Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
The toner formulation with defined vinyl resin particle parameters addresses the misalignment issue in high temperature and humidity, enhancing fine line resolution stability.
Patent Information
- Application Number
- JP2023052434
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Existing toners experience a decrease in fine line resolution when repeatedly forming images in high temperature and high humidity environments due to misalignment of the 'mass center of gravity' and 'geometric center' of toner particles, leading to reduced electrostatic adhesion and increased rolling of toner particles.
The toner formulation includes specific parameters for vinyl resin particles within toner particles, such as area ratios, geometric center usage, and solubility parameters, to maintain uniform dispersion and prevent misalignment, ensuring stable charge and reduced rolling.
The toner suppresses the decrease in fine line resolution by maintaining uniform dispersion and electrostatic adhesion, even in harsh environmental conditions.
Smart Images

Figure 2024141015000006 
Figure 2024141015000007 
Figure 2024141015000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner for developing an electrostatic image, an electrostatic image developer, a toner cartridge, a process cartridge, an image forming apparatus, and an image forming method. [Background technology]
[0002] Patent Document 1 proposes a toner for developing electrostatic images, which comprises "toner particles containing a binder resin containing a polyester resin, a release agent containing a hydrocarbon wax, and a styrene (meth)acrylic resin, wherein 70% or more of the total release agent is present within 800 nm from the surface of the toner particles, the styrene (meth)acrylic resin forms domains in the toner particles having an average diameter of 0.3 μm or more and 0.8 μm or less, and the proportion of the domains falling within the range of the average diameter ±0.1 μm is 65% or more." Patent Document 2 proposes a toner for developing electrostatic images, which comprises toner particles containing a binder resin including a polyester resin, a release agent including a hydrocarbon wax, and a styrene (meth)acrylic resin, in which 70% or more of the total release agent is present within 800 nm from the surface of the toner particles, and the styrene (meth)acrylic resin forms domains with an average diameter of less than 0.3 μm in the toner particles. Patent Document 3 describes a toner that includes a binder resin and rubber particles, and has a compression set of 20% to 50% at a temperature at which the melt viscosity of the toner reaches 104 Pa. A toner for developing electrostatic images has been proposed. Patent Document 4 proposes "a toner for developing electrostatic images, comprising at least a binder resin, a continuous phase containing the binder resin, and a discontinuous phase having a core containing the binder resin and a coating layer containing the binder resin and covering the core, the discontinuous phase being interspersed in the continuous phase." [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-062040 A [Patent Document 2] JP 2016-062042 A [Patent Document 3] JP 2020-046499 A [Patent Document 4] JP 2020-160204 A Summary of the Invention [Problem to be solved by the invention]
[0004] The object of the present invention is to provide a toner for developing electrostatic images, which comprises toner particles containing a binder resin, a colorant, and vinyl resin particles, and to determine the area Sa (μm) of a Voronoi polygon when a Voronoi division is performed with the geometric center of the vinyl resin particle as a generating point in a cross-sectional observation of the toner particle. 2 ) is measured, the median value Sac (μm 2 ), the standard deviation of the area Sa of the Voronoi polygon is Ssd (μm 2 ), the toner for developing electrostatic images is capable of suppressing the decrease in fine line resolution that occurs when images are repeatedly formed under a high-temperature and high-humidity environment, compared to a case in which the following formulas (1) and (2) are not satisfied. [Means for solving the problem]
[0005] Means for solving the above problems include the following aspects. <1> The toner particles include a binder resin and vinyl resin particles, In observing the cross section of the toner particle, the area Sa (μm of the Voronoi polygon when Voronoi division is performed with the geometric center of the vinyl resin particle as the base point is determined. 2 ), the median of the area Sa of the Voronoi polygon is defined as Sac (μm 2 ), the standard deviation of the area Sa of the Voronoi polygon is Ssd (μm 2 ) a toner for developing electrostatic images that satisfies the following formulas (1) and (2): Equation (1): 0.03≦Sac≦0.20 Formula (2): Ssd≦0.10 <2> Satisfying the following formula (11) <1> 2. The toner for developing electrostatic images according to claim 1 . Equation (11): 0.08≦Sac≦0.16 <3> Satisfying the following formula (21) <1> or <2> 2. The toner for developing electrostatic images according to claim 1 . Formula (21) Ssd≦0.07 <4> When a cross-section of the toner particle is observed, the ratio of the area of the vinyl resin particle to the area of the toner particle is more than 0.15 and 0.40 or less. <1> ~ <3> 2. The toner for developing an electrostatic image according to claim 1 . <5> The vinyl resin particles have a volume average particle size of 100 nm or more and 300 nm or less. <1> ~ <4> 2. The toner for developing an electrostatic image according to claim 1 . <6> The glass transition temperature of the vinyl resin particles is 0° C. or more and 30° C. or less. <1> ~ <5> 2. The toner for developing an electrostatic image according to claim 1 . <7> In a cross-sectional observation of the toner particle, the number ratio of the vinyl-based resin particles observed to be overlapped is 50% or less of all the vinyl-based resin particles observed. <1> ~ <6> 2. The toner for developing an electrostatic image according to claim 1 . <8> In a cross-sectional observation of the toner particle, the length of a portion of the contour of the toner particle that overlaps with the vinyl resin particle is 5% or less of the length of the contour of the toner particle. <1> ~ <7> 2. The toner for developing an electrostatic image according to claim 1 . <9> In a cross-sectional observation of the toner particles, the average equivalent circle diameter of the vinyl resin particles observed is 400 nm or less. <1> ~ <8> 2. The toner for developing an electrostatic image according to claim 1 . <10> the vinyl-based resin particles are styrene-(meth)acrylate copolymer particles, a ratio Wa(B) (mol%) of structural units derived from the (meth)acrylate in the entire styrene-(meth)acrylate copolymer particle; and the ratio Wa(S) (mol %) of the structural units derived from the (meth)acrylate on the surface of the styrene-(meth)acrylate copolymer particle, 2≦Wa(S)-Wa(B)≦20 <1> ~ <9> 2. The toner for developing an electrostatic image according to claim 1 . <11> a proportion Wa(S) (mol %) of structural units derived from the (meth)acrylate on the surface of the styrene-(meth)acrylate copolymer particle satisfies 40≦Wa(S)≦80; <10> 2. The toner for developing electrostatic images according to claim 1 . <12> the vinyl-based resin particles are styrene-(meth)acrylate copolymer particles, A ratio Ws(B) (mol%) of structural units derived from the styrene to the entire styrene-(meth)acrylate copolymer particle; and the proportion Ws(S) (mol%) derived from the styrene on the surface of the styrene-(meth)acrylate copolymer particle, 2≦Ws(S)-Ws(B)≦20 <1> ~ <9> 2. The toner for developing an electrostatic image according to claim 1 . <13> The proportion Ws(S) (mol %) derived from styrene on the surface of the styrene-(meth)acrylate copolymer particle satisfies 40≦Ws(S)≦80. <12> 2. The toner for developing electrostatic images according to claim 1 . <14> the solubility parameter SP(sa) of the surface of the vinyl resin particle; The relationship with the solubility parameter SP(ap) of the binder resin is as follows: |SP(ap)-SP(sa)|≦1.0 <10> or <11> 2. The toner for developing electrostatic images according to claim 1 . <15> the solubility parameter SP(sa) of the surface of the vinyl resin particle; The relationship with the solubility parameter SP(ap) of the binder resin is as follows: |SP(ap)-SP(sa)|≦1.0 <12> or <13> 2. The toner for developing electrostatic images according to claim 1 . <16> The binder resin contains an amorphous polyester resin. The amorphous polyester resin is a condensation polymer of a polycarboxylic acid including isophthalic acid and a polyhydric alcohol, The ratio of isophthalic acid to the polycarboxylic acid is 10 mol % or more and 50 mol % or less. <10> , <11> or <14> 2. The toner for developing electrostatic images according to claim 1 . <17> The binder resin contains an amorphous polyester resin. The amorphous polyester resin is a condensation polymer of a polycarboxylic acid including isophthalic acid and a polyhydric alcohol, The ratio of isophthalic acid to the polycarboxylic acid is 10 mol % or more and 50 mol % or less. <12> , <13> or <15> 2. The toner for developing electrostatic images according to claim 1 . <18> The vinyl resin particles are resin particles having a crosslinked structure. <1> ~ <17> 2. The toner for developing an electrostatic image according to claim 1 . <19> <1> ~ <18> 2. An electrostatic image developer comprising the toner for developing electrostatic images according to claim 1. <20> <1> ~ <18> The toner for developing an electrostatic image according to any one of claims 1 to 4 is contained in the electrostatic image developing device. The toner cartridge is attached to and detached from the forming device. <21> <19> and a developing means for developing an electrostatic image formed on a surface of an image carrier by the electrostatic image developer into a toner image, the process cartridge being detachably mountable to an image forming apparatus. <22> An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; <19> a developing means for developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising: <23> a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; <19> a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to claim 1; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1, Effect of the Invention
[0006] <1> According to the invention, in a toner for developing an electrostatic image, which contains toner particles containing a binder resin, a colorant, and vinyl resin particles, when a cross-section of a toner particle is observed, the area Sa (μm) of a Voronoi polygon obtained by Voronoi division using the geometric center of the vinyl resin particle as a generating point is determined. 2 ) is measured, the median value Sac (μm 2 ), the standard deviation of the area Sa of the Voronoi polygon is Ssd (μm 2 ), a toner for developing electrostatic images is provided which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under high temperature and high humidity environments, compared to a case in which the above formulas (1) and (2) are not satisfied.
[0007] <2> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high-temperature and high-humidity environment, as compared to a case where formula (11) is not satisfied. <3> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine-line resolution that occurs when images are repeatedly formed in a high-temperature, high-humidity environment, as compared with a case in which formula (21) is not satisfied.
[0008] <4> According to the invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under a high temperature and high humidity environment, as compared to a case in which the ratio of the area of the vinyl resin particles to the area of the toner particles is 0.15 or less or exceeds 0.40 in cross-sectional observation of the toner particles. <5> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under a high temperature and high humidity environment, as compared to when the volume average particle size of the vinyl resin particles is less than 100 nm or exceeds 300 nm. <6> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under a high temperature and high humidity environment, as compared with the case where the glass transition temperature of the vinyl resin particles is lower than 0°C or higher than 30°C.
[0009] <7> According to the invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under a high temperature and high humidity environment, compared to a case where the number ratio of vinyl resin particles observed to overlap in cross-sectional observation of a toner particle exceeds 50% by number of all vinyl resin particles observed. <8> According to the invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under high temperature and high humidity environments, compared to when the length of the portion of the contour of a toner particle that overlaps with a vinyl resin particle exceeds 5% of the contour length of the toner particle upon cross-sectional observation of the toner particle. <9> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under a high temperature and high humidity environment, as compared to when the average equivalent circular diameter of vinyl resin particles observed in cross-sectional observation of the toner particles exceeds 400 nm.
[0010] <10> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, as compared to a case where 2≦Wa(S)−Wa(B)≦20 is not satisfied. <11> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, as compared to a case where 40≦Wa(S)≦80 is not satisfied.
[0011] <12> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, as compared to a case where 2≦Ws(S)−Ws(B)≦20 is not satisfied. <13> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, as compared to a case where 40≦Ws(S)≦80 is not satisfied.
[0012] <14> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under a high temperature and high humidity environment, as compared to a case where |SP(ap)-SP(sa)|≦1.0 is not satisfied. <15> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under a high temperature and high humidity environment, as compared to a case where |SP(ap)-SP(sa)|≦1.0 is not satisfied.
[0013] <16> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under high temperature and high humidity environments, as compared to when the ratio of isophthalic acid to polyvalent carboxylic acid is less than 0.1 mol % or exceeds 0.5 mol %. <17> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under high temperature and high humidity environments, as compared to when the ratio of isophthalic acid to polyvalent carboxylic acid is less than 0.1 mol % or exceeds 0.5 mol %.
[0014] <18> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under a high temperature and high humidity environment, as compared to when the vinyl resin particles have a non-crosslinked structure.
[0015] <19> , <20> , <21> , <22> or <23> According to the invention, in a toner for developing an electrostatic image, which contains toner particles containing a binder resin, a colorant, and vinyl resin particles, when a cross-section of a toner particle is observed, the area Sa (μm) of a Voronoi polygon obtained by Voronoi division using the geometric center of the vinyl resin particle as a generating point is determined. 2 ) is measured, the median value Sac (μm 2 ), the standard deviation of the area Sa of the Voronoi polygon is Ssd (μm 2 ), the present invention provides an electrostatic image developer, a toner cartridge, a process cartridge, an image forming apparatus, or an image forming method which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, compared to a case in which a toner for developing electrostatic images which does not satisfy the above formulas (1) and (2) is provided. [Brief description of the drawings]
[0016] [Figure 1] 1 is a schematic diagram illustrating an image forming apparatus according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a schematic diagram illustrating a process cartridge according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described as an example. The description and examples are merely illustrative of the embodiment, and are not intended to limit the scope of the present invention. In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples.
[0018] Each component may contain multiple types of the corresponding substance. When referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the amount refers to the total amount of those multiple substances present in the composition, unless otherwise specified. The term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes as long as the intended effect of the process is achieved.
[0019] <Toner for developing electrostatic images> The toner for developing electrostatic images according to the present embodiment (hereinafter, the toner for developing electrostatic images may also be simply referred to as "toner") contains toner particles containing a binder resin and vinyl resin particles. In the cross-sectional observation of the toner particles, the area Sa (μm 2 ) is measured, the median value Sac (μm 2 ), the standard deviation of the area Sa of the Voronoi polygon is Ssd (μm 2 ), the following equations (1) and (2) are satisfied.
[0020] The toner according to the present embodiment, by virtue of the above-mentioned constitution, suppresses the deterioration of fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment (for example, an environment of 28° C. and 85% RH). The reason for this is presumed to be as follows.
[0021] In recent years, with the demand for higher image quality and the diversification of operating environments, there is an increasing demand for printers that are less susceptible to the effects of the operating environment and that maintain high-definition image quality even when images are repeatedly formed. One of the issues is the need to suppress the decrease in fine line resolution when images are repeatedly formed under high temperature and high humidity conditions.
[0022] Here, when images are repeatedly formed, the toner consumption amount in the developing device is small, and the supply of additional toner is small, so the toner in the developing device continues to be subjected to mechanical load due to stirring for charging, which makes the toner particles more likely to crack or chip. Conventionally, in order to prevent toner particles from cracking or chipping due to mechanical load, techniques have been known in which internal additive particles such as resin particles or rubber particles are added to the toner particles or a sea-island structure is formed using two types of binder resins to increase the durability of the toner particles. However, although these toner particles suppress cracking or chipping, fine line resolution may decrease. In toner particles containing internal additive particles or toner particles having a sea-island structure, the internal additive particles and the island portions of the sea-island structure are poorly dispersed, causing a misalignment between the "mass center of gravity" and the "geometric center" of the toner particles.
[0023] Therefore, when images are repeatedly formed under high temperature and high humidity conditions, the external additives tend to be embedded in the toner particles due to mechanical load. When the external additives are embedded, the charge of the toner decreases, and the electrostatic adhesion decreases. In addition to the state where the charge is decreased, if the "mass center of gravity" and the "geometric center" of the toner particles are misaligned and eccentric, the toner tends to roll and move slightly at the edge of the toner image formed on the intermediate transfer body or recording medium. As a result, it is thought that the fine line resolution decreases. For example, when the thinnest line width that can be formed by an image forming device with a resolution of 1200 dpi is 20 μm, and toner with a particle diameter of 5.2 μm rolls half a revolution, the movement distance is 8 μm (= 2πr / 2 = (2 × 3.14 × (5.2 / 2)) / 2). In other words, there is a possibility that the resolution of thin lines may decrease to that extent.
[0024] In contrast, in the toner according to the present embodiment, in toner particles containing a binder resin, a colorant, and vinyl resin particles, when a cross-section of the toner particle is observed, the area Sa (μm 2 ), the median of the area Sa of the Voronoi polygon is Sac (μm2), and the standard deviation of the area Sa of the Voronoi polygon is Ssd (μm 2 ) satisfy the above formulas (1) and (2). This makes the dispersion state of the resin particles in the toner particles nearly uniform. This prevents the toner particles from cracking or chipping, and also makes it difficult for the "mass center of gravity" and "geometric center" of the toner particles to shift. Even if images are repeatedly formed under high temperature and high humidity conditions, causing a decrease in the charge of the toner, the toner is prevented from rolling at the edge of the toner image.
[0025] In addition, toner particles with rubber particles having rubber elasticity added thereto have low affinity with the binder resin of the toner particles due to the adhesiveness of the rubber particles and the lack of an acid value, making it difficult to improve dispersibility. Here, rubber particles are particles that have rubber elasticity at room temperature (25°C), and "rubber elasticity" refers to the property of being easily deformed by a small external force, exhibiting high elongation (100% or more), and recovering to almost the original shape in a short time when the external force is removed. In contrast, vinyl resin particles have low adhesion and an acid value, and therefore have a high affinity with the binder resin of the toner particles, making it easier to improve dispersibility, and the dispersion state of the resin particles in the toner particles can be made nearly uniform.
[0026] From the above, it is presumed that the toner according to this embodiment suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment.
[0027] The toner according to this embodiment will be described in detail below.
[0028] The toner according to the present embodiment is configured to contain toner particles and, if necessary, an external additive.
[0029] (Cross-sectional aspect of toner particle) In the toner according to the present embodiment, when a cross-section of a toner particle is observed, the area Sa (μm 2 ) is measured, the median value Sac (μm 2 ), the standard deviation of the area Sa of the Voronoi polygon is Ssd (μm 2 ), the following equations (1) and (2) are satisfied. Equation (1): 0.03≦Sac≦0.20 Formula (2): Ssd≦0.10
[0030] If the median Sac of the area Sa of the Voronoi polygon is small, the number of vinyl resin particles in the toner becomes too large, the probability of the vinyl resin particles coming into contact with each other increases, the dispersion state of the vinyl resin particles becomes poor, and the misalignment between the "mass center of gravity" and the "geometric center" of the toner particles becomes large, resulting in eccentricity. On the other hand, if the median Sac of the area Sa of the Voronoi polygon is large, the number of vinyl resin particles in the toner is small, the dispersion state of the vinyl resin particles becomes poor, and the misalignment between the "mass center of gravity" and the "geometric center" of the toner particles becomes large, resulting in eccentricity. In addition, if the standard deviation of the area Sa of the Voronoi polygon and the standard deviation of Ssd are large, the deviation between the "mass center of gravity" and the "geometric center" of the toner particle becomes large, resulting in eccentricity. Therefore, by satisfying the formulas (1) and (2), the toner can be prevented from rolling at the edge of the toner image even when images are repeatedly formed in a high-temperature and high-humidity environment, and as a result, the deterioration of fine-line resolution can be prevented.
[0031] In the toner according to this embodiment, it is preferable that the following formulae (11) and (21) are satisfied, and it is more preferable that the following formulae (12) and (22) are satisfied. Equation (11): 0.08≦Sac≦0.16 Formula (21): Ssd≦0.07
[0032] The median Sac and standard deviation Ssd of the area Sa of a Voronoi polygon are measured as follows: First, all the vinyl resin particles present within the area of one toner particle are divided into Voronoi polygons using the centers of gravity of the particles as kernel points (i.e., a perpendicular bisector is drawn on the line connecting adjacent kernel points to divide the area nearest to each kernel point), and the areas Sa of all the Voronoi polygons formed are measured. Specifically, the toner is embedded in an embedding resin, and a section with a thickness of 0.2 μm to 0.3 μm is prepared using a cryotome. The observation surface of the prepared section is stained with ruthenium tetroxide, and an image of the observation surface is taken at a magnification of 20,000 times using a scanning electron microscope (S-4700: manufactured by Hitachi High-Technologies Corporation). Here, for example, vinyl resin particles can be identified based on the difference in the ease of dyeing between the binder resin and the vinyl resin particles. The area Sa of the Voronoi polygon of one toner particle is measured in the captured image using image processing software (ImageJ: manufactured by the National Institutes of Health, USA). The area Sa of the Voronoi polygon is measured by these operations for 200 toner particles, and the median Sac and standard deviation Ssd of the Voronoi polygon area are calculated.
