Insulated wire

The insulated wire with alternating rough and smooth surface areas addresses the flexibility and smoothness trade-off by enhancing adhesion and wear resistance through targeted surface smoothing, ensuring high flexibility and durability.

JP2024142525AInactive Publication Date: 2024-10-11AUTONETWORKS TECH LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023054683
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Insulated wires with high amorphous content for increased flexibility often suffer from low surface smoothness, leading to poor adhesion, reduced wear resistance, and potential damage due to concentrated friction at microscopic contact points.

Method used

The insulated wire features a combination of rough and smooth surface areas along its axial direction, with higher smoothness in the smooth areas to enhance adhesion and wear resistance, achieved by heating the insulation coating with a mold to form a smooth region on a raw wire with a rough surface.

Benefits of technology

This design maintains flexibility in rough areas while improving adhesion and wear resistance in smooth areas, reducing the negative effects of low surface smoothness, such as improved waterproof performance and reduced frictional wear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142525000001_ABST
    Figure 2024142525000001_ABST
Patent Text Reader

Abstract

To provide an insulated wire that has an insulating coating with low surface smoothness, yet is capable of suppressing the effects of low surface smoothness in areas where low surface smoothness is undesirable, such as contact points with other members.SOLUTION: An insulated wire 1 has a conductor 11 and an insulated coating 13 that covers the outer periphery of the conductor 11, the insulated coating 13 having a rough surface region 2 and a smooth surface region 3 along an axial direction, and the smoothness of the surface of the insulated coating 13 is higher in the smooth surface region 3 than in the rough surface region 2.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to insulated wire. [Background technology]

[0002] One of the important properties of an insulated wire is flexibility. For example, in the field of automobiles, the conductor cross-sectional area of ​​an insulated wire is becoming larger due to the need to pass a large current along with the spread of electric vehicles. In such a case, it is important that the insulated wire has high flexibility in order to maintain sufficient wiring. One of the means for increasing the flexibility of an insulated wire is to use a highly flexible material, such as an amorphous organic polymer or an organic polymer material with a large amount of amorphous components, as the constituent material of the insulating coating that covers the outer periphery of the conductor. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-234404 A [Patent Document 2] Patent Publication No. 2022-072651 Summary of the Invention [Problem to be solved by the invention]

[0004] In the case of an insulated wire, when an amorphous material or a material containing a large amount of amorphous components is used as an organic polymer material constituting the insulating coating, the flexibility of the insulated wire can be improved as described above. On the other hand, the surface smoothness of the insulating coating tends to be reduced. This is because, when forming an insulating coating by extrusion molding of a coating material, the slipperiness between the coating material and the surface of the die is reduced, and melt fracture is likely to occur due to friction. In the insulating coating, when the content of amorphous components is increased, the flexibility is improved while the surface smoothness tends to decrease, as is mentioned in, for example, Patent Document 1. In addition to the case where a coating material containing a large amount of amorphous components is used, an insulating coating with a low surface smoothness can also be formed when the insulating coating is formed by increasing the extrusion speed.

[0005] Thus, there are situations in which it is advantageous to adopt an insulated wire with a low surface smoothness of the insulating coating, such as by using a material containing a large amount of amorphous components to improve the flexibility of the insulating coating or by increasing the extrusion speed of the insulating coating to improve productivity. On the other hand, problems may occur due to the low surface smoothness when the insulated wire is used in contact with other members. If the surface smoothness of the insulating coating is low, the surface will have fine irregularities, and at the contact interface where the insulated wire contacts other members, microscopic contact points will be formed intensively at the convex parts of the irregularities. Then, for example, when a member such as a waterproof plug is attached to the outer periphery of the insulated wire, the adhesion with the member may be reduced. The low adhesion with the waterproof plug may lead to a decrease in waterproofness. In addition, when friction occurs between the insulating coating and an external member, the load due to friction will be applied intensively to the microscopic contact points, which may reduce the wear resistance of the insulating coating or cause damage to the external member.

