Interleaving paper, and paper tableware and clothes hanger made therefrom

Interleaf paper with controlled coarseness and fiber length, bonded by an adhesive layer, addresses the limitations of conventional paper products by enhancing strength, moldability, and water absorption resistance, suitable for paper tableware and clothing hanging tools.

JP2024141112APending Publication Date: 2024-10-10OJI HLDG CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023052582
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Conventional paper products used as substitutes for plastics lack sufficient strength, moldability, feel, and water absorption resistance when processed into various products, failing to meet the requirements for excellent paper alternatives.

Method used

The development of interleaf paper comprising at least two sheets of base paper with specific coarseness and length-weighted average fiber length, bonded by an adhesive layer, and optionally featuring a thermoplastic resin layer, with controlled thickness and internal sizing agents to enhance strength, moldability, and water absorption resistance.

Benefits of technology

The interleaf paper exhibits improved strength, moldability, feel, and water absorption resistance after pressure molding, making it suitable for various processed products such as paper tableware and clothing hanging tools.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141112000001_ABST
    Figure 2024141112000001_ABST
Patent Text Reader

Abstract

To provide an interleaving paper for pressure molding which is excellent in all respects: strength, formability, touch, and water absorption resistance of the end face after pressure molding.SOLUTION: An interleaving paper for pressure molding of the invention comprises at least two base papers and an adhesive layer between the at least two base papers, wherein the pulp contained in each of the two or more base papers has a coarseness of 0.03 mg / m to 0.15 mg / m, the length-weighted average fiber length of the pulp is 0.60 mm to 1.50 mm, and the thickness of the interleaving paper is 0.68 mm to 2.10 mm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to interleaf paper formed by bonding a plurality of papers together, and to paper tableware and clothes hanging tools which are processed from the interleaf paper. [Background technology]

[0002] Conventionally, plastic molded products such as synthetic resins have been widely used for disposable tableware, stationery, medical equipment, etc. However, from the viewpoint of environmental protection such as greenhouse gas emissions and marine pollution, the replacement of plastic products with paper products is being promoted. For example, Patent Document 1 discloses a technology for increasing the strength and durability of coated tableware paper by controlling the amount of softwood bleached kraft pulp and hardwood bleached kraft pulp used in each layer of a multi-layer paper and incorporating fully saponified polyvinyl alcohol in the surface layer. Furthermore, Patent Document 2 discloses a technology for controlling the amount of softwood bleached kraft pulp and hardwood bleached kraft pulp used in each layer of a multilayer paper from the standpoint of sufficient thickness and strength, and further controlling the basis weight of each layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-196990 A [Patent Document 2] Patent Publication No. 2021-080590 Summary of the Invention [Problem to be solved by the invention]

[0004] However, according to the inventors' investigations, when it is assumed that the paper will be processed into various products as a replacement for plastic products, it is not sufficient in terms of providing excellent strength, formability, feel (smoothness), and water absorption resistance of the edge surface after pressure molding. The present disclosure provides an interleaf paper for pressure molding that is excellent in all respects: strength, formability, feel, and water absorption resistance of the end faces after pressure molding. [Means for solving the problem]

[0005] As a result of extensive research, the inventors have found that the above-mentioned problems can be solved by using base paper containing pulp having a specific courseness (fiber coarseness) and length-weighted average fiber length, and controlling the thickness of the interleaving paper formed by bonding these base papers together via an adhesive layer.

[0006] That is, the present disclosure relates to the following [1] to

[11] . [1] An interleaving paper for pressure molding, comprising at least two base papers and an adhesive layer between the at least two base papers, The coarseness of the pulp contained in each of two or more sheets of the base paper is 0.03 mg / m to 0.15 mg / m; The length-weighted average fiber length of the pulp is 0.60 mm to 1.50 mm; The thickness of the slip paper is 0.68 mm to 2.10 mm. [2] The interleaf paper according to [1], wherein the interleaf paper has a thermoplastic resin layer on at least one surface. [3] The interleaving paper according to [1] or [2], wherein the pulp has a coarseness of 0.04 mg / m to 0.08 mg / m. [4] The interleaving paper according to any one of [1] to [3], wherein the base paper contains an internal sizing agent, and the content of the internal sizing agent is 0.2 mass% or more relative to the total mass of the base paper. [5] The base paper contains an internal sizing agent, and the internal sizing agent is a rosin-based sizing agent. The interleaving paper according to any one of [1] to [4]. [6] The basis weight of the entire base paper in the interleaving paper is 560 g / m 2 ~1800g / m 2 The interleaving paper according to any one of [1] to [5], [7] The interleaf paper has a thermoplastic resin layer on at least one surface, the base paper contains an internal sizing agent, the internal sizing agent is a rosin-based sizing agent, and the content of the internal sizing agent is 0.2% by mass or more based on the total mass of the base paper; The basis weight of the entire base paper in the interleaving paper is 560 g / m 2 ~1800g / m 2 The interleaving paper according to any one of [1] to [6], [8] Paper tableware, which is a processed product made from the interleaving paper described in any one of [1] to [7]. [9] The paper tableware according to [8], At least a part of the edge of the paper tableware is pressed and crushed in the thickness direction.

[10] A clothes hanging device which is a processed product of the interleaving paper described in any one of [1] to [7].

[11] The clothes hanging device according to

[10] , At least a part of the end of the clothes hanging tool is compressed by pressure in the thickness direction. Effect of the Invention

[0007] According to the present disclosure, it is possible to provide an interleaf paper for pressure molding that is excellent in all respects: strength, formability, feel, and water absorption resistance of the end faces after pressure molding. [Brief description of the drawings]

[0008] [Figure 1] This is an example of an embodiment of an interleaf paper including two base papers (paper base layer). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] In this specification, the description of "X or more and Y or less" or "X to Y" representing a numerical range means a numerical range including the lower and upper limits which are the endpoints, unless otherwise specified. When a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined.

[0010] <Interleaf paper> The interleaving paper according to the present embodiment is for pressure molding and includes at least two base papers and an adhesive layer between the at least two base papers. For example, the interleaving paper may be made of only base paper A, an adhesive layer, and base paper B, or may be made by laminating another base paper via an adhesive layer. The at least two base papers may be three base papers. In this case, the interleaving paper has, for example, base paper A, an adhesive layer, base paper B, an adhesive layer, and base paper C in this order. The interleaf paper may have a thermoplastic resin layer on at least one surface, or on both surfaces. Fig. 1 shows an embodiment in which an interleaf paper 10 has a thermoplastic resin layer 4 on both surfaces. In Fig. 1, base paper 1 and base paper 2 are laminated via adhesive layer 3, and the outer surfaces of base paper 1 and base paper 2 have thermoplastic resin layers 4.

