Cellulose particle

Cellulose particles with specific friction, density, and smoothness properties, optionally coated with fatty acids, address the issues of poor release and extensibility in cosmetics, offering enhanced ingredient delivery and spreadability.

JP2024142154APending Publication Date: 2024-10-10FUJIFILM BUSINESS INNOVATION CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023054186
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing cellulose particles exhibit poor sustained release properties, extensibility, and disintegration properties, particularly when used in cosmetic applications, due to high solidity, dynamic friction coefficient, or surface smoothness.

Method used

Cellulose particles with a dynamic friction coefficient of 0.42 or less, bulk density of 0.40 g/cm³, solidity of 50% or more, and surface smoothness of 80% or less, optionally with a coating layer containing fatty acids or amino acid compounds, are developed to enhance sustained release, extensibility, and disintegration properties.

Benefits of technology

The developed cellulose particles provide excellent sustained release, extensibility, and disintegration properties, improving the performance of cosmetics by ensuring ingredients are effectively released and spread smoothly on the skin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142154000001
    Figure 2024142154000001
Patent Text Reader

Abstract

To provide a cellulose particle excellent in releasability of components, extensibility, and raveling properties.SOLUTION: A cellulose particle is composed mainly of cellulose and has a dynamic friction coefficient of 0.42 or less, a bulk density of 0.40 g / cm3 or less, and a degree of solidness of 50% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to cellulose particles. [Background technology]

[0002] Patent Document 1 proposes "a powder cosmetic preparation characterized by containing spherical cellulose powder coated, impregnated or chemically bonded with one or more types selected from moisturizing polymeric substances."

[0003] Patent document 2 proposes "cellulose particles characterized by an average particle size D50 of 1 μm or more and 50 μm or less, a bulk density of 0.30 g / mL or less, a specific volume of 3.0 mL / g or more, and a linseed oil absorption of 100 mL / 100 g or more."

[0004] Patent Document 3 describes a cellulose crystalline material that "contains cellulose type I crystals, has an average particle size of less than 30 μm, and a bulk density of 0.1 to 0.45 g / cm 3 , tapping density is 0.1~0.5g / cm 3 , angle of repose 35-50°, specific surface area 0.1 or more 20m 2 / g and an internal friction angle of 35 to 42°." [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 1-313413 [Patent Document 2] JP 2019-206662 A [Patent Document 3] Patent No. 5439366 Summary of the Invention [Problem to be solved by the invention]

[0006] The object of the present invention is to provide a solid cellulose particle having a kinetic friction coefficient of more than 0.42 and a bulk density of 0.40 g / cm. 3 The object of the present invention is to provide cellulose particles which are excellent in sustained release properties of ingredients, extensibility and disintegrability, as compared with cellulose particles having a solidity of more than 50% or a solidity of less than 50%. [Means for solving the problem]

[0007] Means for solving the above problems include the following aspects. <1> The main component is cellulose, Dynamic friction coefficient is 0.42 or less, and bulk density is 0.40g / cm 3 Cellulose particles having a solidity of 50% or more and a particle size of 100% or less. <2> The dynamic friction coefficient is 0.39 or less. <1> The cellulose particles according to claim 1. <3> The bulk density is 0.36 g / cm 3 is less than or equal to <2> The cellulose particles according to claim 1. <4> Surface smoothness is 80% or less <1> ~ <3> The cellulose particles according to any one of claims 1 to 5. <5> The surface smoothness is 70% or less. <4> The cellulose particles according to claim 1. <6> Solidity is 80% or more <1> ~ <5> The cellulose particles according to any one of claims 1 to 5. <7> The solidity is 90% or more. <6> The cellulose particles according to claim 1. <8> Surface smoothness is 80% or less and solidity is 80% or more <1> ~ <7> The cellulose particles according to any one of claims 1 to 5. <9> The bulk density is 0.36 g / cm 3 and the surface smoothness is 70% or less. <8> The cellulose particles according to claim 1. <10> The volume average particle size is 1 μm or more and 20 μm or less. <1> ~ <9> The cellulose particles according to any one of claims 1 to 5, <11> The base particles mainly composed of cellulose; a coating layer that coats the base particles; have <1> ~ <10> The cellulose particles according to any one of claims 1 to 5. <12 The coating layer contains at least one coating material selected from the group consisting of fatty acids, fatty acid metal salts, and amino acid compounds. <11> The cellulose particles according to claim 1. Effect of the Invention

