Photoresponsive composition

The photoresponsive composition with perovskite quantum dots protected by multiple layers addresses color mixture issues, ensuring stable and consistent color purity by preventing halogen exchange.

JP2024141032APending Publication Date: 2024-10-10CANON KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023052461
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing photoresponsive compositions using perovskite quantum dots with different compositions experience color mixture due to halogen exchange, leading to changes in composition over time and reduced color purity.

Method used

A photoresponsive composition is developed with perovskite quantum dots of mutually different compositions, each protected by a common medium and multiple protective layers, including organic groups and bonding portions, to prevent halogen exchange and stabilize the composition.

Benefits of technology

The composition effectively reduces color mixture and stabilizes the photoresponsive properties, maintaining consistent color purity over time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141032000001_ABST
    Figure 2024141032000001_ABST
Patent Text Reader

Abstract

To provide a photoresponsive composition which includes perovskite type quantum dots with mutually different compositions supported by a common medium, and in which mixing of colors is reduced.SOLUTION: This photoresponsive composition comprises a medium, a first particle, and a second particle. The first particle is supported by the medium and comprises: a first nanoparticle having a photoresponsive perovskite-type crystal structure; a first protective layer, which protects the first nanoparticle and has a first organic group and a first bonding region that is oriented to the first nanoparticle; and a third protective layer, which protects the first particle and is disposed between the medium and the first protective layer. The second particle is supported by the medium and comprises: a second nanoparticle having a photoresponsive perovskite-type crystal structure different from that of the first nanoparticle; and a second protective layer, which protects the second nanoparticle and has a second organic group and a bonding region that is oriented to the second nanoparticle.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to photoresponsive compositions that respond upon irradiation with light. [Background technology]

[0002] Quantum dots with a perovskite crystal structure are known to be applicable to organic electroluminescence materials and quantum dot light-emitting materials because they have a narrow full width at half maximum in the spectral sensitivity characteristics and exhibit high color purity. In addition, they have the advantage that it is easy to provide materials that respond to light in a wide wavelength range because the absorption and emission wavelengths can be controlled by the halogen composition.

[0003] Patent Document 1 discloses a liquid crystal display device including quantum dots having a perovskite crystal structure that absorbs light from a light-emitting element, converts it into at least one of RGB light, and emits the light, and a light conversion layer including such quantum dots.

[0004] Patent Document 2 discloses a liquid crystal display device including a backlight including a light emitting element and a wavelength conversion layer including perovskite quantum dots of different compositions that convert light from the light emitting element into red light and green light, respectively. The liquid crystal display device disclosed in Patent Document 2 enhances the color purity of red and green contained in the emission of the backlight by including a wavelength conversion layer including perovskite quantum dots in the backlight. In addition, the liquid crystal display device disclosed in Patent Document 2 includes a display device including a liquid crystal element and an optical filter that controls the transmittance of light from the wavelength conversion layer or the light emitting element, thereby adjusting the intensity of the dispersed display color according to the emission color of the pixel.

[0005] On the other hand, when perovskite quantum dots of different compositions are mixed in the same medium, the halogens are exchanged between the perovskite quantum dots of different compositions, causing a change in their compositions and a problem of change in their photoresponse (color mixing).

[0006] In Patent Document 1, perovskite quantum dots with different compositions are provided with a protective layer having an organic group to reduce color mixing. Patent Document 2 does not directly mention color mixing, but uses perovskite quantum dots as green emitters and non-perovskite quantum dots that have low reactivity with perovskite quantum dots as red emitters to avoid color mixing. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2018-197782 A [Patent Document 2] Special Publication No. 2021-6900 Summary of the Invention [Problem to be solved by the invention]

[0008] However, in the wavelength conversion layer described in Patent Document 1, the composition may change over time, causing color mixing. Although the wavelength conversion layer described in Patent Document 1 has a protective layer provided for each quantum dot, there is a concern that the protective effect may not be sufficient. In addition, in the wavelength conversion layer described in Patent Document 2, non-perovskite quantum dots are used for the red of the quantum dots corresponding to green and red, which causes a problem that wavelength selection characteristics such as light absorption and color purity are limited.

[0009] The present invention has been made in consideration of the above problems, and aims to provide a photoresponsive composition that contains perovskite quantum dots supported by a common medium and different compositions, and that has reduced color mixing. [Means for solving the problem]

[0010] A light-responsive composition according to an embodiment of the present invention comprises a first particle supported by the medium, the first particle including: a first nanoparticle having a light-responsive perovskite-type crystal structure; a first protective layer having a first organic group and a first binding portion coordinated to the first nanoparticle and protecting the first nanoparticle; and a third protective layer located between the medium and the first protective layer and protecting the first particle; and a second particle supported by the medium, the second particle including: a second nanoparticle having a perovskite-type crystal structure and a different composition from the first nanoparticle; and a second protective layer having a second organic group and a binding portion coordinated to the second nanoparticle and protecting the second nanoparticle. Effect of the Invention

[0011] According to the present invention, it is possible to provide a photoresponsive composition that contains perovskite quantum dots supported by a common medium and different in composition, and that exhibits reduced color mixing. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a diagram showing a schematic structure of a light-responsive composition according to a first embodiment. [Diagram 2] FIG. 2 is a partial enlarged view showing a schematic configuration of first particles (a) and (b) and second particles (c) and (d) according to the first embodiment. [Diagram 3] FIG. 4 is a diagram showing a schematic structure of a light-responsive composition according to a second embodiment. [Figure 4] FIG. 13 is a diagram showing a schematic structure of a light-responsive composition according to a third embodiment. [Diagram 5] FIG. 13 is a diagram showing a schematic structure of a wavelength conversion layer containing a light-responsive composition according to a fourth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Preferred embodiments of the present invention will be described in detail below with reference to the drawings. The dimensions, materials, shapes, relative positions, and so forth of the components described in these embodiments are not intended to limit the scope of the present invention.

[0014] <First embodiment> The light-responsive composition according to the first embodiment will be described with reference to FIG. 1 and FIG.

[0015] The light-responsive composition 100 according to the first embodiment includes a medium 70. As shown in FIG. 1, the light-responsive composition 100 includes a first nanoparticle 10 having a light-responsive perovskite-type crystal structure, a first protective layer 20 that protects the first nanoparticle 10, and a first particle 30 supported by the medium 70. As shown in FIG. 2, the first protective layer 20 includes a first organic group 122 and a first bonding portion 110 that is coordinated to the first nanoparticle 10, thereby protecting the first nanoparticle 10.

[0016] Additionally, the first particle 30 is further configured to include a third protective layer 80 located between the medium 70 and the first protective layer 20 to protect the first particle.

[0017] 1, the photoresponsive composition 100 includes second nanoparticles 40 having a perovskite-type crystal structure with a different composition from that of the first nanoparticles 10, a second protective layer 50 for protecting the second nanoparticles 40, and a second particle 60 supported by a medium 70. The second protective layer 50 is configured to have a second organic group 123 and a bonding portion 111 coordinated to the second nanoparticles, as shown in FIG.

[0018] (Nanoparticles) In this embodiment, the first nanoparticles 10 and the second nanoparticles 40 are semiconductor nanocrystals having a perovskite crystal structure with A site (monovalent cation), B site (divalent cation), and X site (monovalent anion including halide anion) as constituents. The perovskite crystal structure is alternatively referred to as a perovskite structure, an ABX3 crystal structure, or an ABX3 structure. The double perovskite crystal structure represented as A2B1B2X6 is also included in the perovskite crystal structure. In this specification, at least one of the first nanoparticles 10 and the second nanoparticles 40 may be alternatively referred to as a luminescent nanoparticle, a luminescent nanocrystal, a photoresponsive nanocrystal, or a quantum dot.

