Cellulose particle
Cellulose particles with defined parameters of volume average diameter, circularity, BET specific surface area, and solidity address extensibility and adsorption issues, enhancing their performance in applications like cosmetics.
Patent Information
- Application Number
- JP2023054185
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing cellulose particles lack optimal properties for extensibility, adsorption, and sustained release of components, particularly in applications like cosmetics, due to inappropriate particle size, surface structure, and BET specific surface area.
Cellulose particles with specific parameters: volume average particle diameter of 1 μm to 30 μm, circularity of 0.86 or more, A value less than 0.15, BET specific surface area of 0.25 m²/g to 7 m²/g, and solidity of 90% or more, which enhance extensibility, adsorption, and sustained release properties.
The specified parameters improve cellulose particles' extensibility, adsorption, and sustained release capabilities, making them suitable for applications requiring flexibility and biodegradability, such as cosmetics.
Smart Images

Figure 2024142153000001
Abstract
Description
[Technical field]
[0001] The present invention relates to cellulose particles. [Background technology]
[0002] Patent Document 1 proposes "a method for adjusting the size of micropores in a cellulose material, which comprises treating the cellulose material with a liquid treating agent capable of swelling the cellulose material."
[0003] Patent Document 2 proposes "particles having a wrinkled or pleated uneven structure on the surface, a crystallinity of 80% or less, and containing cellulose or a cellulose derivative as a main component."
[0004] Patent Document 3 proposes "particles having an uneven surface structure and containing cellulose or a cellulose derivative and a clay mineral as main components." [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 2-222401 [Patent Document 2] International Publication No. 2019 / 151486 [Patent Document 3] International Publication No. 2020 / 054810 Summary of the Invention [Problem to be solved by the invention]
[0006] The objective of the present invention is to provide cellulose particles having cellulose as the main component, which have excellent extensibility, adsorption properties, and sustained release properties of components, compared to cellulose particles having a volume average particle size D of less than 1 μm or more than 30 μm, a circularity of less than 0.86, or an A value represented by the following formula (1) of 0.15 or more. do. [Means for solving the problem]
[0007] Means for solving the above problems include the following aspects. <1> The main component is cellulose, The volume average particle size D is 1 μm or more and 30 μm or less, The circularity is 0.86 or more, The A value represented by the following formula (1) is less than 0.15. Solid cellulose particles. Formula (1): A=1 / (D×S) (In formula (1), D is the volume average particle size of the cellulose particles (μm), S is the BET specific surface area of the cellulose particles (m 2 / g). <2> The volume average particle size is 2 μm or more and 20 μm or less. <1> The cellulose particles according to claim 1. <3> The value A in the formula (1) is 0.1 or less. <1> or <2> The cellulose particles according to claim 1. <4> The BET specific surface area is 0.25 m 2 / g or more 7m 2 / g or less <1> ~ <3> The cellulose particles according to any one of claims 1 to 5. <5> The BET specific surface area is 0.5 m 2 / g or more 5m 2 / g or less <4> The cellulose particles according to claim 1. <6> Circularity is 0.88 or more <1> ~ <5> The cellulose particles according to any one of claims 1 to 5. <7> The circularity is 0.9 or more. <6> The cellulose particles according to claim 1. <8> Solidity is 90% or more <1> ~ <7> The cellulose particles according to any one of claims 1 to 5. <9> The solidity is 95% or more. <8> The cellulose particles according to claim 1. <10> The BET specific surface area is 0.25 m 2 / g or more 7m 2 / g or less The circularity is 0.88 or more, Solidity is 90% or more <1> ~ <8> The cellulose particles according to any one of claims 1 to 5. <11> The volume average particle size is 2 μm or more and 20 μm or less, The value A represented by the formula (1) is less than 0.1, The BET specific surface area is 0.5 m 2 / g or more 5m 2 / g or less, The circularity is 0.9 or more, Solidity is 95% or more <1> ~ <8> The cellulose particles according to any one of claims 1 to 5. Effect of the Invention
[0008] <1> According to the present invention, cellulose particles having cellulose as the main component are provided which have excellent extensibility, adsorption properties, and sustained release properties of components, compared to cellulose particles having a volume average particle size D of less than 1 μm or more than 30 μm, a circularity of less than 0.86, or an A value represented by the following formula (1) of 0.15 or more. <2> According to the present invention, there are provided cellulose particles which are excellent in extensibility, adsorptivity, and sustained release of ingredients, as compared with those having a volume average particle size of less than 2 μm or more than 20 μm. <3> According to the present invention, there are provided cellulose particles which are excellent in extensibility, adsorptivity, and sustained release of components, as compared with those in which the A value represented by formula (1) exceeds 0.1. <4> According to the invention, the BET specific surface area is 0.25 m 2 / g or less than 7m 2 / g or more, the cellulose particles provided are superior in elongation, adsorptive properties, and sustained release of