[0011] <Base paper> The base paper is not particularly limited as long as it is a commonly used paper, and is preferably paper containing plant-derived pulp as a main component, and more preferably paper containing wood pulp as a main component. Specific examples of the kraft paper include kraft paper, fine paper, (white) paperboard, base paper for paper containers, base paper for milk cartons, base paper for cups, liner paper, coated paper, one-sided glossy paper, glassine paper, graphene paper, etc. Among these, kraft paper, fine paper, (white) paperboard, base paper for paper containers, base paper for cups, and one-sided glossy paper are preferred, and among (white) paperboards, high-grade paperboard, special paperboard, base paper for cups, and kraft paper are more preferred in terms of rigidity. Examples of the kraft paper include bleached kraft paper, unbleached kraft paper, and one-sided glossy bleached kraft paper, and in terms of printability and hygiene, bleached kraft paper and one-sided glossy bleached kraft paper are preferred.

[0012] <Coarseness, length-weighted average fiber length, thickness of interleaf paper> In order to obtain a slip sheet that is excellent in all respects, including strength, formability, feel, and water absorption resistance of the edge surface after pressure forming, it is necessary to control the coarseness and length-weighted average fiber length of the pulp contained in each of two or more base papers used in the slip sheet within specific ranges, and then to control the thickness of the slip sheet.

[0013] Increasing the basis weight of the base paper or laminating more base papers to make the thickness of the interleaf paper increases the strength of the interleaf paper, but decreases the formability and water absorption resistance of the end surface after pressure molding. Shortening the length-weighted average fiber length of the pulp contained in the base paper improves the formability and water absorption resistance of the end surface after pressure molding of the interleaf paper, but decreases the feel. The inventors of the present invention have conducted research to obtain interleaf paper that is excellent in all of strength, formability, feel, and water absorption resistance of the end surface after pressure molding, and have found that controlling the coarseness and length-weighted average fiber length of the pulp is important.

[0014] Coarseness is the mass of fiber per meter, and when the pulp has a low coarseness value, it indicates that it contains many fibers with large voids. This reduces the strength of the paper itself, but it is assumed that the fibers are more easily crushed, which improves the water absorption resistance of the edge after pressure molding. On the other hand, when the pulp has a high coarseness value, the fibers become rigid and the strength is likely to improve. However, if the coarseness value is too high, it is assumed that the fibers are less likely to be crushed, which reduces the water absorption resistance of the edge after pressure molding.

[0015] When the value of the length-weighted average fiber length of the pulp is small, it indicates that a large amount of short fibers are included. As a result, it is presumed that although the strength of the paper itself decreases, the movement of the fibers is less likely to be hindered and the moldability is more likely to improve. In addition, it is presumed that the gaps between the fibers are small, making it difficult for water to enter between the fibers, and therefore the water absorption resistance of the end face after pressure molding is more likely to improve. However, if the value of the length-weighted average fiber length is too small, the roughness of the end face increases and the feel is reduced. On the other hand, when the value of the length-weighted average fiber length of the pulp is large, it indicates that a large amount of long fibers are included. As a result, the number of starting points for entanglement of the paper and contact between the fibers increases, and the inter-fiber bonds increase, making it easier to improve the strength. In addition, the roughness of the end face decreases and the feel is improved. However, if the value of the length-weighted average fiber length is too large, it is presumed that the paper is less likely to stretch and the moldability is more likely to decrease. In addition, it is presumed that the gaps between the fibers are large, making it easier for water to enter between the fibers, and therefore the water absorption resistance of the end face after pressure molding is more likely to decrease.

[0016] Through investigations, the present inventors have found that by controlling the coarseness and length-weighted average fiber length of the pulp within specific ranges and then controlling the thickness of the entire interleaf paper, it is possible to obtain interleaf paper that is excellent in all respects: strength, formability, feel, and water absorption resistance of the end faces after pressure molding.

[0017] The coarseness of the pulp contained in each of the two or more base papers in the interleaf paper is 0.03 mg / m to 0.15 mg / m. By setting the coarseness of the pulp contained in the base papers within the above range, it is possible to obtain an interleaf paper that is excellent in both strength and water absorption resistance of the end faces after pressure molding. If the coarseness is less than the lower limit, the strength of the slip paper is likely to decrease, whereas if the coarseness is more than the upper limit, the water absorption resistance of the end face of the slip paper after pressure molding is likely to decrease.

[0018] The coarseness of the pulp is preferably 0.04 mg / m to 0.13 mg / m, more preferably 0.05 mg / m to 0.10 mg / m, and even more preferably 0.06 mg / m to 0.08 mg / m. The coarseness of the pulp may be 0.04 mg / m to 0.08 mg / m. It is preferable that the coarseness of the pulp in all base papers contained in the slip paper satisfies the above range. In other words, It is preferable that the coarseness of the pulp contained in the fiberboard satisfies the above range. The coarseness of the pulp can be controlled by the type of pulp used.

[0019] The length-weighted average fiber length of the pulp contained in each of the two or more base papers in the interleaf paper is 0.60 mm to 1.50 mm. By setting the length-weighted average fiber length of the pulp contained in the base papers within the above range, it is possible to obtain interleaf paper that is excellent in all respects: strength, formability, feel, and water absorption resistance of the end face after pressure forming. If the length-weighted average fiber length is less than the lower limit, the strength and feel of the slip paper are likely to decrease, whereas if the length-weighted average fiber length is more than the upper limit, the formability of the slip paper and the water absorption resistance of the end face after pressure molding are likely to decrease.

[0020] The length-weighted average fiber length of the pulp is preferably 0.65 mm to 1.30 mm, more preferably 0.75 mm to 1.10 mm, and even more preferably 0.80 mm to 0.95 mm. It is preferable that the length-weighted average fiber length of the pulp in all base papers contained in the slip paper satisfies the above range. In other words, it is preferable that the length-weighted average fiber length of the pulp contained in each of the base papers in the slip paper satisfies the above range. The length-weighted average fiber length of the pulp can be controlled by the type of pulp used, etc.

