Wafer thinning method
The described method for thinning lithium tantalate wafers uses laser-induced modified layers and sequential ultrasonic applications to address high grindstone consumption and productivity issues, achieving efficient and crack-free peeling.
Patent Information
- Application Number
- JP2023053877
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
The existing methods for thinning lithium tantalate wafers face challenges such as high grindstone consumption and decreased productivity due to the difficulty in forming a peeling layer without cracks, and applying ultrasonic waves after bonding does not significantly improve releasability.
A method involving laser beam irradiation to form a modified layer and cracks within the wafer, followed by sequential ultrasonic applications from both sides to facilitate controlled peeling, using support substrates with different thermal expansion coefficients to minimize grindstone wear and enhance peelability.
This approach reduces grindstone consumption and maintains productivity by enabling efficient thinning of wafers with minimal cracking and improved peelability, thus optimizing the manufacturing process.
Smart Images

Figure 2024141964000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for thinning a wafer. [Background technology]
[0002] Lithium tantalate (lithium tantalate oxide; LiTaO3) is used as a substrate for SAW (Surface Acoustic Wave) filters, but due to its large thermal expansion coefficient, frequency shifts caused by temperature increases are considered problematic. Therefore, a method has been devised to improve frequency-temperature characteristics by bonding a lithium tantalate wafer to a support substrate made of silicon, sapphire, or other material with a small thermal expansion coefficient, thereby suppressing thermal expansion. The bonded wafer thus formed is thinned by grinding or other methods, patterned, and diced along the planned division lines to produce device chips.
[0003] However, there were problems with the grinding of lithium tantalate, such as the excessive consumption of the grinding wheel, which was uneconomical, and the time required for grinding, which reduced productivity. Therefore, a method was attempted in which a laser beam was irradiated inside the wafer to form a peeling layer, and peeling was performed using this peeling layer as the starting point (Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-028072 A Summary of the Invention [Problem to be solved by the invention]
[0005] Incidentally, in order to make the wafer to be peeled as thin as possible, it is necessary to process the peeling layer so that cracks do not appear when the peeling layer is formed, which reduces the peelability. Although there is a method of applying ultrasonic waves to improve the peelability, the peelability is not improved much even if ultrasonic waves are applied after the support substrate is bonded, and there is also a problem that handling becomes difficult if the wafer is completely peeled off before the support substrate is bonded.
[0006] The present invention has been made in consideration of such problems, and its object is to provide a wafer thinning method that can reduce the amount of wear on the grinding wheel while suppressing a decrease in productivity. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems and achieve the object, the wafer thinning method of the present invention is a wafer thinning method for thinning a wafer having a first surface and a second surface opposite to the first surface, the method comprising: a first support substrate bonding step of bonding a first support substrate to the first surface side of the wafer; and a step of irradiating the wafer with the laser beam while relatively moving the focal point and the wafer in a direction parallel to the second surface, thereby forming a modified layer parallel to the second surface and a crack extending from the modified layer. a first ultrasonic application step of applying ultrasonic waves from the second surface side of the wafer after performing the first support substrate bonding step and the separation origin forming step; a second support substrate bonding step of bonding a second support substrate to the second surface side of the wafer after performing the first ultrasonic application step; and a thinning step of thinning the wafer by separating the wafer from the separation origin into a wafer having the first surface and a wafer having the second surface after performing the second support substrate bonding step.
[0008] In addition, it is preferable that the wafer thinning method of the present invention further includes a second ultrasonic application step of applying ultrasonic waves to the wafer from the second support substrate side after performing the second support substrate bonding step and before performing the thinning step.
[0009] Furthermore, in the wafer thinning method of the present invention, it is preferable that in the first ultrasonic application step, ultrasonic waves are applied to a first region of the wafer at a first energy density to form a partial peeled portion that is partially peeled off at the separation starting point, and in the second ultrasonic application step, ultrasonic waves are applied to a second region of the wafer that is larger than the first region at a second energy density lower than the first energy density to form a peeled portion from the partial peeled portion over the entire surface of the wafer.