[0019] The average particle size of the nanoparticles is preferably 1 nm or more and 30 nm or less, more preferably 2 nm or more and 25 nm or less. If the average particle size is less than 1 nm, the stability may be insufficient. If the average particle size is more than 30 nm, the dispersibility may be insufficient.

[0020] [A site of perovskite structure] A monovalent cation is used at the A site. The monovalent cation used at the A site is the ammonium cation (NH4 + ), and alkylammonium cations with carbon atoms of 6 or less, formamidinium cations (HC(NH2)2 + ), guanidinium cation (C(NH2)3 + ), imidazolium cation, pyridinium cation, pyrrolidinium cation, and other nitrogen-containing organic compound cations; and lithium cation (Li + ), sodium cation (Na + ), potassium cation (K + ), rubidium cation (Rb + ), and the cesium cation (Cs + ) and other alkali metal cations.

[0021] These monovalent cations employed in the A site have a small ionic diameter and are small enough to fit into the crystal lattice, enabling the perovskite compound to form stable three-dimensional crystals.

[0022] A preferred example of an alkylammonium cation having 6 or less carbon atoms is a methylammonium cation (CH3NH3 + ), ethylammonium cation (C2H5NH3 + ), propylammonium cation (C3H7NH3 + ) etc.

[0023] From the viewpoint of obtaining high luminous efficiency, it is preferable to use at least one of methylammonium cation, formamidinium cation, and cesium cation as the A site, and from the viewpoint of suppressing color change, it is more preferable to use cesium cation as the A site. Two or more kinds of these monovalent cations employed as the A site may be used in combination.

[0024] When the A site is a cesium cation, cesium salts can be used as raw materials for synthesizing the luminescent nanocrystal first nanoparticle 10 and second nanoparticle 40 described below. As such cesium salts, cesium chloride, cesium bromide, cesium iodide, cesium hydroxide, cesium carbonate, cesium hydrogen carbonate, cesium bicarbonate, cesium formate, cesium acetate, cesium propionate, cesium pivalate, and cesium oxalate can be appropriately used. Among these cesium salt candidates, an appropriate one can be used depending on the synthesis method.

[0025] When the A site is another alkali metal cation, a salt in which the cesium element of the above-mentioned cesium compound is replaced with another alkali metal cation element can be used as the raw material.

[0026] When the A site is a nitrogen-containing organic compound cation such as a methylammonium cation, for example, a neutral compound other than a salt such as methylamine can be used as a raw material. Two or more of these raw materials may be used in combination.

[0027] [Perovskite-type crystal structure B site] The B site of the perovskite crystal structure employs a divalent cation including a divalent transition metal cation or a divalent typical metal cation.

[0028] The divalent transition metal cation is the scandium cation (Sc 2+ ), titanium cation (Ti 2 +), vanadium cation (V 2+ ), chromium cation (Cr 2+ ), manganese cation (Mn 2+ ), iron cation (Fe 2+ ), cobalt cation (Co 2+ ), nickel cation (Ni 2+ ), copper cation (Cu 2+ ), palladium cation (Pd 2+ ), europium cation (Eu 2+ ), ytterbium cation (Yb 2+ ) will be adopted.

[0029] The divalent typical metal cation is the magnesium cation (Mg 2+ ), calcium cation (Ca 2+ ), strontium cation (Sr 2+ ), barium cation (Ba 2+ ), zinc cation (Zn 2+ ), cadmium cation (Cd 2+ ), germanium cation (Ge 2+ ), tin cation (Sn 2+ ), lead cation (Pb 2+ ) may be adopted.

[0030] Among these divalent cations, divalent typical metal cations are preferred from the viewpoint of growing stable three-dimensional crystals, tin cations or lead cations are more preferred, and lead cations are particularly preferred from the viewpoint of obtaining high luminescence intensity. Two or more of these divalent cations may be used in combination, and the perovskite crystal structure may be a so-called double perovskite structure.

[0031] When the B site is a lead cation, the raw material for synthesizing the first nanoparticle 10 and the second nanoparticle 40 described later includes a lead compound, and an appropriate one can be used depending on the synthesis method. As the lead compound, lead chloride, lead bromide, lead iodide, lead oxide, lead hydroxide, lead sulfide, lead carbonate, lead formate, lead acetate, lead 2-ethylhexanoate, lead oleate, lead stearate, lead naphthenate, lead citrate, lead maleate, and lead acetylacetonate are adopted. When the B site is a divalent metal cation, a salt in which the lead element of the above-mentioned lead compound is replaced with another divalent metal cation element can be used as the raw material. Two or more of these raw materials may be used in combination.

[0032] [X site of perovskite crystal structure] X in the perovskite crystal structure is a monovalent anion including a halide anion. The halide anion is a fluoride anion (F - ), chloride anion (Cl - ), bromide anion (Br - ), iodide anion (I - Among them, chloride anion, bromide anion, or iodide anion are preferred because they form stable three-dimensional crystals and emit strong light in the visible light range. The color of the emitted light is blue when chloride anion is used, green when bromide anion is used, and red when iodide anion is used.

[0033] Two or more kinds of halide anions may be used in combination. In particular, when chloride anions, bromide anions, and iodide anions are used in combination, the emission wavelengths of the first nanoparticles 10 and the second nanoparticles 40 can be set to desired wavelengths depending on the content ratio of the anion species. That is, in particular, when chloride anions, bromide anions, and iodide anions are used in combination, it is preferable because it is possible to obtain an emission spectrum that covers almost the entire range of visible light from blue to red while maintaining a narrow full width at half maximum depending on the content ratio of the anion species.

[0034] The X site may contain a monovalent anion other than a halide anion. Examples of such monovalent anions other than a halide anion include pseudohalide anions such as cyanide anion (CN-), thiocyanate anion (SCN-), and isothiocyanate anion (CNS-). As raw materials for synthesizing the first nanoparticles 10 and the second nanoparticles 40, appropriate ones can be selected according to the synthesis method from salts with counter cations at the A site and B site, such as cesium chloride and lead bromide, and salts with other cations.

[0035] The first nanoparticles 10 and the second nanoparticles 40 in this embodiment can be manufactured by the following process. For example, the hot injection method, in which raw material liquids are mixed at high temperature and then rapidly cooled after the generation of fine particles to obtain a stable product, and the ligand-assisted reprecipitation method, in which fine particles are obtained by reprecipitation utilizing the difference in miscibility of the product with the solvent, are adopted.

[0036] Also, a room temperature synthesis method is used in which a mixture of A-site raw materials and B-site raw materials, which are non-halogenated and do not contain X-site components, is mixed with a separately prepared X-site raw material liquid under mild conditions at around room temperature to obtain fine particles.Furthermore, this method is used in a mechanochemical method in which solid raw materials are reacted by mechanical mixing such as milling or ultrasonic treatment to obtain product fine particles, and an in situ synthesis method in which a raw material liquid is applied to a substrate and then directly crystallized to obtain a reaction product.

[0037] It is preferable that the first particles 30 described below contain either bromine or iodine in a large amount, and the second particles 60 contain either the other of bromine and iodine in a large amount.

[0038] (First particle) 1, the first particles 30 in this embodiment include first nanoparticles 10 having a perovskite crystal structure, and a first protective layer 20 having a first organic group 122 and a first bonding portion 110 coordinated to the first nanoparticles 10 and protecting the first nanoparticles 10. The first particles 30 may be separated from each other, or a plurality of first particles 30 may be connected via the first protective layer 20 to form a secondary particle.

[0039] (Second particle) The second particles 60 include second nanoparticles 40 having a perovskite crystal structure, and a second protective layer 50 having a second organic group 123 and a second bonding portion 111 coordinated to the second nanoparticles and protecting the second nanoparticles 40. The second particles 60 may be separated from each other, or a plurality of the second particles 60 may be connected via the second protective layer 50 to form a secondary particle.

