Production method of silica sol, production method of abrasive composition, polishing method, production method of semiconductor wafer and semiconductor device
By controlling the alcohol removal rate during solvent replacement in the silica dispersion process, the method achieves precise silanol group concentration on silica particles, enhancing polishing performance for semiconductor manufacturing.
Patent Information
- Application Number
- JP2023054080
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing methods struggle to precisely control the surface silanol group concentration of silica particles, which significantly affects polishing performance in semiconductor manufacturing, leading to inconsistent results.
A method involving the controlled removal and replacement of the solvent in the silica dispersion process, specifically setting the alcohol removal rate to 150 g/h/kg or more, to maintain a high concentration of silanol groups on the silica particle surface during solvent replacement.
This approach allows for precise control of silanol group concentration, resulting in a polishing composition with enhanced polishing performance for semiconductor wafers and devices, ensuring high precision and reducing defects.
Smart Images

Figure 2024142087000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a silica sol, a method for producing a polishing composition, a polishing method, a method for producing a semiconductor wafer, and a method for producing a semiconductor device. [Background technology]
[0002] Polishing methods using polishing liquids are known as methods for polishing the surfaces of materials such as metals and inorganic compounds. In particular, in the final polishing of prime silicon wafers for semiconductors and reclaimed silicon wafers, and in chemical mechanical polishing (CMP) for planarizing interlayer insulating films during semiconductor device manufacturing, forming metal plugs, forming buried wiring, and the like, the surface condition has a significant effect on the semiconductor characteristics, so the surfaces and end faces of these components are required to be polished with extremely high precision.
[0003] In such precision polishing, a polishing composition containing silica sol is adopted, and colloidal silica is widely used as the abrasive grains, which are the main component. Depending on the manufacturing method, colloidal silica is known to be produced by pyrolysis of silicon tetrachloride (fumed silica, etc.), by deionization of alkali silicate such as water glass, and by hydrolysis reaction of alkoxysilane (generally called the "sol-gel method"). Generally, colloidal silica is often used with water as a dispersion medium.
[0004] It is known that the physical properties of colloidal silica affect its performance as a polishing liquid, and many studies have been conducted on it. In particular, the effect of silanol groups on the surface of colloidal silica particles on polishing performance has been extensively studied not only in the polishing of silicon wafers, but also in the chemical mechanical polishing used in the manufacture of semiconductor devices.
[0005] For example, Patent Document 1 discloses a method for producing a silica sol by hydrolysis and condensation of an alkoxysilane. Patent Document 2 discloses that the surface silanol group concentration of silica particles affects the polishing performance of a cobalt film. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2008 / 015943 [Patent Document 2] JP 2018-107293 A Summary of the Invention [Problem to be solved by the invention]
[0007] It is known that the surface silanol group concentration of silica particles significantly affects the polishing performance when used for polishing, but there is a problem in that it is difficult to precisely control the surface silanol group concentration of silica particles.
[0008] In the method for producing silica sol disclosed in Patent Document 1, no mention is made of the surface silanol group concentration of silica particles. In addition, Patent Document 2 discloses that the surface silanol group concentration of silica particles affects polishing performance, but does not disclose how to precisely control it. Thus, it cannot be said that the conventional methods for producing silica sol and silica particles can sufficiently control the surface silanol group concentration of silica particles, and there is a strong demand for precisely controlling the surface silanol group concentration of silica particles.
[0009] The present invention has been made in view of the above problems, and an object of the present invention is to provide a method for producing a silica sol that can precisely control the surface silanol group concentration of silica particles. [Means for solving the problem]
[0010] As a result of extensive research, the inventors discovered that the surface silanol group concentration of silica particles can be controlled by appropriately setting the solvent distillation rate in the process of replacing the solvent of a silica dispersion with water, and thus completed the present invention.
[0011] That is, the gist of the present invention is as follows. [1] A method for producing a silica dispersion comprising the steps of: (1) removing or replacing a dispersion medium in a silica dispersion containing alcohol and water as a dispersion medium in a reaction tank; a removal rate of the alcohol relative to the weight of the silica dispersion from which the dispersing medium has been removed or replaced in the reaction tank is 150 g / h / kg or more during a period in which a ratio of the alcohol to the water in the silica dispersion from which the dispersing medium has been removed or replaced reaches from 6:94 to 0:100 in the step (1). [2] The method for producing a silica sol according to [1], wherein the silica dispersion is obtained by a hydrolysis reaction and a condensation reaction of a tetraalkoxysilane. [3] The method for producing a silica sol according to [2], wherein the tetraalkoxysilane contains tetramethoxysilane. [4] The method for producing a silica sol according to any one of [1] to [3], wherein the substitution of the dispersion medium is performed by removing the dispersion medium containing the alcohol and adding water. [5] The method for producing a silica sol according to any one of [1] to [3], wherein the removal of the dispersion medium is removal of the dispersion medium containing the alcohol. [6] The method for producing a silica sol according to any one of [1] to [5], wherein the alcohol contains methanol. [7] A method for producing a polishing composition, comprising adding a silica sol obtained by the method according to any one of [1] to [6] to produce a polishing composition. [8] A polishing method comprising the step of polishing with a polishing composition containing the silica sol obtained by the production method according to any one of [1] to [6]. [9] A method for manufacturing a semiconductor wafer, comprising the polishing method described in [8].
[10] A method for manufacturing a semiconductor device, comprising the polishing method described in [8]. Effect of the Invention
[0012] According to the method for producing silica sol of this embodiment, by setting the speed of dispersing medium from silica dispersion to a specific range, the silanol group concentration on the surface of silica particle can be kept high during removing or replacing dispersing medium, and the surface silanol group concentration of silica particle can be precisely controlled.Therefore, the polishing composition that uses the obtained silica sol as a polishing agent also shows very good polishing performance in the polishing of semiconductor wafer or semiconductor device that requires extremely high precision polishing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified in various ways within the scope of the gist. In this specification, when the expression "~" is used, it is used as an expression including the numerical values or physical property values before and after it.
[0014] In this specification, the term "silica dispersion" refers to a liquid in which silica particles are dispersed. The silica dispersion can be obtained, for example, by subjecting tetraalkoxysilane to a hydrolysis reaction and a condensation reaction, as described later in step (0).
[0015] <Method of manufacturing silica sol> The method for producing a silica sol according to this embodiment is characterized by including the following step (1). (1) A step of removing or replacing a dispersion medium in a silica dispersion containing alcohol and water as a dispersion medium in a reaction vessel.
[0016] The method for producing a silica sol according to this embodiment preferably further includes the following step (0) before the step (1). Step (0): A step of obtaining a silica dispersion by subjecting tetraalkoxysilane to a hydrolysis reaction and a condensation reaction.
