Insulating circuit board, semiconductor device, and method for manufacturing insulating circuit board
A laminated copper layer structure with varying semi-softening temperatures addresses thermal stress and cracking issues in insulated circuit boards, ensuring effective heat dissipation and stable operation in high-temperature environments.
Patent Information
- Application Number
- JP2023053120
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing insulated circuit boards face issues with thermal stress and cracking due to increased thickness of copper layers for improved heat dissipation, leading to potential ceramic substrate cracking and reduced bonding reliability with semiconductor elements.
A laminated copper layer structure with varying semi-softening temperatures is used, where the first copper layer on the ceramic substrate side has a semi-softening temperature of 200°C or less, and the second copper layer has a higher temperature, along with a similar configuration for the metal layer, to reduce thermal stress and ensure heat dissipation.
The laminated copper layer structure enhances heat dissipation while reducing thermal stress and cracking, allowing stable operation in severe cooling and heating cycles, and improves bonding reliability with semiconductor elements.
Smart Images

Figure 2024141452000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an insulating circuit board including a ceramic substrate and a circuit layer formed on a surface of the ceramic substrate, a semiconductor device including the insulating circuit board, and a method for manufacturing the insulating circuit board. [Background technology]
[0002] In power modules, LED modules and thermoelectric modules, power semiconductor elements, LED elements and thermoelectric elements are bonded to an insulating circuit board having an insulating layer on one side of which a circuit layer made of a conductive material is formed. For example, power semiconductor elements for controlling large amounts of power used to control wind power generation, electric vehicles, hybrid vehicles, and the like generate a large amount of heat during operation. Therefore, as a substrate for mounting these elements, an insulated circuit board has been widely used which includes a ceramic substrate, a circuit layer formed by bonding a metal plate with excellent electrical conductivity to one surface of the ceramic substrate, and a metal layer for heat dissipation formed by bonding a metal plate to the other surface of the ceramic substrate.
[0003] In recent years, with the increasing integration and output of elements such as power semiconductor elements, LED elements, and thermoelectric elements, there is a demand for improved heat dissipation characteristics in insulating circuit boards. Therefore, in insulating circuit boards, thickening the circuit layer has been considered in order to improve the heat dissipation characteristics of heat generated by the elements. For example, Patent Document 1 describes an insulating circuit board in which a circuit layer is made of a metal material and has a thickness within the range of 0.05 mm to 2.0 mm. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-169540 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when the thickness of the copper in the circuit layer is increased in order to improve heat dissipation, when the circuit layer is used in a high-temperature environment, work hardening of the circuit layer occurs due to thermal cycles, and severe thermal stress is applied, which may cause the ceramic substrate to crack. On the other hand, if the circuit layer is made of pure aluminum, which is easily deformed, in order to reduce the thermal stress applied to the ceramic substrate during the thermal cycle and prevent cracking of the ceramic substrate, the surface of the circuit layer may be deformed in a wavy manner due to the thermal stress of the thermal cycle, which may reduce the reliability of the connection with the semiconductor element. In addition, the thermal conductivity of aluminum is lower than that of copper, so there is a limit to its heat dissipation.
[0006] The present invention has been made in view of the above-mentioned circumstances, and has an object to provide an insulating circuit board that has excellent heat dissipation properties and has thermal cycle reliability enabling use even in applications where severe thermal cycles are applied in high-temperature environments, a semiconductor device using the insulating circuit board, and a method for manufacturing the insulating circuit board. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems, an insulating circuit board according to a first aspect of the present invention is an insulating circuit board comprising a ceramic substrate and a circuit layer formed on the surface of the ceramic substrate, the circuit layer having a first copper layer disposed on the ceramic substrate side and a second copper layer laminated on the first copper layer, the first copper plate constituting the first copper layer having a half-softening temperature of 200°C or lower, and the second copper plate constituting the second copper layer having a half-softening temperature higher than the half-softening temperature of the first copper plate constituting the first copper layer.
[0008] In the insulating circuit board of the first aspect of the present invention, the circuit layer has a structure in which the first copper layer and the second copper layer are laminated, so that the overall thickness of the circuit layer can be ensured, and it is possible to ensure sufficient heat dissipation. Furthermore, since the semi-softening temperature of the first copper plate constituting the first copper layer arranged on the ceramic substrate side is set to 200°C or lower, work hardening can be reduced by recrystallization during cooling and heating cycles, and thermal stress is less likely to increase even when cooling and heating cycles are repeated, thereby suppressing cracking of the ceramic substrate. In addition, since the semi-softening temperature of the second copper plate constituting the second copper layer is higher than the semi-softening temperature of the first copper plate constituting the first copper layer, deformation of the surface of the circuit layer when subjected to a thermal cycle can be suppressed.
[0009] The insulated circuit board of aspect 2 of the present invention is the insulated circuit board of aspect 1, characterized in that a metal layer is formed on the surface of the ceramic substrate opposite to the circuit layer, the metal layer having a third copper layer disposed on the ceramic substrate side and a fourth copper layer laminated on the third copper layer, the third copper plate constituting the third copper layer having a half-softening temperature of 200°C or lower and the fourth copper plate constituting the fourth copper layer having a half-softening temperature higher than the half-softening temperature of the third copper plate constituting the third copper layer.