[0040] It is preferable that the first particles 30 exhibit a light emitting characteristic of emitting more of either green or red light, and the second particles 60 exhibit a light emitting characteristic of emitting more of the other of green or red light.

[0041] (First protective layer, second protective layer) The first nanoparticle 10 is protected by a first protective layer 20 having organic groups 120, 122 and a bonding portion 110, and the second nanoparticle 40 is protected by a second protective layer 50 having organic groups 121, 123 and a bonding portion 111. It is presumed that the protective function is exhibited for the following two reasons. The first presumption is that the hydrophilic bonding portion is coordinated to the nanocrystal, completely or partially bonding with the halogen, which is also hydrophilic, making it difficult for the halogen to be detached from the nanocrystal.

[0042] The second assumption is that the organic group creates a hydrophobic field, which makes it difficult for the hydrophilic halogen to be released from the nanocrystals. The protective layer may be composed of a low molecular weight compound or a high molecular weight compound. It may also contain both a low molecular weight compound and a high molecular weight compound. From the viewpoint of more effectively preventing color mixing, it is preferable that the protective layer is mainly composed of a high molecular weight compound.

[0043] As the polymer compound, a copolymer (described later) obtained by polymerizing at least two kinds of monomers each containing a bond and an organic group as described below can be used.

[0044] (First joint, second joint) Examples of the first binding portion 110 and the second binding portion 111 include cationic groups, anionic groups, zwitterionic groups, and salts thereof. Examples of the anionic group include a carboxy group, a sulfo group, and a phosphoryl group. Examples of the cationic group include an amino group and a quaternary ammonium cation. Examples of the zwitterionic group include a carboxybetaine group, a phosphorylcholine group, and a sulfobetaine group.

[0045] The first connecting portion 110 and the second connecting portion 111 may be the same connecting portion or different connecting portions.

[0046] (First organic group, second organic group) A linear, branched or cyclic alkyl group, a linear, branched or cyclic heteroalkyl group, an aryl group, a heteroaryl group, an aralkyl group or a heteroaralkyl group is adopted as the first organic groups 120, 122 and the second organic groups 121, 123. Any of the first organic groups 120, 122 and the second organic groups 121, 123 may have a substituent in a part of the organic group.

[0047] The first organic groups 120 and 122 and the second organic groups 121 and 123 may be the same organic group or different organic groups.

[0048] (Content of the first and second protective layers) The content of the first protective layer 20 relative to the first nanoparticles 10 is preferably 1 part by mass to 1000 parts by mass, preferably 5 parts by mass to 500 parts by mass, and more preferably 10 parts by mass to 300 parts by mass, assuming that the content of the first nanoparticles 10 is 100 parts by mass. If it is less than 1 part by mass, the effect as a protective layer may not be fully exhibited, and color mixing may not be prevented. If it is more than 1000 parts by mass, the solubility and dispersibility of the first protective layer 20 in the medium 70 may decrease, and color mixing may not be prevented. The content of the first protective layer 20 relative to the first nanoparticles 10 may be appropriately adjusted according to the type and use of the first nanoparticles 10 and the first protective layer 20.

[0049] The content of the second protective layer 50 relative to the second nanoparticles 40 is preferably 1 part by mass to 1000 parts by mass, preferably 5 parts by mass to 500 parts by mass, and more preferably 10 parts by mass to 300 parts by mass, with the content of the second nanoparticles 40 being 100 parts by mass. If it is less than 1 part by mass, the effect of the second protective layer 50 may not be fully exhibited, and color mixing may not be prevented. If it is more than 1000 parts by mass, the solubility and dispersibility of the second protective layer 50 in the medium 70 may decrease, and color mixing may not be prevented. The content of the second protective layer 50 relative to the second nanoparticles 40 may be appropriately adjusted according to the type and application of the second nanoparticles 40 and the second protective layer 50.

[0050] Examples of the method of coordinating the first protective layer 20 on the surface of the first nanoparticle 10 include a method of applying the first protective layer 20 after the synthesis of the first nanoparticle 10, and a method of allowing the first nanoparticle 10 and the first protective layer 20 to coexist during the synthesis of the first nanoparticle 10. Similarly, examples of the method of coordinating the second protective layer 50 on the surface of the second nanoparticle 40 include a method of applying the second protective layer 50 after the synthesis of the second nanoparticle 40, and a method of allowing the second nanoparticle 40 and the second protective layer 50 to coexist during the synthesis of the second nanoparticle 40.

[0051] (Method of producing polymer compound) A detailed description is given below of a method for producing a polymer compound that can be used for the first protective layer 20 and the second protective layer 50. The method for producing the polymer compound is not particularly limited as long as it can produce the above-mentioned structure, but it can be produced, for example, by the following method (i) or (ii).

[0052] That is, the method (i) for producing a polymer compound includes a method of producing a monomer having a structural unit containing a bonding portion or an organic group, and then polymerizing the monomer to produce the polymer compound. Furthermore, the method (ii) for producing a polymer compound includes a method of synthesizing a polymer main chain, and then bonding the bonding portion or the organic group to the polymer main chain.

[0053] From the viewpoints of easy availability of monomers and control of the amount of functional groups, the method shown in (i) is preferable. Hereinafter, a method for synthesizing a polymer compound containing a zwitterionic group as a binding moiety using the method shown in (i) will be described in detail.

[0054] As a monomer for introducing a bond into a polymer compound, a vinyl ether derivative, an acrylate derivative, a methacrylate derivative, an α-olefin derivative, an aromatic vinyl derivative, etc. From the viewpoint of ease of production of the monomer, it is preferable to use an acrylate derivative or a methacrylate derivative as such a monomer.

[0055] The corresponding acrylate or methacrylate derivatives can be prepared by the methods described in the following documents. K. Ishihara and 2 others, "Polymer Journal" (Japan), The Society of Polymer Science, 1990, Vol. 22, p.355-360

[0056] The polymerization method of the above monomers includes radical polymerization and ionic polymerization, and living polymerization can also be used for the purpose of controlling the molecular weight distribution or structure. From an industrial perspective, it is preferable to use radical polymerization.

[0057] Radical polymerization can be carried out by using a radical polymerization initiator, irradiating with light such as radiation or laser light, using a photopolymerization initiator in combination with light irradiation, heating, etc. The radical polymerization initiator may be any that can generate radicals and initiate a polymerization reaction, and is selected from compounds that generate radicals by the action of heat, light, radiation, oxidation-reduction reactions, etc.

[0058] For example, azo compounds, organic peroxides, inorganic peroxides, organometallic compounds, photopolymerization initiators, etc. may be mentioned.

[0059] More specifically, examples of the initiator include azo compounds such as 2,2'-azobisisobutyronitrile (AIBN) and 2,2'-azobis(2,4-dimethylvaleronitrile), organic peroxides such as benzoyl peroxide (BPO), tert-butyl peroxypivalate, and tert-butylperoxyisopropyl carbonate, inorganic peroxides such as potassium persulfate and ammonium persulfate, and redox initiators such as hydrogen peroxide-iron(II) salt, BPO-dimethylaniline, and cerium(IV) salt-alcohol. Photopolymerization initiators include acetophenone, benzoin ether, and ketal. Two or more of these radical polymerization initiators may be used in combination.

[0060] The polymerization temperature of the vinyl monomer is not particularly limited and the preferred temperature range varies depending on the type of polymerization initiator used, but polymerization is generally carried out at a temperature of -30°C to 150°C, and a more preferred temperature range is 40°C to 120°C.

[0061] The amount of the polymerization initiator used in this case is preferably 0.1 to 20 parts by mass per 100 parts by mass of the monomer, and the amount used is preferably adjusted so as to obtain a polymer compound having a target molecular weight distribution.

[0062] The polymerization method is not particularly limited and may be any method such as solution polymerization, suspension polymerization, emulsion polymerization, dispersion polymerization, precipitation polymerization, and bulk polymerization.