[0010] In the wafer thinning method of the present invention, the wafer may be made of lithium tantalate. Effect of the Invention
[0011] The present invention can reduce the wear amount of the grindstone while suppressing a decrease in productivity. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a perspective view of a wafer to be processed by a wafer thinning method according to an embodiment. [Diagram 2] FIG. 2 is a flowchart showing the flow of the wafer thinning method according to the embodiment. [Diagram 3] FIG. 3 is a perspective view showing the first support substrate bonding step shown in FIG. [Figure 4] FIG. 4 is a side view of the wafer after the first support substrate bonding step shown in FIG. [Diagram 5] FIG. 5 is a perspective view showing one state of the separation start point forming step shown in FIG. [Figure 6] FIG. 6 is a side view, partly in section, showing the state shown in FIG. [Figure 7] FIG. 7 is a top view of the wafer in FIG. [Figure 8] FIG. 8 is a side view showing one state of the first ultrasonic wave applying step shown in FIG. [Figure 9] FIG. 9 is a perspective view showing the second support substrate bonding step shown in FIG. [Figure 10] FIG. 10 is a side view of the wafer after the second support substrate bonding step shown in FIG. [Figure 11] FIG. 11 is a side view showing one state of the second ultrasonic wave applying step shown in FIG. [Figure 12] FIG. 12 is a side view showing one state of the thinning step shown in FIG. [Figure 13] FIG. 13 is a side view of the thinning step shown in FIG. 2 in a state subsequent to FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The form (embodiment) for carrying out the present invention will be described in detail with reference to the drawings. The present invention is not limited to the contents described in the following embodiment. Furthermore, the components described below include those that a person skilled in the art can easily imagine and those that are substantially the same. Furthermore, the configurations described below can be appropriately combined. Furthermore, various omissions, substitutions, or modifications of the configurations can be made without departing from the gist of the present invention.
[0014] [Embodiment] A method for thinning a wafer 10 according to an embodiment of the present invention will be described with reference to the drawings. FIG. 1 is a perspective view of a wafer 10 to be processed by the method for thinning a wafer 10 according to the embodiment. The wafer 10 of the embodiment is a lithium tantalate substrate made of lithium tantalate, but may be, for example, a lithium niobate substrate. The wafer 10 is formed in a disk shape with a thickness of about 350 to 500 μm. The wafer 10 has a first surface 11, a second surface 12, a peripheral surface 13, and an orientation flat 14.
[0015] The first surface 11 is circular and is one end surface of the wafer 10 formed in a disk shape. The first surface 11 corresponds to a bonding surface to be bonded to a first support substrate 20 described below. The second surface 12 is circular and is an end surface opposite to the first surface 11 of the wafer 10 formed in a disk shape. The second surface 12 corresponds to a bonding surface to be bonded to a second support substrate 30 described below. The peripheral surface 13 is a surface that is continuous with the outer edge of the first surface 11 and the outer edge of the second surface 12. The orientation flat 14 is a flat surface formed on a part of the peripheral surface 13 to indicate the crystal orientation of the wafer 10.
[0016] 2 is a flowchart showing a flow of a method for thinning the wafer 10 according to the embodiment. The method for thinning the wafer 10 includes a first support substrate bonding step 1, a separation start point forming step 2, a first ultrasonic wave application step 3, a second support substrate bonding step 4, a second ultrasonic wave application step 5, and a thinning step 6.
[0017] (First Support Substrate Bonding Step 1) Fig. 3 is a perspective view showing the first support substrate bonding step 1 shown in Fig. 2. Fig. 4 is a side view of the wafer 10 after the first support substrate bonding step 1 shown in Fig. 2. The first support substrate bonding step 1 is a step of bonding a first support substrate 20 to the first surface 11 side of the wafer 10.
[0018] In the embodiment, the first support substrate 20 is a glass substrate formed in a disk shape having the same diameter as the wafer 10 and a thickness greater than that of the wafer 10, but the material (hardness), size, thickness, and the like are not particularly limited as long as it can support the wafer 10 and ensure handling. The first support substrate 20 is circular, and has a bonding surface 21 which is one end surface of the first support substrate 20 formed in a disk shape, and a circular surface 22 which is the end surface opposite to the bonding surface 21.
