Polyester monofilament

JP2024141435AInactive Publication Date: 2024-10-10TORAY INDUSTRIES INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023053088
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Benefits of technology

【0009】 本発明は、高強度·高モジュラスで、繊維径均一性に優れ、スクリーン紗の染色工程を不要とし、ハレーションを防止する発色性を有する高精細スクリーン印刷用途に好適なスクリーン紗を得ることができるポリエステルモノフィラメントを提供できる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141435000001_ABST
    Figure 2024141435000001_ABST
Patent Text Reader

Abstract

To provide a monofilament suitable for a high-definition screen printing application, which has a high strength and a high modulus, has excellent fiber diameter uniformity, does not require a screen dyeing process, and is capable of preventing halation.SOLUTION: There is provided a monofilament, where the monofilament contains 0.01 to 0.1 wt% of an organic coloring agent and 0.1 to 0.5 wt% of an inorganic non-white coloring agent based on a total weight of the filament; an average reflectance for light with a wavelength of 250 nm to 450 nm is 15% or less; and a fineness is 13.0 dtex or less and a strength is 6.0 cN / dtex or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester monofilament for screen printing. [Background technology]

[0002] As a screen printing fabric, a mesh fabric made of natural fibers such as silk or inorganic fibers such as stainless steel, that is, a screen gauze, has been widely used. In recent years, synthetic meshes, which are excellent in flexibility, durability, and cost performance, have been used favorably. Among them, screen gauze obtained by weaving polyester monofilament is highly suitable for screen printing applications, such as excellent dimensional stability, and is widely used. In the electronics field, which has been growing rapidly in recent years, the printing accuracy of circuit patterns for electronic devices such as home appliances, mobile phones, and personal computers has become stricter, and higher-definition pattern printing is required. In order to obtain high-definition pattern printing, a polyester monofilament with high strength, high modulus, and excellent fiber diameter in the longitudinal direction, i.e., fiber diameter uniformity, is required.

[0003] In the general plate-making process using a screen gauze, a screen gauze made of monofilament is stretched and fixed on a frame, refined to remove unnecessary substances such as oil adhering to the monofilament, then UV-curable resin is applied and dried, and then the screen gauze is brought into close contact with a positive film with a black pattern to be printed, and exposed to UV rays with a wavelength of 250 to 450 nm. At this time, the UV-curable resin that overlaps with the patterned part of the positive film does not solidify, but the other parts are exposed to UV light and solidify through a photochemical reaction, so by washing the plate after exposure with water, the UV-curable resin in the patterned part of the positive film is washed away, creating a printing negative.

[0004] In screen printing, in order to perform more precise and fine printing, it is important to solidify the ultraviolet curable resin according to the pattern design of the positive film. For example, if the ultraviolet reflectance of the screen gauze is high, the ultraviolet light is diffusely reflected on the surface of the screen gauze, and even the pattern parts that do not need to be exposed are exposed to light, which causes so-called halation, and the printing accuracy is significantly reduced. As a method for preventing the diffuse reflection of ultraviolet light, a method of dyeing after weaving the screen gauze with monofilaments is adopted, but the addition of the dyeing process has disadvantages such as increased manufacturing costs and reduced strength of the raw yarn during dyeing processing. In order to eliminate this dyeing process, various studies have been conducted on monofilaments for screen gauze that are mixed with colorants at the spinning process stage, and Patent Documents 1 and 2 disclose inventions in which an organic colorant is incorporated into polyester monofilaments. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-90758 A [Patent Document 2] WO2005 / 118927 publication Summary of the Invention [Problem to be solved by the invention]

[0006] In order to eliminate the dyeing process of the screen gauze, it is necessary to mix a colorant in the spinning process and melt spin the yarn to obtain a dyed yarn. There are organic and inorganic colorants, but since organic colorants have better color development, Patent Documents 1 and 2 both propose dyed yarns using organic colorants. However, when organic colorants are retained in the polymer pipe for a long time in the melt spinning process, there is a problem that gelled matter is generated due to thermal deterioration of the colorant. Since the gelled matter inhibits the extension of the yarn, localized expansion of the fiber diameter (hereinafter, knots) occurs in the gelled matter-containing part. Since the knots impair the uniformity of the fiber diameter of the yarn and induce printing defects when used as a screen gauze, it is necessary to eliminate them as much as possible. On the other hand, inorganic colorants are less likely to gel due to heat compared to organic colorants, but they have inferior color development and it is difficult to produce the necessary color development to prevent halation. Furthermore, when a large amount of colorant is added to enhance color development, there remains a problem that it may cause poor polymer discharge during melt spinning and deteriorate the physical properties of the yarn.

