Method for constructing joint seal
The joint seal construction method employs a thermoplastic resin with voids and electromagnetic induction heating to quickly and easily seal joints without metal components, addressing issues of peeling, denting, and magnetic interference in conventional methods.
Patent Information
- Application Number
- JP2023054373
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional joint sealing methods using reactive or wet sealants result in peeling, denting, and prolonged construction times, requiring skilled labor and potentially causing metal damage or magnetic noise due to electromagnetic induction heating.
A joint seal construction method using a thermoplastic resin-based sealing material with voids, heated by electromagnetic induction through a spacer containing an induction heating element, allowing for quick and simple joint sealing without metal components or magnetic interference.
The method enables rapid, skill-free joint sealing with a flat and aesthetically pleasing finish, avoiding metal damage and magnetic noise, while using non-metallic materials that maintain adhesion and strength.
Smart Images

Figure 2024142256000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a joint seal application method. [Background technology]
[0002] For example, conventionally, when constructing a building, joints formed between the edges of adjacent building components, such as multiple exterior wall panels and interior wall panels, are sealed with a reactive or wet sealant using a sealing gun. After application, reactive or wet sealants shrink as they cure, which can cause the sealant at the joint to peel off or become dented. Peeling of the sealant at the joint can cause problems in terms of performance, such as water leakage and reduced airtightness. Furthermore, peeling or denting not only results in a poor appearance, but can also cause dirt to adhere and mold to grow. In addition, it takes several days for the sealant to harden, and if it shrinks, additional days are required to make repairs, which is one of the reasons that construction time is lengthened. In addition, the work of sealing joints requires skill, and in order to alleviate the recent labor shortage, there is a strong demand for a dry joint sealing method that does not require skill.
[0003] In response to this demand for a dry joint seal construction method, a technology utilizing electromagnetic induction heating (hereinafter also referred to as "IH heating") has been proposed.
[0004] For example, Patent Document 1 proposes a "joint treatment method for architectural surface materials, characterized in that a plurality of architectural surface materials are arranged adjacent to each other, adjacent opposing edges of each of the architectural surface materials are separated to form joints, the joints are filled with an adhesive material that is unlikely to shrink in volume when hardened, and the adhesive material is then hardened by electromagnetic induction heating."
[0005] Furthermore, Patent Document 2 proposes "a method of applying joint sealant for concrete pavement, which comprises forming a joint sealant having the property of softening and melting when heated into a rope or rod shape for joints in concrete pavement, and placing an electromagnetic heating element such as iron wire or iron mesh as a core material inside the formed body of joint sealant, inserting the formed body of joint sealant into a joint groove, and using an electromagnetic induction device to heat the electromagnetic heating element, thereby softening and melting the formed joint sealant material and sealing the joints." [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2001-90215 A [Patent Document 2] JP 2014-141860 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the application method of Patent Document 1 may cause excess adhesive material to protrude from the joints. Also, the application method of Patent Document 2 may cause the sealing material to protrude from the joints because the sealing material is softened and melted. Furthermore, in the construction methods of Patent Documents 1 and 2, in order to achieve a flat surface, the joint seal needs to be leveled with a spatula or the like, and in order to prevent the adhesive material from spilling out, the seal is protected with masking tape, which is then peeled off after the seal has hardened. This type of work takes time, and the flattening work is difficult unless the worker is skilled, and the leveling work can actually worsen the appearance of the joint seal.
[0008] In light of this background, there is a demand for a construction method that can melt-bond the sealant to the panel while flattening the sealant portion of the joint after construction in a simpler and shorter time than conventional construction methods. On the other hand, Patent Document 1 and Patent Document 2 also have the following problems. In Patent Document 1, a sealant containing iron powder or a metal panel, and in Patent Document 2, a sealant containing iron bars, iron netting, etc., a metal or metal compound that generates heat by electromagnetic induction is present inside or in a part of the sealant or in the panel. If this metal or metal compound is in direct contact with a polymer compound made of carbon such as a thermoplastic resin, the deterioration of the polymer compound is accelerated, and the strength and adhesiveness of the sealant are likely to decrease early. There is a demand for a sealing method that does not cause this so-called metal damage. In addition, as a sealant for the walls of a room in which a measuring device or manufacturing device that applies magnetism is installed, it is desirable that the sealant does not contain components that are easily sensitive to electromagnetic waves of a specific frequency, such as iron, aluminum, ferrite, and silicon carbide, inside or in a part of the sealant.