[0021] Of the at least two base papers, the coarseness and length-weighted average fiber length of the pulp contained in each of the two or more base papers satisfy the above-mentioned specific ranges. This means that, of the multiple base papers in the interleaving paper, at least two base papers each satisfy the above-mentioned specific ranges. For example, when there are two base papers in the interleaving paper, this means that both of the two base papers satisfy the above-mentioned specific ranges. When there are three or more base papers in the interleaving paper, it is sufficient that two or more of the base papers satisfy the above-mentioned specific ranges of the pulp coarseness and length-weighted average fiber length.

[0022] For example, it is sufficient that the interleaving paper contains three base papers, and the pulp contained in each of two of the base papers satisfies the above-mentioned ranges of coarseness and length-weighted average fiber length of the specific pulp. When the interleaving paper contains three base papers, it is preferable that the pulp contained in all three base papers satisfies the above-mentioned ranges of coarseness and average fiber length of the specific pulp. In other words, it is preferable that the interleaving paper contains at least two base papers, and each of the at least two base papers satisfies the above-mentioned ranges of coarseness and length-weighted average fiber length of the specific pulp.

[0023] The thickness of the slip paper is 0.68 mm to 2.10 mm. By setting the thickness of the slip paper within the above range, it is possible to obtain slip paper that is excellent in all respects: strength, formability, and water absorption resistance of the end face after pressure molding. If the thickness of the slip paper is less than the above lower limit, the strength of the slip paper is likely to decrease, whereas if the thickness of the slip paper is more than the above upper limit, the formability and the water absorption resistance of the end face after pressure molding are likely to decrease.

[0024] The thickness of the slip sheet is preferably 0.80 mm to 2.00 mm, more preferably 1.00 mm to 1.80 mm, and even more preferably 1.20 mm to 1.70 mm. The thickness of the slip sheet refers to the total thickness of the slip sheet, including the thickness of the adhesive layer between at least two sheets of base paper. When the slip sheet includes a resin layer such as a thermoplastic resin on the front or back surface, the thickness also includes the thickness of the thermoplastic resin layer.

[0025] The coarseness of the pulp contained in the interleaf paper (whole interleaf paper) is preferably 0.03 mg / m to 0.15 mg / m, more preferably 0.04 mg / m to 0.13 mg / m, and further preferably 0.05 mg / m to 0.10 mg / m, and more preferably 0.06 mg / m to 0.15 mg / m. By being in the above range, it becomes easier to obtain an interleaf paper that is excellent in both strength and water absorption resistance of the end face after pressure molding.

[0026] The length-weighted average fiber length of the pulp contained in the slip paper (whole slip paper) is preferably 0.60 mm to 1.50 mm, more preferably 0.65 mm to 1.30 mm, even more preferably 0.75 mm to 1.10 mm, and even more preferably 0.80 mm to 0.95 mm. By being in the above range, it becomes easier to obtain slip paper that is excellent in all of strength, formability, feel, and water absorption resistance of the end face after pressure molding.

[0027] The average fiber width of the pulp contained in each of the two or more base papers in the interleaf paper is not particularly limited, but is preferably 14.0 μm to 35.0 μm, and more preferably 15.0 μm to 34.0 μm. The average fiber width of the pulp can be controlled by, for example, cooking the wood chips. Increasing the cooking temperature or lengthening the cooking time can reduce the average fiber width. On the other hand, decreasing the cooking temperature or shortening the cooking time can increase the average fiber width. If cooking is insufficient, the average fiber width tends to exceed the upper limit.

[0028] The basis weight of each base paper is 290g / m 2 ~880g / m 2 and preferably 350 g / m 2 ~800g / m 2 More preferably, it is 480 g / m 2 ~710g / m 2 It is even more preferable that: When the thickness is within the above range, it becomes easy to obtain an interleaf paper that is excellent in all of strength, formability, and water absorption resistance of the end faces after pressure forming.

[0029] The density of each base paper is usually 0.50g / cm 3 ~1.20g / cm 3 and preferably 0.70 g / cm 3 ~1.00g / cm 3 It is.

[0030] The thickness of each of the base papers is usually 0.10 mm to 1.50 mm, preferably 0.30 mm to 1.20 mm, more preferably 0.50 mm to 1.00 mm, and further preferably 0.60 mm to 0.90 mm.

[0031] At least two sheets of base paper included in the slip paper may each be a base paper of a single layer construction obtained by single layer papermaking described later, or a base paper of a multilayer construction obtained by multilayer papermaking described later, but it is preferable that the base paper is a multilayer construction. By adopting a multilayer construction, the texture can be improved and strength can be ensured. When at least two sheets of base paper included in the slip paper each have a multilayer construction, the number of layers constituting one sheet of base paper is usually 2 to 10, preferably 3 to 9, and more preferably 4 to 8. By being in the above range, it becomes easier to improve the strength of the slip paper while maintaining the interlayer strength.

[0032] When at least two sheets of base paper included in the interleaf are multi-layered base paper, the basis weight of each layer constituting one sheet of base paper is 40 g / m 2 ~180g / m 2 It is preferable that the thickness is 50 g / m 2 ~170g / m 2 More preferably, it is 100 g / m 2 ~1500g / m 2 It is even more preferable that: When the thickness is within the above range, it becomes easy to obtain an interleaf paper that is excellent in all of strength, formability, and water absorption resistance of the end faces after pressure forming.

[0033] The basis weight of the entire base paper in the interleaving paper is 560g / m 2 ~1800g / m 2 and preferably 700 g / m 2 ~1600g / m 2 More preferably, it is 950 g / m 2 ~1400g / m 2 It is more preferable that the basis weight of the entire base paper in the interleaf is the total basis weight of at least two base papers, and does not include the weight of the adhesive layer between the at least two base papers. When the interleaf contains a resin layer such as a thermoplastic resin on the front or back surface, the thermoplastic resin layer is preferably 100% or more. The weight of the resin layer is not included. When the thickness is within the above range, it becomes easy to obtain an interleaf paper that is excellent in all of strength, formability, and water absorption resistance of the end faces after pressure forming.

[0034] The density of the slip sheet is not particularly limited, but is usually 0.50 g / cm 3 ~1.20g / cm 3 and preferably 0.70 g / cm 3 ~1.00g / cm 3 It is.