[0007] The present invention aims to provide a monofilament for screen gauze which has high strength and high modulus, excellent fiber diameter uniformity, does not require a screen gauze dyeing process, and has excellent color development properties that prevent halation, making it suitable for high-definition screen printing applications. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention has the following configuration. That is, it is a polyester monofilament characterized by containing 0.01 to 0.1 wt% of an organic colorant and 0.1 to 0.5 wt% of an inorganic colorant other than a white colorant, having an average reflectance of 15% or less for light with a wavelength of 250 nm to 450 nm, a fineness of 13.0 dtex or less, and a strength of 6.0 cN / dtex or more. Also, it is a core-sheath composite monofilament in which both the core and sheath components are made of polyester, the core component contains 0.01 to 0.1 wt% of an organic colorant and 0.1 to 0.5 wt% of an inorganic non-white colorant, the sheath component does not contain an inorganic non-white colorant, the average reflectance of 15% or less for light with a wavelength of 250 nm to 450 nm, a fineness of 3.0 to 13.0 dtex, and a strength of 6.5 to 9.0 cN / dtex. Effect of the Invention

[0009] The present invention can provide a polyester monofilament which has high strength and high modulus, excellent fiber diameter uniformity, does not require a screen gauze dyeing process, and can provide a screen gauze suitable for high-definition screen printing applications having color development that prevents halation. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a schematic diagram showing a continuous chart of fiber diameters obtained by a fiber diameter measuring device (the horizontal axis is time, and the vertical axis is fiber diameter). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The polyester monofilament of the present invention will be described below.

[0012] The cross-sectional shape of the polyester monofilament of the present invention may be a circle, flat, triangular, square, pentagonal, etc., but a circle cross-section is preferred from the viewpoint of uniformity of the mesh size of the screen gauze. The monofilament of the present invention may be a single-component monofilament made of one polymer component, or a core-sheath composite monofilament made of two polymer components, a core component and a sheath component. The present invention is not limited to either of these forms, but in the case of a core-sheath composite monofilament, the core component is covered and arranged with the sheath component, and only the core component contains a light absorbing substance (hereinafter, a colorant), and further, the core component is arranged with a polyester having a high intrinsic viscosity, and the sheath component is arranged with a polyester having an intrinsic viscosity lower than that of the core component, which is preferable because it can exhibit better abrasion resistance, high strength, and high modulus properties. Here, it is sufficient that the core component is completely covered with the sheath component, and it is not necessarily required to be arranged in a concentric shape, but a concentric shape is more preferable. In the case of a core-sheath composite monofilament, the area ratio of the core component to the sheath component is preferably 70:30 to 90:10, more preferably 80:20 to 90:10. If the core component is less than 70%, sufficient strength and modulus cannot be obtained. Conversely, if the sheath component ratio is less than 10%, the core component may be exposed by scraping during weaving, and abrasion resistance may be impaired.

[0013] The polyester used for the polyester monofilament of the present invention can be polyethylene terephthalate, which has terephthalic acid as the main acid component and ethylene glycol as the main glycol component, and is composed of 90 mol % or more of ethylene terephthalate repeating units.

[0014] However, it may contain a copolymerization component capable of forming other ester bonds at a ratio of less than 10 mol %. Examples of such copolymerization components include, for example, difunctional aromatic carboxylic acids such as isophthalic acid, phthalic acid, dibromoterephthalic acid, naphthalene dicarboxylic acid, and octoethoxybenzoic acid as acid components, difunctional aliphatic carboxylic acids such as sebacic acid, oxalic acid, adipic acid, and dimer acid, and dicarboxylic acids such as cyclohexane dicarboxylic acid. Examples of glycol components include ethylene glycol, diethylene glycol, propanediol, butanediol, neopentyl glycol, bisphenol A, cyclohexane dimethanol, and polyoxyalkylene glycols such as polyethylene glycol and polypropylene glycol.

[0015] The polyester used in the present invention may contain, as required, a white colorant (matte agent) such as titanium dioxide, fine particles of silica or alumina or the like as a lubricant, a hindered phenol derivative as an antioxidant, and further a flame retardant and an antistatic agent.

[0016] As a result of our investigations into achieving both a color that prevents halation and the quality required for a monofilament suitable for high-definition screen printing applications, we discovered that by mixing and incorporating a specified amount of organic colorant and inorganic colorant, we can obtain a monofilament that is suitable for high-definition screen printing applications, which achieves both prevention of halation and knot quality.

[0017] Organic colorants are organic compounds with at least one unsaturated end. The π electrons at the unsaturated end absorb visible light and become excited from the ground state to produce color, so they are characterized by a darker color than inorganic colorants. However, organic colorants have structures with weak bond energy, such as unsaturated ends and carbon single bonds, so they are prone to deterioration due to heat and oxygen. In particular, when spinning monofilaments with low output, they are exposed to heat for a long time during the spinning process, so deterioration is more noticeable. In contrast, inorganic colorants are made of oxides obtained by chemical reactions of natural minerals and metals. Inorganic colorants have excellent heat resistance but weak color development, so in order to obtain a sufficient color to prevent halation, it is necessary to contain a large amount of colorant compared to organic colorants. However, colorants are foreign substances to the molecular chains of polyester, so if a large amount of colorant is contained, it will induce a decrease in the strength of the monofilament and a deterioration in its abrasion resistance.

[0018] The content of colorants in the polyester monofilament of the present invention is 0.01 to 0.1 wt% of organic colorants and 0.1 to 0.5 wt% of inorganic colorants excluding delustering agents (white colorants) such as titanium dioxide, relative to the monofilament in the case of a single component monofilament, and 0.1 to 0.5 wt% of inorganic colorants excluding delustering agents (white colorants) such as titanium dioxide, relative to the core component in the case of a core-sheath composite monofilament. More preferably, the content of organic colorants is 0.05 to 0.1 wt%, and the content of inorganic colorants is 0.3 to 0.5 wt%. In the case of a core-sheath composite monofilament, the core component contains organic colorants and inorganic colorants excluding the white colorant, while the sheath component may contain a white colorant, but does not contain any colorants other than the white colorant.