[0017] The method for producing a silica sol according to this embodiment may further include at least one of the following steps (2-1) and (2-2) before and / or after the step (1). Step (2-1): adding a dispersant to the silica dispersion before or after removing or replacing the dispersion medium. Step (2-2): A step of concentrating the silica dispersion before or after removing or replacing the dispersion medium. Each step will be described below.
[0018] <<Process (1)>> Step (1) is a step of removing or replacing the dispersion medium in a silica dispersion containing alcohol and water as the dispersion medium in a reaction tank. In step (1), the rate of removing alcohol relative to the weight of the silica dispersion in the reaction tank from which the dispersion medium has been removed or replaced is set to 150 g / h / kg or more until the ratio of alcohol to water in the silica dispersion from which the dispersion medium has been removed or replaced reaches from 6:94 to 0:100.
[0019] In this specification, the term "silica dispersion" refers to a liquid in which silica particles are dispersed. The silica dispersion can be obtained, for example, by subjecting tetraalkoxysilane to a hydrolysis reaction and a condensation reaction, as described later in step (0).
[0020] The dispersion medium in the silica dispersion, i.e., the dispersion medium to be removed or replaced, is preferably a liquid containing alcohol. This is because, for example, when tetraalkoxysilane is subjected to hydrolysis reaction and condensation reaction to obtain the silica dispersion, alcohol is used as a solvent, etc. Examples of alcohol include methanol, ethanol, propanol, isopropanol, and ethylene glycol.
[0021] The alternative dispersion medium that is substituted for the dispersion medium in the silica dispersion liquid is preferably water.This is because water has a higher boiling point than alcohol, making it easier to substitute, and by making water the dispersion medium of the obtained silica sol, the dispersibility of silica particles is improved.In addition, by making water the dispersion medium of the obtained silica sol, it can be effectively used as the polishing liquid used in the manufacture of semiconductor wafers or semiconductor devices.
[0022] When the dispersion medium in the silica dispersion (the dispersion medium to be replaced) is a liquid containing alcohol and is replaced with water as another dispersion medium, in addition to removing the liquid containing alcohol and adding water, even if the silica dispersion contains an alkali catalyst in addition to alcohol, the alkali catalyst can be removed together with the alcohol by replacing it with water.
[0023] That is, the removal of the dispersion medium of the silica dispersion preferably includes the removal of the dispersion medium containing alcohol, and more preferably includes the removal of the alcohol and the alkali catalyst. The replacement of the dispersion medium of the silica dispersion preferably includes the removal of the dispersion medium containing alcohol and the addition of water, and more preferably includes the removal of the alcohol and the alkali catalyst, and the addition of water.
[0024] In step (1), the rate of alcohol removal relative to the weight of the silica dispersion from which the dispersing medium has been removed or replaced in the reaction tank is set to 150 g / h / kg or more during the period from when the ratio of alcohol to water in the silica dispersion from which the dispersing medium has been removed or replaced reaches from 6:94 to 0:100. By setting the removal rate to 150 g / h / kg or more, the distillation rate of the solvent from the silica sol is increased, and the solvent can be removed or replaced while maintaining a high concentration of silanol groups on the silica particle surfaces during the removal or replacement of the solvent, thereby enabling precise control of the surface silanol group concentration of the silica particles.
[0025] The removal rate is 150 g / h / kg or more, preferably 170 g / h / kg or more, more preferably 190 g / h / kg or more, and particularly preferably 200 g / h / kg or more. The upper limit of the removal rate is not particularly limited, but from the viewpoint of suppressing agglomerates, it is preferably 2000 g / h / kg or less, more preferably 1500 g / h / kg or less.
[0026] The removal or replacement is preferably carried out in a vessel having a jacket, since the silica dispersion can be easily heated. The jacket means a part having a two-layer structure for enabling temperature control, and is usually provided on the outside of the inner vessel. Steam, water, oil, etc. can be poured into the hollow part of the two-layer structure of the jacket to control the temperature.
[0027] When pouring liquid into the hollow portion of the jacket, it is preferable to perform removal or replacement with the liquid level at a position lower than the silica dispersion inside the container that serves as the inner tank, since this can suppress aggregation of silica particles at the three-phase interface between the wall surface of the tank, the silica particle dispersion, and the gas phase.
[0028] The removal rate can be adjusted by appropriately adjusting the temperature of the heat medium. Examples of methods for adjusting the temperature of the heat medium include a method of heating and cooling the heat medium using a circulating thermostatic device, a method of heating the heat medium using a boiler, and a method of adjusting the flow rate of the heat medium.
[0029] The heating temperature when removing or replacing the dispersion medium in the silica dispersion liquid may be set to the boiling point of the dispersion medium in the silica dispersion liquid, and when the dispersion medium is a liquid containing alcohol, for example, 50°C to 100°C is preferable.
[0030] The ratio of the volume of the dispersion medium distilled off per unit time to the volume of water added is preferably maintained at 4:6 to 6:4, more preferably at 4:6 to 5.5:4.5 or 4.5:5.5 to 6:4, and even more preferably at 4.5:5.5 to 5.5:4.5. When the ratio is within the above range, the variation in viscosity of the obtained silica sol and the aggregation of silica particles can be suppressed.
[0031] The removal or replacement of the dispersion medium in the silica dispersion may be carried out under atmospheric pressure or under reduced pressure. When the pressure is reduced, the boiling point of the dispersion medium is lowered to increase the removal rate of the replaced dispersion medium.
[0032] <<Process(0)>> The step (0) is a step of obtaining a silica dispersion by subjecting tetraalkoxysilane to a hydrolysis reaction and a condensation reaction, and is preferably carried out before the above step (1).
[0033] In step (0), for example, the hydrolysis reaction and condensation reaction of tetraalkoxysilane can be carried out by adding a solution (B) containing tetraalkoxysilane and a solution (C) containing water to a solution (A) containing an alkali catalyst.
[0034] The solution (A) contains an alkali catalyst. Examples of the alkali catalyst in the solution (A) include ethylenediamine, diethylenetriamine, triethylenetetraamine, ammonia, urea, ethanolamine, and tetramethylammonium hydroxide. These alkali catalysts may be used alone or in combination of two or more. Among these alkali catalysts, ammonia is preferred because it has excellent catalytic action, is easy to control the particle shape, can suppress metal contamination, is highly volatile, and is easy to remove after hydrolysis and condensation reactions.
[0035] Moreover, it is preferable that the solution (A) contains an alcohol. Examples of the alcohol include methanol, ethanol, propanol, isopropanol, and ethylene glycol. These alcohols may be used alone or in combination of two or more. Among these alcohols, methanol and ethanol are more preferable, and methanol is even more preferable, because they are easy to dissolve tetraalkoxysilane, and the by-products used in the hydrolysis reaction and the condensation reaction are the same as those used in the hydrolysis reaction and the condensation reaction, and therefore they are convenient to manufacture.