ingredients. <5> According to the invention, the BET specific surface area is 0.5 m 2 / g or less than 5m 2 / g or more, the cellulose particles provided are superior in elongation, adsorptive properties, and sustained release of ingredients. <6> According to the present invention, there are provided cellulose particles which are excellent in extensibility, adsorptivity, and sustained release of ingredients, as compared with cellulose particles having a circularity of less than 0.88. <7> According to the present invention, there are provided cellulose particles which are excellent in extensibility, adsorptive property, and sustained release property of components, as compared with cellulose particles having a circularity of less than 0.9. <8> According to the present invention, there are provided cellulose particles which are excellent in extensibility, adsorptivity, and sustained release of ingredients, as compared with cellulose particles having a solidity of less than 90%. <9> According to the present invention, there are provided cellulose particles which are excellent in extensibility, adsorptivity, and sustained release of ingredients, as compared with cellulose particles having a solidity of less than 95%. <10> According to the invention, the BET specific surface area is 0.25 m 2 / g or less than 7m 2 / g, a circularity of less than 0.88, or a solidity of less than 90%, the cellulose particles provided are excellent in extensibility, adsorption property, and sustained release of ingredients. <11> According to the invention, the volume average particle size is less than 2 μm or exceeds 20 μm, the A value represented by the formula (1) exceeds 0.1, and the BET specific surface area is 0.5 m 2 / g or less than 5m 2 / g, a circularity of less than 0.9, or a solidity of less than 95%, the cellulose particles provided are excellent in extensibility, adsorption property, and sustained release of ingredients. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described as an example. The description and examples are merely illustrative of the embodiment, and are not intended to limit the scope of the present invention. In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples.
[0010] Each component may contain multiple types of the corresponding substance. When referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the amount refers to the total amount of those multiple substances present in the composition, unless otherwise specified.
[0011] <Cellulose particles> The cellulose particles in this embodiment are solid cellulose particles whose main component is cellulose, have a volume average particle size D of 1 μm or more and 30 μm or less, a circularity of 0.86 or more, and an A value represented by the formula (1) described below of less than 0.15.
[0012] The cellulose particles according to the present embodiment have excellent extensibility, adsorptivity, and sustained release of ingredients due to the above-mentioned configuration. The reasons for this are presumed to be as follows.
[0013] Cellulose particles are expected to be a substitute for resin particles in various fields, including cosmetics, due to their high biodegradability and durability. In addition, various functions are required for cellulose particles as the products for each application become more highly functional.
[0014] The functions include extensibility and adsorption. If the cellulose particles have high extensibility, for example, when the cellulose particles are used in cosmetics, the cosmetics themselves spread well and have a smooth feel on the skin. Also, if the adsorption is high, cosmetics with excellent adsorption of ingredients (e.g., sebum, sweat, and active ingredients of cosmetics) can be obtained. As cellulose particles that provide good skin feel and adsorption, for example, porous spherical cellulose particles are known (Patent Document 1). However, while porous cellulose particles are excellent at adsorbing ingredients (e.g., sebum, sweat, active ingredients in cosmetics, etc.), they have low sustained release of the ingredients because the ingredients are taken into the inside of the particles. Similarly, cellulose particles containing many voids also have low sustained release of the ingredients. When the sustained release of the ingredients is low, the moist feeling decreases when the cellulose particles are used in cosmetics.
[0015] In contrast, the cellulose particles according to the present embodiment are solid, with a volume average particle size D of 1 μm or more and 30 μm or less, a circularity of 0.86 or more, and an A value of less than 0.15 as shown in formula (1). The cellulose particles having this property have a solid structure, which makes it difficult for components to be incorporated into the interior. In addition, the A value as shown in formula (1) is an index indicating the size of the uneven structure on the particle surface, and the smaller the A value, the larger the uneven structure on the particle surface. Therefore, by lowering the A value, the particle surface has a large uneven structure, which makes it easier to accumulate components in the recesses. This improves both the adsorption property and the sustained release property. In addition, by providing the particle surface with an uneven structure, the contact area between the particles is small, making the particles easier to disentangle, and thus improving the extensibility. Furthermore, by setting the volume average particle size within the above range, the surface area of the particles is increased, which further improves both the adsorptivity and the sustained release properties, and the cellulose particles become easier to roll, which further improves the extensibility.
