Workpiece processing tape and rear face polishing method of workpiece
A single-layer adhesive tape with a hard surface coating addresses the issues of cost and peeling difficulties in conventional tapes by maintaining adequate adhesive strength and strain properties for complete peeling during workpiece processing.
Patent Information
- Application Number
- JP2023053767
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional workpiece processing tapes with multiple layers face issues such as increased cost, potential delamination leading to adhesive transfer to the workpiece, and difficulty in complete peeling within spatial constraints during processing, especially when using energy ray-curable adhesives.
A workpiece processing tape consisting of a single-layer adhesive layer with a hard surface coating layer, designed to have specific adhesive strength and strain properties, allowing complete peeling within spatial constraints without a base material or intermediate layer.
The tape effectively holds and protects workpieces during processing, ensuring complete peeling without adhesive transfer, reducing costs and operational complexity.
Smart Images

Figure 2024141897000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a workpiece processing tape, particularly to a workpiece processing tape used to temporarily protect the surface of a workpiece and to hold the workpiece when processing such as back grinding is performed on various workpieces such as semiconductor wafers, and also to a method of back grinding the workpiece using the workpiece processing tape. [Background technology]
[0002] Chips on which circuits such as semiconductor chips are formed are obtained as workpieces by dividing a workpiece such as a wafer on which a plurality of circuits are formed. With the rapid progress of miniaturization and multi-functionalization of electronic devices on which such chips are mounted, there is a demand for chips to be smaller, thinner, and more dense. In order to reduce the size and height of a chip, it is common to form a circuit on the front surface of a workpiece, and then grind the back surface of the workpiece to reduce the thickness of the chip.
[0003] When grinding the back surface of a workpiece, a workpiece processing tape called a backgrind tape is applied to the surface of the workpiece in order to temporarily protect the circuits on the surface of the workpiece and to hold the workpiece.
[0004] Such workpiece processing tapes are adhesive tapes consisting of a base film and an adhesive layer. When the workpiece has bumps such as protruding electrodes on its surface, a soft intermediate layer may be interposed between the base film and the adhesive layer to absorb the height difference of the bumps and keep the workpiece flat.
[0005] In order to hold the workpiece during processing and to facilitate removal of the workpiece after processing, an energy ray curable adhesive may be used in the adhesive layer of the tape for processing the workpiece. The energy ray curable adhesive holds the workpiece with sufficient adhesive strength before energy ray irradiation, and is polymerized and cured when irradiated with energy ray, reducing the adhesive strength and making it easy to remove the workpiece from the adhesive layer. An energy ray curable composition may also be used as the intermediate layer.
[0006] However, the adhesive strength of the adhesive layer and intermediate layer is reduced by irradiation with energy rays, which reduces the adhesion between the base film and the adhesive layer, between the intermediate layer and the adhesive layer, and between the base film and the intermediate layer, and sometimes the adhesive or intermediate layer is transferred to the workpiece when the workpiece is removed.
[0007] In order to solve such problems, Patent Document 1 (JP Patent Publication 2013-23665 A) discloses a "substrate film, an anchor coat layer containing a compound having an energy ray-polymerizable group, and an energy ray-curable adhesive layer laminated in this order." Both the anchor coat layer and the adhesive layer are in an uncured state (not irradiated with energy rays), and after a predetermined processing is completed, energy rays are irradiated and the workpiece is removed from the adhesive sheet. When the energy ray-curable adhesive is cured, at least a part of the energy ray-polymerizable group contained in the anchor coat layer is also polymerized, and a covalent bond is formed between a part of the adhesive layer and the anchor coat layer, and the adhesive layer and the substrate are adhered to each other via the anchor coat layer. As a result, even after the energy ray-curable adhesive is cured, the adhesion between the substrate film and the adhesive layer is maintained, and the adhesive layer can be prevented from transferring to the workpiece.
[0008] However, the adhesive sheet of Patent Document 1 requires an anchor coat layer, which increases the number of work steps and the cost of raw materials, resulting in an increase in product price. In addition, because it has a multi-layer structure, the possibility of the adhesive layer transferring to the workpiece due to delamination cannot be completely eliminated. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2013-23665 A Summary of the Invention [Problem to be solved by the invention]
[0010] Therefore, the present inventors have studied the holding and protection of workpieces using a tape for workpiece processing that does not include a substrate or an intermediate layer, and is essentially a single layer of adhesive. However, with a single layer of adhesive, the adhesive layer adheres to the worktable during processing of the workpiece, making it difficult to peel off. For this reason, the inventors came up with the idea of providing a relatively hard surface coat layer on the surface of the adhesive layer on the side of the worktable. With a tape for workpiece processing that is made up of a surface coat layer and an adhesive layer, the number of layers constituting the tape is small, and interlayer peeling is unlikely to occur, so the possibility of the adhesive layer transferring to the workpiece can be reduced, and costs can also be reduced.
[0011] However, because the tape is made of a soft adhesive layer and a very thin surface coat layer, when the tape is peeled off from the surface of the workpiece, various defects occur that do not occur with conventional workpiece processing tapes having a base film. For example, peeling defects are likely to occur due to spatial restrictions in the peeling device. The tape is peeled off in the peeling device. In the peeling process, as shown in FIG. 4, for example, the workpiece processing side (grinding surface) of the workpiece 12 is fixed to another tape 16 such as a dicing tape or a dicing / die bond tape, and a peeling tape 14, which is the starting point of peeling, is pressed onto the workpiece processing tape 10 attached to the workpiece 12, and the peeling tape 14 is pulled up in the folding direction to peel off the workpiece processing tape 10. The peeling device 18 is sealed to prevent the intrusion of dust and the like, so there is a spatial restriction. That is, inside the peeling device 18, the movable distance of the peeling tape 14 is limited. For this reason, if the workpiece processing tape 10 cannot be completely peeled off within the spatial constraints (i.e., before the limit of the movable distance of the peeling tape 14 is reached), it becomes difficult to remove the workpiece processing tape 10 within the device, and work may come to a halt.
[0012] By designing the adhesive layer to be hard, it is possible to create a tape for processing workpieces with low adhesion, but this results in insufficient holding and protection of the workpiece.
[0013] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a tape for work processing that can be peeled off completely within spatial constraints while adequately holding and protecting the workpiece, even without including a base material or intermediate layer. [Means for solving the problem]
[0014] The aspects of the present invention are as follows. (1) A tape for processing a workpiece, which essentially consists of two layers, a surface coating layer and an adhesive layer, The adhesive strength at 23°C to a silicon wafer with a mirror-finished surface is 0.3N / 25mm or more and 3N / 25mm or less. When a tensile test of the tape for workpiece processing is conducted at 23°C, the product of the strain (%) when the tensile stress first reaches 20 MPa and the adhesive strength at 23°C to a silicon wafer with a mirror-finished surface (strain × adhesive strength) is 500 N·% or less. (2) The tape for workpiece processing according to (1), wherein when a tensile test of the tape for workpiece processing is carried out at 23°C, the strain (%) at the time when the tensile stress first reaches 20 MPa is 300% or less. (3) The tape for work processing according to (1), wherein the thickness of the adhesive layer is 90 μm or more. (4) The tape for work processing according to (1), wherein the surface coating layer has a thickness of 0.2 to 5 μm. (5) The tape for work processing according to (1), wherein the pressure-sensitive adhesive layer is a cured product of a composition for pressure-sensitive adhesive layer containing an energy ray-curable compound. (6) A method for grinding the back surface of a workpiece, comprising the steps of: applying the workpiece processing tape described in (1) above to the front surface of the workpiece; grinding the workpiece with the workpiece processing tape applied to its front surface from its back surface; and peeling the workpiece processing tape off the workpiece after the back surface has been ground. Effect of the Invention
[0015] According to the present invention, it is possible to provide a tape for work processing that does not include a base material or intermediate layer, but which can adequately hold and protect a workpiece and can be completely peeled off within spatial constraints. [Brief description of the drawings]
[0016] [Figure 1] 1 is a schematic cross-sectional view of a tape for workpiece processing according to an embodiment of the present invention. [Diagram 2] 3A to 3C are schematic cross-sectional views showing an example of a manufacturing process for the workpiece processing tape according to the present embodiment. [Diagram 3] 5A to 5C are schematic cross-sectional views showing another example of the manufacturing process of the tape for workpiece processing according to the present embodiment. [Figure 4] FIG. 2 is a schematic diagram showing a manner in which a tape for work processing is peeled off from a work (wafer). [Diagram 5] 1 is a schematic cross-sectional view showing a state in which a workpiece processing tape is attached to a circuit surface of a wafer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings based on specific embodiments. First, the main terms used in this specification will be explained.