[0036] Solution (A) preferably contains water because it can promote the hydrolysis of alkoxysilane. Solution (A) may also contain a solvent other than alcohol and water.
[0037] The concentration of the alkali catalyst in the solution (A) is preferably 0.5% by mass or more in 100% by mass of the solution (A) because it suppresses the aggregation of silica particles and provides excellent dispersion stability of the silica particles in the silica sol, and more preferably 0.6% by mass or more. From the viewpoint of reaction controllability, the concentration of the alkali catalyst is preferably 2.0% by mass or less, and more preferably 1.5% by mass or less.
[0038] The concentration of the alcohol in the solution (A) is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, in 100% by mass of the solution (A) in order to provide excellent particle size control of the silica particles and excellent dispersibility of the tetraalkoxysilane in the reaction solution. In addition, the concentration of the alcohol is preferably 96% by mass or less, and more preferably 94% by mass or less, in order to provide excellent dispersibility of the silicic acid produced by the hydrolysis reaction in the reaction solution.
[0039] The water concentration in solution (A) is preferably 3% by mass or more, more preferably 5% by mass or more, in order to improve the dispersibility of silicic acid produced by hydrolysis in the reaction liquid, in 100% by mass of solution (A). In addition, the water concentration is preferably 90% by mass or less, more preferably 50% by mass or less, in order to improve the dispersibility of tetraalkoxysilane in the reaction liquid.
[0040] The concentration of the solvent other than the alcohol and water in the solution (A) is preferably the same as the concentration of the alkali catalyst, the alcohol, and the balance of the water.
[0041] The solution (B) contains a tetraalkoxysilane. Examples of the tetraalkoxysilane include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetraisopropoxysilane. These tetraalkoxysilanes may be used alone or in combination of two or more. Among these tetraalkoxysilanes, tetramethoxysilane and tetraethoxysilane are preferred, and tetramethoxysilane is more preferred, because they undergo a fast hydrolysis reaction, are less likely to leave unreacted substances, are highly productive, and can easily produce a stable silica sol.
[0042] The solution (B) preferably contains a solvent because it has excellent dispersibility of tetraalkoxysilane in the reaction liquid. Examples of the solvent in the solution (B) include alcohols such as methanol, ethanol, propanol, isopropanol, and ethylene glycol; ketones such as acetone and methyl ethyl ketone; and esters such as ethyl acetate. These solvents may be used alone or in combination of two or more. Among these solvents, alcohols are preferred because the solvents used in the hydrolysis reaction and the condensation reaction are the same as the by-products, and are therefore convenient in production. Methanol and ethanol are more preferred, and methanol is even more preferred.
[0043] The concentration of tetraalkoxysilane in solution (B) is preferably 76% by mass or more, more preferably 77% by mass or more, in 100% by mass of solution (B), because the amount of solvent used can be reduced and the productivity of silica particles is excellent. In addition, the concentration of tetraalkoxysilane is preferably 89% by mass or less, more preferably 88% by mass or less, in order to improve the dispersibility of tetraalkoxysilane in the reaction solution.
[0044] The concentration of the solvent in solution (B) is preferably 11% by mass or more, more preferably 12% by mass or more, in 100% by mass of solution (B), because it is excellent in dispersibility of tetraalkoxysilane in the reaction liquid. In addition, the concentration of the solvent is preferably 24% by mass or less, more preferably 23% by mass or less, because it is possible to reduce the amount of the solvent used and the productivity of silica particles is excellent. In addition, the concentration of the solvent in solution (B) is preferably the concentration of the remainder of the tetraalkoxysilane in solution (B).
[0045] The solution (C) is a solution containing water, and preferably further contains an alkali catalyst. Examples of the alkali catalyst in the solution (C) include ethylenediamine, diethylenetriamine, triethylenetetraamine, ammonia, urea, ethanolamine, and tetramethylammonium hydroxide. These alkali catalysts may be used alone or in combination of two or more. Among these alkali catalysts, ammonia is preferred because it has excellent catalytic action, is easy to control the particle shape, can suppress metal contamination, is highly volatile, and is easy to remove after hydrolysis and condensation reactions.
[0046] Solution (C) may contain a solvent other than water. Examples of the solvent other than water in solution (C) include alcohols such as methanol, ethanol, propanol, isopropanol, and ethylene glycol. These solvents may be used alone or in combination of two or more.
[0047] The concentration of the alkali catalyst in solution (C) may be 0% by mass, i.e., it may not be contained, in 100% by mass of solution (C); however, when the alkali catalyst is contained, it is preferably 1% by mass or more, and in order not to cause the reaction to proceed excessively rapidly and to provide excellent reaction controllability, it is preferably 5% by mass or less, and more preferably 4% by mass or less.
[0048] The water concentration in solution (C) is preferably 95% by mass or more in 100% by mass of solution (C) because the silicic acid produced by the hydrolysis reaction has excellent dispersibility in the reaction liquid, and more preferably 96% by mass or more. The water concentration may be 100% by mass, that is, solution (C) may be composed only of water, but when other components are contained, the water concentration is preferably 99% by mass or less.
[0049] The concentration of the solvent other than water in the solution (C) is preferably the concentration of the balance of water and the alkali catalyst.
[0050] It is preferable that the water concentration in the reaction solution in the reaction system of the hydrolysis reaction and the condensation reaction does not change significantly during the reaction. This is because if the water concentration changes through step (1), the dispersibility of the intermediate product silicic acid in the reaction solution changes, and the stability of the alcohol production is impaired. The rate of change in the water concentration is preferably 75% or less, more preferably 50% or less.
[0051] The water concentration in the reaction system refers to the total amount of water in the total amount of liquids and substances dissolved in the liquids in the reaction system in hydrolysis and condensation reactions. The total amount of liquids and substances dissolved in the liquids in the reaction system is only solution (A) at the start of the reaction, and during the reaction is the total amount of solutions (A), (B), (C) and the alcohol produced in the reaction. The liquids and substances dissolved in the liquids in the reaction system do not include silica particles dispersed in the liquids.
[0052] The concentration of the alkali catalyst in the reaction system of the hydrolysis reaction and the condensation reaction is preferably maintained at 0.5% by mass or more in 100% by mass of the reaction solution in the reaction system, since it suppresses the aggregation of silica particles and provides excellent dispersion stability of the silica particles in the silica sol, and more preferably maintained at 0.6% by mass or more.In addition, it is preferably maintained at 2.0% by mass or less, and more preferably maintained at 1.5% by mass or less, since the reaction does not proceed too quickly and provides excellent reaction controllability.