[0035] As described above, the raw material pulp contained in the base paper is preferably wood pulp, and more preferably kraft pulp. As kraft pulp, depending on the difference in raw materials, hardwood kraft pulp (LKP) and softwood kraft pulp (NKP) can be mentioned. In addition, depending on the difference in processing state, bleached kraft pulp (BKP), unbleached kraft pulp (UKP) and oxygen bleached kraft pulp (OKP) can be mentioned, and from the viewpoint of printability, bleached kraft pulp (BKP) is preferred.

[0036] Among these, the raw material pulp is preferably hardwood kraft pulp (LKP) or softwood kraft pulp (NKP), and more preferably, only hardwood kraft pulp (LKP) is used, or hardwood kraft pulp (LKP) and softwood kraft pulp (NKP) are used in combination. The mass ratio (LKP / NKP) when hardwood kraft pulp (LKP) and softwood kraft pulp (NKP) are used in combination is not particularly limited as long as it is a ratio used in general paper, but is preferably 1 / 99 to 99 / 1, more preferably 30 / 70 to 98 / 2, even more preferably 50 / 50 to 97 / 3, even more preferably 70 / 30 to 95 / 5, and even more preferably 80 / 20 to 92 / 8.

[0037] Moreover, as the hardwood kraft pulp (LKP), hardwood bleached kraft pulp (LBKP) is preferable, and as the softwood kraft pulp (NKP), softwood bleached kraft pulp (NBKP) is preferable.

[0038] For hardwood kraft pulp (LKP), wood chips of known hardwoods such as eucalyptus, tanoak, acacia, etc. can be used, while for softwood kraft pulp (NKP), wood chips of known softwoods such as larch, spruce, cedar, slash pine, lodgepole pine, etc. can be used.

[0039] In the papermaking process of the base paper, it is preferable to kraft cook the wood chips. The range of courseness can be easily adjusted by adjusting the temperature and time of kraft cooking. There are no particular restrictions on the cooking white liquor used in kraft cooking, and any known white liquor can be used.

[0040] The Canadian Standard Freeness (CSF) of the pulp is not particularly limited, but is preferably 350 to 700 ml, and more preferably 500 to 600 ml. The CSF is the freeness value measured using a Canadian standard freeness tester in accordance with JIS-P8121 after disintegrating a sample using a standard disintegrator in accordance with JIS-P8220.

[0041] When preparing the base paper, internal additives may be added, such as sizing agents, fillers, paper strength agents, retention aids, pH adjusters, drainage improvers, water resistance agents, softeners, antistatic agents, defoamers, slime control agents, dyes and pigments, etc.

[0042] The base paper preferably contains an internal sizing agent, which makes it easier to improve the water absorption resistance of the end face after pressure molding. Examples of sizing agents include rosin-based, alkyl ketene dimer (AKD)-based, alkenyl succinic anhydride (ASA)-based, styrene-acrylic, higher fatty acid-based, and petroleum resin-based sizing agents. From the viewpoint of further improving the water absorption resistance of the end surface after pressure molding, rosin-based sizing agents are used. A syrup is preferred.

[0043] The content of the internal sizing agent is preferably 0.10% by mass or more, more preferably 0.20% by mass or more, and even more preferably 0.30% by mass or more, based on the total mass of the base paper. The upper limit of the content of the internal sizing agent is not particularly limited, but is usually 2.00% by mass or less. By ensuring that the thickness is within the above range, it becomes easier to improve the water absorption resistance of the end face after pressure molding.

[0044] In preparing the base paper, the internal sizing agent is preferably added in an amount of 0.05 to 0.70 parts, more preferably 0.10 to 0.60 parts, and even more preferably 0.20 to 0.45 parts, per 100 parts of the pulp slurry (converted into solid content). By ensuring that the content is within the above range, water resistance can be improved.

[0045] In making the base paper, a known wet paper machine can be appropriately selected and used, such as a Fourdrinier paper machine, a gap former type paper machine, a cylinder paper machine, or a short wire paper machine. In the case of making base paper, for example, a method is mentioned in which a paper stock is cast onto a wire or the like, dehydrated to obtain a wet paper, and if necessary, a plurality of wet papers are stacked, and this single-layer or multi-layer wet paper is pressed and dried. In this case, if a plurality of wet papers are not stacked, a single-layer paper is obtained, and if a plurality of wet papers are stacked, a multi-layer paper is obtained. The paper layer formed by the paper machine is preferably conveyed, for example, on a felt and dried in a dryer. A multi-stage cylinder dryer may be used as a pre-dryer before drying in the dryer.

[0046] The base paper obtained as described above may be surface-treated with a calendar to make the thickness and profile uniform. For the calendar treatment, a known calendaring machine can be appropriately selected and used.

[0047] The Oken smoothness (JIS P 8155:2010) of the base paper is not particularly limited, but is preferably 5 seconds or more, more preferably 10 to 1000 seconds. The 75° gloss of the base paper is also not particularly limited, but is preferably 5% or more, more preferably 10 to 70%.

[0048] <Adhesive layer> The interleaving paper includes an adhesive layer between at least two base papers. That is, the base papers are laminated via the adhesive layer. The adhesive layer may be a layer made of a material having adhesive properties. The adhesive layer is preferably a resin-based adhesive suitable for dry lamination and wet lamination. An adhesive suitable for wet lamination is more preferable.

[0049] The adhesive layer may be formed by laminating the base paper and the base paper together using an adhesive. The adhesive is not particularly limited, but water-based, solvent-based, UV-based, and other types of adhesives can be used, and among these, water-based adhesives are preferred. That is, the adhesive layer is preferably a water-based adhesive layer formed from a water-based adhesive. Among the water-based adhesives, at least one selected from the group consisting of vinyl acetate adhesives, acrylic adhesives, polyurethane adhesives, and isocyanate adhesives is preferred, and vinyl acetate adhesives are more preferred from the viewpoints of workability and adhesive strength in the base paper bonding process.

[0050] When an adhesive is used, the amount of adhesive layer per unit area (e.g., coating amount after drying) is 1 to 50 g / m 2 and more preferably 5 to 30 g / m 2 It is preferable to coat the base paper so that the solid content is within this range.

[0051] For coating, it is preferable to use a coating liquid containing an adhesive, and it is more preferable to use a mixed coating liquid in which a curing agent is mixed into a coating liquid containing an adhesive. For example, the adhesive layer is preferably a cured product of a water-based adhesive.