[0008] <1> According to the present invention, in a solid cellulose particle mainly composed of cellulose, the dynamic friction coefficient exceeds 0.42 and the bulk density is 0.40 g / cm 3 The present invention provides cellulose particles having excellent sustained release properties, extensibility, and disintegrability as compared to cellulose particles having a solidity of more than 50% or less than 50%. <2> According to the present invention, there are provided cellulose particles which are excellent in sustained release properties of ingredients, extensibility and disintegration properties, as compared with those having a dynamic friction coefficient of more than 0.39. <3> According to the invention, the bulk density is 0.36 g / cm 3 The cellulose particles provided are excellent in sustained release properties of ingredients, extensibility, and disintegration, as compared with the case where the content exceeds 100%. <4> According to the present invention, there are provided cellulose particles which are excellent in sustained release properties of ingredients, extensibility and disintegrability, as compared with those having a surface smoothness of more than 80%. <5> According to the present invention, there are provided cellulose particles which are excellent in sustained release properties of ingredients, extensibility and disintegrability, as compared with those having a surface smoothness of more than 70%. <6> According to the present invention, there are provided cellulose particles which are excellent in sustained release properties of ingredients, extensibility and disintegrability, as compared with cellulose particles having a solidity of less than 80%. <7> According to the present invention, there are provided cellulose particles which are excellent in sustained release properties of ingredients, extensibility and disintegrability, as compared with cellulose particles having a solidity of less than 90%. <8> According to the present invention, there are provided cellulose particles which are excellent in sustained release properties of ingredients, extensibility and disintegrability, as compared with cellulose particles having a surface smoothness of more than 80% and a solidity of less than 80%. <9> According to the invention, the bulk density is 0.36 g / cm 3 The cellulose particles provided are excellent in sustained release properties of ingredients, extensibility, and disintegration, as compared with cellulose particles having a surface smoothness of more than 70% and a surface smoothness of more than 70%. <10> According to the present invention, there are provided cellulose particles which are excellent in sustained release properties of ingredients, extensibility and disintegrability, as compared with cellulose particles having a volume average particle diameter of less than 1 μm or more than 20 μm. <11> According to the present invention, there are provided cellulose particles which are excellent in sustained release of ingredients, extensibility and disintegration, as compared with particles not having a coating layer that coats base particles mainly composed of cellulose. <12> According to the present invention, there are provided cellulose particles which are excellent in sustained release properties of components, extensibility and disintegration properties, as compared with the case where the coating layer contains a silicone compound. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described as an example. The description and examples are merely illustrative of the embodiment, and are not intended to limit the scope of the present invention. In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples.

[0010] Each component may contain multiple types of the corresponding substance. When referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the amount refers to the total amount of those multiple substances present in the composition, unless otherwise specified.

[0011] <Cellulose particles> The cellulose particles according to the present embodiment are mainly composed of cellulose, have a dynamic friction coefficient of 0.42 or less, and a bulk density of 0.40 g / cm 3 or less, and the solidity is 50% or more.

[0012] The cellulose particles according to the present embodiment, due to the above-mentioned constitution, are excellent in sustained release properties of ingredients, extensibility, and disintegration. The reasons for this are presumed to be as follows.

[0013] Cellulose particles are expected to be a substitute for resin particles in various fields, including cosmetics, due to their high biodegradability and durability. In addition, various functions are required for cellulose particles as the products for each application become more highly functional.

[0014] The functions include extensibility and disentanglement. When the cellulose particles have high extensibility and disentanglement, for example, when the cellulose particles are used in cosmetics, the cosmetics themselves spread well and provide a smooth, soft, and light feel on the skin. As cellulose particles that provide a good feel on the skin, for example, porous spherical cellulose particles are known (Prior Document 1, etc.). However, while porous cellulose particles have excellent adsorption properties for ingredients (e.g., sebum, sweat, and active ingredients in cosmetics), they have low sustained release properties for the ingredients because the ingredients are taken into the inside of the particles. Similarly, cellulose particles containing many voids also have low sustained release properties for the ingredients. When the sustained release properties of the ingredients are low, the moist feeling decreases when the cellulose particles are used in cosmetics.

[0015] In contrast, the cellulose particles according to the present embodiment are solid with a solidity of 50% or more, a dynamic friction coefficient of 0.42 or less, and a bulk density of 0.40 g / cm 3 The cellulose particles with this property have a solid structure, which makes it difficult to incorporate ingredients into the inside. In addition, because the bulk density is low, the particle surface has a large uneven structure, which makes it easy to accumulate ingredients in the recesses, and has excellent sustained release properties. In addition, the uneven surface structure of the particles reduces the contact area between the particles, resulting in excellent disentanglement. In addition, the low dynamic friction coefficient also results in excellent elongation.

[0016] From the above, it is presumed that the cellulose particles according to this embodiment have excellent sustained release properties, extensibility, and disintegrability of ingredients due to the above-mentioned configuration.

[0017] (Kinematic friction coefficient) The kinetic friction coefficient of the cellulose particles according to this embodiment is 0.42 or less. If the dynamic friction coefficient of the cellulose particles is high, the extensibility is reduced, so the dynamic friction coefficient of the cellulose particles is set to the above range. The dynamic friction coefficient of the cellulose particles according to the present embodiment is preferably 0.39 or less, and more preferably 0.34 or less. However, if the dynamic friction coefficient is too low, the adhesion to the skin tends to decrease, so that the dynamic friction coefficient is preferably 0.20 or more, for example.

[0018] The coefficient of kinetic friction of cellulose particles is measured as follows. The cellulose particles to be measured were placed on the skin (BioSkin, Bealux) at 0.5 mg / cm 2 The dynamic friction coefficient of the particle-coated surface of the measurement sample is measured using a friction tester (HEIDON). The measurement conditions are as follows: a pseudo fingertip sensor (10 mm square piano wire sensor, manufactured by Kato Tech) as the contactor, a load of 25 g, a speed of 1 mm / sec, and a test distance of 20 mm.