[0019] If the organic colorant is less than 0.01 wt%, the color cannot be sufficiently strong to prevent halation. Conversely, if the content is more than 0.11 wt%, the colorant deteriorates, causing many knots and impairing the uniformity of the fiber diameter of the yarn. Even if the concentration of the organic colorant is 0.01 to 0.1 wt%, if the content of the inorganic colorant is less than 0.1%, the color cannot be sufficient to prevent halation, and conversely, if the content exceeds 0.5 wt%, the yarn strength required for high-definition screen printing applications cannot be obtained.

[0020] The knots caused by the deterioration of organic colorants occur more significantly when the yarn has a lower fineness and is exposed to heat for a longer period during the spinning process, and when a polymer with a higher viscosity is used to increase the strength of the yarn, it is important to mix organic and inorganic colorants to balance the color and quality of the yarn when spinning polyester monofilaments with a fineness of 13.0 dtex or less and a strength of 6.5 cN / dtex or more, especially with a fineness of 8.0 dtex or less and a strength of 7.0 cN / dtex or more. The organic and inorganic colorants used can be any known colorant, and may be appropriately selected depending on the compatibility with the ultraviolet curing resin. In general, warm colors such as red and yellow are preferably used for screen gauze, since they have good absorption of visible light at higher wavelengths and ultraviolet light. Specifically, organic colorants include azo colorants, anthraquinone-based, and isoindoline-based condensed polycyclic colorants, while inorganic colorants include cadmium-based, titanium-based, and lead-based colorants. In the present invention, taking into consideration the color and thermal degradation characteristics of each colorant, 2 wt% of Pigment Yellow 150 (CAS No.: 68511-62-6, chemical formula: C8H6N6O6) or Pigment Yellow 147 (CAS No.: 4118-16-5, chemical formula: C 37 H 21It is preferable to use Pigment Yellow 150 (CAS No.: 1310-39-0, chemical formula: (Fe,Al)2TiO5) as an inorganic colorant, but from the viewpoint of thermal degradation characteristics, it is more preferable to use Pigment Yellow 150. As for inorganic colorants, it is preferable to use Pigment Brown 48 (CAS No.: 1310-39-0, chemical formula: (Fe,Al)2TiO5) as a colorant, from the viewpoint of obtaining a warm color tone with good ultraviolet absorption.

[0021] The polyester monofilament of the present invention has an average reflectance of 15.0% or less, more preferably 13.0% or less, and even more preferably 10.0% or less, for light having a wavelength of 250 nm to 450 nm. The average reflectance in the present invention refers to a value measured by the measurement method described in the Examples section. In forming a print pattern, a print pattern is reproduced with high resolution using an ultraviolet curable resin, and when ultraviolet light is cured using a photosensitive resin in the plate making process, ultraviolet light having a wavelength of 250 to 450 nm is often irradiated according to the photolithography method (JIS Z8788:2009), and it is important to suppress reflection of wavelengths in this range in order to prevent halation. If the average reflectance in the above-mentioned wavelength range is 15.0% or less, reflection of ultraviolet light can be suppressed, no halation occurs, and a clear print pattern can be obtained. If the average reflectance exceeds 15.0%, sufficient halation prevention effect cannot be obtained, ultraviolet light is diffusely reflected on the gauze surface, and even the pattern parts that do not need exposure are exposed to light, causing bleeding of the print pattern. In particular, in recent years, the use of low-wavelength ultraviolet light of 250 to 350 nm, which has greater energy than the conventionally used ultraviolet light of 350 to 450 nm, has been increasing because it can shorten the curing time of the resin, and a screen gauze with a lower reflectance in a wider ultraviolet wavelength range is required. In order to reduce the reflectance in a wider wavelength range, it is effective to mix colorants of different colors. In the present invention, for example, by mixing an inorganic colorant Pigment Brown 48, which develops a slightly brownish yellow color, together with a yellow organic colorant, it is possible to reduce not only the reflectance in the range of 350 to 450 nm, but also the reflectance in the range of 250 to 350 nm. The colorants to be mixed and used do not necessarily have to be limited to two types, and may be appropriately selected to obtain the required reflectance characteristics.

[0022] The polyester monofilament of the present invention has a fineness of 3.0 to 13.0 dtex, more preferably 3.0 to 8.0 dtex. By setting the fineness within this range, a screen gauze suitable for high-precision printing can be obtained. If the fineness is greater than 13.0 dtex, a high-mesh screen gauze cannot be obtained, and printing precision is poor. The lower limit of the fineness is 3.0 dtex in terms of weaving properties, particularly the flying property of the weft in a sluzer-type loom. Furthermore, by reducing the fineness, the size ratio of the deteriorated gelled matter to the fiber diameter increases relatively. Therefore, the gelled matter appears as knots, so that printing defects increase and printing precision decreases.

