Fiber-reinforced composite material, method for producing the same, and molded body

By incorporating a controlled thickness wavelength and difference in the fiber-reinforced composite material, deformation issues like warping and twisting are minimized, ensuring enhanced strength and stability.

JP2024140679APending Publication Date: 2024-10-10MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023051961
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Fiber-reinforced composite materials exhibit high rigidity but are prone to deformation such as warping and twisting, making it difficult to correct once deformation occurs.

Method used

The composite material is engineered with a specific thickness wavelength (λ) of 31 mm to 120 mm and thickness difference (A) of 0.3 μm to 5.0 μm, creating a periodic shape in the fiber orientation direction to suppress warpage and twisting, achieved through controlled heating, pressurizing, and intermittent conveying processes.

Benefits of technology

The material exhibits reduced warpage and twisting while maintaining excellent strength, with improved dimensional stability and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140679000001
    Figure 2024140679000001
Patent Text Reader

Abstract

To provide a fiber-reinforced composite material with little warping or deformation.SOLUTION: There is provided a fiber-reinforced composite material that contains reinforcing fibers and a matrix resin and has a thickness wavelength (λ) of 31 mm or more and 120 mm or less. The thickness wavelength is defined bellow. The thickness wavelength (λ): first, for a fiber-reinforced composite material, a thickness distribution is measured at 1 mm intervals 200 times or more in a case of unidirectional fiber-reinforced composites, a direction is along fibers, and in a case of other fiber-reinforced composite materials, a circular diffraction image is obtained by radiating X-rays, and a diffraction intensity is measured in a direction of an angle with a highest intensity; second, for the thickness distribution curve obtained, each thickness value is fitted with a sine curve by a least squares method. The wavelength of this sine curve is deemed as the thickness wavelength (λ).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fiber-reinforced composite material, a method for producing the same, and a molded article thereof. [Background technology]

[0002] 2. Description of the Related Art Molded articles of fiber-reinforced composite materials in which a matrix resin composition is compounded with a reinforcing fiber substrate are used in various fields such as aircraft parts, automobile parts, and electric and electronic parts.

[0003] Fiber-reinforced composite materials containing reinforcing fibers and matrix resins are required to have little deformation such as warping or twisting when manufacturing intermediate materials such as prepregs or molded articles, from the viewpoint of handling of lamination and reduction in strength due to internal residual stress. For example, Patent Document 1 describes characteristics such as Ra and waviness curves obtained from the roughness of the material surface by providing a special cooling mechanism, and shows the range of roughness of the material surface and a manufacturing method that can suppress the amount of warping of the fiber-reinforced composite material. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2019 / 124203 Summary of the Invention [Problem to be solved by the invention]

[0005] Although Patent Document 1 shows the characteristics of surface roughness measured on only one side of a fiber-reinforced composite material, the fiber-reinforced composite material has high rigidity, and once deformation occurs, it is difficult to correct it. The present invention has been made in view of such circumstances, and aims to suppress deformation such as warping and twisting. Effect of the Invention

[0006] According to the present invention, it is possible to provide a fiber-reinforced composite material which is less susceptible to deformation such as warping or twisting and has excellent strength when formed into a molded article. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] <Fiber-reinforced composite materials> The fiber reinforced composite material of the present invention (hereinafter sometimes referred to as "the present composite material") contains reinforcing fibers and a matrix resin, and has a thickness wavelength (λ) of 31 mm or more and 120 mm or less, as described below. Thickness wavelength (λ): For fiber-reinforced composite materials, obtain a circular diffraction image produced by irradiating X-rays in the direction along the fibers in the case of unidirectional fiber-reinforced composite materials, or in the case of other fiber-reinforced composite materials, and measure the thickness distribution by measuring more than 200 times at 1 mm intervals in the direction showing the highest diffraction intensity angle, to obtain a thickness distribution curve. For the obtained thickness distribution curve, fit each value of the thickness distribution with a sine curve using the least squares method. The wavelength of this sine curve is the thickness wavelength (λ). The composite material may take the form of, for example, a prepreg, which is a sheet-like material in which reinforcing fibers are impregnated with a matrix resin.

[0008] The thickness wavelength (λ) and thickness difference (A) of the composite material with a periodic shape can be obtained by measuring a length of 200 mm or more using the following measurement method. Specifically, the thickness distribution can be measured with a known non-contact laser displacement meter or a contact micrometer. Measurements were taken at 200 points at 1 mm intervals using a laser displacement meter.

