Zirconia sol and zirconia sol production method
A zirconia sol with controlled particle size and shape, produced through specific concentration and droplet volume adjustments, enhances abrasive performance for precision polishing by improving polishing rates and reducing surface roughness.
Patent Information
- Application Number
- JP2023054629
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-30
AI Technical Summary
Existing zirconia sols are not suitable as abrasive grains due to inadequate particle size and shape, which affects their performance in precision polishing applications.
A zirconia sol with particle sizes between 50 nm and 250 nm, containing a proportion of at least 40% angular and distorted particles, is produced by controlling the concentration of zirconium oxychloride and ammonia water during neutralization, with specific droplet volumes and concentrations to manage nucleation and grain growth.
The resulting zirconia sol exhibits higher polishing rates and lower surface roughness, making it more effective for precision polishing of semiconductors and other materials.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a zirconia sol and a method for producing a zirconia sol. [Background technology]
[0002] Zirconia sol is used as a raw material powder for fine ceramics, precision abrasives, cosmetics, paint fillers, zirconia thin films, and the like (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 02-137732 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a zirconia sol which is more suitable as an abrasive grain for polishing, and to provide a method for producing the zirconia sol. [Means for solving the problem]
[0005] The present invention provides the following: [1] Particle size D 50 is within the range of 50 nm or more and 250 nm or less, A zirconia sol obtained by the following procedure, characterized in that the proportion X is 40% or more. <Procedure> Obtain a transmission electron microscope image containing 20 or more isolated particles. The following operations 1) to 5) are carried out for each isolated particle in the transmission electron microscope image. 1) Find the circumscribing circle and the inscribing circle that has the same center as the circumscribing circle. 2) Calculate the ratio of the diameter of the circumscribing circle to the diameter of the inscribing circle [(diameter of the circumscribing circle) / (diameter of the inscribing circle)]. 3) For all isolated particles in the transmission electron microscope image, the ratio [(circumscribed circle diameter) / (inscribed circle diameter)] is calculated. 4) Count the number of isolated particles A whose ratio [(circumscribed circle diameter) / (inscribed circle diameter)] is 2.0 or more. 5) The ratio X of the isolated particles A to all the isolated particles is calculated. (Proportion X(%)) = [(Number of isolated particles A) / (Total number of isolated particles)] × 100
[0006] Particles with the ratio [(circumscribed circle diameter) / (inscribed circle diameter)] of 2.0 or more are said to be angular, distorted particles. According to the configuration of [1], the proportion X is 40% or more, and a certain number or more of angular, distorted particles are included. Zirconia sols containing such particles are useful as polishing abrasives. In particular, according to the configuration of [1] above, the particle diameter D 50 In other words, according to the configuration of [1], the particle diameter D 50 The particle size is in the range of 50 nm to 250 nm, and a certain number of particles with angular or irregular shapes are included. 50 Zirconia sol containing irregularly shaped particles with a particle size of 50 nm or more and 250 nm or less is expected to have a higher rate and higher smoothness (low surface roughness) than existing products, particularly in precision polishing of semiconductors and the like.
[0007] Furthermore, the present invention provides the following: [2] The zirconia sol according to [1], wherein the proportion X is 50% or more.
[0008] When the proportion X is 50% or more, the abrasive grains are more useful as polishing grains.
[0009] Furthermore, the present invention provides the following: [3] The particle diameter D 50 The zirconia sol according to the above [1] or [2], wherein the average particle size is 200 nm or less.
[0010] The particle diameter D 50When the particle size is 200 nm or less, the particle size is more useful as a polishing abrasive grain.
[0011] Furthermore, the present invention provides the following: [4] Step A: Neutralizing the aqueous zirconium oxychloride solution by dropwise addition of aqueous ammonia Including, The concentration of the zirconium oxychloride aqueous solution is 10% by mass or more (ZrO2 equivalent value, the same applies below), The concentration of the ammonia water is 10% by mass or more, The method for producing a zirconia sol according to any one of the above [1] to [3], wherein the volume of the droplets of ammonia water dropped in the step A is 1.0 ml or less.