[0023] In screen printing, in order to improve the accuracy of the printing pattern, a method is generally adopted in which the tension of the screen is increased and the distance between the screen and the printed material is reduced. In order to increase the tension during the screen stretching, it is necessary to improve the strength of each monofilament. In particular, the requirements for a high-precision printing screen gauze are strict, and high mesh, i.e., mesh fabric with high weaving density, are required. The tension applied to the thread during the weaving process is not necessarily proportional to its fineness, and it is necessary that the strength of each monofilament is high. The thinner the monofilament, the lower the strength, so it is necessary to make it stronger. Therefore, it is important that the strength (breaking strength) of the polyester monofilament of the present invention is 6.5 to 9.0 cN / dtex. If the strength is less than 6.5 cN / dtex, the gauze will elongate after stretching, the dimensional stability will decrease, and the mesh will be easily misaligned, which will impair the uniformity of the mesh opening. In addition, the strength of the screen gauze will be insufficient. In the case of a high-mesh screen gauze for high-precision printing, it is preferable that the strength is 7.0 cN / dtex or more. The upper limit of the strength is 9.0 cN / dtex or less, since it is necessary to suppress the orientation and crystallinity from the viewpoint of scum resistance.

[0024] The modulus at 10% elongation of the polyester monofilament of the present invention (hereinafter referred to as 10% modulus) is preferably 5.0 to 8.5 cN / dtex. In order to suppress the occurrence of gauze elongation after stretching, to suppress the decrease in dimensional stability of the screen gauze, to suppress the occurrence of misalignment, and to ensure uniformity in the mesh opening, the 10% modulus is preferably 5.0 cN / dtex or more. More preferably, the strength at 10% elongation is 5.5 cN / dtex or more. The upper limit of the 10% modulus is preferably 8.5 cN / dtex or less, since it is necessary to suppress the orientation and crystallinity from the viewpoint of scum resistance.

[0025] In addition, since the screen gauze for high-definition screen printing is a woven fabric with a short mesh spacing, even if knots are formed, it is necessary to make the diameter of the knots as small as possible and to reduce the number of knots. Conventionally, the number of knots was determined by passing the monofilament through a slit guide with a size 1.1 times the fiber diameter, but as a result of intensive research to obtain a higher degree of uniformity in fiber diameter, it was found that when the diameter and number of knots of the present invention are within a specific range, the variation in mesh openings when made into a gray fabric is reduced, and a screen gauze with excellent printing accuracy can be obtained. That is, it is preferable that the polyester monofilament of the present invention has a sum Z (%) of the increase rate of the diameter of the knots (the increase rate from the average diameter) represented by formula (1) for the knots at 110% of the average fiber diameter present in 1 million m of the fiber longitudinal direction of the monofilament, i.e., the knots having a fiber diameter of 110% or more of the average fiber diameter, is less than 30,000.

[0026]

number

[0027] X n : diameter of nth node, X': average fiber diameter, k: number of nodes contained in 1 million meters in the longitudinal direction of the fiber (here, a node refers to a node having a fiber diameter of 110% or more of the average fiber diameter). Z is the diameter of the node at the mean fiber diameter X' nThe value of Z increases when large knots are present. Z is the diameter of the knots present in 1 million meters in the longitudinal direction of the fiber, X n The increase rate of each of the nodes is added together, and the value of Z increases when there are many nodes. In other words, it is important that the node diameter is small and the number of nodes is small. When Z is less than 30,000, the composite polyester monofilament of the present invention has good uniformity of the monofilament, and when it is made into a green fabric, a high mesh screen gauze with excellent uniformity of mesh opening can be obtained. Z is preferably 20,000 or less, more preferably 10,000 or less. Next, a preferred method for producing the core-sheath type composite monofilament of the present invention will be described.

[0028] The intrinsic viscosity of the polyester of the polyester monofilament of the present invention is preferably 0.70 to 1.50. By setting the intrinsic viscosity to 0.70 or more, a polyester monofilament having both high strength and modulus can be obtained. The upper limit of the intrinsic viscosity is preferably 1.50 or less from the viewpoint of ease of molding such as melt extrusion, and more preferably 0.90 to 1.30 in consideration of the manufacturing cost and the influence of molecular weight reduction due to molecular chain scission caused by heat and shear force during the process. When obtaining a core-sheath composite polyester monofilament, it is preferable to use a polyester having a lower intrinsic viscosity than the core component in the sheath component, since this will exhibit further abrasion resistance, high strength and high modulus properties compared to a single component yarn. The intrinsic viscosity of the sheath component polyester is preferably 0.40 to 0.70. When the intrinsic viscosity of the sheath component polyester is 0.40 or more, the degree of orientation and crystallinity of the fiber surface of the monofilament can be suppressed, and good abrasion resistance can be obtained. A more preferable intrinsic viscosity is 0.45 or more. In order to obtain good abrasion resistance, the upper limit of the intrinsic viscosity is preferably 0.70 or less.