[0006] In view of the above, an object of the present invention is to provide an insulated wire that has an insulating coating with low surface smoothness, yet is capable of suppressing the effects caused by low surface smoothness in areas where low surface smoothness is undesirable, such as contact points with other members. [Means for solving the problem]

[0007] The insulated wire of the present disclosure has a conductor and an insulating coating that covers an outer periphery of the conductor, and the insulating coating has a rough surface region and a smooth region along the axial direction, and the smoothness of the surface of the insulating coating is higher in the smooth region than in the rough surface region. Effect of the Invention

[0008] The insulated wire of the present disclosure has an insulating coating with low surface smoothness, but is capable of suppressing the effects caused by low surface smoothness in areas where low surface smoothness is undesirable, such as contact points with other members. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a perspective view illustrating a schematic diagram of an insulated wire according to one embodiment of the present disclosure. [Diagram 2] 2A and 2B are photographs of a raw insulated electric wire before smoothing, and an insulated electric wire with a smooth region formed in an area including an end portion, respectively. [Diagram 3] 3A and 3B are images of the surfaces of the rough region and the smooth region, respectively, of an insulated electric wire having a smooth region formed therein, observed with an optical microscope.

[0010] [Description of the embodiments of the present disclosure] First, embodiments of the present disclosure will be described. An insulated wire according to the present disclosure has the following configuration.

[0011] [1] The insulated wire of the present disclosure includes a conductor and an insulating coating covering an outer periphery of the conductor. The insulating coating has a roughened region and a smooth region along an axial direction, and the smoothness of the surface of the insulating coating is higher in the smooth region than in the rough region.

[0012] In the insulated wire, a rough surface region with low surface smoothness of the insulating coating and a smooth surface region with high surface smoothness of the insulating coating coexist. In the rough surface region, the properties of the insulating coating with low surface smoothness, such as high flexibility, can be utilized. On the other hand, in the smooth region, the high surface smoothness of the surface makes it easy to form a contact interface with high uniformity even at a microscopic level when the insulating coating is brought into contact with another member, and as a result, effects such as improved adhesion and abrasion resistance with the other member and suppression of damage to the other member can be obtained. In this way, by providing a smooth region in an area of ​​the insulated wire where low surface smoothness is not preferable, such as a contact area with another member, and leaving the other areas as rough surface regions, it is possible to utilize the properties brought about by the insulating coating with low surface smoothness in the rough surface region while suppressing the effects caused by the low surface smoothness in the smooth region. An insulated wire in which a rough surface region and a smooth region coexist can be easily formed by placing a mold around the area to be the smooth region of a raw insulated wire made entirely of a rough surface region and heating the insulating coating at that area through the mold.

[0013] [2] In the above aspect [1], the surface roughness Ra of the insulating coating may be 50% or more smaller in the smooth region than in the rough region, so that the influence of low surface smoothness in the smooth region can be particularly effectively suppressed.

[0014] [3] In the above aspect [1] or [2], the flexibility of the insulating coating may be higher in the rough surface region than in the smooth region. The high flexibility of the insulating coating in the rough surface region allows the insulated electric wire to be flexibly bent using the rough surface region. This improves the convenience of the insulated electric wire in terms of wiring and other operations. As described above, when a smooth region is formed on a raw insulated electric wire entirely made of a rough surface region by heating using a molding die, the flexibility of the insulating coating is likely to decrease in the smooth region while improving the smoothness of the surface of the insulating coating.

[0015] [Details of the embodiment of the present disclosure] In the following, an insulated electric wire according to an embodiment of the present disclosure will be described in detail with reference to the drawings. In this specification, with respect to the structure of each part of the insulated electric wire, concepts indicating the shape and arrangement of members, such as circularity, include errors from the geometric concepts within the range permissible for this type of insulated electric wire, such as deviations of approximately ±15% in length and approximately ±15° in angle.