[0018] The workpiece refers to a plate-shaped body to which the workpiece processing tape according to this embodiment is attached and which is then subjected to processing such as back grinding in that state. Examples of the workpiece include circular wafers (including those having an orientation flat), rectangular panel level packages, and strips (rectangular substrates) sealed with molded resin. Examples of the wafers include semiconductor wafers such as silicon wafers, gallium arsenide wafers, silicon carbide wafers, gallium nitride wafers, and indium phosphide wafers, and insulating wafers such as glass wafers, lithium tantalate wafers, and lithium niobate wafers, and may also be reconstructed wafers made of resin and semiconductors used to manufacture fan-out packages, etc.
[0019] The "front surface" of a workpiece refers to the surface on which circuits, electrodes, etc. are formed, and the "back surface" of a workpiece refers to the surface on which no circuits, etc. are formed. The electrodes may be convex electrodes such as bumps.
[0020] The processing of the workpiece refers to processes such as grinding the back side of the workpiece, dividing the workpiece into individual pieces, marking the back side of the workpiece with a laser marker or the like, and forming circuits or protruding electrodes on the front side of the workpiece. From the viewpoint of easily achieving the effects of the present invention, however, it is more preferable that the processing of the workpiece is a process of grinding the back side of the workpiece.
[0021] The surface coating layer is a thin resin layer that covers one side of the adhesive layer and prevents the workpiece processing tape from sticking to components of semiconductor manufacturing equipment (for example, a suction table).
[0022] "(Meth)acrylate" is used as the term to refer to both "acrylate" and "methacrylate," and similar terms.
[0023] The term "energy rays" refers to ultraviolet rays, electron beams, etc., and is preferably ultraviolet rays.
[0024] Unless otherwise specified, the "weight average molecular weight" is a polystyrene equivalent value measured by gel permeation chromatography (GPC). Measurements by such a method are performed, for example, using a high-speed GPC device "HLC-8120GPC" manufactured by Tosoh Corporation with a high-speed column "TSK guard column H XL -H", "TSK Gel GMH XL ", "TSK Gel G2000 H XL (All of the above are manufactured by Tosoh Corporation) connected in the above order, the column temperature was 40° C., the liquid flow rate was 1.0 mL / min, and the detector was a differential refractometer.
[0025] The release film is a film that supports the pressure-sensitive adhesive layer and the surface coating layer in a releasable manner. The term "film" is not limited to a specific thickness, and is used to include a sheet.
[0026] The mass ratios in the explanations of compositions such as the pressure-sensitive adhesive layer composition are based on the active ingredient (solid content), and do not include the solvent unless otherwise specified.
[0027] Next, the configuration of each component of the tape for workpiece processing according to the present invention will be described in more detail. Note that, hereinafter, the tape for workpiece processing according to the present invention may be simply referred to as "tape".
[0028] (Work processing tape 10) As shown in Fig. 1, the workpiece processing tape 10 is substantially composed of two layers, a surface coat layer 2 and an adhesive layer 4. Here, "substantially composed" means that it does not have any other layers that have functionality in terms of holding and protecting the workpiece, but does not preclude the presence of layers that are not involved in holding and protecting the workpiece. For example, the adhesive layer 4 may be laminated with a release film to prevent dust and the like from adhering to the adhesive layer before the workpiece processing tape 10 is used.
[0029] The surface coating layer 2 may be a laminated structure of two or more layers having similar composition and characteristics, and the adhesive layer 4 may also be a laminated structure of two or more layers having similar composition and characteristics, but from the standpoint of manufacturing efficiency, it is preferable that both are single layers.
[0030] The adhesive layer of the workpiece processing tape 10 is applied to a silicon wafer, and the adhesive strength measured at 23°C when it is peeled off is 0.3 N / 25 mm or more and 3 N / 25 mm or less. The adhesive strength is preferably 0.5 N / 25 mm or more, more preferably 0.7 N / 25 mm or more, and particularly preferably 0.9 N / 25 mm or more, and is preferably 2.6 N / 25 mm or less, more preferably 2.2 N / 25 mm or less, and particularly preferably 1.8 N / 25 mm or less.
[0031] The adhesive strength is measured according to JIS Z 0237. Specifically, a strip-shaped measurement sample cut from the workpiece processing tape 10 to a width of 25 mm is attached to a silicon wafer with a 2 kg roller in an environment of 23°C and 50% relative humidity, and after 20 minutes, the adhesive strength is determined as the peeling force when the tape is peeled in a 180° direction at a speed of 300 mm / min using a universal (peel load) tester. A mirror-finished wafer smoothed to a surface roughness Ra of 5 nm±2 nm by buff polishing or the like is used as the silicon wafer, and the workpiece processing tape is attached to the mirror-finished surface to measure the adhesive strength.
[0032] When the adhesive strength of the workpiece processing tape 10 at 23°C is within the above range, the workpiece such as a semiconductor wafer can be stably held and its surface can be reliably protected when the workpiece is subjected to processing such as back grinding.
[0033] When a tensile test of the workpiece processing tape 10 is performed at 23°C, the product of the strain (%) when the tensile stress first reaches 20 MPa and the adhesive strength at 23°C to a silicon wafer with a mirror-finished surface (strain x adhesive strength) is 500 N·% or less. When the workpiece processing tape 10 is stretched, the tensile stress gradually increases. If the strain (%) is large when this tensile stress reaches 20 MPa, it means that the tape material is easily stretched even with a small force.
[0034] The fact that "strain x adhesive strength" is below a predetermined value means that the tape material is difficult to stretch with a small force and has a small adhesive strength. When "strain x adhesive strength" is below a predetermined value, peeling is completed before the tape can no longer be stretched due to spatial constraints in the peeling device. For this reason, the "strain x adhesive strength" is preferably 400N·% or less, more preferably 300N·% or less, and particularly preferably 250N·% or less. In addition, if the "strain x adhesive strength" is too small, the adhesive strength may be insufficient, so the "strain x adhesive strength" is preferably 3N·% or more, more preferably 7N·% or more, and particularly preferably 10N·% or more.
[0035] Moreover, the strain (%) is preferably 300% or less, more preferably 250% or less, and particularly preferably 200% or less. When the strain (%) is 300(%) or less, it becomes easier to control the "strain x adhesive strength" within the above-mentioned range, and the adhesive strength can be designed to be relatively large, so that the workpiece can be held and protected more reliably. However, when the strain (%) is too small, the adhesive layer becomes excessively hard, and the workability may be poor when applying the workpiece processing tape. Therefore, the strain (%) is preferably 5% or more, more preferably 10% or more, and particularly preferably 15% or more.