[0010] According to the insulating circuit board of the second aspect of the present invention, the metal layer formed on the surface of the ceramic substrate opposite to the circuit layer has a laminated structure of a third copper layer and a fourth copper layer, so that the thickness of the entire metal layer can be ensured and heat dissipation can be further improved. In addition, when the metal layer is bonded to a heat sink via a second bonding layer, the thermal stress on the second bonding layer can also be reduced. In addition, since the semi-softening temperature of the third copper plate constituting the third copper layer arranged on the ceramic substrate side is set to 200°C or lower, the thermal stress applied to the ceramic substrate during thermal cycle loading can be alleviated, and cracking of the ceramic substrate can be suppressed. In addition, since the semi-softening temperature of the fourth copper plate constituting the fourth copper layer is higher than the semi-softening temperature of the third copper plate constituting the third copper layer, deformation of the surface of the metal layer when subjected to a thermal cycle can be suppressed.
[0011] A semiconductor device according to a third aspect of the present invention is characterized in that it comprises the insulating circuit board according to the first or second aspect, and a semiconductor element mounted on the circuit layer. According to the semiconductor device of aspect 3 of the present invention, since it is equipped with the insulating circuit board of aspect 1 or aspect 2, it can efficiently dissipate heat generated from the semiconductor element, and can suppress deformation of the circuit layer surface and cracking of the ceramic substrate due to thermal cycles. Therefore, it can be stably used even in applications where it is subjected to severe thermal cycles, such as when used in a high-temperature environment.
[0012] A semiconductor device according to a fourth aspect of the present invention is characterized in that in the semiconductor device according to the third aspect, the insulating circuit board and the semiconductor element are resin-sealed with an insulating resin. According to the semiconductor device of the fourth aspect of the present invention, the insulating circuit board and the semiconductor element are resin-sealed with insulating resin, so that thermal stress during thermal cycle loading can be further suppressed, and deformation of the circuit layer surface and cracking of the ceramic substrate can be further suppressed. In addition, electrical short-circuiting between the semiconductor element and other members can be suppressed, allowing for stable use. Furthermore, the bonding reliability between the semiconductor element and the insulating circuit board can be improved.
[0013] The manufacturing method for an insulating circuit board of aspect 5 of the present invention is a manufacturing method for an insulating circuit board for manufacturing the insulating circuit board of aspect 1 or aspect 2, and includes a first copper layer forming step of joining the first copper plate to the ceramic substrate to form the first copper layer, and a second copper layer forming step of joining the second copper plate to the first copper layer to form the second copper layer, characterized in that the first copper layer forming step and the second copper layer forming step are carried out simultaneously.
[0014] According to the manufacturing method for an insulated circuit board of aspect 5 of the present invention, a first copper layer formation step of joining the first copper plate to the ceramic substrate to form the first copper layer, and a second copper layer formation step of joining the second copper plate to the first copper layer to form the second copper layer are carried out simultaneously. This reduces the number of manufacturing steps, making it possible to efficiently manufacture an insulated circuit board having a two-layer circuit layer.
[0015] The manufacturing method for an insulating circuit board of aspect 6 of the present invention is a manufacturing method for an insulating circuit board for manufacturing the insulating circuit board of aspect 2, and includes a third copper layer forming step of joining the third copper plate to the ceramic substrate to form the third copper layer, and a fourth copper layer forming step of joining the fourth copper plate to the third copper layer to form the fourth copper layer, characterized in that the third copper layer forming step and the fourth copper layer forming step are carried out simultaneously.
[0016] According to the method for producing an insulating circuit board of aspect 6 of the present invention, a third copper layer formation step of joining the third copper plate to the ceramic substrate to form the third copper layer, and a fourth copper layer formation step of joining the fourth copper plate to the third copper layer to form the fourth copper layer are carried out simultaneously, which reduces the number of production steps and makes it possible to efficiently produce an insulating circuit board having a two-layer metal layer structure.
[0017] The method for manufacturing an insulating circuit board of aspect 7 of the present invention is a method for manufacturing an insulating circuit board of aspect 1 or aspect 2, and is characterized by having a first copper layer formation step of joining the first copper plate to the ceramic substrate to form the first copper layer, a circuit pattern formation step of forming a circuit pattern on the first copper layer, and a second copper layer formation step of joining the second copper plate to at least an element mounting area, on which a semiconductor element is mounted, of the first copper layer on which the circuit pattern is formed, to form the second copper layer.
[0018] The method for manufacturing an insulating circuit board according to aspect 7 of the present invention includes a first copper layer formation step of joining the first copper plate to the ceramic substrate to form the first copper layer, and a circuit pattern formation step of forming a circuit pattern on the first copper layer. Therefore, since the circuit pattern is formed only on the first copper layer in the circuit pattern formation step, it is possible to form the circuit pattern accurately and efficiently by making the first copper layer thin. Furthermore, the method includes a second copper layer formation process in which the second copper layer is formed by joining the second copper plate to at least an element mounting area, on which a semiconductor element is mounted, of the first copper layer on which the circuit pattern is formed. This ensures the thickness of the element mounting area on which the semiconductor element, which serves as a heat source, is mounted, and makes it possible to manufacture an insulated circuit board with excellent heat dissipation properties. Effect of the Invention
[0019] Effects of the Invention According to the present invention, it is possible to provide an insulating circuit board which has excellent heat dissipation properties and thermal cycle reliability enabling use in applications where severe thermal cycles are applied in high-temperature environments, a semiconductor device using this insulating circuit board, and a method for manufacturing the insulating circuit board. [Brief description of the drawings]
[0020] [Figure 1] 1 is a schematic explanatory diagram of a semiconductor device including an insulating circuit board according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a flow diagram of a method for producing an insulating circuit board according to a first embodiment of the present invention. [Diagram 3] 1A to 1C are explanatory diagrams of a method for manufacturing an insulating circuit board according to a first embodiment of the present invention. [Figure 4] FIG. 11 is a schematic explanatory diagram of a semiconductor device including an insulating circuit board according to a second embodiment of the present invention. [Diagram 5] FIG. 6 is a flow diagram of a method for producing an insulating circuit board according to a second embodiment of the present invention. [Figure 6] 5A to 5C are explanatory diagrams of a method for producing an insulating circuit board according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] First Embodiment Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. FIG. 1 shows an insulating circuit board 10 according to a first embodiment of the present invention, and a semiconductor device 1 using this insulating circuit board 10.
