Laminated filter medium for antiviral air filter
The laminated filter medium addresses the re-release of viruses by incorporating antiviral agents in both layers to enhance virus inactivation and collection efficiency, ensuring effective virus containment.
Patent Information
- Application Number
- JP2023054732
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional air filters fail to effectively inactivate viruses trapped on non-antiviral fiber sheets, leading to potential re-release of viruses and fiber dust, which can become sources of infection.
A laminated filter medium with an upstream fiber layer having antiviral properties and a collection efficiency of 10% or less for particles 0.3-0.5 μm, and a downstream fiber layer with a collection efficiency of 90% or more for the same size particles, utilizing antiviral agents like silver-copper zeolite and copper compounds to enhance virus inactivation.
The laminated filter medium efficiently collects and inactivates virus-containing droplet nuclei, reducing the risk of virus re-release and enhancing overall antiviral performance.
Smart Images

Figure 2024142555000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a filtering material for air filters used in air purification devices such as air purifiers, building air conditioners, automobile cabin air conditioners, home air conditioners, and commercial air conditioners. [Background technology]
[0002] Conventionally, air filters have been used to purify the air by removing pollen, dust, etc. from the air. Air filters used in air purifiers and building air conditioners use filter materials made of glass fiber, paper, or nonwoven fabric, and the filter materials are pleated to increase the filtering area and filtering performance. In addition, low-rigidity materials such as meltblown nonwoven fabrics are poor at retaining the pleated shape as filter materials when used alone, so they are usually bonded with rigid nonwoven fabrics for reinforcement.
[0003] In recent years, with the increasing consumer need to prevent viral infections, anti-virus measures are being demanded for air purifiers and the air filters installed in them. Anti-virus measures using air filters involve capturing airborne viruses that are a source of infection in the air filter, and inactivating the viruses on the air filter to prevent them from being re-released from the air filter and becoming a source of infection.
[0004] Viruses are released into the air in the form of droplets when people breathe, talk, cough, or sneeze, and then the water evaporates and the droplets become particles called droplet nuclei that float in the air. Droplet nuclei are often 0.2 μm to 2.5 μm in size. There is also a lot of fibrous dust in the room, which is charged with static electricity and attracts and adsorbs surrounding viruses. Most fibrous dust is 10 μm to 1 mm in size.
[0005] Patent Document 1 proposes an antiviral fiber spun from or carrying a polymer carrying ions of a metal selected from copper, silver, zinc, and nickel, and an antiviral fiber product at least partially containing the antiviral fiber. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2011-42615 A Summary of the Invention [Problem to be solved by the invention]
[0007] Regarding conventional air filter media, the fiber sheet of Patent Document 1 can inactivate viruses captured on the antiviral fiber by using antiviral fibers. However, as an antiviral fiber product, fiber sheets without antiviral function are arranged on the front and back of the antiviral fiber sheet, and fiber dust with viruses adsorbed thereon adheres to these non-antiviral fiber sheets, but since these fiber sheets do not have antiviral function, they cannot inactivate the viruses. In other words, when the viruses and fiber dust that adhere and accumulate on the fiber sheet are released again, they can become a source of infection.
[0008] The present invention has been made to solve the above-mentioned problems, and has an object to provide a filter medium for air filters which comprises a downstream fiber layer that efficiently captures virus-containing droplet nuclei in the air and inactivates the captured viruses, and an upstream fiber layer that inactivates viruses captured together with fibrous dust. [Means for solving the problem]
[0009] As a result of extensive research aimed at solving the above problems, the present invention was achieved.
[0010] That is, the present invention relates to a laminated filter material for air filters, comprising an upstream fiber layer having antiviral properties and a particle collection efficiency of 10% or less for particles with a particle diameter of 0.3 μm or more and 0.5 μm or less, and a downstream fiber layer having antiviral properties and a particle collection efficiency of 90% or more for particles with a particle diameter of 0.3 μm or more and 0.5 μm or less. Effect of the Invention
[0011] According to the filter medium of the present invention, it is possible to provide a filter medium for air filters which comprises a downstream fiber layer that captures virus-containing droplet nuclei in the air with high efficiency and inactivates the captured viruses, and an upstream fiber layer that inactivates viruses captured together with fibrous dust. [Brief description of the drawings]
[0012] [Figure 1] 1 is a cross-sectional view of one embodiment of the filter medium of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The filter media of the present invention has an upstream fibrous layer and a downstream fibrous layer.