[0036] The strain is measured according to JIS K 7161. Specifically, a strip-shaped measurement sample cut from the workpiece processing tape 10 to a width of 15 mm and a length of 150 mm is attached to a precision universal testing machine and stretched at a stretching speed of 200 mm / min, and the strain (%) is calculated from the amount of elongation at the time when the tensile stress reaches 20 MPa. The measurement is performed in an environment with a chuck distance (i.e., initial sample length) of 100 mm, 23°C, and a relative humidity of 50%. The strain (%) is calculated by calculating the amount of elongation Δ, which is the difference between the sample length (chuck distance) at the time when the tensile stress reaches 20 MPa and the initial sample length (100 mm), and the ratio of the amount of elongation Δ to the initial sample length (100 mm) [=(Δ / 100) × 100] is defined as the strain (%).
[0037] The thickness of the adhesive layer is not particularly limited, but from the viewpoint of ensuring the retention of the workpiece, it is preferably 60 μm or more, more preferably 90 μm or more, and particularly preferably 110 μm or more. In addition, since a thick adhesive layer may deteriorate the handling properties, the thickness of the adhesive layer is preferably 200 μm or less, more preferably 160 μm or less, and particularly preferably 140 μm or less.
[0038] The thickness of the surface coating layer is not particularly limited, but from the viewpoint of preventing adhesion to the work table, it is preferably 0.2 to 5 μm, more preferably 0.5 to 5 μm, and particularly preferably 1 to 4 μm. By setting the thickness of the surface coating layer within the above range, high performance tends to be maintained.
[0039] The storage modulus of the surface coat layer is not particularly limited, but from the viewpoint of preventing the workpiece processing tape from sticking to a member (e.g., a suction table) of a semiconductor manufacturing device, the storage modulus (E') measured in a tensile mode is preferably 40 MPa or more, more preferably 60 MPa or more, and even more preferably 80 MPa or more at 23° C. The method for measuring the storage modulus (E') of the surface coat layer in the present invention will be described in detail in the Examples below.
[0040] The thickness of the tape 10 for workpiece processing is not particularly limited, but from the viewpoint of ensuring the holding of the workpiece, it is preferably 61 μm or more, more preferably 91 μm or more, and particularly preferably 111 μm or more. From the viewpoint of handling, the thickness of the tape 10 for workpiece processing is preferably 205 μm or less, more preferably 165 μm or less, and particularly preferably 145 μm or less.
[0041] The workpiece processing tape 10 is not particularly limited in terms of composition or thickness of the surface coating layer or adhesive layer as long as the above-mentioned adhesive strength and "strain x adhesive strength" are satisfied; however, non-limiting examples of the composition of the workpiece processing tape 10 of the present invention are described below.
[0042] (Adhesive layer 4) The adhesive layer is formed from a composition containing various removable pressure-sensitive adhesives, but it is preferable that the adhesive layer be composed of a cured product of a composition for adhesive layers that contains an energy ray-curable compound, which allows relatively easy control of the adhesive strength and "strain x adhesive strength" within the desired range.
[0043] (Composition for pressure-sensitive adhesive layer) The composition for pressure-sensitive adhesive layer containing the energy ray-curable compound is cured by irradiation with energy rays. The curing reduces the fluidity, but maintains the adhesiveness and reduces the stretchability.
[0044] More specifically, from the viewpoint of controlling the adhesive strength and "strain × adhesive strength" within the desired range, the composition for adhesive layer containing an energy ray curable compound preferably contains a urethane (meth)acrylate (d1), more preferably further contains an energy ray curable compound (d3) having an alicyclic group or heterocyclic group with 6 to 20 ring-forming atoms, and may further contain a polyfunctional energy ray curable compound (d2) and / or an energy ray curable compound (d4) having a functional group. Furthermore, the composition for adhesive layer may contain, in addition to the above components, an energy ray curable compound (d5) other than the components (d1) to (d4) and a photopolymerization initiator (i). Furthermore, the adhesive The layer composition may contain other additives as long as the effects of the present invention are not impaired.
[0045] Hereinafter, each component contained in the composition for pressure-sensitive adhesive layer containing the energy ray-curable compound will be described in detail.
[0046] (Urethane (meth)acrylate (d1)) The urethane (meth)acrylate (d1) is a compound having at least a (meth)acryloyl group and a urethane bond, and has the property of being polymerized and cured by irradiation with energy rays. The urethane (meth)acrylate (d1) is an oligomer or polymer.
[0047] The weight average molecular weight (Mw) of component (d1) is preferably 1,000 to 100,000, more preferably 2,000 to 60,000, and even more preferably 3,000 to 20,000. The number of (meth)acryloyl groups in component (d1) (hereinafter also referred to as "functionality") may be monofunctional, bifunctional, or trifunctional or higher, but is preferably monofunctional or bifunctional.
[0048] Component (d1) can be obtained, for example, by reacting a polyol compound with a polyisocyanate compound to obtain a terminal isocyanate urethane prepolymer, and then reacting a (meth)acrylate having a hydroxyl group. Component (d1) may be used alone or in combination of two or more kinds.
[0049] The polyol compound used as the raw material of component (d1) is not particularly limited as long as it is a compound having two or more hydroxyl groups. It may be any of a difunctional diol, a trifunctional triol, and a polyol having four or more functional groups, but a difunctional diol is preferred, and a polyolefin type diol is more preferred.
[0050] Examples of the polyisocyanate compound include aliphatic polyisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, and trimethylhexamethylene diisocyanate; alicyclic diisocyanates such as isophorone diisocyanate, norbornane diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, dicyclohexylmethane-2,4'-diisocyanate, and ω,ω'-diisocyanate dimethylcyclohexane; and aromatic diisocyanates such as 4,4'-diphenylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, tolidine diisocyanate, tetramethylene xylylene diisocyanate, and naphthalene-1,5-diisocyanate.
[0051] Among these, isophorone diisocyanate, hexamethylene diisocyanate, and xylylene diisocyanate are preferred.
[0052] The above-mentioned polyol compound is reacted with a polyisocyanate compound to give a terminal isocyanate urethane prepolymer, and then a hydroxyl group-containing (meth)acrylate is reacted with the urethane (meth)acrylate (d1). The hydroxyl group-containing (meth)acrylate is not particularly limited as long as it is a compound having a hydroxyl group and a (meth)acryloyl group in at least one molecule.
[0053] Specific examples of (meth)acrylates having a hydroxy group include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 4-hydroxycyclohexyl (meth)acrylate, 5-hydroxycyclooctyl (meth)acrylate, 2-hydroxy-3-phenyloxypropyl (meth)acrylate, pentaerythritol tri(meth)acrylate, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate; hydroxy group-containing (meth)acrylamides such as N-methylol (meth)acrylamide; and reaction products obtained by reacting a diglycidyl ester of vinyl alcohol, vinylphenol, or bisphenol A with (meth)acrylic acid; and the like.
[0054] Among these, hydroxyalkyl (meth)acrylate is preferred, and 2-hydroxyethyl (meth)acrylate is more preferred.
[0055] The conditions for reacting the isocyanate-terminated urethane prepolymer and the (meth)acrylate having a hydroxyl group are preferably such that the reaction is carried out at 60 to 100° C. for 1 to 4 hours in the presence of a solvent and a catalyst, which are added as necessary.
[0056] The content of component (d1) in the composition for adhesive layer is preferably 20 to 80 mass%, more preferably 30 to 70 mass%, and even more preferably 40 to 65 mass%, relative to the total amount (100 mass%) of the composition for adhesive layer.