[0019] In the first support substrate bonding step 1, first, the first surface 11 of the wafer 10 and the bonding surface 21 of the first support substrate 20 are opposed to each other with a gap therebetween, as shown in Fig. 3. Next, the first surface 11 of the wafer 10 and the bonding surface 21 of the first support substrate 20 are bonded together, as shown in Fig. 4.
[0020] In this case, when a bonding layer is provided between the wafer 10 and the first support substrate 20, the bonding layer is laminated on one of the first surface 11 of the wafer 10 and the bonding surface 21 of the first support substrate 20, and then the first surface 11 of the wafer 10 and the bonding surface 21 of the first support substrate 20 are bonded together via the bonding layer. The bonding layer may be a double-sided tape having an adhesive layer laminated on the front and back surfaces of a base layer, an oxide film, or a layer formed by applying an adhesive containing a resin or the like.
[0021] (Separation origin formation step 2) Fig. 5 is a perspective view showing one state of the separation origin forming step 2 shown in Fig. 2. Fig. 6 is a side view showing the state shown in Fig. 5 in partial cross section. Fig. 7 is a top view of the wafer 10 in Fig. 6. The separation origin forming step 2 may be performed before the first support substrate bonding step 1 is performed, or may be performed after the first support substrate bonding step 1 is performed. The separation origin forming step 2 is a step of forming separation origins 15 including a modified layer 15-1 parallel to the second surface 12 and a crack 15-2 extending from the modified layer 15-1 by irradiating a laser beam 40 from the second surface 12 side of the wafer 10.
[0022] The separation starting point forming step 2 is performed by a laser processing device 45. The laser processing device 45 includes a holding table 46 and a laser beam irradiation unit 47. The holding table 46 holds the wafer 10 on a holding surface and is rotatable around a vertical axis. The laser beam irradiation unit 47 irradiates the wafer 10 held on the holding table 46 with a laser beam 40. The laser processing device 45 further includes a moving unit (not shown) that relatively moves the holding table 46 and the laser beam irradiation unit 47, and an imaging unit (not shown) that images the wafer 10 held on the holding table 46. In the following description, the X-axis direction is one direction on a horizontal plane. The Y-axis direction is a direction perpendicular to the X-axis direction on a horizontal plane. In the embodiment, the X-axis direction is the processing feed direction, and the Y-axis direction is the index feed direction.
[0023] In the separation starting point forming step 2, the focal point 41 of the laser beam 40 is positioned inside the wafer 10 from the second surface 12 side of the wafer 10, and the laser beam 40 is irradiated while the focal point 41 and the wafer 10 are relatively moved in a direction parallel to the second surface 12. This forms a separation starting point 15 including a modified layer 15-1 parallel to the second surface 12 and a crack 15-2 extending from the modified layer 15-1. The laser beam 40 is a laser beam with a wavelength that is transparent to the wafer 10, for example, infrared rays (IR).
[0024] The modified layer 15-1 refers to a region in which the density, refractive index, mechanical strength, or other physical properties are different from those of the surrounding area. The modified layer 15-1 is, for example, a melting process region, a crack region, a dielectric breakdown region, a refractive index change region, or a region in which these regions are mixed. The modified layer 15-1 has a lower mechanical strength, etc. than other parts of the wafer 10.
[0025] In the separation starting point forming step 2, first, the surface 22 of the first support substrate 20 opposite to the bonding surface 21 is sucked and held on the holding surface (upper surface) of the holding table 46. At this time, the orientation flat 14 of the wafer 10 is adjusted to be parallel to the indexing feed direction (Y-axis direction), in other words, the <11-20> direction indicating the crystal orientation of the wafer 10 is adjusted to be parallel to the processing feed direction (X-axis direction). Next, the wafer 10 is aligned with the condenser of the laser beam irradiation unit 47.
[0026] Specifically, the holding table 46 is moved to an irradiation area below the laser beam irradiation unit 47 by a moving unit (not shown), and the focal point 41 of the laser beam 40 is positioned at a predetermined depth inside the wafer 10. The predetermined depth is a depth of about 20 to 100 μm from the second surface 12 of the wafer 10, and corresponds to the thickness of the wafer 10-2 having the second surface 12 to be separated from the wafer 10-1 having the first surface 11 in a thinning step 6 described later (see FIG. 13).
