Piezoelectric laminate, method for manufacturing piezoelectric laminate, and piezoelectric element

A two-stage film formation process for KNN films addresses the issue of high film stress in piezoelectric materials, resulting in a laminate with enhanced piezoelectric constant and stress resistance, suitable for actuator applications.

JP2024141260APending Publication Date: 2024-10-10SUMITOMO CHEM CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023052800
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing KNN films used in piezoelectric materials face challenges with high piezoelectric constant and DC stress resistance but suffer from high film stress, leading to structural deformation and reduced manufacturing yield in piezoelectric elements.

Method used

A two-stage film formation process where a first KNN film is formed at a temperature ensuring a high (001) orientation rate and low film stress, followed by a second film at a higher temperature to enhance piezoelectric constant and DC stress resistance, resulting in a laminate with a piezoelectric film having a composition of potassium, sodium, and oxygen.

Benefits of technology

The laminate achieves a high piezoelectric constant, low film stress, and improved DC and AC stress resistance, enabling reliable operation of piezoelectric elements and modules, particularly in actuator applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141260000001_ABST
    Figure 2024141260000001_ABST
Patent Text Reader

Abstract

To provide a piezoelectric laminate that includes a piezoelectric film that has a high piezoelectric constant, a high DC stress resistance, a small film stress, and contains potassium, sodium, niobium, and oxygen.SOLUTION: A piezoelectric laminate includes a substrate, a lower electrode film deposited on the substrate, and a piezoelectric film deposited on the lower electrode film and composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, and the piezoelectric film has a piezoelectric constant e31 of 10 C / m2 or more, and when a negative voltage is applied to an upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film provided on the piezoelectric film at a temperature of 200°C, a time from a start of application of the negative voltage until a leakage current density flowing through the piezoelectric film exceeds 30 mA / cm2 is 5 hours or more, and a film stress of the piezoelectric film is 150 MPa or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a piezoelectric laminate, a method for manufacturing a piezoelectric laminate, and a piezoelectric element. [Background technology]

[0002] Piezoelectrics are widely used in functional electronic components such as sensors and actuators. KNN-based ferroelectrics containing potassium, sodium, niobium, and oxygen are used as one of the materials for piezoelectrics, and a laminate having a piezoelectric film (KNN film) formed using such a piezoelectric has been proposed. The KNN film is required to have a high piezoelectric constant and to be resistant to dielectric breakdown even when a large negative voltage is applied to the KNN film for a long period of time (i.e., to have high DC stress resistance). Therefore, a technique for increasing the piezoelectric constant of the KNN film (see, for example, Patent Document 1) and a technique for increasing the DC stress resistance of the KNN film (see, for example, Patent Documents 2 and 3) have been proposed. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-295786 A [Patent Document 2] JP 2017-076730 A [Patent Document 3] JP 2018-207055 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, although the KNN film obtained by the above-mentioned technique has a high piezoelectric constant or high DC stress resistance, it has a large film stress.

[0005] An object of the present disclosure is to provide a piezoelectric laminate having a piezoelectric film containing potassium, sodium, niobium, and oxygen, which has a high piezoelectric constant, a high DC stress resistance, and a small film stress. [Means for solving the problem]

[0006] According to one aspect of the present disclosure, A substrate; A lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; The piezoelectric constant e of the piezoelectric film 31 is 10C / m 2 That's all. When a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film provided on the piezoelectric film at a temperature of 200° C., the leakage current density flowing through the piezoelectric film from the start of application of the negative voltage is 30 mA / cm 2 The time it takes to exceed this limit is 5 hours or more, The membrane stress of the piezoelectric film is 150 MPa or less. A piezoelectric stack and a piezoelectric element are provided.

[0007] According to another aspect of the present disclosure, forming a lower electrode film on a substrate; forming a piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen on the lower electrode film; In the step of forming the piezoelectric film, first, a first piezoelectric film, which is a part of the piezoelectric film, is formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then a second piezoelectric film, which is the other part of the piezoelectric film, is formed at a first temperature at which the piezoelectric constant e 31 is 10C / m 2 or more, when a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film formed on the second piezoelectric film, the leakage current density flowing through the second piezoelectric film is 30 mA / cm 2 The present invention provides a method for producing a piezoelectric laminate, comprising forming the film at a second temperature at which the time until the temperature exceeds the threshold value is 5 hours or more. Effect of the Invention

[0008] According to the present disclosure, it is possible to provide a piezoelectric laminate having a piezoelectric film containing potassium, sodium, niobium, and oxygen, which has a high piezoelectric constant, a high DC stress resistance, and a small film stress. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a diagram showing an example of a cross-sectional structure of a piezoelectric laminate according to an embodiment of the present disclosure. [Diagram 2] 1A and 1B are diagrams illustrating an example of a structure of a simplified piezoelectric element according to an embodiment of the present disclosure. [Diagram 3] FIG. 1 is a diagram showing an example of a schematic configuration of a piezoelectric element according to an embodiment of the present disclosure. [Figure 4] 1 is a diagram illustrating an example of a schematic configuration of a piezoelectric device module according to an embodiment of the present disclosure. [Diagram 5] FIG. 1A is a diagram showing an example of a schematic configuration of a simple unimorph cantilever fabricated using each sample, and FIG. 1B is a diagram illustrating a method for measuring the piezoelectric constant. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] <Knowledge gained by the inventors> The present inventors have conducted intensive research with the aim of realizing a KNN film having both a high piezoelectric constant and high DC stress resistance. As a result, it has been found that when a KNN film is formed on a substrate such as a silicon (Si) substrate by sputtering, a KNN film having both a high piezoelectric constant and high DC stress resistance can be realized by forming the KNN film at a high temperature. However, when the KNN film is formed at a high temperature, the piezoelectric constant and DC stress resistance of the KNN film can be increased, but the film stress of the KNN film increases. Note that when the temperature during sputtering film formation is high, the film stress generated in the KNN film tends to be a tensile stress. If the film stress of the KNN film is large, for example, if the film stress of the KNN film exceeds 150 MPa, large structural deformation occurs when a piezoelectric element such as a membrane structure or a cantilever structure is produced. As a result, the produced piezoelectric element does not function normally. In addition, the manufacturing yield of the piezoelectric element and the piezoelectric device module decreases. For this reason, it is required to keep the film stress of the KNN film low, for example, to keep the film stress of the KNN film to 150 MPa or less.

[0011] The inventors of the present invention have conducted extensive research to develop a KNN film that simultaneously has three characteristics that have not been realized so far: high piezoelectric constant, high DC stress resistance, and low film stress. As a result, the following five findings were obtained. (First finding) The film stress of the KNN film obtained by sputtering depends greatly on the conditions at the initial stage of the KNN film formation. (Second finding) First (at the beginning of film formation), a KNN film is deposited as the first layer (initial layer) under temperature conditions that reduce the film stress, and then a KNN film is deposited on the first layer as the second layer under temperature conditions that increase the piezoelectric constant and DC stress resistance. This significantly reduces the film stress of the entire KNN film (the laminate of the first and second layers) even when the KNN film (second layer) is deposited at a high temperature that would normally generate large film stress. (Third Finding) In order to reproducibly obtain a KNN film having a high piezoelectric constant and DC stress resistance, it is necessary to increase the (001) orientation rate of the KNN film. In order to obtain a KNN film having a high (001) orientation rate, it is usually necessary to set the deposition temperature of the KNN film within a predetermined range. By depositing a KNN film as the first layer under temperature conditions that increase the (001) orientation rate at the beginning of deposition, and then depositing a KNN film as the second layer on the first layer under temperature conditions that increase the piezoelectric constant and DC stress resistance, a KNN film with a high (001) orientation rate can be obtained even if the KNN film (second layer) is deposited at a high temperature that would normally decrease the (001) orientation rate. The (001) orientation rate of the KNN film is the orientation rate of the crystals constituting the KNN film in the (001) plane direction, and will be described in detail later. (Fourth finding) In order to reproducibly obtain a KNN film with high piezoelectric constant and DC stress resistance, the (001) orientation rate of the KNN film must be 90% or more. By depositing a KNN film as the first layer under conditions that give a (001) orientation rate of 95% or more in the initial stage of deposition, a KNN film with a (001) orientation rate of 90% or more can be obtained even if a KNN film as the second layer is subsequently deposited at a high temperature. (Fifth finding) In the early stages of film formation, a KNN film is formed as the first layer under conditions that reduce the film stress and increase the (001) orientation rate. Then, a KNN film is formed on the first layer as the second layer under temperature conditions that increase the piezoelectric constant and DC stress resistance, thereby realizing a KNN film with a high piezoelectric constant and DC stress resistance.

[0012] Based on the above five findings, the inventors have found that a KNN film having a high piezoelectric constant and DC stress resistance and a film stress of 150 MPa or less can be obtained by depositing a KNN film as a first layer under temperature conditions at the beginning of film deposition such that the film stress is 100 MPa or less and the (001) orientation rate is 95% or more, and then depositing a KNN film as a second layer under temperature conditions such that the piezoelectric constant and DC stress resistance of the KNN film are high.

[0013] The present disclosure has been made based on the above-mentioned problems and findings obtained by the present inventors.

[0014] <One aspect of the present disclosure> Hereinafter, one embodiment of the present disclosure will be described with reference to the drawings.