[0029] Next, a method for producing the polyester monofilament of the present invention will be described. The polyester monofilament of the present invention is obtained by melt spinning, by melting a polymer, sending it to a spinning pack, filtering the polymer in the spinning pack, and then spinning it. As a filtering method, it is preferable to filter in a melt spinning pack in which a nonwoven fabric filter layer (hereinafter, gel capture filter) formed by sintering a web of stainless steel fibers opened to a cotton-like shape at high temperature and a filter layer (hereinafter, gel fragmentation filter) formed by sintering metal short fibers having a polygonal cross section are installed. The two types of filter layers with different cross sections of the metal short fibers enable the capture and fragmentation of gel-like matter generated in the molten polymer, and the diameter and number of nodes can be reduced (Z<30,000 is satisfied), resulting in good uniformity of the monofilament. The filtration accuracy of the gel fragmentation filter is 40 μm or less. By setting it in this range, the diameter and number of nodes satisfy Z<30,000, resulting in good uniformity of the monofilament. If the filtration accuracy is too low and exceeds 40 μm, the size of the gel-like matter that passes through without being broken down will become large, and the amount of the gel-like matter will increase, so the diameter and number of the nodes will not satisfy Z<30,000, and the uniformity of the monofilament cannot be obtained. A filtration accuracy of 40 μm means that the filter has the ability to remove 98% or more of gel-like matter (foreign matter) of 40 μm or more. More preferably, it is 30 μm or less. In addition, the upper limit of the preferred filtration accuracy is 5 μm or more, taking into consideration that abnormal retention occurs due to clogging in the filter, and the gel-like matter is cut and broken down, and the gel-like matter is broken down in an insufficient manner, and further, 7 μm or more from the viewpoint of pack pressure. In addition, by making the thickness of the gel-breaking filter 2 mm or more, the filtration flow path becomes long, a sufficient gel-like matter is broken down, the diameter and number of the nodes satisfy Z<30,000, and the monofilament is well uniform. If the thickness is less than 2 mm, the filtration flow path becomes short, the gel-like material cannot be sufficiently broken down, the diameter and number of nodes do not satisfy Z<30,000, and the monofilament cannot be uniform. In addition, although the gel-like material can be broken down more effectively by increasing the thickness, the packing pressure also increases, so the upper limit of the preferable thickness is 3 mm or less from the viewpoint of packing pressure.Next, the filtration accuracy of the gel trapping filter is 10 μm or less. By setting it in this range, the diameter and number of the nodes satisfy Z<30,000, and the uniformity of the monofilament is good. If the filtration accuracy exceeds 10 μm, the size of the gel-like matter that passes without being captured becomes large and the amount increases, so that the diameter and number of the nodes do not satisfy Z<30,000, and the uniformity of the monofilament cannot be obtained. More preferably, it is 7 μm or less. In addition, the upper limit of the preferable filtration accuracy is preferably 5 μm or more, considering that abnormal retention occurs due to clogging in the filter and the capture effect of the gel-like matter becomes insufficient. In addition, from the viewpoint of pack pressure, it is preferable that it is 5 μm or more. It is more preferable to use a filter with a smaller filtration accuracy than the gel fragmentation filter, which is mainly intended for the fragmentation effect of the gel-like matter. By setting the thickness of the gel trapping filter to 2 mm or more, the filtration flow path becomes long, a sufficient capture effect of the gel-like matter is obtained, the diameter and number of the nodes satisfy Z<30,000, and the uniformity of the monofilament is good. If the thickness is less than 1 mm, the filtration flow path becomes short, the gel capturing effect is insufficient, the diameter and number of nodes do not satisfy Z<30,000, and the monofilament cannot be uniform. In addition, although the gel capturing effect is improved by increasing the thickness, the pack pressure also increases, so the upper limit of the preferable thickness is 1.4 mm or less from the viewpoint of pack pressure.

[0030] The two types of filter layers, each having a different cross-sectional shape of the short metal fibers, each exert a different effect of "capturing" and "fragmenting" the gel-like material. Therefore, the order of the filter layers does not greatly affect the effect, but it is more preferable to install the gel-capturing filter upstream.

[0031] To obtain the polyester monofilament of the present invention, a composite spinning machine is used to melt the polyesters of the core component and the sheath component, and a specified amount is sent to a composite spinning pack by a metering pump through the respective polymer pipes of the core component and the sheath component, and after filtering both polymers in the spinning pack, the polyesters are compositely spun into a core-sheath cross-sectional shape by a spinneret. The polyester monofilament can be produced by any of the following methods: a two-step method in which the yarn discharged from the spinneret is once wound up as an undrawn yarn and then drawn, and a direct spinning and drawing method in which the yarn discharged from the spinneret is continuously drawn without once being wound up. However, a direct spinning and drawing method in which drawing is performed directly in connection with the spinning process is preferred from the viewpoints of reducing the number of guides through which the yarn passes during the production process and suppressing yarn shaving.

[0032] Methods for adding organic compound pigments and inorganic particles include a method of melt-spinning pellets obtained by adding a specified organic compound pigment and inorganic particles to polyester using the above-mentioned method, a method of making high-concentration master pellets of about 2 to 20 times the specified content, melt-kneading and diluting with normal polyester, and spinning, etc. In the latter case, the master pellets and normal polyester pellets may be mixed in a pellet state and kneaded in a melt extruder, or they may be melted in separate melt extruders and then kneaded in a molten polymer transport pipe or spinning pack, and in either case, a static kneader may be used to ensure uniform dispersion of the organic compound pigments and inorganic particles.

[0033] The monofilament of the present invention thus obtained has high strength and high modulus, excellent fiber diameter uniformity, and excellent color development properties that prevent halation, making the screen gauze dyeing process unnecessary, and is therefore extremely suitable as a constituent material for screen gauze. EXAMPLES

[0034] The polyester monofilament of the present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. The measurements in the examples were measured by the following methods.