[0016] From the above, it is presumed that the cellulose particles according to this embodiment have excellent extensibility, adsorptive properties, and sustained release properties of ingredients due to the above-mentioned configuration.
[0017] (Volume average particle size) The volume average particle size of the cellulose particles according to this embodiment is preferably 1 μm or more and 30 μm or less. When the volume average particle diameter of the cellulose particles is 1 μm or more, the cellulose particles are less likely to aggregate, the cellulose particles are easier to roll, and the extensibility is improved. When the volume average particle diameter of the cellulose particles is 30 μm or less, the surface area of the particles is large, and the adsorptivity and sustained release properties are further improved. Therefore, the volume average particle diameter of the cellulose particles is set to the above range. The volume average particle size of the cellulose particles is more preferably from 2 μm to 20 μm, and further preferably from 3 μm to 10 μm.
[0018] The volume average particle size of the cellulose particles is measured as follows. The particle size is measured using an LS particle size distribution analyzer "Beckman Coulter LS13 320 (manufactured by Beckman Coulter)" and the cumulative particle size distribution is plotted from the smallest diameter side on a volume basis. The particle size at 50% of the cumulative distribution is determined as the volume average particle size.
[0019] (A value shown in formula (1)) In the cellulose particles according to this embodiment, the A value represented by the following formula (1) is less than 0.15. Formula (1): A=1 / (D×S) (In formula (1), D is the volume average particle size of the cellulose particles (μm), S is the BET specific surface area of the cellulose particles (m 2 / g).
[0020] When the A value shown in formula (1) is high, the surface of the cellulose particles becomes smooth and the uneven structure becomes small. Therefore, the adsorptivity and sustained release of the component are reduced. Therefore, the A value shown in formula (1) is set to the above range. The value A in formula (1) is preferably 0.13 or less, and more preferably 0.1 or less. However, from the viewpoint of sustained release, specifically, from the viewpoint that sustained release becomes difficult when the particle surface has too many irregularities, the value A in formula (1) is preferably 0.05 or more.
[0021] (BET specific surface area) The BET specific surface area of the cellulose particles according to this embodiment is 0.25 m 2 / g or more 7m 2 / g or less is preferable, and 0.5m 2 / g or more 5m 2 / g or less is more preferable, and 1m 2 / g or more 4m 2 / g or less is more preferable. When the BET specific surface area of the cellulose particles is within the above range, the adsorptivity is improved while the sustained release of the component is ensured.
[0022] The BET specific surface area of the cellulose particles is measured using a specific surface area measuring device, "Macsorb HM model-1201" manufactured by Mountech Co., Ltd. Specifically, 50 mg of particles are pretreated at 30°C for 120 minutes, and then the BET specific surface area is determined by the multipoint BET method using nitrogen gas with a purity of 99.99% or higher.
[0023] (Circularity) The circularity of the cellulose particles according to this embodiment is 0.86 or more, preferably 0.88 or more, more preferably 0.89 or more, and even more preferably 0.9 or more. When the circularity of the cellulose particles is 0.86 or more (particularly 0.88 or more), the cellulose particles are close to spherical and roll easily, which improves the extensibility. The circularity of the cellulose particles is ideally 1.
[0024] The circularity of a cellulose particle is calculated by (circular equivalent perimeter) / (perimeter) [(perimeter of a circle having the same projected area as the particle image) / (perimeter of the particle projected image)]. Specifically, it is a value measured by the following method. First, the cellulose particles to be measured are sucked and collected, flattened, and a still image of the particles is captured by instantaneous strobe light emission, and the particle image is analyzed by a flow-type particle image analyzer (FPIA-3000 manufactured by Sysmex Corporation). The number of samples to be taken for calculating the circularity is 3500, and the arithmetic average is calculated.
[0025] (solidity) The solidity of the cellulose particles according to this embodiment is preferably 90% or more, more preferably 95% or more, and ideally, the solidity of the cellulose particles is 100%. When the solidity of cellulose particles is high, it becomes difficult for ingredients to be incorporated inside the particles, and therefore the sustained release of the ingredients is improved.