[0015] (1) Structure of the piezoelectric laminate As shown in FIG. 1, a laminate (laminate substrate) 10 having a piezoelectric film according to this embodiment (hereinafter also referred to as piezoelectric laminate 10) comprises a substrate 1, a lower electrode film 2 deposited on the substrate 1, a piezoelectric film (piezoelectric thin film) 3 deposited on the lower electrode film 2, and an upper electrode film 4 deposited on the piezoelectric film 3.

[0016] The substrate 1 is a substrate having a surface oxide film (SiO 2 A single crystal silicon (Si) substrate 1a on which a surface oxide film 1b is formed, that is, a Si substrate having a surface oxide film, can be preferably used. 2 Alternatively, a Si substrate 1a having an insulating film formed of an insulating material other than SiO 2 can be used. Alternatively, a Si substrate 1a having an exposed Si(100) surface or Si(111) surface, i.e., a Si substrate having no surface oxide film 1b or insulating film, can be used. Alternatively, a silicon on insulator (SOI) substrate, quartz glass (SiO 2 The thickness of the single crystal Si substrate 1a can be, for example, from 300 μm to 1000 μm, and the thickness of the surface oxide film 1b can be, for example, from 1 nm to 4000 nm.

[0017] The lower electrode film 2 can be formed using, for example, platinum (Pt). The lower electrode film 2 is a polycrystalline film. Hereinafter, a polycrystalline film formed using Pt is also referred to as a Pt film. It is preferable that the (111) plane of the Pt film is parallel to the main surface of the substrate 1 (including the case where the (111) plane is inclined at an angle of ±5° or less with respect to the main surface of the substrate 1), that is, the Pt film is oriented in the (111) plane direction. The Pt film being oriented in the (111) plane direction means that no peaks other than those due to the (111) plane are observed in the X-ray diffraction pattern obtained by X-ray diffraction (XRD) measured on the surface of the piezoelectric film 3. Thus, it is preferable that the main surface of the lower electrode film 2 (the surface serving as the base of the piezoelectric film 3) is composed of a Pt (111) plane. The lower electrode film 2 can be formed by a method such as a sputtering method or a vapor deposition method. As the material of the lower electrode film 2, in addition to Pt, various metals such as gold (Au), ruthenium (Ru), iridium (Ir), alloys containing these as main components, strontium ruthenate (SrRuO 3 , abbreviation: SRO) or lanthanum nickel oxide (LaNiO 3 The lower electrode film 2 may be formed using a metal oxide such as SiO2 (abbreviated as LNO). When the lower electrode film 2 is formed using a metal oxide, the crystals constituting the lower electrode film 2 are preferably preferentially oriented in the (001) plane direction with respect to the surface of the substrate 1. The lower electrode film 2 may be a single layer film formed using the above-mentioned metals, an alloy mainly composed of the above-mentioned metals, or a metal oxide. The lower electrode film 2 may be a laminate of a Pt film and a film mainly composed of SRO provided on the Pt film, or a laminate of a Pt film and a film mainly composed of LNO provided on the Pt film. The thickness of the lower electrode film 2 (when the lower electrode film 2 is a laminate, the total thickness of each layer) may be, for example, 100 nm to 400 nm.

[0018] An adhesive layer 6 may be provided between the substrate 1 and the lower electrode film 2 to enhance their adhesion. The adhesive layer 6 may be, for example, a layer containing zinc (Zn) and oxygen (O) as main components (hereinafter also referred to as a "ZnO layer"). The ZnO layer may be formed using, for example, zinc oxide. The composition ratio of Zn and O constituting the ZnO layer preferably satisfies the relationship Zn:O=1:1, but is not limited thereto and may vary to some extent. The ZnO layer is a polycrystalline layer. The ZnO layer is preferably such that its (0001) plane is parallel to the main surface of the substrate 1 (including the case where the (0001) plane is inclined at an angle of ±5° or less with respect to the main surface of the substrate 1), that is, the ZnO layer is preferably oriented in the (0001) plane direction. The ZnO layer being oriented in the (0001) plane direction means that the intensity of the peak due to the (0002) plane is high in the X-ray diffraction pattern obtained by XRD measured on the surface of the piezoelectric film 3. Thus, the main surface of the ZnO layer (the surface serving as the base of the lower electrode film 2) is preferably composed of a ZnO (0001) plane. The ZnO layer can be formed by a method such as sputtering or vapor deposition. The thickness of the ZnO layer can be, for example, 1 nm or more and 200 nm or less, and preferably 10 nm or more and 50 nm or less. The adhesion layer 6 can be, for example, titanium (Ti), tantalum (Ta), titanium oxide (TiO 2 ), nickel (Ni), ruthenium oxide (RuO 2 ), iridium oxide (IrO 2 ) or the like may be provided as a main component. Such an adhesion layer 6 can also be formed by a technique such as a sputtering method or a vapor deposition method, and the thickness of the adhesion layer 6 can be, for example, 1 nm to 200 nm, preferably 10 nm to 50 nm. In this specification, the adhesion layer 6 provided between the substrate 1 and the lower electrode film 2 is sometimes referred to as a lower adhesion layer 6.

[0019] The piezoelectric film 3 is, for example, a film formed from an alkali niobate oxide containing potassium (K), sodium (Na), niobium (Nb), and oxygen (O). That is, the piezoelectric film 3 is a film mainly composed of an alkali niobate oxide containing K, Na, Nb, and O. The piezoelectric film 3 can be formed using an alkali niobate oxide represented by the composition formula (K 1-x Na x )NbO 3 , that is, potassium sodium niobate (KNN). The coefficient x [=Na / (K + Na)] in the above composition formula can be in the range of 0 < x < 1, preferably 0.4 ≦ x ≦ 0.8. The piezoelectric film 3 becomes a polycrystalline film of KNN (hereinafter also referred to as the KNN film 3). Also, the crystal structure of KNN is a perovskite structure. That is, the KNN film 3 has a perovskite structure. Further, it is preferable that more than half of the crystals constituting the KNN film 3 have a columnar structure. In this specification, the crystal system of KNN is regarded as a tetragonal system. The KNN film 3 can be formed by a sputtering method. The thickness of the KNN film 3 can be, for example, 0.5 μm or more and 5 μm or less, preferably 1 μm or more and 3 μm or less.

[0020] The crystals constituting the KNN film 3 are preferentially oriented in the (001) plane direction with respect to the main surface of the substrate 1 (when the substrate 1 is, for example, an Si substrate 1a having a surface oxide film 1b or an insulating film, etc., it is the Si substrate 1a). That is, the main surface of the KNN film 3 (the surface that becomes the base of the upper electrode film 4) is mainly composed of the KNN (001) plane. For example, by directly forming the KNN film 3 on a Pt film (lower electrode film 2) whose main surface is mainly composed of the Pt (111) plane, a KNN film 3 whose main surface is mainly composed of the KNN (001) plane can be obtained.

[0021] In this specification, the crystals constituting the KNN film 3 are oriented in the (001) plane direction means that the (001) plane of the crystals constituting the KNN film 3 is parallel or approximately parallel to the main surface of the substrate 1. In addition, the crystals constituting the KNN film 3 are preferentially oriented in the (001) plane direction means that there are many crystals whose (001) plane is parallel or approximately parallel to the main surface of the substrate 1. For example, it is preferable that 90% or more of the crystals constituting the KNN film 3 are oriented in the (001) plane direction with respect to the main surface of the substrate 1. That is, the orientation rate of the crystals constituting the KNN film 3 in the (001) plane direction (also referred to as the "(001) orientation rate" in this specification) is, for example, preferably 90% or more, more preferably 95% or more. In addition, the "(001) orientation rate" in this specification is a value calculated by the following formula (1) based on the peak intensity of the X-ray diffraction pattern (2θ / θ) obtained by performing XRD measurement on the KNN film 3.

[0022] (001) orientation rate (%) = {(001) peak intensity / ((001) peak intensity + (110) peak intensity)} × 100 (1)

[0023] In addition, the "(001) peak intensity" in the above formula (1) is the intensity of a diffraction peak due to a crystal oriented in the (001) plane direction (i.e., a crystal whose (001) plane is parallel to the main surface of the substrate 1) among the crystals constituting the KNN film 3 in the X-ray diffraction pattern obtained by performing XRD measurement on the KNN film 3, and is the intensity of a peak that appears within a 2θ range of 20° to 23°. In addition, when multiple peaks appear within a 2θ range of 20° to 23°, it is the intensity of the highest peak. In addition, the "(110) peak intensity" in the above formula (1) is the intensity of a diffraction peak due to a crystal oriented in the (110) plane direction (i.e., a crystal whose (110) plane is parallel to the main surface of the substrate 1) among the crystals constituting the KNN film 3 in the X-ray diffraction pattern obtained by performing XRD measurement on the KNN film 3, and is the intensity of a peak that appears within a 2θ range of 30° to 33°. When multiple peaks appear within the 2θ range of 30° to 33°, the intensity is that of the highest peak.

[0024] The alkali niobium oxide constituting the KNN film 3 may be selected from the group consisting of lithium (Li), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), bismuth (Bi), antimony (Sb), vanadium (V), indium (In), tantalum (Ta), molybdenum (Mo), tungsten (W), chromium (Cr), Ti, zirconium (Zr), hafnium (Hf), scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), At least one element (dopant) selected from the group consisting of samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), copper (Cu), zinc (Zn), silver (Ag), manganese (Mn), iron (Fe), cobalt (Co), Ni, aluminum (Al), Si, germanium (Ge), tin (Sn), and gallium (Ga) may further be contained. The concentration of these elements in the alkali niobium oxide can be, for example, 5 at% or less (when a plurality of the above elements are contained, the total concentration is 5 at% or less).