[0053] The concentration of the alkali catalyst in the reaction system refers to the total amount of the alkali catalyst in the total amount of the liquid and the substances dissolved in the liquid in the reaction system in the hydrolysis reaction and the condensation reaction.
[0054] The reaction temperature of the hydrolysis reaction and condensation reaction of the tetraalkoxysilane, i.e., the temperature of the reaction liquid in the reaction system, is preferably 15° C. or higher, more preferably 20° C. or higher, from the viewpoint of preventing the reaction from proceeding too slowly and providing excellent controllability. Moreover, from the viewpoint of providing an excellent balance between the hydrolysis reaction rate and the condensation reaction rate, the temperature is preferably 50° C. or lower, more preferably 45° C. or lower.
[0055] When the dispersion liquid of silica particles obtained in this step (0) contains alcohol, the dispersion medium in the silica dispersion liquid replaced in the above step (1) (the replaced dispersion medium) will also be a liquid containing alcohol.
[0056] <<Process (2-1)>> Step (2-1) is a step of adding a dispersant to the silica dispersion before or after removing or replacing the dispersion medium in the above step (1), and is preferably carried out at least either before or after the above step (1). By adding the dispersant, aggregation of silica particles in the obtained silica sol can be suppressed.
[0057] Examples of dispersants include inorganic acids, inorganic acid salts, organic acids, organic acid salts, surfactants, etc. These dispersants may be used alone or in combination of two or more. Among these dispersants, organic acids and organic acid salts are preferred because they are not easily decomposed even at high temperatures, have low volatility, and can maintain the inhibition of aggregation and precipitation of colloidal silica, and organic acids and organic acid salts having both a decomposition temperature and a boiling point of 60° C. or higher are more preferred, and citric acid, benzoic acid, ammonium benzoate, triammonium citrate, diammonium hydrogen citrate, and tetramethylammonium citrate are even more preferred.
[0058] Examples of inorganic acids include sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, phosphorous acid, hypophosphorous acid, alkyl phosphate esters, boric acid, pyrophosphoric acid, boric fluoride, tetrafluoroboric acid, hexafluorophosphoric acid, benzenesulfonic acid, and naphthalenesulfonic acid. These inorganic acids may be used alone or in combination of two or more. Among these inorganic acids, sulfuric acid and nitric acid are preferred.
[0059] Examples of inorganic acid salts include ammonium sulfate, ammonium hydrochloride, ammonium nitrate, monoammonium phosphate, diammonium hydrogen phosphate, and ammonium borate octahydrate. These inorganic acid salts may be used alone or in combination of two or more. Among these inorganic acid salts, ammonium sulfate and ammonium nitrate are preferred.
[0060] Examples of organic acids include citric acid, oxalic acid, malic acid, maleic acid, tartaric acid, glutaric acid, adipic acid, pimelic acid, succinic acid, malonic acid, fumaric acid, phthalic acid, formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, and lactic acid. These organic acids may be used alone or in combination of two or more. Among these organic acids, citric acid and benzoic acid are preferred.
[0061] Examples of organic acid salts include ammonium benzoate, triammonium citrate, diammonium hydrogen citrate, ammonium oxalate monohydrate, ammonium formate, ammonium salicylate, ammonium adipate, ammonium acetate, and tetramethylammonium citrate. These organic acid salts may be used alone or in combination of two or more. Among these organic acid salts, ammonium benzoate, triammonium citrate, diammonium hydrogen citrate, and tetramethylammonium citrate are preferred.
[0062] The amount of the dispersant added is preferably 10 ppm by mass or more, more preferably 30 ppm by mass or more, and is preferably 3000 ppm by mass or less, more preferably 1200 ppm by mass or less, based on the silica particles. In order to prevent the silica particles in the silica sol from agglomerating, it is preferable to add the dispersant in a range that does not cause the pH to become less than 6.9.
[0063] <<Process (2-2)>> Step (2-2) is a step of concentrating the silica dispersion before or after removing or replacing the dispersion medium in the above step (1), and is preferably carried out at least one of before step (1) and after step (1).
[0064] In addition, when a step of adding a dispersant in step (2-1) is carried out after step (1), it is also preferable to carry out step (2-2) thereafter. Step (2-2) may be carried out only once, or may be carried out multiple times before and after step (1).
[0065] Examples of the method for concentrating the silica dispersion include heating concentration and vacuum concentration.
[0066] The concentration rate in step (2-2) is preferably 101% by mass or more, more preferably 102% by mass or more, from the viewpoint of excellent polishing rate for a polished object such as a silicon wafer, and is preferably 300% by mass or less, more preferably 200% by mass or less, from the viewpoint of suppressing aggregation of silica particles and generation of fine particles.
[0067] The concentration rate can be calculated by the following formula. Concentration rate (mass%) = (α / β) × 100 In the above formula, α means the mass of the silica dispersion before concentration, and β means the mass of the silica dispersion after concentration.
[0068] <Silica sol> The viscosity of the silica sol obtained by the silica sol production method according to this embodiment (hereinafter sometimes referred to as "the silica sol according to this embodiment" or simply as "silica sol") is preferably 30 mPa·s or less, more preferably 20 mPa·s or less, and even more preferably 15 mPa·s or less, from the viewpoint of handleability. There is no particular restriction on the lower limit of the viscosity, but it is usually 2 mPa·s or more. The viscosity of the silica sol in this embodiment is a value measured using an E-type viscometer under conditions of 25°C and a shear rate of 150 / sec.
[0069] The concentration of silica particles in the silica sol is preferably 3% by mass or more, more preferably 4% by mass or more, and even more preferably 5% by mass or more, from the viewpoint of excellent polishing rate for a polished object represented by a silicon wafer. Also, from the viewpoint of suppressing aggregation of silica particles in the silica sol or polishing composition and excellent storage stability of the silica sol or polishing composition, the concentration of silica particles is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less.
[0070] Metals mixed as impurities in silica sol, i.e., metal impurities, adhere to the surface of the object to be polished during polishing of silicon wafers, contaminating the object, and adversely affecting the properties of the object to be polished and the final product.
[0071] Furthermore, when metal impurities are present in the silica sol, a coordinate interaction occurs between the surface silanol groups, which exhibit acidity, and the metal impurities, changing the chemical properties of the surface silanol groups, such as the acidity, and changing the three-dimensional environment of the silica particle surface, i.e., the ease with which the silica particles aggregate, thereby affecting the polishing rate. Therefore, the metal content in the silica sol, that is, the concentration of metal impurities, is preferably 1 ppm by mass or less, and more preferably 0.2 ppm by mass or less.
