Magneto rheological fluid

By using magnetic particles with a defined size and an amide-based anti-settling agent, the MR fluid achieves low viscosity and improved stability for tactile presentation devices.

JP2024142533AInactive Publication Date: 2024-10-11KURIMOTO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023054692
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Tactile presentation devices require an MR fluid with low base viscosity and good sedimentation and redispersibility to accurately reproduce the sensations of touching various substances like gas and water, and existing solutions fail to achieve this effectively.

Method used

Incorporating magnetic particles with a specific size range and an amide-based anti-settling agent within a defined concentration in the MR fluid composition.

Benefits of technology

The MR fluid maintains low base viscosity while significantly reducing sedimentation and improving redispersibility, making it suitable for tactile presentation devices.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To achieve a MR fluid which is low in base viscosity and good in sedimentability and redispersibility.SOLUTION: A magneto rheological fluid contains magnetic particles having a particle size of 0.05 μm or more and 100 μm or less, and an amide-based anti-settling agent with a content of 0.5 wt.% or more and 1.5 wt.% or less based on the total amount.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to magnetorheological fluids, and in particular to magnetorheological fluids suitable for tactile presentation applications. [Background technology]

[0002] Magneto-rheological (MR) fluids are fluids in which magnetic particles such as iron (Fe) are dispersed in a dispersion medium such as oil. In MR fluids, magnetic particles are randomly suspended in the dispersion medium when no magnetic field is applied. When an external magnetic field is applied to MR fluids, the magnetic particles form numerous clusters along the direction of the magnetic field, increasing the yield stress. In this way, MR fluids are materials whose rheological properties or mechanical properties can be easily controlled by electrical signals, and they are used in linear devices such as shock absorbers for automobiles and seat dampers for construction machinery, as well as rotary devices such as clutches and brakes.

[0003] In recent years, tactile presentation devices have been considered that allow an operator to feel that they are operating the touch panels and operation levers of various electronic devices by generating operational resistance according to the operating situation (see, for example, Patent Document 1). In addition, tactile presentation devices that are linked to the operator's operation and present the operator with the tactile sensation of a virtual object displayed on a video screen have also been considered (see, for example, Patent Document 2). MR fluids, whose viscosity changes when an external magnetic field is applied, and which can change the torque required for operation, are expected to be used in such tactile presentation devices. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2021-093022 [Patent Document 2] JP 2017-138651 A Summary of the Invention [Problem to be solved by the invention]

[0005] In particular, tactile presentation devices that present the tactile sensation of virtual objects are required to be able to reproduce not only the sensation of touching a real solid, but also the sensation of touching gas or water. In order to express such subtle tactile sensations, MR fluids with low basal viscosity in the absence of a magnetic field are required. In addition, the torque change caused by the MR fluid must occur instantly and with good reproducibility. For this reason, MR fluids with good sedimentation and redispersibility are required.

[0006] An object of the present disclosure is to realize an MR fluid having a low base viscosity and good sedimentation and redispersibility. [Means for solving the problem]

[0007] One embodiment of the magnetorheological fluid of the present disclosure contains magnetic particles having a particle size of 0.05 μm or more and 100 μm or less, and 0.5 wt % or more and 1.5 wt % or less of an amide-based anti-settling agent.

[0008] One embodiment of the magnetorheological fluid contains 0.5 wt % or more and 1.5 wt % or less of an amide-based anti-settling agent, so that it is possible to keep the base viscosity low, while making it difficult for settling to occur and improving redispersibility. Effect of the Invention

[0009] According to the magnetorheological fluid of the present disclosure, it is possible to suppress the base viscosity to a low level, while suppressing sedimentation and improving redispersibility. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The magnetorheological fluid (MR fluid) of this embodiment has magnetic particles dispersed in a dispersion medium, and contains an amide-based anti-settling agent.

[0011] The magnetic particles have a particle size of 0.05 μm or more, preferably 0.1 μm or more, in order to keep the base viscosity low, and 100 μm or less, preferably 50 μm or less, in order to prevent sedimentation. The particle size of the magnetic particles can be measured using a particle size distribution measuring device using a laser diffraction / scattering method.