[0022] The semiconductor device 1 shown in Figure 1 comprises an insulating circuit board 10 which is the present embodiment, a semiconductor element 3 bonded to one surface (the top surface in Figure 1) of the insulating circuit board 10 via a first bonding layer 2, a terminal material 5 bonded to one surface (the top surface in Figure 1) of the insulating circuit board 10, a heat sink 6 bonded to the underside of the insulating circuit board 10 via a second bonding layer 7, and a sealing resin 8 made of insulating resin.
[0023] The semiconductor element 3 is made of a semiconductor material such as Si, SiC, etc. In this embodiment, the semiconductor element 3 is a power semiconductor, and the semiconductor device 1 is a power module. The first bonding layer 2 interposed between the insulating circuit board 10 and the semiconductor element 3 is made of, for example, a Sn-Ag based, Sn-Cu based, Sn-In based, or Sn-Ag-Cu based solder material (so-called lead-free solder material), or a silver sintered material or a copper sintered material.
[0024] The terminal material 5 is made of a metal having excellent electrical conductivity, and in this embodiment, is a lead frame material made of copper or a copper alloy. Aluminum wire, copper wire, etc. can also be used.
[0025] The heat sink 6 is for dissipating heat on the insulating circuit board 10 side. The heat sink 6 is made of copper or a copper alloy, or aluminum or an aluminum alloy, and in this embodiment, it is a heat sink made of oxygen-free copper. The second bonding layer 7 interposed between the insulating circuit board 10 and the heat sink 6 is made of, for example, a Sn-Ag based, Sn-Cu based, Sn-In based, or Sn-Ag-Cu based solder material (so-called lead-free solder material), or a silver sintered material or a copper sintered material.
[0026] As shown in FIG. 1, the insulating circuit board 10 of this embodiment includes a ceramic substrate 11, a circuit layer 20 disposed on one surface (the upper surface in FIG. 1) of the ceramic substrate 11, and a metal layer 30 disposed on the other surface (the lower surface in FIG. 1) of the ceramic substrate 11.
[0027] The ceramic substrate 11 is made of ceramics such as silicon nitride (Si3N4), aluminum nitride (AlN), and alumina (Al2O3) that have excellent insulating and heat dissipating properties. In this embodiment, the ceramic substrate 11 is made of aluminum nitride (AlN), which has particularly excellent heat dissipating properties. The thickness of the ceramic substrate 11 is set within a range of 0.2 mm to 1.5 mm, for example, and is set to 0.635 mm in this embodiment.
[0028] As shown in FIG. 1, the circuit layer 20 has a first copper layer 21 disposed on one surface of the ceramic substrate 11, and a second copper layer 22 laminated on one surface of the first copper layer 21. In this embodiment, as shown in FIG. 1, a circuit pattern is formed on the circuit layer 20, and an element mounting area on which a semiconductor element 3 is mounted and a terminal joining area on which a terminal material 5 is joined are formed. In this embodiment, as shown in FIG. 1, the second copper layer 22 is formed in the element mounting area where the semiconductor element 3 is mounted, and is not formed in the terminal bonding area where the terminal material 5 is bonded.
[0029] The first copper layer 21 constituting the circuit layer 20 is formed by bonding a first copper plate 41 to one surface of the ceramic substrate 11, as shown in FIG. The second copper layer 22 is formed by joining a second copper plate 42 to the first copper layer 21. In this embodiment, the first copper plate 41 constituting the first copper layer 21 has a semi-softening temperature of 200° C. or lower. The second copper plate 42 constituting the second copper layer 22 has a semi-softening temperature higher than the semi-softening temperature of the first copper plate 41 constituting the first copper layer 21. The semi-softening temperature of the first copper plate 41 constituting the first copper layer 21 is more preferably 180° C. or lower. The semi-softening temperature of the first copper plate 41 constituting the first copper layer 21 may be 80° C. or higher. It is also preferable that the semi-softening temperature is lower than the upper limit temperature of the thermal cycle required for the substrate. The quality of the first copper plate 41 constituting the first copper layer 21 is not particularly specified, but it is preferable that the material be a 1 / 4H material, a 1 / 8H material, or an O material that is less susceptible to work hardening.
[0030] The half-softening temperature of the copper plate can be measured as follows. For copper sheet before joining to other components, the copper sheet is annealed and the 0.2% yield strength is measured by a tensile test. The semi-softening temperature is the annealing temperature corresponding to the 0.2% yield strength at the midpoint between the 0.2% yield strength before annealing and the 0.2% yield strength when completely softened (a state in which the 0.2% yield strength does not change even if the annealing temperature is increased further after 30 minutes of annealing is considered to be completely softened). In addition, in the case of a material (circuit board) after bonding of copper and ceramics, a circuit board sample is subjected to 3000 thermal cycles of -40°C to 150°C in a gas phase, and then heat treatment (annealing) is performed at each temperature at 5°C intervals, for example, and the cross section is cut to expose it, and the yield stress or nanoindentation hardness (hardness) is measured by nanoindentation. In a state where the polished surface is simply polished, the polished surface layer of Cu is slightly hardened due to the influence of processing. Since nanoindentation is an evaluation of the extreme surface layer, in order to eliminate the hardened layer of the surface, the surface that has been further processed with a CP (cross section polisher) is evaluated. In order to eliminate the hardened layer of the surface, chemical polishing with chemicals may be used. The yield stress or hardness is measured at a cross section at a point 100 μm away from the interface between the copper layer and the ceramic layer toward the copper layer side (corresponding to copper with a low half-softening temperature) and at a cross section at a point 100 μm away from the copper layer (on the circuit) farthest from the ceramic toward the ceramic side (corresponding to copper with a high half-softening temperature), with the active metal layer or brazing material layer, if any, being the copper layer, and the oxide or nitride of the active metal, if any, being the ceramic layer. The annealing temperature measured in this way, after the thermal cycle test, that corresponds to the yield stress or hardness at the midpoint between the yield stress or hardness before annealing and the yield stress or hardness when completely softened, is the half-softening temperature.
