Granular carrier, granular pharmaceutical composition, absorbent article, and method for producing granular carrier

The production of biodegradable granular carriers using cross-linked carboxyalkylcellulose salt via reverse-phase suspension polymerization addresses environmental issues of polyacrylic acid-based polymers by creating uniform, strong, and transparent gel particles suitable for drug absorption and disposal.

JP2024141881AActive Publication Date: 2024-10-10S T CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023053742
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

The use of polyacrylic acid-based superabsorbent polymers in disposable products poses environmental concerns due to non-biodegradability, high manufacturing costs, and CO2 emissions, necessitating the development of biodegradable alternatives.

Method used

A method for producing a granular carrier using cross-linked carboxyalkylcellulose salt through reverse-phase suspension polymerization, involving the steps of dissolving carboxyalkylcellulose in an alkaline solution, mixing with a crosslinking agent, and dispersing in a low polar organic solvent to form uniform, spherical gel particles.

Benefits of technology

The method produces biodegradable granular carriers that form gel particles with a smooth surface and uniform size, enhancing strength and transparency, and allows for efficient drug loading and absorption, reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141881000001_ABST
    Figure 2024141881000001_ABST
Patent Text Reader

Abstract

To provide a granular carrier which, by being made to absorb water, forms gel particles having a smooth surface and a uniform size.SOLUTION: The method for producing the granular carrier comprises: dissolving carboxyalkyl cellulose and / or its salt in an alkaline aqueous solution to prepare an aqueous solution of a carboxyalkyl cellulose salt; preparing a mixture of the aqueous solution of the carboxyalkyl cellulose salt and a cross-linking agent; dispersing the mixture in a low-polarity organic solvent to obtain a suspension; and allowing crosslinking polymerization of the carboxyalkyl cellulose salt to proceed in the suspension to form dispersed particles containing cross-linked bodies of the carboxyalkyl cellulose salt. The cross-linking polymerization is made to proceed by carrying out, in this order, a first step of stirring the suspension for 10 minutes or more in a temperature range of 43°C or less and a second step of stirring the suspension in a temperature range of 46°C or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a granular carrier. [Background technology]

[0002] Superabsorbent polymers (SAPs) absorb water when they come into contact with it and instantly become a transparent hydrated gel. This gel has the characteristic of retaining water without releasing water even when pressure is applied.

[0003] The applications of superabsorbent polymers are diverse. For example, in the field of sanitary products, superabsorbent polymers are used as highly absorbent substances in absorbent articles such as paper diapers and sanitary napkins for women. In addition, superabsorbent polymers are also used as carriers in gel preparations that absorb and support aqueous liquid compositions containing chemicals such as fragrances and deodorants. Gel preparations containing carriers made of such superabsorbent polymers are widely used in stationary air fresheners and deodorants because there is no risk of liquid spilling from the container and they have excellent design.

[0004] Currently, polyacrylic acid-based SAP is the mainstream of superabsorbent polymers (SAP) from the viewpoints of ease of synthesis, cost, etc. However, since polyacrylic acid-based SAP is made from petroleum, there is a problem that the production cost is affected by fluctuations and increases in crude oil prices, and there is also a large amount of CO2 emission during production and disposal. In particular, for diaper applications, polyacrylic acid-based SAP is disposed of in a water-absorbed state, so a large amount of energy is required for incineration, resulting in particularly large amounts of CO2 emission. In addition, since polyacrylic acid-based SAP is not biodegradable, problems such as soil pollution occur when it is landfilled.

[0005] Thus, the use of polyacrylic acid-based SAP as a superabsorbent polymer (SAP) may cause environmental problems. Since the demand for paper diapers is expected to rapidly increase in emerging countries in the future, it is desirable to use biodegradable natural polymers as superabsorbent polymers. For these reasons, superabsorbent polymers using plant-derived raw materials such as polysaccharides have been proposed.

[0006] For example, Patent Documents 1 to 3 propose a cellulose-based SAP consisting of a cross-linked polymer of carboxymethyl cellulose (CMC) or CMC salt as a biodegradable, highly water-absorbent polymer to replace polyacrylic acid-based SAP. This CMC is a water-soluble cellulose derivative, and is synthesized by etherifying the hydroxyl groups of cellulose with chloroacetic acid or the like. Its aqueous solution exhibits anionic properties, high viscosity, and excellent dispersibility, and is therefore widely used as a thickener, dispersant, and stabilizer. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2011-140534 A [Patent Document 2] International Publication No. 2012 / 147255 [Patent Document 3] JP 2008-285611 A Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a biodegradable granular carrier which, upon absorption of water, produces gel particles having a smooth surface and uniform size. [Means for solving the problem]

[0009] According to one aspect of the present invention, there is provided a method for producing a granular carrier containing a crosslinked body of a carboxyalkyl cellulose salt, comprising dissolving carboxyalkyl cellulose and / or a salt thereof in an alkaline aqueous solution to prepare an aqueous solution of a carboxyalkyl cellulose salt, preparing a mixture of the aqueous solution of the carboxyalkyl cellulose salt and a crosslinking agent, dispersing the mixture in a low-polarity organic solvent to form a suspension, and allowing crosslinking polymerization of the carboxyalkyl cellulose salt to proceed in the suspension to form dispersed particles containing the crosslinked body of the carboxyalkyl cellulose salt, wherein the crosslinking polymerization proceeds by carrying out, in that order, a first step of stirring the suspension for at least 10 minutes within a temperature range of 43°C or less, and a second step of stirring the suspension within a temperature range of 46°C or more.

[0010] According to another aspect of the present invention, there is provided a method for producing a suspension according to the above aspect, wherein in the first step, the suspension is stirred for a period of 10 to 120 minutes within a temperature range of 15°C to 43°C, and in the second step, the suspension is stirred for a period of 120 to 360 minutes within a temperature range of 46°C to 80°C.

[0011] According to yet another aspect of the present invention, there is provided a manufacturing method according to any of the above aspects, further comprising separating the dispersed particles from the dispersion medium contained in the suspension, washing the dispersed particles separated from the dispersion medium, and drying the washed dispersed particles to obtain a dry granular carrier.

[0012] According to yet another aspect of the present invention, there is provided a method for producing the granular carrier in a dry state, the proportion of the total mass of particles having a particle size in the range of more than 1.4 mm and not more than 3.35 mm being 75% or more of the total mass of all particles.

[0013] According to yet another aspect of the present invention, a carboxyalkyl cellulose and / or a salt thereof having a viscosity of 5 mPa·s to 300 mPa·s in a 1 mass% aqueous solution at 25°C is used in preparing the carboxyalkyl cellulose salt aqueous solution, and the low-polarity organic solvent is a low-polarity organic solvent having a relative dielectric constant of 10 or less at 25°C and a kinetic viscosity of 10 mm 2 / g or more of an organic solvent is used in the process according to any of the above aspects.

[0014] According to yet another aspect of the present invention, there is provided the method according to any one of the above aspects, wherein the low-polarity organic solvent is liquid paraffin or silicone oil.

[0015] According to yet another aspect of the present invention, there is provided a method according to any one of the above aspects, wherein the ratio X / Y of the mass X of the carboxyalkyl cellulose and / or salt thereof to the mass Y of the crosslinking agent in the mixture is within the range of 10 / 2 to 10 / 5.