[0012] The magnetic particles may be, for example, iron, iron nitride, iron carbide, carbonyl iron, chromium dioxide, low carbon steel, nickel, or cobalt. Also usable are iron alloys such as aluminum-containing iron alloys, silicon-containing iron alloys, cobalt-containing iron alloys, nickel-containing iron alloys, vanadium-containing iron alloys, molybdenum-containing iron alloys, chromium-containing iron alloys, tungsten-containing iron alloys, manganese-containing iron alloys, and copper-containing iron alloys. Also usable are paramagnetic, superparamagnetic, or ferromagnetic compound particles made of gadolinium or an organic derivative of gadolinium, and particles made of a mixture thereof. Among these, carbonyl iron is preferred because it is easy to obtain particles having an average particle size suitable for magnetic particles.

[0013] The magnetic particles may be surface-modified. For example, when the dispersion medium is hydrophobic, a surface-modified layer made of a compound having a hydrocarbon chain, an allyl group, or the like may be provided. When the dispersion medium is hydrophilic, a surface-modified layer made of a compound having a hydrophilic functional group such as a hydroxyl group may be provided.

[0014] The dispersion medium may be any liquid capable of dispersing magnetic particles. For example, silicone oil, fluorine oil, polyalphaolefin (PAO), paraffin, ether oil, ester oil, mineral oil, vegetable oil, or animal oil may be used. In addition, organic solvents such as toluene, xylene, hexane, and ethers, or ionic liquids (room-temperature molten salts) such as ethylmethylimidazolium salt, 1-butyl-3-methylimidazolium salt, and 1-methylpyrazolium salt may be used. These may be used alone or in combination of two or more kinds. If a hydrophilic surface modification layer is provided, water, esters, alcohols, or the like may be used as the dispersion medium.

[0015] The concentration (volume fraction) of the magnetic particles in the entire MR fluid is preferably 10 vol% or more, more preferably 15 vol% or more, from the viewpoint of exerting the functions of the MR fluid, and is preferably 40 vol% or less, more preferably 30 vol% or less, from the viewpoint of suppressing the base viscosity of the MR fluid.

[0016] The MR fluid of this embodiment contains an amide-based anti-settling agent. The amide-based anti-settling agent is an anti-settling agent whose main component is amide wax, which is a condensation product of amine and fatty acid. Commercially available products include Disparlon 6100 manufactured by Kusumoto Chemical Co., Ltd. and Flownon RCM-230AF manufactured by Kyoeisha Chemical Co., Ltd.

[0017] The concentration (volume fraction) of the amide-based anti-settling agent in the dispersion medium is 0.5 wt% or more and 1.5 wt% or less from the viewpoint of suppressing an increase in base viscosity while improving sedimentation and redispersibility. By adding the amide-based anti-settling agent, it is possible to improve sedimentation and redispersibility while suppressing an increase in base viscosity. As a method for suppressing the sedimentation of MR fluid, a method of adding inorganic particles such as silica or organic particles such as polystyrene is known. However, in the case of these methods, the viscosity of the fluid increases, so the base viscosity increases. In addition, the redispersibility, which is an index of the ease of returning from a sedimented state to a dispersed state, is not sufficiently improved.

[0018] The MR fluid of this embodiment has a sedimentation height ratio of preferably 65% ​​or more, more preferably 70% or more. The sedimentation height ratio is the ratio (%) of the sedimentation layer of particles to the total height of the fluid after the MR fluid is left to stand for 14 days, and can be measured by the method shown in the Examples. The redispersibility is preferably 8 Nm / s or more, more preferably 10 Nm / s or more. The redispersibility is (maximum torque for 10 seconds from the start of rotation-torque 10 seconds after the start of rotation) / 10 (Nm / s) after the MR fluid is left to stand for 14 days, and can be measured by the method shown in the Examples. The average value of the base viscosity at shear rates of 1 / s, 10 / s, and 100 / s is preferably 1 Pa·s or less, more preferably 0.9 Pa·s or less, and even more preferably 0.8 Pa·s or less.

[0019] In the case of a tactile presentation device, particularly a device that presents the tactile sensation of a virtual object, the operator's movement (operation speed) is mainly in the medium-speed range of shear speeds of about 1 / s to 100 / s, so it is preferable that the base viscosity in this speed range is small. The MR fluid of this embodiment has a small base viscosity in the medium-speed range of 1 / s to 100 / s, is less likely to settle, and has excellent redispersibility, making it particularly useful as a magnetorheological fluid for use in tactile presentation devices and the like.