[0025] As will be described in detail later, in this embodiment, first, a first KNN film 3a (first piezoelectric film, hereinafter also referred to as "KNN film 3a"), which is a part of the KNN film 3, is deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then, a second KNN film 3b (second piezoelectric film, hereinafter also referred to as "KNN film 3b"), which is the other part of the KNN film 3, is deposited on the KNN film 3a at a second temperature at which the piezoelectric constant and DC stress resistance are high. As a result, the KNN film 3 in this embodiment (i.e., a laminate of the KNN film 3a and the KNN film 3b) simultaneously has all of the characteristics 1 to 3 described later. In addition, the KNN film 3 in this embodiment may further have the characteristic 4 described later.

[0026] Hereinafter, features 1 to 4 that the KNN film 3 of this embodiment can have will be described.

[0027] (Feature 1) The KNN film 3 has a piezoelectric constant e 31 is 10C / m 2 That is, the KNN film 3 is characterized by a high piezoelectric constant.

[0028] In this specification, the piezoelectric constant e 31 " is a value measured under conditions in which the lower electrode film 2 is grounded and a negative voltage (e.g., a triangular wave or sine wave voltage) is applied to the upper electrode film 4 so as to generate an electric field of 100 kV / cm between the lower electrode film 2 and the upper electrode film 4 (i.e., the KNN film 3).

[0029] The high piezoelectric constant of the KNN film 3 can improve the performance of the piezoelectric element 20 (piezoelectric device module 30) described below obtained by processing the piezoelectric laminate 10. As a result, the piezoelectric element 20 (piezoelectric device module 30) can be suitably used as an actuator.

[0030] This feature can be exhibited reproducibly (reliably) when the (001) orientation rate of the KNN film 3 (KNN film 3b) is 90% or more.

[0031] (Feature 2) The KNN film 3 has a leakage current density of 30 mA / cm from the start of voltage application when a highly accelerated life test (HALT) is performed in which a negative voltage is applied to the upper electrode film 4 (through the KNN film 3) (with the lower electrode film 2 grounded) so as to generate an electric field of 300 kV / cm between the lower electrode film 2 and the upper electrode film 4 (i.e., the KNN film 3) at a temperature of 200° C. (with the piezoelectric laminate 10 heated to a temperature of 200° C.) (hereinafter also referred to as “when HALT under specified conditions is performed at a temperature of 200° C.”). 2The time until the temperature exceeds the threshold value is 5 hours or more. In this way, the KNN film 3 has a long life against DC stress, that is, has a high DC stress resistance.

[0032] Since the KNN film 3 has high DC stress resistance, the KNN film 3 is less susceptible to dielectric breakdown (the time until the KNN film 3 undergoes dielectric breakdown becomes longer) even when a high voltage (electric field) is applied to the KNN film 3 via the upper electrode film 4 for a long period of time during operation of a piezoelectric element 20 (piezoelectric device module 30) (to be described later) obtained by processing the piezoelectric laminate 10 (hereinafter, also simply referred to as "during operation"). Note that in this embodiment, the leakage current density flowing through the KNN film 3 is 30 mA / cm 2 When this temperature was exceeded, it was determined that the KNN film 3 had reached dielectric breakdown.

[0033] This feature can be exhibited reproducibly (reliably) when the (001) orientation rate of the KNN film 3 (KNN film 3b) is 90% or more.

[0034] (Feature 3) The KNN film 3 further has a feature that the film stress is 150 MPa or less.

[0035] By making the film stress of the KNN film 3 150 MPa or less, it is possible to suppress large structural deformation when processing the piezoelectric stack 10 to fabricate a piezoelectric element 20 having a membrane structure, a cantilever structure, or the like, as described below. This allows the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric stack 10 to operate normally.

[0036] (Feature 4) The KNN film 3 may further have the characteristic that "when a negative AC voltage is continuously applied to the upper electrode film 4 (via the KNN film 3) so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film 2 and the upper electrode film 4 (i.e., the KNN film 3), the number of voltage application cycles until the piezoelectric displacement of the KNN film 3 decreases to 80% or less of its initial value exceeds 10 million."

[0037] For example, in the case of a piezoelectric laminate 10 having a KNN film 3 with a thickness of 2 μm, when the lower electrode film 2 is grounded and a unipolar triangular or sine wave (sine wave) AC voltage with an amplitude in the range of 0 V to -60 V is continuously applied to the KNN film 3 via the upper electrode film 4 at a frequency of 300 Hz so that the direction of the electric field applied to the KNN film 3 is not reversed (so that the direction of the electric field is in one direction), the number of voltage application cycles until the piezoelectric displacement of the KNN film 3 falls to 80% or less of its initial value exceeds 10 million.

[0038] In this specification, the term "unipolar electric field" refers to an electric field that is unidirectional even if the magnitude of the voltage applied to the KNN film 3 via the upper electrode film 4 periodically varies within a range of, for example, 0 V to -60 V. In addition, in this specification, "the number of voltage application cycles until the piezoelectric displacement of the KNN film 3 decreases to 80% or less of the initial value when a negative voltage is continuously applied to the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm in the KNN film 3" is also referred to as "the number of application cycles."

[0039] When an AC voltage is applied to the KNN film 3 via the upper electrode film 4, the KNN film 3 deforms. The higher the applied voltage, the greater the deformation of the KNN film 3. The KNN film 3 in this embodiment can have the characteristic that the amount of piezoelectric displacement is unlikely to decrease even when the KNN film 3 is repeatedly and significantly deformed by continuously applying a large AC voltage, i.e., has excellent AC stress resistance.

[0040] In the piezoelectric laminate 10 obtained by the above-mentioned new method, a KNN film 3a having a high (001) orientation rate and a small film stress, for example, a KNN film 3a having a (001) orientation rate of 95% or more and a film stress of 100 MPa or less, is interposed between the lower electrode film 2 and the KNN film 3b. As a result, the KNN film 3 in this embodiment (a laminate of the KNN film 3a and the KNN film 3b) can have a superior AC stress resistance compared to a case where the KNN film 3a is not interposed. This is considered to be because the interposition of the KNN film 3a can significantly improve the adhesion between the lower electrode film 2 and the KNN film 3. In this way, the interposition of the KNN film 3a can make the above-mentioned number of application cycles exceed 10 million, that is, the AC stress resistance of the KNN film 3 can be improved, which is a new finding first found as a result of the inventors' intensive research.

[0041] Since the KNN film 3 has excellent AC stress resistance, it is possible to improve the reliability of the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10, which will be described later.

[0042] The present inventors have confirmed that in a piezoelectric laminate 10 having a KNN film 3a having a (001) orientation rate of 95% or more and a film stress of 100 MPa or less interposed between a lower electrode film 2 and a KNN film 3b, when a negative voltage is continuously applied to the KNN film 3 via the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm in the KNN film 3, the piezoelectric displacement of the KNN film 3 can be maintained at 80% or more of its initial value even after the number of application cycles exceeds 10 million, and even reaches 50 million or more.

[0043] In contrast, when the KNN film 3a is not interposed, that is, when the KNN film 3 is not composed of a laminate of the KNN film 3a and the KNN film 3b, if a large AC voltage is continuously applied to the KNN film 3 via the upper electrode film 4 and the KNN film 3 is continuously and significantly deformed, the KNN film 3 gradually peels off from the lower electrode film 2. As a result, the piezoelectric displacement of the KNN film 3 is easily reduced.

[0044] The inventors have confirmed that in a piezoelectric laminate in which the KNN film 3a is not interposed between the lower electrode film 2 and the KNN film 3b, when a negative voltage is continuously applied to the KNN film via the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm in the KNN film, the piezoelectric displacement of the KNN film falls to less than 80% of its initial value before the number of application cycles reaches 10 million.

[0045] As described above, the KNN film 3 in this embodiment can have all of the above-mentioned features 1 to 3, and preferably all of the above-mentioned features 1 to 4. When the KNN film 3 has all of the above-mentioned features 1 to 3, it becomes possible to suitably apply the piezoelectric element 20 (piezoelectric device module 30) described below obtained by processing the piezoelectric laminate 10 having the KNN film 3 to actuator applications. Furthermore, when the KNN film 3 has all of the above-mentioned features 1 to 4, it becomes possible to more suitably apply the piezoelectric element 20 (piezoelectric device module 30) described below to actuator applications.

[0046] In this embodiment, when the KNN film 3 is formed, the KNN film 3a is first formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then the KNN film 3b is formed on the KNN film 3a at a second temperature at which the piezoelectric constant and DC stress resistance are high. Therefore, the KNN film 3 in this embodiment has a laminated structure of the KNN film 3a as the first layer (initial layer) formed at the first temperature and the KNN film 3b as the second layer formed at the second temperature.

[0047] The KNN film 3a formed at the first temperature has a low piezoelectric constant and DC stress resistance. Therefore, when the ratio of the thickness of the KNN film 3a to the total thickness of the KNN film 3 (the total thickness of the KNN film 3a and the KNN film 3b) becomes large, at least one of the above-mentioned features 1 and 2 tends to be difficult to be realized. Therefore, it is preferable that the thickness of the KNN film 3a is suppressed to the minimum necessary to relax the film stress of the KNN film 3 and make the film stress of the entire KNN film 3 150 MPa or less. The thickness of the KNN film 3a is not strictly limited, but is preferably, for example, 20% or less of the total thickness of the KNN film 3. This ensures that the KNN film 3 having the above-mentioned features 1 and 2 (i.e., the KNN film 3 having a high piezoelectric constant and DC stress resistance) can be reliably obtained, and preferably, the KNN film 3 having the above-mentioned features 1 and 2 can be reliably obtained with good reproducibility.