[0057] (Multifunctional energy ray curable compound (d2)) The polyfunctional energy ray curable compound refers to a compound other than component (d1) having two or more energy ray curable unsaturated groups. The energy ray curable unsaturated group is a functional group containing a carbon-carbon double bond, such as a (meth)acryloyl group, a vinyl group, an allyl group, a vinylbenzyl group, etc. Two or more types of energy ray curable unsaturated groups may be combined. A three-dimensional network structure (crosslinked structure) is formed by reacting an energy ray curable unsaturated group in the polyfunctional energy ray curable compound with a (meth)acryloyl group in component (d1) or by reacting energy ray curable unsaturated groups in component (d2) with each other. When a polyfunctional energy ray curable compound is used, the crosslinked structure formed by energy ray irradiation increases compared to when a compound containing only one energy ray curable unsaturated group is used, so that the pressure-sensitive adhesive layer exhibits unique viscoelasticity, and it becomes easier to relieve stress during back grinding.
[0058] In addition, although there is some overlap between the definition of component (d2) and the definition of component (d3) or component (d4) described later, the overlapping parts are included in component (d2). For example, a compound having an alicyclic group or heterocyclic group with 6 to 20 ring atoms and having two or more energy ray-curable unsaturated groups is included in the definitions of both component (d2) and component (d3), but in the present invention, the compound is included in component (d2). In addition, a compound containing a functional group such as a hydroxyl group, an epoxy group, an amide group, or an amino group and having two or more energy ray-curable unsaturated groups is included in the definitions of both component (d2) and component (d4), but in the present invention, the compound is included in component (d2).
[0059] From the above viewpoints, the number of energy ray-curable unsaturated groups (number of functional groups) in the polyfunctional energy ray-curable compound is preferably 2 to 10, and more preferably 3 to 6.
[0060] The weight average molecular weight of the component (d2) is preferably 30-40,000, more preferably 100-10,000, and even more preferably 200-1,000.
[0061] Specific examples of the component (d2) include diethylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, divinylbenzene, vinyl (meth)acrylate, divinyl adipate, and N,N'-methylenebis(meth)acrylamide.
[0062] The component (d2) may be used alone or in combination of two or more kinds. Among these, dipentaerythritol hexa(meth)acrylate is preferred.
[0063] The content of component (d2) in the composition for adhesive layer is preferably 0 to 40 mass%, more preferably 0.5 to 20 mass%, and even more preferably 1 to 15 mass%, relative to the total amount (100 mass%) of the composition for adhesive layer.
[0064] (Energy Ray-Curable Compound (d3) Having an Alicyclic or Heterocyclic Group with 6 to 20 Ring Atoms) Component (d3) is an energy ray curable compound other than component (d1) having an alicyclic group or heterocyclic group with 6 to 20 ring atoms, and is preferably a compound having at least one (meth)acryloyl group, more preferably a compound having one (meth)acryloyl group. By using component (d3), the film formability of the obtained pressure-sensitive adhesive layer composition can be improved.
[0065] The definition of component (d3) overlaps with the definition of component (d4) described below, but the overlapping portion is included in component (d4). For example, a compound having at least one (meth)acryloyl group, an alicyclic group or heterocyclic group having 6 to 20 ring atoms, and a functional group such as a hydroxyl group, an epoxy group, an amide group, or an amino group is included in the definitions of both component (d3) and component (d4), but in the present invention, the compound is included in component (d4).
[0066] Specific examples of the component (d3) include alicyclic group-containing (meth)acrylates such as isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, cyclohexyl (meth)acrylate, and adamantane (meth)acrylate; and heterocyclic group-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate and morpholine (meth)acrylate. The component (d3) may be used alone or in combination of two or more kinds.
[0067] Of the alicyclic group-containing (meth)acrylates, isobornyl (meth)acrylate is preferred, and of the heterocyclic group-containing (meth)acrylates, tetrahydrofurfuryl (meth)acrylate is preferred.
[0068] The content of component (d3) in the composition for adhesive layer is preferably 10 to 60 mass%, more preferably 20 to 55 mass%, and even more preferably 25 to 50 mass%, relative to the total amount (100 mass%) of the composition for adhesive layer.
[0069] (Energy ray-curable compound having a functional group (d4)) Component (d4) is an energy ray-curable compound other than component (d1) that contains a functional group such as a hydroxyl group, an epoxy group, an amide group, or an amino group, and is preferably a compound having at least one (meth)acryloyl group, more preferably a compound having one (meth)acryloyl group.
[0070] Component (d4) has good compatibility with component (d1), and the viscosity of the adhesive layer composition can be easily adjusted to a suitable range. In addition, the adhesive layer can have good cushioning performance even if it is relatively thin. In addition, the adhesive strength of the work processing tape can be easily adjusted to the above range by adjusting the polarity of the adhesive layer with the introduction of functional groups.
[0071] Examples of the component (d4) include hydroxyl group-containing (meth)acrylates, epoxy group-containing compounds, amide group-containing compounds, amino group-containing (meth)acrylates, etc. Among these, hydroxyl group-containing (meth)acrylates are preferred.
[0072] Examples of hydroxyl group-containing (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, phenylhydroxypropyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl acrylate.
[0073] The component (d4) may be used alone or in combination of two or more kinds. The content of component (d4) in the composition for adhesive layer is preferably 0 to 30 mass%, more preferably 1 to 20 mass%, and even more preferably 2 to 10 mass%, relative to the total amount (100 mass%) of the composition for adhesive layer, in order to improve the film-forming properties of the composition for adhesive layer and to adjust the polarity of the adhesive layer.
[0074] (Energy ray-curable compound (d5) other than components (d1) to (d4)) The pressure-sensitive adhesive layer-forming composition may contain a monofunctional energy ray-curable compound (d5) other than the above components (d1) to (d4) within the range that does not impair the effects of the present invention.
[0075] Examples of the component (d5) include alkyl (meth)acrylates having an alkyl group having 1 to 20 carbon atoms, and vinyl compounds such as styrene, hydroxyethyl vinyl ether, hydroxybutyl vinyl ether, N-vinyl formamide, N-vinyl pyrrolidone, and N-vinyl caprolactam. The component (d5) may be used alone or in combination of two or more kinds.
[0076] The content of component (d5) in the composition for forming an adhesive layer is preferably 0 to 20 mass%, more preferably 0 to 10 mass%, even more preferably 0 to 5 mass%, and particularly preferably 0 to 2 mass%, relative to the total amount (100 mass%) of the composition for forming an adhesive layer.
[0077] (Photopolymerization initiator (i)) It is preferable that the pressure-sensitive adhesive layer composition further contains a photopolymerization initiator (i) from the viewpoint of shortening the polymerization time by energy ray irradiation and reducing the amount of energy ray irradiation when forming the pressure-sensitive adhesive layer.
[0078] Examples of the photopolymerization initiator include benzoin compounds, acetophenone compounds, acylphosphinoxide compounds, titanocene compounds, thioxanthone compounds, peroxide compounds, and further photosensitizers such as amines and quinones. More specific examples include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzyl phenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyrolnitrile, dibenzyl, diacetyl, 8-chloroanthraquinone, and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.
[0079] These photopolymerization initiators can be used alone or in combination of two or more kinds.
[0080] The content of the photopolymerization initiator in the composition for adhesive layer is preferably 0.05 to 15 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.3 to 5 parts by mass of the energy ray curable compound relative to the total amount (100 parts by mass) of the composition for adhesive layer.
[0081] (Other additives) The adhesive layer composition may contain other additives within the range that does not impair the effects of the present invention. Examples of other additives include antistatic agents, antioxidants, softeners (plasticizers), fillers, rust inhibitors, pigments, dyes, etc. When these additives are blended, the content of each additive in the adhesive layer composition is preferably 0.01 to 6 parts by mass, more preferably 0.1 to 3 parts by mass, based on the total amount (100 parts by mass) of the adhesive layer composition.