[0009] Therefore, an object of the present disclosure is to provide a joint seal construction method that can easily and quickly mold and bond a joint sealant to realize joint sealing.Furthermore, an object of the present disclosure is to provide a joint seal construction method that can use a sealant that does not contain metals that generate heat due to electromagnetic induction and can realize joint sealing without metal damage or magnetic noise. [Means for solving the problem]
[0010] Means for solving the above problems include the following aspects. <1> A step of placing a joint sealant containing a thermoplastic resin and having a gap provided along a longitudinal direction in the joint; a step of heating and melting the joint sealant by heating the electromagnetic induction heating device with the electromagnetic induction heating device facing the joint sealant through a spacer including an electromagnetic induction heating element, thereby sealing the joint; A joint sealing construction method having the above structure. <2> The gap is made of a foam. <1> The joint sealing construction method described above. <3> The foam contains a thermoplastic resin or a thermosetting resin and has an open air structure. <2> The joint sealing construction method described above. <4> The spacer includes the electromagnetic induction heating element, a support member that supports the electromagnetic induction heating element, and a release layer that is provided on an outer surface that comes into contact with the joint sealant. <1> ~ <3> A joint seal construction method described in any one of the items. <5> The joint sealant has a reinforcing member provided along the longitudinal direction. <1> ~ <4> A joint seal construction method described in any one of the items. Effect of the Invention
[0011] According to the present disclosure, a joint sealing method can be provided that can easily and quickly mold a joint sealant while bonding adjacent members that form a joint, thereby realizing joint sealing. Furthermore, a method can be provided that can achieve sealing by electromagnetic induction even when a sealant that does not contain metals is used, thereby realizing joint sealing without metal damage. Furthermore, a method can be provided that can achieve sealing by electromagnetic induction even when a sealant that does not contain a substance that generates heat by electromagnetic induction is used, thereby realizing joint sealing without magnetic noise. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a process diagram for explaining the process of installing a joint sealant in a joint in a joint seal construction method. [Diagram 2] FIG. 2 is a process diagram for explaining the process of sealing joints in the joint seal construction method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] An example of the present disclosure will be described below.
[0014] In the present disclosure, a numerical range indicated using "~" means a range that includes the numerical values before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in the present disclosure. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples. In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments. In the present disclosure, the term "process" refers not only to an independent process, but also to a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.
[0015] The joint seal construction method disclosed herein is A process of installing a joint sealant containing a thermoplastic resin and having a gap provided along the longitudinal direction in the joint (hereinafter also referred to as an "installation process"); A process of melting the joint sealant and sealing the joint (hereinafter also referred to as a "sealing process") by heating the electromagnetic induction heating device with the electromagnetic induction heating device facing the joint sealant through a spacer including an electromagnetic induction heating element; has.
[0016] In the joint seal construction method of the present disclosure, a joint sealant containing a thermoplastic resin and having a void portion provided along the longitudinal direction is used. By using a joint sealant having a void portion, when the sealant melts, the molten thermoplastic resin flows into the void portion. Or, the void portion is compressed. This reduces the apparent volume of the joint sealant, making it difficult for the molten joint sealant to overflow from the joint. Therefore, the seal portion of the joint after construction is easily flattened.