[0072] The metal content of silica sol is measured by inductively coupled plasma mass spectrometry (ICP-MS). Specifically, silica sol containing 0.4 g of silica particles is accurately weighed, sulfuric acid and hydrofluoric acid are added, and the mixture is heated, dissolved, and evaporated. Pure water is added to the remaining sulfuric acid droplets so that the total amount is exactly 10 g to create a test solution, which is then measured using an inductively coupled plasma mass spectrometry device. The target metals are sodium, potassium, iron, aluminum, calcium, magnesium, zinc, cobalt, chromium, copper, manganese, lead, titanium, silver, and nickel, and the sum of the contents of these metals is the metal content.
[0073] The metal content of silica sol can be reduced to 1 ppm by mass or less, for example, by obtaining silica particles by hydrolysis and condensation reactions using alkoxysilane as the main raw material. In the method of deionizing alkali silicate such as water glass, sodium and the like derived from the raw material remain, so it is extremely difficult to reduce the metal content of silica particles to 1 ppm by mass or less.
[0074] The content of the dispersion medium in the silica sol is preferably 50% by mass or more, since it can suppress the aggregation of silica particles in the silica sol or polishing composition and the storage stability of the silica sol or polishing composition is excellent, more preferably 60% by mass or more, and even more preferably 70% by mass or more. In addition, from the viewpoint of excellent polishing rate for the polished object represented by silicon wafer, the content of the dispersion medium is preferably 97% by mass or less, more preferably 96% by mass or less, and even more preferably 95% by mass or less.
[0075] The contents of the silica particles and the dispersion medium in the silica sol can be set within the desired ranges in the step (1) and the step (2-2).
[0076] In addition to the silica particles and the dispersion medium, the silica sol may contain other components such as an oxidizing agent, a preservative, an antifungal agent, a pH adjuster, a pH buffer, a surfactant, a chelating agent, and an antibacterial and biocide, as necessary, within the range that does not impair the performance of the silica sol.
[0077] In particular, it is preferable to include an antibacterial biocide in the silica sol, since this provides excellent storage stability of the silica sol.
[0078] Examples of antibacterial biocides include hydrogen peroxide, ammonia, quaternary ammonium hydroxide, quaternary ammonium salt, ethylenediamine, glutaraldehyde, methyl p-hydroxybenzoate, and sodium chlorite. These antibacterial biocides may be used alone or in combination of two or more. Among these antibacterial biocides, hydrogen peroxide is preferred because of its excellent affinity with silica sol. Antibacterial biocides also include those generally known as bactericides.
[0079] The content of the antibacterial biocide in the silica sol is preferably 0.0001% by mass or more, more preferably 0.001% by mass or more, in order to improve the storage stability of the silica sol. In addition, the content of the antibacterial biocide is preferably 10% by mass or less, more preferably 1% by mass or less, in order not to impair the inherent performance of the silica sol.
[0080] The pH of the silica sol is preferably 6.0 or more, more preferably 6.5 or more, because it has excellent dispersion stability and can suppress the aggregation of silica particles.The pH of the silica sol is preferably 8.0 or less, more preferably 7.8 or less, because it prevents dissolution of silica particles and has excellent long-term storage stability. The pH of the silica sol can be adjusted to a desired range by adding a pH adjuster.
[0081] <Physical properties of silica particles> Preferred physical properties of the silica particles in the silica sol produced by the method for producing a silica sol according to this embodiment will be described below.
[0082] (Average primary particle size) The average primary particle size of the silica particles is preferably 5 nm or more, and more preferably 10 nm or more, because the storage stability of the silica sol is excellent.The average primary particle size of the silica particles is preferably 100 nm or less, and more preferably 60 nm or less, because the surface roughness and scratches of the polished object, such as a silicon wafer, can be reduced, and the sedimentation of the silica particles can be suppressed.
[0083] The average primary particle size of the silica particles is measured by the BET method. Specifically, the specific surface area of the silica particles is measured using an automatic specific surface area measuring device, and the average primary particle size is calculated using the following formula (1). Average primary particle diameter (nm) = 6000 / (specific surface area (m 2 / g) x density (g / cm 3 ))···(1)
[0084] The average primary particle size of the silica particles can be set within a desired range by known conditions and methods.
[0085] (Average secondary particle size) The average secondary particle diameter of the silica particles is preferably 10 nm or more, since it is excellent in the removal of particles and the like during cleaning after polishing and excellent in the storage stability of the silica sol, and more preferably 20 nm or more.In addition, the average secondary particle diameter of the silica particles is preferably 200 nm or less, and more preferably 100 nm or less, since it can reduce the surface roughness and scratches of the polished object represented by a silicon wafer during polishing, is excellent in the removal of particles and the like during cleaning after polishing, and can suppress the sedimentation of the silica particles.
[0086] The average secondary particle size of the silica particles is measured by a DLS method, specifically, using a dynamic light scattering particle size measuring device.
[0087] The average secondary particle size of the silica particles can be set within a desired range by known conditions and methods.
[0088] (cv value) The cv value of the silica particles is preferably 10% or more, since it provides an excellent polishing rate for a polished object such as a silicon wafer and is excellent in productivity of the silicon wafer, more preferably 15% or more, and even more preferably 20% or more. In addition, the cv value of the silica particles is preferably 50% or less, more preferably 40% or less, and even more preferably 35% or less, since it can reduce the surface roughness and scratches of a polished object such as a silicon wafer during polishing and provides excellent removal of particles and the like during cleaning after polishing.
[0089] The cv value of the silica particles is calculated using the following formula (2) by measuring the average secondary particle size of the silica particles using a dynamic light scattering particle size measuring device. cv value (%) = (standard deviation (nm) / average secondary particle size (nm)) × 100 (%) (2)
[0090] (association ratio) The association ratio of silica particles is preferably 1.0 or more, since it provides a superior polishing rate for a polished object such as a silicon wafer and superior productivity of silicon wafers, and is more preferably 1.1 or more. In addition, it is preferably 4.0 or less, and more preferably 3.0 or less, since it can reduce the surface roughness and scratches of a polished object such as a silicon wafer during polishing and can suppress the aggregation of silica particles.
[0091] The association ratio of silica particles is calculated using the following formula (3) from the average primary particle diameter measured by the above-mentioned measuring method and the average secondary particle diameter measured by the above-mentioned measuring method. Association ratio = average secondary particle size / average primary particle size...(3)
[0092] (Surface silanol group concentration) From the viewpoint of dispersion stability, the surface silanol group concentration of the silica particles is preferably 0.2% or more, more preferably 0.5% or more, and even more preferably 0.8% or more, and from the viewpoint of suppressing aggregation of the silica particles, it is preferably 1.35% or less, more preferably 1.3% or less, and even more preferably 1.25% or less.