[0014] The laminated filter material for air filters of the present invention includes an upstream fiber layer having antiviral properties and a particle collection efficiency of 10% or less for particles with a particle diameter of 0.3 μm or more and 0.5 μm or less, and a downstream fiber layer having antiviral properties and a particle collection efficiency of 90% or more for particles with a particle diameter of 0.3 μm or more and 0.5 μm or less.
[0015] As described above, since both the upstream fiber layer and the downstream fiber layer have antiviral properties, the antiviral properties can be exhibited more effectively. In addition, by setting the collection efficiency of the upstream fiber layer to 10% or less for particles with a particle diameter of 0.3 μm to 0.5 μm and the collection efficiency of the downstream fiber layer to 90% or more for particles with a particle diameter of 0.3 μm to 0.5 μm, the difference in collection efficiency between the upstream fiber layer and the downstream fiber layer allows for more efficient collection.
[0016] Examples of the fiber materials constituting the upstream fiber layer and the downstream fiber layer include glass fiber, polyolefin, polyester, polyamide, vinylon, cellulose pulp, etc., and examples of the fiber layer form include paper, nonwoven fabric, knitted fabric, net, etc., among which airlaid nonwoven fabric, wet nonwoven fabric, spunbond nonwoven fabric, meltblown nonwoven fabric, glass fiber nonwoven fabric, polytetrafluoroethylene membrane (PTFE membrane), thermal bond nonwoven fabric, stitch bond nonwoven fabric, needle punch nonwoven fabric, and spunlace nonwoven fabric are preferred from the viewpoint of ease of handling. In particular, the downstream fiber layer that plays a role in capturing droplet nuclei containing viruses is preferably a meltblown nonwoven fabric, glass fiber nonwoven fabric, or polytetrafluoroethylene membrane (PTFE membrane), and from the viewpoint of having a high collection efficiency against pressure loss, the meltblown nonwoven fabric is preferably an electret nonwoven fabric that has been subjected to electret processing. The meltblown nonwoven fabric and the glass fiber nonwoven fabric preferably have an average fiber diameter of 36 μm or less, more preferably 3 μm or less, which allows for a higher collection efficiency of droplet nuclei containing viruses.
[0017] The antiviral agent may be a known antiviral agent, and examples of such antiviral agents include metal nanoparticles such as silver or copper, silver iodide, silver bromide, silver chloride, silver acetate, silver sulfide, silver peroxide, silver oxide, silver thiocyanide, copper iodide (I), copper bromide (I), copper chloride (I), copper acetate (I), copper sulfide (I), copper peroxide (I), copper oxide (I), copper thiocyanide (I), copper iodide (II), copper bromide (II), copper chloride (II), copper acetate (II), copper sulfide (II), copper peroxide (II), copper oxide (II), and copper thiocyanate (II). Examples of the antiviral agent include supports obtained by adding metals such as silver, copper, and zinc to carriers such as calcium phosphate, zeolite, silica gel, glass, calcium phosphate, zirconium phosphate, calcium silicate, magnesium aluminometasilicate, potassium titanate, and zinc oxide, alcohol compounds, phenol compounds, quaternary ammonium salts, benzoic acids, chlorhexidine, sorbic acids, carboxylic acids, aldehydes, ionic surfactants, plant essential oils, and components or derivatives derived from natural products such as catechins and tannins. One or more types of antiviral agents can be used in combination.
[0018] In particular, antiviral agents having metal atoms are compatible with fibers and are easy to be impregnated or kneaded into them, making them preferable as the antiviral agents of the present invention. In addition, since antiviral agents having metal atoms exert their effects slowly, if the number of contacts with viruses is small, the inactivation of viruses does not progress, whereas, like the inactivation of viruses attached to the filter medium of the present invention, if the number of contacts with viruses is large or the contact is long, the effect is more pronounced.
[0019] Antiviral agents that are ionic organic compounds are also preferred for the present invention. Ionic organic compounds are highly reactive with viruses, and therefore have a high inactivation rate when in contact with viruses. In the present invention, the compounds are uniformly dispersed within the filter medium, allowing for efficient contact with viruses.