[0063] The resulting polymer compound may be purified as necessary by any method, including, but not limited to, reprecipitation, dialysis, column chromatography, etc.

[0064] The structure of the produced polymer compound can be identified by various instrumental analyses, such as nuclear magnetic resonance (NMR), gel permeation chromatography (GPC), and inductively coupled plasma atomic emission spectrometry (ICP-AES).

[0065] (medium) As shown in FIG. 1 and FIG. 3, the medium 70, 77 is selected from either a liquid (medium 70) or a solid (medium 77). As the liquid, a solvent or a polymerizable compound can be used. That is, the medium 70 can contain a polymerizable compound 150 or a solvent. As the solid, a polymer matrix can be used. The medium 77 may contain a polymer matrix in which both the first particles 30 and the second particles 60 are dispersed. The polymer matrix can be a polymer obtained by crosslinking and polymerizing a polymerizable compound. The polymer matrix is ​​in the form of a sheet with a sheet thickness that takes into consideration the objective of ensuring the optical coupling surface of light reception and light emission, the deactivation depth (penetration depth) of the primary light, and the extraction efficiency of the secondary light. Examples of the solvent include alkanes such as pentane and hexane, cycloalkanes such as cyclopentane and cyclohexane, esters such as ethyl acetate, butyl acetate, and benzyl acetate, ethers such as diethyl ether and tetrahydrofuran, ketones such as cyclohexanone and acetone, and alcohols such as methanol, ethanol, isopropanol, butanol, and hexanol. In addition, monoacetate compounds such as diethylene glycol monoethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, and dipropylene glycol methyl ether acetate, diacetate compounds such as 1,4-butanediol diacetate and propylene glycol diacetate, and triacetate compounds such as glyceryl triacetate can also be used. Since the solvent is easily removed before the curing of the polymerizable compound, a solvent with a boiling point of 300° C. or less is used. The solvent may be referred to as a solvent in other words.

[0066] (polymerizable compound) Polymerization of the polymerizable compound 150 is accelerated by receiving energy such as light or heat, and the polymerizable compound 150 becomes a component that imparts viscosity to the photoresponsive composition and hardens it. The polymerizable compound may be a radically polymerizable compound or a cationic polymerizable compound. These may be used alone or in combination of two or more. In addition, either a photopolymerizable compound or a thermally polymerizable compound may be used. In the present specification, the form in which the polymerizable compound 150 is polymerized and the viscosity is increased may be referred to as a polymer 160.

[0067] Examples of the radically polymerizable compound that can be used include monofunctional (meth)acrylate compounds, bifunctional (meth)acrylate compounds, trifunctional or higher (meth)acrylate compounds, hydroxyl group-containing (meth)acrylate compounds, carboxy group-containing (meth)acrylate compounds, and vinyl compounds.

[0068] Examples of monofunctional (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, benzyl (meth)acrylate, and 3,3,5-trimethylcyclohexyl acrylate. , tetrahydrofurfuryl (meth)acrylate, phenoxyethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, isobornyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, (3-ethyloxetan-3-yl)methyl (meth)acrylate, and cyclic trimethylolpropane formal (meth)acrylate can be used.

[0069] Examples of bifunctional (meth)acrylate compounds include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol 200 di(meth)acrylate, polyethylene glycol 300 di(meth)acrylate, polyethylene glycol 400 di(meth)acrylate, and polyethylene glycol 600. Di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, polypropylene glycol 400 di(meth)acrylate, polypropylene glycol 700 di(meth)acrylate, neopentyl glycol di(meth)acrylate, neopentyl glycol PO-modified di(meth)acrylate, EO-modified bisphenol A di(meth)acrylate, PO-modified bisphenol A di(meth)acrylate, and hydroxypivalic acid neopentyl glycol di(meth)acrylate can be used.

[0070] Examples of trifunctional or higher (meth)acrylate compounds that can be used include trimethylolpropane tri(meth)acrylate, trimethylolpropane EO-modified tri(meth)acrylate, trimethylolpropane PO-modified tri(meth)acrylate, glycerin propoxy tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, and EO-modified pentaerythritol tetraacrylate.

[0071] Examples of the vinyl-based compound that can be used include vinyl acetate, vinyl benzoate, vinyl pivalate, vinyl butyrate, vinyl methacrylate, and N-vinylpyrrolidone.

[0072] The cationic polymerizable compound may be either a photopolymerizable or a thermally polymerizable compound. These may be used alone or in combination of two or more. Representative cationic polymerizable compounds include, for example, epoxy compounds, oxacene compounds, and vinyl ether compounds.

[0073] The amount of the polymerizable compound including the above radical polymerizable compound and cationic polymerizable compound used is preferably 1 to 99 parts by mass, more preferably 3 to 90 parts by mass, and even more preferably 5 to 80 parts by mass, relative to the total parts by mass of the photoresponsive composition.

[0074] The medium 70, 77 preferably has an organic group. As the organic group, at least one of a linear, branched or cyclic alkyl group, a linear, branched or cyclic heteroalkyl group, an aryl group, a heteroaryl group, an aralkyl group, or a heteroaralkyl group can be used. The substituent possessed by the medium 70, 77 may have a partially substituted substituent.

[0075] (Polymerization initiator) In a polymerization reaction, a polymerization initiator and a polymerizable compound are generally used in combination. The polymerization initiator is a compound that generates an active species that initiates a polymerization reaction by irradiation with active energy rays or heat, and a known polymerization initiator can be used. The main active species that initiate a polymerization reaction include a radical polymerization initiator that generates a radical and a cationic polymerization initiator that generates an acid, and these may be used in combination. Examples of photoradical polymerization initiators that generate radicals by active energy rays include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl methyl ketal, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butane, oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]butane, and oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]butane. acetophenones such as 2-hydroxy-1-[4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl]-2-methylpropan-1-one; benzoins such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; phosphines such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; and other phenyl glyoxylic methyl esters.

[0076] Among the photoradical polymerization initiators, acetophenones such as aminoketones, phosphines, and oxime ester compounds are preferred. These can be used alone or in combination depending on the properties required for the cured product. When using a radical polymerization initiator, the amount used is preferably 0.01 to 100 parts by mass, more preferably 0.1 to 50 parts by mass, based on 100 parts by mass of the total solid content in the composition.

[0077] (Third protective layer) The third protective layer 80 is located between the medium 70, 77 and the first protective layer 20, and protects the first particles 30. The third protective layer 80 is located between the medium 70, 77 and the first protective layer 20, and in other words protects the first protective layer 20. The third protective layer 80 takes an embodiment containing a polymer compound having a third organic group in a side chain. In addition, the third protective layer 80 preferably has a lower absorbance (optical density) than the first nanoparticles in a first wavelength band including at least one of ultraviolet and blue and a second wavelength band related to the emission wavelength of the first nanoparticles. The third protective layer 80 containing the first particles 30 is preferably in the form of particles having a diameter of 10 nm to 10 μm. The third protective layer 80 preferably has a crosslinked structure. The third protective layer 80 is provided such that the first protective layer 20 is in contact with the third protective layer 80, and the second protective layer 50 is not in contact with the third protective layer 80. The third protective layer 80 is configured to encapsulate the first nanoparticles 10 but not the second nanoparticles 40. By providing the third protective layer 80 in this manner, the exchange of halogens originating from the first nanoparticles 10 and the second nanoparticles 40 via the media 70 and 77 is further restricted.

[0078] (Third Organic Group) As the third organic group, at least one of a linear, branched or cyclic alkyl group, a linear, branched or cyclic heteroalkyl group, an aryl group, a heteroaryl group, an aralkyl group, or a heteroaralkyl group can be used. The third organic group may have a substituent that is partially substituted.