[0016] <Insulated wire structure> First, the configuration of a wire harness according to an embodiment of the present disclosure will be described. Fig. 1 is a perspective view showing an outline of an insulated wire 1 according to an embodiment of the present disclosure. The insulated wire 1 has a conductor 11 and an insulating coating 13 that covers the outer periphery of the conductor 11.

[0017] The insulated wire 1 has a rough surface region 2 and a smooth region 3 along the axial direction (longitudinal direction). The smoothness of the surface of the insulating coating 13 is higher in the smooth region 3 than in the rough surface region 2. In the illustrated embodiment, the smooth region 3 is formed in a portion of the insulated wire 1, including the end portion, and the remaining region is the rough surface region 2. The rough surface region 2 and the smooth region 3 are continuous with each other. In other words, the conductor 11 and the insulating coating 13 constituting the insulated wire 1 are integrally continuous between the rough surface region 2 and the smooth region 3, respectively. The difference in state and characteristics between the rough surface region 2 and the smooth region 3 will be described in detail later.

[0018] In the insulated wire 1 according to the present embodiment, the materials constituting the conductor 11 and the insulating coating 13 are not particularly limited. Various metal materials can be used as the material constituting the conductor 11, and examples of such materials include copper and copper alloys, and aluminum and aluminum alloys. In particular, it is preferable to use copper or a copper alloy in terms of high conductivity and flexibility. The conductor 11 may be configured as a single wire, but is preferably made of a plurality of elemental wires 12 in terms of increasing flexibility when bent. The plurality of elemental wires 12 may be bundled to constitute the conductor 11, or may be twisted together to constitute the conductor 11 as a twisted wire. The conductor 11 may be compression molded.

[0019] The insulating coating 13 is made of a material containing an organic polymer. The type of organic polymer is not particularly limited, and examples thereof include olefin-based polymers such as polyolefins and olefin-based copolymers, halogen-based polymers such as polyvinyl chloride (PVC), fluorine-based polymers, various engineering plastics, elastomers, rubbers, etc. The organic polymer may be crosslinked. The organic polymer may also be foamed.

[0020] From the viewpoint of increasing the flexibility of the insulated electric wire 1, it is preferable that the constituent material of the insulating coating 13 contains an amorphous organic polymer or an organic polymer containing a large amount of amorphous components. Suitable amorphous organic polymers and organic polymers containing a large amount of amorphous components include olefin block copolymers, polyolefins such as low-density polyethylene (LDPE), halogen-based polymers such as PVC, and various elastomers. It is preferable that the amorphous organic polymers and organic polymers containing a large amount of amorphous components account for 2 mass% or more of the polymer components constituting the insulating coating 13. It is also preferable that the crystallinity of the entire polymer components constituting the insulating coating 13 is suppressed to 75% or less. As will be described later, when the smooth region 3 is formed by heating the raw insulated electric wire entirely composed of the rough surface region 2, the organic polymer constituting the insulating coating 13 needs to have thermoplasticity, and all of the organic polymers listed here are thermoplastic polymers.

[0021] In addition to the organic polymer, additives may be appropriately contained in the insulating coating 13. Examples of additives include flame retardants, antioxidants, lubricants, metal deactivators, and colorants.

[0022] Although the specific dimensions of the insulated wire 1 are not particularly limited, from the viewpoint of effectively utilizing the high flexibility of the insulating coating 13 exhibited by the rough surface area 2 to improve the convenience of wiring operations, etc., the conductor cross-sectional area is set to 16 mm 2 It is preferable to use a large-diameter electric wire such as 100 mm2 or more. There is no particular upper limit on the conductor cross-sectional area, but it is generally set at 200 mm2 or less. 2It is preferable to set the thickness of the insulating coating 13 to 0.8 mm or less in terms of the thickness in the rough surface region 2, from the viewpoint of increasing the effect of providing the rough surface region 2 and the smooth surface region 3 depending on the state of the insulating coating 13. There is no particular upper limit to the thickness of the insulating coating 13, but it is preferable to set it to about 2.0 mm or less.