[0026] The solidity of cellulose particles is measured as follows. The cellulose particles are embedded in an epoxy resin and then cut with a diamond knife or the like to prepare a sample in which the surface having the cross section of the cellulose particle is the observation surface. The cross-sectional SEM images of cellulose particles taken with a scanning electron microscope (SEM) are analyzed, and the ratio of the area of the part filled with resin (i.e., cellulose) to the total area of the cross-section of the cellulose particle is calculated. The average ratio of the area of the part filled with resin (i.e., cellulose) in the cross-sections of 10 or more randomly selected cellulose particles is taken as the solidity (area %).
[0027] (cellulose) The cellulose particles according to this embodiment contain cellulose as a main component. Here, "containing cellulose as a main component" means that the content of cellulose in the cellulose particles is 90% by mass or more. However, when the cellulose particles have a coating layer and an intermediate layer described below, "containing cellulose as a main component" means that the cellulose content relative to the base particle is 90% by mass or more.
[0028] The number average molecular weight of the cellulose is preferably 37,000 or more, and more preferably 45,000 or more. The upper limit of the number average molecular weight of the cellulose is not particularly limited, but may be, for example, 100,000 or less.
[0029] By making the number-average molecular weight of cellulose 37,000 or more, it becomes easier to obtain cellulose particles with excellent extensibility, adsorptivity, and sustained release of ingredients. In addition, biodegradability is also improved. The reason for this is presumed to be as follows. By making the number-average molecular weight of cellulose 37,000 or more, the number of terminal hydroxyl groups per unit volume of the particle is reduced, and intramolecular and extramolecular hydrogen bonds are suppressed, making the cellulose particles less likely to aggregate, thereby improving the extensibility, adsorption, and sustained release of ingredients. In addition, the specific surface area is increased by suppressing the aggregation of cellulose particles, and biodegradability is improved.
[0030] The number average molecular weight of cellulose was measured by gel permeation chromatography (differential refractometer Optilab T-rEX / Wyatt Technology, multi-angle light scattering detector) The measurement is performed using a DAWN HELEOS II (Wyatt Technology) and columns (TSKgel α-M, α-3000, Tosoh) in dimethylacetamide (with 0.1M lithium chloride added) as the solvent.
[0031] (Other Ingredients) The cellulose particles according to this embodiment may contain other components. However, when the cellulose particles have a coating layer described below, the other components are contained in the base particles that are coated with the coating layer.
[0032] Examples of other components include plasticizers, flame retardants, compatibilizers, release agents, light resistance agents, weather resistance agents, colorants, pigments, modifiers, anti-drip agents, antistatic agents, hydrolysis inhibitors, fillers, reinforcing agents (glass fibers, carbon fibers, talc, clay, mica, glass flakes, milled glass, glass beads, crystalline silica, alumina, silicon nitride, aluminum nitride, boron nitride, etc.), acid acceptors for preventing release of acetic acid (oxides such as magnesium oxide and aluminum oxide; metal hydroxides such as magnesium hydroxide, calcium hydroxide, aluminum hydroxide, and hydrotalcite; calcium carbonate; talc; etc.), and reactive trapping agents (for example, epoxy compounds, acid anhydride compounds, carbodiimides, etc.). The content of the other components is preferably 0% by mass or more and 5% by mass or less based on the total amount of the cellulose particles (or base particles), where "0% by mass" means that no other components are included.
[0033] (particle structure) The cellulose particles according to the present embodiment are preferably cellulose particles having no coating layer, that is, the cellulose particles according to the present embodiment are preferably cellulose particles having a single-layer structure mainly composed of cellulose. In single-layer cellulose particles whose main component is cellulose, hydrophilic cellulose is exposed on the surface, which increases the adsorption of hydrophilic components (e.g., glycerin, hyaluronic acid, amino acids, etc.) and also improves the sustained release of hydrophilic components.
[0034] -External additives- The cellulose particles according to the present embodiment may have inorganic particles added thereto. When inorganic particles are added thereto, secondary aggregation between particles is suppressed, and the particles are more likely to exhibit their inherent properties. Therefore, the extensibility, adsorption, and sustained release of components are more likely to be improved. It is also believed that the decrease in biodegradability is suppressed.
[0035] The external additive may be at least one selected from the group consisting of silicon-containing compound particles and metal oxide particles.
[0036] The silicon-containing compound particles refer to particles that contain silicon. The silicon-containing compound particles may be particles containing only silicon, or may be particles containing silicon and other elements.