[0027] In the separation starting point forming step 2, next, with the focal point 41 of the laser beam 40 positioned inside the wafer 10, the laser beam irradiation unit 47 is moved relatively to the holding table 46 in the processing feed direction (X-axis direction). That is, the laser beam 40 is irradiated from the second surface 12 side while the focal point 41 and the wafer 10 are moved relatively in one direction parallel to the second surface 12 (X-axis direction).
[0028] As a result, a modified layer 15-1 is formed at a predetermined depth inside the wafer 10 along one direction (X-axis direction) parallel to the second surface 12. After the laser beam 40 is irradiated up to the outer edge of the wafer 10, the focal point 41 is relatively moved a predetermined amount in the index feed direction (Y-axis direction) to similarly form a modified layer 15-1 along the processing feed direction (X-axis direction), and the modified layer 15-1 is formed over the entire surface of the wafer 10.
[0029] At this time, the crack 15-2 extends from the modified layer 15-1 along a direction parallel to the second surface 12, and a separation starting point 15 including the modified layer 15-1 and the crack 15-2 parallel to the second surface 12 is formed at a predetermined depth inside the wafer 10. The parallel direction indicates that the inclination of the approximation plane, which approximates the entire extended crack 15-2 to a flat surface, with respect to the horizontal plane is within ±5 degrees, preferably within ±2 degrees. In the separation starting point forming step 2, the output of the laser beam 40 is adjusted to form the modified layer 15-1 so that the extending crack 15-2 does not appear on the second surface 12 side of the wafer 10.
[0030] (First ultrasonic application step 3) Fig. 8 is a side view showing one state of the first ultrasonic wave applying step 3 shown in Fig. 2. The first ultrasonic wave applying step 3 is performed after performing the first support substrate bonding step 1 and the separation start point forming step 2. The first ultrasonic wave applying step 3 is a step of applying ultrasonic waves from the second surface 12 side of the wafer 10.
[0031] The first ultrasonic wave applying step 3 is performed by an ultrasonic wave applying device 50. The ultrasonic wave applying device 50 includes a holding table 51, an ultrasonic nozzle 52, and a moving unit (not shown) that moves the holding table 51 and the ultrasonic nozzle 52 relatively. As shown in FIG. 8, the ultrasonic nozzle 52 of the embodiment has a hollow truncated cone portion whose width narrows toward the lower end, and a cylindrical portion extending upward from the upper end of the truncated cone portion. The lower end surface of the ultrasonic nozzle 52 has an opening and is disposed so as to face the holding surface of the holding table 51.
[0032] The ultrasonic nozzle 52 includes an ultrasonic vibrator and a flow path through which a liquid 55 supplied from a liquid supply source (not shown) flows. The ultrasonic vibrator expands and contracts when AC power is applied to generate ultrasonic vibrations. The liquid 55 is, for example, pure water. The liquid 55 is supplied to a position inside the ultrasonic nozzle 52 to which the vibrations caused by the ultrasonic vibrator are transmitted. The liquid 55 to which the vibrations caused by the ultrasonic vibrator are transmitted passes through the flow path of the ultrasonic nozzle 52 and is supplied from an opening formed on the lower end surface of the ultrasonic nozzle 52 to the second surface 12 of the wafer 10 held on the holding table 51 via the first support substrate 20.
[0033] In the first ultrasonic wave application step 3, first, the surface 22 side opposite to the bonding surface 21 of the first support substrate 20 bonded to the wafer 10 on which the separation starting points 15 are formed is sucked and held by the holding surface (upper surface) of the holding table 51. Next, the lower end surface of the ultrasonic nozzle 52 is made to face the second surface 12 of the wafer 10 held on the holding table 51 via the first support substrate 20 with a predetermined gap therebetween, and they are brought close to each other.
[0034] In the first ultrasonic application step 3, next, AC power is applied to the ultrasonic vibrator built in the ultrasonic nozzle 52, and while the ultrasonic vibrator is vibrating, liquid 55 is supplied to the ultrasonic nozzle 52 from a liquid supply source (not shown). At this time, the liquid 55 is supplied to the second surface 12 of the wafer 10 from an opening formed in the lower end surface of the ultrasonic nozzle 52. With the space between the ultrasonic nozzle 52 and the second surface 12 of the wafer 10 immersed in the liquid 55, the ultrasonic vibrator vibrates, so that the ultrasonic vibration of the ultrasonic nozzle 52 is applied to the second surface 12 of the wafer 10 through the liquid 55.