[0023] <Insulated Wire Manufacturing Method> Before describing the details of the rough surface region 2 and the smooth region 3, an example of a method for producing the insulated wire 1 according to the present embodiment will be described.

[0024] The insulated wire 1 having the rough surface region 2 and the smooth region 3 can be easily manufactured using a raw insulated wire whose entire region is composed of the rough surface region 2, that is, a raw insulated wire whose entire region along the axial direction has the same configuration as the rough surface region 2 to be provided in the insulated wire 1, including the degree of surface smoothness of the insulating coating 13. The raw insulated wire is manufactured by forming the insulating coating 13 around the outer periphery of the conductor 11 by extrusion molding or the like. In this case, the degree of surface smoothness of the formed insulating coating 13 depends on the component composition of the coating material that becomes the insulating coating 13 by extrusion molding or the like, as well as the conditions under which the insulating coating 13 is formed. For example, performing extrusion molding at a high speed makes it easier for melt fracture to occur, resulting in a decrease in the surface smoothness of the insulating coating 13.

[0025] By forming smooth regions 3 at desired positions on a raw insulated electric wire whose entire area is rough surface regions 2 and leaving the remaining areas as rough surface regions 2, it is possible to obtain an insulated electric wire 1 in which rough surface regions 2 and smooth regions 3 coexist. The smooth regions 3 can be formed by heating using a molding die. That is, the molding die is placed in close contact with the surface of the insulating coating 13 of the raw insulated electric wire at the position where the smooth regions 3 are to be formed. The molding die is then heated, thereby heating the insulating coating 13 via the molding die. It is also preferable to preheat the raw insulated electric wire and / or the molding die before placing the molding die around the outer periphery of the raw insulated electric wire.

[0026] By heating the insulating coating 13 through the mold in this way, the surface of the insulating coating 13 becomes smoother than the initial state, and the smooth region 3 can be formed. The smoothing of the surface of the insulating coating 13 by heating is achieved by softening the organic polymer constituting the insulating coating 13 by heating, which eliminates the uneven structure that existed on the surface of the insulating coating 13 of the raw insulated electric wire, and reconstructing a smooth surface that imitates the surface of the mold. In order to effectively smooth the surface of the insulating coating 13, it is preferable to set the heating temperature of the insulating coating 13 to a temperature at which the constituent material of the insulating coating 13 softens at least on the surface. The insulating coating 13 may be heated to a temperature at which the surface of the insulating coating 13 melts. However, it is preferable not to heat the insulating coating 13 to a temperature high enough to melt the entire insulating coating 13. It is preferable to use a mold whose cavity surface has a smoothness equal to or greater than that of the surface of the insulating coating 13 in the smooth region 3 to be produced. In addition, if the insulating coating 13 is heated while applying a force from the outside to the inside using the mold, the smoothness of the insulating coating 13 can be effectively improved.

[0027] The heating of the insulating coating 13 to form the smooth region 3 is a process in which the coating material containing an organic polymer comes into contact with the surface of the mold member at a high temperature, similar to the process in which the insulating coating 13 is formed by extrusion molding in the raw insulated electric wire manufacturing process. However, while friction occurs between the coating material and the surface of the mold member during extrusion molding, which can form a fine uneven structure on the surface of the insulating coating 13, heating to form the smooth region 3 involves heating the insulating coating 13 in a static state, so that the insulating coating 13 does not cause friction against the mold member. Therefore, in this process, the smoothness of the surface of the insulating coating 13 does not substantially decrease due to friction.