[0019] (bulk density) The bulk density of the cellulose particles according to this embodiment is 0.40 g / cm 3 The following is the result. When the bulk density of the cellulose particles is high, the uneven structure on the particle surface is small and the particle surface is smooth, and therefore the disintegration property is reduced. Therefore, the bulk density of the cellulose particles is set in the above range. The bulk density of the cellulose particles according to this embodiment is 0.36 g / cm 3 However, if the bulk density is too low, the handling property tends to deteriorate, so that the bulk density is preferably 0.1 g / cm or less, for example. 3 It is better to do this.

[0020] The bulk density of the cellulose particles is measured as follows. The cellulose particles to be measured are sieved into the measuring cup of a bulk density measuring instrument (JIS-K-5101 for pigments) using a dispersion sieve provided with the measuring instrument. The cellulose particles are leveled off at the top of the measuring cup, and the weight of the particles packed in the cup is calculated from the change in the weight of the measuring cup before and after the particles are packed. The weight is multiplied by the volume of the measuring cup (30 cm 3 ) to calculate bulk density.

[0021] (Surface smoothness) The surface smoothness of the cellulose particles according to this embodiment is preferably 80% or less, and more preferably 70% or less. When the surface smoothness of cellulose particles is low, the particle surface has a large uneven structure, and the bulk density is reduced, which improves the disintegration property. However, since an excessively low surface smoothness tends to deteriorate powder fluidity, the surface smoothness of the cellulose particles is set to, for example, 10% or more.

[0022] The surface smoothness of the cellulose particles is measured as follows. Scanning electron microscope (SEM) images (magnification: 5,000x) of cellulose particles are observed, and the smoothness M of each cellulose particle is calculated from the following formula. The arithmetic mean value of the smoothness M of 10 or more arbitrarily selected cellulose particles is then taken as the surface smoothness. The closer the smoothness M value is to 1, the smoother the surface of the cellulose particle is. M = (1-(S3) / (S2)) x 100 In the above formula, S2 indicates the area (projected area) of the cellulose particle in the image, and S3 indicates the sum of "the area outside the contour of the circle having the same projected area as S2 and inside the contour of the cellulose particle in the image" and "the area inside the contour of the circle having the same projected area as S2 and outside the contour of the cellulose particle in the image" when the cellulose particle in the image is superimposed on a circle having the same projected area as S2. The method for superimposing the cellulose particles in the image onto a circle having the same projected area as S2 is as follows. When the cellulose particles in the image are superimposed on a circle having the same projected area as S2, the two images are superimposed so that the area of ​​overlapping region of the two images (the area inside the contour of the circle having the same projected area as S2 and the area inside the contour of the cellulose particles in the image) is maximized.

[0023] (solidity) The solidity of the cellulose particles according to this embodiment is 50% or more, preferably 80% or more, more preferably 90% or more, and even more preferably 95% or more. Ideally, the solidity of the cellulose particles is 100%. When the solidity of cellulose particles is high, it becomes difficult for ingredients to be incorporated inside the particles, and therefore the sustained release of the ingredients is improved.

[0024] The solidity of cellulose particles is measured as follows. The cellulose particles are embedded in an epoxy resin and then cut with a diamond knife or the like to prepare a sample in which the surface having the cross section of the cellulose particle is the observation surface. The cross-sectional SEM images of cellulose particles taken with a scanning electron microscope (SEM) were analyzed to calculate the ratio of the area of ​​the part filled with resin (i.e., cellulose) to the total area of ​​the cross-section of the cellulose particle. The average ratio of the area of ​​the part filled with resin (i.e., cellulose) in the cross-sections of 10 or more randomly selected cellulose particles was then taken as the solidity (area %).

[0025] (Volume average particle size) The volume average particle size of the cellulose particles according to this embodiment is preferably 1 μm or more and 20 μm or less, more preferably 2 μm or more and 15 μm or less, and even more preferably 5 μm or more and 10 μm or less. When the volume average particle diameter of the cellulose particles is 1 μm or more, the particles are less likely to aggregate, the coefficient of dynamic friction is reduced, and the extensibility is easily improved.When the volume average particle diameter of the cellulose particles is 20 μm or less, the surface area and bulk density are reduced, and the disintegrability is easily improved.

[0026] The volume average particle size of the cellulose particles is measured as follows. The particle size is measured using an LS particle size distribution analyzer "Beckman Coulter LS13 320 (manufactured by Beckman Coulter)" and the cumulative particle size distribution is plotted from the smallest diameter side on a volume basis. The particle size at 50% of the cumulative distribution is determined as the volume average particle size.

[0027] (cellulose) The cellulose particles according to this embodiment contain cellulose as a main component. Here, "containing cellulose as a main component" means that the content of cellulose in the cellulose particles is 90% by mass or more. However, when the cellulose particles have a coating layer and an intermediate layer described below, "containing cellulose as a main component" means that the cellulose content relative to the base particle is 90% by mass or more.

[0028] The number average molecular weight of the cellulose is preferably 37,000 or more, and more preferably 45,000 or more. The upper limit of the number average molecular weight of the cellulose is not particularly limited, but may be, for example, 100,000 or less.