[0012] According to the above-mentioned [4], first, ammonia water is used as a neutralizing agent. Since ammonia water is used as a neutralizing agent, the zirconia sol of the above-mentioned [1], that is, the zirconia sol having the ratio X of 40% or more, can be obtained. Although the reason is unclear, the inventors speculate that since ammonia water is a weak alkali compared to a strong alkali such as a sodium hydroxide aqueous solution, the generation of nuclei that become particles is slow, and the particle size becomes larger and the shape becomes distorted compared to the case where a strong alkali is used. According to the configuration of [4], in the neutralization step A, ammonia water having a specific concentration range is added dropwise to a zirconium oxychloride aqueous solution having a specific concentration range, the volume of the droplets being controlled to a specific range. Specifically, ammonia water having a concentration of 10% by mass or more is added dropwise to a zirconium oxychloride aqueous solution having a concentration of 10% by mass or more. The volume of the droplets of ammonia water added dropwise is 1.0 ml or less. This makes it possible to obtain the zirconia sol of [1], that is, the zirconia sol having the ratio X of 40% or more. Although the reason is unclear, the process in which the zirconium oxychloride aqueous solution reacts with ammonia water to produce zirconium hydroxide is thought to be as follows (1) and (2). (1) The reaction of zirconium oxychloride with ammonia produces a zirconium hydroxide nucleus (presumably a cluster with the chemical formula {Zr(OH)4}n), (2) The aggregation of zirconium hydroxide nuclei and the grain growth of the zirconium hydroxide nuclei proceed simultaneously. In this regard, the inventors presume that the concentration of the initial zirconium oxychloride aqueous solution, the concentration of ammonia water, and the volume of the droplets when the ammonia water is added dropwise are determining factors for the nucleation rate and the density of the nuclei, and as a result, they become factors for controlling the balance between the aggregation of the nuclei and the grain growth of the nuclei in the above (2).The particle characteristics (particle size, shape, etc.) of the finally obtained zirconia sol are considered to be determined by the particle characteristics (particle size, shape, etc.) of the zirconium hydroxide produced in step A. Thus, according to the configuration of [4], ammonia water is used as a neutralizing agent, the concentration of the zirconium oxychloride aqueous solution is set to 10% by mass or more, the ammonia water is added dropwise to the zirconium oxychloride aqueous solution, and the size of the ammonia water droplets during the dropwise addition is controlled to 1.0 ml or less, and the zirconium hydroxide obtained is used as a raw material, thereby obtaining many particles with a large particle size and a distorted shape. That is, a zirconia sol having the proportion X of 40% or more can be obtained. On the other hand, if the concentration of the zirconium oxychloride aqueous solution is less than 10 mass%, if the concentration of the ammonia water is less than 10 mass%, or if the volume of the droplets of the ammonia water when dropped exceeds 1.0 ml, the balance of (2) above becomes inappropriate, making it difficult to obtain the zirconia sol of [1] above. Effect of the Invention
[0013] According to the present invention, it is possible to provide a zirconia sol that is more suitable as an abrasive grain for polishing, and also to provide a method for producing the zirconia sol. [Brief description of the drawings]
[0014] [Figure 1]FIG. 2 is a diagram for explaining the circumscribing circle and the inscribing circle of an isolated particle in a transmission electron microscope image. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, embodiments of the present invention will be described. However, the present invention is not limited to these embodiments. In this specification, zirconia (zirconium oxide) is a general term, and contains 10 mass % or less of impurity metal compounds including hafnia. In addition, in this specification, the expressions "contain" and "include" include the concepts of "contain", "include", "substantially consists of" and "consist only of".
[0016] [Zirconia sol] An example of the zirconia sol according to the present embodiment will be described below, however, the zirconia sol of the present invention is not limited to the following example.
[0017] The zirconia sol according to this embodiment is Particle size D 50 is within the range of 50 nm or more and 250 nm or less, The proportion X obtained by the following procedure is 40% or more. <Procedure> Obtain a transmission electron microscope image containing 20 or more isolated particles. The following operations 1) to 5) are carried out for each isolated particle in the transmission electron microscope image. 1) Find the circumscribing circle and the inscribing circle that has the same center as the circumscribing circle. 2) Calculate the ratio of the diameter of the circumscribing circle to the diameter of the inscribing circle [(diameter of the circumscribing circle) / (diameter of the inscribing circle)]. 3) For all isolated particles in the transmission electron microscope image, the ratio [(circumscribed circle diameter) / (inscribed circle diameter)] is calculated. 4) Count the number of isolated particles A whose ratio [(circumscribed circle diameter) / (inscribed circle diameter)] is 2.0 or more. 5) The ratio X of the isolated particles A to all the isolated particles is calculated. (Proportion X(%)) = [(Number of isolated particles A) / (Total number of isolated particles)] × 100
[0018] As described above, the zirconia sol has a particle diameter D 50 is within the range of 50 nm or more and 250 nm or less. The particle diameter D 50 is preferably 200 nm or less, more preferably 180 nm or less, and further preferably 150 nm or less. The particle diameter D 50 is preferably 55 nm or more, more preferably 60 nm or more, and further preferably 65 nm or more. The particle diameter D 50 is preferably 55 nm or more and 200 nm or less, more preferably 60 nm or more and 180 nm or less, and further preferably 65 nm or more and 150 nm or less. The particle diameter D 50 The measurement method is more specifically the method described in the Examples.