[0035] In the first ultrasonic wave applying step 3, next, liquid 55 is supplied to the second surface 12 of the wafer 10, and while the ultrasonic vibrator is vibrating, the holding table 51 and the ultrasonic nozzle 52 are moved relatively by a moving unit (not shown). As a result, ultrasonic vibration mediated by the liquid 55 is applied to a predetermined area (first area) of the second surface 12 of the wafer 10.
[0036] In the wafer 10, a new crack 15-2 (see FIG. 7) extends at the separation starting point 15 due to the ultrasonic vibration, forming a partially peeled portion 16 that is partially peeled off. In the partially peeled portion 16, the first surface 11 side and the second surface 12 side are separated with the separation starting point 15 as the interface. After applying ultrasonic waves to the first region of the wafer 10, the supply of the liquid 55 is stopped, and the ultrasonic nozzle 52 is moved away from the second surface 12 of the wafer 10.
[0037] (Second Support Substrate Bonding Step 4) Fig. 9 is a perspective view showing the second support substrate bonding step 4 shown in Fig. 2. Fig. 10 is a side view of the wafer 10 after the second support substrate bonding step 4 shown in Fig. 2. The second support substrate bonding step 4 is performed after the first ultrasonic application step 3 is performed. The second support substrate bonding step 4 is a step of bonding a second support substrate 30 to the second surface 12 side of the wafer 10.
[0038] The second support substrate 30 is made of a material with a low thermal expansion coefficient. In the embodiment, the second support substrate 30 is a silicon substrate made of silicon (Si), but may be sapphire (Al2O3) or the like. The second support substrate 30 is formed in a disk shape having the same diameter as the wafer 10 and a thickness greater than that of the wafer 10. The second support substrate 30 is circular and has a bonding surface 31 which is one end surface of the disk-shaped second support substrate 30, and a circular surface 32 which is the end surface opposite to the bonding surface 31.
[0039] In the second support substrate bonding step 4, first, as shown in Fig. 9, the second surface 12 of the wafer 10, in which the first support substrate 20 is bonded to the first surface 11 and the partial peeled portion 16 is formed at the separation starting point 15, is opposed to the bonding surface 31 of the second support substrate 30 with a gap therebetween. Next, as shown in Fig. 10, the second surface 12 of the wafer 10 and the bonding surface 31 of the second support substrate 30 are bonded together.
[0040] In this case, when a bonding layer is provided between the wafer 10 and the second support substrate 30, the bonding layer is laminated on one of the second surface 12 of the wafer 10 and the bonding surface 31 of the second support substrate 30, and then the second surface 12 of the wafer 10 and the bonding surface 31 of the second support substrate 30 are bonded together via the bonding layer. The bonding layer may be a double-sided tape having an adhesive layer laminated on the front and back surfaces of a base layer, an oxide film, or a layer formed by applying an adhesive containing a resin or the like.
[0041] (Second ultrasonic application step 5) Fig. 11 is a side view showing one state of the second ultrasonic wave applying step 5 shown in Fig. 2. The second ultrasonic wave applying step 5 is performed after the second support substrate bonding step 4 is performed and before the thinning step 6 is performed. The second ultrasonic wave applying step 5 is a step of applying ultrasonic waves to the wafer 10 from the second support substrate 30 side.
[0042] The second ultrasonic wave applying step 5 is performed by an ultrasonic wave applying device 60. The ultrasonic wave applying device 60 includes a holding table 61, an ultrasonic horn 62, a liquid supply nozzle 63, and a moving unit (not shown) that relatively moves the holding table 61, the ultrasonic horn 62, and the liquid supply nozzle 63. The ultrasonic horn 62 and the liquid supply nozzle 63 may be a second ultrasonic wave applying unit mounted on a part of the ultrasonic wave applying device 50 shown in FIG. 8, and in this case, the holding table 61 may be shared with the holding table 51 shown in FIG. 8.