[0052] The adhesive layer may be a layer containing a thermoplastic resin. By using a thermoplastic resin, it is possible to easily obtain an interleaving paper as a laminate by coating the base paper with the resin that has been heated and melted, and then laminating another base paper. The thermoplastic resin is not particularly limited and may be appropriately selected from known thermoplastic resins.

[0053] Specific examples of thermoplastic resins include polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polylactic acid, and polybutylene succinate; polyolefin-based resins such as polyvinyl chloride, polyvinylidene chloride, polybutene, polybutadiene, ethylene-vinyl acetate copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, and polymethylpentene; polycarbonate; polyurethane; polyamide; polyacrylonitrile; and poly(meth)acrylate.

[0054] Among these, polyolefins such as polyethylene, polypropylene, and ethylene-propylene copolymers, and polyesters such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polylactic acid, and polybutylene succinate are preferred, polyethylene, polypropylene, polyethylene terephthalate, polylactic acid, and polybutylene succinate are more preferred, polyethylene and polypropylene are even more preferred, and polypropylene is even more preferred. In addition to the above materials, biomass resins and biodegradable resins may be used as the resin. These resins may be used alone or in combination of two or more.

[0055] The thermoplastic resin may be one that can be laminated to the sheet substrate as the laminating layer. Among the thermoplastic resins, polypropylene is preferred from the viewpoints of water resistance and oil resistance.

[0056] The adhesive layer containing a thermoplastic resin may be produced by a method appropriately selected from known production methods, for example, a melt extrusion method, a melt casting method, a calendar method, and the like.

[0057] The adhesive layer may be formed as a single layer of a single resin, or may be formed as a single layer of a mixture of multiple resins, or may be formed as multiple layers made of the same or different types of resins. The thickness of the adhesive layer is not particularly limited, but from the viewpoint of moldability, it is preferably 5 to 100 μm, and more preferably 10 to 50 μm.

[0058] <Thermoplastic resin layer> From the viewpoint of improving waterproofness and stain resistance, the slip paper may have a thermoplastic resin layer on at least one surface. In addition, the slip paper may be provided with other resin layers, etc., to the extent that the above effects are not impaired. The slip paper may have a thermoplastic resin layer on one surface, or may have thermoplastic resin layers on both surfaces.

[0059] The thermoplastic resin used in the thermoplastic resin layer is not particularly limited, and may be appropriately selected from the known thermoplastic resins mentioned above as the thermoplastic resin for the adhesive layer. The thickness of the thermoplastic resin layer is preferably 1 to 200 μm, more preferably 5 to 100 μm, and further preferably 10 to 50 μm.

[0060] <Method of manufacturing interleaf paper> The method for producing the interleaf paper is not particularly limited, and any known method can be used. An example of the production method is shown below. First, base paper A and base paper B are prepared, an adhesive that will become the adhesive layer is coated on one side of base paper A, and base paper B is wet laminated onto this coated surface to obtain an interleaf paper. One or both sides of the obtained interleaf paper may be melt extrusion coated with the thermoplastic resin layer.

[0061] As described above, the interleaf paper includes at least two base papers (for example, base paper A and base paper B), but may include three or more base papers. When the interleaf paper includes three or more base papers, the adhesive layers that bond the base papers together may be different from each other or may be the same.

[0062] Furthermore, the obtained interleaf paper may be cut to an appropriate size taking into consideration the size and shape of the contained items, and suitability for transportation and display. The cutting is preferably performed by punching, from the viewpoint of efficiently obtaining interleaf paper of the same shape. The punching process is preferably carried out using a high-speed automatic punching machine, a flat-bed punching machine, or a rotary punching machine, and more preferably a high-speed automatic punching machine. With the high-speed automatic punching machine or the flat-bed punching machine, interleaf sheets having a rectangular shape, a rounded rectangular shape, an oval shape, etc. can be easily and efficiently obtained.

[0063] <Paper processed products> The use of the slip sheet is not particularly limited as long as it is for pressure molding, and it may be used as a paper processed product by pressure molding and further processing as appropriate. The slip sheet is preferably for a paper processed product. That is, the paper processed product is preferably a pressure molded product of the slip sheet. For example, it is preferable that at least a part of the end of the paper processed product is pressed and crushed in the thickness direction. This can suppress water absorption from the end face and improve water absorption resistance. Examples of paper products include clothing hanging devices such as paper hangers and paper hanger hooks, and paper tableware such as paper cups, paper trays, paper plates, paper spoons, paper forks, paper knives, paper stirrers, and paper straws. The pressure molding in the present invention includes known methods of molding by pressure, such as press molding, pressure molding, vacuum molding, and vacuum pressure molding. The molding may be performed using a molding die or may not require the use of a molding die.

[0064] By improving the feel of the slip paper, for example, a clothes hanger, which is a processed product of the slip paper, has an improved edge feel, and paper tableware, which is a processed product of the slip paper, has an improved tongue feel. Pressurization of the slip paper makes it easier to improve the feel to the hand and tongue.

[0065] (Paper tableware) It is preferable that at least a part of the edge of the paper tableware, which is a processed product of the interleaving paper, is pressed and crushed in the thickness direction, and it is more preferable that the entire edge is pressed and crushed in the thickness direction. For example, it is preferable that a part of the paper tableware 10 mm or less from the edge face is pressed and crushed in the thickness direction. By pressure molding only the edges of paper tableware while leaving the thickness of the center the same, it is possible to maintain strength while suppressing water absorption from the edges.

[0066] (Clothes Hanging Equipment) It is preferable that at least a part of the ends of the clothes hanging device, which is a processed product of the interleaving paper, is pressed and crushed in the thickness direction, and it is more preferable that the entire ends are pressed and crushed in the thickness direction. By pressure molding only the ends of the clothes hanger while leaving the thickness of the central portion unchanged, water absorption from the ends can be suppressed while maintaining strength.

