Method for producing carbon dioxide adsorbent

By impregnating potassium carbonate on α-alumina and drying at controlled temperatures, the method enhances carbon dioxide adsorption capacity in carbon dioxide adsorbents.

JP2024141248AActive Publication Date: 2024-10-10JGC CATALYSTS & CHEMICALS LTD

Patent Information

Application Number
JP2023052781
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Carbon dioxide adsorbents with a basic compound supported on a carrier have a low carbon dioxide adsorption capacity.

Method used

A method involving impregnating potassium carbonate on a carrier made of α-alumina, followed by drying at specific temperatures to create a carbon dioxide adsorbent with enhanced adsorption capacity.

Benefits of technology

The method results in a carbon dioxide adsorbent that can adsorb a large amount of carbon dioxide, utilizing α-alumina's stability and controlled drying to optimize adsorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141248000001
    Figure 2024141248000001
Patent Text Reader

Abstract

To solve a problem that the amount of carbon dioxide adsorbed by an adsorbent carrying a basic compound is small.SOLUTION: A method for producing a carbon dioxide adsorbent comprises the following steps (1) to (4): (1) an impregnation liquid preparation step of dissolving potassium carbonate in water to prepare a potassium carbonate impregnation liquid; (2) a carrier preparation step of preparing a carrier comprising α-alumina; (3) an impregnation step of impregnating the carrier comprising α-alumina with potassium carbonate using the potassium carbonate impregnation liquid to prepare a carbon dioxide adsorbent precursor; and (4) a drying step of drying the adsorbent precursor at a temperature of 50°C or higher and lower than 90°C to prepare a carbon dioxide adsorbent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a carbon dioxide adsorbent. [Background technology]

[0002] One of the causes of global warming is the emission of greenhouse gases. Greenhouse gases include carbon dioxide (CO2), methane (CH4), and fluorocarbons (CFCs, etc.). Carbon dioxide, a representative greenhouse gas, is particularly emitted in large quantities from power plants, steelworks, and oil refineries, so there is growing interest in technologies to reduce carbon dioxide emissions. Meanwhile, apart from technologies to reduce carbon dioxide emissions, there is also interest in technologies to capture and store carbon dioxide (Carbon dioxide Capture and Storage: "CCS").

[0003] In order to store carbon dioxide, it is first necessary to separate the carbon dioxide from a medium (for example, exhaust gas, the atmosphere, etc.). Known methods for separating carbon dioxide include a chemical absorption method in which carbon dioxide is absorbed in an alkaline solution or an amine solution (for example, Patent Document 1), and a physical adsorption method in which carbon dioxide is adsorbed onto an adsorbent and separated (for example, Patent Document 2). Also known is a method in which carbon dioxide is adsorbed onto an adsorbent carrying a basic compound and separated (for example, Patent Documents 3 and 4). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. WO2023 / 013397 [Patent Document 2] JP 2001-347123 A [Patent Document 3] Special Publication No. 2017-524519 [Patent Document 4] JP 2005-40753 A Summary of the Invention [Problem to be solved by the invention]

[0005] A carbon dioxide adsorbent having a basic compound supported on a carrier has a problem in that the amount of carbon dioxide adsorbed is small.

[0006] Therefore, an object of the present invention is to provide a production method for a carbon dioxide adsorbent having a basic compound supported on a carrier, which can obtain a carbon dioxide adsorbent that can adsorb a large amount of carbon dioxide. [Means for solving the problem]

[0007] The present inventors have found that the above problems can be solved by using a method for producing a carbon dioxide adsorbent comprising the following steps (1) to (4). (1) A process for preparing an impregnation solution by dissolving potassium carbonate in water to prepare a potassium carbonate impregnation solution (2) A carrier preparation step for preparing a carrier containing α-alumina (3) an impregnation step of impregnating the α-alumina-containing carrier with potassium carbonate using the potassium carbonate impregnation solution to prepare a carbon dioxide adsorbent precursor; (4) A drying step of drying the adsorbent precursor at a temperature of 50° C. or higher but lower than 90° C. to prepare a carbon dioxide adsorbent. Effect of the Invention

[0008] According to the present invention, it is possible to provide a carbon dioxide adsorbent having a basic compound supported on a carrier, which is capable of adsorbing a large amount of carbon dioxide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention includes an invention related to a method for producing a carbon dioxide adsorbent (hereinafter, also referred to as "the production method of the present invention"). The production method of the present invention will be described in detail below.