[0082] The pressure-sensitive adhesive layer formed from the composition for pressure-sensitive adhesive layer containing the energy ray-curable compound is preferably obtained by polymerizing and curing the composition for pressure-sensitive adhesive layer having the above-mentioned composition by energy ray irradiation. In other words, the pressure-sensitive adhesive layer is preferably a product obtained by curing the composition for pressure-sensitive adhesive layer.
[0083] Therefore, the pressure-sensitive adhesive layer preferably contains a repeating unit derived from component (d1), and more preferably further contains a repeating unit derived from component (d3). The pressure-sensitive adhesive layer may also contain a repeating unit derived from component (d2) and / or a repeating unit derived from component (d4), or may contain a repeating unit derived from component (d5). The content ratio of each repeating unit in the pressure-sensitive adhesive layer usually corresponds to the ratio (feed ratio) of each component constituting the pressure-sensitive adhesive layer composition.
[0084] (Surface Coating Layer 2) The surface coating layer may be formed from a variety of hard thin films, but is preferably a cured product of a composition containing a curable resin (A) and an inorganic filler, since it is easy to produce and a hard surface coating layer can be obtained.
[0085] (Surface Coating Layer Composition) The surface coating layer composition contains preferably 10 to 50 parts by mass, more preferably 15 to 40 parts by mass, and particularly preferably 20 to 30 parts by mass of the inorganic filler relative to 100 parts by mass of the cured product of the surface coating layer composition. It is normal that there is substantially no difference between the amount of inorganic filler blended in the surface coating layer composition before curing and the amount of inorganic filler blended in the cured product of the surface coating layer composition. Therefore, in the present invention, the amount of inorganic filler blended in the surface coating layer composition before curing is regarded as the amount of inorganic filler blended in the cured product of the surface coating layer composition. By setting the content of the inorganic filler in the surface coating layer to the above range, it is possible to exhibit excellent performance as a surface coating layer, and also to prevent cracks from occurring in the surface coating layer in the process of processing the workpiece, and as a result, it is possible to more efficiently suppress the deterioration of performance.
[0086] The curable resin (A) is not particularly limited, but may be an energy ray curable resin, a thermosetting resin, or the like, and preferably an energy ray curable resin containing an energy ray curable group.
[0087] The energy beam curable resin is not particularly limited, but for example, an oligomer-based energy beam curable resin such as an energy beam curable urethane (meth)acrylate oligomer or an epoxy (meth)acrylate oligomer is preferably used. The weight average molecular weight Mw (referring to a polystyrene equivalent value by gel permeation chromatography) of the urethane (meth)acrylate oligomer or the epoxy (meth)acrylate oligomer is usually about 1000 to 70000, preferably in the range of 1500 to 60000. The above urethane (meth)acrylate oligomer or epoxy (meth)acrylate oligomer can be used alone or in combination of two or more.
[0088] The energy ray curable resin may be a polymer having an energy ray curable functional group in the side chain. If such a polymer is used as the energy ray curable resin, the adhesion to the adhesive layer can be improved without decreasing the crosslinking density. For example, such a polymer may have an acrylic polymer main chain and an energy ray curable double bond or an epoxy group as a functional group in the side chain. The surface coating layer composition contains preferably 50 to 90 parts by mass, more preferably 60 to 85 parts by mass, and particularly preferably 70 to 80 parts by mass of the curable resin (A) per 100 parts by mass of the surface coating layer composition.
[0089] By mixing a photopolymerization initiator with the energy ray curable resin, the polymerization curing time and the irradiation amount by the energy ray irradiation can be reduced. Examples of the photopolymerization initiator include photopolymerization initiators such as benzoin compounds, acetophenone compounds, acylphosphinoxide compounds, titanocene compounds, thioxanthone compounds, and peroxide compounds, and photosensitizers such as amines and quinones. Specific examples include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzoin, benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether.
[0090] The surface coating layer composition may contain a binder component other than the curable resin (A) in order to impart flexibility (performance to prevent cracks from occurring) to the surface coating layer. Examples of such binder components include acrylic resins, polyester resins, urethane resins, polyamide resins, etc.
[0091] The composition for the surface coating layer may contain a dispersant to improve the dispersibility of the inorganic filler, and may contain additives such as colorants, e.g., pigments and dyes.
[0092] (Method of manufacturing tape for work processing) Next, the methods for producing the workpiece processing tape will be described. According to the first method, the adhesive strength of the adhesive layer surface can be set relatively high, while according to the second method, it becomes relatively low.
[0093] In the first method, as shown in FIG. 2(a), a coating layer 1 is provided on a first release film 21 to prepare a first release film with a coating layer.
[0094] The release film used is a release film having at least one surface that has been subjected to a release treatment, and specifically, examples thereof include a release film having a release agent applied onto the surface of a release film substrate.
[0095] The substrate for the release film is preferably a resin film, and examples of the resin constituting the resin film include polyester resin films such as polyethylene terephthalate resin, polybutylene terephthalate resin, and polyethylene naphthalate resin, polyolefin resins such as polypropylene resin and polyethylene resin, etc. Examples of the release agent include silicone-based release agents, alkyd-based release agents, and fluorine-based release agents.
[0096] The thickness of the release film is not particularly limited, but is preferably 10 to 200 μm, and more preferably 20 to 150 μm.
[0097] The method of forming the coating layer 1 on the first release film 21 is not particularly limited, and the above-mentioned surface coating layer composition or the coating agent described below may be applied by a known method such as spin coating, spray coating, bar coating, knife coating, roll coating, blade coating, die coating, or gravure coating. The coating thickness of the coating layer 1 may be such that the thickness after the final formation is the thickness of the above-mentioned surface coating 2, and may be dried as necessary. The surface coating layer composition may be diluted with an organic solvent as necessary and applied as a coating agent. Examples of the organic solvent include methyl ethyl ketone, acetone, ethyl acetate, tetrahydrofuran, dioxane, cyclohexane, n-hexane, toluene, xylene, n-propanol, and isopropanol. The surface coating layer composition or the coating agent may be applied once, or may be applied in two or more separate steps. When the surface coating layer composition is applied two or more times, the same surface coating layer composition may be used, or a surface coating layer composition having a similar composition may be used.
[0098] Next, as shown in FIG. 2(b), the adhesive layer composition or the coating agent described below is applied onto the coating layer 1 of the release film with the coating layer to form an uncured adhesive layer 3. The coating method is the same as described above. The coating thickness is such that the thickness after final formation is the thickness of the adhesive layer 4, and the coating may be dried as necessary. The adhesive layer composition may be diluted with an organic solvent as described above to form a coating agent, but it is preferable to use a solvent-free coating agent to reduce environmental load. Coating may be performed in two or more separate steps. When coating the adhesive layer composition two or more times, the same adhesive layer composition may be used, or compositions with similar compositions may be used.
[0099] Next, as shown in FIG. 2(c), energy rays EB are irradiated to semi-cure the energy ray curable components contained in the surface coating layer composition and the adhesive layer composition. The energy rays are irradiated, for example, with a high-pressure mercury lamp. By simultaneously curing the uncured coating layer 1 and adhesive layer 3, the energy ray curable components contained in the coating layer 1 and adhesive layer 3 are bonded together, improving the adhesion between the semi-cured coating layer 1 and adhesive layer 3. The amount of energy rays irradiated may be an amount that partially cures the energy ray curable components contained in the coating layer 1 and adhesive layer 3. The energy rays are preferably ultraviolet rays, and the illuminance thereof is 60 to 320 mW / cm. 2 The light intensity is preferably 30 to 1000 mJ / cm. 2 It is preferable that:
[0100] If energy beam irradiation is performed in an air atmosphere, polymerization is inhibited by oxygen, and polymerization on the surface of the adhesive layer 3 that is attached to the workpiece does not proceed completely, resulting in a relatively soft surface, and the adhesive strength of the adhesive layer can be set high.