[0031] Here, the first copper plate 41 constituting the first copper layer 21 having a softening temperature of 200°C or less can be made of, for example, 6NCu with a purity of 99.9999 mass% or more, or a copper material in which at least one or more trace amounts of elements such as yttrium, scandium, samarium, lanthanum, cerium, boron, titanium, vanadium, chromium, manganese, iron, zirconium, hafnium, neodymium, tantalum, calcium, and manganese have been added to oxygen-free copper with a purity of 99.96 mass% or more. The second copper plate 42 constituting the second copper layer 22 is made of copper or a copper alloy having a higher half-softening temperature than the first copper plate 41 .
[0032] The first copper layer 21 (first copper plate 41) and the second copper layer 22 (second copper plate 42) are directly bonded by solid-state diffusion bonding. The thickness of the first copper layer 21 in the circuit layer 20 is set within the range of 0.1 mm to 1 mm. On the other hand, the thickness of the second copper layer 22 in the circuit layer 20 is set within the range of 0.1 mm to 1 mm.
[0033] The metal layer 30 is formed by bonding a copper plate 50 to the other surface of the ceramic substrate 11, as shown in FIG. Here, the thickness of the metal layer 30 is set within the range of 0.1 mm to 2 mm.
[0034] Next, a method for manufacturing the insulating circuit board 10 according to this embodiment will be described with reference to FIGS.
[0035] (First copper layer and metal layer forming step S01) As shown in FIG. 3, a first copper plate 41 which will become the first copper layer 21 is laminated on one surface of the ceramic substrate 11 via a bonding material 46, and a copper plate 50 which will become the metal layer 30 is laminated on the other surface of the ceramic substrate 11 via a bonding material 56. In this embodiment, the bonding materials 46, 56 are brazing filler metal made of an Ag alloy containing Cu and Ti (for example, Ag-27.4 mass % Cu-2.0 mass % Ti brazing filler metal).
[0036] Then, pressure is applied in the stacking direction (pressure 0.1 to 100 kgf / cm 2 The ceramic substrate 11 is placed in a vacuum heating furnace under a pressure (0.01 to 9.8 MPa) and heated under pressure in the lamination direction, thereby bonding the first copper plate 41 and the ceramic substrate 11 to form the first copper layer 21, and bonding the copper plate 50 and the ceramic substrate 11 to form the metal layer 30. In this embodiment, the first copper layer forming step S11 and the metal layer forming step S12 are carried out simultaneously. Here, the pressure in the vacuum heating furnace is 10 -6 Pa or more 10 -3 It is preferable that the pressure is set within a range of 100 Pa or less, the heating temperature is set within a range of 800° C. or more and 930° C. or less, and the holding time at the heating temperature is set within a range of 5 minutes or more and 120 minutes or less.
[0037] (Circuit pattern formation process S02) Next, a circuit pattern is formed on the first copper layer 21. In this embodiment, the circuit pattern is formed on the first copper layer 21 by an etching method. In this embodiment, the first copper layer 21 is formed to be relatively thin, within a range of 0.1 mm to 0.5 mm, so that a fine pattern can be formed by etching. In addition, it becomes possible to form the circuit pattern efficiently and accurately.
[0038] (Second copper layer formation step S03) Next, a second copper plate 42 which will become the second copper layer 22 is laminated on one surface side (the upper side in FIG. 3) of the first copper layer 21. In this embodiment, the second copper plate 42 is laminated in an area where the semiconductor element 3 is to be mounted. The bonding surfaces of the first copper layer 21 and the second copper plate 42 are smoothed in advance by removing any scratches thereon.
[0039] Then, the laminate is pressed in the lamination direction (pressure 1 to 100 kgf / cm 2 The first copper layer 21 and the second copper plate 42 are bonded to each other by applying a pressure (0.1 to 9.8 MPa) and heating. Here, the heating temperature is preferably set within a range of 800° C. to 930° C., and the holding time at the heating temperature is preferably set within a range of 5 minutes to 120 minutes.
[0040] In this manner, the insulating circuit board 10 of this embodiment is manufactured.
[0041] (Semiconductor element bonding process S04) Next, the semiconductor element 3 is laminated on the element mounting area (second copper layer 22) of the circuit layer 20 via a solder material, and soldered in a reducing furnace.
[0042] (Heat sink bonding process S05) Next, the metal layer 30 and the heat sink 6 are laminated together with a solder material therebetween, and then soldered together in a reducing furnace.
[0043] (Terminal material joining process S06) Next, the terminal material 5 is ultrasonically bonded to the terminal bonding area of the circuit layer 20 .
[0044] (Resin sealing process S07) Next, the semiconductor element 3, the insulating circuit board 10, and the heat sink 6 are sealed with resin. At this time, one end of the terminal material 5 is disposed outside the sealing resin 8.
[0045] In the manner described above, the semiconductor device 1 of this embodiment is manufactured.