[0035] 1. Diameter and number of knots Monofilament is inspected by an optical outer diameter inspection device (PSD-200 manufactured by Sensoptic). The fiber diameter was measured at 0.06 mm intervals along the length of the fiber while unwinding the yarn at a speed of 750 m / min with a sampling frequency of 200,000 times / sec. Figure 1 shows a schematic diagram of the fiber diameter chart obtained. The horizontal axis represents time and the vertical axis represents fiber diameter, and the fiber diameter obtained by the fiber diameter measuring device is continuously shown as a chart. The point at which the fiber diameter value 1 obtained by the fiber diameter measuring device exceeds a threshold value 3, which is 10% higher than the average fiber diameter 2, is defined as the start point 4 of the node portion, and the point at which 0.1 s has elapsed since the fiber diameter value fell below the threshold value is defined as the end point 5 of the node portion. The largest fiber diameter value 6 between the start point 4 and the end point 5 is defined as the diameter of the node. Measurements are performed for 1 million m of the yarn length, and the total value (%) is calculated using formula (1). The smaller the value of formula (1), the better the knot quality of the monofilament.

[0036] X n : node diameter, X': average fiber diameter, k: number of nodes in 1 million meters in the longitudinal direction of the fiber

[0037]

number

[0038] 2. Monofilament fineness (dtex) A 500 m length of monofilament was reeled off, and the mass (g) of the reel was multiplied by 20 to obtain the fineness.

[0039] 3. Monofilament breaking strength (cN / dtex), 10% modulus (cN / dtx), and residual elongation (%) Using an Orientex Tensilon tensile testing machine, the monofilament was measured five times with an initial sample length of 20 cm and a tensile speed of 20 cm / min. From the results, the breaking strength (cN / dtex), residual elongation (%), and strength at 10% elongation (10% modulus, cN / dtex) were calculated.

[0040] 4. Intrinsic viscosity of polyester chips The definition formula for ηr was calculated by dissolving 0.8 g of polyester chips in 10 mL of o-chlorophenol (hereinafter referred to as OCP) with a purity of 98% or higher at 25°C, and calculating the relative viscosity ηr using an Ostwald viscometer at 25°C using the following formula to calculate the intrinsic viscosity. ηr=η / η0=(t×d) / (t0×d0) Intrinsic viscosity=0.0242ηr+0.2634 Here, η is the viscosity of the polymer solution, η0 is the viscosity of the OCP, t is the time it takes for the solution to fall (sec), and d is the density of the solution (g / cm 3 ), t0: OCP fall time (sec), d0: OCP density (g / cm 3 ).

[0041] 5.Average reflectance 10,000 m of polyester monofilament was wound tightly around a plate measuring 6 cm in length and 6 cm in width, and the reflectance was measured at 10 nm intervals between 250 and 450 nm wavelengths using a JASCO Corporation V750 spectrophotometer in accordance with photolithography (JIS Z8722:2009). The measured values ​​were averaged to obtain the average reflectance.

[0042] 6.Weavability The following screen gauze (#350) was woven using polyester monofilaments of each of the Examples and Comparative Examples of the present invention for both warp and weft threads on a Sluzer type loom at a loom speed of 200 rpm. Line density: 350 strands / 2.54cm Latitudinal density: 350 lines / 2.54cm.

[0043] The state of dirt on the reed was noted at that time and judged using the following criteria, with a grade of B or above being considered a pass. S: Very good (almost no scum stains) A: Good (slight staining of the reed due to scum is observed, but the impact is minor) B: Fair (there is some scum on the reed, but it is at an acceptable level) C: Inferior (Continuous weaving is difficult due to reed stains caused by scum) D: Extremely poor condition (weaving is impossible due to significant reed staining caused by scum).

[0044] 7.Halation evaluation The polyester monofilaments of the examples and comparative examples of the present invention were used for both the warp and weft. The following screen gauze (#350) was woven using a sulzer type loom at a rotation speed of 200 rpm. Line density: 350 strands / 2.54cm Latitude density: 350 lines / 2.54cm.

[0045] After that, a line pattern of 50 μm at 50 μm intervals was printed onto the screen gauze, and the product was observed and evaluated under an electron microscope, with a grade of B or above being considered a pass. S: Extremely good (extremely effective in preventing halation. Almost no bleeding of fine patterns) A: Good (great anti-halation effect, slight bleeding of fine patterns) B: Fair (a certain level of anti-halation effect is obtained, and although there is bleeding of fine patterns, it is at an acceptable level) C: Inferior (halation prevention effect is insufficient, and bleeding of fine patterns is observed) D: Extremely poor (a large amount of fine pattern bleeding is observed due to halation).

[0046] 8.Printing accuracy The following screen gauze (#350) was woven using polyester monofilaments of each of the Examples and Comparative Examples of the present invention for both warp and weft threads on a Sluzer type loom at a loom speed of 200 rpm. Line density: 350 strands / 2.54cm Latitude density: 350 lines / 2.54cm.

[0047] After that, a pattern of 50 lines spaced 50 μm apart was formed on the resulting mesh fabric using a photosensitive emulsion, and the printed condition was checked and evaluated by a skilled inspection technician, with a grade of B or above being deemed a pass. S: Very good (line pattern reproduction is very good) A: Good (There are minor printing defects, but it is sufficiently suitable for high-definition screen printing applications) B: Fair (some printing defects are visible, but are at an acceptable level) C: Inferior (due to uneven openings or deformation of the yarn during stretching, the reproducibility of lines is poor, and it cannot be used for high-definition screen printing applications) D: Extremely poor (there are many uneven openings or the yarn is significantly deformed during stretching, resulting in extremely poor line reproducibility and making it impossible to apply to screen printing).