[0029] By making the number-average molecular weight of cellulose 37,000 or more, it becomes easier to obtain cellulose particles with excellent sustained release properties, extensibility, and disintegration properties of the components. In addition, biodegradability is also improved. The reason for this is presumed to be as follows. By making the number-average molecular weight of cellulose 37,000 or more, the number of terminal hydroxyl groups per unit volume of the particle is reduced, and intramolecular and extramolecular hydrogen bonds are suppressed, making the cellulose particles less likely to aggregate, thereby improving the sustained release, extensibility, and disintegrability of the components. In addition, the aggregation of cellulose particles is suppressed, thereby increasing the specific surface area and improving biodegradability.

[0030] The number average molecular weight of cellulose was measured by gel permeation chromatography (differential refractometer Optilab T-rEX / Wyatt Technology, multi-angle light scattering detector) The measurement is performed using a DAWN HELEOS II (Wyatt Technology) and columns (TSKgel α-M, α-3000, Tosoh) in dimethylacetamide (with 0.1M lithium chloride added) as the solvent.

[0031] (Other Ingredients) The cellulose particles according to this embodiment may contain other components. However, when the cellulose particles have a coating layer described below, the other components are contained in the base particles that are coated with the coating layer.

[0032] Examples of other components include plasticizers, flame retardants, compatibilizers, release agents, light resistance agents, weather resistance agents, colorants, pigments, modifiers, anti-drip agents, antistatic agents, hydrolysis inhibitors, fillers, reinforcing agents (glass fibers, carbon fibers, talc, clay, mica, glass flakes, milled glass, glass beads, crystalline silica, alumina, silicon nitride, aluminum nitride, boron nitride, etc.), acid acceptors for preventing release of acetic acid (oxides such as magnesium oxide and aluminum oxide; metal hydroxides such as magnesium hydroxide, calcium hydroxide, aluminum hydroxide, and hydrotalcite; calcium carbonate; talc; etc.), and reactive trapping agents (for example, epoxy compounds, acid anhydride compounds, carbodiimides, etc.). The content of the other components is preferably 0% by mass or more and 5% by mass or less based on the total amount of the cellulose particles (or base particles), where "0% by mass" means that no other components are included.

[0033] (Cellulose particles having a coating layer) The cellulose particles according to this embodiment are preferably cellulose particles having base particles (hereinafter also referred to as cellulose base particles) mainly composed of cellulose, and a coating layer that coats the base particles (hereinafter also referred to as "cellulose particles having a coating layer").

[0034] By forming a coating layer on the cellulose particles according to the present embodiment, the surface properties can be easily controlled, and the dynamic friction coefficient, bulk density, surface smoothness, etc. of the cellulose particles can be easily adjusted to the above-mentioned preferred ranges, which makes it easier to further improve the sustained release properties, extensibility, and disentanglement properties of the components.

[0035] -Mother particle- The base particles are mainly composed of cellulose. The cellulose contained in the base particles is the same as the cellulose described above, and the preferred range is also the same.

[0036] -Coating layer- The coating layer preferably contains at least one coating material selected from the group consisting of fatty acids, fatty acid metal salts, and amino acid compounds. Examples of the coating material include lipid compounds, silicone compounds, fluorine compounds, and ceramide compounds.

[0037] ·fatty acid The fatty acids are linear or branched, saturated or unsaturated fatty acids. The fatty acids may also be mixtures of saturated and unsaturated fatty acids. The fatty acid is preferably a fatty acid having 16 to 22 carbon atoms (preferably 18 to 20 carbon atoms). Specific examples of linear fatty acids having 16 to 22 carbon atoms include behenic acid, arachidic acid, palmitic acid, and the like.

[0038] Fatty acid metal salts The fatty acid metal salt is a metal salt of a linear or branched, saturated or unsaturated fatty acid. The fatty acid metal salt may be a mixture of a saturated fatty acid metal salt and an unsaturated fatty acid metal salt. Examples of the metal salt of a fatty acid include metal salts of fatty acids having 16 to 22 carbon atoms (preferably 18 to 20 carbon atoms). Examples of the metal salt of a fatty acid having 16 to 22 carbon atoms include metal salts of stearic acid, metal salts of behenic acid, and metal salts of palmitic acid. The metal in the fatty acid metal salt may be a divalent metal. Examples of metals in the straight-chain fatty acid metal salts include magnesium, calcium, aluminum, barium, and zinc.

[0039] Amino acid compounds The amino acid compound refers to amino acids and amino acid derivatives. Examples of the amino acid compound include lauryl leucine, lauryl arginine, and myristyl leucine.

[0040] The coating material constituting the coating layer is not limited to the above-mentioned coating materials, and examples thereof include coating materials of lipid compounds (phospholipids, etc.), silicone compounds (dimethylsiloxane, etc.), fluorinated compounds (perfluoropolyether, etc.), and ceramide compounds (hydroxypropylbispalmitamide MEA, etc.).

[0041] From the viewpoint of improving the sustained release properties, extensibility, and disentanglement of the components, the amount of the coating layer applied to the base particle is preferably 0.1% by mass or more and 30% by mass or less, more preferably 0.5% by mass or more and 20% by mass or less, and even more preferably 1% by mass or more and 15% by mass or less. Here, the content of the coating material in the entire coating layer is preferably 90% by mass or more and 100% by mass or less, and more preferably 95% by mass or more and 100% by mass or less.