[0079] (Method of forming third protective layer) The method for forming the third protective layer 80 is not particularly limited, and examples thereof include a top-down method of microparticulating the bulk of the third protective layer 80 including the first particles 30, and a bottom-up method of microparticulating the bulk of the third protective layer 80 including the first particles 30. An appropriate method may be selected depending on the application.

[0080] In the case of top-down microparticulation, a bulk of the third protective layer 80 containing the first particles 30 is first formed. Methods for forming the bulk include a method of polymerizing a mixture containing a polymerizable compound and the first particles 30, and a method of mixing the first particles 30 with a polymer compound. Methods for microparticulating the bulk include dry grinding, wet grinding, freeze grinding, spray freeze drying, and the like. Methods for microparticulating the bottom-up include emulsion polymerization, suspension polymerization, dispersion polymerization, radical polymerization, emulsion polymerization, sol-gel, reprecipitation, microwave heating, and the like.

[0081] In the dispersion polymerization, for example, polydimethylsiloxane terminated with methacryloxypropyl groups is used as a stabilizer to polymerize styrene or methacrylic acid ester in an organic solvent, thereby obtaining fine particles.

[0082] The content of the third protective layer 80 relative to the first nanoparticles is preferably 1 part by mass to 1000 parts by mass, with the content of the first nanoparticles being 1 part by mass.

[0083] When observed under a transmission electron microscope (TEM), the average inter-surface distance of the first nanoparticles is preferably 1 nm to 100 nm.

[0084] (Other additives) In this embodiment, the light-responsive composition may be used in combination with an oxygen remover, an antioxidant, a scattering agent such as titanium oxide, a surfactant, an anti-mold agent, a light stabilizer, or other additives that impart various properties, a diluting solvent, etc., as necessary.

[0085] <Second embodiment> The light-responsive composition according to the second embodiment will be described with reference to Fig. 3. The light-responsive composition 200 according to the second embodiment differs from the light-responsive composition 100 according to the first embodiment in that the medium 77 contains a polymer 160 in which a polymerizable compound 150 is crosslinked to increase the viscosity.

[0086] <Third embodiment> The light-responsive composition according to the third embodiment will be described with reference to Fig. 4. The light-responsive composition 300 according to the third embodiment differs from the light-responsive composition 100 according to the first embodiment and the light-responsive composition 200 according to the second embodiment in that the second particle 66 has a fourth protective layer 90.

[0087] (Fourth protective layer) The fourth protective layer 90 is located between the medium 70, 77 and the second protective layer 50, and protects the second particles. In other words, the fourth protective layer 90 is located between the medium 70, 77 and the second protective layer 50, and protects the second protective layer 50. The fourth protective layer 90 preferably contains a polymer compound having a fourth organic group in a side chain. In addition, the fourth protective layer 90 preferably has a lower absorbance (optical density) than the second nanoparticles in the first wavelength band including at least one of ultraviolet and blue and the third band related to the emission wavelength of the second nanoparticles. The fourth protective layer 90 containing the second particles is preferably particulate with a diameter of 10 nm to 10 μm. The fourth protective layer 90 preferably has a crosslinked structure. Similarly to the third protective layer, the fourth protective layer 90 is provided such that the second protective layer 50 is in contact with the fourth protective layer 90 and the first protective layer 20 is not in contact with the fourth protective layer 90. The fourth protective layer 90 is configured to encapsulate the second nanoparticles 40 but not the first nanoparticles 10. By providing the fourth protective layer 90 in this manner, the exchange of halogens originating from the first nanoparticles 10 and the second nanoparticles 40 via the media 70 and 77 is further restricted.

[0088] (fourth organic group) The fourth organic group may be at least one of a linear, branched or cyclic alkyl group, a linear, branched or cyclic heteroalkyl group, an aryl group, a heteroaryl group, an aralkyl group, and a heteroaralkyl group. The fourth organic group may have a substituent that is partially substituted.

[0089] (Method of forming the fourth protective layer) The method for forming the fourth protective layer 90 is not particularly limited, and may be a top-down method of microparticulating the bulk of the fourth protective layer 90 containing the second particles, or a bottom-up method of microparticulating the bulk of the fourth protective layer 90. An appropriate method may be selected depending on the application.

[0090] In the case of top-down microparticulation, first, a bulk body of the fourth protective layer 90 containing the second particles is formed. Methods for forming the bulk body include a method of polymerizing a mixture containing a polymerizable compound and the second particles, and a method of mixing the second particles with a polymer compound. Methods for microparticulating the bulk body include dry grinding, wet grinding, freeze grinding, spray freeze drying, etc. Methods for microparticulating the bottom-up body include emulsion polymerization, suspension polymerization, dispersion polymerization, radical polymerization, emulsion polymerization, sol-gel, reprecipitation, microwave heating, etc.

[0091] In the dispersion polymerization, for example, polydimethylsiloxane terminated with methacryloxypropyl groups is used as a stabilizer to polymerize styrene or methacrylic acid ester in an organic solvent, thereby obtaining fine particles.

[0092] The content of the fourth protective layer 90 relative to the second nanoparticles is preferably 1 part by mass to 1000 parts by mass, with the content of the second nanoparticles being 1 part by mass.

[0093] When observed under a transmission electron microscope (TEM), the average inter-surface distance of the second nanoparticles is preferably 1 nm to 100 nm.

[0094] <Fourth embodiment> The flowable light-responsive compositions 100, 200, 300 exhibit the effect of the present invention of reducing halogen exchange and stabilizing the composition even when the light-responsive compositions 100, 200, 300 are cured on a substrate. The light-responsive compositions 200 (100, 300) are in the form of a layer supported by another member, and may be referred to as a wavelength conversion layer. Support forms include a laminated form and a dispersed form dispersed in a matrix material. Examples of the wavelength conversion layer include a light-responsive composition coated on a support member (substrate) and cured to form a film, sheet, or patterned pixels.

[0095] FIG. 5 shows a cross-sectional structure of a display element 400 according to the fourth embodiment.

[0096] The display element 400 has a light-emitting layer 410, a dielectric multilayer film 417, and a wavelength conversion layer 420 stacked in a stacking direction D1. The downstream side in the stacking direction D1 corresponds to the side where a user who views an image drawn on the display element is positioned. The wavelength conversion layer 420 is separated from the wavelength conversion layers corresponding to adjacent elements by a black matrix BM that separates the pixels.

[0097] As described above, the light-responsive composition 200 is cured together with the polymerizable compound 150 by carrying out a polymerization process such as a photopolymerization process. The light-responsive composition 200 is cured to become a solid light-responsive composition 426 supported by the dielectric multilayer film 417. The light-responsive composition 426 is configured to satisfy a predetermined dimension, thereby forming the wavelength conversion layer 420 of the display element 400. In other words, the wavelength conversion layer 420 is a layer in which the light-responsive composition 200 is solidified by being entirely cured together with the polymerizable compound 150.

[0098] The light emitting layer 410 corresponds to a light source that emits light L1 of a first wavelength λ1. The wavelength conversion layer 420 has an optical coupling surface 422 that is optically coupled to the light emitting layer 410 on the side of the light emitting layer 410, and has an extraction surface 424 on the opposite side of the light emitting layer 410 that is converted by the wavelength conversion layer 420 and extracts the secondary light L2.

[0099] The wavelength conversion layer 420 of this embodiment receives primary light L1 of wavelength λ1 propagating through the dielectric multilayer film 417. The dielectric multilayer film 417 provides the display element 400 with the spectral transmission characteristics of the primary light from the light emitting layer 410 and the spectral reflection characteristics of secondary light L2 of wavelength λ2 emitted in the wavelength conversion layer 420. The wavelength λ2 of the secondary light L2 is longer than the wavelength λ1 of the primary light L1.

[0100] The dielectric multilayer film 417 can be replaced with another optical member having optical transparency to the first wavelength λ1 emitted by the light emitting layer 410. In addition, another optical member (not shown) can be disposed in front of the extraction surface 424 (opposite side to the light emitting layer 410).