[0020] In addition, air filters are replaced or cleaned frequently, and antiviral agents containing natural products such as catechins and tannins or derivatives thereof, which are less irritating to the skin and have excellent safety, are also preferred in the present invention.
[0021] The antiviral agent used in the present invention preferably has antibacterial properties, mold resistance or antiallergenic properties.This can suppress the growth of bacteria and mold attached to the fiber that constitutes filter material, and inactivate allergens, thereby suppressing the adverse effects on human body caused by bacteria, mold, and allergens that are re-released from air filter.In particular, the bacteria and mold attached to fiber can reach the downstream side of the fiber layer by growth, and at this time, even during ventilation through air filter, the bacteria and mold on the downstream side are released into the air, which causes bacteria and mold to be released to the downstream side of air purifier, which becomes a problem.
[0022] Furthermore, if the antiviral agent further has antibacterial, fungal resistance, or antiallergenic properties, it is not necessary to add a different substance to exhibit these properties, and therefore there is no possibility of functional degradation due to interactions between the antiviral agent and different substances, which is preferable.
[0023] Further, as antiviral agents having antibacterial properties, compounds having metal atoms such as silver-copper-supported zeolite and silver-zinc-supported zeolite can be mentioned.Further, as antiviral agents having mold resistance, organic compounds having ionic properties such as quaternary ammonium salts can be mentioned.Further, as antiviral agents having antiallergenic properties, natural plant extracts such as tannic acid or derivatives thereof can be mentioned.
[0024] In addition, in the laminated filter material for air filters of the present invention, the upstream fiber layer preferably contains silver-copper zeolite and silver-zinc zeolite, and the total adhesion rate of the silver-copper zeolite and silver-zinc zeolite in the upstream fiber layer is 0.3 mass% or more and 10 mass% or less.By making the total adhesion rate of the silver-copper zeolite and silver-zinc zeolite in the upstream fiber layer 0.3 mass% or more, the upstream fiber layer can exhibit sufficient antiviral properties, and by making it 10 mass% or less, it is advantageous in terms of compatibility such as reaction with other drugs in the drug impregnation processing solution and prevention of aggregation, and is advantageous in terms of economic efficiency by saving the amount of antiviral drug used.
[0025] In addition, in the laminated filter material for air filters of the present invention, the downstream fiber layer preferably contains copper compound, and the copper content of the downstream fiber layer is 0.05% by mass or more and 1.0% by mass or less.By making the downstream fiber layer contain the copper compound with a copper content of 0.05% by mass or more, the downstream fiber layer can exhibit sufficient antiviral properties, and by making it 1.0% by mass or less, the downstream fiber layer can prevent thread breakage during spinning, which is advantageous in terms of processability, and is advantageous in terms of economy due to the reduction in the amount of antiviral drug used.
[0026] In addition, in the present invention, the upstream fiber layer and downstream fiber layer may have functional agents with antibacterial properties, mold resistance or antiallergenic properties in addition to the antiviral agent.This can suppress the growth of bacteria and mold attached to the fiber that constitutes the filter medium, and inactivate allergens, thereby suppressing the adverse effects on human body caused by bacteria, mold, and allergens that are re-released from air filter.In particular, the bacteria and mold attached to fiber may reach the downstream side of the fiber layer due to growth, and in this case, even during ventilation through the air filter, the bacteria and mold on the downstream side are released into the air, which causes bacteria and mold to be released to the downstream side of the air purifier, which becomes a problem.
[0027] The antibacterial agent may be a known antibacterial agent, and examples thereof include inorganic antibacterial agents such as metal nanoparticles such as zinc, zeolite, silica gel, glass, calcium phosphate, zirconium phosphate, calcium silicate, magnesium aluminometasilicate, potassium titanate, supports in which a metal such as zinc is attached to a carrier such as zinc oxide, metal oxides such as zinc oxide and titanium dioxide, carbamates such as 3-iodo-2-propynyl butylcarbamate, benzalkonium chloride, and the like.