[0037] The silicon-containing compound particles are preferably silica particles. The silica particles may be crystalline or amorphous as long as they are particles that are mainly composed of silica, i.e., SiO2. The silica particles may be particles manufactured from silicon compounds such as water glass and alkoxysilane as raw materials, or may be particles obtained by crushing quartz. As the metal oxide, oxides of metals other than silicon can be used. Examples of metal oxides include zinc oxide, magnesium oxide, iron oxide, and aluminum oxide.
[0038] The volume average particle size of the external additive is preferably from 1 nm to 100 nm, more preferably from 5 nm to 30 nm, from the viewpoint of texture (specifically, feel on the skin). The volume average particle diameter of the external additive is measured in the same manner as the volume average particle diameter of the cellulose.
[0039] The amount of the external additive added is preferably 0.1% by mass or more and 2% by mass or less with respect to the total mass of the cellulose particles (cellulose particles to which no external additive has been added).
[0040] <Method of manufacturing cellulose particles> The method for producing cellulose particles according to this embodiment is, for example, as follows.
[0041] - Cellulose particle (mother particle) manufacturing process - (1) First, cellulose acylate is dissolved in a mixed solvent of water-soluble organic solvent A and water-soluble organic solvent B, and organic solvent C is added as necessary to prepare cellulose acylate solution A. Note that the addition of organic solvent C forms holes in the particles, decreasing the solidity. (2) Next, the cellulose acylate solution A is added to a calcium carbonate dispersion obtained by dispersing calcium carbonate in water, and the mixture is stirred to prepare a cellulose acylate solution B. (3) Next, the cellulose acylate solution B is added to a mixed solution of carboxymethyl cellulose and water to prepare a cellulose acylate solution C. (4) Next, the cellulose acylate dispersion C is heated to remove the water-soluble organic solvents A and B, hydrochloric acid is added, and methanol is further added to form cellulose acylate particles. The cellulose acylate particles are then filtered, and the filtered cellulose acylate particles are dispersed in water to prepare a cellulose acylate particle dispersion. (5) Next, sodium hydroxide is added to the cellulose acylate particle dispersion, and the cellulose acylate particle dispersion is heated and stirred in a weak alkaline environment to saponify the cellulose acylate particles, thereby preparing a cellulose particle suspension. (6) Next, hydrochloric acid is added to the cellulose particle suspension to adjust the pH of the suspension to near neutral (for example, in the range of 6.5 to 7), and then the cellulose particles are repeatedly filtered and washed with pure water. Then, after the electrical conductivity of the filtrate reaches 10 μs / cm or less, the filtered cellulose particles are dried.
[0042] In the above manufacturing process, the A value, BET specific surface area, solidity, etc., shown in formula (1) of the cellulose particles can be controlled by adjusting the mass ratio of water-soluble organic solvent A, water-soluble organic solvent B, and organic solvent C in the mixed solvent that dissolves the cellulose acylate. In addition, by adjusting the amount of carboxymethyl cellulose, the volume average particle size of the cellulose particles can be controlled. In addition, the circularity of the cellulose particles can be controlled by adjusting the hydrophilicity and hydrophobicity of the cellulose acylate. By controlling these factors, the cellulose particles according to the present embodiment can be obtained.
[0043] Here, cellulose acylate is a cellulose derivative in which at least one hydroxyl group in cellulose is substituted (acylated) with an aliphatic acyl group. AC (R AC represents an aliphatic hydrocarbon group. The water-soluble organic solvent A is a solvent in which 0.1% by mass to 10% by mass of water is dissolved at 25° C., and examples thereof include ethyl acetate and butyl acetate. The water-soluble organic solvent B is a solvent in which 0.1% by mass or more to 30% by mass of water is dissolved at 25° C., and examples thereof include methyl ethyl ketone and methyl formate. Examples of the organic solvent C include heptanol and octanol.
[0044] - Intermediate layer and covering layer formation process - When cellulose particles having a coating layer are produced, it is preferable to include a step of forming a coating layer (a coating layer forming step) after the above-mentioned cellulose particle (base particle) production step. Here, when the coating layer forming step is carried out, a coating layer is formed using the particles obtained in the above-mentioned cellulose particle (base particle) production step as base particles.
[0045] First, an aqueous dispersion of the base particles is prepared. Before preparing the aqueous dispersion, it is preferable to wash the base particles with an acid.