[0046] According to the insulating circuit board 10 of this embodiment configured as described above, since the circuit layer 20 has a structure in which the first copper layer 21 and the second copper layer 22 are laminated, it is possible to ensure the overall thickness of the circuit layer 20 and therefore to ensure sufficient heat dissipation. Since the semi-softening temperature of the first copper plate 41 constituting the first copper layer 21 disposed on the ceramic substrate 11 side is set to 200°C or lower, the first copper layer 21 is easily deformed, recrystallizes during thermal cycles, and is not easily work-hardened. Therefore, the thermal stress applied to the ceramic substrate 11 during thermal cycle loading can be alleviated, and cracking of the ceramic substrate 11 can be suppressed.
[0047] Furthermore, since the semi-softening temperature of the second copper plate 42 constituting the second copper layer 22 is higher than the semi-softening temperature of the first copper plate 41 constituting the first copper layer 21, deformation of the surface of the circuit layer 20 when subjected to a thermal cycle can be suppressed, and deterioration of the bonding with the semiconductor element 3 can be suppressed. Therefore, the battery can be used stably even in applications where it is subjected to severe thermal cycles in a high-temperature environment.
[0048] The semiconductor device 1 of this embodiment has a structure including the insulating circuit board 10 of this embodiment and a semiconductor element 3 mounted on the circuit layer 20. Therefore, the semiconductor device 1 can efficiently dissipate heat generated from the semiconductor element 3 and can suppress deformation of the surface of the circuit layer 20 and cracking of the ceramic substrate 11 due to thermal cycles. Therefore, the semiconductor device 1 can be stably used even in applications where it is subjected to severe thermal cycles in a high-temperature environment.
[0049] In the semiconductor device 1 of this embodiment, when the insulating circuit board 10 and the semiconductor element 3 are resin-sealed with insulating resin, thermal stress during thermal cycle loading can be further suppressed, and deformation of the surface of the circuit layer 20 and cracking of the ceramic substrate 11 can be further suppressed. In addition, short-circuiting between the semiconductor element 3 and the terminal material 5 and other members can be suppressed.
[0050] The manufacturing method for the insulating circuit board 10 of this embodiment includes a first copper layer and metal layer formation step S01 in which a first copper layer 21 is formed by joining a first copper plate 41 to the ceramic substrate 11 and a third copper layer 31 is formed by joining a third copper plate 51 to the ceramic substrate 11, and a circuit pattern formation step S02 in which a circuit pattern is formed on the first copper layer 21. Therefore, since the circuit pattern is formed only on the first copper layer 21 in the circuit pattern formation step S02, it is possible to form the circuit pattern accurately and efficiently. Furthermore, in the second copper layer formation process S03, the second copper layer 22 is formed by joining a second copper plate 52 to the element mounting area, on which the semiconductor element 3 is mounted, of the first copper layer 21 on which the circuit pattern is formed. This ensures the thickness of the element mounting area on which the semiconductor element 3, which serves as a heat source, is mounted, and an insulated circuit board 10 with excellent heat dissipation properties can be manufactured.
[0051] Second Embodiment Next, an embodiment of the present invention will be described with reference to the accompanying drawings. Note that the same members as those in the first embodiment are designated by the same reference numerals and detailed description thereof will be omitted. FIG. 4 shows an insulating circuit board 110 according to a second embodiment of the present invention, and a semiconductor device 101 using this insulating circuit board 110.
[0052] The semiconductor device 101 shown in Figure 4 comprises an insulating circuit board 110 of this embodiment, a semiconductor element 3 bonded to one surface (the upper surface in Figure 4) of the insulating circuit board 110 via a first bonding layer 2, and a heat sink 6 bonded to the underside of the insulating circuit board 110 via a second bonding layer 7.
[0053] As shown in FIG. 4, the insulating circuit board 110 of this embodiment includes a ceramic substrate 11, a circuit layer 120 disposed on one surface (the upper surface in FIG. 4) of the ceramic substrate 11, and a metal layer 130 disposed on the other surface (the lower surface in FIG. 4) of the ceramic substrate 11.
[0054] As shown in FIG. 1, the circuit layer 120 has a first copper layer 121 disposed on one surface of the ceramic substrate 11, and a second copper layer 122 laminated on one surface of this first copper layer 121. In this embodiment, as shown in FIG. 1, the circuit layer 120 has a circuit pattern formed thereon.
[0055] The first copper layer 121 constituting the circuit layer 120 is formed by bonding a first copper plate 141 to one surface of the ceramic substrate 11, as shown in FIG. The second copper layer 122 is formed by joining a second copper plate 142 to the first copper layer 121. In this embodiment, the semi-softening temperature of the first copper plate 141 constituting the first copper layer 121 is set to be equal to or lower than 200° C. Also, the semi-softening temperature of the second copper plate 142 constituting the second copper layer 122 is configured to be higher than the semi-softening temperature of the first copper plate 141 constituting the first copper layer 121. It is more preferable that the semi-softening temperature of the first copper plate 141 constituting the first copper layer 121 is 180° C. or lower. The semi-softening temperature of the first copper plate 141 constituting the first copper layer 121 may be 80° C. or higher. The quality of the first copper plate 141 constituting the first copper layer 121 is not particularly specified, but it is preferable that the material be a 1 / 4H material, a 1 / 8H material, or an O material that is less susceptible to work hardening.