[0010] [Production method of the present invention] The manufacturing method of the present invention comprises the following steps (1) to (4). (1) A process for preparing an impregnation solution by dissolving potassium carbonate in water to prepare a potassium carbonate impregnation solution (2) A carrier preparation step for preparing a carrier containing α-alumina (3) an impregnation step of impregnating the α-alumina-containing carrier with potassium carbonate using the potassium carbonate impregnation solution to prepare a carbon dioxide adsorbent precursor; (4) A drying step of drying the adsorbent precursor at a temperature of 50° C. or higher but lower than 90° C. to prepare a carbon dioxide adsorbent.

[0011] In conventional carbon dioxide adsorbents, adsorption of carbon dioxide occurs on the surface of the adsorbent, so a carrier with a high specific surface area is used. For example, Patent Document 3 describes that an alumina carrier having a γ, χ, or δ structure is preferred, and that the specific surface area is 200 to 350 m. 2 / g is even more preferable. Patent Document 4 also discloses that activated carbon, zeolite, diatomaceous earth, and alumina are used as the porous substance. In contrast, the manufacturing method of the present invention uses a carrier containing α-alumina. α-alumina is the most chemically stable alumina. On the other hand, since it is fired at high temperatures, its specific surface area is extremely small compared to γ-alumina and the like. In this way, a carbon dioxide adsorbent with a large amount of carbon dioxide adsorption can be obtained by impregnating and supporting potassium carbonate on a carrier containing α-alumina, which has characteristics unsuitable for carbon dioxide adsorption, and drying it in a specific temperature range. Each step of the manufacturing method of the present invention will be described in detail below.

[0012] [Impregnation liquid preparation process] The manufacturing method of the present invention includes an impregnation solution preparation step in which potassium carbonate is dissolved in water to prepare a potassium carbonate impregnation solution. The amount of potassium carbonate dissolved in water in this step is preferably 50 g or more and 200 g or less, more preferably 50 g or more and 100 g or less, by mass relative to 100 g of water. In this step, it is preferable that the entire amount of potassium carbonate is dissolved in water, but the effect of the present invention can be obtained even if the potassium carbonate is not completely dissolved in the water and a part of it remains as a solid. If the potassium carbonate is not completely dissolved in the water, it is recommended to increase the temperature of the water to increase the solubility of potassium carbonate.

[0013] [Carrier preparation process] The manufacturing method of the present invention includes a carrier preparation step of preparing a carrier containing α-alumina. In this step, a commercially available α-alumina molded body may be used, or a molded body made by molding α-alumina powder may be used as the carrier, or a molded body of transition alumina having a structure such as γ, χ, δ, etc. may be fired at a high temperature of 1000° C. or higher to form α-alumina.

[0014] In this process, the specific surface area of ​​the support containing α-alumina is increased to 1 m 2 / g or more, 10m 2 / g or less, and 2 / g or more, 8m 2 In this way, by using a carrier having a small specific surface area, potassium carbonate segregates on the surface of the carrier, not in the pores of the carrier, and thus the carbon dioxide contained in a fluid having low diffusivity, such as a liquid, and the potassium carbonate are more likely to come into contact with each other.

[0015] In this step, the sodium content of the carrier containing α-alumina is preferably 0.3 mass% or more and 5 mass% or less, more preferably 0.4 mass% or more and 3 mass% or less, and particularly preferably 0.5 mass% or more and 1 mass% or less, calculated as Na2O based on the total mass of the carrier. The sodium content relative to the specific surface area of ​​the carrier is 0.01 g / m2 calculated as Na2O. 2 More than 50g / m 2 It is preferable that the content is 0.1 g / m or less. 2 More than 30g / m 2 More preferably, it is 0.5 g / m or less. 2 More than 10g / m 2 By adjusting the sodium content per unit specific surface area to fall within the above range, the amount of carbon dioxide adsorption is further increased.

[0016] In this step, the carrier containing α-alumina is preferably a molded body having a spherical, columnar (including cylindrical and four-lobe) shape or a shape similar thereto, and more preferably a spherical shape. The size (the minimum length of the outer shape of the adsorbent) is preferably in the range of 0.5 mm to 6 mm, more preferably in the range of 1 mm to 5 mm, and particularly preferably in the range of 3 mm to 5 mm. A carbon dioxide adsorbent obtained using a carrier molded to such a size has a low pressure loss when passing a fluid containing carbon dioxide through it, and is preferable from the viewpoint of process design.

[0017] [Impregnation process] The production method of the present invention includes an impregnation step of preparing a carbon dioxide adsorbent precursor by impregnating the α-alumina-containing carrier prepared in the above step with potassium carbonate using the potassium carbonate impregnation solution prepared in the above step. In this step, impregnation can be performed by a conventionally known method such as an equilibrium adsorption method, a pore filling method, or a spraying method.