[0009] In the case of a unidirectional fiber-reinforced composite material in which the reinforcing fibers are aligned in one direction, the thickness can be measured along the fiber orientation direction, which is the flow direction during production. In the case of other fiber-reinforced composite materials, for example, in the case of multidirectional fiber-reinforced composite materials in which the reinforcing fiber form is continuous and the reinforcing fiber bundles are aligned in multiple directions, such as plain weave, twill weave, satin weave, non-crimp fabric (NCF), three-dimensional fabric, etc., and in the case of multidirectional fiber-reinforced composite materials in which the reinforcing fiber form is continuous and the reinforcing fiber bundles are aligned in multiple directions, the measurement direction can be specified using X-rays. Specifically, a circular diffraction image generated by irradiating the fiber-reinforced composite material with X-rays is obtained, and the direction in which the thickness distribution is measured can be specified along the direction showing the highest angle of diffraction intensity. For example, in the case of a so-called cross-laminate in which a fiber composite material in which the reinforcing fibers are aligned in the A direction and a fiber composite material in which the reinforcing fibers are aligned in a direction perpendicular to the A direction are stacked, a peak of diffraction intensity appears every 90°. In the case of so-called quasi-isotropic materials, in which the fiber direction of fiber composite materials is shifted by 45° and layered, peaks appear every 45°. In the case of crushed carbon fibers, i.e. completely isotropic materials, the orientation profile has a constant value over the range of φ=0° to 360°. Since the orientation of these reinforcing fibers is strengthened along the flow direction during the production of fiber-reinforced composite materials, the measurement direction is determined by finding the angle at which the X-ray diffraction peak is maximum.

[0010] In order to suppress warping or deformation of a fiber-reinforced composite material, it is preferable to impart a periodic shape to the fiber orientation direction of the fiber-reinforced composite material. In the present invention, the periodic shape is determined to have a specific wavelength (λ) range.

[0011] The periodic shape of the composite material can be quantified by measuring the thickness distribution in the orientation direction of the fibers constituting the fiber-reinforced composite material and fitting the thickness distribution with a sine curve, as described above. In the fiber-reinforced composite material, the wavelength (λ) of the fitted sine curve is 31 mm or more, preferably 33 mm or more, and more preferably 35 mm or more, while it is 120 mm or less, preferably 100 mm or less, and more preferably 80 mm or less. When the wavelength of the sine curve is equal to or more than the lower limit, warping of the fiber-reinforced composite material is reduced, and when the wavelength is equal to or less than the upper limit, twisting of the fiber-reinforced composite material is reduced.

[0012] In addition, when the thickness difference (A) is twice the amplitude of the sine curve obtained by measuring the thickness wavelength (λ), the thickness difference (A) is preferably 0.3 μm or more, more preferably 0.5 μm or more, while it is preferably 5.0 μm or less, more preferably 4.0 μm or less, and even more preferably 3.0 μm or less. When the thickness difference (A) is equal to or more than the lower limit, warping is reduced, and when it is equal to or less than the upper limit, twisting of the fiber reinforced composite material is reduced.

[0013] The periodic shape in the composite material may be a concave or convex shape, and the fiber reinforced composite material may have unevenness in part or overall. The smaller the difference in thickness of the prepreg between the convex and concave parts, the more stable the strength can be obtained by avoiding stress concentration when a load is applied to the fiber reinforced composite material. The periodic shape may be linear, or may be a straight or curved line of points. The periodic shape may be periodically arranged in a plurality of different shapes and in a plurality of different directions, not just the same shape. The direction of the periodic shape is preferably 60 to 90°, more preferably 80 to 90°, with 90° being more preferable, particularly for suppressing warpage in the flow direction.

[0014] The periodic shape of the composite material can be obtained by transferring the periodic shape to the mold used in manufacturing the fiber-reinforced composite material, or to the secondary material or pressure body placed between the mold and the fiber-reinforced composite material, after manufacturing the fiber-reinforced composite material, for example, prepreg. The wavelength (λ) and thickness difference (A) at that time are determined by the periodic shape. The secondary material includes release paper and release film, and the pressure body includes metal plate and C / C composite plate.

[0015] Alternatively, it can be manufactured by repeatedly moving and contacting a mold, auxiliary material, and pressurizing body having a predetermined shape with a fiber-reinforced composite material at a constant interval. The mold, etc. having the shape may move, or the fiber-reinforced composite material may move, or both may move in the same direction or in different directions. By changing the moving distance when the movement and contact are repeated, the thickness wavelength (λ) of the periodic shape can be changed.