[0048] The upper electrode film 4 is mainly composed of various metals such as Pt, Au, Al, Cu, etc., or alloys thereof. The upper electrode film 4 can be formed by a method such as sputtering, vapor deposition, plating, metal paste, etc. The upper electrode film 4 does not have a significant effect on the crystal structure of the KNN film 3, unlike the lower electrode film 2. Therefore, the material, crystal structure, and film formation method of the upper electrode film 4 are not particularly limited. Note that, for example, RuO 2 , IrO 2 , Ti, Ta, TiO 2 Alternatively, an adhesion layer 7 mainly composed of Ni or the like may be provided. The thickness of the upper electrode film 4 may be, for example, 50 nm to 5000 nm, preferably 50 nm to 300 nm, and when the adhesion layer 7 is provided, the thickness of the adhesion layer 7 may be, for example, 1 nm to 200 nm, preferably 5 nm to 50 nm. In this specification, the adhesion layer 7 provided between the KNN film 3 and the upper electrode film 4 may be referred to as the upper adhesion layer 7.

[0049] (2) Methods for manufacturing piezoelectric laminates, piezoelectric elements, and piezoelectric device modules A method for manufacturing the above-mentioned piezoelectric laminate 10, the piezoelectric element, and the piezoelectric device module will now be described.

[0050] (Deposition of lower adhesive layer and lower electrode film) First, a substrate 1 is prepared, and a lower adhesive layer 6 (e.g., a ZnO layer) and a lower electrode film 2 (e.g., a Pt film) are formed in this order by, for example, a sputtering method on one of the main surfaces of the substrate 1. Note that a substrate 1 on which the lower adhesive layer 6 and the lower electrode film 2 have been formed in advance on one of the main surfaces may be prepared.

[0051] The following conditions are exemplified as conditions for depositing the ZnO layer as the lower adhesion layer 6. The deposition time of the lower adhesion layer 6 is appropriately adjusted depending on the target thickness of the lower adhesion layer 6. Target: ZnO sintered body Temperature (substrate temperature): 200° C. or higher and 700° C. or lower, preferably 300° C. or higher and 700° C. or lower, more preferably 500° C. or higher and 700° C. or lower Discharge power density: 2W / cm 2 More than 6W / cm 2 Less than 3W / cm, preferably 3W / cm 2 More than 5W / cm 2 below Atmosphere: Argon (Ar) gas and oxygen (O 2 ) gas mixture atmosphere (hereinafter referred to as "Ar / O 2 (also called "mixed gas atmosphere") O 2 The ratio of the partial pressure of Ar gas to the partial pressure of O 2 Gas partial pressure): 5 / 1 to 30 / 1, preferably 7 / 1 to 20 / 1, more preferably 10 / 1 to 15 / 1 Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 1 nm or more and 200 nm or less, preferably 10 nm or more and 50 nm or less

[0052] In this specification, when a numerical range is expressed, such as "5 / 1 to 30 / 1," it means that the lower limit and the upper limit are included in the range. The same applies to other numerical ranges.

[0053] The conditions for forming the Ti layer or the like as the lower adhesion layer 6 are exemplified as follows. Target: Ti plate, etc. Temperature (substrate temperature): 100°C or higher and 500°C or lower, preferably 200°C or higher and 400°C or lower Atmosphere: Ar gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less The other conditions can be the same as those used when providing the ZnO layer.

[0054] The following conditions are exemplified as conditions for depositing a Pt film as the lower electrode film 2. The deposition time of the lower electrode film 2 is appropriately adjusted according to the target thickness of the lower electrode film 2. Target: Pt plate Temperature (substrate temperature): 200°C or higher and 600°C or lower, preferably 300°C or higher and 500°C or lower Discharge power density: 1W / cm 2 More than 5W / cm 2 Less than 2 W / cm, preferably 2 W / cm 2 More than 4W / cm 2 below Atmosphere: Ar gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 100nm to 400nm

[0055] (KNN membrane production) After the formation of the lower adhesive layer 6 and the lower electrode film 2 is completed, the KNN film 3 is formed on the lower electrode film 2 by a sputtering method such as RF magnetron sputtering. The composition of the KNN film 3 can be adjusted by controlling the composition of the target used during the sputtering deposition. 2 CO 3 Powder, Sodium 2 CO 3 powder, Nb 2 O 5 The target can be made by mixing powders and firing them. The composition of the target is K 2 CO 3 Powder, Sodium 2 CO 3 powder, Nb2 O 5 It can be controlled by adjusting the mixing ratio of the powders, etc. When depositing the KNN film 3 containing the above elements such as Cu and Mn, a target in which Cu powder (or CuO powder), Mn powder (or MnO powder), etc. are mixed in a predetermined ratio in addition to the above powders may be used.

[0056] The KNN film 3 is formed in two stages by changing the temperature conditions. Specifically, first (at the beginning of the film formation), the KNN film 3a is formed at a first temperature, and then the KNN film 3b is formed at a second temperature.

[0057] The first temperature is a temperature at which the (001) orientation rate of the KNN film 3a is 95% or more and the film stress is 100 MPa or less. For example, the first temperature is a temperature at which the (001) orientation rate of the KNN film 3a is 95% or more when the KNN film 3a is formed to a thickness of 2 μm (±10%) at the first temperature. Also, the first temperature is a temperature at which the film stress of the KNN film 3a is 100 MPa or less when the KNN film 3a is formed to a thickness of 2 μm (±10%) at the first temperature.

[0058] The second temperature is the piezoelectric constant e of the KNN film 3b. 31 is 10C / m 2 The second temperature is the temperature at which the leakage current density flowing through the KNN film 3b from the start of voltage application becomes 30 mA / cm when HALT under predetermined conditions is performed at a temperature of 200°C. 2 This is the temperature at which it takes more than 5 hours to exceed the limit.

[0059] Although the first temperature and the second temperature depend somewhat on the sputtering deposition apparatus and deposition conditions, in the sputtering deposition of the KNN film 3 in this embodiment, the second temperature is usually higher than the first temperature (first temperature<second temperature). For example, the first temperature can be in the range of 550°C or more and 600°C or less, and the second temperature can be in the range of 650°C or more and 800°C or less.

[0060] As conditions other than the temperature when forming the KNN film 3 (KNN film 3a, KNN film 3b), the following conditions are exemplified for both the film formation at the first temperature and the film formation at the second temperature. Discharge power density: 2.7W / cm 2 More than 4.1W / cm 2 Less than or equal to 2.8 W / cm 2 More than 3.8W / cm 2 below Atmosphere: Atmosphere containing at least Ar gas, preferably Ar / O 2 Mixed gas atmosphere Ambient pressure: 0.03 Pa or more and 0.5 Pa or less, preferably 0.04 Pa or more and 0.4 Pa or less O vs Ar gas 2 Ratio of partial pressures of gases (O 2 Gas partial pressure / Ar gas partial pressure): 0 to 1 / 20, preferably 0 to 1 / 30 Film-forming speed: 0.5 μm / hr or more and 4 μm / hr or less, preferably 0.5 μm / hr or more and 2 μm / hr or less Total thickness of KNN film: 0.5 μm or more and 5 μm or less, preferably 1 μm or more and 3 μm or less

[0061] In addition, "O 2 "Gas partial pressure / Ar gas partial pressure is 0 (zero)" means that O 2 It means a state where the gas partial pressure is 0, that is, the atmosphere is only Ar gas. In addition, the "total thickness of the KNN film" is the total thickness of the KNN film 3a formed at the first temperature and the KNN film 3b formed at the second temperature. In addition, the deposition time of the KNN film 3a and the KNN film 3b is appropriately adjusted according to the target thickness of the KNN film 3a, 3b. As described above, it is preferable that the thickness of the KNN film 3a is the minimum thickness necessary to reduce the film stress in the KNN film 3b by deposition at the second temperature and to make the film stress of the entire KNN film 3 150 MPa or less. For this reason, it is preferable to adjust the deposition time of the KNN film 3a (deposition time at the first temperature) so that the thickness of the KNN film 3a is 20% or less of the total thickness of the KNN film 3, for example.

[0062] As described above, first, the KNN film 3a is formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then the KNN film 3b is formed on the KNN film 3a at a second temperature at which the piezoelectric constant and DC stress resistance are high. Even if the second temperature is a high temperature at which the KNN film 3b generates a large film stress, the film stress of the entire KNN film 3 after the KNN film 3b is formed can be greatly alleviated. As a result, a KNN film 3 having a high piezoelectric constant and DC stress resistance and a small film stress can be obtained. That is, by forming the KNN film 3 (KNN film 3a and KNN film 3b) in two stages by changing the temperature under the above-mentioned conditions, a KNN film 3 having all of the above-mentioned characteristics 1 to 3 can be obtained. In addition, by forming the KNN film 3 in two stages by changing the temperature under the above-mentioned conditions, that is, by providing the KNN film 3a having a high (001) orientation rate and a small film stress, a KNN film 3 having all of the above-mentioned characteristics 1 to 4 can also be obtained.

[0063] (Deposition of upper adhesive layer and upper electrode film) After the deposition of the KNN film 3 is completed, an upper adhesion layer 7 (e.g., RuO 2 layer) and upper electrode film 4 (for example, a Pt film) are deposited in this order.