[0019] The zirconia sol has a ratio X of 40% or more obtained by the following procedure. <Procedure> Obtain a transmission electron microscope image containing 20 or more isolated particles. The following operations 1) to 5) are carried out for each isolated particle in the transmission electron microscope image. 1) Find the circumscribing circle and the inscribing circle that has the same center as the circumscribing circle. 2) Calculate the ratio of the diameter of the circumscribing circle to the diameter of the inscribing circle [(diameter of the circumscribing circle) / (diameter of the inscribing circle)]. 3) For all isolated particles in the transmission electron microscope image, the ratio [(circumscribed circle diameter) / (inscribed circle diameter)] is calculated. 4) Count the number of isolated particles A whose ratio [(circumscribed circle diameter) / (inscribed circle diameter)] is 2.0 or more. 5) The ratio X of the isolated particles A to all the isolated particles is calculated. (Proportion X(%)) = [(Number of isolated particles A) / (Total number of isolated particles)] × 100
[0020] The proportion X is preferably 50% or more, more preferably 55% or more, and further preferably 60% or more. The larger the ratio X, the more preferable it is, for example, 99% or less, 90% or less. The proportion X is preferably 50% or more and 99% or less, more preferably 55% or more and 90% or less, and further preferably 60% or more and 85% or less. More specifically, the ratio X is a value obtained by the method described in the Examples.
[0021] Particles with the ratio [(circumscribed circle diameter) / (inscribed circle diameter)] of 2.0 or more are said to be angular, distorted particles. According to the zirconia sol, the ratio X is 40% or more, and a certain number of angular, distorted particles are included. Zirconia sol having such particles is useful as abrasive grains. In particular, the zirconia sol has a particle diameter D 50 In other words, the particle diameter D of the zirconia sol is in the range of 50 nm to 250 nm. 50 The particle size is in the range of 50 nm to 250 nm, and a certain number of particles with angular or irregular shapes are included. 50 Zirconia sol containing irregularly shaped particles with a particle size of 50 nm or more and 250 nm or less is expected to have a higher rate and higher smoothness (low surface roughness) than existing products, particularly in precision polishing of semiconductors and the like.
[0022] The concentration of the zirconia sol is not particularly limited, but is usually 5% by mass or more and 80% by mass or less in terms of ZrO2. When the concentration of the zirconia sol is 5% by mass or more, it is possible to prevent the zirconia concentration from decreasing when diluting with another solvent. When the concentration of the zirconia sol is 80% by mass or less, the viscosity of the sol is suppressed, and the stability is excellent. The concentration of the zirconia sol is more preferably 10% by mass or more, and further preferably 15% by mass or more. The concentration of the zirconia sol is more preferably 70% by mass or less, and further preferably 60% by mass or less. The concentration of the zirconia sol is more preferably from 10% by mass to 70% by mass, and further preferably from 15% by mass to 60% by mass.
[0023] The dispersion medium of the zirconia sol is not particularly limited, and examples thereof include water, hydrophilic organic solvents such as methanol, ethanol, 2-propanol, acetone, ether, and mixtures of one or more of the hydrophilic organic solvents. The dispersion medium of the zirconia sol is preferably water (pure water or ion-exchanged water).
[0024] The pH of the dispersion medium of the zirconia sol is not particularly limited, but is usually preferably 7 or less, and more preferably 1 to 6. When the pH of the dispersion medium of the zirconia sol is 7 or less, the pH becomes away from the isoelectric point of zirconia, and the stability is improved.