[0028] <Differences and characteristics of rough and smooth areas> As described above, the insulated wire 1 according to the present embodiment has the rough surface region 2 and the smooth surface region 3, and the surface smoothness of the insulating coating 13 is higher in the smooth surface region 3 than in the rough surface region 2. Generally, factors that cause the surface smoothness of the insulating coating of an insulated wire to be low include the component composition of the insulating coating, such as an organic polymer containing a large amount of amorphous components, and manufacturing conditions, such as performing extrusion molding at a high speed. However, since the insulated wire 1 according to the present embodiment has the rough surface region 2 with low surface smoothness, the properties brought about by these factors can be utilized in the rough surface region 2. For example, when the organic polymer constituting the insulating coating 13 contains a large amount of amorphous components, the insulating coating 13 tends to have high flexibility, so that the insulated wire 1 can be flexibly bent in the rough surface region 2, and operations such as wiring can be performed with high convenience. Furthermore, when the insulating coating 13 is manufactured by extrusion molding at a high speed, high productivity can be obtained.

[0029] On the other hand, the smooth region 3 can suppress the influence caused when the surface has low smoothness, such as the rough region 2. For example, in the rough region 2, due to the fine uneven structure of the surface, the microscopic contact surface is likely to concentrate on the contact surface of the convex parts when it comes into contact with another member, whereas in the smooth region 3, the surface has few and / or small unevenness, so that a contact surface with high uniformity can be formed between the smooth region 3 and the other member even microscopically. Therefore, the smooth region 3 can be suitably used for attaching the other member. In addition, the smooth region 3 can be suitably disposed in a location where contact with the other member may occur. As a specific example, when a waterproof plug constituted as a rubber plug or the like is attached to the outer periphery of the insulated electric wire 1, if it is attached to the outer periphery of the smooth region 3, the waterproof plug will be in close contact with the surface of the insulating coating 13 even microscopically, and a small gap is unlikely to occur between the waterproof plug and the insulated electric wire 1, so that high waterproofing can be obtained. Even if friction occurs between the insulated wire 1 and another member in contact with it in the smooth region 3, the load due to friction is unlikely to be concentrated in a small area, so the insulating coating 13 is unlikely to wear out, resulting in high wear resistance. Similarly, the load is unlikely to be concentrated in a small area on the other member in contact with the insulated wire 1 in the smooth region 3, so it is unlikely to be damaged, such as scratched.

[0030] In this way, by having the rough surface region 2 and the smooth surface region 3 coexist in the insulated wire 1, it is possible to utilize the characteristics of each region. From the viewpoint of ensuring a large difference in characteristics between the rough surface region 2 and the smooth surface region 3, and particularly from the viewpoint of enhancing the characteristics obtained by the high surface smoothness in the smooth surface region 3, it is preferable that the surface roughness Ra of the insulating coating 13 in the smooth surface region 3 is 50% or more smaller than that of the rough surface region 2, as the difference in the degree of smoothness between the rough surface region 2 and the smooth surface region 3. In other words, it is sufficient that the surface roughness Ra of the rough surface region 2 is 100%, and the reduction in the surface roughness Ra in the smooth surface region 3 is 50% or more. More preferably, the reduction is 60% or more, and furthermore, 65% or more. Since the smoothness of the surface of the smooth surface region 3 is preferably high, there is no particular upper limit set for the difference in smoothness between the rough surface region 2 and the smooth surface region 3, but considering the degree of smoothness that can be achieved when the smooth surface region 3 is formed by heating using a molding die, the reduction in the surface roughness Ra in the smooth surface region 3 is approximately 90% or less. The specific values ​​of surface roughness Ra of the rough region 2 and the smooth region 3 are not particularly limited, but examples include a form in which the rough region 2 is 150 μm or more and 500 μm or less, and the smooth region 3 is 50 μm or more and 150 μm or less. Comparison of the surface smoothness of the insulating coating 13 in the rough region 2 and the smooth region 3 can be easily performed by visually comparing the gloss. Alternatively, the surface roughness Ra may be quantitatively evaluated based on JIS B 0601:2013.