[0064] RuO as the upper adhesion layer 7 2 The conditions for forming the layers and the like are exemplified as follows: The film formation time for the upper adhesive layer 7 is appropriately adjusted depending on the target thickness of the upper adhesive layer 7. Target: Ru plate, etc. Temperature (substrate temperature): Room temperature (25℃) or higher and 500℃ or lower Discharge power density: 0.3W / cm 2 More than 2W / cm 2 Less than or equal to 0.5 W / cm 2 More than 1W / cm 2 below Atmosphere: Ar / O 2 Mixed gas atmosphere O 2 The ratio of the partial pressure of Ar gas to the partial pressure of O 2 Gas partial pressure): 3 / 5 to 1 / 1, preferably 3 / 4 to 1 / 1 Ambient pressure: 0.1 Pa or more and 1.0 Pa or less, preferably 0.2 Pa or more and 0.7 Pa or less Thickness: 1 nm or more and 200 nm or less, preferably 5 nm or more and 50 nm or less

[0065] The following conditions are exemplified as conditions for depositing a Pt film or the like as the upper electrode film 4. The deposition time of the upper electrode film 4 is appropriately adjusted according to the target thickness of the upper electrode film 4. Target: Pt plate, etc. Temperature (substrate temperature): Room temperature (25℃) or higher and 500℃ or lower Discharge power density: 1W / cm 2 More than 5W / cm 2 Less than 2 W / cm, preferably 2 W / cm 2 More than 4W / cm 2 below Atmosphere: Ar gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 50 nm or more and 5000 nm or less, preferably 50 nm or more and 300 nm or less

[0066] As described above, the lower adhesive layer 6, the lower electrode film 2, the KNN film 3 (KNN films 3a, 3b), the upper adhesive layer 7, and the upper electrode film 4 are sequentially formed to obtain the piezoelectric stack 10 as shown in FIG.

[0067] (Preparation of piezoelectric elements) After producing the piezoelectric laminate 10 as shown in FIG. 1, the piezoelectric laminate 10 is processed to form an element having a KNN film 3 (also referred to as a piezoelectric element 20).

[0068] Specifically, first, the upper electrode film 4 (including the upper adhesive layer 7) and the KNN film 3 are individually patterned by dry etching using, for example, Ar gas or a reactive gas. In the patterning, the upper electrode film 4 (including the upper adhesive layer 7) and the KNN film 3 are each formed into a predetermined shape, and a part of the lower electrode film 2 is exposed. In the patterning, a photoresist can be used as an etching mask. FIG. 2 shows the piezoelectric stack 10 after the patterning is completed, i.e., a piezoelectric element 20. The piezoelectric element 20 shown in FIG. 2 is also called a simplified piezoelectric element.

[0069] 2, the lower electrode film 2 and the lower adhesive layer 6 are patterned by dry etching using, for example, Ar gas or a reactive gas, to form the lower electrode film 2 and the lower adhesive layer 6 into a predetermined shape. In this patterning, a photoresist can be used as an etching mask.

[0070] After completing the patterning of the lower electrode film 2 and the lower adhesive layer 6, the insulating film 8 and the metal wirings 9a and 9b are provided. Specifically, first, a layer made of an insulating material is provided from the upper electrode film 4 to the substrate 1 so as to cover the side surface of the KNN film 3, and then the insulating layer is heated with Ar gas or CF 4 The layer made of an insulating material is patterned by dry etching using a reactive gas such as a silicon oxide (SiO 2 ), aluminum oxide (Al 2 O 3 ), tantalum oxide (Ta 2 O 5 The insulating film 8 may be a single layer film or a laminated body having multiple layers stacked together. The insulating film 8 may be provided by a method such as a CVD method or a sputtering method.

[0071] After providing the insulating film 8, a layer (metal wiring layer) made of a material containing metal is provided. Then, the metal wiring layer is patterned by dry etching using Ar gas or reactive gas or wet etching to form metal wirings 9a and 9b. The metal wiring 9a is formed (patterned) so as to be connected (contacted) to the lower electrode film 2 and not connected (not contacted) to the upper electrode film 4, and the metal wiring 9b is formed so as to be connected to the upper electrode film 4 and not connected to the lower electrode film 2. The metal wirings 9a and 9b can be formed using various metals such as Au, Al, Ti, and Cr, or alloys mainly composed of these various metals. The metal wirings 9a and 9b may be a single layer film or a laminated body in which multiple layers are laminated. The metal wirings 9a and 9b (metal wiring layer) can be provided by a method such as a sputtering method, a vapor deposition method, a plating method, or a metal paste method.

[0072] Further, a part of the substrate 1 is removed from the back surface side of the substrate 1 (one of the two main surfaces of the substrate 1 opposite to the surface on which the lower electrode film 2 and the like are formed) by Deep-RIE or wet etching, thereby obtaining a piezoelectric element 20 having a membrane structure, a cantilever structure, or the like, for example, a membrane-type MEMS piezoelectric element 20 as shown in FIG.

[0073] The etching conditions for pattern processing when forming the insulating film 8 and the metal wiring 9a, 9b, and the etching conditions for the substrate 1 when processing the piezoelectric laminate 10 into the piezoelectric element 20 can be general etching conditions used in the semiconductor device manufacturing process as long as the conditions do not deteriorate the insulating properties of the KNN film 3.

[0074] (Fabrication of piezoelectric device module) By connecting the voltage application means 11a to the obtained piezoelectric element 20, a device module 30 having a KNN film 3 (hereinafter also referred to as piezoelectric device module 30) is obtained. FIG. 4 shows a schematic configuration diagram of the piezoelectric device module 30 according to this embodiment. The piezoelectric device module 30 at least includes the piezoelectric element 20 and a voltage application means 11a connected to the piezoelectric element 20. The voltage application means 11a is a means for applying a voltage between the lower electrode film 2 and the upper electrode film 4 (between the electrodes). As the voltage application means 11a, various known means can be used.

[0075] By connecting the voltage application means 11a between the lower electrode film 2 and the upper electrode film 4 of the piezoelectric element 20, the piezoelectric device module 30 can function as an actuator. By applying a voltage between the lower electrode film 2 and the upper electrode film 4 by the voltage application means 11a, the KNN film 3 can be deformed. This deformation action can operate various members connected to the piezoelectric element 20. In this case, examples of applications of the piezoelectric element 20 include heads for inkjet printers, MEMS mirrors for scanners, and vibrators for ultrasonic generators.

[0076] (3) Effects According to this aspect, one or more of the following effects can be obtained.

[0077] (a) The KNN film 3 has a piezoelectric constant e 31 is 10C / m 2 or more (Feature 1 above); when HALT under specified conditions is performed at a temperature of 200°C, the leakage current density flowing through the KNN film 3 from the start of voltage application is 30 mA / cm 2 The KNN film 3 simultaneously has both the feature that it takes 5 hours or more for the temperature to exceed 100° C. (Feature 2 above) and the feature that the film stress is 150 MPa or less (Feature 3 above). In other words, the KNN film 3 is a film with a high piezoelectric constant and DC stress resistance, and a small film stress.

[0078] Piezoelectric constant e of KNN film 3 31 is 10C / m 2The above makes it possible to improve the piezoelectric characteristics of the KNN film 3. Furthermore, since the KNN film 3 has high DC stress resistance, the KNN film 3 is less susceptible to dielectric breakdown even when a high voltage is applied to the KNN film 3 via the upper electrode film 4 for a long period of time when the piezoelectric element 20 (piezoelectric device module 30) is driven. These make it possible to suitably apply the piezoelectric element 20 (piezoelectric device module 30) to actuator applications.

[0079] Since the film stress of the KNN film 3 is 150 MPa or less, it is possible to suppress large structural deformation when processing the piezoelectric stack 10 to fabricate the piezoelectric element 20 (piezoelectric device module 30) having a membrane structure, a cantilever structure, or the like. This allows the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric stack 10 to operate normally. For example, it becomes possible for the piezoelectric element 20 (piezoelectric device module 30) to function reliably as an actuator.

[0080] In this way, when the KNN film 3 has all of the above-mentioned characteristics 1 to 3, the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 can be suitably used as an actuator.

[0081] (b) Since the KNN film 3a having a high (001) orientation rate and small film stress is interposed between the lower electrode film 2 and the KNN film 3b, the KNN film 3 can have the above-mentioned feature (feature 4) of having the above-mentioned number of application cycles exceeding 10 million, in addition to the above-mentioned features 1 to 3. That is, the KNN film 3 can be a film having a high piezoelectric constant and DC stress resistance, small film stress, and excellent AC stress resistance.

[0082] Since the KNN film 3 has excellent AC stress resistance, that is, the piezoelectric displacement amount is unlikely to decrease even if the KNN film 3 is repeatedly and significantly deformed, it is possible to improve the reliability of the piezoelectric element 20 (piezoelectric device module 30).

[0083] In this way, when the KNN film 3 has all of the above-mentioned characteristics 1 to 4, the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 can be more suitably used as an actuator.

[0084] (c) When forming the KNN film 3, first, the KNN film 3a is formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then the KNN film 3b is formed on the KNN film 3a at a second temperature at which the piezoelectric constant and DC stress resistance are high, thereby obtaining a KNN film 3 having all of the above-mentioned characteristics 1 to 3, preferably all of the above-mentioned characteristics 1 to 4.

[0085] (4) Variations The present disclosure is not limited to the above-described aspects and can be modified, for example, as follows.