[0025] <Polishing performance> The zirconia sol is preferably diluted with pure water to a concentration of 5.0 mass % in terms of ZrO2 and used as an abrasive to polish soda glass (surface roughness Ra (arithmetic mean roughness): 0.3 μm to 0.5 μm) with a polishing rate of 0.12 μm / min or more and a surface roughness Ra of 0.6 nm or less of the polished surface. When the polishing rate is 0.12 μm / min or more and the surface roughness Ra of the polished surface is 0.6 nm or less, a polished surface with low surface roughness can be obtained in a short time.
[0026] The polishing rate is more preferably 0.13 μm / min or more, and further preferably 0.14 μm / min or more. As long as the surface roughness does not exceed a certain level, the higher the polishing rate, the better. Specifically, the polishing rate is more preferably 1.0 μm / min or less, and even more preferably 0.7 μm / min or less. The polishing rate is more preferably 0.12 μm / min or more and 1.0 μm / min or less, and further preferably 0.13 μm / min or more and 0.7 μm / min or less.
[0027] The surface roughness Ra of the polished surface is more preferably 0.55 nm or less, and further preferably 0.50 nm or less. The smaller the surface roughness Ra of the surface to be polished, the more preferable it is, for example, 0.10 nm or more, 0.20 nm or more. The surface roughness Ra of the surface to be polished is more preferably 0.10 nm or more and 0.55 nm or less, and further preferably 0.20 nm or more and 0.50 nm or less.
[0028] The zirconia sol according to this embodiment can be obtained, for example, by the following method for producing a zirconia sol.
[0029] [Method of manufacturing zirconia sol] An example of the method for producing the zirconia sol will be described below, however, the method for producing the zirconia sol is not limited to the following example.
[0030] The method for producing the zirconia sol according to this embodiment is as follows: Step A: Neutralizing the aqueous zirconium oxychloride solution by dropwise addition of aqueous ammonia Including, The concentration of the aqueous zirconium oxychloride solution is 10% by mass or more, The concentration of the ammonia water is 10% by mass or more, The volume of the droplets of ammonia water dropped in the step A is 1.0 ml or less.
[0031] <Process A> First, in step A, aqueous ammonia is added dropwise to an aqueous zirconium oxychloride solution to neutralize it.
[0032] In this embodiment, ammonia water is used as a neutralizing agent for zirconium oxychloride. The concentration of the ammonia water is 10% by mass or more. The concentration of the ammonia water is preferably 15% by mass or more, and more preferably 20% by mass or more. The concentration of the ammonia water has no particular upper limit, but is, for example, 30% by mass or less, 28% by mass or less. The concentration of the ammonia water is preferably 15% by mass or more and 30% by mass or less, and more preferably 20% by mass or more and 28% by mass or less.
[0033] The concentration of the aqueous zirconium oxychloride solution is 10% by mass or more. The concentration of the aqueous zirconium oxychloride solution is preferably 15% by mass or more, and more preferably 18% by mass or more. The concentration of the aqueous zirconium oxychloride solution has no particular upper limit, but is, for example, 28% by mass or less, 25% by mass or less, and the like. The concentration of the aqueous zirconium oxychloride solution is preferably 15% by mass or more and 28% by mass or less, and more preferably 18% by mass or more and 25% by mass or less.
[0034] The volume of the droplets of ammonia water dropped in the step A is 1.0 ml or less. The volume of the droplet is preferably 0.7 ml or less, more preferably 0.5 ml or less. The smaller the volume of the droplet, the more preferable, for example, 0.05 ml or more, 0.1 ml or more. The volume of the droplet is preferably 0.05 ml to 0.7 ml, more preferably 0.1 ml to 0.5 ml.
[0035] The time for dropping the aqueous ammonia in the step A is not particularly limited, but for example, when 1000 ml of the aqueous ammonia is dropped into 1000 ml of the aqueous zirconium oxychloride solution, the time is preferably from 10 minutes to 120 minutes. The dropping time is more preferably 90 minutes or less, and further preferably 60 minutes or less. The dropping time is not particularly limited as long as it is within a range in which the reaction proceeds appropriately, and is, for example, 15 minutes or more, 20 minutes or more, etc. The dropping time is preferably from 15 minutes to 90 minutes, and more preferably from 20 minutes to 60 minutes.