[0016] According to yet another aspect of the present invention, there is provided the method according to any one of the above aspects, wherein the crosslinking agent is a compound having two or more epoxy groups in the molecule.

[0017] According to yet another aspect of the present invention, there is provided a dry granular carrier produced by the production method according to any one of the above aspects.

[0018] According to yet another aspect of the present invention, there is provided a dry granular carrier comprising a crosslinked salt of carboxyalkyl cellulose, wherein the proportion of the total mass of particles having a particle size in the range of more than 1.4 mm and not more than 3.35 mm to the total mass of all particles is 75% or more, and the granular carrier produces gel particles having a smooth surface upon absorbing water.

[0019] According to yet another aspect of the present invention, there is provided a granular carrier according to any of the above aspects, wherein the proportion of the total mass of particles having a particle size in the range of more than 1.4 mm and not more than 3.35 mm to the total mass of all particles is 99% or less.

[0020] According to yet another aspect of the present invention, there is provided a granular carrier according to any of the above aspects, wherein the proportion of the total mass of particles having a particle size in the range of greater than 2.0 mm and not greater than 3.35 mm to the total mass of all particles is in the range of 56% to 86%.

[0021] According to yet another aspect of the present invention, there is provided a granular carrier according to any of the above aspects, wherein the proportion of the total mass of particles having a particle size of 1.4 mm or less in the total mass of all particles is 10% or less, and the proportion of the total mass of particles having a particle size larger than 3.35 in the total mass of all particles is 15% or less.

[0022] According to yet another aspect of the present invention, there is provided a granular carrier according to any of the above aspects for use in carrying a drug.

[0023] According to yet another aspect of the present invention, there is provided a granular drug composition comprising a granular carrier according to any of the above aspects and a liquid composition supported on the granular carrier and containing at least one drug selected from drugs having aromatic, deodorizing, odor eliminating, insect repellent, insecticidal or antifungal properties.

[0024] According to yet another aspect of the present invention, there is provided a granular pharmaceutical composition according to the above aspect, which is an air freshener composition or a deodorant composition.

[0025] According to yet another aspect of the present invention, there is provided an absorbent article comprising a granular carrier according to any of the above aspects. Effect of the Invention

[0026] According to the present invention, there is provided a biodegradable granular carrier which upon absorption of water produces gel particles having a smooth surface and uniform size. [Brief description of the drawings]

[0027] [Figure 1] FIG. 1 is a flow diagram showing an example of a method for producing a granular carrier according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a graph showing an example of heating conditions that can be employed in the reversed phase suspension polymerization step in the method for producing a granular carrier according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a photograph of the granular carrier produced in Example 3-4, where (a) shows the dry gel particles and (b) shows the water-absorbed gel particles. [Figure 4] Figure 4 is a photograph comparing the particle shape of the granular carrier of the reference example with the particle shape of crushed gel particles for comparison, where (a) shows the crushed gel particles (dry state) produced in Example 4-1, and (b) shows the granular carrier 2 (dry state) produced in Example 1-2. [Diagram 5] Figure 5 is a photograph comparing the particle shape of the granular carrier of the reference example with the particle shape of crushed gel particles for comparison, where (a) shows the crushed gel particles (in a water-absorbed state) produced in Example 4-1, and (b) shows the granular carrier 2 (in a water-absorbed state) produced in Example 1-2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments described below are more specific embodiments of any of the above aspects. The following items can be incorporated into each of the above aspects alone or in combination.

[0029] The granular carrier according to the embodiment of the present invention is a dried product of gel particles containing a crosslinked body of carboxyalkyl cellulose salt, and is obtained by drying gel particles derived from dispersed particles formed by suspension polymerization (i.e., reversed-phase suspension polymerization) in a suspension containing a low-polarity organic solvent as a dispersion medium, as described below. The granular carrier derived from dispersed particles obtained through the formation of a crosslinked body of carboxyalkyl cellulose salt by reversed-phase suspension polymerization produces gel particles with a smooth surface, for example, a substantially spherical shape, and a uniform size, when absorbed with water. These gel particles are also excellent in strength and transparency. According to the manufacturing method according to the embodiment of the present invention, a granular carrier having such characteristics can be easily obtained without undergoing processes such as crushing and classifying the gel body.

[0030] The method for producing a granular carrier according to an embodiment of the present invention includes dissolving carboxyalkyl cellulose and / or its salt in an alkaline aqueous solution to prepare an aqueous solution of a carboxyalkyl cellulose salt, preparing a mixture of the aqueous solution of a carboxyalkyl cellulose salt and a crosslinking agent, dispersing the mixture in a low-polarity organic solvent to obtain a suspension, and crosslinking polymerization of the carboxyalkyl cellulose salt in the suspension to form dispersed particles containing a crosslinked body of the carboxyalkyl cellulose salt. The crosslinking polymerization is then carried out in the following order: a first step of stirring the suspension under first conditions; and a second step of stirring the suspension under second conditions.

[0031] In this manufacturing method, the carboxyalkyl cellulose or its salt used as the raw material is preferably a carboxyalkyl cellulose or its salt having an alkyl group having 1 to 3 carbon atoms, for example, from the viewpoint of manufacturing cost. Specific examples of the carboxyalkyl cellulose or its salt include carboxymethyl cellulose, carboxyethyl cellulose, carboxybutyl cellulose, and salts thereof. The carboxyalkyl cellulose and / or its salt can be used alone or in combination of two or more.

[0032] It is preferable to select carboxyalkyl cellulose and / or its salts having a viscosity of 1% by mass aqueous solution within a predetermined range. The longer the polymer chain of carboxyalkyl cellulose, the higher the viscosity when dissolved, and the lower the handling property when injected into the low-polarity organic solvent, which is the dispersion medium. As a result, there is a risk of adversely affecting the uniformity of the particle shape and particle size of the obtained granular carrier. On the other hand, the longer the polymer chain of carboxyalkyl cellulose, the higher the water absorption. A high water absorption means that a large amount of drug can be supported when the granular carrier is used as a drug carrier. However, if the water absorption is too high, problems such as a decrease in gel strength and an increase in water separation may occur. From these points of view, it is preferable to use carboxyalkyl cellulose and / or its salts having a viscosity of 5 mPa·s or more and 300 mPa·s or less in a 1% by mass aqueous solution.

[0033] Here, the viscosity of a 1% by mass aqueous solution of carboxyalkyl cellulose and / or a salt thereof is the viscosity value measured with a B-type viscometer for a 200 mL aqueous solution of carboxyalkyl cellulose prepared to have a solid content of 1% by mass. Hereinafter, the viscosity of a 1% by mass aqueous solution of carboxyalkyl cellulose and / or a salt thereof measured under these conditions will be simply referred to as the "viscosity of carboxyalkyl cellulose." The viscosity of carboxyalkyl cellulose is preferably 10 mPa·s or more and 100 mPa·s or less, more preferably 20 mPa·s or more and 50 mPa·s or less.

[0034] In addition, the average degree of etherification (average degree of substitution, DS) of the carboxyalkyl cellulose is, for example, 0.5 to 1.5. By using a carboxyalkyl cellulose having an average degree of etherification in this range, the water absorption and strength of the gel can be easily improved. The average degree of etherification (average degree of substitution) is the average of the degrees of substitution of hydroxyl groups at the 2nd, 3rd, and 6th positions of the glucose units constituting the cellulose.