[0016] Alternatively, the periodic shape may be formed by cutting the fiber-reinforced composite material using a known tool after production, or by pressing a heater or vibrator against the composite material to deform it, thereby forming the composite material.

[0017] When the fiber reinforced composite material is in the form of a prepreg, the thickness is preferably 0.015 to 10.0 mm, more preferably 0.04 to 6.0 mm, and even more preferably 0.1 to 0.5 mm, from the viewpoint of residual stress when a molded article is produced.

[0018] The void ratio of the fiber reinforced composite material is preferably 0.1 to 20 volume%, more preferably 0.2 to 2 volume%, and even more preferably 0.2 to 1 volume%. When the void ratio is equal to or greater than the lower limit, productivity is excellent, and when the void ratio is equal to or less than the upper limit, mechanical properties are excellent. From the viewpoint of rigidity and strength, the fiber volume content (Vf) of the fiber reinforced composite material is preferably 20 to 75 volume%, and more preferably 40 to 65 volume%.

[0019] In order to improve the dimensional accuracy of processing, the fiber reinforced composite material preferably has a thickness variation coefficient of 5% or less, and more preferably has a thickness variation coefficient of 4% or less. A fiber reinforced composite material containing a thermoplastic resin and reinforcing fibers and having a thickness variation coefficient of 4% or less is preferable, and a fiber reinforced composite material having a flat plate shape with a thickness of 40 μm to 50,000 μm and a thickness variation coefficient of 4% or less is more preferable.

[0020] [Reinforced fiber] Examples of the reinforcing fibers used in the present composite material include carbon fibers, glass fibers, metal fibers, and resin fibers, and a combination of a plurality of these fibers may be used. From the viewpoint of rigidity and strength, the present composite material preferably contains carbon fibers. Examples of carbon fibers include polyacrylonitrile (PAN)-based, petroleum / coal pitch-based, rayon-based, and lignin-based. The proportion of reinforcing fibers in the reinforcing fiber substrate is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 100% by mass, based on the total mass of the reinforcing fiber substrate. A reinforcing fiber bundle can be made by bundling a plurality of reinforcing fibers and applying a sizing agent thereto.

[0021] (Reinforced fiber bundle) As the reinforcing fiber bundle, a tow consisting of 3,000 to 60,000 fibers is preferable from the viewpoint of excellent productivity and mechanical properties on an industrial scale. In order to obtain a molded body having excellent tensile strength, the strand strength of the reinforcing fiber bundle is preferably 4000 MPa or more, more preferably 5000 MPa or more. The strand modulus of the reinforcing fiber bundle is preferably 200 GPa or more, more preferably 230 GPa or more, because sufficient rigidity of the molded body is easily expressed. In addition, the graphite crystal size on the surface and inside of the reinforcing fiber becomes small, and the decrease in the strength in the fiber cross section direction and the compressive strength in the fiber axis direction is easily suppressed, so that it is preferably 380 GPa or less, more preferably 350 GPa or less. The strand strength and strand modulus of the reinforcing fiber bundle are measured by a method conforming to ASTM D4018. A reinforcing fiber base material can be obtained by arranging the reinforcing fiber bundles.

[0022] (Reinforced fiber base material) The form of the reinforcing fiber substrate includes a unidirectional continuous fiber form in which continuous reinforcing fiber bundles are aligned in one direction, a woven form such as a plain weave, a twill weave, a satin weave, a non-crimp fabric (NCF), or a three-dimensional fabric using continuous reinforcing fiber bundles, and a multidirectional fiber form such as a continuous strand mat or a chopped strand mat using reinforcing fiber bundles. In order to maintain the arrangement of the fabric, a fixing method such as stitching with reinforcing fibers or welding of thermosetting resin or thermoplastic resin fibers can be applied. Since the unidirectional continuous fiber form is more susceptible to deformation, the effect of suppressing deformation by the periodic shape is large.