[0018] [Drying process] The manufacturing method of the present invention includes a drying step in which the carbon dioxide adsorbent precursor obtained in the above step is dried at a temperature of 50° C. or more and less than 90° C. to prepare a carbon dioxide adsorbent. In this step, the drying temperature is particularly important. In this step, drying is preferably performed at a temperature of 60° C. or more and 80° C. or less. By adjusting the drying temperature to within the above range, the amount of carbon dioxide adsorbed is increased.

[0019] In this step, the carbon dioxide adsorbent precursor can be dried by a conventionally known method. For example, drying can be performed by a drying method such as reduced pressure drying or normal pressure drying. In this step, drying is preferably performed using normal pressure drying. In addition, when performing normal pressure drying, drying is preferably performed with air circulating. In this step, it is sufficient to dry the carbon dioxide adsorbent precursor to such an extent that the solvent cannot be visually observed on the surface of the carbon dioxide adsorbent precursor. The drying time is preferably adjusted to a range of 1 hour or more and 24 hours or less.

[0020] The production method of the present invention preferably does not include a calcination step. Specifically, it is preferable not to heat at a temperature above 90° C. in an oxygen-containing atmosphere. In this way, by not including a calcination step, the production method of the present invention can increase the carbon dioxide adsorption amount of the carbon dioxide adsorbent.

[0021] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0022] [Example 1] <Impregnation solution preparation process> A potassium carbonate impregnation solution was prepared by dissolving 70 g of potassium carbonate in 140 g of ion-exchanged water.

[0023] <Carrier preparation process> A carrier containing α-alumina was prepared by calcining commercially available γ-alumina (manufactured by YINGHE CHEMICAL CO., LTD., product name 3A-SC, 4 mmφ spherical) at 1200° C. for 4 hours. The specific surface area and sodium content of the obtained carrier were measured by the following method.

[0024] [Specific surface area measurement] The specific surface area of ​​the support was calculated by the nitrogen adsorption method (BET method). Specifically, using a specific surface area measuring device (Macsorb1220, manufactured by Mountech), about 0.1 g of the support was placed in a measurement cell, and degassed for 40 minutes at 250°C in a nitrogen gas flow, after which the support was kept at liquid nitrogen temperature in a mixed gas flow of 30% by volume of nitrogen and 70% by volume of helium, and nitrogen was adsorbed on the support in equilibrium. Then, the temperature of the support was gradually raised to room temperature while passing this mixed gas, and the amount of nitrogen desorbed during that time was measured, and the specific surface area of ​​the support was calculated by dividing the amount by the mass of the support after measurement.

[0025] [Sodium content and sodium content per unit surface area] The carrier was dissolved in acid and diluted with water to an appropriate concentration, and then the sodium content was measured using an ICP optical emission spectrometer (Agilent Technologies, 730ICP-OES, inductively coupled plasma optical emission spectrometry). Using this sodium content, the sodium content was calculated in terms of Na2O, based on the total amount of the carrier. The sodium content was also divided by the specific surface area to calculate the sodium content per unit surface area.

[0026] <Impregnation process> 100 g of the carrier containing α-alumina obtained in the above step was immersed in 210 g of the potassium carbonate impregnation solution prepared in the above step and held for 30 minutes.

[0027] <Drying process> The water contained in the potassium carbonate impregnated solution was evaporated using a rotary evaporator set at 80°C to obtain a carbon dioxide adsorbent in which potassium carbonate was supported on a carrier containing α-alumina. The carbon dioxide adsorption amount of the obtained carbon dioxide adsorbent was measured using the following evaluation method. The results are shown in Table 1 together with the preparation conditions.

[0028] [Evaluation of carbon dioxide adsorption amount] <Blank measurement> The reaction tube filled with 10 cc of carbon dioxide adsorbent was attached to a flow-type adsorption test apparatus. Nitrogen was then passed through the reaction tube, and pretreatment was carried out at 170°C for 2 hours. After the pretreatment was completed, the carbon dioxide adsorbent was removed from the reaction tube, and the amount of carbon (C blank ) was analyzed.