[0101] 2(d), a second release film 22 is laminated on the semi-cured pressure-sensitive adhesive layer 3. As the second release film, a film similar to the first release film is used, but it is preferable to use a film having high transmittance to energy rays.
[0102] 2(e), energy rays EB are irradiated to cure all of the energy ray curable components contained in the coating layer 1 and the adhesive layer 3, obtaining a surface coating layer 2 from the coating layer 1, and converting the uncured adhesive layer 3 into a cured adhesive layer 4. The energy rays are preferably ultraviolet rays, and the illuminance thereof is 100 to 400 mW / cm. 2 The light intensity is preferably 200 to 1500 mJ / cm 2 Even if energy rays are irradiated in this state, the surface of the pressure-sensitive adhesive layer 4 that has been inhibited from polymerization cannot be sufficiently cured, and the surface remains relatively soft and maintains high adhesive strength.
[0103] After going through the above steps, the first release film is peeled off to obtain a laminate (i.e., a workpiece processing tape with a release film) in which the second release film is laminated on the workpiece processing tape 10 having the configuration shown in FIG. 1.
[0104] In the second manufacturing method, inhibition of polymerization on the surface of the adhesive layer to be attached to the workpiece is avoided, and the surface of the adhesive layer can be made relatively hard and the adhesive strength can be set low.
[0105] In the second method, as shown in Fig. 3(a), the composition for the pressure-sensitive adhesive layer is applied onto a second release film 22 to form an uncured pressure-sensitive adhesive layer 3. The application method and application thickness are the same as those in the first method.
[0106] Next, as shown in Fig. 3(b), energy rays are irradiated to semi-cure the energy ray-curable component contained in the composition for pressure-sensitive adhesive layer. The energy rays are preferably ultraviolet rays, and the illuminance thereof is 60 to 320 mW / cm 2 The light intensity is preferably 30 to 1000 mJ / cm. 2 It is preferable that the surface of the substrate is made of a soft material. When the energy beam irradiation is performed in an air atmosphere, polymerization inhibition occurs due to oxygen. However, as described later, the soft surface formed by the polymerization inhibition has a surface coating layer 2 formed thereon, and is not used as an adhesive surface to be attached to a workpiece.
[0107] Separately from the above, a coating layer 1 is provided on a first release film 21 to prepare a first release film with a coating layer.
[0108] 3(c), the coating layer 1 of the first release film with a coating layer is laminated on the semi-cured pressure-sensitive adhesive layer 3. As the first release film, it is preferable to use a film having high transmittance to energy rays.
[0109] Next, as shown in Fig. 3(d), energy rays are irradiated to cure the energy ray curable components contained in the surface coating layer composition and the pressure-sensitive adhesive layer composition. The unreacted energy ray curable components in the semi-cured pressure-sensitive adhesive layer 3 and the energy ray curable components contained in the uncured coating layer 1 are polymerized and cured, obtaining a surface coating layer 2 from the coating layer 1, and converting the uncured pressure-sensitive adhesive layer 3 into a cured pressure-sensitive adhesive layer 4. Ultraviolet rays are preferable as the energy rays, and the illuminance thereof is 100 to 400 mW / cm. 2 The light intensity is preferably 200 to 1500 mJ / cm 2 It is preferable that the adhesiveness between the cured surface coating layer and the pressure-sensitive adhesive layer 4 is improved by the curing of the energy ray-curable component.
[0110] After going through the above steps, the first release film is peeled off to obtain a laminate (i.e., a workpiece processing tape with a release film) in which the second release film is laminated on the workpiece processing tape 10 having the configuration shown in FIG. 1.
[0111] (Control of adhesive strength and distortion of tape for workpiece processing) As described above, according to the first manufacturing method, the adhesive strength of the tape for workpiece processing can be set relatively high by utilizing polymerization inhibition, whereas according to the second manufacturing method, the adhesive strength can be set relatively low.
[0112] Furthermore, by increasing the amount of crosslinked structures contained in the pressure-sensitive adhesive layer 4 (for example, by increasing the amount of the polyfunctional energy ray-curable compound (d2) in the composition for pressure-sensitive adhesive layer), the adhesive strength decreases and the distortion decreases.
[0113] Furthermore, by increasing the amount of the energy ray-curable compound having a heterocyclic group in the composition for the pressure-sensitive adhesive layer, the adhesive strength tends to be increased.
[0114] In addition, by adding an energy ray-curable compound (d4) having a functional group to the composition for the adhesive layer, the adhesive strength can be adjusted by changing the polarity of the adhesive layer, and in particular, by adding an energy ray-curable compound having a hydroxyl group, the adhesive strength tends to be increased.
[0115] In addition, although the level of adhesive strength is affected by differences in the energy ray irradiation method (for example, differences in the energy ray irradiation method between the first manufacturing method and the second manufacturing method), the adhesive strength can be adjusted by adjusting the weight average molecular weight (Mw) of the urethane (meth)acrylate (d1) in the composition for the adhesive layer.
[0116] Furthermore, in the work processing tape produced by the second production method, there is a tendency that the adhesive strength can be increased by increasing the amount of urethane (meth)acrylate (d1) in the adhesive layer composition.
[0117] Furthermore, by increasing the content of photopolymerization initiator in the composition for adhesive layer or increasing the illuminance or light amount in the energy ray irradiation, the adhesive strength may be lowered and the distortion may be smaller than when there is a small amount of photopolymerization initiator or when the energy ray irradiation conditions are weak.
[0118] (Workpiece processing method) The tape for workpiece processing of the present invention is used for temporarily protecting the surface of a workpiece and for holding the workpiece when processing such as back grinding is performed on various workpieces such as semiconductor wafers. The tape for workpiece processing of the present invention is preferably used for protecting the surface of the workpiece by being attached to the surface of the workpiece when back grinding is performed on the workpiece.
[0119] As a non-limiting example of the use of the tape for processing a workpiece, a method for grinding the backside of a workpiece will be described in more detail below, in which the workpiece is a wafer and the processing includes grinding the backside.
[0120] Specifically, the method for grinding the back surface of a workpiece (wafer) includes at least the following steps 1 to 3. Step 1: A process of attaching the above-mentioned work processing tape to the surface of the wafer. Process 2: The wafer with the workpiece processing tape attached to its surface is ground from the back side. Step 3: The process of peeling off the workpiece processing tape from the wafer after back grinding.
[0121] Each step of the above-mentioned method for grinding the back surface of a wafer will now be described in detail.
[0122] (Process 1) In step 1, as shown in Fig. 5, the adhesive layer 4 of the tape 10 for workpiece processing according to this embodiment is applied to a surface 12a of a wafer 12 as a workpiece. By applying the tape for workpiece processing to the surface of the wafer, the surface of the wafer is sufficiently protected.
[0123] The thickness of the wafer before grinding is not particularly limited, but is usually about 500 to 1000 μm. The wafer usually has a circuit formed on its surface. The formation of the circuit on the wafer surface can be performed by various methods including conventionally widely used methods such as etching and lift-off.
[0124] The wafer with the workpiece processing tape attached is placed on a suction table (an example of a working table) and is adsorbed and held on the suction table. At this time, the surface coating layer side of the workpiece processing tape is placed on the table side and adsorbed.
[0125] (Process 2) After step 1, the back surface of the wafer on the suction table is ground to obtain a back-ground wafer. In this embodiment, the thickness of the wafer after back-grinding is not particularly limited, but may be, for example, 200 μm or less, or 100 μm or less. When the thickness of the wafer after back-grinding is within the above range, it is easy to realize a smaller chip and a lower profile.
[0126] (Step 3) Next, the workpiece processing tape 10 is peeled off from the wafer. This step is carried out, for example, as shown in FIG.