[0035] Fig. 1 is a flow diagram showing an example of a method for producing a granular carrier according to an embodiment of the present invention. The production method shown in Fig. 1 includes a step S1 of dissolving carboxyalkyl cellulose and / or its salt in an alkaline aqueous solution to prepare a carboxyalkyl cellulose salt aqueous solution, a step S2 of preparing a mixture of the carboxyalkyl cellulose salt aqueous solution obtained in step S1 and a crosslinking agent, a step S3 of dispersing the mixture obtained in step S2 in a low-polarity organic solvent to form a suspension (reverse phase suspension), and a step S4 of forming dispersed particles containing a crosslinked body of the carboxyalkyl cellulose salt by proceeding with crosslinking polymerization of the carboxyalkyl cellulose salt in this suspension, and a step S4 of separating (filtering) the dispersed particles formed in step S3 from the suspension, washing, and drying.

[0036] As described above, the manufacturing method shown in Fig. 1 is one example. In other examples, the manufacturing method according to the embodiment of the present invention may further include other steps not shown in Fig. 1. Furthermore, step S4 is an optional step that is performed as necessary, as described below. In other words, the manufacturing method according to the embodiment of the present invention may not include step S4.

[0037] In step S1, carboxyalkyl cellulose and / or its salt are added (injected) into an aqueous alkali solution, and completely dissolved, for example, by stirring at room temperature, to prepare an aqueous carboxyalkyl cellulose salt solution. In step S1, the time required to prepare the aqueous carboxyalkyl cellulose salt solution can be appropriately set, but according to one example, it can be 1 to 5 hours. After adding the carboxyalkyl cellulose to the aqueous alkali solution, a defoaming treatment can be performed, if necessary, by reducing the pressure or by leaving the solution at normal pressure for a predetermined time.

[0038] In step S1, the carboxyalkyl cellulose and / or a salt thereof may be one obtained by carboxyalkylating cellulose such as pulp as a starting material in a conventional manner, or a commercially available carboxyalkyl cellulose and / or a salt thereof may be used.

[0039] The carboxyalkylcellulose salt contained in the carboxyalkylcellulose salt aqueous solution obtained in step S1 is, for example, an alkali metal salt or an alkaline earth metal salt of carboxyalkylcellulose. In this case, an alkali aqueous solution containing an alkali metal or an alkaline earth metal is used as the alkali aqueous solution to which carboxyalkylcellulose and / or its salt is added. Examples of carboxyalkylcellulose salts include sodium salts, potassium salts, and calcium salts. In this case, an aqueous solution of sodium hydroxide, potassium hydroxide, or calcium hydroxide is used as the alkali aqueous solution to which carboxyalkylcellulose is added. According to one example, sodium carboxymethylcellulose (CMC-Na) is used as the carboxyalkylcellulose and / or its salt, and sodium hydroxide is used as the alkali aqueous solution to prepare a CMC-Na aqueous solution in step S1.

[0040] In step S2, the carboxyalkyl cellulose salt aqueous solution obtained in step S1 is mixed with a crosslinking agent to prepare a mixture of the carboxyalkyl cellulose salt aqueous solution and the crosslinking agent. In the following, when the term "mixture" is used simply, this refers to the mixture of the carboxyalkyl cellulose salt aqueous solution and the crosslinking agent prepared in step S2.

[0041] The mixing of the aqueous carboxyalkyl cellulose salt solution and the crosslinking agent is preferably carried out at a temperature range of 15°C to 43°C, more preferably at a temperature range of 20°C to 35°C, for example, using a static mixer. If the temperature is lowered, the viscosity of the mixture increases, and the handling properties decrease. In addition, in step S2, the crosslinking reaction of the carboxyalkyl cellulose salt starts immediately after the crosslinking agent is added to the aqueous carboxyalkyl cellulose salt solution, and the viscosity starts to increase. By appropriately lowering the temperature during this mixing, the crosslinking reaction can be prevented from proceeding too quickly or excessively, and excellent handling properties can be achieved. After mixing, a degassing operation under reduced pressure may be performed as necessary.

[0042] The above-mentioned crosslinking agent is not particularly limited as long as it can crosslink carboxyalkyl cellulose.As this crosslinking agent, for example, polyepoxy compound, polyglycidyl compound, polyaldehyde compound, polycarboxylic acid, vinyl ether compound, methylol compound, polyisocyanate, polyoxazoline compound, polyvinyl compound, polyacrylate compound, polymethacrylate compound, polyhalogen compound, methylenebisacrylamide, epichlorohydrin, polyacid anhydride, citric acid, methylenebisacrylamide, glycidyl methacrylate and other known compounds can be used.

[0043] Preferred specific examples of the crosslinking agent include (a) a compound having two or more hydroxyl groups in the molecule, (b) a compound having two or more polymerizable double bonds, and (c) a compound having two or more epoxy groups.

[0044] (a) Examples of compounds having two or more hydroxyl groups in the molecule include ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, glycerin, polyglycerin, propylene glycol, diethanolamine, polyoxypropylene, sorbitan fatty acid esters, trimethylolpropane, pentaerythritol, 1,3-propanediol, and sorbitol.

[0045] (b) Examples of compounds having two or more polymerizable double bonds in the molecule include bis(meth)acrylamide, allyl(meth)acrylamide, diethylene glycol diacrylate, trimethylolpropane triacrylate, polyethylene glycol diacrylate, and ethoxylated trimethylolpropane triacrylate.

[0046] (c) Examples of compounds having two or more epoxy groups in the molecule include ethylene glycol diglycidyl ether (EGDE), polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerin triglycidyl ether, resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, and polyglycidyl ethers such as glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, sorbitol polyglycidyl ether, and pentaerythritol polyglycidyl ether.

[0047] Among these, from the viewpoints of reactivity and the water absorption performance of the resulting granular carrier, (b) a compound having two or more polymerizable double bonds in its molecule, and (c) a compound having two or more epoxy groups in its molecule are preferred, (c) a compound having two or more epoxy groups in its molecule is more preferred, polyglycidyl ether is even more preferred, and ethylene glycol diglycidyl ether (EGDE) is particularly preferred.

[0048] The compounding ratio of the carboxyalkyl cellulose and / or its salt to the crosslinking agent can be appropriately set. From the viewpoint of the shape, transparency and strength of the granular carrier, the ratio X / Y of the mass X of the carboxyalkyl cellulose and / or its salt to the mass Y of the crosslinking agent is preferably within the range of 10 / 2 to 10 / 5, more preferably within the range of 10 / 2 to 10 / 4.

[0049] In step S3, the mixture obtained in step S2 is added (injected) into a low-polarity organic solvent and dispersed to form a suspension (reverse phase suspension), and dispersed particles containing crosslinked bodies of carboxyalkyl cellulose salt are formed by crosslinking polymerization in this suspension.

[0050] The low-polarity organic solvent used as the dispersion medium in step S3 is a low-polarity organic solvent having a relative dielectric constant at 25°C of, for example, 10 or less, and has a lower polarity than the above mixture of dispersoids. Therefore, the suspension prepared in step S3 is a reversed-phase suspension, and the cross-linking polymerization of the carboxyalkyl cellulose salt is reversed-phase suspension polymerization. Here, the relative dielectric constant is the relative dielectric constant at 25°C measured by a capacitance meter. It is more preferable that the low-polarity organic solvent used as the dispersion medium has a relative dielectric constant in the range of 3 to 6.