[0029] <Carbon dioxide adsorption test> A reaction tube filled with 10 cc of carbon dioxide adsorbent was attached to a flow-type adsorption test apparatus. Nitrogen was then passed through the reaction tube, and pretreatment was carried out at 170°C for 2 hours, after which the reaction tube was cooled to 50°C. A mixed gas containing carbon dioxide (carbon dioxide concentration 7.6 vol% / nitrogen balance) was then passed through the reaction tube at a supply rate of 20 cc / min for 2 hours. After the mixed gas had been passed through, the carbon dioxide adsorbent was removed, and the amount of carbon (C) contained in the carbon dioxide adsorbent was measured using a solid carbon / sulfur analyzer (HORIBA, model EMIA-Pro). ads ) was analyzed.

[0030] <Calculation of carbon dioxide adsorption amount> Using the results of the blank measurement and the carbon dioxide adsorption test described above, the amount of carbon dioxide adsorption was calculated in terms of carbon according to the following formula. Carbon dioxide adsorption amount [gC / g-adsorbent] = C ads - C blank

[0031] [Example 2] A carbon dioxide adsorbent was obtained in the same manner as in Example 1, except that the amount of potassium carbonate added in the impregnation solution preparation step was changed from 70 g to 140 g, and that an electric dryer was used instead of a rotary evaporator in the drying step, and the drying temperature was changed from 80° C. to 60° C. The carbon dioxide adsorbent thus obtained was measured for its carbon dioxide adsorption amount in the same manner as in Example 1. The results are shown in Table 1 together with the preparation conditions.

[0032] [Example 3] A carbon dioxide adsorbent was obtained in the same manner as in Example 2, except that the drying temperature in the drying step was changed from 60° C. to 80° C. For the obtained carbon dioxide adsorbent, the carbon dioxide adsorption amount was measured in the same manner as in Example 2. The results are shown in Table 1 together with the preparation conditions.

[0033] [Comparative Example 1] A carbon dioxide adsorbent was obtained in the same manner as in Example 2, except that the drying temperature in the drying step was changed from 80°C to 120°C. For the obtained carbon dioxide adsorbent, the carbon dioxide adsorption amount was measured in the same manner as in Example 2. The results are shown in Table 1 together with the preparation conditions. An α-alumina carrier was impregnated with an aqueous potassium carbonate solution in the same manner as in Example 2.

[0034] [Comparative Example 2] A carbon dioxide adsorbent was obtained in the same manner as in Example 1, except that an electric dryer was used instead of a rotary evaporator in the drying step, and the drying temperature was changed from 80° C. to 120° C. The carbon dioxide adsorption amount of the obtained carbon dioxide adsorbent was measured in the same manner as in Example 1. The results are shown in Table 1 together with the preparation conditions.

[0035] [Comparative Example 3] A carbon dioxide adsorbent was obtained in the same manner as in Example 1, except that the amount of potassium carbonate added in the impregnation solution preparation step was changed from 70 g to 140 g, and the drying temperature in the drying step was changed from 80° C. to 95° C. The carbon dioxide adsorption amount of the obtained carbon dioxide adsorbent was measured in the same manner as in Example 1. The results are shown in Table 1 together with the preparation conditions.

[0036] [Table 1]

Claims

1. A method for producing a carbon dioxide adsorbent, comprising the following steps (1) to (4). (1) A process for preparing an impregnation solution by dissolving potassium carbonate in water to prepare a potassium carbonate impregnation solution (2) A carrier preparation step for preparing a carrier containing α-alumina (3) an impregnation step of impregnating the α-alumina-containing carrier with potassium carbonate using the potassium carbonate impregnation solution to prepare a carbon dioxide adsorbent precursor; (4) A drying step of drying the adsorbent precursor at a temperature of 50° C. or higher but lower than 90° C. to prepare a carbon dioxide adsorbent.

2. The specific surface area of ​​the carrier containing α-alumina is 1 m 2 / g or more, 10m 2 The method for producing the carbon dioxide adsorbent according to claim 1, wherein the adsorbent has a molecular weight of 1:1 or less.

3. The sodium content of the carrier containing α-alumina is, based on the total mass of the carrier, Na 2 3. The method for producing a carbon dioxide adsorbent according to claim 1, wherein the concentration of the carbon dioxide adsorbent is in the range of 0.3% by mass or more and 5% by mass or less in terms of O.

Citation Information

Patent Citations

  • Carbon dioxide adsorbent

    JP1993049918A

  • Gaseous carbon dioxide adsorbent, gaseous carbon dioxide adsorptive body, removal of gaseous carbon dioxide and device therefor

    JP1999244652A

  • Purification of gases using solid adsorbents

    US5614000A

  • Base treated alumina in pressure swing adsorption

    US5656064A

  • Adsorptive separation method for carbon dioxide

    JP2001347123A

Cited By

  • Carbon dioxide capture methods

    JP2026150220A