[0043] As shown in Fig. 11, the ultrasonic horn 62 of the embodiment is a cylindrical vibration member that is wider than the cylindrical portion of the ultrasonic nozzle 52 shown in Fig. 8. The lower end surface of the ultrasonic horn 62 is provided so as to face the holding surface of the holding table 61. The ultrasonic horn 62 has a built-in ultrasonic vibrator similar to the ultrasonic vibrator built into the ultrasonic nozzle 52 shown in Fig. 8. The built-in ultrasonic vibrator vibrates, causing the entire ultrasonic horn 62 to vibrate.
[0044] The liquid supply nozzle 63 is provided at a position adjacent to the ultrasonic horn 62, and supplies liquid 65 from a liquid supply source (not shown). The liquid 65 is, for example, pure water. The liquid 65 supplied from the liquid supply source (not shown) passes through a flow path in the liquid supply nozzle 63, and is supplied from an opening formed in the lower end surface of the liquid supply nozzle 63 to a surface 32 opposite to a bonding surface 31 of a second support substrate 30 held on the holding table 61 via the first support substrate 20 and the wafer 10.
[0045] In the second ultrasonic wave applying step 5, first, the surface 22 side opposite to the bonding surface 21 of the first support substrate 20 bonded to the wafer 10 to which the second support substrate 30 is bonded is sucked and held by the holding surface (upper surface) of the holding table 61. Note that if the holding table 61 is also the holding table 51 shown in Fig. 8 and the second support substrate bonding step 4 is performed on the holding table 51, this step may be omitted. Next, the lower end surface of the ultrasonic horn 62 is made to face the surface 32 opposite to the bonding surface 31 of the second support substrate 30 held on the holding table 61 via the first support substrate 20 and the wafer 10 at a predetermined interval, and they are brought close to each other.
[0046] In the second ultrasonic wave applying step 5, next, AC power is applied to the ultrasonic vibrator built in the ultrasonic horn 62, and while the entire ultrasonic horn 62 is vibrated, liquid 65 is supplied from a liquid supply source (not shown) to the lower end surface of the ultrasonic horn 62 through the liquid supply nozzle 63. At this time, the liquid 65 is supplied to the surface 32 opposite to the bonding surface 31 of the second support substrate 30. With the space between the ultrasonic horn 62 and the surface 32 of the second support substrate 30 immersed in the liquid 65, the ultrasonic horn 62 vibrates, and ultrasonic vibrations are applied to the surface 32 of the second support substrate 30 through the liquid 65.
[0047] In the second ultrasonic wave applying step 5, next, liquid 65 is supplied to surface 32 of second support substrate 30, and while ultrasonic horn 62 is vibrated, holding table 61 and ultrasonic horn 62 are moved relatively by a moving unit (not shown). As a result, ultrasonic vibration mediated by liquid 65 is applied to a predetermined region (second region) of surface 32 of second support substrate 30.
[0048] The area of the lower end surface of the ultrasonic horn 62 is larger than the area of the opening provided on the lower end surface of the ultrasonic nozzle 52 shown in Fig. 8. Therefore, the second region is larger than the first region to which ultrasonic waves are applied in the first ultrasonic application step 3. In addition, the energy density (first energy density) of the ultrasonic waves applied using the ultrasonic nozzle 52 in the first ultrasonic application step 3 shown in Fig. 8 is higher than the energy density (second energy density) of the ultrasonic waves applied using the ultrasonic horn 62 in the second ultrasonic application step 5 shown in Fig. 11.
[0049] Preferably, the ultrasonic application conditions in the first ultrasonic application step 3 shown in Fig. 8 are that the opening diameter of the ultrasonic nozzle 52 is about 5 to 30 mm, and the output of AC power applied to the ultrasonic transducer is about 10 to 100 W. Moreover, the ultrasonic application conditions in the second ultrasonic application step 5 shown in Fig. 11 are that the lower end surface of the ultrasonic horn 62 is a square or rectangular shape of about 50 mm x 50 mm to 200 mm x 200 mm, and the output of AC power applied to the ultrasonic transducer is about 50 to 150 W.