[0046] Next, the aqueous dispersion in which the base particles are dispersed is mixed with an aqueous solution containing a compound that constitutes the intermediate layer. As a result, for example, the hydroxyl groups of the resin contained in the base particles react with the amine sites, carboxyl groups, amino groups, etc. of the compound that constitutes the intermediate layer, or the hydroxyl groups form hydrogen bonds to form the intermediate layer. Then, the aqueous dispersion in which the base particles with the intermediate layer formed are dispersed is mixed with an emulsion that contains a compound that constitutes the coating layer. As a result, the coating layer is formed. Here, when no intermediate layer is formed, the coating layer is formed by mixing an aqueous dispersion in which the base particles obtained by the above-mentioned cellulose particle (base particle) manufacturing process are dispersed with an emulsion containing the compound that constitutes the coating layer.
[0047] The cellulose particles having the coating layer are then taken out from the mixture. The cellulose particles having the coating layer are taken out, for example, by filtering the mixture. The taken-out cellulose particles having the coating layer are preferably washed with water. This makes it possible to remove unreacted surface treatment polymer. The cellulose particles having the coating layer are then dried to obtain the cellulose particles according to this embodiment.
[0048] -External addition process- An external additive may be added to the obtained cellulose particles. The external addition step may be, for example, a process in which an external additive is added to cellulose particles using a mixing mill, a V-type blender, a Henschel mixer, a Loedige mixer, or the like.
[0049] <Application> Applications of the cellulose particles according to this embodiment include granular materials such as cosmetics, rolling agents, abrasives, scrubbing agents, display spacers, materials for forming beads, light diffusing particles, resin reinforcing agents, refractive index control agents, biodegradation promoters, fertilizers, water absorbing particles, toner particles, and anti-blocking particles.
[0050] The cellulose particles according to this embodiment are preferably used in cosmetics. Among these, the cellulose particles according to this embodiment are preferably used as a cosmetic additive. The cellulose particles according to this embodiment have excellent flexibility, and therefore when used as a cosmetic additive, the cosmetic spreads well and does not easily slide on the skin when applied to the skin.
[0051] The cellulose particles according to the present embodiment can be used in, for example, cosmetics for base makeup (for example, makeup base, concealer, foundation, face powder, etc.); cosmetics for makeup (for example, lipstick, gloss, lip liner, blush, eye shadow, eyeliner, mascara, etc.); The present invention can be applied as a cosmetic additive in cosmetics such as cosmetics for eyebrows, nails, nail care, etc.; cosmetics for skin care (for example, facial cleansers, cleansing lotions, lotions, beauty serums, packs, face masks, cosmetics for eye and mouth care, etc.); etc. In particular, since cosmetic additives for makeup cosmetics are required to be flexible and biodegradable, the resin particles according to this embodiment are preferably used as cosmetic additives for makeup cosmetics. EXAMPLES
[0052] Examples will be described below, but the present invention is not limited to these examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.
[0053] <Preparing each ingredient> The following materials were prepared:
[0054] (Cellulose Acylate) CA-1: Diacetyl cellulose, Daicel Corporation "L50", number average molecular weight 58,000 CA-2: Cellulose acetate propionate, Eastman Chemical "CAP482-0.5", number average molecular weight 25000
[0055] <Examples 1 to 9> - Formation of mother particles - The type and amount of cellulose acylate shown in Table 1 was dissolved in a mixed solvent of ethyl acetate and methyl ethyl ketone (MEK) mixed in the amounts shown in Table 1, or a mixed solvent of ethyl acetate, methyl ethyl ketone (MEK) and heptanol. This was added to a dispersion in which calcium carbonate in the amount shown in Table 1 was dispersed in 500 parts of pure water, and stirred for 3 hours. To this, carboxymethylcellulose (CMC) in the amount shown in Table 1 was added to a dispersion in which carboxymethylcellulose (CMC) in the amount shown in Table 1 was dispersed in 600 parts of pure water, and stirred at 80°C for 3 hours to remove ethyl acetate and methyl ethyl ketone. 10 parts of dilute hydrochloric acid was added to this to dissolve calcium carbonate. When heptanol was used at this time, methanol was added in an amount 10 times that of heptanol. The residue was filtered and dispersed again in 900 parts of pure water to obtain a mother particle slurry.
[0056] -Saponification of mother particles- 17.5 parts of 20% NaOH was added to 500 parts of the base particle slurry (solid concentration 10%) and stirred for 6 hours in an environment of 30°C. Hydrochloric acid was added to the saponified slurry to adjust the pH to 7, and then filtration and washing were repeated until the filtrate conductivity was 10 μs / cm or less, yielding cellulose particles. The obtained base particles were dried at 80°C for 3 hours to remove the solvent. As a result, a base particle cake was obtained.