[0048] Example 1 A polyethylene terephthalate chip having an intrinsic viscosity of 0.70 and containing 0.1 wt% titanium oxide as a matting agent was coated with 2 wt% of an organic colorant, Pigment Yellow 150 (CAS No.: 68511-62-6, chemical formula: C8H6N6O6), and 2 wt% of an inorganic colorant, Pigment Brown 48 (CAS A master chip was obtained by mixing 8 wt% of 1310-39-0 (chemical formula: (Fe,Al)2TiO5). In order to obtain a core-sheath composite monofilament, 5.0 wt% of the master chip was mixed with polyethylene terephthalate chips (hereinafter referred to as the main material) containing 0.5 wt% titanium oxide as a matting agent (white coloring agent) and an intrinsic viscosity of 1.20 as the core component, and the master chip was fed to an extruder and melted at a temperature of 297°C. In addition, polyethylene terephthalate chips containing 0.4 wt% titanium oxide as a matting agent (white coloring agent) and an intrinsic viscosity of 0.51 as the sheath component were melted at a temperature of 297°C using another extruder. After melting using the extruder, the polymer was metered by pump so that the core-sheath ratio was 80:20 at a polymer temperature of 275 to 285°C, and the mixture was allowed to flow into a melt spinning pack. Melt spinning pack The gel-like matter generated by the thermal degradation of the polymer was broken down by passing through a gel-fragmentation filter (filtration accuracy 40 μm, thickness 2 mm) layer made of sintered metal short fibers having a polygonal cross section installed in the inside of the gel-fragmentation filter, and the gel-like matter that could not be broken down by the gel-fragmentation filter was passed through a gel-capturing filter (filtration accuracy 10 μm, thickness 1.4 mm) layer made of sintered metal short fibers having a circular cross section installed downstream of the gel-fragmentation filter, so that the gel-like matter was sufficiently captured. Thereafter, the yarn was made to flow into a known composite spinneret so as to have a core-sheath type, and a yarn was spun out. The monofilament discharged from the spinneret was actively heated and kept warm so that the atmospheric temperature immediately below the spinneret was 300°C, and then cooled by a yarn cooling blower, and while applying a spinning oil, it was taken up by an unheated first godet roll at a speed of 611 m / min. The glass transition temperature of this undrawn yarn was 80°C.Without being wound once, the filament was drawn around a first hot roll heated to 90°C at a speed of 615 m / min, a second hot roll heated to 90°C at a speed of 2,096 m / min, and a third hot roll heated to 190°C at a speed of 2998 m / min, and then drawn and heat-set. The draw ratio was 5.11 times. After drawing around an unheated godet roll at a speed of 2998 m / min, the spindle rotation speed was controlled so that the winding tension was 0.417 g / dtex, and the filament was wound around a package to obtain a concentric core-sheath composite polyester monofilament of 8.0 dtex. The properties of the polyester monofilament are shown in Table 1, and excellent weavability, halation suppression effect, and printing accuracy for high-definition screen printing applications were obtained.

[0049] (Examples 2 and 3) Polyester monofilaments having finenesses of 3.0 and 13.0 dtex were obtained in the same manner as in Example 1, except that the discharge amount was changed as shown in Table 1. The properties of the polyester monofilaments are shown in Table 1. All of them had sufficient weaving properties, halation suppression effect, printing accuracy, and fiber diameter uniformity. In Example 2, knots were more likely to occur due to the thinner fiber diameter, and printing accuracy was slightly worse than in Example 1, but the level was acceptable for application to high-definition screen printing applications.

[0050] Comparative Example 1 A polyester monofilament having a fineness of 8.0 dtex was obtained in the same manner as in Example 1, except that the master batch was not mixed into the main material. The properties of the polyester monofilament are shown in Table 1. Compared to Example 1, the strength and modulus were increased, and the deformation of the yarn during stretching could be further suppressed, but the frequent bleeding of fine patterns due to halation made it impossible to apply the polyester monofilament to high-definition screen printing applications.

[0051] [Table 1]

[0052] (Examples 4 and 5) A polyester monofilament was obtained in the same manner as in Example 1, except that the intrinsic viscosity of the main material of the core component was 1.40 (Example 4) or 1.00 (Example 5). The properties of the polyester monofilament are shown in Table 2.

[0053] In Example 4, by increasing the viscosity of the polymer of the main material, the strength and modulus increased and high tensioning stability was obtained. On the other hand, the number of knots increased slightly and printing accuracy deteriorated slightly, but it was at a level that was acceptable for application to high-definition screen printing applications. In Example 5, by decreasing the viscosity of the polymer of the main material, good weaving properties were obtained, but the printing accuracy also decreased due to the decrease in tensioning stability, but it was still at a level that was acceptable for application to high-definition screen printing applications. Comparative Example 2 A polyester monofilament was obtained in the same manner as in Example 1, except that the intrinsic viscosity of the main material of the core component was 0.70. The properties of the polyester monofilament are shown in Table 2. By significantly lowering the polymer viscosity of the main material, the amount of weaving scum generated during weaving was significantly reduced, and extremely good weaving properties were obtained. The significant decrease in the gauze tension stability led to a deterioration in printing accuracy, making it impossible to apply the product to high-definition screen printing applications.