[0101] (Method of forming wavelength conversion layer) The method for forming the wavelength conversion layer is not particularly limited, and examples thereof include a method in which a photoresponsive composition is applied onto a substrate, and then pre-dried as necessary, and further, if necessary, heated or irradiated with active energy rays to cure the film. The thickness of the cured wavelength conversion layer is preferably 0.1 to 200 μm, more preferably 1 to 100 μm.

[0102] The active energy ray in the active energy ray irradiation is appropriately selected from electromagnetic waves such as heat rays, ultraviolet rays, visible rays, near infrared rays, and electron beams that reduce fluidity and promote curing through polymerization, crosslinking, drying, etc. As a light source for applying active energy rays, a light source having a main wavelength of emission in the wavelength region of 100 to 450 nm is preferable. Examples of such light sources include ultra-high pressure mercury lamps, high pressure mercury lamps, medium pressure mercury lamps, mercury xenon lamps, metal halide lamps, high power metal halide lamps, xenon lamps, pulsed xenon lamps, deuterium lamps, fluorescent lamps, ND-YAG triple wave lasers, HE-CD lasers, nitrogen lasers, XE-Cl excimer lasers, XE-F excimer lasers, semiconductor pumped solid state lasers, and LED lamp light sources having emission wavelengths of 365 nm, 375 nm, 385 nm, 395 nm, and 405 nm.

[0103] ((Measurement method)) The various physical property measurements can be carried out as follows.

[0104] ((Molecular weight distribution measurement)) The molecular weight distribution of the polymer compound in the first and second protective layers can be calculated in terms of monodisperse polymethyl methacrylate by gel permeation chromatography (GPC). Measurement of the molecular weight by GPC can be performed, for example, as follows.

[0105] The sample is added to the eluent below so that the sample concentration becomes 1% by mass, and the solution is left to stand at room temperature for 24 hours to dissolve. The solution is then filtered through a solvent-resistant membrane filter with a pore size of 0.45 μm to obtain the sample solution, which is then measured under the following conditions. Apparatus: Agilent 1260 infinity system (Agilent Technologies) Column: PFG analytical linear M columns (PSS) Eluent: 2,2,2-trifluoroethanol Flow rate: 0.2ml / min Oven temperature: 40℃ Sample injection volume: 20 μL

[0106] In calculating the molecular weight distribution of the sample, a molecular weight calibration curve prepared using a standard polymethyl methacrylate resin (EasiVial PM Polymer Standard Kit manufactured by Agilent Technologies) is used.

[0107] ((composition analysis)) The composition of the first and second protective layers can be analyzed by nuclear magnetic resonance (NMR). For example, 1H-NMR and 13C-NMR spectrum measurements are performed using an ECA-600 (600 MHz) manufactured by JEOL Ltd. The measurements are performed at 25°C in a deuterated solvent containing tetramethylsilane as an internal standard. The chemical shift value is read as a ppm shift value (δ value) with the internal standard tetramethylsilane set to 0.

[0108] ((Crystal structure analysis)) The crystal structure and composition of the first and second nanoparticles can be analyzed by X-ray diffraction (XRD). For example, the crystal structure and composition can be analyzed by measuring the X-ray diffraction pattern using a RINT 2100 (manufactured by Rigaku). Depending on the shape and size of the sample to be analyzed, electron diffraction (ED) accompanying a cross-sectional TEM may be employed.

[0109] ((Composition analysis of the first nanoparticle and the second nanoparticle)) The compositional analysis of the first nanoparticles and the second nanoparticles can also be performed using XPS and ICP emission spectroscopy. The molar ratio of A and B can be measured from the signal intensity of XPS, and the concentration of X can be measured from the emission intensity of ICP emission spectroscopy (e.g., CIROS CCD (SPECTRO)).

[0110] ((amount of first nanoparticles, second nanoparticles)) The amount of the first nanoparticles 10 or the second nanoparticles 40 contained in the light-responsive composition 100 can be measured using ICP optical emission spectroscopy. For example, the amount of Pb can be measured from the emission intensity of ICP optical emission spectroscopy, and compared with the composition information of the first nanoparticles 10 and the second nanoparticles 40 obtained by the above method, thereby calculating the amount of the first nanoparticles 10 and the second nanoparticles 40.

[0111] ((Amount of the first and second protective layers for nanoparticles)) The amounts of the first and second protective layers on the first and second nanoparticles, respectively, can be determined by TG-DTA measurement. They can also be determined from the NMR integrated intensity of the first particle 30 or the second particle 40.

[0112] ((Medium Composition)) When the medium 70 is in a liquid or fluid form, composition analysis can be performed using NMR and mass spectrometry. When the medium 77 is in a solid (cured) form, composition analysis can be performed using pyrolysis gas chromatography.

[0113] ((Confirmation of the presence of the third protective layer in the photoresponsive composition)) When the light-responsive composition 100, 300 (medium 70) is liquid, this can be confirmed by separating the first particles 30 including the medium 70 and the third protective layer 80 from the light-responsive composition 100, 300 by centrifugation. When the light-responsive composition 200 (medium 77) is solid, this can be confirmed by TEM observation. When the third protective layer 80 is not present, the first particles 30 are observed to be uniformly spread throughout the medium, but when the third protective layer 80 is present, a bias in the distribution is observed.

[0114] ((Amount of first nanoparticles 10 in first particle 30)) The amount of the first nanoparticles 10 contained in the first particles 30 can be measured using ICP emission spectrometry. A mixture containing the third protective layer 80, the first nanoparticles 10, and the first protective layer 20 may be decomposed with an acid and analyzed by ICP emission spectrometry. The amount of the second particles 40 contained in the second particles 60 may be determined in the same manner.

[0115] ((Method of Calculating Particle Size of First Particle 30)) The particle size of the first particle 30 including the third protective layer 80 can be calculated by TEM observation.

[0116] ((Average surface distance of the first nanoparticles 10 contained in the first particle 30)) The average inter-surface distance of the first nanoparticles 10 contained in the first particle 30 can be calculated by TEM observation. EXAMPLES

[0117] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited thereto.

[0118] [Production of polymer compound a] A reaction vessel equipped with a cooling tube, a stirrer, a thermometer, and a nitrogen inlet tube was prepared. 26.5 parts of 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propane-1-sulfonic acid, 42.3 parts of hexyl methacrylate, 3.9 parts of azobisisobutyronitrile, and 900 parts of 2,2,2-trifluoroethanol were charged into the reaction vessel. Nitrogen was then bubbled into the reaction vessel for 30 minutes.

[0119] The resulting reaction mixture was heated at 70°C for 8 hours under a nitrogen atmosphere to complete the polymerization reaction. After cooling the reaction solution to room temperature, 300 parts of water was added to precipitate the product. After centrifugation, the supernatant was removed. The solvent was removed by distillation under reduced pressure, and the polymer compound a was obtained by drying under reduced pressure at 50°C and 0.1 kPa or less. NMR measurement confirmed that the ratio of units containing sulfobetaine groups in the polymer was 18 mol%.

[0120] [Production of polymer compound b] Polymer compound b was produced in the same manner as polymer compound a, except that the amount of 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propane-1-sulfonic acid was changed from 26.5 parts to 10.2 parts, and the amount of hexyl methacrylate was changed from 42.3 parts to 45.4 parts in the production of polymer compound a. NMR measurement confirmed that the ratio of units containing sulfobetaine groups in the polymer was 12 mol%.

[0121] [Production of polymer compound c] Polymer compound c was produced in the same manner as polymer compound a, except that 25.4 parts of 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propane-1-sulfonic acid was replaced with 4.7 parts of methacrylic acid and 42.3 parts of hexyl methacrylate, instead of 45.4 parts. NMR measurement confirmed that the ratio of units containing carboxy groups in the polymer was 18 mol%.