[0093] The surface silanol group concentration of the silica particles is measured by the Sears method. Specifically, the measurement is performed under the following conditions, and the concentration is calculated.
[0094] Take a silica sol equivalent to 1.5 g of silica particles, add pure water to make the liquid volume 90 mL, add 0.1 mol / L hydrochloric acid aqueous solution in an environment of 25°C until the pH becomes 3.6, then add 30 g of sodium chloride, gradually add pure water to completely dissolve the sodium chloride, and finally add pure water until the total volume of the test liquid is 150 mL to obtain the test liquid.
[0095] The obtained test liquid is placed in an automatic titrator, and 0.1 mol / L aqueous sodium hydroxide solution is added dropwise to measure the titer A (mL) of 0.1 mol / L aqueous sodium hydroxide solution required to change the pH from 4.0 to 9.0.
[0096] The method for measuring and calculating the surface silanol group concentration of the above silica particles is based on "GW Ears, Jr., Analytical Chemistry, Vol. 28, No. 12, pp. 1981-1983 (1956)," "Haba Shinichi, Development of Abrasives for Semiconductor Integrated Circuit Processing, Doctoral Dissertation, Kochi University of Technology, pp. 39-45, March 2004," "Patent No. 5967118," and "Patent No. 6047395."
[0097] The surface silanol group concentration of the silica particles was calculated by calculating the consumption amount V (mL) of 0.1 mol / L aqueous sodium hydroxide solution required for the pH to change from 4.0 to 9.0 per 1.5 g of silica particles using the following formula (4), and the surface silanol group concentration C of the silica particles was calculated using the following formula (5). OH (%) was calculated. V=(A×f×100×1.5) / (W×C)...(4) A: The amount (mL) of 0.1 mol / L sodium hydroxide solution required to change the pH from 4.0 to 9.0 per 1.5 g of silica particles f: Potency of the 0.1 mol / L sodium hydroxide solution used C SiO2 : Concentration of silica particles in silica sol (mass%) W: Amount of silica sol collected (g) C OH =(B×M OH ) / m×100···(5) B: The amount of sodium hydroxide (mol) required to change the pH from 4.0 to 9.0 per 1.5 g of silica particles calculated from V M OH : Molar mass of OH (17g / mol) m: amount of silica particles (1.5g)
[0098] The surface silanol group concentration of the silica particles can be precisely controlled by setting the rate of removal of the alcohol relative to the weight of the silica dispersion in the reaction tank to 150 g / h / kg or more during the period in which the ratio of alcohol to water in the silica dispersion from which the dispersing medium has been removed or replaced reaches from 6:94 to 0:100 in the above step (1).
[0099] (shape) Examples of the shape of silica particles include spherical, chain-like, cocoon-like (also called lump-like or peanut-like), irregular shapes (for example, wart-like, bent, branched, etc.) etc. Among these silica particle shapes, when it is desired to reduce the surface roughness or scratches of a polished object, such as a silicon wafer, during polishing, a spherical shape is preferred, and when it is desired to increase the polishing rate of a polished object, such as a silicon wafer, an irregular shape is preferred.
[0100] [Polishing composition] The silica sol obtained by the method for producing a silica sol according to this embodiment can be suitably used as a polishing composition. The polishing composition preferably contains the silica sol produced by the method for producing a silica sol according to this embodiment and a water-soluble polymer.
[0101] The water-soluble polymer enhances the wettability of the polishing composition to the object to be polished, such as a silicon wafer. The water-soluble polymer is preferably a polymer having a functional group with high water affinity, and the functional group with high water affinity has a high affinity with the surface silanol group of the silica particles, so that the silica particles and the water-soluble polymer are stably dispersed in the polishing composition in a closer vicinity. Therefore, when polishing the object to be polished, such as a silicon wafer, the effects of the silica particles and the water-soluble polymer function synergistically.
[0102] Examples of the water-soluble polymer include cellulose derivatives, polyvinyl alcohol, polyvinylpyrrolidone, copolymers having a polyvinylpyrrolidone skeleton, and polymers having a polyoxyalkylene structure.
[0103] Examples of cellulose derivatives include hydroxyethyl cellulose, hydrolyzed hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, ethyl cellulose, ethyl hydroxyethyl cellulose, and carboxymethyl cellulose.
[0104] An example of the copolymer having a polyvinylpyrrolidone skeleton is a graft copolymer of polyvinyl alcohol and polyvinylpyrrolidone.
[0105] Examples of polymers having a polyoxyalkylene structure include polyoxyethylene, polyoxypropylene, and copolymers of ethylene oxide and propylene oxide.
[0106] These water-soluble polymers may be used alone or in combination of two or more. Among these water-soluble polymers, cellulose derivatives are preferred, and hydroxyethyl cellulose is more preferred, because they have high affinity with the surface silanol groups of silica particles and act synergistically to impart good hydrophilicity to the surface of the polished object.
[0107] The weight-average molecular weight of the water-soluble polymer is preferably 1,000 or more, since the hydrophilicity of the polishing composition is improved, more preferably 5,000 or more, and even more preferably 10,000 or more.In addition, since the water-soluble polymer has excellent affinity with silica sol and has an excellent polishing rate for a polished object such as a silicon wafer, the weight-average molecular weight is preferably 3,000,000 or less, more preferably 2,000,000 or less, and even more preferably 1,000,000 or less.
[0108] The weight-average molecular weight of the water-soluble polymer is measured by size exclusion chromatography using a 0.1 mol / L NaCl solution as the mobile phase, in terms of polyethylene oxide.
[0109] The content of the water-soluble polymer in the polishing composition is preferably 0.02% by mass or more, more preferably 0.05% by mass or more, because the hydrophilicity of the polishing composition is improved. Also, the content of the water-soluble polymer is preferably 10% by mass or less, more preferably 5% by mass or less, because the aggregation of silica particles during preparation of the polishing composition can be suppressed.
[0110] In addition to the silica sol and the water-soluble polymer, the polishing composition may contain other components, such as a basic compound, a polishing accelerator, a surfactant, a hydrophilic compound, a preservative, an antifungal agent, a pH adjuster, a pH buffer, a chelating agent, and an antibacterial and biocide, as necessary, within the range that does not impair the performance of the polishing composition.
[0111] In particular, it is preferable to include a basic compound in the polishing composition, since it is possible to perform chemical polishing, i.e., chemical etching, by applying a chemical action to the surface of an object to be polished, such as a silicon wafer, and it is possible to improve the polishing rate of an object to be polished, such as a silicon wafer, due to a synergistic effect with the surface silanol groups of the silica particles.