[0056] Here, the first copper plate 141 constituting the first copper layer 121 having a softening temperature of 200°C or less can be made of, for example, 6NCu with a purity of 99.9999 mass% or more, or a copper material in which at least one or more trace amounts of elements such as yttrium, scandium, samarium, lanthanum, cerium, boron, titanium, vanadium, chromium, manganese, iron, zirconium, hafnium, neodymium, tantalum, calcium, and manganese have been added to oxygen-free copper with a purity of 99.96 mass% or more. The second copper plate 142 constituting the second copper layer 122 is made of copper or a copper alloy having a higher half-softening temperature than the first copper plate 141 .
[0057] The first copper layer 121 (first copper plate 141) and the second copper layer 122 (second copper plate 142) are directly bonded by solid-state diffusion bonding. The thickness of the first copper layer 121 in the circuit layer 120 is set within the range of 0.1 mm to 1 mm. On the other hand, the thickness of the second copper layer 122 in the circuit layer 120 is set within the range of 0.1 mm to 1 mm.
[0058] As shown in FIG. 4, the metal layer 130 has a third copper layer 131 disposed on the other surface of the ceramic substrate 11, and a fourth copper layer 132 laminated on the other surface of this third copper layer 131. The third copper layer 131 constituting the metal layer 130 is formed by bonding a third copper plate 151 to the other surface of the ceramic substrate 11, as shown in FIG. The fourth copper layer 132 is formed by joining a fourth copper plate 152 to the third copper layer 131 . In this embodiment, the semi-softening temperature of the third copper plate 151 constituting the third copper layer 131 is set to be equal to or lower than 200° C. Also, the semi-softening temperature of the fourth copper plate 152 constituting the fourth copper layer 132 is configured to be higher than the semi-softening temperature of the third copper plate 151 constituting the third copper layer 131. It is more preferable that the semi-softening temperature of the third copper plate 151 constituting the third copper layer 131 is 180° C. or lower. The semi-softening temperature of the third copper plate 151 constituting the third copper layer 131 may be 80° C. or higher. The quality of the third copper plate 151 constituting the third copper layer 131 is not particularly specified, but it is preferable that the third copper plate 151 be a 1 / 4H material, a 1 / 8H material, or an O material that has little work hardening.
[0059] Here, the third copper plate 151 constituting the third copper layer 131 having a softening temperature of 200°C or less can be made of, for example, 6NCu with a purity of 99.9999 mass% or more, or a copper material in which at least one or more trace amounts of elements such as yttrium, scandium, samarium, lanthanum, cerium, boron, titanium, vanadium, chromium, manganese, iron, zirconium, hafnium, neodymium, tantalum, calcium, and manganese have been added to oxygen-free copper with a purity of 99.96 mass% or more. Moreover, the fourth copper plate 152 constituting the fourth copper layer 132 is made of copper or a copper alloy having a higher half-softening temperature than the third copper plate 151 .
[0060] The third copper layer 131 (third copper plate 151) and the fourth copper layer 132 (fourth copper plate 152) are directly bonded by solid-phase diffusion bonding. The thickness of the third copper layer 131 in the metal layer 130 is set within the range of 0.1 mm to 1 mm. On the other hand, the thickness of the fourth copper layer 132 in the metal layer 130 is set within the range of 0.1 mm to 1 mm.
[0061] Next, a method for manufacturing the insulating circuit board 110 of this embodiment will be described with reference to FIGS.
[0062] (First copper plate and second copper plate preparation process S101) First, the first copper plate 141 and the second copper plate 142 are prepared by processing the copper plate into shapes that will form the circuit pattern of the circuit layer 120. In this embodiment, the first copper plate 141 and the second copper plate 142 that will form the circuit pattern are prepared by punching a copper plate.
[0063] (Circuit layer and metal layer formation process S102) 6, a first copper plate 141 which becomes the first copper layer 121 is laminated on one surface of the ceramic substrate 11 via a bonding material 46, and a third copper plate 151 which becomes the third copper layer 131 is laminated on the other surface of the ceramic substrate 11 via a bonding material 56. The first copper plate 141 is arranged so as to form a circuit pattern. In this embodiment, the bonding materials 46, 56 are brazing filler metal made of an Ag alloy containing Cu and Ti (for example, Ag-27.4 mass % Cu-2.0 mass % Ti brazing filler metal).
[0064] Furthermore, a second copper plate 142 which becomes the second copper layer 122 is laminated on one surface side (the upper side in FIG. 6) of the first copper plate 141 which is arranged so as to form a circuit pattern. Moreover, a fourth copper plate 152 which becomes the fourth copper layer 132 is laminated on the other surface side of the third copper plate 151 (the lower side in FIG. 6). The bonding surfaces of the first copper plate 141, the second copper plate 142, the third copper plate 151, and the fourth copper plate 152 are smoothed in advance by removing any scratches thereon.
[0065] Then, pressure is applied in the stacking direction (pressure 1 to 100 kgf / cm 2 The ceramic substrate 11 is then placed in a vacuum heating furnace under a pressure of 0.1 to 9.8 MPa and heated in the stacking direction to bond the first copper plate 141 to the ceramic substrate 11 to form the first copper layer 121, and the third copper plate 151 to the ceramic substrate 11 to form the third copper layer 131. Furthermore, the first copper layer 121 (first copper plate 141) and the second copper plate 142 are solid-state diffusion bonded to form the second copper layer 122, and the third copper layer 131 (third copper plate 151) and the fourth copper plate 152 are solid-state diffusion bonded to form the fourth copper layer 132. That is, in this embodiment, the first copper layer forming step S121, the second copper layer forming step S122, the third copper layer forming step S123, and the fourth copper layer forming step S124 are carried out simultaneously. Here, the pressure in the vacuum heating furnace is 10 -6 Pa or more 10 -3 It is preferable that the pressure is set within a range of 100 Pa or less, the heating temperature is set within a range of 800° C. or more and 930° C. or less, and the holding time at the heating temperature is set within a range of 5 minutes or more and 120 minutes or less.