[0067] The measurement methods for each physical property are described below. <Pulp coarseness, length-weighted average fiber length and average fiber width> The length-weighted average fiber length of the pulp contained in the base paper is measured in accordance with ISO 16065-2:2007, specifically as follows:

[0068] (Separation of base paper) The separation of each base paper from the interleaf paper is performed as follows. First, one side of the interleaf paper cut to a specified size (40 cm square) is dipped in an enzyme such as cellulase, and it is confirmed that the base paper on one side of the interleaf paper has completely dissolved. If the interleaf paper is formed of three base papers, two of them can be dissolved to obtain one base paper to be measured. The length-weighted average fiber length of the pulp is then measured using the obtained base paper. Note that a resin layer may be added to the base paper, and this does not result in any difference in the length-weighted average fiber length of the pulp contained in the base paper. Alternatively, the interleaf paper is immersed in hot water at 100°C, and the base paper portion is sampled with a spatula or the like, and the sample is used to measure the length-weighted average fiber length of the pulp.

[0069] (Measurement method) The base paper is cut into 40 cm squares, soaked in ion-exchanged water, adjusted to a solids concentration of 2% by mass, and soaked for 24 hours. After soaking for 24 hours, a standard disintegrator (manufactured by Kumagai Riki Kogyo Co., Ltd.) is used to disintegrate the pulp into fibers for 20 minutes. If undisintegrated pulp remains, disintegration is performed again for 20 minutes to disintegrate the pulp into fibers. If the base paper has a resin layer, the above disintegration is performed with the resin layer, and the slurry (dispersion of pulp fibers) is separated. If the resin layer can be removed, it is preferable to perform the disintegration with the resin layer removed. Disintegration is performed in accordance with JIS P8220-2:2012.

[0070] The obtained slurry was adjusted to a solids concentration of 0.1% by mass, and the pulp solids concentration was adjusted to JISP8. Calculate in accordance with 225:2003. This is a solids concentration of 0.004 mass%, 500g Adjust to a slurry and record the amount dispensed. Calculate the dry weight of the sample using the solids concentration and the amount of the slurry dispensed. Using the obtained fiber samples, the length-weighted average fiber length, fiber width, and weight coarseness are measured using a fiber length measuring instrument (Valmet FS-5 with UHD base unit, manufactured by Valmet Co., Ltd.) in accordance with ISO 16065-2:2007. The device can also detect and measure each fiber using an attached camera, and images are taken within a measurement cell (flow cell) with a depth of field of 0.5 mm in accordance with the ISO16505-2:2007 standard. The device captures fiber lengths between 0.01 mm and 10.00 mm. Fibers between 0.2 mm and 7.0 mm in length should be selected for the measurement of "fiber length" and "fiber width."

[0071] The above method can simultaneously measure the coarseness and fiber width. The coarseness is the gravimetric coarseness, which is the fiber roughness measured by applying the sum of fiber lengths obtained by image analysis and the dry weight of the sample input into the device. The average fiber width is the arithmetic mean value of the fiber widths of all the fibers obtained.

[0072] The pulp coarseness and length-weighted average fiber length in the entire interleaf paper shall be calculated based on all the coarseness and fiber lengths measured from the separated base papers.

[0073] <Basic weight> The basis weight of the base paper or interleaf paper is measured in accordance with JIS P 8124:2011. In addition to the base paper, the interleaf paper has an adhesive layer and may also have a resin layer. The basis weight of the base paper can be calculated by specifying the weight, material, thickness and density of the resin layer and adhesive layer according to the method and procedure described below. Specifically, the weight of the interleaf paper cut to a predetermined size and provided with the resin layer and adhesive layer is measured (total weight), and then the interleaf paper with the resin layer and adhesive layer is immersed in an enzyme such as cellulase to confirm that the base paper has been completely dissolved, and then the weight of only the resin layer (resin layer weight) is measured. In addition, the resin layer and paper layer are removed from the same size interleaf paper using a grinding device (manufactured by Sagawa Seisakusho Co., Ltd., grinding wheel dimensions φ50.8 × 12.7 mm) so that only the adhesive layer remains, and the weight of only the adhesive layer (adhesive layer weight) is measured. The weight of only the base paper is calculated by subtracting the resin layer weight and adhesive layer weight from the total weight, and the basis weight of the base paper is measured.

[0074] <Thickness> The thickness of the interleaf paper (paper thickness) is measured in accordance with JIS P 8118: 2014. A paper thickness meter (company name: Toyo Seiki Seisakusho Co., Ltd., model number: No. 132 digital thickness measuring instrument) can be used as the measuring device.

[0075] <density> The density of the base paper is calculated from the thickness and basis weight obtained by the above-mentioned measuring method.

[0076] <Content of internal sizing agent> (rosin) The sizing agent is quantified using a pyrolysis GC-FID (model GC2025, Shimadzu Corporation). After adding TMAH reagent for 5 minutes to a paper sample with all layers punched out, it is methylated and set in the sampler of a pyrolysis device (model: PY-2010SL, Frontier Labs, decomposition temperature 450°C) and measurement is performed using N2 as carrier gas and H2 / Air as reaction gas. The sizing agent content (mass% of pulp) is calculated from the sum of the peak areas of rosin and reinforced rosin in the obtained mass chromatogram based on the calibration curve of the standard product.

[0077] (AKD,ASA) Using a pyrolysis GC-MS (model GCMS-QP2010, manufactured by Shimadzu Corporation), size The amount of sizing agent is quantified. The paper sample with all layers punched out is placed in the sampler of a pyrolysis device (model: PY-3030D, manufactured by Frontier Labs, decomposition temperature 500°C) and measurement is performed. The sizing agent content (mass % of pulp) is calculated from the sum of the AKD or ASA peak areas in the obtained mass chromatogram based on the calibration curve of the standard product. EXAMPLES

[0078] The present invention will be specifically described below using examples, but the scope of the invention is not limited to the description of the examples. In addition, unless otherwise specified, "parts" refers to "parts by mass".

[0079] <Preparation of Pulps A to I> Using the wood chips listed in Table 1, cooking white liquor was prepared with a liquor ratio of 4, a sulfidity of 30%, and an effective alkali amount (as Na2O) such that the kappa number (measured in accordance with JIS P 8211:2011) was 20 for hardwood pulp and 30 for softwood pulp. The liquor ratio is the ratio of the mass of white liquor (sodium sulfide (Na2S) + caustic soda (NaOH)) to the mass of pulp. The sulfidity (%) is calculated by sodium sulfide concentration / (caustic soda concentration + sodium sulfide concentration) x 100.

[0080] The resulting cooking white liquor was added to wood chips in an autoclave, and then kraft cooking was carried out at a cooking temperature of 165°C for 2 hours.