[0023] [Matrix resin] The matrix resin used in the composite material may be a thermosetting resin such as an epoxy resin or a vinyl ester resin, or a thermoplastic resin such as a polypropylene resin, a polyamide resin, a polycarbonate resin, a polyphenylene sulfide resin, a polyether sulfone resin, a polyetherimide resin, a polyether ether ketone resin, a polyether ketone ketone resin, or a combination thereof. Among these, from the viewpoint of the molding cycle, a thermoplastic resin is preferred, and it is preferable to include at least one selected from a polyamide resin, a polyphenylene sulfide resin, a polyetherimide resin, a polyether ether ketone resin, and a polyether ketone ketone resin. A resin that can be polymerized after impregnating a monomer or a low molecular weight substance such as an acrylic resin, a polyamide resin, or a thermoplastic epoxy resin into a reinforcing fiber substrate may be used. As the matrix resin, a matrix resin composition containing various additives such as a known thermosetting resin, a filler, a heat stabilizer, an antioxidant, an anti-aging agent, a flame retardant, and a pigment, as necessary, may be used as long as it does not impair the effects of the invention.

[0024] The softening temperature of the matrix resin is the melting point when the crystalline melting enthalpy ΔHm measured by a differential scanning calorimeter (DSC) is 10 J / g or more, and is (Tg+100)(°C) when it is less than 10 J / g. Here, Tg is the glass transition temperature. The crystalline melting enthalpy ΔHm, the glass transition temperature Tg, and the melting point can be measured by a method conforming to ISO11357.

[0025] (Method of manufacturing fiber-reinforced composite materials) The method for producing the composite material is not particularly limited, but specific examples are given below.

[0026] The method for producing a fiber-reinforced composite material of the present invention includes the steps of: preparing a fiber-reinforced composite material precursor in which reinforcing fibers and a matrix resin film are laminated; heating the fiber-reinforced composite material precursor to a temperature equal to or higher than the softening temperature of the matrix resin; pressurizing the fiber-reinforced composite material precursor with one or more independent pressurizing bodies; and intermittently transporting the fiber-reinforced composite material precursor, wherein the travel distance of the fiber-reinforced composite material precursor in the intermittent transport step is 35 mm or more and 130 mm or less.

[0027] First, in the step of preparing a fiber-reinforced composite material precursor, the reinforcing fibers are unwound from a roll, and the matrix resin films are placed on the upper and lower surfaces of the reinforcing fibers via a pressure roller together with a matrix resin film unwound from a plurality of rolls to form a fiber-reinforced composite material precursor. The obtained fiber-reinforced composite material precursor is preheated with a heater, and then release films are placed on the upper and lower surfaces of the fiber-reinforced composite material precursor.

[0028] Next, in the step of heating the fiber-reinforced composite material precursor to a temperature equal to or higher than the softening point of the matrix resin, the fiber-reinforced composite material precursor is heated by contacting a heated hot plate, pressure body, or mold with the fiber-reinforced composite material precursor. The heating temperature at this time is preferably 400° C. or higher, more preferably 410° C. or higher, and even more preferably 420° C. or higher. By heating within the above range, a periodic shape is more easily formed, and warping and twisting are reduced.

[0029] In the step of pressurizing the fiber-reinforced composite material precursor, the heated fiber-reinforced composite material precursor is pressurized by one or more independent pressurizing bodies. The pressure applied by the pressurizing bodies is preferably 2 MPa or more, more preferably 3 MPa or more, and further preferably 4 MPa or more. Pressurizing within the above range makes it easier to form a periodic shape, and reduces warping and twisting.

[0030] In the step of intermittently conveying the fiber-reinforced composite material precursor, the fiber-reinforced composite material precursor is pressed once, and then the pressurized body is separated from the fiber-reinforced composite material precursor, and the fiber-reinforced composite material precursor is conveyed forward by a certain distance. Then, the fiber-reinforced composite material precursor is pressed again by the pressurized body. By repeating this pressurization and conveying process, the fiber-reinforced composite material precursor is conveyed intermittently. The moving distance in the intermittent conveying step is 35 mm or more, preferably 36 mm or more, more preferably 37 mm or more, while it is 130 mm or less, preferably 120 mm or less, and more preferably 100 mm or less. The warping of the fiber-reinforced composite material obtained by being equal to or more than the lower limit is reduced, and the twisting of the fiber-reinforced composite material obtained by being equal to or less than the upper limit is reduced. After the intermittent conveying, the release film is removed to obtain the fiber-reinforced composite material.