[0033] The procedure for measuring the area Sa of a Voronoi polygon using image processing software (ImageJ: manufactured by the National Institutes of Health, USA) is as follows. 1. Define the relationship between the number of pixels on the image and the actual distance by selecting Analyze → Set Scale. For example, if 144 pixels corresponds to 1.5 μm, enter Distance in Pixes: 144, Known distance: 1.5, and check the Global checkbox. 2. Select Image→Type→8-bit. 3. Select Image→Adjust→Threshold, check Dark background, and click the Auto button. 4. Remove speckled image noise by going to Process→Noise→Despeckle. 5. Using Process → Binary → Watershed, vinyl resin particles that are observed overlapping are separated by a process that emphasizes the contours of the vinyl resin particles. 6. Using the Process→Binary→Voronoi process, a Voronoi polygon is created with the "geometric center" of the vinyl resin particle as the generating point. 7. Remove the lines that originate from the outermost vinyl resin particles and do not form Voronoi polygons. 8. Select Image→Type→8-bit. 8. Use Image→Adjust→Threshold to adjust the edges of the Voronoi polygons so that they turn red. 9. Use the Edit→Invert process to invert the edges of the Voronoi polygons so that they become white. 9. Calculate the area Sa of the Voronoi polygon by processing Analyze → AnalyzeParticle (size: 0-Infinity, Circularity: 0.00-1.00, Show: Outlines).
[0034] -Area of vinyl resin particles- In observing a cross section of a toner particle, the ratio of the area of the vinyl resin particles to the area of the toner particle is preferably more than 0.15 and 0.40 or less, more preferably 0.20 or more and 0.30 or less, and further preferably 0.22 or more and 0.28 or less. If the ratio of the area of the vinyl resin particles is more than 0.15, cracking or chipping of the toner particles is easily suppressed. On the other hand, if the ratio of the area of the vinyl resin particles is 0.40 or less, the "mass center of gravity" and the "geometric center" of the toner particles are less likely to shift, and eccentricity is suppressed. Therefore, fine line resolution is easily suppressed.
[0035] The area of the vinyl resin particles is measured as follows. In the same manner as in the measurement of the area Sa of the Voronoi polygon, a black-and-white inverted image is obtained so that the vinyl resin particles in the cross section of the toner particle are white. Next, the ratio of the area of the vinyl resin particles to the area of the toner particle is calculated from the image. This operation is performed for 200 toner particles, and the arithmetic average is calculated.
[0036] -Number ratio of vinyl resin particles observed overlapping- The number ratio of vinyl resin particles observed overlapping is preferably 50% or less by number of all vinyl resin particles observed, more preferably 45% or less by number, even more preferably 35% or less by number, and ideally 0% by number. When the number ratio of vinyl resin particles observed to overlap is within the above range, the dispersibility of the styrene-(meth)acrylate copolymer particles in the toner particles is increased, the "mass center of gravity" and the "geometric center" of the toner particles are less likely to shift, and eccentricity is suppressed. Therefore, fine line resolution is easily suppressed.
[0037] The number ratio of vinyl resin particles observed to be overlapped is measured as follows. In the same manner as in the measurement method of the area Sa of the Voronoi polygon, a photographed image is obtained in which the vinyl resin particles in the cross section of the toner particle are inverted black and white so that they are white. Next, the total number of vinyl resin particles is counted from the photographed image, and the number of vinyl resin particles observed overlapping among them is counted. Then, the ratio of the number of vinyl resin particles observed overlapping to the total vinyl resin particles observed is calculated. This operation is carried out for 200 toner particles, and the arithmetic average is calculated.
[0038] -The ratio of the length of the part of the toner particle's contour that overlaps with the vinyl resin particle- In observing the cross section of a toner particle, the length of the part of the contour line of the toner particle that overlaps with the vinyl resin particle is preferably 5% or less of the contour line length of the toner particle, more preferably 4% or less, and even more preferably 3.5% or less. The contour line length of the toner particle is ideally 0%. When the contour length of the toner particles is 5% or less, the amount of exposed vinyl resin particles on the surface of the toner particles is reduced. As a result, the number of protrusions due to the exposed vinyl resin particles in the toner particles is reduced, and the rolling of the toner caused by the protrusions is suppressed. Therefore, the fine line resolution is easily suppressed.
[0039] The ratio of the length of the portion of the contour line of the toner particle that overlaps with the vinyl resin particle (i.e., the ratio of the length of the portion of the contour line of the toner particle that overlaps with the vinyl resin particle to the length of the contour line of the toner particle) is measured as follows. In the same manner as in the measurement method for the area Sa of the Voronoi polygon, a black-and-white inverted image is obtained so that the vinyl resin particles in the cross section of the toner particle are white. Next, the ratio of the length of the part of the contour line of the toner particle that overlaps with the vinyl resin particle is calculated from the captured image. This operation is performed for 200 toner particles, and the arithmetic average is calculated.
[0040] - Average circle equivalent diameter of vinyl resin particles observed in toner cross section observation - In observing a cross section of a toner particle, the average equivalent circle diameter of the vinyl resin particles observed is preferably 400 nm or less, and more preferably 300 nm or less. When the average equivalent circular diameter of the observed vinyl resin particles is 400 nm or less, the particle size of the vinyl resin particles becomes appropriate, cracking or chipping of the toner particles is suppressed, and the "mass center of gravity" and the "geometric center" of the toner particles are less likely to shift, suppressing eccentricity, which makes it easier to suppress fine line resolution. Here, the circle-equivalent diameter of a vinyl-based resin particle is the circle-equivalent diameter of a single vinyl-based resin particle when a single vinyl-based resin particle is observed alone, and is the circle-equivalent diameter calculated from the area of the region surrounded by the outlines of multiple overlapping vinyl-based resin particles when multiple vinyl-based resin particles are observed overlapping each other.
[0041] The difference between the average equivalent circle diameter of the vinyl resin particles and the average primary particle diameter of the vinyl resin particles is preferably 50 nm or less, more preferably 40 nm or less, and even more preferably 30 nm or less. When the difference between the average circle equivalent diameter of the vinyl resin particles and the average primary particle diameter of the vinyl resin particles is 50 nm or less, the dispersibility of the styrene-(meth)acrylate copolymer particles in the toner particles is increased, the "mass center of gravity" and the "geometric center" of the toner particles are less likely to shift, and eccentricity is suppressed. Therefore, fine line resolution is easily suppressed.
[0042] The average equivalent circular diameter of the observed vinyl resin particles is measured as follows. In the same manner as in the measurement of the area Sa of the Voronoi polygon, a black-and-white inverted image is obtained so that the vinyl resin particles in the cross section of the toner particle are white. Next, the average circle equivalent diameter of the vinyl resin particles observed is calculated from the image. This operation is performed on 200 toner particles, and the arithmetic average is calculated.
[0043] (Composition of toner particles) The toner particles contain a binder resin and vinyl resin particles, and may contain a colorant, a release agent, and other additives, if necessary.
[0044] -Binding resin- Examples of the binder resin include vinyl resins made of homopolymers of monomers such as styrenes (e.g., styrene, parachlorostyrene, α-methylstyrene, etc.), (meth)acrylic acid esters (e.g., methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, 2-ethylhexyl methacrylate, etc.), ethylenically unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), vinyl ethers (e.g., vinyl methyl ether, vinyl isobutyl ether, etc.), vinyl ketones (vinyl methyl ketone, vinyl ethyl ketone, vinyl isopropenyl ketone, etc.), and olefins (e.g., ethylene, propylene, butadiene, etc.), or copolymers of two or more of these monomers. Examples of the binder resin include non-vinyl resins such as epoxy resins, polyester resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosin, mixtures of these with the vinyl resins, and graft polymers obtained by polymerizing vinyl monomers in the coexistence of these. These binder resins may be used alone or in combination of two or more kinds.
[0045] The binder resin is preferably a polyester resin. The polyester resin may be, for example, a known amorphous polyester resin. The polyester resin may be used in combination with a crystalline polyester resin. However, the content of the crystalline polyester resin is preferably in the range of 2% by mass to 40% by mass (preferably 5% by mass to 25% by mass) based on the total binder resin.
[0046] The "crystalline" nature of a resin refers to the presence of a clear endothermic peak rather than a stepwise change in the amount of endothermic heat in differential scanning calorimetry (DSC); specifically, the half-width of the endothermic peak is within 10°C when measured at a heating rate of 10 (°C / min). On the other hand, the term "amorphous" for a resin refers to a half-width exceeding 10° C., a stepwise change in endothermic heat quantity, or no clear endothermic peak being observed.
[0047] Amorphous polyester resin The amorphous polyester resin may be, for example, a condensation polymer of a polyvalent carboxylic acid and a polyhydric alcohol. The amorphous polyester resin may be a commercially available product or a synthesized product.
[0048] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, sebacic acid, etc.), alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). Among these, aromatic dicarboxylic acids are preferable as polyvalent carboxylic acids. Polycarboxylic acids are trivalent or higher carboxylic acids that have a crosslinked or branched structure, along with dicarboxylic acids. Examples of trivalent or higher carboxylic acids include trimellitic acid, pyromellitic acid, anhydrides thereof, and lower alkyl esters thereof (for example, having 1 to 5 carbon atoms). The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0049] Examples of polyhydric alcohols include aliphatic diols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, etc.), alicyclic diols (e.g., cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, etc.), and aromatic diols (e.g., ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, etc.). Among these, examples of polyhydric alcohols include aromatic diols and alicyclic diols, and more preferably aromatic diols. As the polyhydric alcohol, a polyhydric alcohol having a crosslinked or branched structure of three or more may be used in combination with the diol. Examples of the polyhydric alcohol having a trihydric or higher valence include glycerin, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.
[0050] Here, when the vinyl resin particles are styrene-(meth)acrylate copolymer particles, the amorphous polyester resin is a condensation polymer of a polycarboxylic acid containing isophthalic acid and a polyhydric alcohol, and the ratio of isophthalic acid to the polycarboxylic acid is preferably 10 mol% or more and 50 mol% or less, more preferably 15 mol% or more and 40 mol% or less. When two or more kinds of amorphous polyester resins are used in combination, the weighted average ratio of isophthalic acid is set to be within the above range. When the ratio of isophthalic acid to polycarboxylic acid is within the above range, the dispersibility of styrene-(meth)acrylate copolymer particles in toner particles is increased, and the "mass center of gravity" and the "geometric center" of the toner particles are less likely to shift, suppressing eccentricity. Therefore, fine line resolution is easily suppressed. The reason for this is assumed to be as follows. The benzene ring contained in the skeleton of the structure derived from isophthalic acid in the amorphous polyester resin and the benzene ring contained in the styrene skeleton in the styrene (meth)acrylate copolymer are stabilized by π-π stacking, and the affinity between the polyester and the styrene (meth)acrylate copolymer resin particles is improved. This is because isophthalic acid has a carbonyl group at the meta position and is biased, so the benzene ring of styrene is easily approached. On the other hand, there is terephthalic acid as a polycarboxylic acid having a similar structure, but since the carbonyl group is at the para position, the benzene ring of styrene is difficult to approach due to steric hindrance, and does not contribute to improving the affinity between the amorphous polyester resin and the styrene (meth)acrylate copolymer resin particles. Therefore, when the ratio of isophthalic acid to the polycarboxylic acid is within the above range, the dispersibility of the styrene-(meth)acrylate copolymer particles in the toner particles is increased, and the fine line resolution is easily suppressed.
[0051] The glass transition temperature (Tg) of the amorphous polyester resin is preferably 50°C or higher and 80°C or lower, and more preferably 50°C or higher and 65°C or lower. The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC), more specifically, from the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics."
[0052] The weight average molecular weight (Mw) of the amorphous polyester resin is preferably 5,000 or more and 1,000,000 or less, and more preferably 7,000 or more and 500,000 or less. The number average molecular weight (Mn) of the amorphous polyester resin is preferably 2,000 or more and 100,000 or less. The molecular weight distribution Mw / Mn of the amorphous polyester resin is preferably 1.5 or more and 100 or less, and more preferably 2 or more and 60 or less. The weight average molecular weight and number average molecular weight are measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120GPC as the measuring device, a Tosoh TSKgel SuperHM-M (15 cm) column, and THF solvent. The weight average molecular weight and number average molecular weight are calculated from the measurement results using a molecular weight calibration curve created with a monodisperse polystyrene standard sample.
[0053] The amorphous polyester resin can be obtained by a known manufacturing method, for example, by carrying out the reaction while removing water and alcohol generated during condensation by setting the polymerization temperature to 180° C. or higher and 230° C. or lower, and reducing the pressure in the reaction system as necessary. If the raw material monomer is not soluble or compatible at the reaction temperature, a high boiling point solvent may be added as a solubilizing agent to dissolve it. In this case, the polycondensation reaction is carried out while distilling off the solubilizing agent. If a monomer with poor compatibility is present, it is recommended that the monomer with poor compatibility is condensed in advance with the acid or alcohol to be polycondensed, and then polycondensed with the main component.
[0054] Crystalline polyester resin The crystalline polyester resin may be, for example, a polycondensate of a polyvalent carboxylic acid and a polyhydric alcohol. The crystalline polyester resin may be a commercially available product or a synthesized product. Here, the crystalline polyester resin has an aromatic group so as to easily form a crystalline structure. A polycondensation product using a polymerizable monomer having a linear aliphatic chain is preferred over a polymerizable monomer.
[0055] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,18-octadecanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent carboxylic acid include aromatic carboxylic acids (e.g., 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, etc.), their anhydrides, and their lower alkyl esters (e.g., carbon number 1 to 5). As the polyvalent carboxylic acid, a dicarboxylic acid having a sulfonic acid group and a dicarboxylic acid having an ethylenic double bond may be used in combination with these dicarboxylic acids. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0056] Examples of polyhydric alcohols include aliphatic diols (for example, straight-chain aliphatic diols having 7 to 20 carbon atoms in the main chain). Examples of aliphatic diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanedecanediol. Among these, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are preferred as aliphatic diols. The polyhydric alcohol may be a trihydric or higher alcohol having a crosslinked or branched structure in combination with the diol. Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.
[0057] Here, the polyhydric alcohol has an aliphatic diol content of 80 mol % or more, preferably 90 mol % or more.
[0058] The melting temperature of the crystalline polyester resin is preferably 50°C or higher and 100°C or lower, more preferably 55°C or higher and 90°C or lower, and even more preferably 60°C or higher and 85°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K7121-1987 "Method for measuring transition temperature of plastics."
[0059] The weight average molecular weight (Mw) of the crystalline polyester resin is preferably 6,000 or more and 35,000 or less.
[0060] The crystalline polyester resin can be obtained by a known manufacturing method, for example, in the same manner as the amorphous polyester.
[0061] The content of the binder resin is, for example, preferably from 40% by mass to 95% by mass, more preferably from 50% by mass to 90% by mass, and even more preferably from 60% by mass to 85% by mass, based on the total amount of the toner particles.
[0062] -Vinyl resin particles- The vinyl resin particles are resin particles of a homopolymer or copolymer of a vinyl monomer. Examples of vinyl resin particles include styrene resins (polystyrene, α-polymethylstyrene, etc.), (meth)acrylic resins (polymethyl methacrylate, polyacrylonitrile, etc.), and copolymers thereof. These resins may be used alone or in combination of two or more types, as required. From the viewpoints of improving dispersibility in toner particles and suppressing a decrease in fine line resolution, styrene-(meth)acrylic copolymer particles are preferred as the vinyl resin particles.
[0063] Here, the styrene-(meth)acrylic copolymer may be a copolymer obtained by copolymerizing at least a styrene monomer and a (meth)acrylic monomer. The styrene-(meth)acrylic resin may be a copolymer obtained by copolymerizing other monomers in addition to the styrene monomer and the (meth)acrylic monomer. Here, the term "(meth)acrylic" and the like includes both "acrylic" and "methacrylic", and the like.
[0064] The styrene monomer is a monomer having a styrene skeleton. Specific examples of the styrene monomer include styrene, vinylnaphthalene, alkyl-substituted styrenes such as α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, and pn-dodecylstyrene, aryl-substituted styrenes such as p-phenylstyrene, alkoxy-substituted styrenes such as p-methoxystyrene, halogen-substituted styrenes such as p-chlorostyrene, 3,4-dichlorostyrene, 4-fluorostyrene, and 2,5-difluorostyrene, and nitro-substituted styrenes such as m-nitrostyrene, o-nitrostyrene, and p-nitrostyrene. Among these, from the viewpoints of improving dispersibility in toner particles and suppressing a decrease in fine line resolution, styrene, p-ethylstyrene, pn-butylstyrene, and the like are preferred as styrene-based monomers. These styrene monomers may be used alone or in combination of two or more.
[0065] The (meth)acrylic monomer is a monomer having a (meth)acryloyl group. Specific examples of the (meth)acrylic monomer include n-methyl (meth)acrylate, n-ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, n-lauryl (meth)acrylate, n-tetradecyl (meth)acrylate, and n-hexa (meth)acrylate. decyl, n-octadecyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, amyl (meth)acrylate, neopentyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, (meth)acrylic acid alkyl esters such as stearyl acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and isobornyl (meth)acrylate; di(meth)acrylic acid esters such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, pentanediol di(meth)acrylate, hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, and decanediol di(meth)acrylate; (meth)acrylic acid carboxy-substituted alkyl esters such as β-carboxyethyl (meth)acrylate; (meth)acrylic acid hydroxy-substituted alkyl esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; (Meth)acrylic acid alkoxy-substituted alkyl esters such as 2-methoxyethyl (meth)acrylate; and the like. Examples of the (meth)acrylic monomer include (meth)acrylic acid in addition to the above-mentioned (meth)acrylic acid esters. Among these, from the viewpoint of improving dispersibility in toner particles and suppressing deterioration of fine line resolution, (meth)acrylic acid esters having an alkyl group having 2 to 14 carbon atoms (preferably 2 to 10 carbon atoms, more preferably 3 to 8 carbon atoms) are preferred. These (meth)acrylic monomers may be used alone or in combination of two or more.
[0066] The other monomers include, for example, crosslinking agents for imparting a crosslinked structure. Examples of the crosslinking agent for crosslinking include aromatic polyvinyl compounds such as divinylbenzene and divinylnaphthalene; polyvinyl esters of aromatic polyvalent carboxylic acids such as divinyl phthalate, divinyl isophthalate, divinyl terephthalate, divinyl homophthalate, divinyl trimesate, trivinyl trimesate, divinyl naphthalenedicarboxylate, and divinyl biphenylcarboxylate; divinyl esters of nitrogen-containing aromatic compounds such as divinyl pyridinedicarboxylate; vinyl esters of unsaturated heterocyclic carboxylic acids such as vinyl pyromucate, vinyl furancarboxylate, vinyl pyrrole-2-carboxylate, and vinyl thiophenecarboxylate; and (meth)acrylic esters of linear polyhydric alcohols such as butanediol methacrylate, hexanediol acrylate, octanediol methacrylate, decanediol acrylate, and dodecanediol methacrylate. Acid esters; (meth)acrylic acid esters of branched, substituted polyhydric alcohols such as neopentyl glycol dimethacrylate and 2-hydroxy, 1,3-diacryloxypropane; polyvinyl esters of polyvalent carboxylic acids such as polyethylene glycol di(meth)acrylate, polypropylene polyethylene glycol di(meth)acrylate, divinyl succinate, divinyl fumarate, vinyl maleate, divinyl maleate, divinyl diglycolate, vinyl itaconate, divinyl itaconate, divinyl acetone dicarboxylate, divinyl glutarate, divinyl 3,3'-thiodipropionate, divinyl trans-aconitate, trivinyl trans-aconitate, divinyl adipate, divinyl pimelate, divinyl suberate, divinyl azelaate, divinyl sebacate, divinyl dodecanedioate, and divinyl brassylate. The crosslinking agent may be used alone or in combination of two or more.
[0067] Here, the styrene-(meth)acrylic copolymer particles may have a relationship between the proportion Wa(B) (mol %) of structural units derived from the (meth)acrylate in the entire styrene-(meth)acrylate copolymer particle and the proportion Wa(S) (mol %) of structural units derived from the (meth)acrylate on the surface of the styrene-(meth)acrylate copolymer particle such that 2≦Wa(S)-Wa(B)≦20 (preferably 5≦Wa(S)-Wa(B)≦15). In this embodiment, the proportion Wa(S) (mol %) of structural units derived from (meth)acrylate on the surface of the styrene-(meth)acrylate copolymer particle preferably satisfies 40≦Wa(S)≦80, and more preferably 45≦Wa(S)≦75. When Wa(S) and Wa(B) have the above relationship, the surface of the styrene-(meth)acrylic copolymer particle contains many structural units derived from (meth)acrylate. The styrene-(meth)acrylic copolymer particle having this structure has a low glass transition temperature on the surface and is soft, so that it is easy to absorb external impacts. This prevents the toner particles from cracking or chipping. Therefore, the fine line resolution is easily suppressed. The styrene-(meth)acrylic copolymer particles having this structure can be obtained, for example, by successively dropping emulsions having different ratios of styrene and (meth)acrylate in an emulsion polymerization method.