[0031] In the insulated wire 1 according to the present embodiment, as described above, the smooth region 3 has a higher smoothness on the surface of the insulating coating 13 than the rough region 2, but on the other hand, it is preferable that the flexibility of the insulating coating 13 is higher in the smooth region 3 in the rough region 2. If the rough region 2 has high flexibility, the smooth region 3 can be suitably used for applications in which the insulating coating 13 comes into contact with other members, while the rough region 2 can be used to flexibly bend the insulated wire 1, thereby improving the convenience of the operation of wiring and the like. As described above, when the insulating coating 13 is formed using an amorphous organic polymer or an organic polymer containing a large amount of amorphous components, the surface smoothness of the insulating coating 13 tends to be low, but the amorphous organic polymer or the organic polymer containing a large amount of amorphous components has high flexibility. Therefore, the rough region 2 is easily formed as a region having low surface smoothness and high flexibility. In addition, as described above, when the smooth region 3 is formed by heating the raw insulated wire whose entire region is made of the rough region 2 using a molding die, the flexibility of many organic polymers that can form the insulating coating 13 tends to decrease.

[0032] The difference in flexibility of the insulating coating 13 between the rough surface region 2 and the smooth surface region 3 can be evaluated, for example, by a three-point bending test of the insulated electric wire 1. The three-point bending test can be performed as a bending test conforming to JIS K 7171:2016. That is, the maximum value of the repulsive force when the sample electric wire is supported at two points separated by a predetermined fulcrum distance along the length direction and the central part is bent is measured as the repulsive load. The smaller the value of the repulsive load obtained, the higher the flexibility of the insulated electric wire 1. The three-point bending test can be performed by making the fulcrum distance as a ratio to the outer diameter of the insulated electric wire 1 uniform for each of the rough surface region 2 and the smooth surface region 3 (for example, as in the later-described examples, the fulcrum distance is set to four times the outer diameter of the insulated electric wire 1 in each of the regions 2 and 3), and comparing the repulsive loads. For example, it is sufficient that the repulsive load in the smooth surface region 3 is 20% or more higher than that in the rough surface region 2. In other words, the repulsive load of the rough surface region 2 is taken as 100%, and the increase in the repulsive load of the smooth region 3 should be 20% or more. In this case, the bending flexibility of the rough surface region 2 can be considered to be sufficiently higher than that of the smooth region 3. More preferably, the increase in the repulsive load should be 25% or more, and even more preferably 30% or more. There is no particular upper limit to the increase in the repulsive load, but it is preferable to keep it to, for example, 60% or less from the viewpoint of ensuring a certain degree of flexibility even in the smooth region 3. The flexibility of the insulated wire 1 evaluated by the repulsive load obtained in the three-point bending test includes the contribution of the conductor 11. However, if the conductor cross-sectional area is within the range given above as a preferable range, the increase in the repulsive load within the above range can be obtained, and it can be considered that there is a sufficient difference in the flexibility of the insulating coating 13 between the rough surface region 2 and the smooth region 3.

[0033] In the insulated electric wire 1, the specific positions and lengths of the rough surface region 2 and the smooth surface region 3 are not particularly specified, and the smooth surface region 3 may be provided in regions where undesirable effects may occur if the surface smoothness of the insulating coating 13 is low, such as positions where other members are attached or positions where undesired contact with other members is expected. In this way, the effect of suppressing effects that may be caused by low surface smoothness by the surface smoothness of the smooth surface region 3 can be effectively utilized. For example, when a member such as a waterproof plug is attached to the end of the insulated electric wire 1 or in the vicinity thereof, or when a connector is attached to the end of the insulated electric wire 1, and there is a concern that the insulating coating 13 may be worn due to contact with the connector housing, the smooth surface region 3 may be provided in a region including the end of the insulated electric wire 1. In addition, when a member such as a protective material is attached to the midway portion of the insulated electric wire 1 in the axial direction, or when there is a possibility that the midway portion of the insulated electric wire 1 may come into undesired contact with an external member provided nearby, and there is concern that such contact may cause wear of the insulating coating 13 or damage to the external member, the smooth region 3 may be provided at a necessary location in the midway portion of the insulated electric wire 1 in the axial direction. The rough surface region 2 and / or the smooth region 3 may be provided at multiple locations. When the smooth region 3 is provided at two or more locations, the smoothness of the surface of the smooth region 3 may be the same or different from each other. The ratio of the length of the rough surface region 2 to the smooth region 3 is not particularly specified, but from the viewpoint of effectively utilizing the properties of the rough surface region 2, such as high flexibility, it is preferable to set the total length of the rough surface region 2 longer than the total length of the smooth region 3.