[0050] In the second ultrasonic application step 5, a new crack 15-2 (see FIG. 7) extends at the separation starting point 15 of the wafer 10 due to the ultrasonic vibration, and a peeled portion 17 is formed over the entire surface of the wafer 10 from the partial peeled portion 16 formed at the separation starting point 15. In the peeled portion 17, the first surface 11 side and the second surface 12 side are separated with the separation starting point 15 as the interface.
[0051] That is, in the first ultrasonic wave applying step 3 shown in Fig. 8, ultrasonic waves are applied to a first region of the wafer 10 at a first energy density to form a partially peeled portion 16 that is partially peeled off at the separation starting point 15, and in the second ultrasonic wave applying step 5 shown in Fig. 11, ultrasonic waves are applied to a second region wider than the first region at a second energy density lower than the first energy density to form a peeled portion 17 from the partially peeled portion 16 over the entire surface of the wafer 10. After applying ultrasonic waves to the second region of the wafer 10, the supply of the liquid 65 is stopped, and the ultrasonic horn 62 is separated from the surface 32 of the second support substrate 30. Note that in the present invention, the second ultrasonic wave applying step 5 may be omitted.
[0052] (Thinning Step 6) Fig. 12 is a side view showing one state of the thinning step 6 shown in Fig. 2. Fig. 13 is a side view showing one state of the thinning step 6 shown in Fig. 2 after Fig. 12. The thinning step 6 is performed after the second ultrasonic wave application step 5 is performed. Note that, in the case where the second ultrasonic wave application step 5 is omitted, the thinning step 6 is performed after the second support substrate bonding step 4 is performed. The thinning step 6 is a step of thinning the wafer 10.
[0053] The thinning step 6 is performed by a peeling device 70. The peeling device 70 includes a holding table 71, a peeling unit 72, and a moving unit (not shown) that moves the holding table 71 and the peeling unit 72 toward and away from each other. The peeling unit 72 may be mounted on a part of the ultrasonic wave applying device 50 shown in Fig. 8 or the ultrasonic wave applying device 60 shown in Fig. 11, and in this case, the holding table 71 may be shared with the holding table 51 shown in Fig. 8 or the holding table 61 shown in Fig. 11.
[0054] The peeling unit 72 has a suction plate 73 with a plurality of suction ports provided on the lower surface thereof. The plurality of suction ports are connected to a suction source (not shown) via a flow path provided inside the suction plate 73. The peeling device 70 suction-holds one surface of an object with the holding table 71 and suction-holds the other surface with the suction plate 73, and separates the holding table 71 and the peeling unit 72 from each other, thereby peeling the object into one surface side and the other surface side.
[0055] In the thinning step 6, first, the surface 22 side opposite to the bonding surface 21 of the first support substrate 20 bonded to the wafer 10 is suction-held by the holding surface (upper surface) of the holding table 71. Note that this step may be omitted if the holding table 71 is also used as the holding table 61 shown in Fig. 11. Next, the lower end surface of the suction plate 73 of the peeling unit 72 is brought close to the surface 32 opposite to the bonding surface 31 of the second support substrate 30 held by the holding table 71 via the first support substrate 20 and the wafer 10, and the suction plate 73 suction-holds the surface 32.
[0056] 13, next, the peeling unit 72 is moved away from the holding table 71. As a result, the wafer 10 pulled vertically is separated at the separation starting point 15 as an interface, and is separated into a wafer 10-1 having a first surface 11 of the wafer 10 and a wafer 10-2 having a second surface 12 of the wafer 10. That is, by separating the wafer 10 from the separation starting point 15 into the wafer 10-1 having the first surface 11 and the wafer 10-2 having the second surface 12, the wafer 10 is thinned into the wafer 10-2.
[0057] The thinned wafer 10-2 becomes, for example, a bonded wafer including a second support substrate 30, and the peeled surface 19 is ground and flattened, and processed into a device wafer. The wafer 10-1 having the first surface 11 from which the wafer 10-2 is peeled is, for example, ground and flattened at the peeled surface 18 to become a new second surface 12, and is used again as a recycled wafer, as the wafer 10. In this case, the first support substrate bonding step 1 of the thinning method of the wafer 10 shown in the flowchart of FIG. 2 is omitted, and the steps from the separation origin formation step 2 to the thinning step 6 are repeatedly performed to generate a plurality of thinned wafers 10-2. Note that the peeled surface 18 of the wafer 10-1 having the first surface 11 and the peeled surface 19 of the wafer 10-2 having the second surface 12 may be subjected to ultrasonic waves before being ground to remove peeled debris.