[0068] On the other hand, the styrene-(meth)acrylic copolymer particles may have a relationship between the proportion Ws(B) (mol %) of structural units derived from styrene in the entire styrene-(meth)acrylate copolymer particle and the proportion Ws(S) (mol %) of the structural units derived from styrene on the surface of the styrene-(meth)acrylate copolymer particle that satisfies 2≦Ws(S)-Ws(B)≦20 (preferably satisfies 5≦Wa(S)-Wa(B)≦15). In this embodiment, the proportion Ws(S) (mol %) of styrene on the surface of the styrene-(meth)acrylate copolymer particle satisfies 40≦Ws(S)≦80, and more preferably 45≦Ws(S)≦75. When Ws(S) and Ws(B) have the above relationship, many structural units derived from styrene are present on the surface of the styrene-(meth)acrylic copolymer particles. The styrene-(meth)acrylic copolymer particles of this configuration suppress the low molecular weight components inside the particles from precipitating to the outside of the particles. Therefore, the decrease in the chargeability of the toner due to the precipitating of the unreacted low molecular weight components is suppressed. As a result, the rolling of the toner due to the decrease in the electrostatic adhesion of the toner is suppressed, and the fine line resolution is easily suppressed. The styrene-(meth)acrylic copolymer particles having this structure can be obtained, for example, by successively dropping emulsions having different ratios of styrene and (meth)acrylate in an emulsion polymerization method.
[0069] Here, the proportion of each constituent unit in the entirety and on the surface of the styrene-(meth)acrylic copolymer particle is measured as follows. The ratio of each structural unit of the styrene-(meth)acrylic copolymer particles is measured by preparing a tablet-shaped measurement sample by the KBr method and measuring it using a Kiyoki infrared absorption spectrophotometer. -1 and 698 cm due to the CH out-of-plane bending vibration of the benzene ring of the styrene structure. -1 Using the absorption of styrene, a resin consisting of only styrene and a resin consisting of only (meth)acrylate are prepared, and a calibration curve is created to calculate the amount from the magnitude of absorption. The proportion of each constituent unit is determined from the magnitude of absorption of the styrene-(meth)acrylic copolymer. The proportion of each structural unit on the surface of a styrene-(meth)acrylic copolymer particle is determined by performing surface composition analysis using an X-ray photoelectron spectroscopy (XPS) and calculating the ratio O(p) of oxygen to the total of carbon and oxygen elements in the styrene-(meth)acrylic copolymer particle using the following formula. O(p) = number of oxygen elements / (number of carbon elements + number of oxygen elements) In addition, a resin consisting only of (meth)acrylate is prepared, and the ratio O(a) of the oxygen element in the (meth)acrylate is determined in the same manner. From these measurement results, when the sum of styrene and (meth)acrylate is set to 1, the surface (meth)acrylate ratio Wa(S) and the surface styrene ratio Ws(S) can be calculated using the following formula. Wa(S)=O(p) / O(a) Ws(S)=1-(O(p) / O(a))
[0070] The vinyl resin particles preferably have a crosslinked structure. The vinyl resin particles have a crosslinked structure, which makes the resin particles more elastic. Therefore, the toner particles also tend to have elasticity. This makes it easier to prevent the toner particles from cracking or chipping. As a result, it makes it easier to prevent the fine line resolution from decreasing.
[0071] Here, the vinyl resin particles having a crosslinked structure means that the resin particles have a crosslinked structure between specific atoms in the polymer structure. Examples of the crosslinked structure of the vinyl resin particles include a crosslinked structure crosslinked by an ionic bond, a crosslinked structure crosslinked by a covalent bond, etc. Among these, it is preferable that the vinyl particles have a crosslinked structure crosslinked by a covalent bond.
[0072] The volume average particle size of the vinyl resin particles is preferably 100 nm or more and 300 nm or less, more preferably 120 nm or more and 250 nm or less, and even more preferably 140 nm or more and 220 nm or less. When the volume average particle size of the vinyl resin particles is within the above range, the particle size of the vinyl resin particles becomes appropriate, cracking or chipping of the toner particles is suppressed, and the "mass center of gravity" and the "geometric center" of the toner particles are less likely to shift, suppressing eccentricity, which makes it easier to suppress fine line resolution.
[0073] The volume average particle size of the vinyl resin particles is measured as follows. The vinyl resin particles are extracted from the toner by utilizing the difference in solubility in an organic solvent between the vinyl resin particles and organic matter other than the vinyl resin particles. For example, a method of extracting the vinyl resin particles from the toner includes a method of immersing the toner in a solvent that dissolves the binder resin but not the resin particles, and dissolving the binder resin in the solvent to extract the vinyl resin particles. When the toner contains inorganic substances such as external additives and colorants, the inorganic substances are separated by centrifugation to collect the vinyl resin particles. The particle size distribution of the vinyl resin particles obtained is obtained by measuring with a laser wave type particle size distribution analyzer (e.g., LS-13 320 manufactured by Beckman Coulter, Inc.). The particle size distribution obtained is used to divide the particle size range (channel), and the cumulative distribution is subtracted from the small particle size side for the volume, and the volume average particle size D50v is defined as the cumulative 50% of the total particles.
[0074] The glass transition temperature Tg of the vinyl resin particles is preferably 0°C or higher and 30°C or lower, and more preferably 5°C or higher and 25°C or lower. When the glass transition temperature Tg of the vinyl resin particles is within the above range, the toner particles have appropriate flexibility, and while deformation is suppressed, cracking or chipping of the toner particles is suppressed, and the "mass center of gravity" and the "geometric center" of the toner particles are unlikely to shift, suppressing eccentricity, which makes it easier to suppress fine line resolution.
[0075] The glass transition temperature Tg of the vinyl resin particles is measured as follows. The vinyl resin particles are extracted from the toner by utilizing the difference in solubility in an organic solvent between the vinyl resin particles and organic matter other than the vinyl resin particles. For example, a method of extracting the vinyl resin particles from the toner includes a method of immersing the toner in a solvent that dissolves the binder resin but not the resin particles, and dissolving the binder resin in the solvent to extract the vinyl resin particles. When the toner contains inorganic substances such as external additives and colorants, the inorganic substances are separated by centrifugation to collect the vinyl resin particles. Pressure is applied to vinyl resin particles to create a disk-shaped sample with a thickness of 2 mm and a diameter of 8 mm, which is used as the measurement sample. The obtained disk-shaped sample is then sandwiched between parallel plates with a diameter of 8 mm, and the measurement temperature is raised from 10° C. to 150° C. at a rate of 2° C. / min with a strain of 0.1 to 100%, to perform dynamic viscoelasticity measurement under the following conditions: The storage modulus G' and loss tangent tanδ are determined from the curves of the storage modulus and loss modulus obtained by the measurement, and the peak temperature of the loss tangent tanδ is taken as the glass transition temperature Tg.
[0076] The relationship between the solubility parameter SP(sa) of the surface of the vinyl resin particle and the solubility parameter SP(ap) of the binder resin preferably satisfies |SP(ap)-SP(sa)|≦1.0, and more preferably |SP(ap)-SP(sa)|≦0.6. When the relationship between the solubility parameter SP(sa) of the surface of the vinyl resin particle and the solubility parameter SP(ap) of the binder resin satisfies the above relationship, the dispersibility of the vinyl resin particle is increased, the "mass center of gravity" and the "geometric center" of the toner particle are less likely to shift, and eccentricity is suppressed. Therefore, fine line resolution is easily suppressed.
[0077] The solubility parameter (SP value) is a value defined as a function of cohesive energy density by the following formula. δ = (ΔE / V) 1 / 2 △E: Intermolecular cohesive energy (heat of vaporization) V: Overall quality of the mixture △E / V: Cohesive energy density In addition, when the monomer composition of the resin is known, the calculation can be performed using the following method of Fedor et al. (described in Polym. Eng. Sci., 14[2] (1974)). SP value = (ΣΔei / ΣΔvi) 1 / 2 Δei: Evaporation energy of an atom or group of atoms Δvi: Molar volume of an atom or group of atoms The solubility parameter (SP value) described in this specification is primarily a value calculated from the monomer composition. The solubility parameter SP(sa) of the surface of the vinyl resin particle is calculated by determining the proportion of each structural unit on the surface of the vinyl resin particle using the same method as in the "Measurement of the proportion of each structural unit on the surface of a styrene-(meth)acrylic copolymer particle" described above.
[0078] The content of the vinyl resin particles is preferably from 5% by mass to 15% by mass, more preferably from 7% by mass to 13% by mass, and even more preferably from 8% by mass to 12% by mass, based on the total mass of the toner particles. By setting the content of the resin particles in the above range with respect to the entire toner particles, the toner can be appropriately Therefore, cracking or chipping of the toner particles is suppressed, and as a result, deterioration of fine line resolution is easily suppressed.
[0079] -Coloring agent- Examples of colorants include carbon black, chrome yellow, Hansa Yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, Balkan orange, watch young red, permanent red, brilliant carmine 3B, brilliant carmine 6B, DuPont oil red, pyrazolone red, lithol red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, ultramarine blue, and tetrahydrofuran. Examples of the dyes include various pigments such as phosphorus blue, chalcoil blue, methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, and malachite green oxalate, and various dyes such as acridine-based, xanthene-based, azo-based, benzoquinone-based, azine-based, anthraquinone-based, thioindigo-based, dioxazine-based, thiazine-based, azomethine-based, indigo-based, phthalocyanine-based, aniline black-based, polymethine-based, triphenylmethane-based, diphenylmethane-based, and thiazole-based dyes. The colorant may be used alone or in combination of two or more kinds.
[0080] The colorant may be surface-treated as necessary, or may be used in combination with a dispersant. In addition, a plurality of types of colorants may be used in combination.
[0081] The content of the colorant is, for example, preferably from 1% by mass to 30% by mass, and more preferably from 3% by mass to 15% by mass, based on the total mass of the toner particles.
[0082] -Release agent- Examples of the release agent include hydrocarbon waxes, natural waxes such as carnauba wax, rice wax, and candelilla wax, synthetic or mineral / petroleum waxes such as montan wax, and ester waxes such as fatty acid esters and montan acid esters. The release agent is not limited to these.
[0083] The melting temperature of the release agent is preferably 50°C or higher and 110°C or lower, and more preferably 60°C or higher and 100°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" as described in the method for determining melting temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics."
[0084] The content of the release agent is, for example, preferably from 1% by mass to 20% by mass, and more preferably from 5% by mass to 15% by mass, based on the total amount of the toner particles.
[0085] -Other additives- Examples of other additives include well-known additives such as magnetic materials, charge control agents, inorganic powders, etc. These additives are contained in the toner particles as internal additives.
[0086] -Characteristics of toner particles, etc.- The toner particles may be toner particles having a single layer structure, or may be toner particles having a so-called core-shell structure composed of a core portion (core particle) and a coating layer (shell layer) that coats the core portion.
[0087] The volume average particle size (D50v) of the toner particles is preferably from 2 μm to 10 μm, and more preferably from 4 μm to 8 μm.
[0088] The various average particle sizes and particle size distribution indexes of the toner particles are measured using a Coulter Multisizer II (manufactured by Beckman Coulter, Inc.), and the electrolyte is measured using an ISOTON-II (manufactured by Beckman Coulter, Inc.). For the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5% aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant, and this is then added to 100 ml to 150 ml of the electrolyte. The electrolyte with the sample suspended in it is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with diameters in the range of 2 μm to 60 μm is measured using a Coulter Multisizer II with an aperture diameter of 100 μm. The number of particles sampled is 50,000. Based on the measured particle size distribution, cumulative distributions of volume and number are drawn for each divided particle size range (channel) from the smallest diameter side, and the particle size at 16% of the cumulative size is defined as the volume particle size D16v, the number particle size D16p, the particle size at 50% of the cumulative size as the volume average particle size D50v, the cumulative number average particle size D50p, and the particle size at 84% of the cumulative size as the volume particle size D84v and number particle size D84p. Using these, the volumetric particle size distribution index (GSDv) is (D84v / D16v) 1 / 2 The number size distribution index (GSDp) is (D84p / D16p) 1 / 2 It is calculated as:
[0089] The average circularity of the toner particles is preferably 0.94 or more and 1.00 or less, and more preferably 0.95 or more and 0.98 or less.
[0090] The average circularity of toner particles is calculated by (circular equivalent perimeter) / (perimeter) [(perimeter of a circle having the same projected area as the particle image) / (perimeter of the particle projected image)]. Specifically, it is a value measured by the following method. First, the toner particles to be measured are sucked and collected, flattened, and a still image of the particles is captured by instantaneous strobe light emission, and the particle image is analyzed by a flow-type particle image analyzer (FPIA-3000 manufactured by Sysmex Corporation). The number of samples to be taken in order to calculate the average circularity is 3,500. When the toner contains an external additive, the toner (developer) to be measured is dispersed in water containing a surfactant, and then ultrasonic treatment is performed to obtain toner particles from which the external additive has been removed.
[0091] (External additives) The external additive may be, for example, inorganic particles. Examples of the inorganic particles include SiO 2 , TiO 2 , Al 2 O 3 , CuO, ZnO, SnO 2 , CEO 2 , Fe 2 O 3 , MgO, BaO, CaO, K 2 O, Na 2 O, ZrO 2 , CaO SiO 2 , K 2 O (TiO 2 )n, Al 2 O 3 2SiO 2 , CaCO 3 , MgCO 3 , BaSO 4 , MgSO 4 etc.
[0092] The surface of the inorganic particles as an external additive may be subjected to a hydrophobic treatment. The hydrophobic treatment may be performed, for example, by immersing the inorganic particles in a hydrophobic treatment agent. The hydrophobic treatment agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is usually, for example, 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the inorganic particles.
[0093] Examples of external additives include resin particles (resin particles such as polystyrene, polymethyl methacrylate (PMMA), and melamine resin), cleaning agents (for example, metal salts of higher fatty acids such as zinc stearate, and fluorine-based polymer particles).
[0094] The amount of the external additive added is, for example, preferably from 0.01% by mass to 5% by mass, and more preferably from 0.01% by mass to 2.0% by mass, based on the toner particles.
[0095] (Toner manufacturing method) Next, a method for producing the toner according to the present embodiment will be described. The toner according to the exemplary embodiment is obtained by producing toner particles and then externally adding an external additive to the toner particles.
[0096] The toner particles are preferably obtained by an aggregation and coalescence method.
[0097] Specifically, toner particles are manufactured through, for example, a step of preparing a binder resin particle dispersion liquid in which binder resin particles that become a binder resin are dispersed, and a vinyl resin particle dispersion liquid in which vinyl resin particles are dispersed (dispersion liquid preparation step), a step of aggregating the binder resin particles and the vinyl resin particles (or other particles as necessary) in the dispersion liquid (in the dispersion liquid after mixing with other particle dispersion liquids as necessary) to form aggregated particles (aggregated particle formation step), and a step of heating the aggregated particle dispersion liquid in which the aggregated particles are dispersed, fusing and coalescing the aggregated particles, and forming toner particles (fusion and coalescence step).
[0098] Toner particles satisfying the formulas (1) and (2) can be obtained, for example, by the following method. In the dispersion preparation step, a mixed dispersion is prepared by mixing a vinyl resin particle dispersion and a dispersion in which particles other than vinyl resin particles (binder resin particles, colorant particles, release agent particles, etc.) are dispersed. The pH of the mixed dispersion is adjusted to a value between 2 and 5, and the vinyl resin particle dispersion is dropped into the mixed dispersion slowly stirred at a tip speed of, for example, 0.28 m / sec to 0.57 m / sec (for example, in the case of a stirring blade with a diameter of 20 cm, the rotation speed is 26.7 rpm to 54.4 rpm) to form aggregated particles. Thereby, the vinyl resin particles are aggregated with good dispersibility relative to other particles. As a result, the dispersibility of the vinyl resin particles in the toner particles is increased, and toner particles that satisfy formulas (1) and (2) are obtained. When the vinyl resin particle dispersion is dropped into the mixed dispersion to form aggregated particles, an aggregating agent may be added to the mixed dispersion.
[0099] Each step will be described in detail below. In the following description, a method for obtaining toner particles containing a colorant and a release agent will be described, but the colorant is used as necessary. Of course, additives other than the colorant may be used.
[0100] -Dispersion liquid preparation process- First, a binder resin particle dispersion in which binder resin particles that become a binder resin are dispersed, a colorant particle dispersion in which colorant particles are dispersed, and a release agent particle dispersion in which release agent particles are dispersed are prepared.
[0101] Here, the binder resin particle dispersion liquid is prepared, for example, by dispersing binder resin particles in a dispersion medium with the aid of a surfactant.
[0102] The dispersion medium used in the binder resin particle dispersion liquid is, for example, an aqueous medium. Examples of the aqueous medium include water such as distilled water and ion-exchanged water, alcohols, etc. These may be used alone or in combination of two or more kinds.
[0103] Examples of the surfactant include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. Among these, anionic surfactants and cationic surfactants are particularly preferred. The nonionic surfactants may be used in combination with anionic surfactants or cationic surfactants. The surfactant may be used alone or in combination of two or more kinds.
[0104] In the binder resin particle dispersion liquid, examples of a method for dispersing the binder resin particles in a dispersion medium include general dispersion methods using, for example, a rotary shear type homogenizer, a ball mill having a medium, a sand mill, a dyno mill, etc. Depending on the type of the binder resin particles, the binder resin particles may be dispersed in the binder resin particle dispersion liquid using, for example, a phase inversion emulsification method. The phase inversion emulsification method is a method in which the resin to be dispersed is dissolved in a hydrophobic organic solvent in which the resin is soluble, a base is added to the organic continuous phase (O phase) to neutralize it, and then an aqueous medium (W phase) is added to effect conversion of the resin from W / O to O / W (so-called phase inversion), resulting in a discontinuous phase, and the resin is dispersed in particulate form in the aqueous medium.
[0105] The volume average particle size of the binder resin particles dispersed in the binder resin particle dispersion is, for example, preferably from 0.01 μm to 1 μm, more preferably from 0.08 μm to 0.8 μm, and even more preferably from 0.1 μm to 0.6 μm. The volume average particle size of the binder resin particles is determined by using a particle size distribution obtained by measurement using a laser wave type particle size distribution measuring device (e.g., LS-13 320 manufactured by Beckman Coulter, Inc.), and subtracting the cumulative distribution from the small particle size side for the volume of the divided particle size range (channel). The particle size that is 50% of the total particles is measured as the volume average particle size D50v. The volume average particle sizes of particles in other dispersions are also measured in the same manner.
[0106] The content of the binder resin particles in the binder resin particle dispersion is, for example, preferably from 5% by mass to 50% by mass, and more preferably from 10% by mass to 40% by mass.
[0107] In addition, for example, a colorant particle dispersion liquid and a release agent particle dispersion liquid are also prepared in the same manner as the binder resin particle dispersion liquid. That is, the volume average particle size, dispersion medium, dispersion method, and particle content of the particles in the binder resin particle dispersion liquid are the same for the colorant particles dispersed in the colorant particle dispersion liquid and the release agent particles dispersed in the release agent particle dispersion liquid.
[0108] Preparation of vinyl resin particle dispersion The vinyl resin particle dispersion can be prepared by any known method, such as emulsion polymerization, melt kneading using a Banbury mixer or a kneader, suspension polymerization, spray drying, etc., with emulsion polymerization being preferred.
[0109] From the viewpoint of controlling the loss factor within a preferred range, it is preferable to use a styrene-based monomer and a (meth)acrylic acid-based monomer as the monomers and to polymerize them in the presence of a crosslinking agent. In the production of the vinyl resin particles, it is preferable to carry out emulsion polymerization a number of times. The method for producing the vinyl resin particles will be described in more detail below.
[0110] The method for preparing a vinyl resin particle dispersion includes the steps of: A step of obtaining an emulsion containing a monomer, a crosslinking agent, a surfactant, and water (an emulsion preparation step); a step of adding a polymerization initiator to the emulsion and polymerizing the monomers by heating (first emulsion polymerization step); It is preferable to include a step (second emulsion polymerization step) of adding an emulsion containing a monomer to the reaction solution after the first emulsion polymerization step and heating the mixture to polymerize the monomer.