[0086] (Variation 1) After the deposition of the KNN film 3, preferably after the deposition of the KNN film 3 and before the deposition of the upper electrode film 4 (upper adhesive layer 7), the KNN film 3 may be annealed. In this modification, the same effects as those of the above-mentioned embodiment can be obtained. In addition, in this modification, the DC stress resistance can be further improved. That is, when HALT under specified conditions is performed at a temperature of 200°C, the leakage current density flowing through the KNN film 3 from the start of voltage application is 30 mA / cm. 2 In addition, the time required for the piezoelectric constant e 31 can also be increased reliably.

[0087] The annealing conditions are exemplified as follows. Atmosphere: O-containing atmosphere such as air Temperature: 500°C or higher and 700°C or lower, preferably 550°C or higher and 650°C or lower Time: 10 minutes to 5 hours, preferably 30 minutes to 3 hours

[0088] <Other aspects> One embodiment of the present invention has been specifically described above. However, the present invention is not limited to the above embodiment, and various modifications can be made without departing from the spirit of the present invention. In addition, these embodiments can be combined in any manner.

[0089] In the above embodiment, the piezoelectric device module 30 is caused to function as an actuator, but the invention is not limited thereto. That is, the piezoelectric device module 30 may be caused to function as a sensor. In this case, the piezoelectric device module 30 includes at least a piezoelectric element 20 obtained by forming the above-mentioned piezoelectric laminate 10 into a predetermined shape, and a voltage detection means 11b (see FIG. 4) connected to the piezoelectric element 20. The voltage detection means 11b is a means for detecting a voltage generated between the lower electrode film 2 and the upper electrode film 4 (between the electrodes). Various known means can be used as the voltage detection means 11b. By connecting the voltage detection means 11b between the lower electrode film 2 and the upper electrode film 4 of the piezoelectric element 20, the piezoelectric device module 30 can be caused to function as a sensor. When the KNN film 3 is deformed in accordance with a change in some physical quantity, a voltage is generated between the lower electrode film 2 and the upper electrode film 4 due to the deformation. By detecting this voltage by the voltage detection means 11b, the magnitude of the physical quantity applied to the KNN film 3 can be measured. In this case, examples of applications of the piezoelectric device module 30 include an angular velocity sensor, an ultrasonic sensor, a pressure sensor, and an acceleration sensor.

[0090] Furthermore, for example, when the above-mentioned piezoelectric laminate 10 is molded into the piezoelectric element 20, the substrate 1 of the piezoelectric laminate 10 may be replaced with another substrate, so long as the piezoelectric device module 30 produced using the piezoelectric laminate 10 (piezoelectric element 20) can be applied to a desired purpose such as an actuator. EXAMPLES

[0091] Hereinafter, experimental results that support the effects of the above-described embodiment will be described.

[0092] [Experiment 1] An experiment was carried out to confirm the applicable temperatures for the first temperature and the second temperature when depositing a KNN film.

[0093] (Preparation of samples A to J) A Si substrate with a surface orientation of (100), a thickness of 610 μm, a diameter of 6 inches (also referred to as "φ6 inches"), and a thermally oxidized film (thickness of 200 nm) formed on the surface was prepared as the substrate. On the thermally oxidized film of this Si substrate, a ZnO layer (thickness of 25 nm) was formed as a lower adhesive layer, a Pt film (preferentially oriented in the (111) plane orientation with respect to the surface of the substrate, thickness of 200 nm) was formed as a lower electrode film, a KNN film (thickness of 2 μm) was formed as a piezoelectric film, and a RuO 2 A KNN layer (thickness 10 nm) as a top electrode film, and a Pt film (thickness 100 nm) as a top electrode film were deposited in this order to fabricate samples A to J, which are piezoelectric laminates. In samples A to J, the bottom adhesive layer, bottom electrode film, KNN film, top adhesive layer, and top electrode film were all deposited by RF magnetron sputtering.

[0094] The conditions for depositing the ZnO layer as the lower adhesive layer were as follows. Target: ZnO sintered body Substrate temperature: 500℃ Discharge power density: 4W / cm 2 Atmosphere: Ar / O 2 Mixed gas atmosphere Ambient pressure: 0.3Pa Ar gas partial pressure / O 2 Gas partial pressure: 10 / 1 Film deposition time: 3 minutes (thickness 25 nm)

[0095] The conditions for depositing the Pt film as the lower electrode film were as follows. Target: Pt plate Substrate temperature: 500℃ Discharge power density: 2W / cm 2 Atmosphere: Ar gas atmosphere Ambient pressure: 0.3Pa Film deposition time: 14 minutes (thickness 200 nm)

[0096] The conditions for forming the KNN membrane were as follows: Target: KNN sintered body Discharge power density: 3W / cm 2 Atmosphere: Ar / O 2 Mixed gas atmosphere Ambient pressure: 0.1Pa O 2 Gas partial pressure / Ar gas partial pressure: 1 / 20 Film forming temperature: A specified temperature within the range of 300°C to 800°C Film deposition time: 60 minutes (thickness 2000 nm (2 μm))

[0097] RuO as top adhesion layer 2 The conditions for forming the layers were as follows: Target: Ru plate Substrate temperature: Room temperature (25℃) Discharge power density: 0.5W / cm 2 Atmosphere: Ar / O 2 Mixed gas atmosphere Ambient pressure: 0.3Pa Ar gas partial pressure / O 2 Gas partial pressure: 1 / 1 Film deposition time: 6 minutes (thickness 10 nm)

[0098] The conditions for depositing the Pt film as the upper electrode film were as follows. Target: Pt plate Substrate temperature: Room temperature (25℃) Discharge power density: 2W / cm 2 Atmosphere: Ar gas atmosphere Ambient pressure: 0.3Pa Film deposition time: 7 minutes (thickness 100 nm)

[0099] Each of the samples A to J was produced under the same conditions as described above, except for the deposition temperature of the KNN film. The deposition temperatures of the KNN films of the samples A to J are as shown in Table 1 below.

[0100] <Evaluation> For samples A to J, the (001) orientation rate, film stress, DC stress resistance, and piezoelectric constant e 31 was evaluated.

[0101] (Evaluation of (001) orientation rate) The (001) orientation rate of the KNN film was evaluated by calculating using the above formula (1) based on the peak intensity of the X-ray diffraction pattern (2θ / θ) obtained by performing XRD measurement on the KNN film. The XRD measurement was performed after the KNN film was formed and before the upper adhesive layer and the upper electrode film were formed. The calculation results of the (001) orientation rate are shown in Table 1 below. In Table 1, the "orientation rate" refers to the (001) orientation rate of the KNN film.

[0102] (Evaluation of membrane stress) The stress of the thin film on the substrate can be calculated by measuring the amount of warpage of the substrate caused by the thin film, specifically, the radius of curvature of the warpage of the substrate, as shown in the following formula (2). Therefore, in this evaluation, first, the radius of curvature R of the warpage of the substrate (Si substrate) of each sample was measured after the lower adhesive layer, the lower electrode film, and the KNN film were formed, and before the upper adhesive layer and the upper electrode film were formed. Then, the film stress of the KNN film of each sample was calculated using the following formula (2). In this evaluation, the radius of curvature R of the Si substrate was calculated from the warpage shape of the Si substrate after the lower adhesive layer, the lower electrode film, and the KNN film were formed, measured by a laser displacement meter.

[0103] TIFF2024141260000002.tif17170

[0104] In the above formula (2), σ is the stress of the thin film (KNN film), E s / (1-ν s) is the biaxial elastic modulus of the substrate (Pa), h is the thickness of the substrate (m), R is the radius of curvature of the warp of the substrate (m), and t is the thickness of the KNN film (m). In samples A to J, a Si substrate was used as the substrate, so the value of the biaxial elastic modulus was set to 30.3. In addition, the film stress (σ) of the KNN film was calculated assuming that the Si substrate was sufficiently flat. In addition, in samples A to J, a lower adhesive layer (ZnO layer) and a lower electrode film (Pt film) were formed, but the thickness of the lower adhesive layer (25 nm) and the thickness of the lower electrode film (200 nm) were sufficiently smaller than the thickness of the KNN film (2 μm). For this reason, the influence of the lower adhesive layer and the lower electrode film was ignored to calculate the film stress of the KNN film.

[0105] The calculation results of the film stress of the KNN film of samples A to J are shown in the following Table 1. In Table 1, "compressive" means that the film stress is compressive stress, and "tensile" means that the film stress is tensile stress.

[0106] (Piezoelectric constant e 31 Evaluation) Piezoelectric constant e of KNN film 31 was calculated by the following method. First, a small rectangular piece of 20 mm long x 2.5 mm wide was cut out from each of the samples A to J. Then, as shown in FIG. 5(a), one end in the longitudinal direction of each small piece obtained from the samples A to J was fixed by a clamp, and a voltage application means (not shown) was connected between the lower electrode film and the upper electrode film to fabricate a simple unimorph cantilever. Then, using the voltage application means, a sine wave negative voltage was applied to the KNN film via the upper electrode film while the lower electrode film was grounded so as to generate an electric field of 100 kV / cm between the lower electrode film and the upper electrode film (i.e., the KNN film), thereby expanding and contracting (deforming) the KNN film. The deformation of the KNN film causes the entire cantilever to bend and expand (vibrate), and the tip of the cantilever to reciprocate in the vertical direction. The displacement Δ (piezoelectric displacement) of the tip of the cantilever was measured by irradiating the tip of the cantilever with laser light L from a laser Doppler displacement meter as shown in Figure 5(b). The piezoelectric constant e at an applied electric field of 100 kV / cm was calculated using the displacement Δ of the tip of the cantilever, the length of the cantilever, and the applied voltage. 31The piezoelectric constant e 31 The measurement results are shown in Table 1.