[0051] Examples of low-polarity organic solvents having a relative dielectric constant of 10 or less include aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, liquid paraffin, and silicone oil. These can be used alone or in combination of two or more.

[0052] The low polarity organic solvent used in step S3 has a kinetic viscosity of 10 mm at 37.8° C. 2 It is preferable that the dispersion medium is a viscous fluid having a kinetic viscosity of 10 mm / s or more. When the dispersion medium is a viscous fluid, the aggregation of the generated spherical gel particles can be suppressed, or the adhesion between the spherical gel particles can be suppressed, thereby suppressing the formation of clumps of the spherical gel particles. 2 It is important that the molecular weight is at least 1 / s in order to obtain granular carriers that are spherical in shape and uniform in size.

[0053] Here, the kinematic viscosity is the kinematic viscosity at 37.8° C. measured by a vibration viscometer. According to one example, the low polarity organic solvent used as the dispersion medium has a kinematic viscosity of 10 mm 2 / s~100mm 2 / s, and according to other examples, 15 mm 2 / s~80mm 2 / s, and according to another example, 20 mm 2 / s~50mm 2 / s range.

[0054] Among the above-mentioned specific examples of low-polarity organic solvents having a relative dielectric constant of 10 or less, liquid paraffin and silicone oil are particularly preferable as the low-polarity organic solvent to be used in step S3 because they are viscous fluids.

[0055] The liquid paraffin is not particularly limited as long as it is a paraffin that is liquid at room temperature, and examples thereof include liquid saturated hydrocarbons having 12 to 50 carbon atoms, and may be any of n-paraffin, isoparaffin, and naphthene. In addition, examples of commercially available products that can be used include Moresco White, Moresco Bioless (all trade names, manufactured by Matsumura Oil Research Institute), Stanol, Krystoll, Esso White Oil, and Purelex (all trade names, manufactured by Esso Oil). These may be used alone, or two or more of them may be used in combination.

[0056] Silicone oil is not particularly limited as long as it is liquid at room temperature and has a siloxane structure, and examples thereof include polysiloxane oils such as dimethyl silicone oil. Silicone oils may have functional groups such as hydroxyl, carboxyl, amino, epoxy, cyano, mercapto, trifluoropropyl, chlorophenyl, and long-chain alkyl groups, or may be modified silicone oils modified with polyether, alcohol, etc. These may be used alone or in combination of two or more.

[0057] In step S3, the above-mentioned crosslinking agent may be further added to the low-polarity organic solvent to cause surface crosslinking (secondary crosslinking) in the gel particles, thereby providing a portion with high crosslink density in the surface layer. By causing surface crosslinking (secondary crosslinking), it is possible to improve the gel strength while maintaining the water absorption capacity.

[0058] In step S3, the low-polarity organic solvent is adjusted to a sufficiently low temperature immediately before the mixture obtained in step S2 is added. The temperature of the low-polarity organic solvent is preferably kept within a range of 15° C. to 43° C., and more preferably within a range of 15° C. to 30° C.

[0059] The mixture obtained in step S2 is also adjusted to a sufficiently low temperature immediately before being added to the low-polarity organic solvent. The temperature of this mixture is preferably within the above-mentioned range for the temperature when the aqueous carboxyalkyl cellulose salt solution and the crosslinking agent are mixed.

[0060] As described above, the crosslinking reaction of the carboxyalkyl cellulose salt starts immediately after the crosslinking agent is added to the aqueous carboxyalkyl cellulose salt solution. It is preferable that the time from mixing the aqueous carboxyalkyl cellulose salt solution with the crosslinking agent to adding this mixture to the low-polarity organic solvent is within 30 minutes.

[0061] In step S3, stirring of the low polarity organic solvent is started before the addition of the mixture obtained in step S2, and this stirring is continued at least until the crosslinking polymerization is completed. Examples of the stirring device include a mechanical stirrer, and examples of the stirring blade include an anchor type, a propeller type, and a paddle type, and can be appropriately selected and used. According to one example, in step S3, the low polarity organic solvent is stirred at a rotation speed of 50 to 500 rpm, according to another example, at a rotation speed of 200 to 500 rpm, and according to yet another example, at a rotation speed of 250 to 400 rpm.

[0062] In step S3, the mixture obtained in step S2 is added (injected) into the low-polarity organic solvent, for example, by dripping the mixture drop by drop from the liquid surface of the low-polarity organic solvent using a pipette (hereinafter, sometimes referred to as the "drop injection method"). Another example is by continuously injecting the mixture while immersing a pipette in the low-polarity organic solvent (hereinafter, sometimes referred to as the "continuous injection method"). The drop injection method is preferred because it is easy to obtain uniform particle sizes of dispersed particles. The continuous injection method is preferred because it can be easily performed in a short time.

[0063] In step S3, the total time required for the cross-linking polymerization reaction of the carboxyalkyl cellulose salt can be appropriately set. According to one example, it can be set to 1 hour to 6 hours.

[0064] In step S3, the cross-linking polymerization is carried out by carrying out a first step of stirring the suspension under a first condition and a second step of stirring the suspension under a second condition in this order. This will be described with reference to FIG.

[0065] Fig. 2 is a graph showing an example of heating conditions that can be used in the reverse phase suspension polymerization step in the method for producing a granular carrier according to an embodiment of the present invention. In Fig. 2, the curve marked "room temperature" shows an example of heating conditions that can be used in the reverse phase suspension polymerization step in the method for producing a granular carrier according to an embodiment of the present invention. In addition, the curve marked "heated" shows an example of heating conditions according to a comparative example.

[0066] The stirring under the first conditions is stirring of the suspension for a time t1 of 10 minutes or more at a first temperature T1 in a temperature range of 43° C. or less. The time t1 described here is the elapsed time from the time point at which the addition of the mixture obtained in step S2 to the low-polarity organic solvent is completed. The stirring under the first conditions is preferably stirring for a time t1 of 10 minutes to 120 minutes at a temperature range of 15° C. to 43° C., and more preferably stirring for a time of 20 minutes to 60 minutes at a temperature range of 15° C. to 40° C.

[0067] The stirring under the second conditions is stirring of the suspension at a second temperature T2 higher than the first temperature T1, which is a temperature range of 46° C. or higher. The stirring under the second conditions is preferably stirring at a temperature range of 46° C. to 80° C. for a time t2 of 120 to 360 minutes, and more preferably stirring at a temperature range of 46° C. to 60° C. for a time t2 of 240 to 300 minutes.

[0068] Immediately after the mixture obtained in step S2 is added to the low-polarity organic solvent, coalescence or splitting of the dispersed particles may occur. As shown by the curve labeled "warming", if the temperature is set high when the mixture obtained in step S2 is added to the low-polarity organic solvent and the temperature is then rapidly increased, cross-linking polymerization proceeds rapidly. Therefore, splitting of the coalesced dispersed particles and coalescence of the split dispersed particles are unlikely to occur. Therefore, the particle size of the dispersed particles at the end of step S3 is not sufficiently uniform.

[0069] In contrast, in the method of the present embodiment, as shown by the curve labeled "room temperature", first, in the first step, stirring is continued for a sufficiently long time under temperature conditions where cross-linking polymerization does not proceed rapidly. Therefore, in the first step, the particle size becomes uniform due to the coalescence or division of the dispersed particles. In addition, in the first step, since the cross-linking polymerization proceeds slowly, further coalescence or division of the dispersed particles becomes difficult to occur as the particle size becomes uniform. Therefore, the particle size of the dispersed particles is uniform at the time when the first step is completed.