[0081] After cooking, the black liquor was separated, and the resulting pulp was defibrated using a high-concentration disintegrator, then centrifugal dehydration and water washing were repeated three times. Next, undigested matter was removed using a screen, and centrifugal dehydration was performed to obtain cooked and unbleached hardwood or softwood pulp with a sterol ester compound content of 0.012% by mass based on the bone dry pulp mass.

[0082] The hardwood pulp was then bleached using a bleaching sequence of oxygen bleaching, chlorine dioxide bleaching, alkaline peroxide bleaching, and chlorine dioxide bleaching to obtain bleached pulp LBKP. Softwood pulp was bleached using the following bleaching sequence: oxygen bleaching, chlorine dioxide bleaching, alkaline peroxide bleaching, peroxide bleaching, and chlorine dioxide bleaching, to obtain bleached pulp NBKP.

[0083] Of the resulting bleached pulps, pulp G and pulp I were classified using a Bauer-McNett type classifier specified in TAPPI T233. The coarseness, length-weighted average fiber length, and average fiber width of the resulting pulp are shown in Table 1.

[0084] [Table 1]

[0085] <Preparation of base paper> The pulp shown in Table 2 was beaten to a CSF of 500 mL to obtain a pulp slurry. 0.50 parts by mass of an internal paper strength agent, 0.13 parts by mass of starch, an internal sizing agent, and aluminum sulfate were added to 100 parts of the obtained pulp slurry (solid content equivalent) in the amounts shown in Table 2 to prepare a paper stock. Using this paper stock, base papers of Examples 1 to 15 and Comparative Examples 1 to 6 were made on a six-layer short wire paper machine. The basis weight of each layer and the basis weight of the base paper were as shown in Table 2.

[0086] [Table 2]

[0087] <Making interleaving paper> (Examples 1 to 12, Comparative Examples 1 to 6) The front surface (first layer surface) of the base paper of Examples 1 to 12 and Comparative Examples 1 to 6 was melt-extrusion coated with polypropylene (Novatec PP FL02T, manufactured by Japan Polypropylene Corporation) to a film thickness of 20 μm to obtain two base papers with a laminated front surface. The back surface (sixth layer surface) of one of the two base papers with a laminated front surface was coated with the dried coating. The work weight is 15g / m 2 In order to achieve this, a vinyl acetate adhesive (Polysol AX-505ZH, The adhesive was applied to the surface using a reverse roll coater. The back side of the other base paper with the front side laminated was attached to the first base paper, and wet laminated to obtain a two-sheet laminate.

[0088] (Example 13) The front surface of the base paper of Example 13 was melt-extrusion coated with polypropylene (Novatec PP FL02T, manufactured by Japan Polypropylene Corporation) to a film thickness of 20 μm, to obtain two base papers with a laminated front surface. Of the two base papers with a laminated front surface, the back surface of one of the two base papers was coated with a coating amount of 15 g / m2 after drying. 2A vinyl acetate adhesive (Polysol AX-505ZH, Showa Denko K.K.) was applied using a reverse roll coater so that the thickness of the adhesive layer was 100 μm. The front surface of the unlaminated base paper of Example 13 was attached to the adhesive-coated surface and wet laminated. Furthermore, a 15 g / m2 coating was applied to the back surface of the laminated base paper. 2 In order to achieve this, a vinyl acetate adhesive (Polysol AX-505ZH, Showa The adhesive was applied using a reverse roll coater (manufactured by Denko Co., Ltd.). The back side of another sheet of base paper with the front side laminated was attached to the adhesive-coated surface, and wet laminated to obtain a three-sheet interleaving paper.

[0089] Example 14 The front surface of the base paper of Example 14 was melt-extrusion coated with polypropylene (Novatec PP FL02T, manufactured by Japan Polypropylene Corporation) to a film thickness of 20 μm to obtain one sheet of base paper with a laminated front surface. The back surface of the base paper was coated with a coating amount of 15 g / m2 after drying. 2 A vinyl acetate adhesive (Polysol AX-505ZH, Showa Denko Co., Ltd.) was used. The adhesive was applied using a reverse roll coater. The back side of the unlaminated base paper of Example 14 was attached to the adhesive-coated surface, and wet laminated to obtain a two-sheet interleaving paper.

[0090] Example 15 The back side of the base paper of Example 15 was coated with 15 g / m2 of paint after drying. 2 A vinyl acetate adhesive (Polysol AX-505ZH, Showa Denko) was applied to the film using a reverse roll coater. The back side of the base paper of Example 15 was attached to the adhesive-coated surface and wet-laminated to obtain an interleaving paper of two base papers.

[0091] <Strength evaluation> The obtained slip sheets of Examples 1 to 15 and Comparative Examples 1 to 6 were evaluated for strength as follows. The slip sheets produced in the Examples and Comparative Examples were punched and press-molded to produce spoons of the following sizes. The resulting spoons were left to stand in an environment of 23°C and 50% Rh for 24 hours to adjust the temperature and humidity. Long side direction (CD): pot: 50mm, handle: 75mm, handle end: 30mm Short side direction (MD) (longest part): lid: 35mm, handle: 20mm, handle end: 35mm Height: Max. 10mm

[0092] A commercially available cup ice cream (vanilla, manufactured by Häagen-Dazs Japan) was taken out of a -18°C freezer, and while it was still ice-cold, a spoon was inserted 25 mm into the surface of the ice cream at a 45° angle, and then lifted vertically to scoop the ice cream. This was repeated until the spoon broke. The number of times the spoon was used to scoop ice cream before it broke was counted and rated according to the following criteria, with 2 or more being considered good and 1 being considered bad. The results are shown in Table 3. [Evaluation Criteria] It didn't break even after 3:25 scoops. 2:11 or more times, but less than 24 times, it broke. 1: It broke after scooping it more than once but less than 10 times.

