In addition, in the manufacturing method A to which the present invention is applied, in addition to the methods listed above, known fractionation methods can be used appropriately according to the type of ceramic raw material and the size and proportion of the pores to be formed.
[0066] In the molding step (reference symbol S4), the following method can be used as an example.
[0067] First, the raw material particles (powder) fractionated in the classification step (reference symbol S3) are packed into a ceramic container such as an alumina container and sintered. In this method, the shape of the resulting molded product depends on the shape of the ceramic container.
[0068] In addition, in the molding process (symbol S4), an organic binder and a small amount of water can be added to the raw material particles (powder) fractionated in the classification process (symbol S3) to make it into a clay-like material, which can then be molded in various ways (by hand, on a potter's wheel, on a mechanical potter's wheel, or in a roller machine).
[0069] In the molding step (reference symbol S4), an organic binder and water may be added to the raw material particles (powder) fractionated in the classification step (reference symbol S3) to make it into a slurry state, and various molding methods (sludge casting, pressure casting) may be used.
[0070] In addition, in the manufacturing method A to which the present invention is applied, in addition to the methods listed above, known molding techniques can be used as appropriate depending on the type of ceramic raw material and the size and proportion of the pores to be formed.
[0071] In the main firing step (reference symbol S5), it is more preferable to set the heating temperature as follows depending on the type of ceramic raw material.
[0072] For example, for porcelain raw materials, it is more preferable that the heating temperature in the firing step (reference symbol S5) is set to a temperature of 1250° C. or more and 1400° C. or less. For pottery raw materials, it is more preferable that the heating temperature in the firing step (reference symbol S5) is set to a temperature of 1200° C. or more and 1350° C. or less. For fine ceramics, it is more preferable that the heating temperature in the firing step (reference symbol S5) is set to a temperature of 1700° C. or more and 1800° C. or less.
[0073] In this way, by setting the heating temperature in the main firing step (symbol S5) to a preferred temperature depending on the type of ceramic raw material, the molded body can be sufficiently fired and sintered to form a hard, porous ceramic with pores of the desired size between the raw material particles.
[0074] The method for manufacturing porous ceramics according to the embodiment of the present invention described above makes it possible to form a porous structure in a simple manner by utilizing existing ceramics manufacturing techniques and equipment.
[0075] Furthermore, in the method for producing porous ceramics according to the embodiment of the present invention, it is possible to control the size and proportion of pores between the raw material particles.
[0076] In addition, since the finally formed porous ceramic is composed only of structures derived from various ceramic raw materials, it is possible to impart strength, heat resistance, or chemical resistance to the porous ceramic according to the type of ceramic raw material. In other words, it is possible to form porous ceramic with excellent physical properties.
[0077] Furthermore, since known raw materials can be used as the types of ceramic raw materials and the types of raw materials are simplified, the manufacturing cost can be reduced.
[0078] As described above, the method for manufacturing porous ceramics to which the present invention is applied is a simple method that can produce porous structures with excellent physical properties and that makes it possible to control the size and proportion of pores between raw material particles.
[0079] The invention made by the inventor has been specifically described above based on an embodiment, but it goes without saying that the present invention is not limited to the above embodiment and can be modified in various ways without departing from the gist of the invention. EXAMPLES
[0080] Hereinafter, an embodiment of the present invention will be described.
[0081] [▲Ka▼Baking process] Amakusa clay and heat-resistant clay (petalite) were selected as the raw materials for the porous ceramics. These commercially available raw materials were prepared in a vacuum clay kneader and cut into circular disks. They were then heated to 900°C at a heating rate of 100°C / h in an electric furnace, held at 900°C for 1 hour, and then naturally cooled to form the calcination process for the raw materials.
[0082] [Crushing process and classification process] The disk-shaped raw material obtained above after the calcination process was coarsely crushed using a jaw crusher, and then further finely pulverized using a roll crusher. The raw material particles (powders) obtained by these two stages of crushing contained particles of various sizes, large and small, and had an extremely wide particle size distribution. These raw material particles (powders) were sieved using a wire mesh into three particle sizes: 500 μm to 2.36 mm, less than 500 μm, and less than 600 μm.