[0111] Here, when a styrene-based monomer and a (meth)acrylic acid-based monomer are used as monomers, the molecular chain state or the crosslinked state of the resin can be changed by adjusting the ratio of the styrene-based monomer in the monomers contained in the reaction solution in the first emulsion polymerization step and the ratio of the styrene-based monomer in the monomers added in the second emulsion polymerization step, taking into consideration the difference in reactivity. In addition to adjusting the monomer ratio, the molecular chain state or the crosslinked state of the resin can be changed by taking into consideration the reactivity of the monomers, the polymerization temperature, the amount and method of polymerization initiator added, the dripping speed of the emulsion, the amount of crosslinking agent added, etc.
[0112] ·Emulsion preparation process This is a process for obtaining an emulsion containing a monomer, a crosslinking agent, a surfactant, and water. It is preferable to obtain an emulsion by emulsifying a monomer, a crosslinking agent, a surfactant, and water using an emulsifier. Examples of emulsifiers include rotary mixers equipped with propeller-type, anchor-type, paddle-type, or turbine-type stirring blades, static mixers such as static mixers, rotor-stator type emulsifiers such as homogenizers and Clearmix, mill-type emulsifiers equipped with a grinding function, high-pressure emulsifiers such as Manton-Gaulin pressure emulsifiers, high-pressure nozzle type emulsifiers that generate cavitation under high pressure, high-pressure collision type emulsifiers such as microfluidizers that apply shear force by colliding liquids with each other under high pressure, ultrasonic emulsifiers that generate cavitation using ultrasound, and membrane emulsifiers that perform uniform emulsification through fine pores.
[0113] As the monomer, it is preferable to use a styrene-based monomer and a (meth)acrylic acid-based monomer. It is. As the crosslinking agent, those already mentioned are applicable.
[0114] Examples of the surfactant include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. The nonionic surfactants may be used in combination with anionic surfactants or cationic surfactants. Among these, anionic surfactants are preferred. The surfactants may be used alone or in combination with two or more.
[0115] The emulsion may contain a chain transfer agent. There is no particular limitation on the chain transfer agent, but a compound having a thiol component can be used. Specifically, alkyl mercaptans such as hexyl mercaptan, heptyl mercaptan, octyl mercaptan, nonyl mercaptan, decyl mercaptan, and dodecyl mercaptan are preferred.
[0116] ·First emulsion polymerization process This is a process in which a polymerization initiator is added to the emulsion and then heated to polymerize the monomers. During polymerization, it is preferable to stir the emulsion (reaction solution) containing the polymerization initiator with a stirrer. The agitator may be a rotary agitator equipped with a propeller-type, anchor-type, paddle-type, or turbine-type agitator blade. As the polymerization initiator, ammonium persulfate is preferably used.
[0117] ·Second emulsion polymerization process This is a step in which an emulsion containing a monomer is added to the reaction solution after the first emulsion polymerization step, and the monomer is polymerized by heating. During the polymerization, it is preferable to stir the reaction solution in the same manner as in the first emulsion polymerization step. In this step, the emulsion containing the monomers may be added in portions by changing the ratio of the styrene monomer and the (meth)acrylate monomer in the emulsion. The emulsion containing the monomer is preferably obtained by emulsifying the monomer, a surfactant, and water using an emulsifier.
[0118] It is preferable to prepare a vinyl resin particle dispersion liquid by the above steps.
[0119] -Agglomerated particle formation process- Next, the colorant particle dispersion and the release agent particle dispersion are mixed together with the binder resin particle dispersion. The pH of the mixed dispersion is adjusted to a value between 2 and 5, and the pH of the vinyl resin particle dispersion is adjusted to within ±0.5 of the pH of the mixed dispersion. Then, while slowly stirring the mixed dispersion at a tip speed of the stirring blade of, for example, 0.28 m / sec or more and 0.57 m / sec or less (for example, in the case of a stirring blade with a diameter of 20 cm, the rotation speed is 26.7 rpm or more and 54.4 rpm or less), the vinyl resin particle dispersion is dropped into the mixed dispersion, and the binder resin particles, colorant particles, release agent particles, and vinyl resin particles are hetero-aggregated to form aggregated particles containing the binder resin particles, colorant particles, release agent particles, and vinyl resin particles and having a diameter close to the diameter of the target toner particles.
[0120] Specifically, for example, an aggregating agent is added to the mixed dispersion, the pH of the mixed dispersion is adjusted to be acidic (e.g., pH 2 or more and 5 or less), a dispersion stabilizer is added as necessary, and then the mixed dispersion is heated to a temperature of the glass transition temperature of the resin particles (specifically, for example, a temperature of the glass transition temperature of the binder resin particles -30°C or more and the glass transition temperature -10°C or less), and the particles dispersed in the mixed dispersion are aggregated to form aggregated particles. In the aggregated particle formation process, for example, the mixed dispersion into which the vinyl resin particle dispersion has been dropped may be stirred with a rotary shear homogenizer while the above-mentioned aggregating agent is added at room temperature (e.g., 25°C), the pH of the mixed dispersion may be adjusted to an acidic state (e.g., pH 2 or more and 5 or less), and a dispersion stabilizer may be added as necessary, followed by the above-mentioned heating.
[0121] Examples of the flocculant include a surfactant having a polarity opposite to that of the surfactant used as the dispersant added to the mixed dispersion, an inorganic metal salt, and a divalent or higher metal complex. In particular, when a metal complex is used as the flocculant, the amount of surfactant used is reduced and the charging characteristics are improved. If necessary, an additive that forms a complex or a similar bond with the metal ions of the flocculant may be used, and a chelating agent is preferably used as this additive.
[0122] Examples of inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. The chelating agent may be a water-soluble chelating agent, for example, oxycarboxylic acid such as tartaric acid, citric acid, gluconic acid, iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), ethylenediaminetetraacetic acid (EDTA), etc. The amount of the chelating agent added is, for example, preferably 0.01 parts by mass or more and 5.0 parts by mass or less, and more preferably 0.1 parts by mass or more and less than 3.0 parts by mass, relative to 100 parts by mass of the resin particles.
[0123] -Fusion / coalescence process- Next, the aggregated particle dispersion liquid in which the aggregated particles are dispersed is heated, for example, to a temperature equal to or higher than the glass transition temperature of the binder resin particles (for example, a temperature 10 to 30° C. higher than the glass transition temperature of the binder resin particles) to fuse and coalesce the aggregated particles, thereby forming toner particles.
[0124] Through the above steps, toner particles are obtained. Note that, after obtaining an aggregated particle dispersion in which the aggregated particles are dispersed, the toner particles may be manufactured through a process of further mixing the aggregated particle dispersion with a binder resin particle dispersion and aggregating the aggregated particles so that the binder resin particles are further attached to the surfaces of the aggregated particles to form second aggregated particles, and a process of heating the second aggregated particle dispersion in which the second aggregated particles are dispersed to fuse and coalesce the second aggregated particles to form toner particles having a core / shell structure.
[0125] After the fusion and coalescence process, the toner particles formed in the solution are subjected to a known washing process, solid-liquid separation process, and drying process to obtain toner particles in a dried state. In the washing step, it is preferable to carry out sufficient replacement washing with ion-exchanged water from the viewpoint of electrostatic charge. In addition, the solid-liquid separation step is not particularly limited, but it is preferable to carry out suction filtration, pressure filtration, etc. from the viewpoint of productivity. In addition, in the drying step, there is no particular limit to the method, but it is preferable to carry out freeze drying, air flow drying, fluidized drying, vibration type fluidized drying, etc. from the viewpoint of productivity.
[0126] The toner according to the present embodiment is produced, for example, by adding an external additive to the obtained toner particles in a dry state and mixing them. The mixing may be performed, for example, by using a V blender, a Henschel mixer, a Loedige mixer, etc. Furthermore, if necessary, coarse particles of the toner may be removed using a vibration sieve, an air sieve, etc.
[0127] <Electrostatic image developer> The electrostatic image developer according to this embodiment contains at least the toner according to this embodiment. The electrostatic image developer according to the present embodiment may be a one-component developer containing only the toner according to the present embodiment, or may be a two-component developer in which the toner is mixed with a carrier.
[0128] The carrier is not particularly limited, and may be any known carrier. Examples of the carrier include a coated carrier in which the surface of a core material made of magnetic powder is coated with a coating resin; a magnetic powder dispersion type carrier in which magnetic powder is dispersed and mixed in a matrix resin; and a porous magnetic powder impregnated with a resin. and the like. The magnetic powder dispersion type carrier and the resin impregnated type carrier may be a carrier in which the constituent particles of the carrier are used as a core material and are coated with a coating resin.
[0129] Examples of the magnetic powder include magnetic metals such as iron, nickel, and cobalt, and magnetic oxides such as ferrite and magnetite.
[0130] Examples of the coating resin and matrix resin include polyethylene, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl ether, polyvinyl ketone, vinyl chloride-vinyl acetate copolymer, styrene-acrylic acid ester copolymer, straight silicone resin containing an organosiloxane bond or a modified product thereof, fluororesin, polyester, polycarbonate, phenolic resin, and epoxy resin. The coating resin and the matrix resin may contain other additives such as conductive particles. Examples of the conductive particles include particles of metals such as gold, silver, and copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, and potassium titanate.
[0131] Here, the method of coating the surface of the core material with the coating resin includes a method of coating with a solution for forming a coating layer in which the coating resin and, if necessary, various additives are dissolved in an appropriate solvent, etc. The solvent is not particularly limited and may be selected taking into consideration the coating resin to be used, the suitability for application, etc. Specific resin coating methods include an immersion method in which the core material is immersed in a solution for forming a coating layer, a spray method in which the solution for forming a coating layer is sprayed onto the surface of the core material, a fluidized bed method in which the solution for forming a coating layer is sprayed onto the core material while it is suspended in flowing air, and a kneader coater method in which the core material of a carrier and the solution for forming a coating layer are mixed in a kneader coater and the solvent is removed.
[0132] In the two-component developer, the mixture ratio (mass ratio) of the toner and the carrier is preferably toner:carrier=1:100 to 30:100, and more preferably 3:100 to 20:100.
[0133] <Image forming device / image forming method> An image forming apparatus / image forming method according to this embodiment will be described. The image forming apparatus according to the present embodiment includes an image carrier, a charging means for charging the surface of the image carrier, an electrostatic image forming means for forming an electrostatic image on the surface of the charged image carrier, a developing means for containing an electrostatic image developer and developing the electrostatic image formed on the surface of the image carrier as a toner image with the electrostatic image developer, a transfer means for transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing means for fixing the toner image transferred to the surface of the recording medium. The electrostatic image developer according to the present embodiment is used as the electrostatic image developer.
[0134] In the image forming apparatus according to this embodiment, an image forming method (the image forming method according to this embodiment) is carried out, which includes a charging step of charging the surface of an image carrier, an electrostatic image forming step of forming an electrostatic image on the surface of the charged image carrier, a developing step of developing the electrostatic image formed on the surface of the image carrier as a toner image using an electrostatic image developer according to this embodiment, a transfer step of transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing step of fixing the toner image transferred to the surface of the recording medium.
[0135] The image forming apparatus according to the present embodiment is a direct transfer type apparatus in which a toner image formed on the surface of an image carrier is directly transferred to a recording medium; Well-known image forming apparatuses that can be used include an intermediate transfer type apparatus in which a toner image is primarily transferred onto the surface of a recording medium, and the toner image transferred onto the surface of an intermediate transfer body is then secondarily transferred onto the surface of a recording medium; an apparatus equipped with a cleaning means for cleaning the surface of an image carrier before charging after the toner image is transferred; and an apparatus equipped with a discharging means for irradiating the surface of an image carrier with discharging light to discharge it before charging after the toner image is transferred. In the case of an intermediate transfer type device, the transfer means has, for example, an intermediate transfer body onto whose surface a toner image is transferred, a primary transfer means which primarily transfers the toner image formed on the surface of the image carrier onto the surface of the intermediate transfer body, and a secondary transfer means which secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto the surface of a recording medium.
[0136] In the image forming apparatus according to the present embodiment, for example, a portion including the developing means may have a cartridge structure (process cartridge) that is detachably attached to the image forming apparatus. As the process cartridge, for example, a process cartridge including a developing means that contains the electrostatic image developer according to the present embodiment is preferably used.
[0137] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this. Note that only the main parts shown in the drawings will be described, and descriptions of the rest will be omitted.
[0138] FIG. 1 is a schematic diagram showing the configuration of an image forming apparatus according to the present embodiment. The image forming apparatus shown in Fig. 1 includes first to fourth electrophotographic image forming units 10Y, 10M, 10C, and 10K (image forming means) that output images of each color of yellow (Y), magenta (M), cyan (C), and black (K) based on color-separated image data. These image forming units (hereinafter sometimes simply referred to as "units") 10Y, 10M, 10C, and 10K are arranged in parallel at predetermined distances from each other in the horizontal direction. These units 10Y, 10M, 10C, and 10K may be process cartridges that are detachable from the image forming apparatus.
[0139] Above each of the units 10Y, 10M, 10C, and 10K in the drawing, an intermediate transfer belt 20 is provided as an intermediate transfer body extending through each unit. The intermediate transfer belt 20 is provided wound around a drive roll 22 and a support roll 24 that are arranged from left to right in the drawing at a distance from each other and contact the inner surface of the intermediate transfer belt 20, and is adapted to run in a direction from the first unit 10Y to the fourth unit 10K. Note that a force is applied to the support roll 24 in a direction away from the drive roll 22 by a spring or the like (not shown), and tension is applied to the intermediate transfer belt 20 wound around them. In addition, an intermediate transfer body cleaning device 30 is provided on the image carrier side of the intermediate transfer belt 20, facing the drive roll 22. Further, the developing devices (developing means) 4Y, 4M, 4C, and 4K of the units 10Y, 10M, 10C, and 10K are supplied with toner including four colors of toner, yellow, magenta, cyan, and black, contained in toner cartridges 8Y, 8M, 8C, and 8K, respectively.
[0140] Since the first to fourth units 10Y, 10M, 10C, and 10K have the same configuration, the first unit 10Y that forms a yellow image and is disposed upstream in the direction in which the intermediate transfer belt travels will be described here as a representative example. Note that by assigning reference numerals of magenta (M), cyan (C), and black (K) instead of yellow (Y) to parts equivalent to those of the first unit 10Y, descriptions of the second to fourth units 10M, 10C, and 10K will be omitted.
[0141] The first unit 10Y has a photoconductor 1Y that acts as an image carrier. Around the photoconductor 1Y, there is a charging roll (one example of a charging means) 2Y that charges the surface of the photoconductor 1Y to a predetermined potential, and a laser beam 3Y that charges the charged surface based on a color-separated image signal. Arranged in this order are an exposure device (an example of an electrostatic image forming means) 3 that exposes the electrostatic charge to form an electrostatic image, a development device (an example of a development means) 4Y that supplies charged toner to the electrostatic charge image to develop it, a primary transfer roll 5Y (an example of a primary transfer means) that transfers the developed toner image onto the intermediate transfer belt 20, and a photoreceptor cleaning device (an example of a cleaning means) 6Y that removes toner remaining on the surface of the photoreceptor 1Y after the primary transfer. The primary transfer roll 5Y is disposed inside the intermediate transfer belt 20 and is provided at a position facing the photoconductor 1Y. Furthermore, a bias power supply (not shown) that applies a primary transfer bias is connected to each of the primary transfer rolls 5Y, 5M, 5C, and 5K. Each bias power supply varies the transfer bias applied to each primary transfer roll under the control of a control unit (not shown).
[0142] Hereinafter, an operation of forming a yellow image in first unit 10Y will be described. First, prior to operation, the surface of the photoconductor 1Y is charged to a potential of −600V to −800V by the charging roll 2Y. The photoconductor 1Y has a conductivity (for example, a volume resistivity at 20° C. of 1×10 -6The photosensitive layer is formed by laminating a photosensitive layer on a substrate having a resistivity of Ωcm or less. This photosensitive layer is usually highly resistive (the resistance of ordinary resins), but when irradiated with a laser beam 3Y, the resistivity of the portion irradiated with the laser beam changes. A laser beam 3Y is output to the charged surface of the photoreceptor 1Y via an exposure device 3 in accordance with image data for yellow sent from a control unit (not shown). The laser beam 3Y is irradiated onto the photosensitive layer on the surface of the photoreceptor 1Y, and an electrostatic charge image of a yellow image pattern is formed on the surface of the photoreceptor 1Y.
[0143] An electrostatic image is an image formed on the surface of the photoconductor 1Y by electrostatic charging. The laser beam 3Y reduces the resistivity of the irradiated parts of the photosensitive layer, causing the charged charges on the surface of the photoconductor 1Y to flow, while the charges remain in the parts not irradiated by the laser beam 3Y. This is a so-called negative latent image. The electrostatic image formed on the photoconductor 1Y is rotated to a predetermined developing position as the photoconductor 1Y travels. Then, at this developing position, the electrostatic image on the photoconductor 1Y is made visible as a toner image (developed image) by the developing device 4Y.
[0144] The developing device 4Y contains an electrostatic image developer including at least yellow toner and a carrier, for example. The yellow toner is triboelectrically charged by being stirred inside the developing device 4Y, and is held on a developer roll (an example of a developer holder) with a charge of the same polarity (negative polarity) as the charge on the photoconductor 1Y. As the surface of the photoconductor 1Y passes through the developing device 4Y, the yellow toner electrostatically adheres to the discharged latent image portion on the surface of the photoconductor 1Y, and the latent image is developed with the yellow toner. The photoconductor 1Y on which the yellow toner image has been formed continues to travel at a predetermined speed, and the toner image developed on the photoconductor 1Y is transported to a predetermined primary transfer position.
[0145] When the yellow toner image on the photoreceptor 1Y is transported to the primary transfer, a primary transfer bias is applied to the primary transfer roll 5Y, and an electrostatic force from the photoreceptor 1Y toward the primary transfer roll 5Y acts on the toner image, and the toner image on the photoreceptor 1Y is transferred onto the intermediate transfer belt 20. The transfer bias applied at this time has a polarity (+) opposite to the polarity (-) of the toner, and in the first unit 10Y, for example, it is controlled to +10 μA by a control unit (not shown). On the other hand, the toner remaining on the photoconductor 1Y is removed and collected by the photoconductor cleaning device 6Y.
[0146] Further, the primary transfer bias applied to the primary transfer rolls 5M, 5C, and 5K subsequent to the second unit 10M is also controlled in accordance with the first unit. In this way, the intermediate transfer belt on which the yellow toner image is transferred by the first unit 10Y is The toner image 20 is conveyed through the second to fourth units 10M, 10C, and 10K in order, and the toner images of the respective colors are transferred and superimposed on each other.
[0147] The intermediate transfer belt 20 onto which the four color toner images have been transferred in multiple layers through the first to fourth units reaches a secondary transfer section that is composed of the intermediate transfer belt 20, a support roll 24 that contacts the inner surface of the intermediate transfer belt, and a secondary transfer roll (an example of a secondary transfer means) 26 arranged on the image bearing surface side of the intermediate transfer belt 20. Meanwhile, a recording paper (an example of a recording medium) P is fed at a predetermined timing into the gap between the secondary transfer roll 26 and the intermediate transfer belt 20 via a supply mechanism, and a secondary transfer bias is applied to the support roll 24. The transfer bias applied at this time has a (-) polarity that is the same as the (-) polarity of the toner, and an electrostatic force from the intermediate transfer belt 20 toward the recording paper P acts on the toner image, so that the toner image on the intermediate transfer belt 20 is transferred onto the recording paper P. The secondary transfer bias at this time is determined according to the resistance detected by a resistance detection means (not shown) that detects the resistance of the secondary transfer section, and is voltage-controlled.
[0148] Thereafter, the recording paper P is sent to a pressure contact portion (nip portion) of a pair of fixing rolls in a fixing device (one example of a fixing means) 28, where the toner image is fixed onto the recording paper P, forming a fixed image.
[0149] The recording paper P onto which the toner image is transferred can be, for example, plain paper used in electrophotographic copying machines, printers, etc. In addition to the recording paper P, other examples of the recording medium include overhead projector sheets, etc. To further improve the smoothness of the image surface after fixing, it is preferable that the surface of the recording paper P is also smooth. For example, coated paper in which the surface of ordinary paper is coated with resin or the like, art paper for printing, etc. are preferably used.
[0150] After the color image has been fixed, the recording paper P is conveyed toward the discharge section, and the series of color image forming operations is completed.