[0093] <Evaluation of moldability> The obtained interleaf papers of Examples 1 to 15 and Comparative Examples 1 to 6 were evaluated for formability as follows. The slip sheets prepared in the Examples and Comparative Examples were cut into 150 mm (MD) x 40 mm (CD). The cut samples were left to stand in an environment of 23°C and 50% RH for 24 hours to adjust the temperature and humidity. 30 mm from one end of the obtained sample was fixed to a metal roll with a diameter of 80 mm using tape (75 mm wide packaging adhesive tape No. 3305, manufactured by Nitto Denko Corporation), and the sample was wrapped around the metal roll by manually rolling it on a table. The change in the sample when it was released from the wrapped state was visually confirmed. The number of wrinkles was counted within 10 cm of the sample in the MD direction and evaluated according to the following criteria. 2 or more was evaluated as good, and 1 or less was evaluated as bad. The results are shown in Table 3. [Evaluation Criteria] 4: After the test, only shallow wrinkles were observed on the inside of the sample where it was wrapped. The number of wrinkles of 1 cm or more was less than 0.6 wrinkles / cm. 3: After the test, wrinkles were formed on the inside of the wrapped sample. The number of wrinkles over 1 cm was 0.6 or more / cm but less than 1.9 / cm. 2: After the test, deep wrinkles were formed on the inside of the wrapped sample. The number of wrinkles over 1 cm was between 1.9 and 2.4 wrinkles / cm. 1: After the test, deep wrinkles were formed on the inside of the sample where it was wrapped, and folds were formed on the outside of the sample where it was wrapped. The number of wrinkles over 1 cm was 2.4 / cm or more.

[0094] <Evaluation of water absorption resistance of end surface after pressure molding> For the obtained interleaf papers of Examples 1 to 15 and Comparative Examples 1 to 6, the end faces after pressure molding were evaluated for water absorption resistance as follows. The slip papers prepared in the Examples and Comparative Examples were cut into 297 mm (MD) x 105 mm (CD). The cut samples were left to stand in an environment of 23°C and 50% Rh for 24 hours to adjust the temperature and humidity. The obtained samples were pressed four times in total, twice on each side, using a super calendar (made by Marukyo Giken, steel roll) at a linear pressure of 350 kN / m (room temperature). After pressing, the slip papers of Examples 14 and 15 had packaging adhesive tape (No. 3305, made by Nitto Denko Corporation) attached to the side without the resin layer for adhesion. The obtained samples were cut into 25 mm (MD) x 75 mm (CD) so that the edges were exposed, and the weights were measured. The cut samples were immersed in ion-exchanged water (23°C) for 10 minutes, after which the moisture on the surface was wiped off and the weights were measured. The amount of water absorbed on the edges was calculated using the following formula and evaluated according to the following criteria. 2 or more was evaluated as good, and 1 was evaluated as poor. The results are shown in Table 3. Amount of water absorbed at the end surface [g / m] = (weight of sample after water absorption - weight of sample before water absorption) [g] / length of sample end surface [m] [Evaluation Criteria] 4: Less than 0.14 [g / m] 3: 0.14[g / m] or more and less than 0.17[g / m] 2: 0.17[g / m] or more and less than 0.19[g / m] 1:0.19[g / m] or more

[0095] <Evaluation of texture> The obtained slip sheets of Examples 1 to 15 and Comparative Examples 1 to 6 were evaluated for feel as follows. The slip sheets prepared in the examples and comparative examples were cut into 100 mm (MD) x 10 mm (CD). The cut samples were left to stand for 24 hours in an environment of 23°C and 50% Rh to control the temperature and humidity. The edges (end faces) of the obtained samples were traced with the hand, and a sensory evaluation was performed on the texture from 1 to 4 points as follows. [Sensory evaluation score] 4 points: Very smooth to the touch. 3 points: Feels rather smooth to the touch. 2 points: Slightly rough to the touch. Score 1: Very rough to the touch. Sensory evaluation was carried out by 10 people, and the average score of the 10 people was calculated and rated according to the following criteria. A score of 2 or more was considered to be good, and a score of 1 was considered to be bad. The results are shown in Table 3. [Evaluation Criteria] 4:3.3 points or higher 3: 2.5 points or more and less than 3.3 points 2: 1.8 to less than 2.5 points 1: 1.0 to less than 1.8 points

[0096] [Table 3]

[0097] In Table 3, the base paper basis weight indicates the basis weight of only the base paper in the interleaf paper. [Explanation of symbols]

[0098] 1.2 Base paper 3 Adhesion layer 4 Thermoplastic resin layer 10 Paper folding

Claims

1. An interleaving paper for pressure molding, comprising at least two base papers and an adhesive layer between the at least two base papers, the coarseness of the pulp contained in each of two or more sheets of the base paper is 0.03 mg / m to 0.15 mg / m; The pulp has a length-weighted average fiber length of 0.60 mm to 1.50 mm; The thickness of the slip paper is 0.68 mm to 2.10 mm.

2. The interleaf paper according to claim 1 , wherein the interleaf paper has a thermoplastic resin layer on at least one surface.

3. 2. The interleaf paper according to claim 1, wherein the pulp has a coarseness of 0.04 mg / m to 0.08 mg / m.

4. 2. The interleaf paper according to claim 1, wherein the base paper contains an internal sizing agent, and the content of the internal sizing agent is 0.2% by mass or more based on the total mass of the base paper.

5. 2. The interleaving paper according to claim 1, wherein the base paper contains an internal sizing agent, and the internal sizing agent is a rosin-based sizing agent.

6. The basis weight of the entire base paper in the interleaving paper is 560 g / m 2 ~1800g / m 2 The interleaf paper according to claim 1 ,

7. The interleaf paper has a thermoplastic resin layer on at least one surface, the base paper contains an internal sizing agent, the internal sizing agent is a rosin-based sizing agent, and the content of the internal sizing agent is 0.2% by mass or more based on the total mass of the base paper; The basis weight of the entire base paper in the interleaving paper is 560 g / m 2 ~1800g / m 2 The interleaf paper according to claim 1 ,

8. A paper tableware product which is a processed product of the interleaf paper according to any one of claims 1 to 7.

9. The paper tableware according to claim 8, At least a part of the edge of the paper tableware is pressed and crushed in the thickness direction.

10. A clothes hanging tool which is a processed product of the interleaf paper according to any one of claims 1 to 7.

11. The clothes hanging device according to claim 10, At least a part of the end of the clothes hanging tool is compressed by pressure in the thickness direction.

Citation Information

Patent Citations

  • Cellulose pulp with improved latent softness and method for making such pulp

    JP1996511837A

  • Manufacturing method for paper vessel, and paper vessel

    JP2001260254A

  • Base paper for molded container, and paper-made molded container

    JP2007314246A

  • Method for forming rim and end section seal for heat insulation cup

    JP2008162700A

  • Laminated paper, base material for laminated paper, paper container and production method of laminated paper

    JP2020116937A