[0036] The temperature of the aqueous zirconium oxychloride solution and the temperature of the ammonia water before carrying out the step A are not particularly limited, and may be, for example, an environmental temperature (for example, within a range of 20° C. to 40° C.). The temperature of the aqueous zirconium oxychloride solution and the temperature of the ammonia water before carrying out the step A may be adjusted in advance. When the temperature is adjusted, the temperature of the aqueous zirconium oxychloride solution and the temperature of the aqueous ammonia before the step A is performed are preferably 50° C. or lower, and more preferably 40° C. or lower. When adjusting the temperature, the lower limit of the temperature of the aqueous zirconium oxychloride solution and the temperature of the aqueous ammonia before performing the step A is not particularly limited as long as it is within a range in which the reaction proceeds appropriately, and is, for example, 5°C or higher, 10°C or higher, etc. When the temperature is adjusted, the temperature of the aqueous zirconium oxychloride solution and the temperature of the aqueous ammonia before the step A is preferably 5° C. or higher and 50° C. or lower, more preferably 10° C. or higher and 40° C. or lower.
[0037] According to the method for producing the zirconia sol, since ammonia water is used as a neutralizing agent, the zirconia sol, that is, the zirconia sol in which the ratio X is 40% or more, can be obtained. According to the method for producing the zirconia sol, in the neutralization step A, ammonia water having a concentration of 10% by mass or more is added dropwise to an aqueous solution of zirconium oxychloride having a concentration of 10% by mass or more, and the droplet volume of the ammonia water added dropwise is set to 1.0 ml or less, so that a large particle size and many distorted particles can be obtained. That is, a zirconia sol having the ratio X of 40% or more can be obtained. In this way, according to the method for producing the zirconia sol, by using ammonia water as a neutralizing agent, setting the concentration of the zirconium oxychloride aqueous solution to 10% by mass or more, setting the concentration of the ammonia water to 10% by mass or more, and setting the volume of the droplets of the ammonia water dropped to 1.0 ml or less, a large particle size and many distorted particles can be obtained. That is, a zirconia sol having the ratio X of 40% or more can be obtained.
[0038] After the step A, stirring is performed as necessary to homogenize the mixture. This results in a precipitate of zirconium hydroxide. The stirring time is not particularly limited, and is, for example, from 15 minutes to 120 minutes.
[0039] Thereafter, the zirconium hydroxide is washed as necessary. The washing is performed, for example, until the Cl concentration becomes a predetermined concentration or less. The predetermined concentration is preferably, for example, 0.01% or less. The washing method is not particularly limited, but for example, a method of repeatedly filtering out the zirconium hydroxide and dispersing it in ion-exchanged water can be mentioned.
[0040] Next, an acid is added as a peptizer. The deflocculating agent for zirconium hydroxide is not particularly limited so long as it is a water-soluble inorganic or organic acid, and examples thereof include hydrochloric acid, nitric acid, sulfuric acid, acetic acid, lactic acid, citric acid, tartaric acid, malic acid, mandelic acid, and the like. Hydrochloric acid and nitric acid are preferred because, even if they are present in excess in the zirconia sol, they can be easily removed by purification with water after the zirconia sol is produced. The amount of the deflocculating agent to be added is preferably acid / ZrO2 (molar ratio)=0.01 or more and 3 or less, more preferably 0.1 or more and 1.5 or less. When the acid / ZrO2 (molar ratio) is 0.01 or more, the zirconium hydroxide can be sufficiently peptized. Also, since there is little quantitative effect even if the acid / ZrO2 (molar ratio) exceeds 3, it is economical to set the acid / ZrO2 (molar ratio) to 3 or less.
[0041] Next, in order to peptize the zirconium hydroxide, heating and aging are performed. From the viewpoint of yield, the heating and aging temperature is preferably 80°C or higher, more preferably 90°C or higher. The heating temperature is preferably 110°C or lower, more preferably 105°C or lower. The heating temperature is preferably 80°C or higher and 110°C or lower, more preferably 90°C or higher and 105°C or lower. From the viewpoint of yield, the heating and aging time is preferably 24 hours or more, more preferably 48 hours or more. The heating and aging time is preferably 120 hours or less, more preferably 100 hours or less. The heating and aging time is preferably 24 hours or more and 120 hours or less, more preferably 48 hours or more and 100 hours or less.
[0042] Thereafter, after cooling to room temperature, ultrafiltration may be carried out to concentrate the zirconia sol. Excess acid can be easily removed using ultrafiltration.