[0017] In addition, in the joint seal construction method of the present disclosure, the electromagnetic induction heating device is placed facing the joint sealant through a spacer including an electromagnetic induction heating element, and the electromagnetic induction heating element is heated by the electromagnetic induction heating device. Then, the joint sealant is heated and melted by the heat generated by the electromagnetic induction heating element of the spacer. The resin of the joint sealant is pressed by the spacer in a melted state, and the resin of the joint sealant is cooled and solidified in a state of contact with the spacer, so that the shape of the spacer surface can be transferred to the surface of the seal portion. In this way, the surface of the seal portion can be molded into a desired shape such as a flat surface. Also, if the spacer surface is given a grained shape or a specific pattern, the pattern can be transferred to the surface of the seal portion. The heat generated by the electromagnetic induction heating device from the electromagnetic induction heating element reaches the desired temperature in a short time, and there is little waiting time. In addition, when installing, a spacer containing an electromagnetic induction heating element is interposed between the joint sealant and the electromagnetic induction heating device to heat and melt the joint sealant, making it easy to install the joint sealant regardless of the material of the adjacent components (building components, etc.).
[0018] As described above, the joint sealing construction method disclosed herein can easily and quickly mold the joint sealant while bonding adjacent components that form the joint, thereby achieving joint sealing.
[0019] In addition, as described above, the joint seal construction method of the present disclosure can also perform joint seal construction for joints between building components made of materials that do not undergo electromagnetic induction heating, such as wood, cement, ceramics (with some exceptions), etc. In addition, it is not necessary to use special joint seal materials, such as seal materials containing metal powder, etc., or seal materials containing metal wires or metal mesh, etc., as the joint seal material. From this point of view, the joint sealing method disclosed herein is a method that allows for easy joint sealing. In addition, in the construction method of the present disclosure, if a metal-free sealing material is selected, the sealing portion after construction does not contain metal components, so there is no metal damage. Also, if a sealing material that is not sensitive to electromagnetic waves of a specific frequency is selected, there is no magnetic noise.
[0020] The details of the joint seal construction method according to this embodiment will be described below.
[0021] (Installation process) In the installation step, a long joint sealant is installed in the joint. Specifically, for example, a joint sealant is installed in the joint between two panels, which are an example of adjacent components (construction components, etc.) (see Figure 1). The joint sealant is installed in the joint between the two panels in a tight contact state or with a small gap between them, rather than in an adhesive state. There are several methods for installing the joint sealant in the joints, such as sandwiching the sealant between two panels, or inserting the sealant between the two panels afterwards. Note that after the joint sealant is installed in the joint, part of the joint sealant protrudes from the flat surface of the panel. In FIG. 1, 10 denotes a joint sealant, 12 denotes a joint, and 14 denotes a panel.
[0022] -Joint sealant- The joint sealant includes a thermoplastic resin and has a gap provided along the longitudinal direction of the joint sealant. Specifically, for example, the joint sealant has a core portion consisting of a void portion arranged along the longitudinal direction of the joint sealant, a sheath portion containing a thermoplastic resin, and a reinforcing member arranged along the longitudinal direction of the joint sealant (see Figure 1). In FIG. 1, 10A denotes a core portion (void portion), 10B denotes a sheath portion, and 10C denotes a reinforcing member.
[0023] The void portion constituting the core may be made of a foam, or may be composed only of a hollow portion (i.e., composed of a through hole).
[0024] --Core (void)-- The void portion constituting the core is made of, for example, a foam. The foam contains, for example, a thermoplastic resin or a thermosetting resin. The foam is preferably a foam having a continuous ventilation structure. By applying a foam having a continuous ventilation structure, when the thermoplastic resin contained in the joint sealant melts, the molten thermoplastic resin easily flows into the pores of the foam. As a result, the seal portion of the joint after construction is easily flattened, while the molten resin of the joint sealant adheres to the panel without overflowing, resulting in a beautiful finish. In addition, it is desirable that the foam is soft and flexible so that it easily deforms when pressed with a spacer. When the foam deforms, the thermoplastic resin is forced into the inside of the joint, making it easier to flatten the joint seal portion. In addition, the pressed foam presses the sheath containing the thermoplastic resin against the panel, improving adhesion to the panel. From these viewpoints, it is even more desirable that the foam be a flexible foam having a continuous ventilation structure.