[0127] After the backside grinding, another tape 16 such as a dicing tape or a dicing / die bonding tape is applied to the backside of the wafer. At this time, the outer peripheral edge of the other tape 16 is fixed to a ring frame (not shown). Next, the workpiece processing tape 10 is peeled off from the wafer held on the other tape 16. To peel off the workpiece processing tape 10, the peeling tape 14, which is the starting point of peeling, is pressed against the surface coating layer 2 of the workpiece processing tape, and the peeling tape 14 is pulled up in the folding back direction to peel off the workpiece processing tape 10.
[0128] Since the workpiece processing tape of this embodiment has the characteristics described above, it has sufficient adhesive strength to hold and protect the wafer, while its extensibility is appropriately suppressed, so that the workpiece processing tape can be stably peeled off even in a peeling device with spatial limitations.
[0129] The tape for work processing according to the present invention can also be suitably used in a method for producing individual pieces (chips) using a pre-dicing method.
[0130] In addition to steps 1 to 3 above, the chip manufacturing method using the pre-dicing method includes a step (step 4) of forming grooves from the front surface side of the wafer, or forming modified regions inside the wafer from the front or back surface of the wafer.
[0131] When forming a modified region in the wafer, it is preferable to carry out step 1 before step 4. On the other hand, when forming grooves in the wafer surface by dicing or the like, step 1 is carried out after step 4. That is, in step 1, a workpiece processing tape is attached to the surface of the wafer having the grooves formed in step 4 described below.
[0132] In step 4, a groove is formed from the front surface side of the wafer, or a modified region is formed inside the wafer from the front surface or rear surface of the wafer.
[0133] The grooves formed in this step are shallower than the thickness of the wafer. The grooves can be formed by dicing using a conventionally known wafer dicing device or the like. The grooves are the starting points for dicing along the grooves by back grinding in the above-mentioned step 2.
[0134] The modified region is an embrittled portion of the wafer, and is a region that becomes the starting point for breaking and dicing the modified region of the wafer when the wafer becomes thinner due to grinding in the grinding process or when a grinding force is applied. That is, in step 4, the grooves and modified region are formed so as to follow the parting lines when the wafer is diced in the above-mentioned step 2.
[0135] The modified region is formed by irradiating a laser focused on the inside of the wafer, and the modified region is formed inside the wafer. The laser may be irradiated from the front side or the back side of the wafer. In the embodiment in which the modified region is formed, when step 4 is performed after step 1 and the laser is irradiated from the front side of the wafer, the laser is irradiated onto the wafer through the workpiece processing tape.
[0136] In the first dicing method, the back grinding in step 2 is performed so as to thin the wafer at least to the bottom of the groove if a groove is to be formed in the wafer. This back grinding turns the groove into a cut that penetrates the wafer, and the wafer is divided into individual pieces by the cut.
[0137] On the other hand, when a modified region is formed, the grinding surface (wafer back surface) may reach the modified region by grinding, but it does not have to reach the modified region strictly. In other words, it is sufficient to grind to a position close to the modified region so that the wafer is broken and divided into individual pieces starting from the modified region. The workpiece processing tape can be peeled off from the divided wafer (i.e., chip) in the same manner as in step 3 above.
[0138] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES
[0139] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.
[0140] The measurement and evaluation methods in the present examples are as follows.
[0141] (Adhesive strength) The adhesive strength is measured according to JIS Z 0237. Specifically, the workpiece processing tape 10 is cut into a strip of 25 mm width and attached to a silicon wafer with a 2 kg roller under an environment of 23° C. and 50% relative humidity. After 20 minutes, the adhesive strength is determined by the peeling force when peeled in the 180° direction at a speed of 300 mm / min using a universal (peel load) tester Tensilon (manufactured by A&D Co., Ltd.). A mirror-finished wafer with a surface roughness Ra of 5 nm±2 nm is used as the silicon wafer, and the workpiece processing tape is attached to the mirror-finished surface to measure the adhesive strength. The measurement length is 70 mm, and the measurement value at the first 10 mm length and the measurement value at the last 10 mm length are excluded from the effective value. The average value of the measured values is determined as the adhesive strength (mN / 25 mm), and the measurement of the adhesive strength is performed twice, and the average value at that time is adopted.
[0142] (Distortion) The strain is measured according to JIS K 7161. Specifically, the workpiece processing tape 10 is cut into a strip-shaped measurement sample with a width of 15 mm and a length of 150 mm, which is attached to a precision universal testing machine (Shimadzu Corporation), stretched at a stretching speed of 200 mm / min, and the strain (%) is calculated from the elongation amount Δ at the time when the tensile stress reaches 20 MPa. The measurement is performed in an environment with a chuck distance (i.e., initial sample length) of 100 mm, 23°C, and a relative humidity of 50%. The strain (%) is calculated by calculating the elongation amount Δ, which is the difference between the sample length (chuck distance) at the time when the tensile stress reaches 20 MPa and the initial sample length (100 mm), and the ratio of the elongation amount Δ to the initial sample length (100 mm) [=(Δ / 100) × 100] is defined as the strain (%).
[0143] (Tape peeling suitability after grinding the backside of silicon wafers) A tape for workpiece processing was applied to a silicon mirror wafer (a mirror-finished wafer with a surface roughness Ra of 5 nm ± 2 nm) using a tape application device (RAD-3510F / 12) manufactured by Lintec Corporation. The wafer was then ground to a thickness of 50 μm using a back grinding device (DGP8760) manufactured by Disco Corporation. The peeling of the tape for workpiece processing was then evaluated using a tape peeling device (RAD-2700F / 12) manufactured by Lintec Corporation.
[0144] <conditions> 1. Tape is applied to a 300 mm diameter silicon wafer (780 μm thick, mirror wafer without circuits) (Rintec RAD-3510F / 12: application speed 20 mm / sec. temperature 23°C). 2. Wafer grinding: Final wafer thickness 50μm 3. Apply another tape (Litec dicing tape Adwill (registered trademark) D-175D*) to the grinding surface of the silicon wafer. 4. Apply peeling tape to the surface coating layer of the workpiece processing tape (Rintec RAD-2700F / 12, peeling tape: Rintec S-75C, 210℃ 5 seconds application) 5. Peel off the workpiece processing tape (Rintec RAD-2700F / 12: Start peeling speed at 2mm / sec, accelerate to 4mm / sec, and then 8mm / sec. Ambient temperature 23°C, Wafer suction table temperature: No heating (23°C)). During peeling, the longest length of the tape (initially 300mm, the same size as the wafer, but how much it stretches during peeling) was measured and recorded. 6. Peelability was evaluated according to the following criteria.
[0145] <<Judgment criteria>> Grade A (Pass): The tape was peeled off from the wafer. The longest length of the tape during peeling was less than 400 mm. Grade B (Pass): The tape was peeled off from the wafer. The longest length of the tape during peeling was 400 mm or more (i.e., it stretched by 100 mm or more). Grade F (Fail): The tape could not be peeled off due to spatial restrictions of the peeling device, or the tape broke during peeling.
[0146] (Preparation of urethane acrylate oligomer (component (d1)) Three types of bifunctional urethane acrylate oligomers (UA-1, UA-2, UA-3) were prepared as components of the adhesive layer composition. The urethane acrylate oligomers were obtained by reacting 2-hydroxyethyl acrylate with a urethane prepolymer whose terminal isocyanate derived from isocyanate, which was obtained by reacting polypropylene glycol with isophorone diisocyanate. The monomer composition of each urethane acrylate oligomer is shown in the table below.