[0043] The method for producing the zirconia sol according to this embodiment has been described above. EXAMPLES
[0044] The present invention will be described in detail below using examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention. Note that the zirconia sol in the examples and comparative examples contains 1 to 3 mass % of hafnium as an inevitable impurity relative to zirconium (calculated by the following formula (X)). <Formula (X)> ([Mass of hafnium oxide] / ([Mass of zirconium oxide]+[Mass of hafnium oxide]))×100(%)
[0045] The maximum and minimum values of the content of each component shown in the following examples should be considered as the preferred minimum and maximum values of the present invention, regardless of the contents of other components. Furthermore, the maximum and minimum values of the measured values shown in the following examples should be considered as the preferred minimum and maximum values of the present invention, regardless of the content (composition) of each component.
[0046] [Preparation of zirconia sol] Example 1 1380g of ammonia water (10% by mass) adjusted to 25°C was added dropwise over 30 minutes to 1000g of zirconium oxychloride aqueous solution (10% by mass in terms of ZrO2) adjusted to 25°C in a thermostatic bath. At this time, the number of liquid delivery tubes and the dropping speed were adjusted so that the volume of the ammonia water droplets was in the range of 0.1 to 0.5 ml. Thereafter, stirring was continued for 30 minutes to obtain a precipitate of zirconium hydroxide. The zirconium hydroxide was filtered off and dispersed again in ion-exchanged water, and a washing operation was repeated. The above operation was performed until the Cl concentration became 0.01% or less. The concentration of the zirconium hydroxide after washing was 31.9 mass% in terms of ZrO2. 300 g of the obtained zirconium hydroxide was mixed with 299 g of ion-exchanged water and 39.1 g of nitric acid (60 mass%), and the prepared slurry was stirred and held under reflux at 100°C for 48 hours, and the obtained zirconia sol precursor was purified using ultrafiltration to obtain the zirconia sol according to Example 1.
[0047] (Examples 2 to 4, Comparative Example 1) Zirconia sols according to Examples 2 to 4 and Comparative Example 1 were obtained in the same manner as in Example 1, except that the concentration of the zirconium oxychloride aqueous solution and / or the concentration of the ammonia water were changed as shown in Table 1. In addition, in Table 1, "ZOC" means zirconium oxychloride. (Comparative Example 2 to Comparative Example 3) Zirconia sols according to Comparative Examples 2 to 3 were obtained in the same manner as in Example 1, except that the concentration of the zirconium oxychloride aqueous solution and / or the concentration of the ammonia water, and the volume of the ammonia water droplets were changed as shown in Table 1.
[0048] Comparative Example 4 A zirconia sol according to Comparative Example 4 was obtained in the same manner as in Example 2, except that 15 mass % caustic soda (aqueous sodium hydroxide solution) was used instead of the ammonia water.
[0049] Comparative Example 5 A zirconia sol according to Comparative Example 5 was obtained in the same manner as in Example 1, except that a zirconia sol precursor was used, which was obtained by holding an aqueous solution of zirconium oxychloride diluted with pure water to 1 mass % in terms of ZrO2 under reflux at 100°C for 60 hours.
[0050] [Particle size D 50 Measurement of The zirconia sol of each of the examples and comparative examples was diluted with ion-exchanged water to 0.1% by mass in terms of ZrO2, and then placed in an apparatus (a dynamic light scattering particle size distribution measuring apparatus ("Zetasizer Nano ZS" manufactured by Malvern Panalytical)) to measure the particle diameter D of the zirconia sol. 50 The results are shown in Table 1. <Measurement conditions> Measurement temperature: 25℃ Scattering angle: 173° Dispersoid: ZrO2 Dispersion medium: water Cell: Genuine disposable cell
[0051] [Measurement of particle shape] First, TEM images (transmission electron microscope images) of the zirconia sols of the examples and comparative examples were obtained. The TEM images were taken using a transmission electron microscope (Hitachi, Ltd., product name: HV-8100) with a field of view of 1.15 μm×0.90 μm. Next, the number of isolated particles was counted visually. Specifically, the number of particles whose circumscribing circles had diameters of 50 nm or more was counted. When there were multiple circumscribing circles around a particle, the one with the smallest ratio (see "2") between the diameter of the circumscribing circle and the diameter of the inscribing circle (concentric inscribing circle) with the same center as the circumscribing circle was used. Note that particles whose circumscribing circles had diameters of less than 50 nm were not counted because such particles have low effectiveness as abrasives. When the number of isolated particles was 20 or more, the TEM image was used as the image to be evaluated. When the number of isolated particles was less than 20, a TEM image of a different field of view was taken, and this was repeated until a TEM image with 20 or more isolated particles was obtained. The following procedure was carried out for each isolated particle in the obtained TEM image (the isolated particle to be counted). 1) First, the circumscribing circle of the particle and the inscribing circle with the same center (concentric inscribing circle) were obtained (see Figure 1). The definitions of the circumscribing circle and inscribing circle are the same as those in the MCC method of circularity in JIS B 7451:1997. 2) Next, the ratio of the diameter of the obtained circumscribing circle to the diameter of the inscribing circle [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] was calculated. 3) The ratio [(circumscribed circle diameter) / (inscribed circle diameter)] was calculated for all isolated particles in the TEM image (all isolated particles that were counted). 4) The number of isolated particles (hereinafter also referred to as "isolated particles A") having a ratio [(circumscribed circle diameter) / (inscribed circle diameter)] of 2.0 or more was counted. 5) The proportion of isolated particles A to all isolated particles (all isolated particles counted) (hereinafter also referred to as "proportion X") was determined. (Proportion X(%)) = [(Number of isolated particles A) / (Total number of isolated particles)] × 100 The results are shown in Table 1.