[0025] The foam having an open air structure is a foam having a closed cell ratio of 5% or less, and more preferably a closed cell ratio of 1% or less. The closed cell ratio is measured by the Remington method (based on ASTM D 1940-62T). Specifically, a mercury manometer is used to measure the sample chamber volume R1. Next, a sample with measured volume V and weight W is placed in the sample chamber and sealed. In this state, a mercury manometer is used to measure the sample chamber volume R2. The closed cell ratio (%) is calculated using the following formula. (R1-R2-W / d) / (VW / d) x 100 R1; Sample chamber volume (blank) (ml) R2: Sample chamber volume (with sample) (ml) W: sample weight (g) d; True specific gravity (g / cm 3 ) V: sample volume (apparent volume) (cm 3 )
[0026] --Sheath section-- The sheath contains a thermoplastic resin. The sheath may be made of a non-foamed thermoplastic resin or a foamed thermoplastic resin.
[0027] --Reinforcement material-- The reinforcing member is a member that reinforces the joint sealant. Specifically, for example, the reinforcing member is a member that prevents the joint sealant from stretching in the longitudinal direction. By providing the reinforcing member, the self-supporting ability of the joint sealant is improved, and installation workability is improved. The reinforcing member is a member that is provided in the joint sealant as required.
[0028] The reinforcing member is provided along the longitudinal direction of the joint sealant. Specifically, for example, the reinforcing member is provided inside the core portion and extends from one end to the other end in the longitudinal direction of the joint sealant. The reinforcing member is not limited to the core portion, but may be provided in the sheath portion or on the outer surface of the sheath portion. In other words, the reinforcing member may be provided inside and on the outer surface of the joint sealant, extending from one end to the other end in the longitudinal direction of the joint sealant.
[0029] Examples of the reinforcing member include a wire material, a sheet material, or a self-skin layer of a foam. Examples of wire materials include resin wire materials (wire materials such as polyester, polyolefin, rigid polyvinyl chloride, polyamide, polyimide, polystyrene, polyurethane, and wire materials (yarns) made by twisting fibers of these materials), metal wire materials (wire materials such as stainless steel, copper, tungsten, nickel, and various other alloys), and aggregates of these (aggregates of twisted wire materials, aggregates of bundled wire materials, aggregates of parallel wire materials, etc.). Examples of sheet materials include resin sheet materials (sheet materials such as polyester, polyolefin, rigid polyvinyl chloride, polyamide, polyimide, polystyrene, polyurethane, etc.), metal sheet materials (sheet materials such as stainless steel, copper, tungsten, nickel, and various other alloys), woven fabrics, knitted fabrics, nonwoven fabrics, cheesecloth, etc. Another example of the sheet material is an adhesive tape (double-sided tape, etc.). This is because the release paper of the adhesive tape can exert an anti-stretching function. The sheet material also includes a narrow, so-called ribbon-shaped material. The native skin layer is, for example, a coating (skin) that is formed on the surface of a foam when the foam is foamed.
[0030] The reinforcing member is preferably flexible. In other words, the reinforcing member is preferably a member that has flexibility and restorability. If the reinforcing member is flexible, the shape of the joint sealant is easily maintained when the joint sealant is deformed (bent, twisted, etc.) and then returned to its original shape. The presence of the reinforcing member contributes to increasing the mechanical strength of the entire sealant, and also contributes to maintaining the shape by suppressing elongation during deformation. Therefore, it is not only advantageous for packaging, transportation, and storage of the sealant, but also improves the ease of installation and removal during the installation process. Furthermore, it also improves the ease of removal of the sealant after the sealing process is completed. If a non-metallic reinforcing member is selected, the resulting seal will not contain any metal components, so there will be no metal damage. Also, if a reinforcing member that is not sensitive to electromagnetic waves of a specific frequency is selected, there will be no magnetic noise.
[0031] The size of the reinforcing member is, for example, 0.5 to 3 mm in diameter in the case of wire material, 0.1 to 3 mm in thickness in the case of sheet material, and 0.1 to 500 μm in thickness in the case of an own skin layer, with 0.1 to 100 μm being preferable for softness.
[0032] -Other aspects of joint sealant- The joint sealant is not limited to the above embodiment, but may be any of the following embodiments. 1) A mode in which the core is made of a non-foamed material and the sheath is made of a foamed material (i.e., the sheath is made of voids) 2) An embodiment in which both the core and the sheath are made of foam (i.e., both the core and the sheath are made of voids).