[0151] <Process cartridge / toner cartridge> The process cartridge according to this embodiment will be described. The process cartridge according to this embodiment is a process cartridge that contains the electrostatic image developer according to this embodiment, is equipped with a developing means that develops an electrostatic image formed on the surface of an image carrier using the electrostatic image developer into a toner image, and is detachably attached to an image forming apparatus.
[0152] In addition, the process cartridge according to this embodiment is not limited to the above configuration, and may be configured to include a developing device and, as necessary, at least one other means selected from an image carrier, a charging means, an electrostatic image forming means, and a transfer means.
[0153] An example of a process cartridge according to the present embodiment will be described below, but the present invention is not limited to this example. Note that only the main parts shown in the drawings will be described, and descriptions of the rest will be omitted.
[0154] FIG. 2 is a schematic diagram showing the process cartridge according to the present embodiment. The process cartridge 200 shown in FIG. 2 is configured by, for example, a housing 117 having a mounting rail 116 and an opening 118 for exposure, and integrally combining and holding a photoconductor 107 (an example of an image carrier), a charging roll 108 (an example of a charging means) provided around the photoconductor 107, a developing device 111 (an example of a developing means), and a photoconductor cleaning device 113 (an example of a cleaning means), which are assembled into a cartridge. In FIG. 2, 109 is an exposure device (an example of an electrostatic image forming means), 112 is a transfer device (an example of a transfer means), 115 is a fixing device (an example of a fixing means), and 300 is a recording paper (one example of a recording medium). Example) is shown.
[0155] Next, the toner cartridge according to this embodiment will be described. The toner cartridge according to the present embodiment is a toner cartridge that contains the toner according to the present embodiment and is detachably attached to an image forming apparatus. The toner cartridge contains replenishment toner to be supplied to a developing unit provided in the image forming apparatus.
[0156] 1 is an image forming apparatus having a configuration in which toner cartridges 8Y, 8M, 8C, and 8K can be attached and detached, and the developing devices 4Y, 4M, 4C, and 4K are connected to the toner cartridges corresponding to the respective developing devices (colors) through toner supply pipes (not shown). When the toner contained in the toner cartridge becomes low, the toner cartridge is replaced. EXAMPLES
[0157] Examples will be described below, but the present invention is not limited to these examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.
[0158] <Preparation of amorphous resin particle dispersion> (Preparation of amorphous polyester resin particle dispersion (1)) Terephthalic acid: 28 parts by mole Isophthalic acid (IPA): 15 parts by mole Adipic acid: 5 mol parts Trimellitic anhydride: 2 mole parts Bisphenol A propylene oxide 2 mole adduct: 50 mole parts The above materials were charged into a reaction vessel equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, the temperature was raised to 190°C over 1 hour, and 1.2 parts of dibutyltin oxide was added per 100 parts of the above materials. The temperature was raised to 240°C over 6 hours while distilling off the generated water, and the dehydration condensation reaction was continued for 3 hours while maintaining the temperature at 240°C, followed by cooling to obtain polyester resin (1). The amorphous polyester resin (1) had an acid value of 10.5 and a glass transition temperature of 59.0°C.
[0159] Amorphous polyester resin (1): 100 parts Methyl ethyl ketone: 60 parts Isopropanol: 10 parts 10% ammonia solution: 3.5 parts The above materials were put into a jacketed reaction tank equipped with a condenser, a thermometer, a water dropping device and an anchor blade, and the resin was dissolved while stirring and mixing at 100 rpm while maintaining the liquid temperature at 50 ° C. in a water circulation type thermostatic bath. Next, the water circulation type thermostatic bath was set to 40 ° C., and a total of 300 parts of ion-exchanged water kept at 40 ° C. was dropped at a speed of 3 parts / min to invert the phase and obtain an emulsion. The obtained emulsion was placed in an eggplant flask and set in an evaporator equipped with a vacuum control unit via a trap bulb. The eggplant flask was heated in a hot water bath at 60 ° C. while rotating, and the pressure was reduced to 7 kPa while paying attention to bumping to remove the solvent, and then the pressure was returned to normal pressure, and the eggplant flask was water-cooled to obtain a dispersion. Ion-exchanged water was added to the dispersion to obtain an amorphous polyester resin particle dispersion liquid (1) with a solid content of 20%. The volume average particle size of the resin particles in the amorphous polyester resin particle dispersion liquid (1) was 180 nm.
[0160] (Preparation of amorphous polyester resin particle dispersion (2)) Amorphous polyester resin particle dispersion (2) was obtained in the same manner as in the preparation of amorphous polyester resin dispersion (1), except that terephthalic acid: 28 molar parts was changed to 43 molar parts, and isophthalic acid (IPA): 15 molar parts was changed to 0 molar parts. The amorphous polyester resin (2) had an acid value of 10.5, a glass transition point of 62° C., a volume average particle size of the resin particles in the amorphous polyester resin dispersion (2) of 185 nm, and a solid content of 20%.
[0161] (Preparation of amorphous polyester resin particle dispersion (3)) Amorphous polyester resin particle dispersion (3) was obtained in the same manner as in the preparation of amorphous polyester resin dispersion (1), except that terephthalic acid: 28 parts by mol was changed to 20 parts by mol, and isophthalic acid (IPA): 15 parts by mol was changed to 23 parts by mol. The amorphous polyester resin (3) had an acid value of 10.5, a glass transition point of 60° C., a volume average particle size of the resin particles in the amorphous polyester resin dispersion (3) of 183 nm, and a solid content of 20%.
[0162] (Preparation of amorphous polyester resin particle dispersion (4)) Amorphous polyester resin particle dispersion (4) was obtained in the same manner as in the preparation of amorphous polyester resin dispersion (1), except that terephthalic acid: 28 molar parts was changed to 17 molar parts, and isophthalic acid (IPA): 15 molar parts was changed to 26 molar parts. The amorphous polyester resin (4) had an acid value of 10.5, a glass transition point of 55° C., a volume average particle size of the resin particles in the amorphous polyester resin dispersion (4) of 180 nm, and a solid content of 20%.
[0163] (Preparation of amorphous polyester resin particle dispersion (5)) Amorphous polyester resin particle dispersion (5) was obtained in the same manner as in the preparation of amorphous polyester resin dispersion (1), except that terephthalic acid: 28 molar parts was changed to 37 molar parts, and isophthalic acid (IPA): 15 molar parts was changed to 6 molar parts. The amorphous polyester resin (5) had an acid value of 10.5, a glass transition point of 61° C., a volume average particle size of the resin particles in the amorphous polyester resin dispersion (5) of 187 nm, and a solid content of 20%.
[0164] (Preparation of amorphous polyester resin particle dispersion (6)) Amorphous polyester resin particle dispersion (6) was obtained in the same manner as in the preparation of amorphous polyester resin dispersion (1), except that 28 mol parts of terephthalic acid was replaced with 33 mol parts, 5 mol parts of adipic acid was replaced with 0 part, 50 mol parts of bisphenol A propylene oxide 2 mol adduct, and 50 mol parts of bisphenol A ethylene oxide 2 mol adduct. The amorphous polyester resin (6) had an acid value of 11.0 and a glass transition point of 61° C., and the volume average particle size of the resin particles in the amorphous polyester resin dispersion (5) was 185 nm and the solid content was 20%.
[0165] (Preparation of amorphous polyester resin particle dispersion (7)) Bisphenol A ethylene oxide 2.2 mole adduct: 40 mole parts Bisphenol A propylene oxide 2.2 mole adduct: 60 mole parts Dimethyl terephthalate: 60 parts by mole Dimethyl fumarate: 15 parts by mole Dodecenylsuccinic anhydride: 20 mole parts Trimellitic anhydride: 5 mol parts In a reaction vessel equipped with a stirrer, a thermometer, a condenser, and a nitrogen gas inlet tube, the above monomers other than fumaric acid and trimellitic anhydride, and tin dioctanoate were added in an amount of 0.25 parts per 100 parts of the total of the above monomers. After reacting at 235°C for 6 hours under a nitrogen gas stream, the temperature was lowered to 200°C, and fumaric acid and trimellitic anhydride were added and reacted for 1 hour. The temperature was raised to 220°C over 5 hours, and polymerization was carried out under a pressure of 10 kPa until the desired molecular weight was reached, to obtain a pale yellow transparent polyester resin (7). The polyester resin (7) had a glass transition temperature of 59°C. Next, the obtained polyester resin (7) was dispersed using a disperser modified from a Cavitron CD1010 (manufactured by Eurotech Co., Ltd.) into a high-temperature, high-pressure type. The composition ratio was 80% ion-exchanged water and 20% polyester resin, the pH was adjusted to 8.5 with ammonia, and the Cavitron was operated under the following conditions: rotor speed 60Hz, pressure 5Kg / cm2, and heating by a heat exchanger at 140°C, to obtain a polyester resin dispersion (solid content 20%). The volume average particle size of the resin particles in this dispersion was 130 nm. Ion-exchanged water was added to the dispersion to adjust the solid content to 20%, and this was used as polyester resin particle dispersion (7).
[0166] In Table 1, the amorphous polyester resin particle dispersions (1) to (7) are abbreviated as Amo1 to Amo7.
[0167] <Preparation of crystalline resin dispersion> (Preparation of Crystalline Polyester Resin Particle Dispersion (1)) Dodecanedioic acid: 50 parts by mole 1,6-Hexanediol: 50 parts by mole The above materials were charged into a reaction vessel equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, and the temperature was raised to 160°C over 1 hour, and 0.8 parts of dibutyltin oxide was added per 100 parts of the above materials. The temperature was raised to 180°C over 6 hours while distilling off the generated water, and the mixture was stirred for 5 hours while maintaining 180°C, and the reaction was allowed to proceed under reflux. Next, the temperature was gradually raised to 230°C under reduced pressure (3 kPa), and the mixture was stirred for 2 hours while maintaining 230°C. Next, the reaction product was cooled. After cooling, solid-liquid separation was performed, and the solid matter was dried to obtain crystalline polyester resin (1). The weight average molecular weight of the crystalline polyester resin (1) was 29,000.
[0168] Crystalline polyester resin (1): 100 parts Methyl ethyl ketone: 70 parts Isopropanol: 12 parts 10% ammonia solution: 3 parts The above materials were put into a jacketed reaction tank equipped with a condenser, a thermometer, a water dropping device and an anchor blade, and the resin was dissolved while stirring and mixing at 100 rpm while maintaining the liquid temperature at 80 ° C. in a water circulation type thermostatic bath. Next, the water circulation type thermostatic bath was set to 60 ° C., and a total of 300 parts of ion-exchanged water kept at 60 ° C. was dropped at a rate of 3 parts / min to invert the phase and obtain an emulsion. The obtained emulsion was placed in an eggplant flask and set in an evaporator equipped with a vacuum control unit via a trap bulb. The eggplant flask was heated in a hot water bath at 60 ° C. while rotating, and the pressure was reduced to 7 kPa while paying attention to bumping to remove the solvent, and then the pressure was returned to normal pressure, and the eggplant flask was water-cooled to obtain a dispersion. Ion-exchanged water was added to the dispersion to obtain a crystalline polyester resin particle dispersion liquid (1) with a solid content of 20%. The volume average particle size of the resin particles in the crystalline polyester resin particle dispersion liquid (1) was 160 nm.
[0169] (Preparation of Crystalline Polyester Resin Particle Dispersion (2)) Dodecanedioic acid: 50 parts by mole 1,9-nonanediol: 50 parts by mole The monomers were placed in a reaction vessel equipped with a stirrer, a thermometer, a condenser, and a nitrogen gas inlet tube, and the inside of the reaction vessel was replaced with dry nitrogen gas, after which 0.25 parts of titanium tetrabutoxide was added per 100 parts of the monomers. After stirring and reacting for 3 hours at 170°C under a nitrogen gas stream, the temperature was further raised to 210°C over 1 hour, the pressure inside the reaction vessel was reduced to 3 kPa, and stirring and reacting under reduced pressure for 13 hours gave a crystalline polyester resin (2). The crystalline polyester resin (2) had a weight average molecular weight of 25,000. Next, the obtained crystalline polyester resin (2) was dispersed using a disperser modified from a Cavitron CD1010 (manufactured by Eurotech Co., Ltd.) into a high-temperature, high-pressure type. The composition ratio was 80% ion-exchanged water and 20% polyester resin, the pH was adjusted to 8.5 with ammonia, and the Cavitron was operated under the following conditions: rotor speed 60Hz, pressure 5Kg / cm2, and heating by a heat exchanger at 140°C, to obtain a polyester resin dispersion (solid content 20%). The volume average particle size of the resin particles in this dispersion was 180 nm. Ion-exchanged water was added to the dispersion to adjust the solid content to 20%, and this was used as crystalline polyester resin particle dispersion (2).
[0170] In Table 1, the crystalline polyester resin particle dispersion (1) 2 is abbreviated as Cry1 to 2.
[0171] <Preparation of vinyl resin particle dispersion> (Preparation of vinyl resin particle dispersion (1) [Preparation of emulsions (1-1) to (1-4)] -Emulsion (1-1)- Styrene: 60 parts n-Butyl acrylate: 38.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (1-1).
[0172] -Emulsion (1-2)- Styrene: 55 parts n-Butyl acrylate: 43.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (1-2).
[0173] -Emulsion (1-3)- Styrene: 45 parts n-Butyl acrylate: 53.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (1-3).
[0174] -Emulsion (1-4)- Styrene: 40 parts n-Butyl acrylate: 58.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (1-4).
[0175] -Vinyl resin particle dispersion (1)- In a reaction vessel equipped with a stirrer and a nitrogen inlet tube, the inside of the reaction vessel was replaced with nitrogen, and then 1.1 parts of anionic surfactant (Eleminol MON-2) and 400 parts of ion-exchanged water were added. The reaction solution was heated in an oil bath while stirring, and the temperature of the reaction solution was set to 7065°C. After adding 10 parts of emulsion (1-1), 20 parts of an aqueous ammonium persulfate solution with a concentration adjusted to 10% by mass was further added and maintained for 30 minutes. Thereafter, while maintaining the temperature of the reaction solution at 70° C., 190 parts of emulsion (1-1) was gradually dripped into the reaction vessel over 30 minutes using a pump. Further, 200 parts of emulsion (1-2) was dripped over 30 minutes. Next, 200 parts of emulsion (1-3) was dripped over 40 minutes, and 200 parts of emulsion (1-4) was dripped over 40 minutes. After the dropwise addition, the mixture was held for 60 minutes, and then 2 parts of 10% by mass ammonium persulfate was added, and the mixture was held for another 3 hours and then cooled to room temperature. Then, ion-exchanged water and nitric acid were added to the mixture so that the solid content concentration was 20% by mass, to obtain a vinyl resin particle dispersion (1). The resulting resin particles had a volume average particle size of 165 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0176] (Preparation of vinyl resin particle dispersion (2)) Vinyl-based resin particle dispersion liquid (2) was obtained in the same manner as vinyl-based resin particle dispersion liquid (1), except that the amount of the anionic surfactant (Eleminol MON-2) was changed from 1.1 parts to 4.4 parts. The resulting resin particles had a volume average particle size of 100 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0177] (Preparation of vinyl resin particle dispersion (3)) Vinyl-based resin particle dispersion (3) was obtained in the same manner as in the vinyl-based resin particle dispersion (1), except that the amount of the anionic surfactant (Eleminol MON-2) was changed from 1.1 parts to 0.6 parts. The resulting resin particles had a volume average particle size of 200 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0178] (Preparation of vinyl resin particle dispersion (4)) Vinyl-based resin particle dispersion (3) was obtained in the same manner as in the vinyl-based resin particle dispersion (1), except that the amount of the anionic surfactant (Eleminol MON-2) was changed from 1.1 parts to 0.2 parts. The resulting resin particles had a volume average particle size of 300 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0179] (Preparation of vinyl resin particle dispersion (5)) [Preparation of emulsions (5-1) to (5-4)] -Emulsion (5-1)- Styrene: 47.6 parts n-Butyl acrylate: 50.9 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (5-1).
[0180] -Emulsion (5-2)- Styrene: 43.7 parts n-Butyl acrylate: 54.8 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (5-2).
[0181] -Emulsion (5-3)- Styrene: 35.7 parts n-Butyl acrylate: 62.8 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (5-3).
[0182] -Emulsion (5-4)- Styrene: 31.8 parts n-Butyl acrylate: 66.7 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (5-4).
[0183] -Vinyl resin particle dispersion (5)- Vinyl-based resin particle dispersion liquid (5) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (5-1), emulsion (1-2) to emulsion (5-2), emulsion (1-3) to emulsion (5-3), and emulsion (1-4) to emulsion (5-4). The resulting resin particles had a volume average particle size of 165 nm and a glass transition temperature of 1° C. as measured by a differential scanning calorimeter.
[0184] (Preparation of vinyl resin particle dispersion (6)) [Preparation of emulsions (6-1) to (6-4)] -Emulsion (6-1)- Styrene: 67.9 parts n-Butyl acrylate: 30.6 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (6-1).
[0185] -Emulsion (6-2)- Styrene: 62.3 parts n-Butyl acrylate: 36.2 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (6-2).
[0186] -Emulsion (6-3)- Styrene: 51.0 parts n-Butyl acrylate: 47.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (6-3).
[0187] -Emulsion (6-4)- Styrene: 45.3 parts n-Butyl acrylate: 53.2 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (6-4).
[0188] -Vinyl resin particle dispersion (6)- Vinyl-based resin particle dispersion liquid (6) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (6-1), emulsion (1-2) to emulsion (6-2), emulsion (1-3) to emulsion (6-3), and emulsion (1-4) to emulsion (6-4). The resulting resin particles had a volume average particle size of 165 nm and a glass transition temperature of 29° C. as measured by a differential scanning calorimeter.
[0189] (Preparation of vinyl resin particle dispersion (7)) Vinyl-based resin particle dispersion (7) was obtained in the same manner as in the vinyl-based resin particle dispersion (1), except that the amount of the anionic surfactant (Eleminol MON-2) was changed from 1.1 parts to 0.18 parts. The resulting resin particles had a volume average particle size of 310 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0190] (Preparation of vinyl resin particle dispersion (8)) Vinyl-based resin particle dispersion liquid (8) was obtained in the same manner as vinyl-based resin particle dispersion liquid (1), except that the amount of the anionic surfactant (Eleminol MON-2) was changed from 1.1 parts to 5.1 parts. The resulting resin particles had a volume average particle size of 90 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0191] (Preparation of vinyl resin particle dispersion (9)) [Preparation of emulsions (9-1) to (9-4)] -Emulsion (9-1)- Styrene: 70.1 parts n-Butyl acrylate: 28.4 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (9-1).
[0192] -Emulsion (9-2)- Styrene: 64.3 parts n-Butyl acrylate: 34.2 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (9-2).
[0193] -Emulsion (9-3)- Styrene: 52.6 parts n-Butyl acrylate: 45.9 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (9-3).
[0194] -Emulsion (9-4)- Styrene: 46.8 parts n-Butyl acrylate: 51.7 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (9-4).
[0195] -Vinyl resin particle dispersion (9)- Vinyl-based resin particle dispersion liquid (9) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (9-1), emulsion (1-2) to emulsion (9-2), emulsion (1-3) to emulsion (9-3), and emulsion (1-4) to emulsion (9-4). The resulting resin particles had a volume average particle size of 165 nm and a glass transition temperature of 32° C. as measured by a differential scanning calorimeter.
[0196] (Preparation of vinyl resin particle dispersion (10)) [Preparation of emulsions (10-1) to (10-4)] -Emulsion (10-1)- Styrene: 43.5 parts n-Butyl acrylate: 55.0 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were charged into a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (10-1).
[0197] -Emulsion (10-2)- Styrene: 38.5 parts n-Butyl acrylate: 60.0 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (10-2).
[0198] -Emulsion (10-3)- Styrene: 33.6 parts n-Butyl acrylate: 64.9 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (10-3).
[0199] -Emulsion (10-4)- Styrene: 28.6 parts n-Butyl acrylate: 69.9 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (10-4).
[0200] -Vinyl resin particle dispersion (10)- Vinyl-based resin particle dispersion liquid (10) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (10-1), emulsion (1-2) to emulsion (10-2), emulsion (1-3) to emulsion (10-3), and emulsion (1-4) to emulsion (10-4). The resulting resin particles had a volume average particle size of 165 nm and a glass transition temperature of -5°C as measured by a differential scanning calorimeter.