[0083] Example 1 Porous pottery made from heat-resistant clay (petalite) (oxidation firing, no organic binders) The raw material particles of heat-resistant clay, adjusted to a particle size of less than 500μm, were placed in an alumina crucible so that the volume was 1 / 4 of the internal volume, and the crucible was tapped on a table several times to fill the pot with the gravity of the raw material particles alone and molded. The crucible containing the raw material particles was heated to 1250℃ at a heating rate of 100℃ / h in an electric furnace, and then oxidized and fired at 1250℃ for 1 hour (main firing process; same below), after which it was naturally cooled to obtain a molded body.
[0084] Example 2 Porous pottery made from heat-resistant clay (petalite) (oxidation firing, organic binder used) CMC (carboxymethylcellulose) was added at 5% by weight to the raw material particles of heat-resistant clay adjusted to a particle size of less than 600μm, and an appropriate amount of water was added. The mixture was mixed and kneaded by hand and placed in a stainless steel cylindrical mold so that the volume was 1 / 3 of the original volume. The contents were compressed by hand using a stainless steel cylindrical pressing tool with a diameter slightly smaller than the inner diameter of the cylinder, and then molded by filling. The molded contents were removed from the cylindrical mold and transferred to an alumina container, which was then heated to 1280℃ at a heating rate of 100℃ / h in an electric furnace, and oxidized by holding the temperature at 1280℃ for 1 hour, and then naturally cooled to obtain a molded body.
[0085] Example 3 Porous pottery made from heat-resistant clay (petalite) (reduced firing, uses organic binder) CMC (carboxymethylcellulose) was added at 5% by weight to the raw material particles of heat-resistant clay adjusted to a particle size of less than 600μm, and an appropriate amount of water was added. The mixture was mixed and kneaded by hand and placed in a stainless steel cylindrical mold so that the volume was 1 / 3 of the original volume. The contents were compressed by hand using a stainless steel cylindrical press with a diameter slightly smaller than the inner diameter of the cylinder, and then molded by filling. The molded contents were removed from the cylindrical mold and transferred to an alumina container, which was then heated to 1280℃ at a rate of 100℃ / h in a gas kiln, and reduced and fired by holding the temperature at 1280℃ for 1 hour, after which it was naturally cooled to obtain a molded body.
[0086] Example 4 Porous porcelain made from Amakusa clay (large particle size powder, oxidized firing, organic binder used) Amakusa clay raw material particles with particle size adjusted to 500μm~2.36mm were mixed with 5% CMC (carboxymethylcellulose) based on the particle weight, and an appropriate amount of water was added. The mixture was mixed and kneaded by hand and placed in a stainless steel cylindrical mold so that the volume was 1 / 3 of the original volume. A stainless steel cylindrical press with a diameter slightly smaller than the inner diameter of the cylinder was used to compress the contents by hand and fill the mold. The molded contents were removed from the cylindrical mold and transferred to an alumina container, which was then heated to 1280℃ at a heating rate of 100℃ / h in an electric furnace, and oxidized by holding the temperature at 1280℃ for 1 hour, and then naturally cooled to obtain a molded body.
[0087] Example 5 Porous porcelain made from Amakusa clay (large particle size powder, reduction firing, organic binder used) The raw material particles of heat-resistant clay, adjusted to a particle size of 500μm~2.36mm, were mixed and kneaded by hand with 5% CMC (carboxymethylcellulose) based on the particle weight, and an appropriate amount of water was added. The mixture was then placed in a stainless steel cylindrical mold to a volume of 1 / 3, and the contents were compressed and filled by hand using a stainless steel cylindrical press with a diameter slightly smaller than the inner diameter of the cylinder to form a mold. The molded contents were removed from the cylindrical mold and transferred to an alumina container, which was then heated to 1280℃ at a rate of 100℃ / h in a gas kiln, and reduced and fired by holding the temperature at 1280℃ for 1 hour, after which it was naturally cooled to obtain a molded body.