[0033] -Joint sealant materials- The thermoplastic resin and the thermosetting resin to be used in the joint sealant will be described below.
[0034] --Thermoplastic resin-- Examples of thermoplastic resins include acrylic resins, polyacetal, polycarbonate, polystyrene, polyethylene copolymers, soft polyvinyl chloride, various thermoplastic elastomers, soft ester resins, soft polyamide resins, soft polypropylene resins, ABS resins obtained by copolymerization of acrylonitrile, butadiene, and styrene, and AS resins obtained by copolymerization of acrylonitrile and styrene. Examples of the thermoplastic resin include hot melt type resins such as olefin-based, nylon-based, polyester-based, polyurethane-based, styrene-butadiene rubber-based, and styrene-isoprene-based resins.
[0035] Thermoplastic elastomers include polyethylene-based elastomers, vinyl chloride-based thermoplastic elastomers, olefin-based thermoplastic elastomers, styrene-based thermoplastic elastomers, urethane-based thermoplastic elastomers, amide-based thermoplastic elastomers, and ester-based thermoplastic elastomers. Examples of the thermoplastic elastomer include various thermoplastic elastomers such as elastomers and acrylic thermoplastic elastomers.
[0036] The polyethylene elastomer may be a copolymer of ethylene and an α-olefin.
[0037] A vinyl chloride-based thermoplastic elastomer is an elastomer having at least a polymer obtained by polymerizing vinyl chloride. Examples of vinyl chloride-based thermoplastic elastomers include a blended elastomer obtained by mixing polyvinyl chloride and nitrile rubber (NBR), and a blended elastomer obtained by partially crosslinking polyvinyl chloride or nitrile rubber.
[0038] The olefin-based thermoplastic elastomer is an elastomer having at least a polymer obtained by polymerizing an olefin, and examples of such elastomers include a blend type elastomer of an olefin-based rubber and a polyolefin resin, a partially crosslinked blend type elastomer obtained by partially crosslinking an olefin-based rubber and a polyolefin resin, and a completely crosslinked blend type elastomer of an ethylene propylene diene rubber (EPDM) and a polypropylene.
[0039] The styrene-based thermoplastic elastomer is an elastomer having at least a polymer obtained by polymerizing styrene. Examples of the elastomer include an elastomer having a polystyrene-isoprene-polystyrene (SIS) block structure, an elastomer having a polystyrene-poly(ethylene-butylene)-polystyrene (SEBS) block structure, an elastomer having a polystyrene-polybutadiene-polystyrene (SBS) block structure, and an elastomer having a polystyrene-poly(ethylene-propylene)-polystyrene (SEPS) block structure.
[0040] The urethane-based thermoplastic elastomer is an elastomer having at least a polymer having a urethane structure, and examples thereof include elastomers having a block structure of polyester and polyurethane, and elastomers having a block structure of polyether and polyurethane.
[0041] An example of the acrylic thermoplastic elastomer is a block copolymer of polymethyl methacrylate and an acrylic ester.
[0042] When the thermoplastic resin is a crystalline resin, from the viewpoint of easy application of the joint sealant, the melting point of the thermoplastic resin is preferably 65°C to 270°C, more preferably 80°C to 230°C, and even more preferably 160°C to 200°C. When the thermoplastic resin is a non-crystalline resin, the glass transition point of the thermoplastic resin is preferably from -35 to 200°C, and more preferably from 70 to 160°C, from the viewpoint of easy application of the joint sealant. The melting point and the glass transition point are measured by using a differential scanning calorimeter.
[0043] The thermoplastic resin foam may be one obtained by foaming a thermoplastic resin by a known method.
[0044] The thermoplastic resins may be used alone or in combination of two or more kinds.