[0054] Comparative Example 3 A polyester monofilament was obtained in the same manner as in Comparative Example 2, except that the draw ratio was set to 6.0 times. The properties of the polyester monofilament are shown in Table 2. While the printing accuracy was improved, the weaving properties were extremely deteriorated due to the scraping of the yarn during weaving, making it impossible to apply the polyester monofilament to high-definition screen printing applications.

[0055] [Table 2]

[0056] Example 6 A polyester monofilament was obtained in the same manner as in Example 5, except that only the core component was extruded and the amount of master batch mixed into the main material was changed to 2.5% to obtain a single-component polyester monofilament having a fineness of 8.0 dtex. The properties of the polyester monofilament are shown in Table 3. Compared to Example 5, the weavability was slightly worse, but was at a level acceptable for application to high-definition screen printing applications.

[0057] Example 7 A polyester monofilament was obtained in the same manner as in Example 5, except that the masterbatch was not mixed into the main material of the core component, and 12.5% ​​of the masterbatch was mixed only into the main material of the sheath component. The properties of the polyester monofilament are shown in Table 3. Compared to Example 5, the weavability was slightly worse, but was at a level acceptable for application to high-definition screen printing.

[0058] [Table 3]

[0059] Example 8 The organic colorant to be mixed into the master batch is Pigment Yellow 147 (CAS No.: 4118-16-5, chemical formula: C 37 H 21 A polyester monofilament was obtained in the same manner as in Example 1, except that the carbon black was changed to N5O4. The properties of the polyester monofilament are shown in Table 4. Compared to Example 1, the number of knots increased and the printing accuracy was slightly worse, but it was at a level acceptable for application to high-definition screen printing.

[0060] Comparative Example 4 A polyester monofilament was obtained in the same manner as in Example 1, except that a masterbatch containing only Pigment Yellow 150 (AS No.: 68511-62-6, chemical formula: C8H6N6O6) mixed at 10 wt% was used, and 6.25 wt% of the masterbatch was mixed into the main material of the core component in order to obtain the same level of reflectance as in Example 1. The properties of the polyester monofilament are shown in Table 4. Compared to Example 1, the number of knots increased and printing accuracy was impaired, making it impossible to apply the polyester monofilament to high-definition screen printing applications.

[0061] Comparative Example 5 A polyester monofilament was obtained in the same manner as in Comparative Example 6, except that the mixing ratio of the master batch to the main material of the core component was 1 wt %. The properties of the polyester monofilament are shown in Table 4. A sufficient halation suppression effect was not obtained, and bleeding of fine patterns occurred due to halation, making it impossible to apply the polyester monofilament to high-definition screen printing applications.

[0062] Comparative Example 6 A polyester monofilament was obtained in the same manner as in Example 1, except that a masterbatch containing only Pigment Brown 48 (CAS No.: 1310-39-0, chemical formula: (Fe,Al)2TiO5) mixed at 10 wt% was used as the masterbatch, and 20 wt% of the masterbatch was mixed into the main material of the core component. The properties of the polyester monofilament are shown in Table 4. No halation suppression effect was obtained, bleeding of fine patterns occurred due to halation, and further, the strength was reduced and printing accuracy was impaired, making it impossible to apply the polyester monofilament to high-definition screen printing applications.

[0063] [Table 4] [Explanation of symbols]

[0064] 1: Measured fiber diameter 2: Average fiber diameter 3: Threshold value 10% higher than the average fiber diameter 4: The beginning of the section 5:End of clause 6: Nodal diameter

Claims

1. The polyester monofilament comprises 0.01 to 0.1 wt % of an organic colorant and 0.1 to 0.5 wt % of an inorganic non-white colorant, has an average reflectance of 15% or less for light having a wavelength of 250 nm to 450 nm, has a fineness of 3.0 to 13.0 dtex, and has a strength of 6.5 to 9.0 cN / dtex.

2. A core-sheath composite monofilament in which both the core and sheath components are made of polyester, the core component containing 0.01 to 0.1 wt % of an organic colorant and 0.1 to 0.5 wt % of an inorganic non-white colorant, the sheath component containing no inorganic non-white colorant, an average reflectance of 15% or less for light with wavelengths of 250 nm to 450 nm, a fineness of 3.0 to 13.0 dtex, and a strength of 6.5 to 9.0 cN / dtex.

3. 3. The polyester monofilament according to claim 1 or 2, wherein for nodes present in 1 million meters in the longitudinal direction of the fiber and having a fiber diameter of 110% or more of the fiber diameter, the sum Z (%) of the increase rates of the node diameters represented by formula (1) is less than 30,000. [0010]

4. 3. The polyester monofilament according to claim 1, which satisfies the following items A to C: A. Fineness: 3.0 to 8.0 dtex B. Tenacity: 7.0 to 9.0 cN / dtex C. 10% modulus is 5.0 to 8.5 cN / dtex

Citation Information

Patent Citations

  • Method for producing monofilament for screen gauze

    JP2020090758A

  • Monofilament for screen gauze and screen gauze therefrom

    WO2005118927A1