[0112] Examples of the basic compound include organic basic compounds, alkali metal hydroxides, alkali metal hydrogen carbonates, alkali metal carbonates, and ammonia. These basic compounds may be used alone or in combination of two or more. Among these basic compounds, ammonia, tetramethylammonium hydroxide, tetraethylammonium hydroxide, ammonium hydrogen carbonate, and ammonium carbonate are preferred because they are highly water-soluble and have excellent affinity with silica particles and water-soluble polymers, and ammonia, tetramethylammonium hydroxide, and tetraethylammonium hydroxide are more preferred, with ammonia being even more preferred.
[0113] The content of basic compound in the polishing composition is preferably 0.001 mass% or more, since it can improve the polishing speed of the object to be polished, such as silicon wafer, and more preferably 0.01 mass% or more.In addition, the content of basic compound is preferably 5 mass% or less, and more preferably 3 mass% or less, since it is excellent in stability of the polishing composition.
[0114] The pH of the polishing composition is preferably 8.0 or more, since it can suppress the aggregation of silica particles in the polishing composition and the dispersion stability of the polishing composition is excellent, and more preferably 9.0 or more.In addition, the pH of the polishing composition is preferably 12.0 or less, and more preferably 11.0 or less, since it can suppress the dissolution of silica particles and the stability of the polishing composition is excellent. The pH of the polishing composition can be adjusted to a desired range by adding a pH adjuster.
[0115] The polishing composition can be obtained by mixing the silica sol according to this embodiment, the water-soluble polymer, and, if necessary, other components. However, taking into consideration storage and transportation, the composition may be prepared at a high concentration and then diluted with water or the like immediately before polishing.
[0116] [Polishing method] The polishing method according to this embodiment includes a step of polishing with a polishing composition containing the silica sol obtained by the method for producing a silica sol according to this embodiment. The polishing composition is preferably the above-mentioned polishing composition. Since the clogging coefficient of the silica sol is small and the aggregation of silica particles in the silica sol is suppressed, the polishing method according to the present embodiment can suppress the occurrence of polishing unevenness and polishing scratches.
[0117] A specific example of the polishing method is a method in which the surface of a silicon wafer is pressed against a polishing pad, the polishing composition is dropped onto the polishing pad, and the surface of the silicon wafer is polished.
[0118] [Methods of manufacturing semiconductor wafers and semiconductor devices] The method for manufacturing a semiconductor wafer according to this embodiment and the method for manufacturing a semiconductor device according to this embodiment include the polishing method according to this embodiment.
[0119] [Application] The silica sol according to this embodiment can be suitably used for polishing purposes, for example, polishing semiconductor materials such as silicon wafers, polishing electronic materials such as hard disk substrates, polishing in the planarization process in manufacturing integrated circuits (chemical mechanical polishing), polishing synthetic quartz glass substrates used for photomasks and liquid crystals, polishing magnetic disk substrates, and the like, and among these, it can be particularly suitably used for polishing silicon wafers and chemical mechanical polishing. EXAMPLES
[0120] The present invention will be described in more detail below using examples. However, the present invention is not limited to the description of the following examples as long as it does not deviate from the gist of the present invention.
[0121] [Measurement method] (Measurement of average primary particle size) The silica sol obtained in the examples and comparative examples was dried at 150°C, and the specific surface area of the silica particles was measured using an automatic specific surface area measuring device "BELSORP-MR1" (model name, Microtrack BEL Co., Ltd.). The density was calculated to be 2.2 g / cm using the following formula (1). 3 The average primary particle size was calculated. Average primary particle diameter (nm) = 6000 / (specific surface area (m 2 / g) x density (g / cm 3 ))···(1)
[0122] (Measurement of average secondary particle size) The average secondary particle size of the silica particles in the silica sols obtained in the Examples and Comparative Examples was measured using a dynamic light scattering particle size measurement device "Zetersizer Nano ZS" (model name, manufactured by Malvern Instruments).
[0123] (Calculation of association ratio) The association ratio was calculated from the measured average primary particle size and average secondary particle size using the following formula (3). Association ratio = average secondary particle size / average primary particle size...(3)
[0124] (Measurement of surface silanol group concentration) The silica sol obtained in each of the Examples and Comparative Examples was placed in a 200 mL tall beaker in an amount equivalent to 1.5 g of silica particles, and purified water was added to make the liquid volume 90 mL. In an environment of 25°C, a pH electrode was inserted into the tall beaker, and the test solution was stirred for 5 minutes with a magnetic stirrer. With stirring continued with the magnetic stirrer, 0.1 mol / L aqueous hydrochloric acid was added until the pH reached 3.6. The pH electrode was removed from the tall beaker, and with stirring continued with the magnetic stirrer, 30 g of sodium chloride was added, and pure water was gradually added until the sodium chloride was completely dissolved. Finally, pure water was added until the total volume of the test solution was 150 mL, and the test solution was stirred with a magnetic stirrer for 5 minutes to obtain a test solution. The tall beaker containing the obtained test solution was placed in an automatic titration device "COM-1600" (manufactured by Hiranuma Sangyo Co., Ltd.), and the pH electrode and burette included with the device were inserted into the tall beaker. While stirring the test solution with a magnetic stirrer, 0.1 mol / L aqueous sodium hydroxide solution was dropped through the burette, and the titration amount A (mL) of 0.1 mol / L aqueous sodium hydroxide solution required to change the pH from 4.0 to 9.0 was measured. The consumption amount V (mL) of 0.1 mol / L sodium hydroxide solution required for the pH to change from 4.0 to 9.0 per 1.5 g of silica particles was calculated using the following formula (4), and the surface silanol group concentration C of the silica particles was calculated using the following formula (5). OH (%) was calculated. V=(A×f×100×1.5) / (W×C)...(4) A: The amount (mL) of 0.1 mol / L sodium hydroxide solution required to change the pH from 4.0 to 9.0 per 1.5 g of silica particles f: Potency of the 0.1 mol / L sodium hydroxide solution used C SiO2 : Concentration of silica particles in silica sol (mass%) W: Amount of silica sol collected (g) C OH =(B×M OH ) / m ×100···(5) B: The amount of sodium hydroxide (mol) required to change the pH from 4.0 to 9.0 per 1.5 g of silica particles calculated from V M OH: Molar mass of OH (17g / mol) m: amount of silica particles (1.5g)
[0125] [Comparative Example 1] A solution (B) of 85 mass% tetramethoxysilane and 15 mass% methanol was mixed, and a solution (C) of 3 mass% aqueous ammonia was prepared. A reaction vessel equipped with a thermometer, a stirrer, a supply pipe, and a distillation line was charged with a solution (A) of methanol, pure water, and ammonia mixed in advance. The concentration of methanol in solution (A) was 84.5 mass%, the concentration of water in solution (A) was 15 mass%, and the concentration of ammonia in solution (A) was 0.5 mass%.