[0058] As described above, in the method for thinning the wafer 10 according to the embodiment, ultrasonic waves are further applied to the wafer 10 on which the separation starting points 15 are formed to form the partial peeled portion 16 that serves as the peeling starting point, thereby improving the peelability. That is, even if the peelability is reduced at the time when the separation starting points 15 are formed by suppressing the output of the irradiated laser beam 40 so that the cracks 15-2 do not extend too much in the separation starting point forming step 2, the wafer 10-2 to be peeled can be made as thin as possible. This reduces the amount of grinding of the wafer 10-2 after peeling, thereby providing the effect of suppressing a decrease in productivity while reducing the wear of the grindstone.
[0059] Furthermore, after ultrasonic waves are applied to the wafer 10 to form the partial peeled portion 16, a second support substrate 30 is bonded to the second surface 12 of the wafer 10, and ultrasonic waves are applied again through the second support substrate 30, thereby forming a peeled portion 17 across the entire surface of the wafer 10 from the partial peeled portion 16, thereby further improving the peelability. By applying ultrasonic waves in two stages in this manner, it is possible to significantly improve the peelability and suppress cracking of the wafer 10 during peeling.
[0060] It should be noted that the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the gist of the present invention. [Explanation of symbols]
[0061] 10, 10-1, 10-2 wafers 11 First Side 12 The Second Side 15 Separation starting point 15-1 Modified layer 15-2 Crack 16 Partial peeling area 17 Peeling section 20 First supporting substrate 30 Second Support Substrate 40 Laser Beam 41 Focus point 45 Laser processing equipment 50, 60 Ultrasonic application device 52 Ultrasonic nozzle 62 Ultrasonic Horn 63 Liquid supply nozzle 55, 65 liquid 70 Peeling device
Claims
1. A wafer thinning method for thinning a wafer having a first surface and a second surface opposite the first surface, comprising the steps of: a first support substrate bonding step of bonding a first support substrate to the first surface side of the wafer; a separation origin forming step of positioning a focal point of a laser beam having a wavelength that is transparent to the wafer inside the wafer from the second surface side of the wafer, and irradiating the wafer with the laser beam while moving the focal point and the wafer relatively in a direction parallel to the second surface, thereby forming a separation origin including a modified layer parallel to the second surface and a crack extending from the modified layer; a first ultrasonic wave applying step of applying ultrasonic waves from the second surface side of the wafer after performing the first support substrate bonding step and the separation starting point forming step; a second support substrate bonding step of bonding a second support substrate to a second surface side of the wafer after the first ultrasonic wave application step is performed; and a thinning step of thinning the wafer by separating the wafer from the separation starting point into a wafer having the first surface and a wafer having the second surface after performing the second support substrate bonding step.
1. A method for thinning a wafer, comprising:
2. The method further includes a second ultrasonic wave applying step of applying ultrasonic waves to the wafer from the second support substrate side after the second support substrate bonding step and before the thinning step.
2. The method for thinning a wafer according to claim 1 .
3. In the first ultrasonic wave application step, ultrasonic waves are applied to a first region of the wafer at a first energy density to form a partially peeled portion that is partially peeled off at the separation starting point; In the second ultrasonic wave application step, ultrasonic waves are applied to a second region of the wafer that is larger than the first region at a second energy density lower than the first energy density, thereby forming a peeled portion from the partial peeled portion over the entire surface of the wafer.
3. The wafer thinning method according to claim 2 .
4. The wafer is lithium tantalate.
4. The method for thinning a wafer according to claim 1, wherein the method comprises the steps of:
Citation Information
Patent Citations
Wafer production method
JP2017121742A
Methods for making single crystal piezoelectric layers and microelectronic, photonic or optical devices including such layers - Patents.com
JP2019506782A
SiC SUBSTRATE PROCESSING METHOD
JP2020035873A
Peeling method and peeling device
JP2022180703A
Laser-assisted method for cutting crystalline materials
JP2022518126A