[0031] In addition, in the pressurizing step, it is preferable to cool the fiber-reinforced composite material precursor by at least one pressurizing body. In that case, it is preferable to have at least one pressurizing body that heats to the softening point of the matrix resin or higher and at least one mold that cools to the softening point of the matrix resin or lower. When the temperature of the pressurizing body that heats to the softening point of the matrix resin or higher is T1 (°C), the temperature that heats to the softening point of the matrix resin or lower is T2 (°C), and the moving distance from the mold that heats to the softening point of the matrix resin or higher to the mold that cools to the softening point of the matrix resin or lower is d (mm), the cooling distance D (mm / °C) represented by the following formula is preferably 0.3 mm / °C or higher, more preferably 0.31 mm / °C or higher, and even more preferably 0.32 mm / °C or higher, while it is preferably 1.0 mm / °C or lower, more preferably 0.9 mm / °C or lower, and even more preferably 0.7 mm / °C or lower. When it is equal to or higher than the lower limit, warping is reduced. When it is equal to or lower than the upper limit, twisting of the fiber-reinforced composite material is reduced. Mold temperature above softening temperature: T1 (℃) Mold temperature below softening temperature: T2 (℃) Distance traveled by fiber-reinforced composite precursor: d (mm) Cooling distance: D=d / (T1-T2)(mm / ℃)

[0032] Another example of a manufacturing method is to add resin fibers or resin particles formed using a matrix resin instead of a matrix resin film to the reinforcing fibers, heat and melt the fibers to impregnate them with the matrix resin, and remove air between the fibers.

[0033] When resin fibers of the matrix resin are used instead of the matrix resin film, the fiber diameter of the resin fibers is preferably 5 to 50 μm. When resin particles of the matrix resin are used instead of the matrix resin film, the average particle diameter of the resin particles is preferably 10 to 100 μm. In addition, a method of laminating a film formed using a matrix resin composition with reinforcing fibers to obtain a fiber-reinforced composite material precursor, heating and melting the film to impregnate the matrix resin, and removing air between the fibers to obtain a fiber-reinforced composite material is exemplified. When the matrix resin is in the form of a film, the thickness of the film is preferably 10 to 100 μm. The film may be a non-stretched film or a stretched film, and a non-stretched film is preferred from the viewpoint of excellent secondary processability. The non-stretched film includes a film having a stretch ratio of less than 2 times. When the matrix resin is in the form of a film, the method of producing the film is not particularly limited, and a known method can be adopted. For example, a method of melt-kneading a material used for the matrix resin, extruding it into a film, and cooling the film can be exemplified. For melt-kneading, a known kneader such as a single-screw or twin-screw extruder can be used. The extrusion molding can be carried out, for example, by using a mold such as a T-die. The melting temperature can be appropriately adjusted depending on the type and mixing ratio of the resin, and the presence and type of additives. The cooling can be, for example, by contacting the resin with a cooling machine such as a cooled cast roll.

[0034] [Molded body] The composite material can be molded into a molded product. This molded product can be continuously manufactured in a continuous shape. For example, open cross-sectional shapes such as a prism, cylinder, I-shape, H-shape, C-shape, hat-shape, etc., and closed cross-sectional shapes such as a cylinder and hollow shape can be manufactured. The thickness of the molded product can be appropriately determined depending on the shape of the molded product, for example, from 0.1 to 50 mm.

[0035] (Method of Manufacturing Molded Product) When the composite material is molded into a molded body, the molded body can be produced by passing the composite material through a mold to which the shape of the molded body has been imparted, in the same manner as the composite material, by intermittently conveying the material through the mold. In this case, a method of heating and pressurizing the reinforced fiber composite material using a known method to eliminate voids is preferred. The periodic shape may be imparted during or after the production of the molded body. The method of imparting the periodic shape after the production of the molded body may be inline or off-line. EXAMPLES

[0036] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the following description. The values ​​of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values ​​in the embodiments of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values ​​and the values ​​of the following examples or values ​​between the examples.

[0037] [Example 1] A unidirectional fiber substrate using carbon fiber MR50R (manufactured by Mitsubishi Chemical Corporation) and a 27μm thick film extruded with PEEK resin (3300G manufactured by Daicel Evonik Co., Ltd., melting point 330-340℃) using a T-die are bonded by heat fusion to produce a carbon fiber area weight (FAW) of 72g / m. 2 Thus, a fiber-reinforced composite material precursor was obtained in which 100% of the fibers remained unimpregnated.

[0038] A composite mold was prepared in a hydraulic press with a groove shape of about 1 mm length between a flat plate mold 1 adjusted to 420°C and a flat plate mold 2 adjusted to 300°C, and a pressurized body 1 and a pressurized body 2 (C / C composite plate of about 3 mm thickness) were placed therein. Next, the two overlapped fiber reinforced composite material precursors were laminated with release films (Upilex 50S manufactured by Ube Industries) on both sides and passed between the pressurized body 1 and the pressurized body 2, heated and pressurized in the mold 1 adjusted to 420°C, moved 75 mm toward the mold 2 adjusted to 300°C, and pressurized again and cooled and solidified, and the process was repeated to obtain a fiber reinforced composite material of about 0.13 mm thickness impregnated at an average pressure of 4.1 MPa.