[0107] In addition, in Figures 5(a) and 5(b), for ease of understanding, the lower adhesive layer and the upper adhesive layer are omitted, and the stack of the first KNN film and the second KNN film is illustrated as a KNN film.

[0108] (Evaluation of DC stress resistance) The DC stress resistance was evaluated by measuring the DC stress life. Specifically, the DC stress life was measured when the leakage current density flowing through the KNN film from the start of voltage application was 30 mA / cm when HALT was performed at a temperature of 200°C by applying a negative voltage to the upper electrode film (through the KNN film) so as to generate an electric field of 300 kV / cm in the KNN film. 2 The evaluation was performed by measuring the time until the voltage exceeded the threshold. In the HALT, a certain negative voltage was applied to the upper electrode film while the lower electrode film was grounded. The measurement results are shown in Table 1 below.

[0109] [Table 1]

[0110] In sample A, the crystal structure of the KNN film was not a perovskite structure. Therefore, in the X-ray diffraction pattern obtained by performing XRD measurement, a peak could not be observed at least within the range of 2θ of 20° to 23°, and as a result, the (001) orientation rate could not be calculated. In addition, since the crystal structure of the KNN film was not a perovskite structure, the KNN film had low pressure resistance and the piezoelectric constant e 31 When measuring the piezoelectric constant e, it was not possible to apply a certain voltage to the KNN film through the upper electrode film. 31 From these, it can be confirmed that neither the first temperature nor the second temperature can be applied to the film formation temperature of sample A.

[0111] In samples B to D, the film stress is more than 100 MPa and the piezoelectric constant e 31 is 10C / m2 and the DC stress lifetime is less than 5 hours. From this, it can be confirmed that neither the first temperature nor the second temperature is applicable to the film formation temperatures of Samples B to D.

[0112] In samples E and F, the (001) orientation rate is 95% or more, and the film stress is 100 MPa or less. This confirms that the film formation temperature of samples E and F, that is, the temperature range of 550°C to 600°C, is applicable to the first temperature. On the other hand, in samples E and F, the piezoelectric constant e 31 is 10C / m 2 The DC stress lifetime is less than 5 hours. From this, it can be confirmed that the deposition temperatures of samples E and F cannot be applied to the second temperature.

[0113] In samples G to J, the piezoelectric constant e 31 is 10C / m 2 and the DC stress life is 5 hours or more. This confirms that the film deposition temperatures of samples G to J, i.e., the temperature range of 650°C or higher and 800°C or lower, are applicable to the second temperature. On the other hand, in samples G to J, the (001) orientation rate is less than 95%, and the film stress is more than 100 MPa. This confirms that the film deposition temperatures of samples G to J are not applicable to the first temperature.

[0114] [Experiment 2] An experiment was conducted to confirm the effect of depositing the KNN film in two stages at different temperatures.

[0115] (Preparation of samples 1 to 14) A Si substrate with a surface orientation of (100), thickness of 610 μm, diameter of 6 inches, and a thermal oxide film (thickness of 200 nm) formed on the surface was prepared as the substrate. On the thermal oxide film of this Si substrate, a ZnO layer (thickness of 25 nm) was formed as a lower adhesive layer, a Pt film (preferentially oriented in the (111) plane orientation with respect to the surface of the substrate, thickness of 200 nm) as a lower electrode film, a KNN film (thickness of 2 μm) as a piezoelectric film, and a RuO 2A KNN layer (thickness 10 nm) as a top electrode film, and a Pt film (thickness 100 nm) as a top electrode film were deposited in this order to fabricate piezoelectric laminates, Samples 1 to 14. The bottom adhesive layer, bottom electrode film, KNN film, top adhesive layer, and top electrode film were all deposited by RF magnetron sputtering.

[0116] In the samples 1 to 11, the KNN film was formed in two stages by changing the temperature conditions. Specifically, the first KNN film was formed at the first temperature, and then the second KNN film was formed on the first KNN film at the second temperature different from the first temperature. The first and second temperatures for forming the KNN films of the samples 1 to 11 were as shown in the following Table 2, respectively, and the film formation time at the first temperature was 6 minutes (thickness 200 nm), and the film formation time at the second temperature was 54 minutes (thickness 1800 nm). In the samples 12 to 14, the KNN film was formed at a predetermined temperature without changing the temperature conditions. The temperature for forming the KNN films of the samples 12 to 14 was as shown in the "second temperature" column in the following Table 2, and the film formation time was 60 minutes (thickness 2000 nm). The conditions other than the deposition temperature and deposition time when depositing the KNN film, and the deposition conditions for each film (each layer) other than the KNN film, were the same as those in the above-mentioned Experiment 1. Moreover, each of Samples 1 to 14 was produced under the same conditions as described above, except for the deposition temperature (first temperature, second temperature) of the KNN film.

[0117] <Evaluation> For samples 1 to 14, the piezoelectric constant e of the KNN film 31 The DC stress resistance, film stress, (001) orientation rate, and AC stress resistance were evaluated.

[0118] (Evaluation of the piezoelectric constant, DC stress resistance, film stress, and (001) orientation rate of KNN films) Piezoelectric constant e of samples 1 to 14 31 , DC stress resistance, film stress, and (001) orientation rate of the KNN film in the above experiment 1 are calculated by the piezoelectric constant e 31The evaluation results are shown in Table 2 below.

[0119] In addition, in samples 1 to 14, the lower adhesive layer and the lower electrode film are also formed, but similar to samples A to J, the thickness of the lower adhesive layer and the lower electrode film is sufficiently smaller than the thickness of the KNN film. Therefore, the influence of the lower adhesive layer and the lower electrode film was ignored to calculate the film stress of the KNN film. Also, in Table 2, "compression" means that the film stress is compressive stress, and "tensile" means that the film stress is tensile stress.

[0120] (Evaluation of AC stress resistance) The AC stress resistance was evaluated by measuring the AC stress life. The evaluation of the AC stress life was carried out as follows. First, small rectangular pieces measuring 20 mm in length and 2.5 mm in width were cut out from each of Samples 1 to 14. Then, the piezoelectric constant e 31 A simple unimorph cantilever as shown in FIG. 5(a) was fabricated by the same method as described in the evaluation of . Then, a negative voltage was continuously applied to the upper electrode film (through the KNN film) so that a unipolar AC electric field of 300 kV / cm was generated in the KNN film. Specifically, with the lower electrode film grounded, a unipolar sine wave AC voltage with an amplitude of 0 V to -60 V was continuously applied to the KNN film through the upper electrode film at a frequency of 300 Hz, thereby continuously deforming each small piece of KNN film (thickness 2 μm). The deformation of the KNN film causes the entire cantilever to bend and stretch (vibrate), and the tip of the cantilever continuously reciprocates in the vertical direction. The displacement amount Δ (piezoelectric displacement amount) of the tip of the cantilever at this time was calculated by the piezoelectric constant e in the above-mentioned experiment 1. 31The measurements were performed using the same method as described in the evaluation of . In this evaluation, the displacement Δ was measured every time the number of applied cycles reached 1 million. The number of applied cycles at which the displacement Δ became 80% or less of its initial value was taken as the AC stress life. If the displacement Δ was still 80% or more of its initial value after the number of applied cycles reached 50 million, the measurement was stopped and the measurement result of the AC stress life was taken as more than 50 million cycles (>50 million cycles). The measurement results are shown in Table 2 below.

[0121] [Table 2]

[0122] In samples 3 to 5, 7, and 8, the piezoelectric constant e 31 is 10C / m 2 The KNN film is formed from samples 3 to 5, 7, and 8 by first forming a first KNN film at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then forming a second KNN film on the first KNN film at a second temperature at which the piezoelectric constant and DC stress resistance are high. 31 is 10C / m 2 It can be seen that a KNN film having all three characteristics, i.e., a DC stress life of 5 hours or more (characteristic 1 described above), a DC stress life of 5 hours or more (characteristic 2 described above), and a film stress of 150 MPa or less (characteristic 3 described above), can be obtained.

[0123] In samples 1, 2, and 6, the piezoelectric constant e 31 is 10C / m 2 and the DC stress life is less than 5 hours. This is believed to be because in Samples 1, 2, and 6, the second temperature is less than 650° C. (400° C., 500° C.). This shows that if the second temperature is not a temperature at which the piezoelectric constant and DC stress resistance of the second KNN film are high, a KNN film with a high piezoelectric constant and DC stress resistance, i.e., a KNN film having the above-mentioned features 1 and 2, cannot be obtained.

[0124] In Samples 9 to 11, the film stress exceeds 150 MPa. This is believed to be because in Samples 9 and 10, the first temperature is less than 550°C (400°C, 500°C), while in Sample 11, the first temperature is more than 600°C (650°C). Samples 9 to 11 show that if the first temperature is not a temperature at which the film stress of the first KNN film is 100 MPa or less, a KNN film with low film stress cannot be obtained. Also, in Samples 9 to 11, the (001) orientation rate of the KNN film is less than 90%. Samples 9 to 11 show that if the first temperature is not a temperature at which the (001) orientation rate of the first KNN film is 95% or more, the (001) orientation rate of the second KNN film cannot be 90% or more.

[0125] In addition, in Samples 1 to 8, the number of application cycles until the displacement Δ became 80% or less of the initial value exceeded 50 million, and the samples had excellent AC stress resistance. This is believed to be due to the presence of a KNN film with a high (001) orientation rate and low film stress (for example, a KNN film with a (001) orientation rate of 95% or more and a film stress of 100 MPa or less) between the lower electrode film and the second KNN film.