[0034] The specific shapes of the rough surface region 2 and the smooth region 3 are not particularly specified. In the illustrated embodiment, both the smooth surface region 3 and the rough surface region 2 are configured to have a circular cross section, and their outer diameters are not significantly different. In this manner, by configuring the rough surface region 2 and the smooth surface region 3 so as not to change their cross-sectional shapes and sizes as much as possible, the insulated electric wire 1 can be made to have a small difference in overall outer shape from a conventional insulated electric wire whose surface smoothness does not change over the entire area. As described above, when the raw insulated electric wire whose entire area is made of the rough surface region 2 is heated using a forming mold to form the smooth region 3, the outer diameter of the smooth region 3 may become smaller than that of the rough surface region 2 due to the force applied to the raw insulated electric wire from the forming mold. However, from the viewpoint of minimizing changes in the cross-sectional shape and cross-sectional size of the smooth region 3 and the rough region 2, it is advisable to keep the difference in outer diameter between the smooth region 3 and the rough region 2 to 20% or less, or even 10%, of the outer diameter of the rough region 2, by using a molding die having a cavity with a shape and size similar to that of the raw insulated electric wire.

[0035] On the other hand, it is also possible to actively change the cross-sectional shapes and / or cross-sectional sizes of the smooth region 3 and the rough region 2. For example, when the cross-sectional shape of the rough region 2 is not circular, the cross-sectional shape of the smooth region 3 can be made closer to circular, or when the cross-sectional size of the rough region 2 is large, the cross-sectional size of the smooth region 3 can be made smaller, which may improve the convenience of attaching other components to the smooth region 3. In addition, as a change in the cross-sectional shape, it is possible to make the cross-section of one of the rough region 2 and the smooth region 3 a flat shape, such as one that can approximate an oval or a rectangle, and the cross-section of the other a shape with a lower degree of flatness, such as one that can approximate a circle or a square. To make the cross-sectional shape and / or cross-sectional size of the smooth region 3 and the rough region 2 different, for example, when a raw insulated electric wire whose entire area is rough region 2 is heated using a molding die to form smooth region 3, a molding die having a cavity corresponding to the shape and cross-sectional size of the smooth region 3 to be formed is used to apply a force that deforms insulating coating 13 and conductor 11, thereby smoothing the surface of insulating coating 13 and changing the cross-sectional shape and / or cross-sectional size at the same time. EXAMPLES

[0036] Examples are shown below. The present invention is not limited to the examples. In these examples, insulated electric wires having a smooth area and a rough area were prepared, and the smoothness and flexibility of the surface of the smooth area and the rough area were compared. Unless otherwise specified, the preparation and evaluation of the samples were performed at room temperature in the air.

[0037] <Sample preparation> The raw insulated wire was prepared by extruding an insulating coating of uniform thickness around the conductor. The conductor was a stranded wire made by twisting together copper alloy wires. The conductor cross-sectional area was 95 mm 2 The insulating coating was made of cross-linked polyethylene and had a thickness of 2.0 mm.

[0038] The raw insulated electric wire was cut to a length of 300 mm, and a smooth region was formed in a region extending 150 mm from one end. The remaining region was left as a rough surface region, and an insulated electric wire having both a smooth region and a rough surface region was obtained. The smooth region was formed by placing a molding die having a cylindrical cavity with an inner diameter slightly smaller than the outer diameter of the raw insulated electric wire around the outer periphery of the raw insulated electric wire and heating it. The temperature of the molding die was set to 150°C.