[0039] The obtained fiber reinforced composite material had a convex shape in the direction perpendicular to the fiber orientation direction due to the groove shape of mold 1 and mold 2. A rectangle of 300 mm in the fiber orientation direction and 200 mm in the direction perpendicular to the fiber orientation direction was cut out, and the thickness of the fiber reinforced composite material was measured from both sides using the laser displacement function of a benchtop density meter (manufactured by Hutec Co., Ltd.), and the thickness distribution was measured at 1 mm intervals in the fiber orientation direction. The obtained thickness distribution was fitted using the least squares method. The wavelength (λ) and thickness difference (A) of the obtained sine curve are shown in Table 1.

[0040] Next, the rectangular prepreg, 300 mm long and 200 mm wide, was placed on a flat surface with the bottom convex, and the height between the four corners of the rectangular prepreg and the flat surface was measured using a metal ruler, and the average of the four corners was obtained. The presence or absence of warping or twisting was also observed. The results of the difference in height between the four corners and the flat surface and the presence or absence of warping or twisting are shown in Table 1. An overall evaluation was also performed based on the following judgment. This overall evaluation was evaluated as A being the best and D being the worst. (comprehensive evaluation) A: The average height of the flat area from the four corners is 10 mm or less, and no warping or twisting was observed. B: The average height of the flat area from the four corners exceeds 10 mm, but no warping or twisting was observed. C: The average height of the flat area from the four corners is 10 mm or less, but warping or twisting is observed. D: The average height of the flat area from the four corners exceeds 10 mm, and warping or twisting is observed.

[0041] [Example 2] The manufacturing method was the same as that of Example 1, except that the moving distance to the mold 2 whose temperature was adjusted to 300° C. was changed to 50 mm. The results are shown in Table 1.

[0042] [Example 3] The manufacturing method was the same as that of Example 1, except that the moving distance to the mold 2 whose temperature was adjusted to 300° C. was changed to 38 mm. The results are shown in Table 1.

[0043] [Comparative Example 1] The manufacturing method was the same as that of Example 1, except that the moving distance to the mold 2 whose temperature was adjusted to 300° C. was changed to 30 mm. The results are shown in Table 1.

[0044] [Comparative Example 2] The manufacturing method was the same as that of Example 1, except that the moving distance to the mold 2 whose temperature was adjusted to 300° C. was changed to 150 mm. The results are shown in Table 1.

[0045] [Table 1]