[0088] Example 6 Porous porcelain made from Amakusa clay (small particle size powder, oxidized firing, organic binder used) Amakusa clay raw material particles with particle size adjusted to less than 500μm were mixed with 5% CMC (carboxymethylcellulose) based on the particle weight, and an appropriate amount of water was added. The mixture was mixed and kneaded by hand and placed in a stainless steel cylindrical mold so that the volume was 1 / 3 of the original volume. A stainless steel cylindrical press with a diameter slightly smaller than the inner diameter of the cylinder was used to compress and pack the contents by hand. The molded contents were removed from the cylindrical mold and transferred to an alumina container, which was then heated to 1280℃ at a heating rate of 100℃ / h in an electric furnace, and oxidized by holding the temperature at 1280℃ for 1 hour, after which it was naturally cooled to obtain a molded body.
[0089] Example 7 Porous porcelain made from Amakusa clay (small particle size powder, reduction firing, organic binder used) The raw material particles of heat-resistant clay, adjusted to a particle size of less than 500μm, were mixed and kneaded by hand with 5% CMC (carboxymethylcellulose) based on the particle weight, and an appropriate amount of water was added. The mixture was then placed in a stainless steel cylindrical mold to a volume of 1 / 3, and the contents were compressed and filled by hand using a stainless steel cylindrical press with a diameter slightly smaller than the inner diameter of the cylinder to form a mold. The molded contents were removed from the cylindrical mold and transferred to an alumina container, which was then heated to 1280℃ at a rate of 100℃ / h in a gas kiln, and reduced and fired by holding the temperature at 1280℃ for 1 hour, after which it was naturally cooled to obtain a molded body.
[0090] [Alkaline resistance comparison test (Example 8)] Test pieces were cut out from the molded body obtained in Example 7 above using a diamond cutter, and an alkali resistance test was carried out under the following conditions. A test piece was placed in a plastic beaker containing 20 cc of a 5 mass % NaOH aqueous solution, and this was left to stand for 24 hours while being heated in an oil bath set to 90°C, after which the condition of the test piece was visually confirmed (Example 8).
[0091] A comparative test piece (glass-using method, conventional technology) was prepared by the following method, and an alkali resistance test was performed under the same conditions. As a comparative test piece, 10% glass frit was added to ceramic waste (cerben) particles adjusted to a particle size of 300 to 500 μm, and an appropriate amount of water was added, and the mixture was mixed and kneaded by hand, and placed in a stainless steel cylindrical mold so that the volume was 1 / 3 of the volume, and the contents were compressed and filled by hand using a stainless steel cylindrical pressing tool with a diameter slightly smaller than the inner diameter of the cylindrical mold. The molded contents were removed from the cylindrical mold and transferred to an alumina container, and then heated to 1280°C at a heating rate of 100°C / h in an electric furnace, and oxidized and fired at 1280°C for 1 hour, and then naturally cooled to obtain a molded body. A test piece was cut out from the obtained molded body with a diamond cutter and subjected to an alkali resistance test (Comparative Example 1).
[0092] [Porosity comparison test] For the molded bodies obtained in Examples 2 to 7 above, the open porosity was calculated by the Archimedes method, and the total porosity was calculated from the true density measured by a dry automatic densimeter and the bulk density measured by the Archimedes method.
[0093] A comparative test piece (pore-forming agent method, conventional technology) was prepared by the following method, and the porosity was measured under the same conditions. For the comparative test piece, water was added to Amakusa clay to prepare a slurry with a moisture content of 30%. Wheat flour was added as a pore-forming agent at an external ratio of 5% based on the dry weight of the Amakusa clay in the slurry, and an appropriate amount of water was added to the slurry to obtain a viscosity suitable for casting. The slurry was cast into a plaster mold and dried at room temperature to form the molded product. The molded product was released from the plaster mold and transferred to an alumina container, which was then heated to 1250°C at a heating rate of 100°C / h in an electric furnace, and then oxidized and fired by holding the temperature at 1250°C for 1 hour, followed by natural cooling to obtain a molded product. A test piece was cut out from the obtained molded product using a diamond cutter and subjected to porosity measurement (Comparative Example 2).