[0039] <Sample evaluation> The obtained insulated wire was visually observed to confirm that a smooth area was formed in addition to a rough area. Furthermore, the surface of the insulating coating was observed with an optical microscope for each of the rough and smooth areas, and the surface roughness Ra was evaluated using a surface roughness measuring device in accordance with JIS B 0601:2013.

[0040] Furthermore, a three-point bending test was conducted in accordance with JIS K 7171:2016 to measure the repulsive load of the insulated electric wire in the rough and smooth areas. In this case, the insulated electric wire was cut to a length of 150 mm in each of the rough and smooth areas to be used as a test specimen. Each test specimen was supported at two points separated by a predetermined support distance, and the central part was bent to measure the maximum repulsive force (unit: N) and recorded as the repulsive load. The support distance was set to four times the outer diameter of each test specimen. Specifically, since the outer diameter of the insulated electric wire was 17.8 mm in the rough area and 16.6 mm in the smooth area, the support distance was set to 71.2 mm for the test specimen in the rough area and 66.4 mm for the test specimen in the smooth area.

[0041] <Evaluation Results> Figures 2A and 2B show photographs of the raw insulated electric wire before the formation of the smooth region, and the insulated electric wire after the formation of the smooth region, respectively. Figures 3A and 3B show images of the insulated electric wire after the formation of the smooth region, observed with an optical microscope. Figure 3A shows the rough region, and Figure 3B shows the smooth region. Furthermore, Table 1 below shows the evaluation results of the surface roughness Ra and the rebound load in a three-point bending test for the rough and smooth regions. Table 1 also shows the amount of change in the value of the smooth region based on the value of the rough region.

[0042] [Table 1]

[0043] Comparing the photographs in Figures 2A and 2B, it can be seen that the entire area in Figure 2A has a matte surface, whereas in Figure 2B, only the area on the left side where the smooth area is formed is glossy. This confirms that a smooth area with improved surface smoothness of the insulating coating can be formed by heating using a molding die. Furthermore, comparing the microscope images in Figures 3A and 3B, it can be seen that in Figure 3A, which shows the rough area, a microstructure with unevenly distributed light and dark areas indicating an uneven structure can be seen, whereas in Figure 3B, which shows the smooth area, a highly uniform surface can be seen, confirming that the surface is smoother.

[0044] Furthermore, looking at the evaluation results in Table 1, as seen by comparing Figures 3A and 3B, the surface roughness Ra is smaller in the smooth area than in the rough area, quantitatively confirming that smoothness has been improved. The surface roughness Ra is 68% smaller in the smooth area than in the rough area. The rebound load in the three-point bending test is larger in the smooth area than in the rough area, indicating that the rough area has higher flexibility. The rebound load in the smooth area is 31% higher than in the rough area.

[0045] The above results confirm that it is possible to manufacture an insulated electric wire having both rough and smooth regions by heating the raw insulating coating using a molding die. It also confirms that the smoothness of the surface of the insulating coating is higher in the smooth region than in the rough region. It is also found that the flexibility of the insulating coating is higher in the rough region than in the smooth region.

[0046] Although the embodiments of the present disclosure have been described in detail above, the present invention is not limited to the above-described embodiments, and various modifications are possible without departing from the gist of the present invention. [Explanation of symbols]

[0047] 1. Insulated wire 11 Conductor 12 Wire 13 Insulation coating 2 Rough surface area 3 Smooth region

Claims

1. A conductor and an insulating coating that covers an outer periphery of the conductor, The insulating coating has a roughened region and a smooth region along an axial direction, an insulating coating having a surface that is smoother in the smooth region than in the rough region;

2. 2. The insulated wire according to claim 1, wherein the surface roughness Ra of the insulating coating is smaller in the smooth region by 50% or more than in the rough region.

3. 3. The insulated wire according to claim 1, wherein the insulating coating has a higher flexibility in the rough region than in the smooth region.

Citation Information

Patent Citations

  • Polyolefin-based coated electric wire

    JP2014234404A

  • Coated wire, and wire harness

    JP2022072651A