[0020] Tactile presentation devices can be used, for example, to give a sense of operation to the operating levers of various devices, as training equipment used to strengthen muscles, as rehabilitation equipment used by users to restore muscle strength, and as tactile presentation devices that work in conjunction with a display to convey the sensation of virtual objects to the hand.

[0021] In addition to the amide-based anti-settling agent, various additives can be added to the MR fluid of this embodiment. However, it is preferable to have a small amount of additives that increase viscosity, and it is even more preferable to have no additives added.

[0022] The MR fluid of the present disclosure will be described in more detail below using examples. The following examples are illustrative and are not intended to limit the invention of the present disclosure.

[0023] <Measurement of Settlement Height Rate> About 100 mL of MR fluid was placed in a container and allowed to stand for 14 days at 40° C. After that, the total height and the height of the particle settling layer were measured, and the settling layer height ratio was calculated using the following formula. Settling layer height rate (%) = (total height - particle settling layer height) / total height x 100 The larger the sedimentation layer height ratio, the more difficult it is for the magnetic particles to settle, indicating a stable MR fluid.

[0024] <Evaluation of redispersibility> Approximately 100 mL of MR fluid was placed in a container and allowed to stand at 40°C for 14 days. After this, a stirring rod with stirring blades was inserted to the bottom of the sedimentation layer, and the torque was measured when rotating at 200 RPM without applying a magnetic field. The redispersibility was evaluated using the following formula. Redispersibility (Nm / s) = (Maximum torque in 10 seconds from the start of rotation - Torque 10 seconds after the start of rotation) / 10 A higher redispersibility value indicates that redispersion is more easily achieved.

[0025] <Evaluation of base viscosity> The basal viscosity was measured using a parallel plate type rotational viscometer (MCR301, manufactured by Anton Paar Japan). The distance between the plates was 500 μm, and parallel plates with a diameter of 20 mm were used. The shear stress was measured at a constant shear rate of 1 / s, 10 / s, and 100 / s for 30 seconds without applying a magnetic field.

[0026] Example 1 Carbonyl iron (BASF, CS) with an average primary particle size of 6 μm was used as the magnetic particles, and polyalphaolefin-based synthetic hydrocarbon oil was used as the dispersion medium. The concentration of the magnetic particles was 20 vol%. 0.58 wt% of an amide-based anti-settling agent (Kusumoto Chemical, Disparlon 6100) was added to the dispersion medium.

[0027] The settling height ratio was 74.2%. The redispersibility was 11.94 Nm / s. The base viscosities at shear rates of 1 / s, 10 / s, and 100 / s were 0.71 Pa s, 0.22 Pa s, and 0.10 Pa s, respectively, with an average value of 0.34 Pa s.

[0028] Example 2 An MR fluid was prepared in the same manner as in Example 1, except that the concentration of the amide-based anti-settling agent was 1.45 wt %.

[0029] The settling height ratio was 83.7%. The redispersibility was 30.05 Nm / s. The base viscosities at shear rates of 1 / s, 10 / s, and 100 / s were 1.54 Pa s, 0.44 Pa s, and 0.14 Pa s, respectively, with an average value of 0.70 Pa s.

[0030] Comparative Example 1 An MR fluid was prepared in the same manner as in Example 1, except that no amide-based anti-settling agent was added.

[0031] The settling height ratio was 54.6%. The redispersibility was 3.64 Nm / s. The base viscosities at shear rates of 1 / s, 10 / s, and 100 / s were 1.42 Pa s, 1.19 Pa s, and 0.27 Pa s, respectively, with an average value of 0.96 Pa s.

[0032] Comparative Example 2 An MR fluid was prepared in the same manner as in Example 1, except that 0.58 wt % of nanometer-sized hydrophilic silica (AEROSIL200, average particle size 12 nm, manufactured by Nippon Aerosil Co., Ltd.) was added instead of the amide-based anti-settling agent.

[0033] The settling height ratio was 74.0%. The redispersibility was 1.76 Nm / s. The base viscosities at shear rates of 1 / s, 10 / s, and 100 / s were 4.17 Pa s, 3.20 Pa s, and 0.60 Pa s, respectively, with an average value of 2.65 Pa s.