[0094] [Confirmation test of the effect of adding organic binder on pore formation] Two types of molded bodies were produced from Amakusa clay, one with an organic binder added and one without the addition, and the pore distribution and porosity were measured using mercury intrusion porosity to confirm the effect of the organic binder on pore formation in porous ceramics.
[0095] For the test pieces, Amakusa clay was mixed with water to prepare a slurry with a moisture content of 30%. To this, 2.5% CMC (carboxymethylcellulose) was added as an organic binder based on the dry weight of the Amakusa clay in the slurry, and an appropriate amount of water was added to make the slurry viscous enough for casting. Two types of slurry, one with no CMC added, were cast into plaster molds and dried at room temperature to form the molds. The molded pieces were released from the plaster molds and transferred to alumina containers, which were then heated to 1250°C at a rate of 100°C / h in an electric furnace, and then oxidized and fired at 1250°C for 1 hour. They were then naturally cooled to obtain molded bodies. The molded bodies obtained were coarsely crushed in a mortar and subjected to porosity measurements.
[0096] [result] Example 1 The obtained molded body is shown in Figure 2. A cookie-like porous structure was visually confirmed (see Figure 2). Figure 3 shows an enlarged image of the structure surface taken with a digital microscope. It was confirmed that the raw material particles were bonded together through sintering at the points where they came into contact, forming numerous pores consisting of the gaps between the particles (see Figure 3).
[0097] Example 2 The obtained molded body is shown in Figure 4. The same porous structure as in Example 1 was confirmed.
[0098] Example 3 The obtained molded body is shown in Figure 5. The same porous structure as in Example 1 was confirmed.
[0099] Example 4 The obtained molded product is shown in Figure 6. A rice-like porous structure was visually confirmed.
[0100] Example 5 The obtained molded product is shown in Figure 7. A rice-like porous structure was visually confirmed.
[0101] Example 6 The obtained molded body is shown in Figure 8. The same porous structure as in Example 1 was confirmed.
[0102] Example 7 The obtained molded body is shown in Figure 9. The same porous structure as in Example 1 was confirmed.
[0103] From the above, it was confirmed that a porous structure can be formed by oxidation firing or reduction firing, whether the ceramic raw material is heat-resistant clay or Amakusa clay. This means that a porous structure can be manufactured regardless of the firing equipment (electric furnace, gas kiln).
[0104] Example 8 The results of the alkali resistance test are shown in Figure 10. In the porous structure of Example 8 (upper part of Figure 10), no change was observed before and after the alkali resistance test. On the other hand, in the porous structure formed by the glass utilization method of Comparative Example 1 (lower part of Figure 10), partial collapse was observed after the alkali resistance test. The partially collapsed area of Comparative Example 1 is indicated by an arrow in the figure.
[0105] In Example 8, Amakusa clay is used as the raw material, and the raw material particles that are crushed after the calcination process are bonded together at their contact points by sintering, so no raw material components other than Amakusa clay are included. Porcelain made from Amakusa clay is known to have excellent chemical resistance.
[0106] On the other hand, in the porous structure formed by the glass utilization method of Comparative Example 1, glass is mixed with ceramic waste (ceramic waste), and the ceramic waste is bonded together by the glass melting during the firing stage. In other words, the glass acts as an adhesive to hold the ceramic waste together, and because glass has lower alkali resistance than porcelain, it is believed that the glass acting as an adhesive melted and was no longer able to hold the ceramic waste together, resulting in partial collapse.
[0107] [Porosity comparison test] The porosity measurement results of the test pieces derived from the molded bodies obtained in Examples 2 to 7 and Comparative Example 2 are shown in Table 1.