[0046] [summary] In summary, the present invention may have the following embodiments. [Embodiment 1] A fiber-reinforced composite material comprising reinforcing fibers and a matrix resin, and having a thickness wavelength (λ) of 31 mm or more, 33 mm or more, or 35 mm or more. Thickness wavelength (λ): For fiber-reinforced composite materials, obtain a circular diffraction image produced by irradiating X-rays in the direction along the fibers in the case of unidirectional fiber-reinforced composite materials, or in the case of other fiber-reinforced composite materials, and measure the thickness distribution by measuring more than 200 times at 1 mm intervals in the direction showing the highest diffraction intensity angle, to obtain a thickness distribution curve. For the obtained thickness distribution curve, fit each thickness value with a sine curve using the least squares method. The wavelength of this sine curve is the thickness wavelength (λ). [Embodiment 2] 2. The fiber-reinforced composite material of claim 1, wherein the thickness wavelength (λ) is 120 mm or less, 100 mm or less, or 80 mm or less. [Embodiment 3] A fiber-reinforced composite material comprising reinforcing fibers and a matrix resin, the thickness wavelength (λ) being 120 mm or less, 100 mm or less, or 80 mm or less. Thickness wavelength (λ): For fiber-reinforced composite materials, obtain a circular diffraction image produced by irradiating X-rays in the direction along the fibers in the case of unidirectional fiber-reinforced composite materials, or in the case of other fiber-reinforced composite materials, and measure the thickness distribution by measuring more than 200 times at 1 mm intervals in the direction showing the highest diffraction intensity angle, to obtain a thickness distribution curve. For the obtained thickness distribution curve, fit each thickness value with a sine curve using the least squares method. The wavelength of this sine curve is the thickness wavelength (λ). [Embodiment 4] A fiber-reinforced composite material, in which the thickness difference (A) is 0.3 μm or more, 0.4 μm or more, or 0.5 μm or more. Thickness difference (A): The thickness difference (A) is defined as twice the amplitude of the sine curve obtained by measuring the thickness wavelength (λ). [Embodiment 5] 5. The fiber-reinforced composite material according to embodiment 4, wherein the thickness difference (A) is 5.0 μm or less, 4.0 μm or less, or 3.0 μm or less. [Embodiment 6] 4. The fiber-reinforced composite material according to any one of embodiments 1 to 3, wherein the thickness difference (A) is 5.0 μm or less, 4.0 μm or less, or 3.0 μm or less. Thickness difference (A): The thickness difference (A) is defined as twice the amplitude of the sine curve obtained by measuring the thickness wavelength (λ). [Embodiment 7] 4. The fiber-reinforced composite material according to any one of embodiments 1 to 3, wherein the thickness difference (A) is 0.3 μm or more, 0.4 μm or more, or 0.5 μm or more. Thickness difference (A): The thickness difference (A) is defined as twice the amplitude of the sine curve obtained by measuring the thickness wavelength (λ). [Embodiment 8] 8. The fiber-reinforced composite material according to embodiment 7, wherein the thickness difference (A) is 5.0 μm or less, 4.0 μm or less, or 3.0 μm or less. [Embodiment 9] 9. The fiber-reinforced composite material according to any one of claims 1 to 8, wherein the matrix resin is a thermoplastic resin. [Embodiment 10] The fiber-reinforced composite material according to any one of claims 1 to 9, wherein the reinforcing fibers are aligned in one direction. [Embodiment 11] 11. The fiber-reinforced composite material according to any one of claims 1 to 10, having a thickness of at least 0.015 mm, at least 0.04 mm, or at least 0.1 mm. [Embodiment 12] 12. The fiber-reinforced composite material of any one of claims 1 to 11, having a thickness of at most 10.0 mm, at most 6.0 mm, at most 1.0 mm, or at most 0.5 mm. [Embodiment 13] 13. The fiber-reinforced composite material according to any one of claims 1 to 12, comprising carbon fibers as the reinforcing fibers. [Embodiment 14] A molded article obtained by molding the fiber-reinforced composite material according to any one of embodiments 1 to 13. [Embodiment 15] 1. A method for producing a fiber-reinforced composite material, comprising the steps of: preparing a fiber-reinforced composite material precursor in which reinforcing fibers and a matrix resin film are layered together; heating the fiber-reinforced composite material precursor to a temperature equal to or higher than the softening temperature of the matrix resin; pressurizing the fiber-reinforced composite material precursor with one or more independent pressurizing bodies; and intermittently transporting the fiber-reinforced composite material precursor, wherein the travel distance of the fiber-reinforced composite material precursor in the intermittent transport step is 35 mm or more, 36 mm or more, or 37 mm or more. [Embodiment 16] 1. A method for producing a fiber-reinforced composite material, comprising the steps of: preparing a fiber-reinforced composite material precursor in which reinforcing fibers and a matrix resin film are layered together; heating the fiber-reinforced composite material precursor to a temperature equal to or higher than the softening temperature of the matrix resin; pressurizing the fiber-reinforced composite material precursor with one or more independent pressurizing bodies; and intermittently transporting the fiber-reinforced composite material precursor, wherein the travel distance of the fiber-reinforced composite material precursor in the intermittent transport step is 130 mm or less, 120 mm or less, or 100 mm or less. [Embodiment 17] 17. The method for producing a fiber-reinforced composite material according to claim 16, wherein the distance traveled by the fiber-reinforced composite material precursor in the intermittent transport step is 35 mm or more, 36 mm or more, or 37 mm or more. [Embodiment 18] 18. The method of any one of claims 15 to 17, wherein the heating temperature in the heating step is 400°C or more, 410°C or more, or 420°C or more. [Embodiment 19] 19. The method for producing a fiber-reinforced composite material according to any one of claims 15 to 18, wherein the pressure applied by the pressurizing body is 2 MPa or more, 3 MPa or more, or 4 MPa or more. [Embodiment 20] 20. The method for producing a fiber-reinforced composite material according to any one of embodiments 15 to 19, further comprising the step of cooling the fiber-reinforced composite material precursor by the pressurizing body in the pressurizing step, wherein the fiber-reinforced composite material precursor is cooled from a softening temperature or higher to a softening temperature or lower at a cooling distance D of 0.3 mm / °C or more, 0.31 mm / °C or more, or 0.32 mm / °C or more in the cooling step. Mold temperature above softening temperature: T1 (℃) Mold temperature below softening temperature: T2 (℃) Distance traveled by fiber-reinforced composite precursor: d (mm) Cooling distance: D=d / (T1-T2)(mm / ℃) [Embodiment 21] 21. The method for producing a fiber-reinforced composite material according to any one of embodiments 15 to 20, further comprising the step of cooling the fiber-reinforced composite material precursor by the pressurizing body in the pressurizing step, wherein the cooling step is performed at a cooling distance D of 1.0 mm / °C or less, 0.9 mm / °C or less, or 0.7 mm / °C or less when cooling from a softening temperature or higher to a softening temperature or lower. Mold temperature above softening temperature: T1 (℃) Mold temperature below softening temperature: T2 (℃) Distance traveled by fiber-reinforced composite precursor: d (mm) Cooling distance: D=d / (T1-T2)(mm / ℃)