[0028] The antifungal agent may be a known antifungal agent, for example, benzimidazole-based agents such as 2-(4-thiazolyl)-benzimidazole (thiabendazole) and methyl-2-benzimidazole carbamate (carbendazim), sulfamide-based agents such as N-dichlorofluoromethylthio-N',N'-dimethyl-N-phenylsulfamide (dichlohlanide) and N-dichlorofluoromethylthio-N',N'-dimethyl-Np-tolylsulfamide (trifluanid), 2-bromo-2-nitropropane-1,3-diol, orthophenylphenol, etc. In addition, some of the above-mentioned antibacterial agents have mold resistance, and these can also be used appropriately.
[0029] The antiallergen agent may be a known antiallergen agent, and examples of such antiallergen agents include alkaline earth metal salts such as calcium salts and strontium salts, zirconium salts such as zirconyl chloride, zirconium hydroxide, zirconium carbonate, and aluminum salts such as alum and aluminum sulfate. In addition, some of the above-mentioned antibacterial agents and antifungal agents have antiallergenic properties, and these may also be used as appropriate.
[0030] The antiviral agent is dispersed in a sufficiently fine state and is present on the fiber, so that the contact efficiency with the virus is improved compared to the case where the dispersion is insufficient, and the antiviral properties are advantageous in terms of the virus inactivation speed and the high virus inactivation rate in a certain time. A dispersion aid may be used to disperse the antiviral agent in a sufficiently fine state. The dispersion aid may be a commonly used dispersion aid, and examples of the dispersion aid include polycarboxylic acid, naphthalenesulfonic acid formalin condensation, polyethylene glycol, polycarboxylic acid partial alkyl ester, polyether, polyalkylene polyamine, alkyl sulfonic acid, quaternary ammonium, higher alcohol alkylene oxide, polyhydric alcohol ester, polyalkyl polyamine, polyphosphate, carboxymethyl cellulose, polysaccharide, etc.
[0031] In the laminated filter medium for air filters of the present invention, the upstream fiber layer has an average fiber diameter of 20 μm or more and 60 μm or less and a basis weight of 40 g / m 2 More than 110g / m 2 By making the average fiber diameter 20 μm or more and 60 μm or less, sufficient breathability, rigidity, smoothness, ease of folding processing when heated, shape retention when cooled, appropriate dust and airborne dust collection performance, and dust collection and retention performance can be obtained. In addition, the basis weight is 40 g / m 2 More than 110g / m 2 By satisfying the following, it is possible to obtain sufficient breathability and rigidity, appropriate thickness, heating and cooling in a short time, ease of bending when heated, shape retention when cooled, appropriate dust and airborne particle collection performance, and dust collection and retention performance.
[0032] An intermediate layer containing a deodorant having a function of adsorbing or decomposing gas may be disposed between the upstream fiber layer and the downstream fiber layer. The presence of the intermediate layer containing a deodorant makes it possible to remove odorous gas components such as ammonia, toluene, acetic acid, formaldehyde, and acetaldehyde from the air. Examples of deodorants generally include activated alumina, activated carbon, activated carbon fiber, silica gel, and zeolite, and further include deodorants impregnated with acidic or basic chemicals for the purpose of neutralizing and decomposing acidic or basic gases.
[0033] A flame retardant assistant may be used in the upstream fiber layer, downstream fiber layer, and intermediate layer. Typical examples include phosphorus-based flame retardants, nitrogen-based flame retardants, halogen-based flame retardants, bromine-based flame retardants, composites of these, magnesium hydroxide, aluminum hydroxide, antimony-based flame retardants, thermally expandable graphite, and silicone-based flame retardants.
[0034] In the case of a filter medium in which an upstream fiber layer and a downstream fiber layer are bonded, the peel strength of the two layers is preferably 0.5N or more when measured according to JIS L 1086 (2013) standard 7.10.1. By being 0.5N or more, peeling between the upstream fiber layer and the downstream fiber layer is unlikely to occur, and the influence during molding processing and high-order processing is reduced. It is preferable to use an adhesive to bond the upstream fiber layer and the downstream fiber layer, and the adhesive is generally an aqueous system such as polyethylene resin, melamine resin, phenol resin, vinyl acetate resin, etc., a chemical reaction system such as epoxy resin, urethane resin, a solvent system, a hot melt system, etc. In particular, a hot melt adhesive is preferable in terms of process passability, workability, and cost of the filter medium.