[0108] [Table 1] JPEG2024140673000003.jpg3195
[0109] As shown in Table 1, it was confirmed that the open porosity and total porosity in Examples 2 to 7 were both larger and higher than those in Comparative Example 2. This suggests that the method for producing porous ceramics to which the present invention is applied can produce porous ceramics having a porosity equal to or higher than that of the conventional method, without using a pore-forming agent that is expensive and difficult to handle, such as for dispersion.
[0110] In addition, in a comparison between Example 2 and Example 3, between Example 4 and Example 5, and between Example 6 and Example 7, which used the same raw materials and particles with the same particle size distribution, it was confirmed that oxidation firing tended to have a higher porosity than reduction firing.
[0111] [Confirmation test of the effect of adding organic binder on pore formation] Figure 11 shows the results of pore size distribution measurement using mercury porosimetry for cast bodies made from slip prepared with Amakusa clay, one without added organic binder (Amakusa clay (standard)) and one with added organic binder (Amakusa clay + CMC 2.5%).
[0112] As shown on the left side of Figure 11, the median pore size was 0.83 μm for the standard and 0.49 μm for the CMC-added sample. As shown on the right side of Figure 11, the distribution showed that the CMC-added sample had smaller pore sizes than the standard sample, but no significant difference was observed. The porosity calculated from the obtained measurement data was 10.6% for the standard and 9.6% for the CMC-added sample, and no significant difference was observed.
[0113] From the above, it is confirmed that even if an organic binder is added during molding, the organic binder does not act as a pore-forming agent, and that in the present invention, the raw material particles crushed after the calcination process are bonded together at their contact points by sintering, thereby producing porous ceramics. [Explanation of symbols]
[0114] S1 ▲Caking process S2 Grinding process S3 Classification process S4 Molding process S5 Main firing process
Claims
1. The firing process involves heating the ceramic raw materials and baking them to a state before sintering is completed. a crushing step of crushing the product produced through the calcination step to obtain raw material particles having different particle sizes; A classification step of classifying the raw material particles into a plurality of sections according to particle size; a molding step of selecting at least one section from the plurality of sections and molding the raw material particles in the selected section; and a firing step in which the molded product that has been subjected to the molding step is heated at a temperature higher than the heating temperature of the calcination step to complete sintering. How porous ceramics are made.
2. The heating temperature of the calcination is 300 degrees or more and 1000 degrees or less. A method for producing the porous ceramic ware according to claim 1.
3. The ceramic raw material is A ceramic raw material, a pottery raw material, and a fine ceramics raw material, or a combination of a ceramic raw material, a pottery raw material, and a fine ceramics raw material, and an organic binder. A method for producing the porous ceramic ware according to claim 1.
4. In the molding step, two or more sections are selected from the plurality of sections, and the raw material particles in the selected sections are molded. A method for producing the porous ceramic ware according to claim 1.
5. The molded body that has undergone the main firing step is formed only of the structure derived from the ceramic raw material. A method for producing the porous ceramic ware according to claim 1.
6. The ceramic raw material is The ceramic raw material, or a combination of the ceramic raw material and the organic binder, The heating temperature of the calcination is 500 degrees or more and 900 degrees or less. A method for producing the porous ceramic ware according to claim 3.
7. The ceramic raw material is The ceramic raw material or a combination of the ceramic raw material and the organic binder, The heating temperature of the calcination is 400 degrees or more and 800 degrees or less. A method for producing the porous ceramic ware according to claim 3.
8. The ceramic raw material is The fine ceramic or a combination of the fine ceramic and the organic binder, The heating temperature of the calcination is 900 degrees or more and 1000 degrees or less. A method for producing the porous ceramic ware according to claim 3.
Citation Information
Patent Citations
Water-permeable ceramic tile and production thereof
JP1992260649A
Production of porous ceramic product
JP2000128657A
Production of sintered compact using exhaust powder in cast process as raw material
JP2001058869A
Method for manufacturing bone prosthesis
JP2014042615A
Method of manufacturing porous ceramic, and porous ceramic
JP2018083742A