[0070] In the method of the present embodiment, the stirring in the second step is performed at a higher temperature, which allows the cross-linking polymerization to proceed sufficiently, and therefore allows the step S3 to be completed in a sufficiently short time.

[0071] Thereafter, as shown in FIG. 1, step S4 is carried out. That is, the dispersed particles formed in the suspension in step S3 are removed from the suspension by, for example, filtration, and washed and dried as necessary. The washing after filtration includes, for example, washing the low polarity organic solvent attached to the surface of the gel particles with an aqueous detergent solution such as a surfactant, and / or immersing the gel particles in ethanol to dehydrate and dealkalize them. Drying can be carried out, for example, by air drying. When a solvent with a low boiling point such as n-hexane is used as the low polarity organic solvent, the solvent on the surface of the gel particles can be removed without washing by using a method such as reduced pressure distillation.

[0072] As described above, step S4 is an optional step, and the dispersed particles may be distributed as a product in a state where they are dispersed in the dispersion medium contained in the suspension without being taken out of the suspension. That is, the granular carrier according to this embodiment may be gel particles, which are dispersed particles generated by reverse phase suspension polymerization in the suspension formed in step S3, and the gel particles may be taken out of the dispersion medium or may be dispersed in the dispersion medium. In addition, the granular carrier according to this embodiment may be a dried product of the gel particles. Alternatively, the granular carrier according to this embodiment may be a gel particle obtained by absorbing a liquid into the dried product. Note that these dried products can absorb water to produce gel particles having a smooth surface, for example, gel particles having a shape almost the same as that before drying.

[0073] As described above, the method of the present embodiment can produce gel particles having a uniform particle size. Since the gel particles have a uniform particle size, the dried product thereof, i.e., the granular carrier in a dry state, also has a uniform particle size.

[0074] According to one example, the ratio of the total mass of particles having a particle diameter in the range of more than 1.4 mm and less than 3.35 mm to the total mass of all particles in the dry granular carrier is 75% or more. In this case, the ratio of the total mass of particles having a particle diameter in the range of more than 1.4 mm and less than 3.35 mm to the total mass of all particles is 99% or less. In this case, according to one example, the ratio of the total mass of particles having a particle diameter of 1.4 mm or less to the total mass of all particles is 10% or less, and the ratio of the total mass of particles having a particle diameter of more than 3.35 mm to the total mass of all particles is 15% or less. And in this case, the ratio of the total mass of particles having a particle diameter in the range of more than 2.0 mm and less than 3.35 mm to the total mass of all particles is in the range of 56% to 86%.

[0075] According to another example, the proportion of the total mass of particles having a particle diameter in the range of more than 1.4 mm and not more than 3.35 mm in the total mass of all particles in the dry granular carrier is 80% or more. In this case, the proportion of the total mass of particles having a particle diameter in the range of more than 1.4 mm and not more than 3.35 mm in the total mass of all particles is 99% or less in one example. In this case, according to one example, the proportion of the total mass of particles having a particle diameter in the range of more than 1.4 mm and not more than 3.35 mm in the total mass of all particles is 8% or less, and the proportion of the total mass of particles having a particle diameter in the range of more than 3.35 mm in the total mass of all particles is 12% or less. And in this case, the proportion of the total mass of particles having a particle diameter in the range of more than 2.0 mm and not more than 3.35 mm in the total mass of all particles is in the range of 61% to 81% in one example.

[0076] According to yet another example, the proportion of the total mass of particles having a particle diameter in the range of more than 1.4 mm and not more than 3.35 mm in the total mass of all particles in the dry granular carrier is 84% ​​or more. In this case, the proportion of the total mass of particles having a particle diameter in the range of more than 1.4 mm and not more than 3.35 mm in the total mass of all particles is 99% or less according to one example. In this case, the proportion of the total mass of particles having a particle diameter in the range of more than 1.4 mm and not more than 3.35 mm in the total mass of all particles is 7% or less, and the proportion of the total mass of particles having a particle diameter in the range of more than 3.35 mm in the total mass of all particles is 9% or less according to one example. And in this case, the proportion of the total mass of particles having a particle diameter in the range of more than 2.0 mm and not more than 3.35 mm in the total mass of all particles is in the range of 66% to 76% according to one example.

[0077] The proportion of the total mass of particles having a particle size of 1.4 mm or less to the total mass of all particles is 0% or more in one example, 1% or more in another example, and 3% or more in yet another example. Also, the proportion of the total mass of particles having a particle size of more than 3.35 mm to the total mass of all particles is 0% or more in one example, 1% or more in another example, and 3% or more in yet another example.

[0078] The above ratio is a value obtained by the following method. That is, the dry granular carrier is sieved with three sieves having nominal openings of 3.35 mm, 2 mm, and 1.4 mm as specified in JIS Z8801-1:2019 to obtain four particle groups. Then, the masses of these four particle groups are measured. The above ratio is calculated from the values ​​obtained thereby. The dry granular carrier obtained by the above method may have various particle sizes. This particle size can be adjusted, for example, by the rotation speed of the stirring blade in step S3, particularly the first step of step S3, the heating conditions in the first step, the viscosity of the low-polarity organic solvent, and the viscosity of the mixture added to the low-polarity organic solvent. When the particle size of the dried product is uniform, the gel particles generated by absorbing water from these also have a uniform particle size.

[0079] The dry granular carrier can be used as a highly absorbent material in absorbent articles such as disposable diapers, sanitary products (napkins, tampons, etc.), pads (sweat pads, breast milk pads, incontinence pads, etc.), and pet toilets.

[0080] The granular carrier can also be used as a drug carrier. That is, a liquid composition containing at least one drug selected from drugs having, for example, aromatic, deodorant, deodorizing, insect repellent, insecticidal or antifungal properties is absorbed and carried by the granular carrier in a dry state. This makes it possible to provide gel preparations such as granular drug compositions, such as a granular fragrance composition, a granular deodorant composition, a granular deodorant composition, a granular insect repellent composition, a granular insecticide composition, and a granular antifungal composition.

[0081] In a gel preparation consisting of such a granular pharmaceutical composition, the pharmaceutical component contained in the liquid composition to be absorbed and carried by the granular carrier can be any of a variety of commonly used drugs depending on the purpose. For example, specific examples of aromatic drugs include animal fragrances such as musk, spirit cat fragrance, and dragon jasmine fragrance, and vegetable fragrances such as abies oil, acorn oil, almond oil, angelica root oil, page oil, bergamot oil, perch oil, boa rose oil, kayabuchi oil, gananga oil, capsicum oil, caraway oil, cardamom oil, cassia oil, celery oil, cinnamon oil, citronella oil, cognac oil, coriander oil, cumin oil, camphor oil, basil oil, estugoran oil, eucalyptus oil, fennel oil, garlic oil, ginger oil, grapefruit oil, hop oil, lemon oil, lemongrass oil, nutmeg oil, mandarin oil, peppermint oil, orange oil, sage oil, star anise oil, turpentine oil, rosemary oil, eucalyptus oil, anise oil, lavender oil, cumin oil, cinnamon oil, and hiba oil. In addition, artificial fragrances such as synthetic fragrances or extracted fragrances can also be used. Specific examples include hydrocarbon fragrances such as pinene and limonene, alcohol fragrances such as linalool, geraniol, citronellol, menthol, borneol, benzyl alcohol, anise alcohol, and β-phenethyl alcohol, phenol fragrances such as anethole and eugenol, aldehyde fragrances such as n-butyraldehyde, isobutyraldehyde, hexylaldehyde, citral, citronellal, benzaldehyde, and cinnamic aldehyde, ketone fragrances such as carvone, menthone, camphor, acetophenone, and ionone, lactone fragrances such as γ-butyrolactone, coumarin, and cineol, and ester fragrances such as octyl acetate, benzyl acetate, cinnamyl acetate, butyl propionate, and methyl benzoate. These may be used alone or in any combination of two or more.