[0066] In this manner, the insulating circuit board 110 of this embodiment is manufactured.
[0067] (Heat sink bonding process S104) Next, the fourth copper layer 132 of the metal layer 130 and the heat sink 6 are laminated together via a solder material, and solder-bonded in a reduction furnace.
[0068] (Semiconductor element bonding process S106) Next, the semiconductor element 3 is laminated on the circuit layer 120 via a solder material, and soldered in a reducing furnace.
[0069] In the manner described above, the semiconductor device 101 of this embodiment is manufactured.
[0070] According to the insulating circuit board 110 according to this embodiment configured as above, it is possible to achieve the same effects as those of the first embodiment. Furthermore, in the insulating circuit board 110 of this embodiment, a metal layer 130 is formed on the surface of the ceramic substrate 11 opposite the circuit layer 120, and when the metal layer 130 has a third copper layer 131 disposed on the ceramic substrate 11 side and a fourth copper layer 132 laminated on the third copper layer 131, it is possible to ensure the overall thickness of the metal layer 130, and further improve the heat dissipation properties.
[0071] In addition, since the semi-softening temperature of the third copper plate 151 constituting the third copper layer 131 arranged on the ceramic substrate 11 side is set to 200°C or lower, the thermal stress applied to the ceramic substrate 11 during thermal cycle loading can be alleviated, and cracking of the ceramic substrate 11 can be suppressed. Furthermore, since the semi-softening temperature of the fourth copper plate 152 constituting the fourth copper layer 132 is higher than the semi-softening temperature of the third copper plate 151 constituting the third copper layer 131, deformation of the surface of the metal layer 30 when subjected to a thermal cycle can be suppressed, and deterioration of the bond with the heat sink 6 can be suppressed. Therefore, the battery can be used stably even in applications where it is subjected to severe thermal cycles in a high-temperature environment.
[0072] In the manufacturing method of the insulating circuit board 110 of the present embodiment, a first copper layer formation step S111 of joining a first copper plate 141 to the ceramic substrate 11 to form a first copper layer 121, a second copper layer formation step 112 of joining a second copper plate 142 to the first copper layer 121 to form a second copper layer 122, a third copper layer formation step S113 of joining a third copper plate 151 to the ceramic substrate 11 to form a third copper layer 131, and a fourth copper layer formation step S114 of joining a fourth copper plate 152 to the third copper layer 131 to form a fourth copper layer 132 are simultaneously carried out, which reduces the number of manufacturing steps and makes it possible to efficiently manufacture the insulating circuit board 110 in which the circuit layer 120 and the metal layer 130 each have a two-layer structure.
[0073] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. For example, in this embodiment, the semiconductor device has been described as a power module equipped with a power semiconductor, but this is not limited to this, and other semiconductor devices may be used as long as they have the insulating circuit board of this embodiment. EXAMPLES
[0074] The results of confirmation experiments carried out to confirm the effects of the present invention will be described below.
[0075] First, a ceramic substrate (40 mm×40 mm×thickness 0.32 mm) made of silicon nitride was prepared. Copper plates (37 mm × 37 mm × thickness shown in Table 1) shown in Table 1 were prepared as copper plates constituting the circuit layer (first copper layer and second copper layer) and the metal layer (third copper layer and fourth copper layer). In Table 1, "6NCu" is pure copper with a purity of 99.9999 mass% or more, "TPC" is tough pitch copper, "OFC" is oxygen-free copper, and "Cu1" is oxygen-free copper with a purity of 99.96 mass% or more to which 9 mol ppm of yttrium (Y) has been added.
[0076] Then, as shown in Table 1, a copper plate was bonded to the ceramic substrate, and the copper plates were bonded to each other, thereby producing insulating circuit boards of invention examples 1 to 8 and comparative examples 1 to 3. The ceramic substrate and the copper plate were joined using a brazing material consisting of Ag-27.4 mass% Cu-2.0 mass% Ti, and the copper plates were joined together by solid-phase diffusion bonding.
[0077] Here, in the column of the bonding method in Table 1, "1" indicates that bonding between a ceramic substrate and a copper plate and bonding between copper plates were performed simultaneously. The bonding conditions were a vacuum atmosphere of 10 -5 The pressure load was 1 MPa, the heating temperature was 950°C, and the holding time was 1 hour. In the column of the bonding method in Table 1, "2" refers to bonding a ceramic substrate and a copper plate, and then bonding the copper plates together by solid-phase diffusion bonding. The bonding conditions for the ceramic substrate and the copper plate were 1000 s in a vacuum atmosphere. -5 The bonding conditions for the solid-phase diffusion bonding of the copper plates were 1000 Pa, 1 MPa pressure, 800°C heating temperature, and 1 hour heating time. -5 The pressure load was 1 MPa, the heating temperature was 950°C, and the holding time was 1 hour.
[0078] The insulating circuit boards of Examples 1 to 8 of the present invention and Comparative Examples 1 to 3 were evaluated as follows. The evaluation results are shown in Table 1.
[0079] (Reliability of thermal cycles) The above-mentioned insulating circuit board was subjected to a thermal cycle of -45°C for 5 minutes ←→ 175°C for 5 minutes in a liquid bath (Fluorinert, manufactured by 3M Japan Co., Ltd.). The ceramic substrate was checked for cracks every 500 thermal cycles, and the number of thermal cycles at which cracks occurred was confirmed (referred to as "Number of times cracks occurred in the ceramic substrate" in Table 1).