[0201] (Preparation of vinyl resin particle dispersion (11)) [Preparation of emulsions (11-1) to (11-4)] -Emulsion (11-1)- Styrene: 60.9 parts n-Butyl acrylate: 39.1 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (11-1).
[0202] -Emulsion (11-2)- Styrene: 55.8 parts n-Butyl acrylate: 44.2 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (11-2).
[0203] -Emulsion (11-3)- Styrene: 45.7 parts n-Butyl acrylate: 54.3 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (11-3).
[0204] -Emulsion (11-4)- Styrene: 40.6 parts n-Butyl acrylate: 59.4 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (11-4).
[0205] -Vinyl resin particle dispersion (11)- Vinyl-based resin particle dispersion liquid (11) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (11-1), emulsion (1-2) to emulsion (11-2), emulsion (1-3) to emulsion (11-3), and emulsion (1-4) to emulsion (11-4). The resulting resin particles had a volume average particle size of 165 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0206] (Preparation of vinyl resin particle dispersion (12)) [Preparation of emulsions (12-1) to (12-4)] -Emulsion (12-1)- Styrene: 40.0 parts n-Butyl acrylate: 58.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (12-1).
[0207] -Emulsion (12-2)- Styrene: 45.0 parts n-Butyl acrylate: 53.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (12-2).
[0208] -Emulsion (12-3)- Styrene: 55.0 parts n-Butyl acrylate: 43.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (12-3).
[0209] -Emulsion (12-4)- Styrene: 60.0 parts n-Butyl acrylate: 38.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (12-4).
[0210] -Vinyl resin particle dispersion (12)- Vinyl-based resin particle dispersion liquid (12) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (12-1), emulsion (1-2) to emulsion (12-2), emulsion (1-3) to emulsion (12-3), and emulsion (1-4) to emulsion (12-4). The resulting resin particles had a volume average particle size of 165 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0211] (Preparation of vinyl resin particle dispersion (13)) [Preparation of emulsions (13-1) to (13-4)] -Emulsion (13-1)- Styrene: 49.2 parts n-Butyl acrylate: 49.3 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (13-1).
[0212] -Emulsion (13-2)- Styrene: 48.5 parts n-Butyl acrylate: 50.0 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (13-2).
[0213] -Emulsion (13-3)- Styrene: 47.8 parts n-Butyl acrylate: 50.7 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (13-3).
[0214] -Emulsion (13-4)- Styrene: 47.2 parts n-Butyl acrylate: 51.3 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (13-4).
[0215] -Vinyl resin particle dispersion (13)- Vinyl-based resin particle dispersion liquid (13) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (13-1), emulsion (1-2) to emulsion (13-2), emulsion (1-3) to emulsion (13-3), and emulsion (1-4) to emulsion (13-4). The resulting resin particles had a volume average particle size of 164 nm and a glass transition temperature of 15° C. as measured by a differential scanning calorimeter.
[0216] (Preparation of vinyl resin particle dispersion (14)) [Preparation of emulsions (14-1) to (14-4)] -Emulsion (14-1)- Styrene: 53.0 parts n-Butyl acrylate: 45.0 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (14-1).
[0217] -Emulsion (14-2)- Styrene: 51.0 parts n-Butyl acrylate: 47.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (14-2).
[0218] -Emulsion (14-3)- Styrene: 49.0 parts n-Butyl acrylate: 49.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (14-3).
[0219] -Emulsion (14-4)- Styrene: 47.0 parts n-Butyl acrylate: 51.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (14-4).
[0220] -Vinyl resin particle dispersion (14)- Vinyl-based resin particle dispersion liquid (14) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (14-1), emulsion (1-2) to emulsion (14-2), emulsion (1-3) to emulsion (14-3), and emulsion (1-4) to emulsion (14-4). The resulting resin particles had a volume average particle size of 166 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0221] (Preparation of vinyl resin particle dispersion (15)) [Preparation of emulsions (15-1) to (15-4)] -Emulsion (15-1)- Styrene: 67.4 parts n-Butyl acrylate: 31.1 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (15-1).
[0222] -Emulsion (15-2)- Styrene: 55.8 parts n-Butyl acrylate: 42.7 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (15-2).
[0223] -Emulsion (15-3)- Styrene: 44.2 parts n-Butyl acrylate: 54.3 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (15-3).
[0224] -Emulsion (15-4)- Styrene: 32.6 parts n-Butyl acrylate: 65.9 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (15-4).
[0225] -Vinyl resin particle dispersion (15)- Vinyl-based resin particle dispersion liquid (15) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (15-1), emulsion (1-2) to emulsion (15-2), emulsion (1-3) to emulsion (15-3), and emulsion (1-4) to emulsion (15-4). The resulting resin particles had a volume average particle size of 165 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0226] (Preparation of vinyl resin particle dispersion (16)) [Preparation of emulsions (16-1) to (16-4)] -Emulsion (16-1)- Styrene: 71.1 parts n-Butyl acrylate: 27.4 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (16-1).
[0227] -Emulsion (16-2)- Styrene: 57.0 parts n-Butyl acrylate: 41.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (16-2).
[0228] -Emulsion (16-3)- Styrene: 43.0 parts n-Butyl acrylate: 55.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (16-3).
[0229] -Emulsion (16-4)- Styrene: 28.9 parts n-Butyl acrylate: 69.6 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (16-4).
[0230] -Vinyl resin particle dispersion (16)- Vinyl-based resin particle dispersion liquid (16) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (16-1), emulsion (1-2) to emulsion (16-2), emulsion (1-3) to emulsion (16-3), and emulsion (1-4) to emulsion (16-4). The resulting resin particles had a volume average particle size of 165 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0231] (Preparation of vinyl resin particle dispersion (17)) [Preparation of emulsions (17-1) to (17-4)] -Emulsion (17-1)- Styrene: 44.2 parts n-Butyl acrylate: 54.3 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (17-1).
[0232] -Emulsion (17-2)- Styrene: 48.1 parts n-Butyl acrylate: 50.4 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (17-2).
[0233] -Emulsion (17-3)- Styrene: 51.9 parts n-Butyl acrylate: 46.6 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (17-3).
[0234] -Emulsion (17-4)- Styrene: 55.7 parts n-Butyl acrylate: 42.8 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (17-4).
[0235] -Vinyl resin particle dispersion (17)- Vinyl-based resin particle dispersion liquid (17) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (17-1), emulsion (1-2) to emulsion (17-2), emulsion (1-3) to emulsion (17-3), and emulsion (1-4) to emulsion (17-4). The resulting resin particles had a volume average particle size of 165 nm and a glass transition temperature of 18° C. as measured by a differential scanning calorimeter.
[0236] (Preparation of vinyl resin particle dispersion (18)) [Preparation of emulsions (18-1) to (18-4)] -Emulsion (18-1)- Styrene: 48.3 parts n-Butyl acrylate: 50.2 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (18-1).
[0237] -Emulsion (18-2)- Styrene: 49.4 parts n-Butyl acrylate: 49.1 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (18-2).
[0238] -Emulsion (18-3)- Styrene: 50.5 parts n-Butyl acrylate: 48.0 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (18-3).
[0239] -Emulsion (18-4)- Styrene: 51.6 parts n-Butyl acrylate: 46.9 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (18-4).
[0240] -Vinyl resin particle dispersion (18)- Vinyl-based resin particle dispersion liquid (18) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (18-1), emulsion (1-2) to emulsion (18-2), emulsion (1-3) to emulsion (18-3), and emulsion (1-4) to emulsion (18-4). The resulting resin particles had a volume average particle size of 166 nm and a glass transition temperature of 18° C. as measured by a differential scanning calorimeter.
[0241] (Preparation of vinyl resin particle dispersion (19)) [Preparation of emulsions (19-1) to (19-4)] -Emulsion (19-1)- Styrene: 81.3 parts n-Butyl acrylate: 17.2 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (19-1).
[0242] -Emulsion (19-2)- Styrene: 60.4 parts n-Butyl acrylate: 38.1 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (19-2).
[0243] -Emulsion (19-3)- Styrene: 39.5 parts n-Butyl acrylate: 59.0 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (19-3).
[0244] -Emulsion (19-4)- Styrene: 18.7 parts n-Butyl acrylate: 79.8 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (19-4).
[0245] -Vinyl resin particle dispersion (19)- Vinyl-based resin particle dispersion liquid (19) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (19-1), emulsion (1-2) to emulsion (19-2), emulsion (1-3) to emulsion (19-3), and emulsion (1-4) to emulsion (19-4). The resulting resin particles had a volume average particle size of 167 nm and a glass transition temperature of 18° C. as measured by a differential scanning calorimeter.
[0246] (Preparation of vinyl resin particle dispersion (20)) [Preparation of emulsions (20-1 to 20-4)] -Emulsion (20-1)- Styrene: 85.6 parts n-Butyl acrylate: 12.9 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (20-1).
[0247] -Emulsion (20-2)- Styrene: 61.8 parts n-Butyl acrylate: 36.7 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (20-2).
[0248] -Emulsion (20-3)- Styrene: 38.1 parts n-Butyl acrylate: 60.4 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (20-3).
[0249] -Emulsion (20-4)- Styrene: 14.3 parts n-Butyl acrylate: 84.2 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (20-4).
[0250] -Vinyl resin particle dispersion (20)- A vinyl-based resin particle dispersion liquid (20) was obtained in the same manner as in the preparation of the vinyl-based resin particle dispersion liquid (1), except that the emulsion (1-1) was changed to emulsion (20-1), the emulsion (1-2) to emulsion (20-2), the emulsion (1-3) to emulsion (20-3), and the emulsion (1-4) to emulsion (20-4). The resulting resin particles had a volume average particle size of 165 nm and a glass transition temperature of 18° C. as measured by a differential scanning calorimeter.
[0251] (Preparation of vinyl resin particle dispersion (21)) [Preparation of emulsions (21-1) to (21-4)] -Emulsion (21-1)- Styrene: 49.0 parts n-Butyl acrylate: 49.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (21-1).
[0252] -Emulsion (21-2)- Styrene: 49.7 parts n-Butyl acrylate: 48.8 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (21-2).
[0253] -Emulsion (21-3)- Styrene: 50.3 parts n-Butyl acrylate: 48.2 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (21-3).
[0254] -Emulsion (21-4)- Styrene: 51.0 parts n-Butyl acrylate: 47.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (21-4).
[0255] -Vinyl resin particle dispersion (21)- Vinyl-based resin particle dispersion liquid (21) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (21-1), emulsion (1-2) to emulsion (21-2), emulsion (1-3) to emulsion (21-3), and emulsion (1-4) to emulsion (21-4). The resulting resin particles had a volume average particle size of 163 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0256] (Preparation of vinyl resin particle dispersion (22)) [Preparation of emulsions (22-1) to (22-4)] -Emulsion (22-1)- Styrene: 47.0 parts n-Butyl acrylate: 51.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (22-1).
[0257] -Emulsion (22-2)- Styrene: 49.0 parts n-Butyl acrylate: 49.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (22-2).
[0258] -Emulsion (22-3)- Styrene: 51.0 parts n-Butyl acrylate: 47.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (22-3).
[0259] -Emulsion (22-4)- Styrene: 53.0 parts n-Butyl acrylate: 45.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (22-4).
[0260] -Vinyl resin particle dispersion (22)- Vinyl-based resin particle dispersion liquid (22) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (22-1), emulsion (1-2) to emulsion (22-2), emulsion (1-3) to emulsion (22-3), and emulsion (1-4) to emulsion (22-4). The resulting resin particles had a volume average particle size of 167 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0261] (Preparation of vinyl resin particle dispersion (23)) [Preparation of emulsions (23-1) to (23-4)] -Emulsion (23-1)- Styrene: 31.2 parts n-Butyl acrylate: 67.3 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (23-1).
[0262] -Emulsion (23-2)- Styrene: 43.7 parts n-Butyl acrylate: 54.8 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (23-2).
[0263] -Emulsion (23-3)- Styrene: 56.3 parts n-Butyl acrylate: 42.2 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (23-3).
[0264] -Emulsion (23-4)- Styrene: 68.8 parts n-Butyl acrylate: 29.7 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (23-4).
[0265] -Vinyl resin particle dispersion (23)- Vinyl-based resin particle dispersion liquid (23) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (23-1), emulsion (1-2) to emulsion (23-2), emulsion (1-3) to emulsion (23-3), and emulsion (1-4) to emulsion (23-4). The resulting resin particles had a volume average particle size of 165 nm and a glass transition temperature of 17° C. as measured by a differential scanning calorimeter.
[0266] (Preparation of vinyl resin particle dispersion (24)) [Preparation of emulsions (24-1) to (24-4)] -Emulsion (24-1)- Styrene: 23.5 parts n-Butyl acrylate: 75.0 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (24-1).
[0267] -Emulsion (24-2)- Styrene: 38.7 parts n-Butyl acrylate: 58.8 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (24-2).
[0268] -Emulsion (24-3)- Styrene: 54.0 parts n-Butyl acrylate: 44.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (24-3).
[0269] -Emulsion (24-4)- Styrene: 69.2 parts n-Butyl acrylate: 29.3 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (24-4).
[0270] -Vinyl resin particle dispersion (24)- Vinyl-based resin particle dispersion liquid (24) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (24-1), emulsion (1-2) to emulsion (24-2), emulsion (1-3) to emulsion (24-3), and emulsion (1-4) to emulsion (24-4). The resulting resin particles had a volume average particle size of 164 nm and a glass transition temperature of 12° C. as measured by a differential scanning calorimeter.
[0271] (Preparation of vinyl resin particle dispersion (25)) [Preparation of emulsions (25-1) to (25-4)] -Emulsion (25-1)- Styrene: 67.1 parts n-Butyl acrylate: 31.4 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (25-1).
[0272] -Emulsion (25-2)- Styrene: 55.7 parts n-Butyl acrylate: 42.8 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (25-2).
[0273] -Emulsion (25-3)- Styrene: 44.2 parts n-Butyl acrylate: 54.3 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (25-3).
[0274] -Emulsion (25-4)- Styrene: 32.8 parts n-Butyl acrylate: 65.7 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (25-4).
[0275] -Vinyl resin particle dispersion (25)- Vinyl-based resin particle dispersion liquid (25) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (25-1), emulsion (1-2) to emulsion (25-2), emulsion (1-3) to emulsion (25-3), and emulsion (1-4) to emulsion (25-4). The resulting resin particles had a volume average particle size of 166 nm and a glass transition temperature of 18° C. as measured by a differential scanning calorimeter.
[0276] (Preparation of vinyl resin particle dispersion (26)) [Preparation of emulsions (26-1) to (26-4)] -Emulsion (26-1)- Styrene: 63.4 parts n-Butyl acrylate: 35.1 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (26-1).
[0277] -Emulsion (26-2)- Styrene: 54.4 parts n-Butyl acrylate: 44.1 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (26-2).
[0278] -Emulsion (26-3)- Styrene: 45.5 parts n-Butyl acrylate: 53.0 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (26-3).
[0279] -Emulsion (26-4)- Styrene: 36.6 parts n-Butyl acrylate: 61.9 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (26-4).
[0280] -Vinyl resin particle dispersion (26)- Vinyl resin dispersion (26) was obtained in the same manner as in the preparation of vinyl resin particle dispersion (1), except that emulsion (1-1) was changed to emulsion (26-1), emulsion (1-2) to emulsion (26-2), emulsion (1-3) to emulsion (26-3), and emulsion (1-4) to emulsion (26-4). The resulting resin particles had a volume average particle size of 165 nm and a glass transition temperature of 18° C. as measured by a differential scanning calorimeter.
[0281] (Preparation of vinyl resin particle dispersion (27)) [Preparation of emulsions (27-1) to (27-4)] -Emulsion (27-1)- Styrene: 27.6 parts n-Butyl acrylate: 70.9 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (27-1).
[0282] -Emulsion (27-2)- Styrene: 42.5 parts n-Butyl acrylate: 56.0 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (27-2).
[0283] -Emulsion (27-3)- Styrene: 57.4 parts n-Butyl acrylate: 41.1 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (27-3).
[0284] -Emulsion (27-4)- Styrene: 72.4 parts n-Butyl acrylate: 26.1 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (27-4).
[0285] -Vinyl resin particle dispersion (27)- Vinyl resin particle dispersion liquid (27) was obtained in the same manner as in the preparation of vinyl resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (27-1), emulsion (1-2) to emulsion (27-2), emulsion (1-3) to emulsion (27-3), and emulsion (1-4) to emulsion (27-4). The resulting resin particles had a volume average particle size of 164 nm and a glass transition temperature of 18° C. as measured by a differential scanning calorimeter.
[0286] (Preparation of vinyl resin particle dispersion (28)) [Preparation of emulsions (28-1) to (28-4)] -Emulsion (28-1)- Styrene: 22.0 parts n-Butyl acrylate: 76.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (28-1).
[0287] -Emulsion (28-2)- Styrene: 40.6 parts n-Butyl acrylate: 57.9 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (28-2).
[0288] -Emulsion (28-3)- Styrene: 59.3 parts n-Butyl acrylate: 39.2 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (28-3).
[0289] -Emulsion (28-4)- Styrene: 78.0 parts n-Butyl acrylate: 20.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (28-4).
[0290] -Vinyl resin particle dispersion (28)- Vinyl resin particle dispersion liquid (28) was obtained in the same manner as in the preparation of vinyl resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (28-1), emulsion (1-2) to emulsion (28-2), emulsion (1-3) to emulsion (28-3), and emulsion (1-4) to emulsion (28-4). The resulting resin particles had a volume average particle size of 166 nm and a glass transition temperature of 18° C. as measured by a differential scanning calorimeter.
[0291] (Preparation of vinyl resin particle dispersion (29)) [Preparation of emulsions (29-1) to (29-4)] -Emulsion (29-1)- Styrene: 57.8 parts n-Butyl acrylate: 40.7 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (29-1).
[0292] -Emulsion (29-2)- Styrene: 53.0 parts n-Butyl acrylate: 45.5 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (29-2).
[0293] -Emulsion (29-3)- Styrene: 43.3 parts n-Butyl acrylate: 55.2 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (29-3).
[0294] -Emulsion (29-4)- Styrene: 38.5 parts n-Butyl acrylate: 60.0 parts 1,10-Decanediol diacrylate: 1.5 parts Anionic surfactant (Eleminol MON-2): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare an emulsion (29-4).
[0295] -Vinyl resin particle dispersion (29)- Vinyl-based resin particle dispersion liquid (29) was obtained in the same manner as in the preparation of vinyl-based resin particle dispersion liquid (1), except that emulsion (1-1) was changed to emulsion (29-1), emulsion (1-2) to emulsion (29-2), emulsion (1-3) to emulsion (29-3), and emulsion (1-4) to emulsion (29-4), and the amount of anionic surfactant (Eleminol MON-2) was changed from 1.1 parts to 2.7 parts. The resulting resin particles had a volume average particle size of 120 nm and a glass transition temperature of 15° C. as measured by a differential scanning calorimeter.
[0296] (Preparation of vinyl resin particle dispersion (30)) Styrene: 77 parts n-Butyl acrylate: 23 parts 1,10-Decanediol diacrylate: 0.4 parts Dodecanethiol: 0.7 parts The above materials were mixed and dissolved, and a solution of 1.0 part of anionic surfactant (Dowfax, manufactured by The Dow Chemical Company) dissolved in 60 parts of ion-exchanged water was added to the mixture, and the mixture was dispersed and emulsified in a flask to produce an emulsion. Next, 3 parts of an anionic surfactant (Dowfax manufactured by Dow Chemical Company) was dissolved in 90 parts of ion-exchanged water, 30 parts of the emulsion was added thereto, and 10 parts of ion-exchanged water in which 1.0 part of ammonium persulfate had been dissolved was further added. Thereafter, the remainder of the emulsion was added over a period of 3 hours, and the atmosphere in the flask was replaced with nitrogen. The solution in the flask was then heated to 65°C in an oil bath while stirring, and emulsion polymerization was continued for 5 hours to obtain a vinyl resin particle dispersion (29). The solid content of the vinyl resin particle dispersion (29) was adjusted to 32% by adding ion-exchanged water as necessary.
[0297] In Table 1, the vinyl resin particle dispersions (1) to (30) are abbreviated as Vinyl 1 to 30.