[0042] -Middle class- In the cellulose particles having a coating layer, it is preferable that an intermediate layer is provided between the base particle and the coating layer, and the intermediate layer preferably contains at least one intermediate material selected from the group consisting of a polyamine compound, a polyquaternium, a polysaccharide compound, and a polyacrylic acid.

[0043] In the cellulose particles according to the present embodiment, by providing an intermediate layer between the base particle and the coating layer, peeling of the coating layer is suppressed, and the sustained release properties, extensibility, and disintegrability of the component are easily maintained. In particular, the intermediate material enhances the adhesion between the cellulose base particle and the coating layer containing the coating material, and the sustained release properties, extensibility, and disintegrability of the component are easily maintained.

[0044] A polyamine compound is a general term for an aliphatic hydrocarbon having two or more primary amino groups. Examples of the polyamine compound include polyalkyleneimine, polyallylamine, polyvinylamine, and polylysine. From the viewpoint of improving biodegradability, the polyalkyleneimine is preferably a polyalkyleneimine having a structural unit with an alkylene group having 1 to 6 carbon atoms (preferably 1 to 4 carbon atoms, more preferably 1 to 2 carbon atoms), and more preferably polyethyleneimine. Examples of polyallylamine include homopolymers or copolymers of allylamine, allylamine amide sulfate, diallylamine, dimethylallylamine, and the like. An example of the polyvinylamine is one produced by hydrolyzing poly(N-vinylformamide) with an alkali, and a specific example thereof is "PVAM-0595B" manufactured by Mitsubishi Chemical Corporation. The polylysine may be one extracted from a natural product, one produced by a transformed microorganism, or one chemically synthesized.

[0045] Examples of polyquaterniums include polyquaternium-6, polyquaternium-7, polyquaternium-10, polyquaternium-11, polyquaternium-51, polyquaternium-61, and polyquaternium-64. The content of the polyquaternium is preferably 0.2% by mass or more and 2% by mass or less based on the total mass of the cellulose particles.

[0046] The coverage of the intermediate layer on the base particles is preferably from 0.1 to 10% by mass, more preferably from 0.25 to 3% by mass, from the viewpoint of improving sustained release of the component, spreadability, and disentanglement. The content of the intermediate material in the entire intermediate layer is preferably 90% by mass or more and 100% by mass or less, and more preferably 95% by mass or more and 100% by mass or less.

[0047] -External additives- The cellulose particles according to the present embodiment may have inorganic particles added thereto. When inorganic particles are added thereto, secondary aggregation between the particles is suppressed, and the particles are more likely to exhibit their inherent properties. Therefore, the sustained release, extensibility, and disintegrability of the components are more likely to be improved. It is also believed that the decrease in biodegradability is suppressed.

[0048] The external additive may be at least one selected from the group consisting of silicon-containing compound particles and metal oxide particles.

[0049] The silicon-containing compound particles refer to particles that contain silicon. The silicon-containing compound particles may be particles containing only silicon, or may be particles containing silicon and other elements.

[0050] The silicon-containing compound particles are preferably silica particles. The silica particles may be crystalline or amorphous as long as they are particles that are mainly composed of silica, i.e., SiO2. The silica particles may be particles manufactured from silicon compounds such as water glass and alkoxysilane as raw materials, or may be particles obtained by crushing quartz. As the metal oxide, oxides of metals other than silicon can be used. Examples of metal oxides include zinc oxide, magnesium oxide, iron oxide, and aluminum oxide.

[0051] The volume average particle size of the external additive is preferably from 1 nm to 100 nm, more preferably from 5 nm to 30 nm, from the viewpoint of texture (specifically, feel on the skin). The volume average particle diameter of the external additive is measured in the same manner as the volume average particle diameter of the cellulose.

[0052] The amount of the external additive added is preferably 0.1% by mass or more and 2% by mass or less with respect to the total mass of the cellulose particles (cellulose particles to which no external additive has been added).

[0053] <Method of manufacturing cellulose particles> The method for producing cellulose particles according to this embodiment is, for example, as follows.

[0054] - Cellulose particle (mother particle) manufacturing process - (1) First, cellulose acylate is dissolved in a mixed solvent of a water-soluble organic solvent A and a water-soluble organic solvent B to prepare a cellulose acylate solution A. (2) Next, the cellulose acylate solution A is added to a calcium carbonate dispersion obtained by dispersing calcium carbonate in water, and the mixture is stirred to prepare a cellulose acylate solution B. (3) Next, the cellulose acylate solution B is added to a mixed solution of carboxymethyl cellulose, the water-soluble organic solvent B, and water, and the mixture is stirred at high speed to prepare a cellulose acylate solution C. (4) Next, sodium hydroxide is added to the cellulose acylate solution C. The cellulose acylate dispersion C is heated to remove the water-soluble organic solvents A and B, and hydrochloric acid is added to form cellulose acylate particles. The cellulose acylate particles are then filtered, and the filtered cellulose acylate particles are dispersed in water to prepare a cellulose acylate particle dispersion. (5) Next, sodium hydroxide is added to the cellulose acylate particle dispersion, and the cellulose acylate particle dispersion is heated and stirred in a weak alkaline environment to saponify the cellulose acylate particles, thereby preparing a cellulose particle suspension. (6) Next, hydrochloric acid is added to the cellulose particle suspension to adjust the pH of the suspension to near neutral (for example, in the range of 6.5 to 7), and then the cellulose particles are repeatedly filtered and washed with pure water. Then, after the electrical conductivity of the filtrate reaches 10 μs / cm or less, the filtered cellulose particles are dried.