[0045] --Thermosetting resin-- Examples of the thermosetting resin include phenol resin, epoxy resin, melamine resin, urea resin, unsaturated polyester, diallyl phthalate resin, polyurethane resin, silicone resin, etc. From the viewpoint of more easily improving the flatness, the thermosetting resin is preferably soft. As the thermosetting resin foam, a thermosetting resin foamed by a known method can be used. The thermosetting resin may be used alone or in combination of two or more kinds.
[0046] --Additives-- The joint sealant may contain additives other than the resin. The additives may include well-known additives such as flame retardants, antioxidants, colorants (pigments, etc.), ultraviolet absorbers, and inorganic fillers such as calcium carbonate. The additives may be used alone or in combination of two or more kinds.
[0047] (Sealing process) In the sealing process, an electromagnetic induction heating device is placed facing the joint sealant via a spacer, and the electromagnetic induction heating device heats an electromagnetic induction heating element, melting and pressurizing the joint sealant to form and adhere it, thereby sealing the joint (see Figure 2). After the sealing process, the top of the sealant is molded against the flat surface of the panel, and the panel and both lateral parts of the sealant at the joint are in an adhesive state. In FIG. 2, 10 denotes a joint sealant, 10A denotes a core (gap), 10B denotes a sheath, 10C denotes a reinforcing member, 12 denotes a joint, 14 denotes a panel, 16 denotes a spacer, and 18 denotes an electromagnetic induction heating device.
[0048] In the sealing process, for example, a spacer is placed between the joint sealant inserted into the joint, and both the spacer and the electromagnetic induction heating device are moved in the longitudinal direction of the joint sealant, while the joint sealant in the spacer is melted and pressurized to seal the joint.
[0049] In the sealing process, for example, a spacer may be placed on the joint sealant in the area to be melted in advance, and the electromagnetic induction heating device may be moved alone in the longitudinal direction of the joint sealant to melt and pressurize the spacer's joint sealant to seal the joint.
[0050] In the sealing process, for example, the spacer is brought into contact with the joint sealant to seal the joint. This makes the sealed portion of the joint flat after construction. If the surface of the spacer (i.e., the surface that comes into contact with the joint sealant) is embossed or has a specific pattern, the joint is sealed by the seal portion having a surface to which the pattern is transferred.
[0051] -Electromagnetic induction heating device- The electromagnetic induction heating device may be a well-known device that includes an electromagnetic induction coil wound around the outer periphery of a cylindrical insulating member made of a non-magnetic material. From the viewpoint of workability, it is preferable that the electromagnetic induction heating device is small and lightweight.
[0052] -Spacer- The spacer is composed of a member having an electromagnetic induction heating element. Specifically, for example, the spacer includes an electromagnetic induction heating element, a support member that supports the electromagnetic induction heating element, and a release layer provided on the outer surface that comes into contact with the joint sealant (see FIG. 2). In FIG. 2, 16 denotes a spacer, 16A denotes an electromagnetic induction heating element, 16B denotes a supporting member, and 16C denotes a release layer.
[0053] By providing the spacer with a release layer, the molten joint sealant is prevented from adhering to the outer surface of the spacer. However, when the electromagnetic induction heating element itself has releasability, such as when the electromagnetic induction heating element contains metal powder in a heat-resistant resin having releasability, there is no need to provide a release layer.
[0054] --Electromagnetic induction heating element-- The electromagnetic induction heating element may be a member that generates heat by being heated by electromagnetic induction. Examples of metal members include nickel, iron, steel (e.g., carbon steel), magnetic stainless steel, aluminum, copper, silver, zinc, cobalt-nickel alloy, iron-nickel alloy, etc. Examples of non-metal members include ferrite, zinc oxide, carbon, silicon carbide, etc. As the electromagnetic induction heating element, carbon steel, magnetic stainless steel, aluminum, silicon carbide, etc., which have high heat generation during electromagnetic induction and high heat dissipation thereafter, are particularly preferred. The electromagnetic induction heating element may also have a hollow structure or a structure made of a composite material. Furthermore, the electromagnetic induction heating element may contain a cooling structure to improve heat dissipation performance.
[0055] The shape of the electromagnetic induction heating element may be, for example, any of a wire shape (metal wire, etc.), a coil shape (metal coil, etc.), a pipe shape (metal pipe, etc.), a mesh shape (metal mesh, etc.), a plate shape (metal plate, etc.), and a powder shape (metal powder, etc.).