[0052] [Polishing performance evaluation] The zirconia sol of each of the examples and comparative examples was diluted with pure water to a concentration of 5.0 mass % in terms of ZrO2, and used as an abrasive to polish soda glass (Ra: 0.3 to 0.5 μm), and the polishing speed and surface roughness Ra of the polished surface were measured. The polishing conditions were as follows: Substrate (polished object): Soda glass (surface roughness Ra (arithmetic mean roughness): 0.3 μm to 0.5 μm) Polishing device: Single-sided polishing device (manufactured by ENGIS EJ-380N) Polishing pad: suede type pad Polishing load: 100g / cm2 (9.8kPa) Rotation speed of the platen: 80 rpm (linear speed: 9.5 m / min) Polishing time: 15 minutes Supply rate of polishing composition: 10 mL / min Measurement area of polished object: 0.143 x 0.107 mm (surface roughness) Pitch: 0.164μm
[0053] The removal rate was measured by measuring the weight of the substrate before and after polishing and calculating the difference therebetween. The surface roughness (arithmetic mean roughness (Ra)) of the polished surface after polishing was measured using AMETEC's non-contact 3D shape measurement / surface roughness measuring instrument "NewView5032" under conditions of a viewing angle of 0.143 x 0.107 mm. The results are shown in Table 1.
[0054] [Table 1]
Claims
1. Particle diameter D 50 is in the range of 50 nm or more and 250 nm or less, A zirconia sol obtained by the following procedure, characterized in that the ratio X is 40% or more. <Procedure> A transmission electron microscope image is obtained that contains 20 or more isolated particles. The following operations 1) to 5) are carried out for each isolated particle in the transmission electron microscope image. 1) Find the circumscribing circle and the inscribing circle that has the same center as the circumscribing circle. 2) The ratio of the diameter of the obtained circumscribing circle to the diameter of the inscribing circle [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] is calculated. 3) For all isolated particles in the transmission electron microscope image, the ratio [(circumscribed circle diameter) / (inscribed circle diameter)] is calculated. 4) The number of isolated particles A having a ratio [(circumscribed circle diameter) / (inscribed circle diameter)] of 2.0 or more is counted. 5) The ratio X of the isolated particles A to all the isolated particles is calculated. (Proportion X (%)) = [(Number of isolated particles A) / (Total number of isolated particles)] × 100
2. 2. The zirconia sol according to claim 1, wherein the ratio X is 50% or more.
3. The particle diameter D 50 3. The zirconia sol according to claim 1, wherein the average particle diameter is 200 nm or less.
4. Step A: Neutralizing the aqueous zirconium oxychloride solution by dropwise addition of aqueous ammonia Including, The concentration of the aqueous zirconium oxychloride solution is 10% by mass or more, The concentration of the ammonia water is 10% by mass or more, 3. The method for producing a zirconia sol according to claim 1, wherein the volume of the droplets of ammonia water dropped in the step A is 1.0 ml or less.
Citation Information
Patent Citations
Calcium zirconate-based powder and method for producing the same
JP2021075413A
Zirconia sol and method for producing the same
JP5019826B2
Production of aqueous weakly acidic crystallized zirconia-based sol