[0055] In the above manufacturing process, the dynamic friction coefficient, bulk density, surface smoothness, solidity, etc. of the cellulose particles can be controlled by adjusting the mass ratio of water-soluble organic solvent A to water-soluble organic solvent B in the mixed solvent that dissolves the cellulose acylate. Also, by adding heptanol to the cellulose acylate solution A, the degree of solidity can be controlled. In addition, by adjusting the amount of carboxymethyl cellulose, the volume average particle size of the cellulose particles can be controlled. By controlling these factors, the cellulose particles according to the present embodiment can be obtained.

[0056] Here, cellulose acylate is a cellulose derivative in which at least one hydroxyl group in cellulose is substituted (acylated) with an aliphatic acyl group. AC (R AC represents an aliphatic hydrocarbon group. The water-soluble organic solvent A is a solvent in which 0.1% by mass to 10% by mass of water is dissolved at 25° C., and examples thereof include ethyl acetate and butyl acetate. The water-soluble organic solvent B is a solvent in which 0.1% by mass to 10% by mass of water is dissolved at 25° C., and examples thereof include methyl ethyl ketone and acetone.

[0057] - Intermediate layer and covering layer formation process - When cellulose particles having a coating layer are produced, it is preferable to include a step of forming a coating layer (a coating layer forming step) after the above-mentioned cellulose particle (base particle) production step. Here, when the coating layer forming step is carried out, a coating layer is formed using the particles obtained in the above-mentioned cellulose particle (base particle) production step as base particles.

[0058] First, an aqueous dispersion of the base particles is prepared. Before preparing the aqueous dispersion, it is preferable to wash the base particles with an acid.

[0059] Next, the aqueous dispersion in which the base particles are dispersed is mixed with an aqueous solution containing a compound that constitutes the intermediate layer. As a result, for example, the hydroxyl groups of the resin contained in the base particles react with the amine sites, carboxyl groups, amino groups, etc. of the compound that constitutes the intermediate layer, or the hydroxyl groups form hydrogen bonds, forming an intermediate layer. Then, the aqueous dispersion in which the base particles with the intermediate layer formed are dispersed is mixed with an emulsion that contains a compound that constitutes the coating layer. As a result, the coating layer is formed. Here, when no intermediate layer is formed, the coating layer is formed by mixing an aqueous dispersion in which the base particles obtained by the above-mentioned cellulose particle (base particle) manufacturing process are dispersed with an emulsion containing the compound that constitutes the coating layer.

[0060] The cellulose particles having the coating layer are then taken out from the mixture. The cellulose particles having the coating layer are taken out, for example, by filtering the mixture. The taken-out cellulose particles having the coating layer are preferably washed with water. This makes it possible to remove unreacted surface treatment polymer. The cellulose particles having the coating layer are then dried to obtain the cellulose particles according to this embodiment.

[0061] -External addition process- An external additive may be added to the obtained cellulose particles. The external addition step may be, for example, a process in which an external additive is added to cellulose particles using a mixing mill, a V-type blender, a Henschel mixer, a Loedige mixer, or the like.

[0062] <Application> Applications of the cellulose particles according to this embodiment include granular materials such as cosmetics, rolling agents, abrasives, scrubbing agents, display spacers, materials for forming beads, light diffusing particles, resin reinforcing agents, refractive index control agents, biodegradation promoters, fertilizers, water absorbing particles, toner particles, and anti-blocking particles.

[0063] The cellulose particles according to this embodiment are preferably used in cosmetics. Among these, the cellulose particles according to this embodiment are preferably used as a cosmetic additive. The cellulose particles according to this embodiment have excellent flexibility, and therefore when used as a cosmetic additive, the cosmetic spreads well and does not easily slide on the skin when applied to the skin.

[0064] The cellulose particles according to the present embodiment can be used in, for example, cosmetics for base makeup (for example, makeup base, concealer, foundation, face powder, etc.); cosmetics for makeup (for example, lipstick, gloss, lip liner, blush, eye shadow, eyeliner, mascara, etc.); The present invention can be applied as a cosmetic additive in cosmetics such as cosmetics for eyebrows, nails, nail care, etc.; cosmetics for skin care (for example, facial cleansers, cleansing lotions, lotions, beauty serums, packs, face masks, cosmetics for eye and mouth care, etc.); etc. In particular, since cosmetic additives for makeup cosmetics are required to be flexible and biodegradable, the resin particles according to this embodiment are preferably used as cosmetic additives for makeup cosmetics. EXAMPLES

[0065] Examples will be described below, but the present invention is not limited to these examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.