[0056] The electromagnetic induction heating element may be made of a heat-resistant resin material in which powder (metal powder, etc.) is dispersed. The electromagnetic induction heating element may be disposed independently of the support, or may be disposed embedded in the support member.
[0057] --Supporting member-- The support member is made of, for example, a heat-resistant resin, ceramics, or the like. Examples of heat-resistant resins include polyimide resins, polyamide resins, polyamideimide resins, polyether ether ester resins, polyphenylene sulfide resins, polyarylate resins, polyether ether ketone resins, and polybenzimidazole polyester resins. Examples of ceramics include aluminum nitride, silicon nitride, alumina, sapphire, and cermet. Ferrite, zinc oxide, carbon, and silicon carbide generate heat through electromagnetic induction, and are therefore not suitable as support members that come into contact with electromagnetic induction devices. Suitable support members for use in the present application include aluminum nitride, silicon carbide, and alumina, which have high heat resistance and high heat dissipation properties. The support member may also be hollow or made of a composite material. The support member may also include a cooling structure to enhance heat dissipation performance.
[0058] --Release layer-- The release layer is made of, for example, a heat-resistant release material. Examples of the release material include polyethylene terephthalate resin, PEEK (polyether ether ketone) resin, PPS (polyphenylene sulfide) resin, PEI (polyetherimide) resin, PPSU (polyphenylsulfone) resin, silicone resin, and fluororesin (particularly, PVDF polyvinylidene fluoride). Examples of the release agent include ceramics (alumina) and graphite carbon. The release agent for use in the present invention is preferably a material having high heat resistance and high heat dissipation properties. In addition, since the heat of the electromagnetic induction heating element is transferred to the thermoplastic resin via the release material, it is preferable that the release material be thin. The thickness of the release material is preferably 0.05 mm to 20 mm, and more preferably 0.05 mm to 1 mm.
[0059] The surface of the release layer may be a mirror surface, or may have a textured or specific pattern to improve the appearance of the joint sealant. As a result, the surface properties of the release layer are transferred to the sealed portion of the joint after application, improving the design, such as a matte finish.
[0060] In the joint seal construction method of the present disclosure described above, the joint sealant installed in the joint is melted and pressurized by the above-mentioned installation process and sealing process, and then cooled, thereby sealing the joint at the seal portion. In other words, the resin of the sealant is melted and pressurized between adjacent members (such as building members), bonding the panels together and flattening them in a position parallel to the member surfaces. [Explanation of symbols]
[0061] 10 Joint sealant 10A Core (void) 10B Scabbard part 10C Reinforcement members 12 Joint 14 Panel 16 Spacer 16A Electromagnetic Induction Heater 16B Support member 16C Release layer 18 Electromagnetic induction heating device
Claims
1. A step of placing a joint sealant containing a thermoplastic resin and having a gap provided along a longitudinal direction in the joint; a step of heating and melting the joint sealant by heating the electromagnetic induction heating device with the electromagnetic induction heating device facing the joint sealant through a spacer including an electromagnetic induction heating element, thereby sealing the joint; A joint sealing construction method having the above structure.
2. The joint seal construction method according to claim 1 , wherein the gap is made of a foam.
3. The joint seal construction method according to claim 2, wherein the foam contains a thermoplastic resin or a thermosetting resin and has a continuous air permeable structure.
4. The joint seal construction method according to claim 1 , wherein the spacer comprises the electromagnetic induction heating element, a support member supporting the electromagnetic induction heating element, and a release layer provided on an outer surface that comes into contact with the joint sealant.
5. The joint seal construction method according to claim 1 , wherein the joint seal material has a reinforcing member provided along the longitudinal direction.
Citation Information
Patent Citations
Water proofing method of prefabricated building
JP1978072312A
Deformation of lumpy body
JP1986165404A
Method of forming resin joint
JP1989052952A
Joint structure and method for sealing joint
JP1995076889A
Joint filler and cut-off structure
JP1997203129A