[0122] [Preparation of polymer solution] (Toluene solution of polymer compound a) In a reaction vessel equipped with a stirrer, a thermometer, and a reflux condenser, 1 part of polymer compound a and 99 parts of toluene were charged, and the temperature was raised to 110° C. and heated for 5 minutes. After confirming that polymer compound a was completely dissolved, the mixture was cooled to room temperature to obtain a toluene solution of polymer compound a.

[0123] (Toluene solution of polymer compound b) A toluene solution of polymer compound b was prepared in the same manner as the toluene solution of polymer compound a, except that polymer compound b was used instead of polymer compound a.

[0124] (Toluene solution of polymer compound c) A toluene solution of polymer compound c was prepared in the same manner as the toluene solution of polymer compound a, except that polymer compound c was used instead of polymer compound a.

[0125] [Preparation of first nanoparticle dispersion a] 10 parts of cesium carbonate, 27 parts of oleic acid, and 385 parts of 1-octadecene were placed in a flask, heated to 120°C, and degassed with a vacuum pump for 30 minutes. The mixture was further heated to 150°C under a dry nitrogen stream and held for 30 minutes to obtain a cation raw material liquid.

[0126] Separately, 10 parts of lead(II) bromide and 494 parts of 1-octadecene were placed in a flask, heated to 120°C, and degassed with a vacuum pump for 1 hour. 89 parts of oleic acid and 31 parts of oleylamine were added, and the mixture was degassed with a vacuum pump for 30 minutes. The nitrogen flow was then replaced and the liquid temperature was raised to 185°C.

[0127] 40 parts of the cation raw material solution was added, and after 5 seconds, the mixture was cooled on ice. 2000 parts of ethyl acetate was added, and the mixture was centrifuged to remove the supernatant. The resulting residue was dispersed in toluene to adjust the solid content to 1% by weight, and a first nanoparticle dispersion a having a perovskite crystal structure of CsPbBr3 was obtained.

[0128] [Preparation of second nanoparticle dispersion b] A second nanoparticle dispersion b having a perovskite crystal structure of CsPb(Br / I)3 was obtained in the same manner as in the luminescent nanocrystal dispersion a, except that 3.2 parts of lead(II) bromide and 9.3 parts of lead(II) iodide were used instead of 10 parts of lead(II) bromide.

[0129] Example 1 [Preparation of first particles 30-1] 10 parts of the first nanoparticle dispersion a was placed in a container, and the solvent was distilled off under reduced pressure. 10 parts of a toluene solution of polymer compound a was added thereto, and the mixture was stirred for 1 hour, and the solvent was distilled off under reduced pressure. 10 parts of hexane was added to obtain a hexane dispersion of the first particles 30-1.

[0130] [Preparation of second particles 60-1] A hexane dispersion of second particles 60-1 was obtained in the same manner as for the first particles 30-1, except that the second nanoparticle dispersion b was used instead of the first nanoparticle dispersion a.

[0131] [Preparation of Particle 1 Including Third Protective Layer 80 and First Particle] 30 parts of the hexane dispersion of the first particles 30-1, 200 parts of hexane, 5 parts of polydimethylsiloxane terminated with methacryloxypropyl groups (manufactured by Gelest, product name DMS-R22), 30 parts of methyl methacrylate, 3 parts of trimethylolpropane trimethacrylate, and 2 parts of 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) were mixed and reacted at 40°C for 2 hours.

[0132] After the reaction was stopped by cooling on ice, 200 parts of hexane was added, centrifuged, and the supernatant was removed. 400 parts of hexane was added to redisperse the mixture, centrifuged, and the supernatant was removed. The solvent was distilled off under reduced pressure to obtain a first particle 30-1 including a third protective layer 80, a first nanoparticle 10, and a first protective layer 20.

[0133] [Preparation of second particle 60-1 including fourth protective layer 90, second nanoparticle 40, and second protective layer 50] A second particle 60-1 including a fourth protective layer 90, a second particle 40, and a second protective layer 50 was obtained in the same manner as the first particle 30-1 including a third protective layer 80, a first nanoparticle 10, and a first protective layer 20, except that a second particle 60-1 was used instead of the first particle 30-1.

[0134] [Preparation of Photoresponsive Composition 1] A third protective layer 80, a first nanoparticle 10, 10 parts of a first particle 30-1 including a first protective layer 20, a fourth protective layer 90, a second particle 40, 10 parts of a particle 1 including a second protective layer 50, 75 parts of butyl acrylate, and 5 parts of 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (manufactured by IGM Resins, product name Omnirad TPO) were mixed to obtain a photoresponsive composition 1.

[0135] Example 2 [Preparation of first particles 30-2] A hexane dispersion of the first particles 30-2 was obtained in the same manner as the hexane dispersion of the first particles 30-1, except that the polymer compound a was changed to the polymer compound c.

[0136] [Preparation of second particles 60-2] A hexane dispersion of second particles 60-2 was obtained in the same manner as the hexane dispersion of second particles 60-1, except that the polymer compound b was changed to the polymer compound c.

[0137] [Preparation of first particle 30-2 including third protective layer 80, first nanoparticle 10, and first protective layer 20] A first particle 30-2 including a third protective layer 80, a first nanoparticle 10, and a first protective layer 20 was obtained in the same manner as the first particle 30-1 including a third protective layer 80, a first nanoparticle 10, and a first protective layer 20, except that a first particle 30-2 was used instead of the first particle 30-1.

[0138] [Preparation of second particle 60-2 including fourth protective layer 90 and second nanoparticle 40] A second particle 60-2 including a fourth protective layer 90, a second nanoparticle 40, and a second protective layer 50 was obtained in the same manner as the first particle 30-1 including a fourth protective layer 90, a second nanoparticle 40, and a second protective layer 50, except that the first particle 30-2 was used instead of the first particle 30-1.

[0139] [Preparation of Photoresponsive Composition 2] Photoresponsive composition 2 was obtained in the same manner as photoresponsive composition 1, except that first particle 30-2 was used instead of first particle 30-1, and second particle 60-2 was used instead of second particle 60-1.

[0140] Example 3 [Preparation of Photoresponsive Composition 3] 10 parts of the hexane dispersion of the second particles 60-1 were placed in a container and the solvent was removed under reduced pressure. 10 parts of the first particles 30-1 including the third protective layer 80 and the first nanoparticles 10, 75 parts of butyl acrylate, and 5 parts of 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (manufactured by IGM Resins, product name Omnirad TPO) were mixed therein to obtain a photoresponsive composition 3.

[0141] Comparative Example 1 10 parts of the hexane dispersion of the first particles 30-1 and 10 parts of the hexane dispersion of the second particles 60-1 were placed in a container and the solvent was removed under reduced pressure. 75 parts of butyl acrylate and 5 parts of 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (manufactured by IGM Resins, product name OmniradTPO) were then mixed therein to obtain a photoresponsive composition 4.

[0142] The composition of each photoresponsive composition is shown in Table 1.

[0143] [Table 1]

[0144] <Evaluation of photoresponsive composition> The obtained light-responsive composition was subjected to the following evaluations, and the results are shown in Table 2.

[0145] [Color mixing evaluation] The emission peak wavelength of each photoresponsive composition was measured immediately after preparation and 5 minutes later under the following measurement conditions and evaluation criteria:

[0146] <Measurement conditions> Measurement equipment: Absolute PL quantum yield measurement equipment C9920-03 (Hamamatsu Photonics) Excitation light wavelength: 460 nm Excitation light integration range: Excitation light wavelength ±10nm Emission integral range: (excitation light wavelength + 20) nm to 770 nm

[0147] <Evaluation criteria> The absolute value of the difference in the wavelength at which the emission was maximum in the range of 500 nm to 600 nm was calculated immediately after preparation and 5 minutes later, and evaluation was performed according to the following criteria. A: The absolute value of the difference in wavelength above is 0 nm or more and less than 20 nm B: The absolute value of the difference in wavelength above is 20 nm or more and less than 50 nm C: The absolute value of the difference in wavelength above is 50 nm or more

[0148] The evaluation results are shown in Table 2.