[0066] <Preparing each ingredient> The following materials were prepared:

[0067] (Cellulose Acylate) CA-1: Diacetyl cellulose, Daicel Corporation "L50", number average molecular weight 58,000

[0068] (covering material) ST-1: Calcium stearate (fatty acid metal salt), NOF Corp. "Calcium stearate vegetable oil" ST-2: Behenic acid (fatty acid), NOF "NAA-222S"

[0069] (Intermediate material) AA-1: Polyethyleneimine (polyamine compound), Nippon Shokubai Co., Ltd. "PEI-1500"

[0070] <Examples 1 to 9, Comparative Example 1> - Formation of mother particles - 130 parts of cellulose acylate of the type shown in Table 1 was dissolved in a mixed solvent of ethyl acetate and methyl ethyl ketone (MEK) mixed in the amounts shown in Table 1, or in a single solvent of ethyl acetate in the amount shown in Table 1. If necessary, heptanol in the amount shown in Table 1 was added thereto and stirred. This was added to a dispersion in which 50 parts of calcium carbonate were dispersed in 500 parts of pure water, and stirred for 3 hours. This was added to a dispersion in which carboxymethylcellulose was dispersed in 600 parts of pure water, and stirred at 80°C for 3 hours to remove ethyl acetate and methyl ethyl ketone. 10 parts of dilute hydrochloric acid was added thereto to dissolve calcium carbonate. The residue was filtered and dispersed again in 900 parts of pure water to obtain a mother particle slurry.

[0071] -Saponification of mother particles- 17.5 parts of 20% NaOH was added to 500 parts of particle slurry (solid concentration 10%) and stirred for 6 hours in an environment of 30°C. Hydrochloric acid was added to the saponified slurry to adjust the pH to 7, and then filtration and washing were repeated until the filtrate conductivity was 10 μs / cm or less, yielding cellulose particles. The obtained base particles were dried at 80°C for 3 hours to remove the solvent. As a result, a base particle cake was obtained.

[0072] -Surface treatment- The washed base particle cake was reslurried with ion-exchanged water to adjust the weight to 500 g, and then an intermediate material was added in an amount corresponding to the type and coating amount shown in Table 1 and mixed for 1 hour, and then a coating material was added in an amount corresponding to the type and coating amount shown in Table 1 and stirred for 24 hours. As a result, an intermediate layer and a coating layer were formed on the base particles. Thereafter, the base particles having the intermediate layer and the coating layer formed thereon were repeatedly filtered and washed until the filtrate had a filtrate conductivity of 10 μs / cm or less. After washing, the resulting cake was dried to obtain cellulose acetate particles having an intermediate layer and a coating layer. The obtained particles were mixed in an FM mixer (FM40, manufactured by Nippon Coke and Engineering Co., Ltd.) for 2000 min while maintaining the mixer temperature at 25°C. -1 The mixture was stirred at a rotation speed of 1000 for 3 hours to tan the surface of the coating layer.

[0073] In addition, in some examples, as indicated by "-" in Table 1, cellulose particles were prepared without one or more of the formation of an intermediate layer, the formation of a coating layer, and the external addition of an external additive.

[0074] <Comparative Examples 2 to 4> The following commercially available cellulose particles were used as the cellulose particles of Comparative Examples 2-4. Comparative Example 2: Daito Kasei Kogyo Co., Ltd. "CELLULOBEADS D5 Magnesium stearate treated product" Comparative Example 3: Daito Kasei Kogyo Co., Ltd. "CELLULOBEADS USF-X" Comparative Example 4: JNC Corporation "Cellflow C25"

[0075] <Physical property evaluation> (particle properties) For the cellulose particles obtained in each example, the following particle properties were measured according to the methods described above. Dynamic friction coefficient of cellulose particles Bulk density of cellulose particles Surface smoothness of cellulose particles Solidity of cellulose particles Volume average particle size of cellulose particles (referred to as "particle size" in the table)

[0076] <Evaluation> The cellulose particles of each example were evaluated for the sustained release of the component, the extensibility, and the disintegrability as follows.

[0077] - Sustained release of ingredients (moisturizing effect) - Ten female monitors were asked to make face powder by mixing 75 parts of talc, 10 parts of mica, 10 parts of cellulose particles, 3 parts of titanium dioxide, and 2 parts of sodium hyaluronate. Ten female monitors applied 0.3g of each face powder sample to the back of their hands, and after 30 minutes, they were asked to rate the moist feeling, with 10 being the best and 0 being the worst. The scores of the 10 monitors were then averaged to evaluate the results.

[0078] -Extensibility- Ten female panelists were asked to place 0.3 g of each sample of cellulose granules on the back of their hands, stretch them out, and rate them, with 10 being the best and 0 being the worst. The scores of the ten panelists were then averaged to evaluate the results.

[0079] -Unraveling property- Ten female panelists were asked to place 0.3 g of each sample of cellulose granules on the back of their hands, spread it, and rate the degree to which the powder disintegrated, with 10 being the best and 0 being the worst. The scores of the ten panelists were then averaged to evaluate the results.

[0080] [Table 1]

[0081] From the above results, it is apparent that the cellulose particles of this Example are superior in sustained release properties of ingredients, extensibility, and disintegration properties compared to the cellulose particles of the Comparative Example.