[0082] The deodorant agent may be either a volatile agent or a non-volatile agent. Specific examples of deodorant agents include metal oxides such as titanium oxide and zinc oxide, flavonoid compounds, plant extracts such as catechin and polyphenol or derivatives thereof, cyclodextrin or derivatives thereof, and amine compounds. These may be used alone or in any combination of two or more.

[0083] Specific examples of deodorizing agents include carbon-based adsorbents, for example, activated carbon such as coconut shell activated carbon and charcoal such as binchotan charcoal, and silica-based adsorbents such as zeolite, silica gel, and layered zinc aluminosilicate, etc. These may be used alone or in any combination of two or more.

[0084] Specific examples of agents having insect repellent or insecticidal properties include pyrethroid insecticidal components such as empenthrin, transfluthrin, allethrin, fenothrin, eminence, and profluthrin, and volatile insect repellent and insecticidal components such as paradichlorobenzene, naphthalene, camphor, 2-phenoxyethanol, hinokitiol, and allyl isothiocyanate. These can be used alone or in any combination of two or more.

[0085] In addition to the above-mentioned drugs, various additives can be used in the liquid composition, specific examples of which include surfactants, colorants, preservatives, and pH adjusters.

[0086] The granular pharmaceutical composition can be prepared, for example, by impregnating a dry granular carrier with a liquid pharmaceutical composition.

[0087] Crushed gel particles (crushed gel) finely granulated by crushing are typically in the form of fragments having sharp corners, and most of the particles have a distorted shape that is difficult to call spherical. Moreover, such crushed gel particles have a non-uniform particle size. Therefore, most of the water-absorbed gel particles obtained by allowing the dried product of such crushed gel particles to absorb liquid also have sharp corners and are non-uniform in particle size.

[0088] When such water-absorbent gel particles are filled in a container, the gaps between the particles are small, making it difficult for air to flow. If air does not flow easily, when the water-absorbent gel particles contain a volatile chemical such as a fragrance or a non-volatile chemical such as a non-volatile deodorant, the chemical cannot function efficiently. In addition, such dried crushed gel particles or water-absorbed gel particles having non-uniform particle size and shape are not preferable from the viewpoint of aesthetics.

[0089] In contrast, according to the method described with reference to Figures 1 and 2, it is possible to produce granular carriers in a dry state with a uniform particle size, as described above. When these granular carriers absorb liquids such as water or liquid pharmaceutical compositions, they produce gel particles with a smooth surface, e.g., a substantially spherical shape, and a uniform size.

[0090] When such gel particles are filled in a container, the gaps between the particles are large, and air flow is likely to occur. Therefore, when the gel particles contain a volatile agent such as a fragrance or a non-volatile agent such as a non-volatile deodorant, the agent can be made to function efficiently. In addition, such gel particles having a uniform particle size and shape are also preferable from the viewpoint of aesthetics. Furthermore, the granular carrier in a dry state produced by absorbing water such as this gel particle also has a uniform particle size and shape, and has an excellent aesthetic appearance.

[0091] Furthermore, gel particles having a smooth surface are less likely to scatter light on the particle surface, unlike crushed gel particles that have been finely divided by crushing. That is, the dry granular carrier obtained by the method described with reference to Figures 1 and 2 produces gel particles with excellent transparency when liquid is absorbed into the carrier. In this respect, these gel particles also have excellent aesthetic appearance.

[0092] Furthermore, gel particles having a smooth surface are less likely to break than crushed gel particles that have been finely crushed. Similarly, dry granular carriers that produce gel particles having a smooth surface are less likely to break than dried crushed gel particles that have been finely crushed. In other words, the dry granular carriers obtained by the method described with reference to Figures 1 and 2 and the gel particles obtained by absorbing liquid therein are excellent in strength. EXAMPLES

[0093] ≪Example 1≫ CMC-Na viscosity <Example 1-1: Production of Granular Carrier 1> Sodium carboxymethylcellulose (CMC-Na) (Daicel 1110, Daicel Miraize Co., Ltd.) with a viscosity in the range of 10 to 20 mPa s was prepared. The viscosity here is the viscosity of a 1% by mass aqueous solution of CMC-Na at 25°C measured by the above-mentioned method.

[0094] 10.0 g of the above CMC-Na (Daicel 1110) was dissolved in 100 mL of 0.5 mol / L aqueous sodium hydroxide solution. 4.0 g of ethylene glycol diglycidyl ether (EGDE) (Denacol EX-810, Nagase ChemteX Corporation) was added dropwise to this aqueous solution as a crosslinking agent, and the solution was stirred for 20 minutes, after which it was degassed for 5 minutes under reduced pressure. This resulted in a mixture of an aqueous CMC-Na solution and EGDE. In this example, the blending mass ratio of CMC-Na to the crosslinking agent EGDE (CMC-Na / EGDE) was 10 / 4.

[0095] The mixture was then heated to 60° C. and stirred at a stirring speed (rotation speed of the stirring blade) of 250 rpm in a liquid paraffin (Moresco White P-100, manufactured by MORESCO Corporation, kinematic viscosity 20.5 mm 2 / s). A high-viscosity pipette was used to inject the mixture, and the tip of the pipette was immersed in the liquid paraffin while the mixture was injected. The mixture was allowed to react in the liquid paraffin for 4 hours while maintaining the temperature above. After the reaction, the gel particles formed were filtered off, and the liquid paraffin adhering to the gel particle surface was washed off with an appropriate amount of aqueous surfactant solution. The gel particles were then immersed in ethanol to dehydrate and dealkalize, and then air-dried to obtain a white to pale yellow solid (granular carrier 1).

[0096] <Examples 1-2 to 1-6: Production of Granular Carriers 2 to 6> Granular carriers 2 to 6 were produced in the same manner as in Example 1-1, except that CMC-Na shown in Table 1 below was used instead of CMC-Na (Daicel 1110, viscosity 10 to 20 mPa·s).

[0097] <Evaluation> [Handling when pouring into liquid paraffin (ease of pouring)] In the manufacturing process of each granular carrier, the handling property when injecting the mixture of CMC sodium salt and EGDE into liquid paraffin was evaluated from the viewpoint of ease of drawing into a pipette and ease of injection from the pipette into liquid paraffin according to the following criteria. The evaluation results are shown in Table 1. A: It can be easily aspirated and injected. B: Aspiration and injection take some time, but are not difficult. C: Difficult to suction and inject.