[0126] To 132 mass% of solution (A), 100 mass% of solution (B) and 37 mass% of solution (C) were added at equal rates over 612 minutes to obtain a dispersion of silica particles with a silica particle content of approximately 12.5 mass%.
[0127] The obtained dispersion of silica particles was heated and concentrated so that the content of silica particles was about 17.5% by mass. Next, methanol and ammonia were removed while adding pure water so as to keep the amount of the dispersion of silica particles constant. Next, the dispersion of silica particles was concentrated to obtain a dispersion of silica particles (silica sol) with a content of silica particles of about 20% by mass. For the water replacement, the temperature of the heat medium was adjusted so that the average alcohol removal rate relative to the weight of the dispersion in the tank was 35 g / h / kg until the ratio of methanol to water in the dispersion of silica particles reached from 6:94 to 0:100.
[0128] [Comparative Example 2] A solution (B) of 85 mass% tetramethoxysilane and 15 mass% methanol was mixed, and a solution (C) of 3 mass% aqueous ammonia was prepared. A reaction vessel equipped with a thermometer, a stirrer, a supply pipe, and a distillation line was charged with a solution (A) of methanol, pure water, and ammonia mixed in advance. The concentration of methanol in solution (A) was 84.5 mass%, the concentration of water in solution (A) was 15 mass%, and the concentration of ammonia in solution (A) was 0.5 mass%.
[0129] To 132 mass% of solution (A), 100 mass% of solution (B) and 37 mass% of solution (C) were added at equal rates over 612 minutes to obtain a dispersion of silica particles with a silica particle content of approximately 12.5 mass%.
[0130] The obtained dispersion of silica particles was heated and concentrated so that the content of silica particles was about 17.5% by mass. Next, methanol and ammonia were removed while adding pure water so as to keep the amount of the dispersion of silica particles constant. Next, the dispersion of silica particles was concentrated to obtain a dispersion of silica particles (silica sol) with a content of silica particles of about 20% by mass. For the water replacement, the temperature of the heat medium was adjusted so that the average alcohol removal rate relative to the weight of the dispersion in the tank was 120 g / h / kg until the ratio of methanol to water in the dispersion of silica particles reached from 6:94 to 0:100.
[0131] [Example 1] A solution (B) of 85 mass% tetramethoxysilane and 15 mass% methanol was mixed, and a solution (C) of 3 mass% aqueous ammonia was prepared. A reaction vessel equipped with a thermometer, a stirrer, a supply pipe, and a distillation line was charged with a solution (A) of methanol, pure water, and ammonia mixed in advance. The concentration of methanol in solution (A) was 84.5 mass%, the concentration of water in solution (A) was 15 mass%, and the concentration of ammonia in solution (A) was 0.5 mass%.
[0132] To 132 mass% of solution (A), 100 mass% of solution (B) and 37 mass% of solution (C) were added at equal rates over 612 minutes to obtain a dispersion of silica particles with a silica particle content of approximately 12.5 mass%.
[0133] The obtained dispersion of silica particles was heated and concentrated so that the content of silica particles was about 17.5% by mass. Next, methanol and ammonia were removed while adding pure water so as to keep the amount of the dispersion of silica particles constant. Next, the dispersion of silica particles was concentrated to obtain a dispersion of silica particles (silica sol) with a content of silica particles of about 20% by mass. For the water replacement, the temperature of the heat medium was adjusted so that the average alcohol removal rate relative to the weight of the dispersion in the tank was 206 g / h / kg during the period when the ratio of methanol to water in the dispersion of silica particles reached from 6:94 to 0:100.
[0134] The evaluation results of the obtained silica sol are shown in Table 1.
[0135] [Table 1]
[0136] As shown in Table 1, according to the method for producing a silica sol according to this embodiment, the average alcohol removal rate relative to the weight of the dispersion in the tank during the period from when the ratio of methanol to water in the dispersion of silica particles reaches 0:100 to 6:94 is 150 g / h / kg or more, and therefore it is possible to precisely control the surface silanol group concentration of the silica particles. It was also found that the surface silanol group concentration of the silica sol obtained by the method for producing a silica sol according to this embodiment is precisely controlled. [Industrial Applicability]
[0137] The silica sol obtained by the method for producing a silica sol according to this embodiment can be suitably used for polishing purposes, such as polishing semiconductor materials such as silicon wafers, polishing electronic materials such as hard disk substrates, polishing in the planarization process when manufacturing integrated circuits (chemical mechanical polishing), polishing synthetic quartz glass substrates used for photomasks and liquid crystals, polishing magnetic disk substrates, polishing metals such as Si, Cu, W, Ti, Cr, Co, Zr, Hf, Mo, Ta, Ru, Au, Pt, or Ag, and metal compounds such as oxides, nitrides, and silicides of the above metals, and among these, it can be particularly suitably used for polishing silicon wafers and chemical mechanical polishing.
Claims
1. The method includes a step (1) of removing or replacing a dispersion medium in a silica dispersion containing alcohol and water as a dispersion medium in a reaction tank, a removal rate of the alcohol relative to the weight of the silica dispersion from which the dispersion medium has been removed or replaced in the reaction tank is 150 g / h / kg or more during a period in which a ratio of the alcohol to the water in the silica dispersion from which the dispersion medium has been removed or replaced reaches from 6:94 to 0:100 in the step (1).
2. The method for producing a silica sol according to claim 1 , wherein the silica dispersion is obtained by a hydrolysis reaction and a condensation reaction of a tetraalkoxysilane.
3. The method for producing a silica sol according to claim 2 , wherein the tetraalkoxysilane includes tetramethoxysilane.
4. The method for producing a silica sol according to claim 1 , wherein the substitution of the dispersion medium comprises removing the dispersion medium containing the alcohol and adding water.
5. The method for producing a silica sol according to claim 1 , wherein the removal of the dispersion medium is removal of the dispersion medium containing an alcohol.
6. The method for producing a silica sol according to claim 1 , wherein the alcohol comprises methanol.
7. A method for producing a polishing composition, comprising adding the silica sol obtained by the method according to claim 1 to produce a polishing composition.
8. A polishing method comprising a step of polishing with a polishing composition containing the silica sol obtained by the production method according to claim 1.
9. A method for producing a semiconductor wafer, comprising the polishing method according to claim 8.
10. A method for manufacturing a semiconductor device, comprising the polishing method according to claim 8.
Citation Information
Patent Citations
Composition for chemical mechanical polishing, and chemical mechanical polishing method
JP2018107293A
Silica sol and process for production thereof
WO2008015943A1