[0149] [Table 2]

[0150] According to Table 2, the light-responsive compositions 1 to 3 according to Examples 1 to 3 have reduced color mixing compared to the light-responsive composition 4 according to Comparative Example 1. This is presumably because the two types of nanoparticles having a perovskite structure are protected by multiple protective layers having specific structures.

[0151] The light-responsive composition according to each embodiment described in the present specification corresponds to at least one of the following configurations 1 to 18.

[0152] Configuration 1 The media and a first nanoparticle having a photoresponsive perovskite-type crystal structure; a first protective layer having a first organic group and a first binding portion coordinated to the first nanoparticle and protecting the first nanoparticle; and a third protective layer located between the medium and the first protective layer and protecting the first particle; and a first particle supported by the medium; a second nanoparticle having a perovskite-type crystal structure with a different composition from that of the first nanoparticle; and a second protective layer having a second organic group and a binding portion that coordinates to the second nanoparticle and that protects the second nanoparticle, the second particle being supported by the medium; A light-responsive composition comprising:

[0153] Configuration 2 The photoresponsive composition according to configuration 1, wherein the third protective layer contains a polymer having a third organic group in a side chain.

[0154] Configuration 3 The light-responsive composition according to configuration 1 or 2, wherein the first protective layer is in contact with the third protective layer, and the second protective layer is not in contact with the third protective layer.

[0155] Configuration 4 The light-responsive composition according to configuration 1 or 2, wherein the first protective layer is protected by the third protective layer.

[0156] Configuration 5 The light-responsive composition according to any one of configurations 1 to 4, wherein the third protective layer encapsulates the first particles but does not encapsulate the second particles.

[0157] Configuration 6 The photoresponsive composition according to any one of configurations 1 to 5, wherein the third protective layer has lower absorbance than the first nanoparticles in a first wavelength band including at least one of ultraviolet and blue and in a second wavelength band corresponding to the emission wavelength of the first nanoparticles.

[0158] Configuration 7 The light-responsive composition according to any one of aspects 1 to 6, wherein the medium contains a polymerizable compound.

[0159] Configuration 8 8. The light-responsive composition according to claim 7, wherein the medium comprises a solvent.

[0160] Configuration 9 The light-responsive composition according to any one of configurations 1 to 8, wherein the medium includes a polymer matrix in which the first particles and the second particles are each dispersed.

[0161] Configuration 10 The photoresponsive composition according to claim 9, wherein the medium is a sheet-like solid.

[0162] Configuration 11 The light-responsive composition according to configuration 1, wherein the second particles are located between the medium and the second protective layer, and further comprises a fourth protective layer that protects the second particles.

[0163] Configuration 12 The photoresponsive composition according to embodiment 11, wherein the fourth protective layer contains a polymer having a fourth organic group in a side chain.

[0164] Configuration 13 The light-responsive composition according to configuration 11 or 12, wherein the second protective layer is in contact with the fourth protective layer, and the first protective layer is not in contact with the fourth protective layer.

[0165] Configuration 14 The light-responsive composition according to any one of configurations 11 to 13, wherein the second protective layer is protected by the fourth protective layer.

[0166] Configuration 15 15. The light-responsive composition according to claim 11, wherein the fourth protective layer encapsulates the second particles but does not encapsulate the first particles.

[0167] Configuration 16 The photoresponsive composition according to any one of configurations 11 to 15, wherein the fourth protective layer has lower absorbance than the first nanoparticles in a first wavelength band including at least one of ultraviolet and blue and in a third wavelength band corresponding to the emission wavelength of the second nanoparticles.

[0168] Configuration 17 The photoresponsive composition according to any one of configurations 1 to 16, wherein the first particles exhibit a light-emitting characteristic of emitting more of either green or red, and the second particles exhibit a light-emitting characteristic of emitting more of the other of green or red.

[0169] Configuration 18 The photoresponsive composition according to any one of configurations 1 to 17, wherein the first particles contain either bromine or iodine in a large amount, and the second particles contain either the other of bromine or iodine in a large amount. [Explanation of symbols]

[0170] 10 The first nanoparticles 20 First protective layer 30 1st particle 40 The second nanoparticle 50 Second layer of protection 60 2nd particle 70 Medium 80 Third Layer of Protection 90 The Fourth Layer of Protection 110 First joint 120 First Organic Group 150 Polymerizable compounds 160 Polymer 100, 200, 300 Photoresponsive composition

Claims

1. The media and a first nanoparticle having a photoresponsive perovskite-type crystal structure; a first protective layer having a first organic group and a first bonding portion coordinated to the first nanoparticle, and protecting the first nanoparticle; and a third protective layer located between the medium and the first protective layer, and protecting the first particle; and a first particle supported by the medium; a second nanoparticle having a perovskite-type crystal structure with a different composition from that of the first nanoparticle; and a second protective layer having a second organic group and a binding portion coordinated to the second nanoparticle and protecting the second nanoparticle, the second particle being supported by the medium; A light-responsive composition comprising:

2. The light-responsive composition according to claim 1 , wherein the third protective layer contains a polymer having a third organic group in a side chain.

3. 3. The light-responsive composition according to claim 1, wherein the first protective layer is in contact with the third protective layer, and the second protective layer is not in contact with the third protective layer.

4. The light-responsive composition according to claim 1 or 2, wherein the first protective layer is protected by the third protective layer.

5. The light-responsive composition according to claim 1 or 2, wherein the third protective layer encapsulates the first particles but does not encapsulate the second particles.

6. 3. The light-responsive composition according to claim 1, wherein the third protective layer has a lower absorbance than the first nanoparticles in a first wavelength band including at least one of ultraviolet and blue and in a second wavelength band corresponding to the emission wavelength of the first nanoparticles.

7. The photoresponsive composition according to claim 1 or 2, wherein the medium contains a polymerizable compound.

8. The light-responsive composition of claim 7 , wherein the medium comprises a solvent.

9. The light-responsive composition according to claim 1 or 2, wherein the medium comprises a polymer matrix in which the first particles and the second particles are each dispersed.

10. The light-responsive composition according to claim 9 , wherein the medium is a sheet-like solid.

11. The light-responsive composition of claim 1 , wherein the second particles are provided with a fourth protective layer located between the medium and the second protective layer and protecting the second particles.

12. The light-responsive composition according to claim 11 , wherein the fourth protective layer contains a polymer having a fourth organic group in a side chain.

13. The light-responsive composition according to claim 11 or 12, wherein the second protective layer is in contact with the fourth protective layer, and the first protective layer is not in contact with the fourth protective layer.

14. The light-responsive composition according to claim 11 or 12, wherein the second protective layer is protected by the fourth protective layer.

15. The light-responsive composition according to claim 1 or 2, wherein the fourth protective layer encapsulates the second particles but does not encapsulate the first particles.

16. The photoresponsive composition according to claim 11 or 12, wherein the fourth protective layer has a lower absorbance than the first nanoparticles in a first wavelength band including at least one of ultraviolet and blue and in a third wavelength band corresponding to the emission wavelength of the second nanoparticles.

17. 3. The photoresponsive composition according to claim 1 or 2, wherein the first particles have an emission characteristic of emitting more of either green or red, and the second particles have an emission characteristic of emitting more of the other of green or red.

18. 3. The light-responsive composition according to claim 1, wherein the first particles contain a large amount of either bromine or iodine, and the second particles contain a large amount of the other of either bromine or iodine.

Citation Information

Patent Citations

  • Light conversion film and liquid crystal display element using the same

    JP2018197782A

  • Luminescent component

    JP2021006900A