[0098] [Shape of granular carrier (dried gel)] The shape of each of the resulting granular carriers (dried gels) was visually evaluated according to the following criteria. The evaluation results are shown in Table 1. A: Spherical dry gels make up almost the entire sample, and non-spherical dry gels are hardly observed. B: Mostly spherical dry gel. Flat or thread-like dry gel is mixed in, but not noticeable. C: Most of the gel is thread-like, with few spherical gels.

[0099] [Transparency] Each of the obtained granular carriers (dried gel) was immersed in ion-exchanged water to absorb the maximum amount of water that it could absorb, and the transparency of the water-absorbed gel particles was evaluated visually according to the following criteria. The evaluation results are shown in Table 1. A: There is no cloudiness and the overall transparency is high. B: Some parts are cloudy, but more than 80% is transparent, and the overall appearance is transparent. C: There are many cloudy areas or the whole is cloudy, with low transparency overall.

[0100] [Strength] 1 g of each of the obtained granular carriers (dried gel particles) was filled into a 200 mL beaker, 150 mL of ion-exchanged water was added, and the mixture was left to stand overnight to obtain water-absorbed gel particles carrying the maximum amount of water that they could absorb. The water-absorbed gel particles were filtered to remove excess water, and then the water-absorbed gel particles were filled into a 200 mL beaker again. At this time, the inside of the container was piled up with approximately six layers of particles from the bottom to the top. These were used as evaluation samples, and the strength was evaluated according to the following criteria. The evaluation results are shown in Table 1. A: The strength at which a particle located at the bottom of a container and bearing a weight approximately six times its own weight maintains its spherical shape and uniformly sized gaps form between particles throughout the packed structure. B: Strength where at least some of the particles located at the bottom of the container and bearing a weight approximately six times their own weight are unable to maintain their spherical shape, and there are areas where no gaps are formed between the particles at the bottom. C: The strength at which a sphere cannot be maintained by its own weight alone.

[0101] [Table 1]

[0102] From Table 1, it can be seen that granular carriers 1 to 5 of Examples 1-1 to 1-5 are excellent in particle shape, transparency, and strength. Moreover, Examples 1-1 to 1-5 are also excellent in handleability when injecting the mixture into liquid paraffin, and it can be seen that granular carriers (gel particles) excellent in particle shape, transparency, and strength can be easily obtained by reverse suspension polymerization. On the other hand, it can be seen that it is difficult to produce spherical gel particles by reverse suspension polymerization in Example 1-6 (Comparative Example), which uses CMC with high viscosity.

[0103] Example 2: CMC-Na / crosslinking agent (mass ratio) <Examples 2-1 and 2-2: Production of Granular Carriers 7 and 8> Granular carriers 7 and 8 were produced in the same manner as in Example 1-2, except that the blending mass ratio of CMC-Na and EGDE was changed as shown in Table 2. The dried gel shape, transparency, and strength of each granular carrier were evaluated in the same manner as in Example 1-1. The evaluation results are shown in Table 2.

[0104] [Table 2]

[0105] In addition, in Example 2-1, the strength evaluation was B, but the portion where no gaps occurred between the particles was only a part of the bottommost part of the packed particles, and the fluidity of the air was ensured.

[0106] <Example 3> Dynamic viscosity of liquid paraffin and stirring speed <Examples 3-1 to 3-5: Production of Granular Carriers 9 to 13> Granular carriers were produced in the same manner as in Example 1-2, except that the liquid paraffin and stirring speed were changed as shown in Table 3. The dried gel shape of each granular carrier was evaluated in the same manner as in Example 1-1. The evaluation results are shown in Table 3.

[0107] [Table 3]

[0108] Low viscosity (kinematic viscosity 4.51mm 2In Examples 3-1 and 3-2, in which liquid paraffin (100 g / s) was used, the mixture accumulated at the bottom and coalesced, and granular gel particles could not be obtained.

[0109] In Example 3-3, the strength evaluation was B, but the portion where no gaps occurred between the particles was only a part of the bottom part of the packed particles, and air fluidity was ensured.

[0110] Example 4: Comparison of gel particle shapes <Example 4-1: Production of crushed gel> 10.0 g of CMC-Na (Daicel 1120, Daicel Miraize Co., Ltd.) was dissolved in 100 mL of 0.5 mol / L aqueous sodium hydroxide solution. 4.0 g of EGDE (Denacol EX-810, Nagase ChemteX Co., Ltd.) was added dropwise to this aqueous solution and stirred for 20 minutes. After degassing for 5 minutes under reduced pressure, the mixture was reacted for 4 hours in a thermostatic bath at 60°C. After the reaction, the gel-like material formed was removed from the beaker and roughly crushed using a mixer. The crushed gel obtained was immersed in ethanol to dehydrate and dealkalize, and then air-dried to obtain a white to pale yellow solid.

[0111] <Evaluation> Fig. 4(a) is a photograph of the dried pulverized gel particles produced in Example 4-1, and Fig. 5(a) is a photograph of the water-absorbed state thereof. Fig. 4(b) is a photograph of the granular carrier 2 (dried gel particles) produced in Example 1-2, and Fig. 5(b) is a photograph of the water-absorbed state thereof.

[0112] A comparison between (a) and (b) of FIG. 4 and a comparison between (a) and (b) of FIG. 5 makes it clear that the particle shapes of the granular carrier and the pulverized gel particles are completely different.

[0113] That is, from (a) of Figure 4 and (a) of Figure 5, it can be seen that the crushed gel particles obtained by the conventional method of crushing the hydrogel formed by aqueous solution polymerization are in the form of fragments having sharp corners, and most of the particles have a distorted shape that cannot be said to be spherical. On the other hand, from (b) of Figure 4 and (b) of Figure 5, the gel particles derived from the dispersed particles formed by reversed-phase suspension polymerization are spherical in shape and have a more uniform particle size than the crushed gel particles. From the above, it can be seen that the manufacturing method using reversed-phase suspension polymerization can easily obtain high-quality gel particles.

[0114] Example 5: Uniformity of particle shape and size Figure 3 is a photograph of the granular carrier 12 obtained in Example 3-4. (a) is a dry gel particle, and (b) is a water-absorbed gel particle. From the photograph in Figure 3, it can be seen that the granular carrier 12 is dominated by roughly spherical particles and has excellent uniformity in particle size.

[0115] Example 6: Heating conditions and particle size uniformity <Example 6-1: Production of Granular Carrier 14> Sodium carboxymethylcellulose (CMC-Na) (Daicel 1120, Daicel Miraize Co., Ltd.) with a viscosity in the range of 10 to 20 mPa s was prepared. The viscosity here is the viscosity of a 1% by mass aqueous solution of CMC-Na at 25°C measured by the above-mentioned method.

[0116] 10.0 g of the above CMC-Na (Daicel 1120) was dissolved in 100 mL of 0.5 mol / L aqueous sodium hydroxide solution. The solution was then left to stand overnight to defoam. 4.0 g of ethylene glycol diglycidyl ether (EGDE) (Denacol EX-810, Nagase ChemteX Corporation) was added dropwise to the aqueous solution as a crosslinking agent, and the solution was stirred at a stirring speed of 250 rpm for 30 minutes. This resulted in a mixture of an aqueous CMC-Na solution and EGDE. In this example, the blending mass ratio of CMC-Na to the crosslinking agent EGDE (CMC-Na / EGDE) was 10 / 4.