[0057] <Comparative Examples 1 to 4> The following commercially available cellulose particles were used as the cellulose particles of Comparative Examples 1-4. Comparative Example 1: JNC Corporation "Cellflow C-25" Comparative Example 2: Daito Kasei Kogyo Co., Ltd. "CELLULOBEADS D-30" Comparative Example 3: Daito Kasei Kogyo Co., Ltd. "CELLULOBEADS D-10" Comparative Example 4: Daito Kasei Kogyo Co., Ltd. "CELLULOBEADS USF-X"
[0058] <Physical property evaluation> (particle properties) For the cellulose particles obtained in each example, the following particle properties were measured according to the methods described above. Volume average particle size of cellulose particles (referred to as "particle size" in the table) The A value of cellulose particles as shown in formula (1) BET specific surface area of cellulose particles Circularity of cellulose particles Solidity of cellulose particles
[0059] <Evaluation> The cellulose particles of each example were evaluated for extensibility, adsorptivity, and sustained release of ingredients as follows.
[0060] -Extensibility- Ten female panelists were asked to place 0.5 g of each sample of cellulose granules on the back of their hands, stretch them out, and rate them, with 10 being the best and 0 being the worst. The scores of the ten panelists were then averaged to evaluate the results.
[0061] -Adsorption- The oil absorption of linseed oil by the cellulose particles was measured as follows. 10 g of linseed oil and 1 g of cellulose particles were mixed and centrifuged at 10,000 rpm for 30 minutes. After removing the supernatant linseed oil, the particle weight was measured and the oil absorption rate was calculated using the following formula. Formula: Oil absorption rate = (weight increase after centrifugation ÷ particle weight before centrifugation) × 100 The adsorptivity was evaluated according to the following criteria. A:120%<oil absorption rate B:100%≦Oil absorption rate<120% C:80%≦Oil absorption rate<100% D: Oil absorption <80%
[0062] - Sustained release of ingredients (moisturizing effect) - A face powder was made by mixing 75 parts of talc, 10 parts of mica, 10 parts of cellulose particles, 3 parts of titanium dioxide, and 2 parts of sodium hyaluronate. Ten female monitors applied 0.5g of each face powder sample to the back of their hands and scored the moist feeling after one hour, with 10 being the best and 0 being the worst. The scores of the 10 monitors were then averaged to evaluate the results.
[0063] [Table 1]
[0064] From the above results, it is apparent that the cellulose particles of this Example are superior in extensibility, adsorptivity, and sustained release of ingredients compared to the cellulose particles of the Comparative Example.
[0065] The present embodiment includes the following aspects. (((1))) The main component is cellulose, The volume average particle size D is 1 μm or more and 30 μm or less, The circularity is 0.86 or more, The A value represented by the following formula (1) is less than 0.15. Solid cellulose particles. Formula (1): A=1 / (D×S) (In formula (1), D is the volume average particle size of the cellulose particles (μm), S is the BET specific surface area of the cellulose particles (m 2 / g). (((2))) The cellulose particles according to (((1))), wherein the volume average particle size is 2 μm or more and 20 μm or less. (((3))) The cellulose particles according to (((1))) or (((2))), wherein the value A represented by formula (1) is 0.1 or less. (((4))) The BET specific surface area is 0.25 m 2 / g or more 7m 2 The cellulose particles according to any one of (((1))) to (((3))), wherein the cellulose particles have a molecular weight of 1 / g or less. (((5))) The BET specific surface area is 0.5 m 2 / g or more 5m 2 / g or less (((4))). (((6))) The cellulose particles according to any one of (((1))) to (((5))), having a circularity of 0.88 or more. (((7))) The cellulose particles according to (((6))), wherein the circularity is 0.9 or more. (((8))) The cellulose particles according to any one of (((1))) to (((7))), having a solidity of 90% or more. (((9))) The cellulose particles according to (((8))), wherein the solidity is 95% or more. (((10))) The BET specific surface area is 0.25 m 2 / g or more 7m 2 / g or less The circularity is 0.88 or more, The cellulose particles according to any one of (((1))) to (((8))), having a solidity of 90% or more. (((11))) The volume average particle size is 2 μm or more and 20 μm or less, The value A represented by the formula (1) is less than 0.1, The BET specific surface area is 0.5 m 2 / g or more 5m 2 / g or less, The circularity is 0.9 or more, The cellulose particles according to any one of (((1))) to (((8))), having a solidity of 95% or more.