[0298] <Preparation of rubber particle dispersion> (Preparation of styrene butadiene rubber particle dispersion (1)) In a polymerization reactor, 400 parts of ion-exchanged water, 100 parts of styrene, 80 parts of butadiene, 24 parts of methyl acrylate, 8 parts of acrylic acid, 6 parts of potassium persulfate, and 3 parts of n-dodecyl mercaptan were placed and polymerized for 5 hours under a nitrogen atmosphere at a temperature of 85°C, and then the reaction was continued for 2 hours to terminate the polymerization. The obtained dispersion was adjusted to a solid content concentration of 20% to obtain a rubber particle dispersion. The glass transition temperature of the rubber particles was -20°C, and the volume average particle size was 180 nm. In Table 1, the styrene-butadiene rubber particle dispersion (1) is abbreviated as Rubber 1.
[0299] <Preparation of colorant dispersion> (Preparation of Colorant Dispersion (1)) Cyan pigment (Pigment Blue 15:3 (copper phthalocyanine), manufactured by Dainichi Seika Chemicals): 98 parts Anionic surfactant (Neopelex G-65, Kao): 2 parts - Ion-exchanged water: 400 parts The above components were mixed and then dispersed using a homogenizer (IKA Ultra Turrax T50) to obtain a colorant dispersion (1) having a volume average particle size of 160 nm and a solid content concentration of 20%.
[0300] (Preparation of Colorant Dispersion (2)) Carbon black (Regal 330, manufactured by Cabot Corporation): 98 parts Anionic surfactant (Neopelex G-65, Kao): 2 parts - Ion-exchanged water: 400 parts The above components were mixed and then dispersed using a homogenizer (Ultra Turrax T50, manufactured by IKA Corporation) to obtain a colorant dispersion (2) having a volume average particle size of 180 nm and a solid content concentration of 20%.
[0301] (Preparation of Colorant Dispersion (3)) Carbon black (Cabot, Regal 330): 250 parts Anionic surfactant (Daiichi Kogyo Seiyaku Co., Ltd., Neogen SC): 33 parts (60% active ingredient, 8% colorant) -Ion-exchanged water: 750 parts 280 parts of ion-exchanged water and 33 parts of anionic surfactant were placed in a stainless steel container of a size such that the height of the liquid surface would be about 1 / 3 of the height of the container when all of the above components were added, and after the surfactant was sufficiently dissolved, all of the solid solution pigment was added and stirred with a stirrer until there was no unwetted pigment, and the mixture was sufficiently defoamed. After defoaming, the remaining ion-exchanged water was added, and the mixture was dispersed for 10 minutes at 5000 rpm using a homogenizer (IKA Ultra Turrax T50), and then defoamed by stirring with a stirrer for 1 day and night. After defoaming, the mixture was dispersed again for 10 minutes at 6000 rpm using a homogenizer, and then defoamed by stirring with a stirrer for 1 day and night. Subsequently, the dispersion was dispersed at a pressure of 240 MPa using a high-pressure impact disperser Ultimizer (Sugino Machine Co., Ltd., HJP30006). Dispersion was performed for 25 passes, calculated from the total amount charged and the processing capacity of the device. The obtained dispersion liquid was left for 72 hours to remove the precipitate, and ion-exchanged water was added to adjust the solid concentration to 15%, to obtain colorant particle dispersion liquid (3). The volume average particle diameter D50 of the particles in this colorant particle dispersion liquid (3) was 135 nm.
[0302] In Table 1, the colorant dispersion (1) prepared as above is abbreviated as Cyan1, the colorant dispersion (2) as Black1, and the colorant dispersion (3) as Black2.
[0303] <Preparation of release agent dispersion> (Preparation of release agent dispersion (1)) Synthetic wax (FT100, made by Nippon Seiro): 100 parts Anionic surfactant (Neopelex G-65, Kao): 5 parts - Ion-exchanged water: 300 parts After mixing the above components, the mixture was heated to 100°C and dispersed using a homogenizer (Ultra Turrax T50 manufactured by IKA). The mixture was further dispersed using a Manton-Gaulin high pressure homogenizer (manufactured by Gaulin), and ion-exchanged water was added to the dispersion to obtain a release agent dispersion (1) with a solid content of 20%. The volume average particle size of the release agent particles in the release agent dispersion (1) was 230 nm.
[0304] (Preparation of release agent dispersion (2)) Polyethylene wax (hydrocarbon wax: trade name "Polywax 725 (manufactured by Baker Petrolite Co., Ltd.)", melting temperature 104°C): 270 parts Anionic surfactant (Dai-ichi Kogyo Seiyaku Co., Ltd., Neogen RK, active ingredient amount: 60%): 13.5 parts (as an active ingredient, 3.0% relative to the release agent) Ion-exchanged water: 21.6 parts The above components were mixed, and the release agent was dissolved in a pressure discharge homogenizer (Gaulin homogenizer, manufactured by Gaulin Co., Ltd.) at an internal liquid temperature of 120°C. The mixture was then dispersed at a dispersion pressure of 5 MPa for 120 minutes, then at 40 MPa for 360 minutes, and cooled to obtain a release agent dispersion (2). The volume average particle size D50 of the particles in this release agent dispersion (1) was 225 nm. Ion-exchanged water was then added to adjust the solid content concentration to 20.0%.
[0305] In Table 1, the release agent dispersions (1) and (2) prepared above are abbreviated as WAX1 and WAX2.
[0306] <Preparation of Mixed Particle Dispersion (1): Comparative Example 5 Used for Toner 47> 400 parts of the amorphous polyester resin particle dispersion (7), 60 parts of the release agent dispersion (2), and 2.9 parts of an anionic surfactant (Dowfax2A1, manufactured by The Dow Chemical Company) were mixed, and then 1.0% nitric acid was added at a temperature of 25° C. to adjust the pH to 3.0, thereby obtaining a mixed particle dispersion (1).
[0307] <Example 1> (Preparation of Toner (1)) Amorphous polyester resin particle dispersion (1) (solid content 20% by mass): 492 parts Crystalline polyester resin particle dispersion (1) (solid content 20% by mass): 228 parts Colorant dispersion (1) (solid content 20% by mass): 90 parts Release agent dispersion (1) (solid content 20% by mass): 120 parts Anionic surfactant Eleminol MON-2: 10.5 parts -Ion-exchanged water: 750 parts The above components were placed in a 3-liter reaction vessel equipped with a thermometer, a pH meter, a stirrer, and a 20 cm diameter stirring blade, and the mixture was maintained for 30 minutes while stirring at 35 rpm and keeping the temperature of the reaction vessel at 20° C. Then, a 0.3 N aqueous solution of nitric acid was added to adjust the pH to 4.5. Next, in a vessel equipped with a stirrer and stirring blades, Vinyl resin particle dispersion (1) (solid content 20% by mass): 150.0 parts The pH was adjusted to 4.5 with stirring. Next, while the 3-liter reaction vessel was kept at 20° C. and stirred at 35 rpm, the vinyl resin particle dispersion liquid (1) after pH adjustment was added dropwise at a rate of 7 g / min. Next, a 2% aqueous aluminum sulfate solution was added while dispersing with a homogenizer (Ultra Turrax T50), and the mixture was heated to 45°C at a rate of 0.4°C / min while stirring, and maintained at that temperature for 30 minutes. Next, 420 parts of the amorphous polyester resin particle dispersion liquid (1) was added and held for 30 minutes. Next, a 0.1N aqueous sodium hydroxide solution was added to adjust the pH to 8.5 and held for 15 minutes, and then the temperature was raised to 80°C at a rate of 1°C / min while continuing to stir, and 80°C was held for 5 hours. Next, the mixture was cooled, solid-liquid separated, and the solid matter was washed with ion-exchanged water, and then dried in a vacuum freeze dryer for 24 hours to obtain toner particles (1) having a volume average particle size of 5.5 μm. 100 parts of the toner particles (1) and 2.0 parts of hydrophobic silica (manufactured by Nippon Aerosil: product name RY200) were mixed in a Henschel mixer to obtain a toner (1).
[0308] <Example 2> Toner 2 was obtained in the same manner as in Example 1, except that the vinyl-based resin particle dispersion (2) was used instead of the vinyl-based resin particle dispersion (1).
[0309] <Example 3> Toner 3 was obtained in the same manner as in Example 1, except that 552 parts of amorphous polyester resin particle dispersion liquid (1) were used instead of 492 parts, 243 parts of crystalline polyester resin particle dispersion liquid (1) were used instead of 228 parts, and 75 parts of vinyl resin particle dispersion liquid (3) were used instead of 150.0 parts of vinyl resin particle dispersion liquid (1).
[0310] <Example 4> Amorphous polyester resin particle dispersion (1): 420 parts instead of 492 parts, crystalline polyester resin particle dispersion (1): 210 parts instead of 228 parts, vinyl resin particle dispersion (1): 150.0 parts instead of vinyl resin particle dispersion (4): 240 parts were used. Other than that, the same procedure as in Example 1 was carried out to obtain Toner 4.
[0311] <Example 5> Toner 5 was obtained in the same manner as in Example 1, except that the vinyl-based resin particle dispersion (5) was used instead of the vinyl-based resin particle dispersion (1).
[0312] <Example 6> Toner 6 was obtained in the same manner as in Example 1, except that the vinyl-based resin particle dispersion (6) was used instead of the vinyl-based resin particle dispersion (1).
[0313] <Example 7> Toner 7 was obtained in the same manner as in Example 1, except that 384 parts of amorphous polyester resin particle dispersion liquid (1) were used instead of 492 parts, 201 parts of crystalline polyester resin particle dispersion liquid (1) were used instead of 228 parts, and 285 parts of vinyl resin particle dispersion liquid (3) were used instead of 150.0 parts of vinyl resin particle dispersion liquid (1).
[0314] <Example 8> Toner 8 was obtained in the same manner as in Example 1, except that 396 parts of amorphous polyester resin particle dispersion liquid (1) were used instead of 492 parts, 204 parts of crystalline polyester resin particle dispersion liquid (1) were used instead of 228 parts, and 270 parts of vinyl resin particle dispersion liquid (7) were used instead of 150.0 parts of vinyl resin particle dispersion liquid (1).
[0315] <Example 9> Toner 9 was obtained in the same manner as in Example 1, except that 516 parts of amorphous polyester resin particle dispersion liquid (1) were used instead of 492 parts, 234 parts of crystalline polyester resin particle dispersion liquid (1) were used instead of 228 parts, and 120 parts of vinyl resin particle dispersion liquid (8) were used instead of 150.0 parts of vinyl resin particle dispersion liquid (1).
[0316] <Example 10> Toner 10 was obtained in the same manner as in Example 1, except that 560.4 parts of amorphous polyester resin particle dispersion (1) were used instead of 492 parts, 245.1 parts of crystalline polyester resin particle dispersion (1) were used instead of 228 parts, and 64.5 parts of vinyl resin particle dispersion (1) were used instead of 150.0 parts.
[0317] <Example 11> Toner 11 was obtained in the same manner as in Example 1, except that 372 parts of amorphous polyester resin particle dispersion liquid (1) were used instead of 492 parts, 198 parts of crystalline polyester resin particle dispersion liquid (1) were used instead of 228 parts, and 300 parts of vinyl resin particle dispersion liquid (3) were used instead of 150.0 parts of vinyl resin particle dispersion liquid (1).
[0318] <Example 12> Toner 12 was obtained in the same manner as in Example 1, except that the vinyl-based resin particle dispersion (9) was used instead of the vinyl-based resin particle dispersion (1).
[0319] <Example 13> Toner 13 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (10) was used instead of the vinyl resin particle dispersion (1).
[0320] <Example 14> Toner 14 was obtained in the same manner as in Example 1, except that 720 parts of the amorphous polyester resin particle dispersion (1) was used instead of 492 parts, and 0 parts of the crystalline polyester resin particle dispersion (1) was used instead of 228 parts.
[0321] <Example 15> Toner 15 was obtained in the same manner as in Example 1, except that 702 parts of amorphous polyester resin particle dispersion (1) were used instead of 492 parts, and 210 parts of amorphous polyester resin particles were added after heating to 45°C instead of 420 parts.
[0322] <Example 16> Toner 16 was obtained in the same manner as in Example 1, except that 792 parts of amorphous polyester resin particle dispersion (1) were used instead of 492 parts, and 120 parts of amorphous polyester resin particles were added after heating to 45°C instead of 420 parts.
[0323] <Example 17> Toner 17 was obtained in the same manner as in Example 1, except that the stirring speed during mixing of the materials was changed from 35 rpm to 45 rpm, and the adjusted pH of the vinyl resin particle dispersion liquid (1) was changed from 4.5 to 4.7.
[0324] <Example 18> Toner 18 was obtained in the same manner as in Example 1, except that the stirring speed during mixing of the materials was changed from 35 rpm to 54 rpm, and vinyl-based resin particle dispersion liquid (4) was used instead of vinyl-based resin particle dispersion liquid (1).
[0325] <Example 19> Toner 19 was obtained in the same manner as in Example 1, except that colorant dispersion (2) was used instead of colorant dispersion (1).
[0326] <Example 20> A toner 20 was obtained in the same manner as in Example 1, except that the amorphous polyester resin particle dispersion (2) was used instead of the amorphous polyester resin particle dispersion (1).
[0327] <Example 21> Toner 21 was obtained in the same manner as in Example 1, except that the vinyl-based resin particle dispersion (11) was used instead of the vinyl-based resin particle dispersion (1).
[0328] <Example 22> Toner 22 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (12) was used instead of the vinyl resin particle dispersion (1).
[0329] <Example 23> Toner 23 was obtained in the same manner as in Example 1, except that the amorphous polyester resin particle dispersion (1) was replaced with the amorphous polyester resin particle dispersion (3).
[0330] <Example 24> Toner 24 was obtained in the same manner as in Example 1, except that the amorphous polyester resin particle dispersion (4) was used instead of the amorphous polyester resin particle dispersion (1).
[0331] <Example 25> Toner 25 was obtained in the same manner as in Example 1, except that the amorphous polyester resin particle dispersion (5) was used instead of the amorphous polyester resin particle dispersion (1).
[0332] <Example 26> Toner 26 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (13) was used instead of the vinyl resin particle dispersion (1).
[0333] <Example 27> Toner 27 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (14) was used instead of the vinyl resin particle dispersion (1).
[0334] <Example 28> Toner 28 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (15) was used instead of the vinyl resin particle dispersion (1).
[0335] <Example 29> Toner 29 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (16) was used instead of the vinyl resin particle dispersion (1).
[0336] <Example 30> A toner 30 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (17) was used instead of the vinyl resin particle dispersion (1).
[0337] <Example 31> Toner 31 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (18) was used instead of the vinyl resin particle dispersion (1).
[0338] <Example 32> Toner 32 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (19) was used instead of the vinyl resin particle dispersion (1).
[0339] <Example 33> Toner 33 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (20) was used instead of the vinyl resin particle dispersion (1). <Example 34> Toner 34 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (21) was used instead of the vinyl resin particle dispersion (1).
[0340] <Example 35> Toner 35 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (22) was used instead of the vinyl resin particle dispersion (1).
[0341] <Example 36> Toner 36 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (23) was used instead of the vinyl resin particle dispersion (1).
[0342] <Example 37> Toner 37 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (24) was used instead of the vinyl resin particle dispersion (1).
[0343] <Example 38> Toner 38 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (25) was used instead of the vinyl resin particle dispersion (1).
[0344] <Example 39> Toner 39 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (26) was used instead of the vinyl resin particle dispersion (1).
[0345] <Example 40> A toner 40 was obtained in the same manner as in Example 1, except that the vinyl-based resin particle dispersion (27) was used instead of the vinyl-based resin particle dispersion (1).
[0346] <Example 41> Toner 41 was obtained in the same manner as in Example 1, except that the vinyl resin particle dispersion (28) was used instead of the vinyl resin particle dispersion (1).
[0347] <Example 42> Toner 42 was obtained in the same manner as in Example 1, except that the amorphous polyester resin particle dispersion (6) was used instead of the amorphous polyester resin particle dispersion (1).
[0348] <Comparative Example 1> Toner 43 was obtained in the same manner as in Example 1, except that 390 parts of amorphous polyester resin particle dispersion liquid (1) were used instead of 492 parts, 202.5 parts of crystalline polyester resin particle dispersion liquid (1) were used instead of 228 parts, and 277.5 parts of vinyl resin particle dispersion liquid (29) were used instead of 150.0 parts of vinyl resin particle dispersion liquid (1).
[0349] <Comparative Example 2> Toner 44 was obtained in the same manner as in Example 1, except that 498 parts of amorphous polyester resin particle dispersion liquid (1) were used instead of 492 parts, 229.5 parts of crystalline polyester resin particle dispersion liquid (1) were used instead of 228 parts, and 142.5 parts of vinyl resin particle dispersion liquid (29) were used instead of 150.0 parts of vinyl resin particle dispersion liquid (1).
[0350] <Comparative Example 3> Toner 45 was obtained in the same manner as in Example 1, except that the stirring speed during mixing of the materials was changed from 35 rpm to 100 rpm, and the adjusted pH of the vinyl resin particle dispersion liquid (1) was changed from 4.5 to 5.2.
[0351] <Comparative Example 4> Toner 46 was obtained in the same manner as in Example 1, except that the vinyl-based resin particle dispersion (1) was replaced with the styrene-butadiene rubber particle dispersion (1).
[0352] <Comparative Example 5> Amorphous polyester resin particle dispersion (7): 700 parts Crystalline polyester resin particle dispersion (2): 50 parts Vinyl resin particle dispersion (30): 205 parts Colorant dispersion (3): 133 parts Release agent dispersion (2): 15 parts Ion exchange water: 600 parts Anionic surfactant (Dowfax2A1, manufactured by The Dow Chemical Company): 2.9 parts The above materials were placed in a 3-liter reaction vessel equipped with a thermometer, a pH meter, and a stirrer, and 1.0% nitric acid was added at 25° C. to adjust the pH to 3.0. Then, 100 parts of a 2% aqueous aluminum sulfate solution was added while dispersing the materials at 3,000 rpm using a homogenizer (IKA Ultra Turrax T50). During the dropping of the coagulant, the viscosity of the raw dispersion liquid increased rapidly, so the dropping speed was slowed down at the point where the viscosity increased so that the coagulant would not be concentrated in one place. After the dropping of the coagulant was completed, the rotation speed was increased to 5,000 rpm and the mixture was stirred for 5 minutes. Thereafter, a stirrer and a mantle heater were placed in the reaction vessel, and while adjusting the rotation speed of the stirrer so that the slurry was sufficiently stirred, the temperature was increased at a rate of 0.2°C / min up to 40°C, and then at a rate of 0.05°C / min from 40°C to 53°C, and the particle size was measured every 10 minutes using a Multisizer II (aperture diameter 50 μm, manufactured by Beckman Coulter, Inc.). When the volume average particle size reached 5.0 μm, the temperature was maintained, and 460 parts of the mixed particle dispersion (1) was added over a period of 5 minutes. After keeping at 50°C for 30 minutes, 8 parts of 20% EDTA (ethylenediaminetetraacetic acid) solution was added to the reaction vessel to stop the growth of the aggregated particles that formed the coating layer, and then 1 mole / liter of sodium hydroxide aqueous solution was added to control the pH of the raw material dispersion at 9.0. Thereafter, the temperature was raised to 90°C at a rate of 1°C / min while adjusting the pH to 9.0 every 5°C, and the temperature was maintained at 90°C. When the particle shape and surface properties were observed with an optical microscope and a field emission scanning electron microscope (FE-SEM), particle coalescence was confirmed at the 6th hour, so the vessel was cooled to 30°C over 5 minutes with cooling water. The cooled slurry was passed through a nylon mesh with 15 μm openings to remove coarse powder, and the toner slurry that passed through the mesh was filtered under reduced pressure with an aspirator. The solids remaining on the filter paper were crushed as finely as possible by hand, and then added to ion-exchanged water at a temperature of 30° C. with 10 times the amount of solids, and mixed by stirring for 30 minutes. The mixture was then filtered under reduced pressure with an aspirator, and the solids remaining on the filter paper were crushed as finely as possible by hand, and then added to ion-exchanged water at a temperature of 30° C. with 10 times the amount of solids, and then mixed by stirring for 30 minutes. The mixture was then filtered under reduced pressure with an aspirator again, and the electrical conductivity of the filtrate was measured. This operation was repeated until the electrical conductivity of the filtrate was 10 μS / cm or less, and the solids were washed. The washed solid content was finely crushed with a wet-dry type granulator (Comil) and vacuum dried in an oven at 35° C. for 36 hours to obtain toner particles (47). The toner particles (47) had a volume average particle size of 6.0 μm. 100 parts of the toner particles (47) and 2.0 parts of hydrophobic silica (manufactured by Nippon Aerosil: product name RY200) were mixed in a Henschel mixer to obtain a toner (47).