[0147] [Table 1]
[0148] (Preparation of Composition for Pressure-Sensitive Adhesive Layer) The urethane acrylate oligomer synthesized above, the acrylic monomers shown in the table below, and 2-hydroxy-2-methyl-1-phenyl-1-propanone (IGM Resins, product name "Omnirad 1173") as a photopolymerization initiator (i-1) were mixed to prepare a pressure-sensitive adhesive layer composition, which was used to produce each of the workpiece processing tapes of Examples 1 to 10 and Comparative Examples 1 to 5.
[0149] [Table 2]
[0150] (Preparation of Surface Coating Layer Composition) 100 parts by mass of epoxy acrylate resin (manufactured by Arkema, product name "CN104 NS"), 30 parts by mass of silica filler (manufactured by Nissan Chemical Industries, Ltd., product name "Snowtex (registered trademark) UP"), and 5 parts by mass of phenyl-1-hydroxycyclohexyl-ketone (manufactured by IGM Resins, product name "Omnirad (registered trademark) 184") as a photopolymerization initiator were dissolved and dispersed in toluene to an active ingredient concentration of 5 mass%, to obtain a coating agent for a composition for surface coating layer.
[0151] (Measurement of storage modulus (E') of surface coating layer) The coating agent of the surface coating layer composition was applied onto the release-treated surface of a process release film (manufactured by Lintec Corporation, product name "SP-PET381031", a polyethylene terephthalate (PET) film with silicone release treatment, thickness: 38 μm), and dried at 100° C. for 2 minutes to form an uncured coating layer. 2 , light intensity 700mJ / cm 2The coating layer was cured by irradiation with ultraviolet light (100 Hz) to obtain a surface coating layer sample (55 μm thick) for measuring the storage modulus (E'). The surface coating layer sample was cut to a width of 4 mm, and the release film for processing was removed. The storage modulus (E') of the surface coating layer sample was measured using a dynamic viscoelasticity measuring device (RHEOVIBRON DDV-01FP manufactured by A&D Co., Ltd.) under the following conditions: tension mode, sample length of the measurement section of 20 mm, temperature from -30°C to 120°C, temperature rise of 3°C / min, and measurement frequency of 1 Hz.
[0152] The storage modulus (E') at 23° C. was read from the measured values, and the storage modulus (E') of the surface coating layer was 92 MPa.
[0153] (Manufacture of tape for work processing) The tapes for work processing of Examples 1 to 10 and Comparative Examples 1 to 5 were produced by any of the following methods.
[0154] (First manufacturing method) As shown in FIG. 2(a), a composition for a surface coating layer was applied to the release-treated surface of a first release film 21 (manufactured by Lintec Corporation, product name "SP-PET381031", a polyethylene terephthalate (PET) film with a silicone release treatment, thickness: 38 μm), and then dried to form an uncured coating layer.
[0155] Next, as shown in FIG. 2(b), the composition for pressure-sensitive adhesive layer was applied onto the coating layer 1 of the release film with the coating layer to form an uncured pressure-sensitive adhesive layer 3.
[0156] Next, as shown in Fig. 2(c), the energy beam (illuminance 130 mW / cm 2 , light intensity 50mJ / cm 2 The composition was then exposed to ultraviolet light (300 .mu.m) to semi-cure the energy ray-curable components contained in the surface coating layer composition and the pressure-sensitive adhesive layer composition.
[0157] Next, as shown in FIG. 2(d), a second release film 22 (manufactured by Lintec Corporation, product name "SP-PET381031") was laminated on the semi-cured pressure-sensitive adhesive layer 3.
[0158] Furthermore, as shown in Fig. 2(e), the energy rays (illuminance 350 mW / cm 2 , light intensity 700mJ / cm 2 The energy ray curable components contained in the coating layer 1 and the adhesive layer 3 were all cured, resulting in a surface coating layer 2 (thickness 2 μm) from the coating layer 1, and the uncured adhesive layer 3 was converted into a cured adhesive layer 4 (thickness 123 μm), thereby obtaining a workpiece processing tape 10 having the configuration shown in FIG. 1.
[0159] (Second manufacturing method) As shown in FIG. 3(a), a composition for adhesive layer was applied onto a second release film 22 (manufactured by Lintec Corporation, product name "SP-PET381031") to form an uncured adhesive layer 3.
[0160] Next, as shown in Fig. 3(b), energy rays (illuminance 130 mW / cm 2 , light intensity 50mJ / cm 2 The adhesive layer composition was then exposed to ultraviolet light (ultraviolet rays) to semi-cure the energy ray-curable component contained in the adhesive layer composition.
[0161] Separately from the above, a coating layer 1 was provided on a first release film 21 (manufactured by Lintec Corporation, product name "SP-PET381031") to prepare a first release film with a coating layer.
[0162] Next, as shown in FIG. 3( c ), the coating layer 1 of the first release film with a coating layer was laminated on the semi-cured pressure-sensitive adhesive layer 3 .
[0163] Next, as shown in Fig. 3(d), energy rays (illuminance 350 mW / cm 2 , light intensity 700mJ / cm 2 The composition was then irradiated with energy ray curable light (ultraviolet rays) to cure the energy ray curable components contained in the surface coating layer composition and the pressure sensitive adhesive layer composition.
[0164] The adhesive strength and distortion of each of the workpiece processing tapes obtained above were measured, and the peelability of the tape after grinding the backside of the silicon wafer was evaluated. The results are shown in the table below. In addition, in the tape for processing the workpiece of Comparative Example 4, peeling occurred in the tape for processing the workpiece at the stage of adhering to the silicon wafer in the evaluation of the peeling suitability of the tape after grinding the back surface of the silicon wafer, and the wafer surface (i.e., the workpiece surface) could not be sufficiently protected. Therefore, evaluation was not performed after the wafer grinding process.
[0165] [Table 3] [Industrial Applicability]
[0166] As shown in Table 3, the tape for workpiece processing of the present invention has excellent peeling properties, and the tape for workpiece processing can be peeled off after processing the workpiece to produce a processed workpiece. Specifically, it can be applied to grinding the backside of a wafer. [Explanation of symbols]
[0167] 10...Tape for work processing 1…Uncured coating layer 2...Hardened coating layer 3...Uncured adhesive layer 4...Cured adhesive layer 12...Work (wafer) 12a... Surface of work (circuit surface of wafer) 14…Removal tape 16...Other tapes 18…Tape peeling device 21…First release film 22...Second release film
Claims
1. A work processing tape essentially consisting of two layers, a surface coating layer and a pressure-sensitive adhesive layer, The adhesive strength at 23°C to a silicon wafer having a mirror-finished surface is 0.3 N / 25 mm or more and 3 N / 25 mm or less; When a tensile test of the workpiece processing tape is carried out at 23°C, the product (strain x adhesive strength) of the strain (%) when the tensile stress first reaches 20 MPa and the adhesive strength at 23°C to a silicon wafer having a mirror-finished surface is 500 N-% or less.
2. 2. The tape for workpiece processing according to claim 1, wherein when a tensile test of the tape for workpiece processing is carried out at 23° C., the strain (%) at the time when the tensile stress first reaches 20 MPa is 300% or less.
3. 2. The tape for workpiece processing according to claim 1, wherein the thickness of the adhesive layer is 90 μm or more.
4. 2. The tape for workpiece processing according to claim 1, wherein the surface coating layer has a thickness of 0.2 to 5 μm.
5. 2. The tape for workpiece processing according to claim 1, wherein the adhesive layer is a cured product of a composition for adhesive layer containing an energy ray-curable compound.
6. 13. A method for grinding the back surface of a workpiece, comprising the steps of: applying the workpiece processing tape according to claim 1 to the front surface of the workpiece; grinding the workpiece with the workpiece processing tape applied to its front surface from the back surface side; and peeling the workpiece processing tape from the workpiece after back surface grinding.
Citation Information
Patent Citations
Adhesive sheet
JP2013023665A