[0034] Comparative Example 3 An MR fluid was prepared in the same manner as in Example 1, except that 1.45 wt % of nanometer-sized hydrophilic silica (AEROSIL200, average particle size 12 nm, manufactured by Nippon Aerosil Co., Ltd.) was added instead of the amide-based anti-settling agent.

[0035] The settling height ratio was 91.3%. The redispersibility was 5.03 Nm / s. The base viscosities at shear rates of 1 / s, 10 / s, and 100 / s were 7.29 Pa s, 5.31 Pa s, and 1.55 Pa s, respectively, with an average value of 4.72 Pa s.

[0036] Comparative Example 4 An MR fluid was prepared in the same manner as in Example 1, except that 0.58 wt % of nanometer-sized hydrophobic silica (AEROSIL R974, average particle size 12 nm, manufactured by Nippon Aerosil Co., Ltd.) was added instead of the amide-based anti-settling agent.

[0037] The settling height ratio was 68.6%. The redispersibility was 5.11 Nm / s. The base viscosities at shear rates of 1 / s, 10 / s, and 100 / s were 4.50 Pa s, 1.50 Pa s, and 0.27 Pa s, respectively, with an average value of 2.09 Pa s.

[0038] Comparative Example 5 An MR fluid was prepared in the same manner as in Example 1, except that 1.45 wt % of nanometer-sized hydrophobic silica (AEROSIL R974, average particle size 12 nm, manufactured by Nippon Aerosil Co., Ltd.) was added instead of the amide-based anti-settling agent.

[0039] The settling height ratio was 81.5%. The redispersibility was 13.41 Nm / s. The base viscosities at shear rates of 1 / s, 10 / s, and 100 / s were 12.00 Pa s, 3.67 Pa s, and 0.59 Pa s, respectively, with an average value of 5.42 Pa s.

[0040] Comparative Example 6 An MR fluid was prepared in the same manner as in Example 1, except that 0.58 wt % of bentonite (Garamite 1958, manufactured by Big Chemie Japan) was added instead of the amide-based anti-settling agent.

[0041] The settling height ratio was 71.1%. The redispersibility was 2.57 Nm / s. The base viscosities at shear rates of 1 / s, 10 / s, and 100 / s were 4.44 Pa s, 1.94 Pa s, and 0.25 Pa s, respectively, with an average value of 2.21 Pa s.

[0042] Comparative Example 7 An MR fluid was prepared in the same manner as in Example 1, except that 1.45 wt % of bentonite (Garamite 1958, manufactured by Big Chemie Japan) was added instead of the amide-based anti-settling agent.

[0043] The settling height ratio was 85.8%. The redispersibility was 7.13 Nm / s. The base viscosities at shear rates of 1 / s, 10 / s, and 100 / s were 31.82 Pa s, 4.01 Pa s, and 0.66 Pa s, respectively, with an average value of 12.16 Pa s.

[0044] Examples and comparative examples are summarized in Table 1. The MR fluids of the examples containing an amide-based anti-settling agent have a lower base viscosity in the medium speed range, are less susceptible to settling, and have excellent redispersibility compared to MR fluids containing fine particles.

[0045] [Table 1] [Industrial Applicability]

[0046] The magnetorheological fluid of the present disclosure has a low base viscosity, is resistant to sedimentation, and has excellent redispersibility, making it particularly useful in applications such as tactile presentation devices.

Claims

1. Magnetic particles having a particle size of 0.05 μm or more and 100 μm or less; A magnetorheological fluid containing an amide-based anti-settling agent in an amount of 0.5 wt % or more and 1.5 wt % or less based on the total amount.

2. The magnetorheological fluid according to claim 1 , comprising 10 vol % or more and 40 vol % or less of the magnetic particles.

3. 2. The magnetic rheological fluid according to claim 1, wherein after standing at 40° C. for 14 days, the settling height ratio represented by the following formula 1 is 65% or more, and the average value of the base viscosity at three shear rates of 1 / s, 10 / s and 100 / s is 1 Pa·s or less. Settling height ratio = (total height - height of particle settling layer) / total height x 100 ... formula 1

Citation Information

Patent Citations

  • Force sense presentation apparatus

    JP2017138651A

  • Operation lever system

    JP2021093022A