[0066] The advantages of the above aspect are as follows. According to the invention (((1))), there is provided cellulose particles having excellent extensibility, adsorption properties, and sustained release properties of components, compared with cellulose particles having a volume average particle size D of less than 1 μm or more than 30 μm, or a value A of 0.15 or more as shown in the following formula (1). According to the invention related to (((2))), there are provided cellulose particles which are excellent in extensibility, adsorptivity, and sustained release of ingredients, as compared with those having a volume average particle size of less than 2 μm or more than 20 μm. According to the invention (((3))), there are provided cellulose particles which are excellent in extensibility, adsorptivity, and sustained release of components, as compared with the case where the A value represented by formula (1) exceeds 0.1. According to the invention related to (((4))), the BET specific surface area is 0.25 m 2 / g or less than 7m 2 / g or more, the cellulose particles provided are superior in elongation, adsorptive properties, and sustained release of ingredients. According to the invention related to (((5))), a BET specific surface area of 0.5 m 2 / g or less than 5m 2 / g or more, the cellulose particles provided are superior in elongation, adsorptive properties, and sustained release of ingredients. According to the invention related to (((6))), there are provided cellulose particles which are excellent in extensibility, adsorptivity, and sustained release of components, as compared with cellulose particles having a circularity of less than 0.88. According to the invention related to (((7))), there are provided cellulose particles which are excellent in extensibility, adsorptivity, and sustained release of ingredients, as compared with cellulose particles having a circularity of less than 0.9. According to the invention related to (((8))), there are provided cellulose particles which are excellent in extensibility, adsorptivity, and sustained release of ingredients, as compared with cellulose particles having a solidity of less than 90%. According to the invention (((9))), there are provided cellulose particles which are excellent in extensibility, adsorptivity, and sustained release of ingredients, as compared with cellulose particles having a solidity of less than 95%. According to the invention (((10))), a BET specific surface area of 0.25 m 2 / g or less than 7m 2 / g, a circularity of less than 0.88, or a solidity of less than 90%, the cellulose particles provided are excellent in extensibility, adsorption property, and sustained release of ingredients. According to the invention of (((11))), the volume average particle size is less than 2 μm or exceeds 20 μm, the A value represented by the formula (1) exceeds 0.1, and the BET specific surface area is 0.5 m 2 / g or less than 5m 2 / g, a circularity of less than 0.9, or a solidity of less than 95%, the cellulose particles provided are excellent in extensibility, adsorption property, and sustained release of ingredients.
Claims
1. The main component is cellulose, The volume average particle diameter D is 1 μm or more and 30 μm or less, The circularity is 0.86 or more, The A value represented by the following formula (1) is less than 0.
15. Solid cellulose particles. Formula (1): A=1 / (D×S) (In formula (1), D is the volume average particle size (μm) of the cellulose particles, and S is the BET specific surface area (m 2 / g).
2. 2. The cellulose particles according to claim 1, wherein the volume average particle size is from 2 μm to 20 μm.
3. 2. The cellulose particles according to claim 1, wherein the value A in formula (1) is 0.1 or less.
4. The BET specific surface area is 0.25 m 2 / g or more 7m 2 The cellulose particles according to claim 1, wherein the molecular weight is 1 / g or less.
5. The BET specific surface area is 0.5 m 2 / g or more 5m 2 The cellulose particles according to claim 4, wherein the molecular weight is 1 / g or less.
6. 2. The cellulose granules according to claim 1, having a circularity of 0.88 or more.
7. 7. The cellulose granules according to claim 6, wherein the circularity is 0.9 or more.
8. 2. The cellulose granules according to claim 1, having a solidity of 90% or more.
9. The cellulose particles according to claim 8, wherein the solidity is 95% or more.
10. The BET specific surface area is 0.25 m 2 / g or more 7m 2 / g or less The circularity is 0.88 or more, 2. The cellulose granules according to claim 1, having a solidity of 90% or more.
11. The volume average particle size is 2 μm or more and 20 μm or less, The value A represented by the formula (1) is less than 0.1, The BET specific surface area is 0.5 m 2 / g or more 5m 2 / g or less, The circularity is 0.9 or more, 2. The cellulose granules according to claim 1, having a solidity of 95% or more.
Citation Information
Patent Citations
Control of very small pore size of cellulose material
JP1990222401A
Functional polysaccharide particle
WO2019151486A1
Functional complex polysaccharide particle