[0080] [Table 1]
[0081] In Comparative Example 1, the circuit layer and metal layer had a single-layer structure of oxygen-free copper with a semi-softening temperature of 290°C, and cracks occurred in the ceramic substrate after 500 to 1000 cooling and heating cycles, but the cracks were minor and were presumed to have occurred around 1000 cycles. In Comparative Example 2, the circuit layer and the metal layer were made of a single layer of tough pitch copper with a half-softening temperature of 230°C, and cracks occurred in the ceramic substrate after 500 to 1000 cooling and heating cycles. The cracks were larger than those in Comparative Example 1, and were presumably generated around 500 cycles.
[0082] In Comparative Example 3, the first copper layer and the third copper layer on the ceramic substrate side were oxygen-free copper with a semi-softening temperature of 290°C, the second copper layer laminated on the first copper layer and the fourth copper layer laminated on the third copper layer were Cu1 with a semi-softening temperature of 175°C, and cracks occurred in the ceramic substrate after 500 to 1000 cooling and heating cycles. As in Comparative Example 1, the cracks were minor and therefore it is assumed that they occurred around 1000 cycles.
[0083] In contrast, in Examples 1 to 7 of the present invention, the first copper layer and the third copper layer on the ceramic substrate side were composed of copper plates with a half-softening temperature of 200°C or lower, and the half-softening temperatures of the second copper layer laminated on the first copper layer and the fourth copper layer laminated on the third copper layer were higher than the half-softening temperatures of the copper plates that constitute the first copper layer and the third copper layer. No cracks were generated in the ceramic substrate even after 2000 cooling and heating cycles, and the reliability of the cooling and heating cycles was excellent.
[0084] In addition, in Example 8 of the present invention, the first copper layer on the ceramic substrate side was composed of a copper plate with a half-softening temperature of 200°C or lower, and the half-softening temperature of the second copper layer laminated on the first copper layer was higher than the half-softening temperature of the copper plate constituting the first copper layer. No cracks were generated in the ceramic substrate after 2000 cooling and heating cycles, and the thermal cycle reliability was excellent. In Examples 1 to 7 of the present invention, the first copper layer had a thickness of 0.1 mm or more and 0.3 mm or less, and the second copper layer had a thickness of 0.5 mm or more and 0.9 mm or less, with the second copper layer being thicker than the first copper layer.
[0085] From the results of the above confirmatory experiments, it was confirmed that the present invention can provide an insulating circuit board having thermal cycle reliability that enables use even in applications where severe thermal cycles are applied in high-temperature environments and excellent heat dissipation properties, a semiconductor device using this insulating circuit board, and a method for manufacturing the insulating circuit board. [Explanation of symbols]
[0086] 1,101 Semiconductor devices 11 Ceramic substrate 20,120 circuit layers 21,121 Copper 1 layer 22,122 Copper 2 layer 30,130 metal layer 131 Third copper layer 132 4th copper layer
Claims
1. An insulating circuit board comprising a ceramic substrate and a circuit layer formed on a surface of the ceramic substrate, the circuit layer has a first copper layer disposed on the ceramic substrate side and a second copper layer laminated on the first copper layer, The first copper plate constituting the first copper layer has a semi-softening temperature of 200° C. or less, 1. An insulating circuit board, comprising: a second copper plate constituting the second copper layer having a half-softening temperature higher than a half-softening temperature of a first copper plate constituting the first copper layer.
2. a metal layer is formed on a surface of the ceramic substrate opposite to the circuit layer, the metal layer having a third copper layer disposed on the ceramic substrate side and a fourth copper layer laminated on the third copper layer; The third copper plate constituting the third copper layer has a semi-softening temperature of 200° C. or less, 2. The insulating circuit board according to claim 1, wherein the semi-softening temperature of the fourth copper plate constituting the fourth copper layer is higher than the semi-softening temperature of the third copper plate constituting the third copper layer.
3. A semiconductor device comprising: the insulating circuit board according to claim 1; and a semiconductor element mounted on the circuit layer.
4. 4. The semiconductor device according to claim 3, wherein the insulating circuit board and the semiconductor element are resin-encapsulated with an insulating resin.
5. A method for producing the insulating circuit board according to claim 1, comprising the steps of: a first copper layer forming step of joining the first copper plate to the ceramic substrate to form the first copper layer, and a second copper layer forming step of joining the second copper plate to the first copper layer to form the second copper layer, A method for producing an insulating circuit board, comprising the steps of: forming the first copper layer and forming the second copper layer simultaneously.
6. A method for producing the insulating circuit board according to claim 2, comprising the steps of: a third copper layer forming step of joining the third copper plate to the ceramic substrate to form the third copper layer, and a fourth copper layer forming step of joining the fourth copper plate to the third copper layer to form the fourth copper layer, 4. A method for producing an insulating circuit board, comprising the steps of: forming the third copper layer and forming the fourth copper layer simultaneously.
7. A method for producing the insulating circuit board according to claim 1, comprising the steps of: a first copper layer forming step of joining the first copper plate to the ceramic substrate to form the first copper layer; a circuit pattern forming step of forming a circuit pattern on the first copper layer; a second copper layer forming step of bonding the second copper plate to at least an element mounting area, on which a semiconductor element is mounted, of the first copper layer on which the circuit pattern is formed, to form the second copper layer; 2. A method for producing an insulating circuit board comprising the steps of:
Citation Information
Patent Citations
Circuit board and semiconductor module employing it
JP2007299973A
Power module substrate, power module substrate with heat sink, power module and power module substrate manufacturing method
JP2013041913A
Insulation circuit board and manufacturing method thereof
JP2019149460A
Insulation circuit board and manufacturing method of the insulation circuit board
JP2019169540A