[0126] In particular, in samples 3 to 5, 7, and 8, the piezoelectric constant e 31 is 10C / m 2 or more, the DC stress life is 5 hours or more, the film stress is 150 MPa or less, and the number of application cycles described above is more than 10 million times (50 million times or more). That is, it is understood that Samples 3 to 5, 7, and 8 have the feature of excellent AC stress resistance (feature 4 described above) in addition to the features 1 to 3 described above. From Samples 3 to 5, 7, and 8, it is understood that when forming a KNN film, a first KNN film is first formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then a second KNN film is formed on the first KNN film at a second temperature that is a predetermined temperature higher than the first temperature, thereby obtaining a KNN film having all of the features 1 to 4 described above.

[0127] In contrast, in samples 9 to 14, the number of application cycles until the displacement Δ becomes 80% or less of the initial value is 10 million or less, and the AC stress resistance is low. This is because, in samples 9 to 11, the first KNN film is not formed at a temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, that is, the first KNN film has a low (001) orientation rate and a large film stress. In addition, in samples 12 to 14, the KNN film is not formed by a laminate of the first KNN film and the second KNN film, specifically, a KNN film with a high (001) orientation rate and a small film stress is not interposed between the lower electrode film and the KNN film.

[0128] In addition, in the deposition of the KNN film, the deposition time at the first temperature was set to 6 minutes in Samples 1 to 11, but is not limited to this. The inventors have confirmed that the same results as those described above can be obtained if the deposition time at the first temperature is in the range of 1 minute to 12 minutes. In the deposition of the KNN film, it has been confirmed that the deposition time at the first temperature, i.e., the optimal value of the thickness of the KNN film deposited at the first temperature, may have a certain degree of range.

[0129] (Evaluation of membrane stress) In the above-mentioned Experiments 1 and 2, the membrane stress of the KNN film was calculated from the amount of warping of the substrate (Si substrate), i.e., the radius of curvature of the warping of the substrate, but this is not limited to this. The membrane stress of the KNN film can be known by comparing the MEMS simulation with the shape of the actual object even in the state of a piezoelectric element (piezoelectric device module) in which a MEMS structure is fabricated by processing a piezoelectric laminate.

[0130] <Preferred aspects of the present disclosure> Preferred aspects of the present disclosure will be described below.

[0131] (Appendix 1) According to one aspect of the present disclosure, A substrate; A lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; The piezoelectric constant e of the piezoelectric film 31 is 10C / m 2 That's all. When a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film provided on the piezoelectric film at a temperature of 200° C., the leakage current density flowing through the piezoelectric film from the start of application of the negative voltage is 30 mA / cm 2 The time it takes to exceed this limit is 5 hours or more, The membrane stress of the piezoelectric film is 150 MPa or less. A piezoelectric stack is provided.

[0132] (Appendix 2) The piezoelectric laminate according to claim 1, preferably When a negative voltage is continuously applied to the upper electrode film so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and the upper electrode film, the number of voltage application cycles until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.

[0133] (Appendix 3) The piezoelectric laminate according to claim 1 or 2, preferably A layer containing zinc and oxygen is provided between the substrate and the lower electrode film.

[0134] (Appendix 4) The piezoelectric laminate according to any one of Supplementary Notes 1 to 3, preferably The piezoelectric film contains at least one element selected from copper and manganese as a dopant at a concentration of 0.1 at % to 2.0 at %.

[0135] (Appendix 5) According to another aspect of the present disclosure, forming a lower electrode film on a substrate; forming a piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen on the lower electrode film; In the step of forming the piezoelectric film, first, a first piezoelectric film, which is a part of the piezoelectric film, is formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then a second piezoelectric film, which is the other part of the piezoelectric film, is formed at a first temperature at which the piezoelectric constant e 31 is 10C / m 2 When a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film formed on the second piezoelectric film, the leakage current density flowing through the second piezoelectric film is 30 mA / cm 2 A film is formed on the first piezoelectric film at a second temperature at which the time until the temperature exceeds the second temperature is 5 hours or more. A method for manufacturing a piezoelectric stack is provided.

[0136] (Appendix 6) The method according to claim 5, preferably comprising: The thickness of the first piezoelectric film is 20% or less of the total thickness of the piezoelectric film.

[0137] (Appendix 7) The method according to claim 5 or 6, preferably comprising The first temperature is a temperature at which, when the first piezoelectric film is deposited to a thickness of 2 μm at the first temperature, the (001) orientation rate of the first piezoelectric film is 95% or more.

[0138] (Appendix 8) The method according to any one of appendix 5 to 7, preferably comprising: The first temperature is a temperature at which the film stress of the first piezoelectric film becomes 100 MPa or less when the first piezoelectric film is formed to a thickness of 2 μm at the first temperature.

[0139] (Appendix 9) The method according to any one of appendix 5 to 8, preferably comprising: The method further includes a step of providing a layer containing zinc and oxygen on the substrate before the step of forming the piezoelectric film, In the step of forming the lower electrode film, the lower electrode film is formed on the layer containing zinc and oxygen.

[0140] (Appendix 10) According to yet another aspect of the present disclosure, A substrate; A lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; an upper electrode film formed on the piezoelectric film; The piezoelectric constant e of the piezoelectric film 31 is 10C / m 2 That's all. When a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film at a temperature of 200° C., the leakage current density flowing through the piezoelectric film from the start of application of the negative voltage is 30 mA / cm 2 The time it takes to exceed this limit is 5 hours or more. A piezoelectric element or device module is provided.

[0141] (Appendix 11) According to yet another aspect of the present disclosure, A piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, Piezoelectric constant e 31 is 10C / m 2 That's all. When a negative voltage is applied to the upper electrode film provided on the piezoelectric film so as to generate an electric field of 300 kV / cm in the piezoelectric film at a temperature of 200° C., the leakage current density flowing in the piezoelectric film from the start of application of the negative voltage is 30 mA / cm 2 The time it takes to exceed this limit is 5 hours or more, The membrane stress is 150 MPa or less. A piezoelectric film is provided.

[0142] (Appendix 12) The piezoelectric film, the piezoelectric element, or the piezoelectric device module according to claim 10 or 11, preferably When a negative AC voltage is continuously applied to the upper electrode film (the upper electrode film provided on the piezoelectric film) so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and the upper electrode film (to the piezoelectric film), the number of voltage application cycles until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million. [Explanation of symbols]

[0143] 1 Board 2 Lower electrode film 3. Piezoelectric film 4 Upper electrode film 6 (Bottom) Adhesion layer 7 (Upper) Adhesion layer 10 Piezoelectric laminate 20 Piezoelectric element 30 Piezoelectric Device Module

Claims

1. A substrate; A lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; The piezoelectric constant e of the piezoelectric film 31 is 10 C / m 2 That's all. When a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film provided on the piezoelectric film at a temperature of 200° C., the leakage current density flowing through the piezoelectric film from the start of application of the negative voltage is 30 mA / cm 2 The time it takes to exceed this limit is 5 hours or more, The membrane stress of the piezoelectric film is 150 MPa or less. Piezoelectric stack.

2. 2. The piezoelectric stack of claim 1, wherein when a negative AC voltage is continuously applied to the upper electrode film so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and the upper electrode film, the number of cycles of application of the voltage until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.

3. 3. The piezoelectric stack according to claim 1, wherein the piezoelectric film contains at least one element selected from copper and manganese as a dopant at a concentration of 0.1 at % to 2.0 at %.

4. forming a lower electrode film on a substrate; forming a piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen on the lower electrode film; In the step of forming the piezoelectric film, first, a first piezoelectric film, which is a part of the piezoelectric film, is formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then a second piezoelectric film, which is the other part of the piezoelectric film, is formed at a first temperature at which the piezoelectric constant e 31 is 10 C / m 2or more, and when a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film formed on the second piezoelectric film, the leakage current density flowing through the second piezoelectric film is 30 mA / cm 2 A film is formed on the first piezoelectric film at a second temperature at which the time until the temperature exceeds the second temperature is 5 hours or more. A method for manufacturing a piezoelectric laminate.

5. A substrate; A lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; an upper electrode film formed on the piezoelectric film; The piezoelectric constant e of the piezoelectric film 31 is 10 C / m 2 That's all. When a negative voltage is applied to the upper electrode film so as to generate an electric field of 300 kV / cm between the lower electrode film and the upper electrode film at a temperature of 200° C., the leakage current density flowing through the piezoelectric film from the start of application of the negative voltage is 30 mA / cm 2 The time it takes to exceed this limit is 5 hours or more, A piezoelectric element, wherein the piezoelectric film has a film stress of 150 MPa or less.

6. 6. The piezoelectric element of claim 5, wherein when a negative voltage is continuously applied to the upper electrode film so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and the upper electrode film, the number of cycles of application of the voltage until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.

Citation Information

Patent Citations

  • Piezoelectric thin-film device, piezoelectric sensor, and vibration power generator

    JP2014207429A

  • Piezoelectric elements, piezoelectric actuators, hard disk drives, inkjet printers, and piezoelectric sensors

    JP2015529963A

  • Piezoelectric thin film-attached laminate board, piezoelectric thin-film device and manufacturing method thereof

    JP2017076730A

  • Piezoelectric laminate, piezoelectric element, and manufacturing method of piezoelectric laminate

    JP2021012909A

  • sputtering target material

    JP2022165896A