[0082] The present embodiment includes the following aspects. (((1))) The main component is cellulose, Dynamic friction coefficient is 0.42 or less, and bulk density is 0.40g / cm 3 Cellulose particles having a solidity of 50% or more and a particle size of 100% or less. (((2))) The cellulose particles according to (((1))), wherein the dynamic friction coefficient is 0.39 or less. (((3))) The bulk density is 0.36 g / cm 3 The cellulose particles according to (((2))) below. (((4))) The cellulose particles according to any one of (((1))) to (((3))), having a surface smoothness of 80% or less. (((5))) The cellulose particles according to (((4))), wherein the surface smoothness is 70% or less. (((6))) The cellulose particles according to any one of (((1))) to (((5))) above, having a solidity of 80% or more. (((7))) The cellulose particles according to (((6))), wherein the solidity is 90% or more. (((8))) The cellulose particles according to any one of (((1))) to (((7))), having a surface smoothness of 80% or less and a solidity of 80% or more. (((9))) The bulk density is 0.36 g / cm 3 Cellulose particles as described below in (((8))), wherein the surface smoothness is 70% or less. (((10))) The cellulose particles according to any one of (((1))) to (((9))), having a volume average particle size of 1 μm or more and 20 μm or less. (((11))) The base particles mainly composed of cellulose; a coating layer that coats the base particles; The cellulose particles according to any one of (((1))) to (((10))), having (((12 The cellulose particles according to (((11))), wherein the coating layer comprises at least one coating material selected from the group consisting of fatty acids, fatty acid metal salts, and amino acid compounds.

[0083] The advantages of the above aspect are as follows. According to the invention of (((1))), a solid cellulose particle mainly composed of cellulose has a dynamic friction coefficient of more than 0.42 and a bulk density of 0.40 g / cm 3 The present invention provides cellulose particles having excellent sustained release properties, extensibility, and disintegrability as compared to cellulose particles having a solidity of more than 50% or less than 50%. According to the invention related to (((2))), there are provided cellulose particles which are excellent in sustained release properties of ingredients, extensibility and disintegration properties, as compared with those having a dynamic friction coefficient of more than 0.39. According to the invention related to (((3))), the bulk density is 0.36 g / cm 3The cellulose particles provided are excellent in sustained release properties of ingredients, extensibility, and disintegration, as compared with the case where the content exceeds 100%. According to the invention related to (((4))), there are provided cellulose particles which are excellent in sustained release properties of ingredients, extensibility and disintegrability, as compared with those having a surface smoothness of more than 80%. According to the invention (((5))), there are provided cellulose particles which are excellent in sustained release properties of ingredients, extensibility and disintegrability, as compared with those having a surface smoothness of more than 70%. According to the invention related to (((6))), there are provided cellulose particles which are excellent in sustained release properties of ingredients, extensibility and disintegrability, as compared with cellulose particles having a solidity of less than 80%. According to the invention related to (((7))), there are provided cellulose particles which are excellent in sustained release properties of ingredients, extensibility and disintegrability, as compared with cellulose particles having a solidity of less than 90%. According to the invention (((8))), there is provided a cellulose particle having excellent sustained release properties, extensibility, and disintegrability compared to a particle having a surface smoothness of more than 80% and a solidity of less than 80%. According to the invention (((9))), the bulk density is 0.36 g / cm 3 The cellulose particles provided are excellent in sustained release properties of ingredients, extensibility, and disintegration, as compared with cellulose particles having a surface smoothness of more than 70% and a surface smoothness of more than 70%. According to the invention (((10))), there is provided a cellulose particle having excellent sustained release properties, extensibility, and disintegrability of ingredients, compared with a cellulose particle having a volume average particle diameter of less than 1 μm or more than 20 μm. According to the invention (((11))), there are provided cellulose particles which are excellent in sustained release of ingredients, extensibility, and disintegration, compared to particles which do not have a coating layer covering base particles mainly composed of cellulose. According to the invention (((12))), there are provided cellulose particles which are excellent in sustained release of ingredients, extensibility and disintegration, as compared with cases in which the coating layer contains a lipid compound.

Claims

1. The main component is cellulose, Dynamic friction coefficient is 0.42 or less, and bulk density is 0.40 g / cm 3 Cellulose particles having a solidity of 50% or more.

2. 2. The cellulose particles according to claim 1, wherein the dynamic friction coefficient is 0.39 or less.

3. The bulk density is 0.36 g / cm 3 The cellulose particles according to claim 2, wherein:

4. 2. The cellulose granules according to claim 1, having a surface smoothness of 80% or less.

5. 5. The cellulose particles according to claim 4, wherein the surface smoothness is 70% or less.

6. 2. The cellulose granules according to claim 1, having a solidity of 80% or more.

7. 7. The cellulose particles according to claim 6, wherein the solidity is 90% or more.

8. 2. The cellulose granules according to claim 1, which have a surface smoothness of 80% or less and a solidity of 80% or more.

9. The bulk density is 0.36 g / cm 3 9. The cellulose granules according to claim 8, wherein the surface smoothness is 70% or less.

10. 2. The cellulose granules according to claim 1, having a volume average particle size of 1 μm or more and 20 μm or less.

11. The base particles mainly composed of cellulose; a coating layer that coats the base particles; The cellulose particles according to any one of claims 1 to 10, comprising:

12. The cellulose particles according to claim 11, wherein the coating layer comprises at least one coating material selected from the group consisting of fatty acids, fatty acid metal salts, and amino acid compounds.

Citation Information

Patent Citations

  • Method of forming sheet spring material and sheet spring material

    JP1979039366A

  • Powder cosmetic

    JP1989313413A

  • Cellulose particle, and method for producing the same

    JP2019206662A