[0117] Next, liquid paraffin (Moresco White P-100, MORESCO Corporation, kinetic viscosity 20.5 mm) was placed in a 500 mL glass beaker. 2 The mixture was poured into a liquid paraffin (100 ml / s) stirred at 250 rpm while maintaining its temperature at room temperature. A high-viscosity pipette was used to inject the mixture, and the tip of the pipette was immersed in the liquid paraffin while the mixture was being injected. With stirring continued, the liquid temperature was kept at room temperature without heating for 5 minutes after the mixture had been injected, and then heating was started.

[0118] The liquid temperature changed as shown by the curve labeled "room temperature" in Figure 2. That is, the liquid temperature rose steadily from the start of heating. Once the liquid temperature reached 48.2°C, stirring was continued for an additional 4.5 hours.

[0119] The gel particles thus produced were then filtered, and the liquid paraffin adhering to the surface of the gel particles was washed off with an appropriate amount of an aqueous surfactant solution. The gel particles were then immersed in ethanol to dehydrate and dealkalinize them. The gel particles were then dried overnight at room temperature, and then further dried under reduced pressure. The drying under reduced pressure was carried out for approximately 3 hours using a desiccator connected to a pump. In this manner, a white to pale yellow solid (granular carrier 14) was obtained.

[0120] <Example 6-2: Production of Granular Carrier 15> A granular carrier 15 was produced in the same manner as in Example 6-1, except for the following points. That is, prior to injecting the mixture of the CMC-Na aqueous solution and EGDE, the temperature of the liquid paraffin was heated to 55.8°C. The liquid paraffin was stirred at a stirring speed of 250 rpm, and the mixture was injected into it. The mixture was injected in the same manner as in Example 6-1.

[0121] When heating was performed under the above conditions, the liquid temperature changed as shown by the curve labeled "Heating" in Figure 2. That is, the liquid temperature rose steadily. After the liquid temperature reached 49.2°C, stirring was continued for an additional 4.5 hours.

[0122] <Evaluation> Granular carriers 14 and 15 were each classified using sieves with openings of 3.35 mm, 2 mm, and 1.4 mm into particle sizes D (particle size)>3.35 mm, 3.35 mm≧D>2 mm, 2 mm≧D>1.4 mm, and 1.4 mm≧D. The results are shown in Table 4.

[0123] [Table 4]

[0124] From Table 4, it can be seen that granular carrier 14 is superior to granular carrier 15 in uniformity of particle size.

[0125] The present invention is not limited to the above-mentioned embodiment, and can be modified in various ways without departing from the gist of the present invention. The embodiments may be combined as appropriate, and in that case, the combined effect can be obtained. Furthermore, the above-mentioned embodiment includes various inventions, and various inventions can be extracted by combinations selected from the multiple components disclosed. For example, if the problem can be solved and the effect can be obtained even if some components are deleted from all the components shown in the embodiment, the configuration from which the components are deleted can be extracted as an invention. [Explanation of symbols]

[0126] S1...process, S2...process, S3...process, S4...process.

Claims

1. A method for producing a granular carrier containing a crosslinked product of a carboxyalkyl cellulose salt, comprising the steps of: dissolving carboxyalkyl cellulose and / or a salt thereof in an alkaline aqueous solution to prepare a carboxyalkyl cellulose salt aqueous solution; preparing a mixture of the aqueous carboxyalkyl cellulose salt solution and a crosslinking agent; dispersing the mixture in a low-polarity organic solvent to form a suspension, and allowing cross-linking polymerization of the carboxyalkyl cellulose salt to proceed in the suspension to form dispersed particles containing a cross-linked body of the carboxyalkyl cellulose salt; Including, The method for producing a granular carrier, in which the cross-linking polymerization proceeds by carrying out, in the order of a first step, stirring the suspension within a temperature range of 43°C or less for a period of 10 minutes or more, and a second step, stirring the suspension within a temperature range of 46°C or more.

2. 2. The method according to claim 1, wherein in the first step, the suspension is stirred for a time period of 10 to 120 minutes within a temperature range of 15° C. to 43° C., and in the second step, the suspension is stirred for a time period of 120 to 360 minutes within a temperature range of 46° C. to 80° C.

3. separating the dispersed particles from the dispersion medium contained in the suspension; washing the dispersed particles separated from the dispersion medium; drying the washed dispersed particles to obtain a dry granular carrier; The method of claim 1 further comprising:

4. 4. The method according to claim 3, wherein the proportion of the total mass of particles having a particle size in the range of 1.4 mm or more and less than 3.35 mm to the total mass of all particles in the dry state is 75% or more.

5. A carboxyalkyl cellulose and / or a salt thereof having a viscosity of 5 mPa·s to 300 mPa·s in a 1% by mass aqueous solution at 25° C. is used to prepare the carboxyalkyl cellulose salt aqueous solution, and the low-polarity organic solvent has a relative dielectric constant of 10 or less at 25° C. and a kinetic viscosity of 10 mm at 37.8° C. 2 The method according to claim 1, wherein an organic solvent having a viscosity of 1 / g or more is used.

6. The method according to claim 1, wherein the low polarity organic solvent is liquid paraffin or silicone oil.

7. The method according to claim 1, wherein the ratio X / Y of the mass X of the carboxyalkyl cellulose and / or its salt to the mass Y of the crosslinking agent in the mixture is within a range of 10 / 2 to 10 / 5.

8. The method according to claim 1, wherein the crosslinking agent is a compound having two or more epoxy groups in the molecule.

9. A dry granular carrier produced by the method according to claim 1.

10. A granular carrier in a dry state containing a crosslinked salt of carboxyalkyl cellulose, wherein the proportion of the total mass of particles having a particle size in the range of more than 1.4 mm and not more than 3.35 mm to the total mass of all particles is 75% or more, and the granular carrier produces gel particles having a smooth surface when absorbed by water.

11. 11. The granular carrier according to claim 10, wherein the proportion of the total mass of particles having a particle size in the range of more than 1.4 mm and not more than 3.35 mm is 99% or less of the total mass of all particles.

12. 11. The granular carrier according to claim 10, wherein the proportion of the total mass of particles having a particle size in the range of more than 2.0 mm and not more than 3.35 mm to the total mass of all particles is in the range of 56% to 86%.

13. A granular carrier as described in claim 10, wherein the proportion of the total mass of particles having a particle size of 1.4 mm or less in the total mass of all particles is 10% or less, and the proportion of the total mass of particles having a particle size larger than 3.35 mm in the total mass of all particles is 15% or less.

14. The granular carrier according to any one of claims 9 to 13, which is used for carrying a drug.

15. A granular drug composition comprising a granular carrier described in any one of claims 9 to 13 and a liquid composition supported on the granular carrier and containing at least one drug selected from drugs having aromatic, deodorizing, odor eliminating, insect repellent, insecticidal or antifungal properties.

16. 16. The granular pharmaceutical composition according to claim 15, which is an air freshener composition or a deodorant composition.

17. An absorbent article comprising a granular carrier according to any one of claims 9 to 13.

Citation Information

Patent Citations

  • Production of water-base gel base material and water-base gel base material produced thereby

    JP1998251447A

  • Process for producing crosslinked gel and its crosslinked gel

    JP2008285611A

  • Composite polymer presenting gel form by water absorption

    JP2014227519A

  • Absorbent and manufacturing method thereof

    JP2023176772A

  • High water-absorbing polymer

    JP2011140534A