Claims

1. A fiber-reinforced composite material comprising reinforcing fibers and a matrix resin, the fiber-reinforced composite material having a thickness wavelength (λ) of 31 mm or more and 120 mm or less. Thickness wavelength (λ): For fiber-reinforced composite materials, obtain a circular diffraction image generated by irradiating X-rays in the direction along the fibers in the case of unidirectional fiber-reinforced composite materials, and in the case of other fiber-reinforced composite materials, measure the thickness distribution by measuring 200 times or more at 1 mm intervals in the direction showing the highest diffraction intensity angle, and obtain a thickness distribution curve. For the obtained thickness distribution curve, fit each thickness value with a sine curve by the least squares method. The wavelength of this sine curve is the thickness wavelength (λ).

2. The fiber-reinforced composite material according to claim 1, wherein the thickness difference (A) is 0.3 μm or more and 5.0 μm or less. Thickness difference (A): The thickness difference (A) is defined as twice the amplitude of the sine curve obtained by measuring the thickness wavelength (λ).

3. 3. The fiber-reinforced composite material according to claim 1, wherein the matrix resin is a thermoplastic resin.

4. 3. The fiber-reinforced composite material according to claim 1, wherein the reinforcing fibers are aligned in one direction.

5. 3. The fiber-reinforced composite material according to claim 1, having a thickness of 0.1 to 0.5 mm.

6. The fiber-reinforced composite material according to claim 1 or 2, wherein the reinforcing fibers include carbon fibers.

7. A molded article obtained by molding the fiber-reinforced composite material according to claim 1 or 2.

8. The molded article according to claim 7, wherein the matrix resin is a thermoplastic resin.

9. The fiber-reinforced composite material molded product according to claim 7, wherein the reinforcing fibers are aligned in one direction.

10. The fiber-reinforced composite material molded article according to claim 7, wherein the fiber-reinforced composite material has a thickness of 0.1 to 0.5 mm.

11. The fiber-reinforced composite material molded product according to claim 7, wherein the reinforcing fibers are carbon fibers.

12. A step of preparing a fiber-reinforced composite material precursor in which reinforcing fibers and a matrix resin film are laminated; heating the fiber-reinforced composite precursor to a temperature equal to or higher than the softening temperature of the matrix resin; Pressurizing the fiber-reinforced composite material precursor with one or more independent pressurizing bodies; The method includes a step of intermittently conveying the fiber-reinforced composite material precursor, a moving distance of the fiber-reinforced composite material precursor in the intermittent conveying step is 35 mm or more and 130 mm or less.

13. The method for producing a fiber-reinforced composite material according to claim 12, wherein the heating temperature in the heating step is 400°C or higher.

14. The method for producing a fiber-reinforced composite material according to claim 11 or 12, wherein the pressure applied by the pressurizing body is 2 MPa or more.

15. The pressurizing step includes a step of cooling the fiber-reinforced composite material precursor by the pressurizing body, 13. The method for producing a fiber-reinforced composite material according to claim 11, wherein in the cooling step, cooling from a temperature above the softening temperature to a temperature below the softening temperature is performed at a cooling distance D of 0.3 mm / °C or more and 1.0 mm / °C or less. Mold temperature above softening temperature: T1 (℃) Mold temperature below softening temperature: T2 (°C) Distance traveled by fiber-reinforced composite precursor: d (mm) Cooling distance: D=d / (T1-T2) (mm / ℃)

Citation Information

Patent Citations

  • Tape-shaped prepreg and production method therefor

    WO2019124203A1