[0353] <Various physical properties> The following characteristics of the toner of each example are shown in Table 1.
[0354] The median of the area Sa of the Voronoi polygons is Sac (μm 2 ) Standard deviation Ssd of the area Sa of the Voronoi polygon (μm 2 ) The area Sa (μm) of the Voronoi polygon when Voronoi division is performed with the geometric center of the vinyl resin particle as the generating point 2 )
[0355] - Volume average particle size D50v of internally added resin particles (vinyl resin particles, rubber particles) · Glass transition temperature Tg of internal resin particles (vinyl resin particles, rubber particles) The length of the part of the contour line of a toner particle that overlaps with the internal resin particle (vinyl resin particle, etc.) (the ratio of the length of the part of the contour line of a toner particle that overlaps with the internal resin particle (vinyl resin particle, etc.) to the length of the contour line of the toner particle) Lout Average circle equivalent diameter Dce of internally added resin particles (vinyl resin particles, rubber particles) Proportion Wa(B) (mol%) of structural units derived from (meth)acrylate in the entire styrene-(meth)acrylate copolymer particles (St / Ac) as internal resin particles Proportion of structural units derived from (meth)acrylate on the surface of styrene-(meth)acrylate copolymer particles (St / Ac) as internal resin particles Wa(S) (mol%) Proportion of structural units derived from styrene in the entire styrene-(meth)acrylate copolymer particles (St / Ac) as internal resin particles Ws(B) (mol%) The proportion of styrene on the surface of styrene-(meth)acrylate copolymer particles (St / Ac) as internal resin particles, Ws(S) (mol%)
[0356] Solubility parameter SP(sa) of the surface of the internally added resin particles (vinyl resin particles, rubber particles) Solubility parameter SP(ap) of binder resin (amorphous polyester resin)
[0357] - Ratio of isophthalic acid to polycarboxylic acid in amorphous polyester resin (IPA ratio)
[0358] <Evaluation> (Preparation of developer) 8 parts of the toner of each example was mixed with 100 parts of a carrier prepared by the following procedure to obtain a developer. -Creating the carrier- Ferrite particles (average particle size 50 μm) 100 parts Toluene 14 parts Styrene / methyl methacrylate copolymer (copolymer ratio 15 / 85) 3 parts Carbon black 0.2 parts The above components except for the ferrite particles were dispersed in a sand mill to prepare a dispersion liquid, and this dispersion liquid was placed in a vacuum degassing kneader together with the ferrite particles, and the mixture was dried under reduced pressure while stirring to obtain a carrier.
[0359] (Fine line resolution maintenance) The developer containing each of the toners was filled into the developing machine of a color printer "ApeosPrint C5570 (manufactured by FUJIFILM Business Innovation Co., Ltd.). This color copying machine was left standing under high temperature and high humidity conditions (28° C., 85% RH) for 12 hours. Then, an image in which thin lines of 20 μm width were arranged at 3 cm intervals on A4 paper was outputted under the same environment using a color copier. After outputting 500,000 sheets, the state of the thin lines was observed and evaluated according to the following criteria. A: Even when observed with a loupe at 100x magnification, no fine line blurring is observed at all. (Acceptable range) B: Between A and C (tolerance range) C: When observed with a loupe at 100x magnification, slight fine line blurring is partially observed (within acceptable range). D: Between C and E (tolerance range) E: When observed using a loupe at 100x magnification, slight fine line blurring is observed overall (within the acceptable range). F: Slight fine line blurring is visible overall (within acceptable range) G: Fine line blur is clearly visible overall. (Fail)
[0360] Examples are listed in Table 1. In Table 1, "Shell layer Amo ratio" indicates the ratio (mass %) of the amorphous resin in the shell layer to the toner particles.
[0361] [Table 1-1]
[0362] [Table 1-2]
[0363] [Table 1-3]
[0364] [Table 1-4]
[0365] [Table 1-5]
[0366] From the above results, it is understood that the present embodiment is superior in maintaining fine line resolution under high temperature and high humidity conditions as compared with the comparative example.
[0367] The present embodiment includes the following aspects. (((1))) The toner particles include a binder resin and vinyl resin particles, In observing the cross section of the toner particle, the area Sa (μm of the Voronoi polygon when Voronoi division is performed with the geometric center of the vinyl resin particle as the base point is determined. 2 ), the median of the area Sa of the Voronoi polygon is defined as Sac (μm 2 ), the standard deviation of the area Sa of the Voronoi polygon is Ssd (μm 2 ) a toner for developing electrostatic images that satisfies the following formulas (1) and (2): Equation (1): 0.03≦Sac≦0.20 Formula (2): Ssd≦0.10 (((2))) The toner for developing electrostatic images according to (((1))) above, which satisfies the following formula (11): Equation (11): 0.08≦Sac≦0.16 (((3))) The toner for developing electrostatic images according to (((1))) or (((2))), which satisfies the following formula (21): Formula (21) Ssd≦0.07 (((4))) The toner for developing electrostatic images according to any one of (((1))) to (((3))), wherein, upon cross-sectional observation of the toner particle, the ratio of the area of the vinyl resin particles to the area of the toner particle is greater than 0.15 and is 0.40 or less. (((5))) The toner for developing electrostatic images according to any one of ((1))) to (((4))), wherein the volume average particle size of the vinyl resin particles is 100 nm or more and 300 nm or less. (((6))) The toner for developing electrostatic images according to any one of ((1))) to (((5))), wherein the glass transition temperature of the vinyl resin particles is from 0° C. to 30° C. (((7))) The toner for developing electrostatic images according to any one of (((1))) to (((6))), wherein, in a cross-sectional observation of the toner particle, the number ratio of the vinyl-based resin particles observed to be overlapped is 50% or less of all the vinyl-based resin particles observed. (((8))) The toner for developing electrostatic images according to any one of (((1))) to (((7))), wherein, upon observation of a cross section of the toner particle, the length of a portion of the contour line of the toner particle that overlaps with the vinyl resin particle is 5% or less of the length of the contour line of the toner particle. (((9))) The toner for developing electrostatic images according to any one of ((1))) to (((8))), wherein, upon cross-sectional observation of the toner particles, the average equivalent circular diameter of the vinyl resin particles observed is 400 nm or less. (((10))) the vinyl-based resin particles are styrene-(meth)acrylate copolymer particles, a ratio Wa(B) (mol%) of structural units derived from the (meth)acrylate in the entire styrene-(meth)acrylate copolymer particle; and the ratio Wa(S) (mol %) of the structural units derived from the (meth)acrylate on the surface of the styrene-(meth)acrylate copolymer particle, The toner for developing electrostatic images according to any one of ((1))) to (((9))), which satisfies 2≦Wa(S)−Wa(B)≦20. (((11))) The toner for developing electrostatic images according to (((10))), wherein a proportion Wa(S) (mol %) of structural units derived from the (meth)acrylate on the surface of the styrene-(meth)acrylate copolymer particles satisfies 40≦Wa(S)≦80. (((12))) the vinyl-based resin particles are styrene-(meth)acrylate copolymer particles, A ratio Ws(B) (mol%) of structural units derived from the styrene to the entire styrene-(meth)acrylate copolymer particle; and the proportion Ws(S) (mol%) derived from the styrene on the surface of the styrene-(meth)acrylate copolymer particle, The toner for developing electrostatic images according to any one of ((1))) to (((9))), which satisfies 2≦Ws(S)−Ws(B)≦20. (((13))) The toner for developing electrostatic images according to (((12))), wherein a proportion Ws(S) (mol %) derived from styrene on the surface of the styrene-(meth)acrylate copolymer particles satisfies 40≦Ws(S)≦80. (((14))) the solubility parameter SP(sa) of the surface of the vinyl resin particle; The relationship with the solubility parameter SP(ap) of the binder resin is as follows: The toner for developing electrostatic images according to (((10))) or (((11))), which satisfies |SP(ap)-SP(sa)|≦1.0. (((15))) the solubility parameter SP(sa) of the surface of the vinyl resin particle; The relationship with the solubility parameter SP(ap) of the binder resin is as follows: The toner for developing electrostatic images according to (((12))) or (((13))), which satisfies |SP(ap)-SP(sa)|≦1.0. (((16))) The binder resin contains an amorphous polyester resin. The amorphous polyester resin is a condensation polymer of a polycarboxylic acid including isophthalic acid and a polyhydric alcohol, The toner for developing electrostatic images according to (((10))), (((11))), or (((14))), wherein the ratio of isophthalic acid to the polycarboxylic acid is 10 mol % or more and 50 mol % or less. (((17))) The binder resin contains an amorphous polyester resin. The amorphous polyester resin is a condensation polymer of a polycarboxylic acid including isophthalic acid and a polyhydric alcohol, The toner for developing electrostatic images according to (((12))), (((13))), or (((15))), wherein the ratio of isophthalic acid to the polycarboxylic acid is 10 mol % or more and 50 mol % or less. (((18))) The toner for developing electrostatic images according to any one of ((1))) to (((17))), wherein the vinyl resin particles are resin particles having a crosslinked structure. (((19))) An electrostatic image developer comprising the toner for developing electrostatic images according to any one of (((1))) to (((18))). (((20))) The toner for developing an electrostatic image according to any one of (((1))) to (((18))) is contained, and an image forming The toner cartridge is attached to and detached from the forming device. (((twenty one))) (((19))) is accommodated in the electrostatic image developer, and the electrostatic image formed on the surface of an image carrier is developed into a toner image by the electrostatic image developer. (((twenty two))) An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; a developing means for containing the electrostatic image developer according to (((19))) and developing the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising: (((twenty three))) a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to (((19))); a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1,
[0368] The advantages of the above aspect are as follows. According to the invention related to (((1))), in a toner for developing electrostatic images, which contains toner particles containing a binder resin, a colorant, and vinyl resin particles, the area Sa (μm of a Voronoi polygon obtained by Voronoi division using the geometric center of the vinyl resin particle as a generating point in a cross-sectional observation of the toner particle is 2 ) is measured, the median value Sac (μm 2 ), the standard deviation of the area Sa of the Voronoi polygon is Ssd (μm 2 ), a toner for developing electrostatic images is provided which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under high temperature and high humidity environments, compared to a case in which the above formulas (1) and (2) are not satisfied.
[0369] According to the invention related to (((2))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high-temperature, high-humidity environment, as compared to a case in which formula (11) is not satisfied. According to the invention related to (((3))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine-line resolution that occurs when images are repeatedly formed in a high-temperature, high-humidity environment, as compared to a case in which formula (21) is not satisfied.
[0370] According to the invention related to (((4))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under a high temperature and high humidity environment, as compared with a case in which the ratio of the area of the vinyl resin particles to the area of the toner particles is 0.15 or less or exceeds 0.40 in cross-sectional observation of the toner particles. According to the invention related to (((5))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under a high temperature and high humidity environment, as compared with a case in which the volume average particle size of the vinyl resin particles is less than 100 nm or exceeds 300 nm. According to the invention related to (((6))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under a high temperature and high humidity environment, as compared with the case where the glass transition temperature of the vinyl resin particles is less than 0°C or more than 30°C.
[0371] According to the invention related to (((7))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, compared to a case in which the number ratio of vinyl resin particles observed to overlap in cross-sectional observation of a toner particle exceeds 50% by number of all vinyl resin particles observed. According to the invention related to (((8))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under high temperature and high humidity environments, as compared with a case in which, upon cross-sectional observation of the toner particle, the length of the portion of the contour line of the toner particle that overlaps with a vinyl resin particle exceeds 5% of the length of the contour line of the toner particle. According to the invention related to (((9))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under a high temperature and high humidity environment, as compared to when the average equivalent circular diameter of vinyl resin particles observed in cross-sectional observation of the toner particles exceeds 400 nm.
[0372] According to the invention related to (((10))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, as compared to a case where 2≦Wa(S)−Wa(B)≦20 is not satisfied. According to the invention related to (((11))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, as compared to a case where 40≦Wa(S)≦80 is not satisfied.
[0373] According to the invention related to (((12))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, as compared to a case where 2≦Ws(S)−Ws(B)≦20 is not satisfied. According to the invention related to (((13))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, as compared to a case where 40≦Ws(S)≦80 is not satisfied.
[0374] According to the invention related to (((14))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, as compared to a case where |SP(ap)-SP(sa)|≦1.0 is not satisfied. According to the invention related to (((15))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, as compared to a case where |SP(ap)-SP(sa)|≦1.0 is not satisfied.
[0375] According to the invention related to (((16))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, as compared to when the ratio of isophthalic acid to polyvalent carboxylic acid is less than 0.1 mol % or exceeds 0.5 mol %. According to the invention related to (((17))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, as compared to when the ratio of isophthalic acid to polyvalent carboxylic acid is less than 0.1 mol % or exceeds 0.5 mol %.
[0376] According to the invention related to (((18))), there is provided a toner for developing electrostatic images which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed under a high temperature and high humidity environment, as compared to when the vinyl resin particles have a non-crosslinked structure.
[0377] According to the invention of (((19))), (((20))), (((21))), (((22))) or (((23))), in a toner for developing electrostatic images, which contains toner particles containing a binder resin, a colorant and vinyl resin particles, the area Sa (μm) of a Voronoi polygon obtained by Voronoi tessellation using the geometric center of the vinyl resin particle as a generating point in cross-sectional observation of the toner particle is 2 ) is measured, the median value Sac (μm 2 ), the standard deviation of the area Sa of the Voronoi polygon is Ssd (μm 2 ), the present invention provides an electrostatic image developer, a toner cartridge, a process cartridge, an image forming apparatus, or an image forming method which suppresses the decrease in fine line resolution that occurs when images are repeatedly formed in a high temperature and high humidity environment, compared to a case in which a toner for developing electrostatic images which does not satisfy the above formulas (1) and (2) is provided. [Explanation of symbols]
[0378] 1Y, 1M, 1C, 1K Photoconductor (an example of an image carrier) 2Y, 2M, 2C, 2K Charging roll (an example of a charging means) 3 Exposure device (an example of an electrostatic image forming means) 3Y, 3M, 3C, 3K laser beam 4Y, 4M, 4C, 4K developing device (an example of developing means) 5Y, 5M, 5C, 5K Primary transfer roll (an example of a primary transfer means) 6Y, 6M, 6C, 6K Photoconductor cleaning device (an example of a cleaning means) 8Y, 8M, 8C, 8K toner cartridges 10Y, 10M, 10C, 10K Image forming units 20 Intermediate transfer belt (an example of an intermediate transfer body) 22 Driving Roll 24 Support roll 26 Secondary transfer roll (an example of a secondary transfer means) 30 Intermediate transfer body cleaning device 107 Photoconductor (an example of an image carrier) 108 Charging roll (an example of charging means) 109 Exposure device (an example of electrostatic image forming means) 111 Developing device (an example of developing means) 112 Transfer device (an example of a transfer means) 113 Photoconductor cleaning device (an example of a cleaning means) 115 Fixing device (an example of fixing means) 116 Mounting Rail 118 Exposure Aperture 117 Cabinet 200 Process Cartridge 300 Recording paper (an example of a recording medium) P Recording paper (an example of a recording medium)
Claims
1. The toner particles include a binder resin and vinyl resin particles, In observing the cross section of the toner particle, the area Sa (μm of the Voronoi polygon when Voronoi division is performed with the geometric center of the vinyl resin particle as the base point is determined. 2 ), the median of the area Sa of the Voronoi polygon is Sac (μm 2 , the standard deviation of the area Sa of the Voronoi polygon is Ssd (μm 2 ) a toner for developing an electrostatic image that satisfies the following formulas (1) and (2): Formula (1): 0.03≦Sac≦0.20 Formula (2): Ssd≦0.10
2. The toner for developing electrostatic images according to claim 1 , which satisfies the following formula (11): Formula (11): 0.08≦Sac≦0.16
3. The toner for developing electrostatic images according to claim 2 , which satisfies the following formula (21): Formula (21) Ssd≦0.07
4. 2. The toner for developing electrostatic images according to claim 1, wherein, upon cross-sectional observation of the toner particle, the ratio of the area of the vinyl resin particles to the area of the toner particle is greater than 0.15 and not greater than 0.
40.
5. 2. The toner for developing electrostatic images according to claim 1, wherein the volume average particle size of the vinyl resin particles is from 100 nm to 300 nm.
6. 2. The toner for developing electrostatic images according to claim 1, wherein the glass transition temperature of the vinyl resin particles is from 0° C. to 30° C.
7. 2. The toner for developing electrostatic images according to claim 1, wherein, in a cross-sectional observation of the toner particle, a number ratio of the vinyl resin particles observed to be overlapped with each other is 50% or less of the number of all the vinyl resin particles observed.
8. 2. The toner for developing electrostatic images according to claim 1, wherein, upon cross-sectional observation of the toner particle, a length of a portion of the contour of the toner particle that overlaps with the vinyl resin particle is 5% or less of the length of the contour of the toner particle.
9. 2. The toner for developing electrostatic images according to claim 1, wherein, upon cross-sectional observation of the toner particles, the average equivalent circular diameter of the vinyl resin particles observed is 400 nm or less.
10. the vinyl-based resin particles are styrene-(meth)acrylate copolymer particles, a ratio Wa(B) (mol %) of structural units derived from the (meth)acrylate in the entire styrene-(meth)acrylate copolymer particle; and the ratio Wa(S) (mol %) of the structural units derived from the (meth)acrylate on the surface of the styrene-(meth)acrylate copolymer particle, 2. The toner for developing electrostatic images according to claim 1, wherein the relationship 2≦Wa(S)−Wa(B)≦20 is satisfied.
11. The toner for developing electrostatic images according to claim 10, wherein a ratio Wa(S) (mol %) of the structural units derived from the (meth)acrylate on the surface of the styrene-(meth)acrylate copolymer particle satisfies 40≦Wa(S)≦80.
12. the vinyl-based resin particles are styrene-(meth)acrylate copolymer particles, a ratio Ws(B) (mol%) of structural units derived from the styrene to the entire styrene-(meth)acrylate copolymer particle; and the proportion Ws(S) (mol%) derived from the styrene on the surface of the styrene-(meth)acrylate copolymer particle, 2. The toner for developing electrostatic images according to claim 1, which satisfies 2≦Ws(S)−Ws(B)≦20.
13. The toner for developing electrostatic images according to claim 12, wherein a ratio Ws(S) (mol %) derived from styrene on the surface of the styrene-(meth)acrylate copolymer particles satisfies 40≦Ws(S)≦80.
14. The solubility parameter SP (sa) of the surface of the vinyl resin particle, The relationship with the solubility parameter SP(ap) of the binder resin is as follows: The toner for developing electrostatic images according to claim 10, wherein |SP(ap)-SP(sa)|≦1.0 is satisfied.
15. the solubility parameter SP(sa) of the surface of the vinyl resin particle; The relationship with the solubility parameter SP(ap) of the binder resin is as follows: The toner for developing electrostatic images according to claim 12, wherein |SP(ap)-SP(sa)|≦1.0 is satisfied.
16. The binder resin contains an amorphous polyester resin. The amorphous polyester resin is a condensation polymer of a polycarboxylic acid including isophthalic acid and a polyhydric alcohol, 11. The toner for developing electrostatic images according to claim 10, wherein the ratio of isophthalic acid to the polycarboxylic acid is from 10 mol % to 50 mol %.
17. The binder resin contains an amorphous polyester resin. The amorphous polyester resin is a condensation polymer of a polycarboxylic acid including isophthalic acid and a polyhydric alcohol, 13. The toner for developing electrostatic images according to claim 12, wherein the ratio of isophthalic acid to the polycarboxylic acid is from 10 mol % to 50 mol %.
18. 2. The toner for developing electrostatic images according to claim 1, wherein the vinyl resin particles have a crosslinked structure.
19. 19. An electrostatic image developer comprising the toner for developing electrostatic images according to any one of claims 1 to 18.
20. A toner for developing an electrostatic image according to any one of claims 1 to 18 is contained, and an image forming The toner cartridge is attached to and detached from the forming device.
21. 20. A process cartridge detachably mountable to an image forming apparatus, comprising: a developing means for accommodating the electrostatic image developer according to claim 19 and developing an electrostatic image formed on a surface of an image carrier by the electrostatic image developer into a toner image.
22. An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; a developing unit that contains the electrostatic image developer according to claim 19 and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising:
23. a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to claim 19; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1,
Citation Information
Patent Citations
Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
JP2016062040A
Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
JP2016062042A
Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
JP2020046499A
Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
JP2020160204A