[0035] When the filter medium is made up of two layers, an upstream fiber layer and a downstream fiber layer, the adhesive used to bond the upstream fiber layer and the downstream fiber layer is 1.0 to 20.0 g / m 2 It is preferable that the thickness is 1.0 g / m 2 This ensures sufficient adhesion between the upstream and downstream fiber layers, and is 20.0 g / m 2 By setting the thickness to be equal to or less than 1 mm, it is possible to prevent the antiviral agent contained in the upstream fiber layer or the downstream fiber layer from being covered with the adhesive, thereby preventing a decrease in antiviral performance.
[0036] When there is one or more intermediate layers between the upstream fiber layer and the downstream fiber layer, the adhesive is preferably 5% by mass to 40% by mass, more preferably 15% by mass to 40% by mass, based on the basis weight of the intermediate layer. When the adhesive is 5% by mass or more, the adhesion between the upstream fiber layer and the downstream fiber layer becomes more sufficient, and when the adhesive is 40% by mass or less, problems such as a decrease in particle collection efficiency and gas deodorization efficiency due to a large area covered by the surface of the fibers and particles of the upstream fiber layer, downstream fiber layer, and intermediate layer, and an increase in the pressure loss of the filter medium due to an increase in the number of places where the air passage is blocked can be suppressed.
[0037] Regarding the method of impregnating the upstream fiber layer or downstream fiber layer of the present invention, the antiviral agent and the dispersion aid may be mixed in an aqueous solvent in the same bath to prepare a processing liquid, and the processing liquid may be impregnated into the fiber or spray-coated. The antiviral agent and the dispersion aid may be kneaded into other fiber materials and spun. The antiviral agent and the dispersion aid may be mixed into white water in which the fiber is dispersed, and paper may be made. When the fiber layer is subjected to electret processing for the purpose of improving the collection performance, a method in which the antiviral agent and the dispersion aid are kneaded into other fiber materials and spun is preferred. When the electret fiber is coated with a chemical solution from above after the electret processing, the charged fiber surface is covered, and the collection performance is reduced compared to before the chemical solution is coated. When the functional drug is mixed in the same bath as the antiviral agent, it is preferable to impregnate it in a separate process because there is a concern that the drug aggregation may occur if the compatibility between the drugs is poor. When the processing solution is impregnated into the fibers or sprayed onto them, it is preferable to stir the processing solution until just beforehand, which can suppress self-aggregation and aggregation of the antiviral agent.
[0038] Here, the aqueous solvent includes water alone, or an aqueous solution containing a water-soluble organic solvent such as lower alcohols such as methanol and ethanol, lower ketones such as acetone and methyl ethyl ketone, lower carboxylic acids such as acetic acid, and glycols such as ethylene glycol, propylene glycol, and diethylene glycol, and can be selected depending on the type of antiviral agent, etc.
[0039] The method for drying the fiber layer impregnated with the processing liquid is not particularly limited, but a hot air drying method, a Yankee drum method, or the like is preferably adopted. The drying temperature is preferably 100 to 230°C, and more preferably 110 to 150°C. By setting the drying temperature to 100°C or higher, the drying time can be sufficiently shortened. In addition, by setting the drying temperature to 230°C or lower, the decomposition of the antiviral agent, the dispersing agent, and the functional agent can be further suppressed, and the antiviral properties can be fully exhibited.
[0040] The filter material of the present invention is preferably used for air filter applications, particularly as air purifiers such as air cleaners, building air conditioners, automobile cabin air conditioners, home air conditioners, and commercial air conditioners, so that it is preferable that the filter material has good pleat shape retention when processed into pleats, that is, when folded, heated, and cooled.As the stiffness of the filter material, the bending resistance measured by the Gurley method is preferably 150mN or more. EXAMPLES
[0041] The present invention will be specifically described below using examples, but the present invention is not necessarily limited to these.
[0042] [Measurement and evaluation method] (1) Weight The sheet to be evaluated was cut into a size of 316 mm x 316 mm, and the mass was measured to calculate the mass per unit area, i.e., basis weight. Measurements were taken at four locations, and the average value was used as the evaluation value.
[0043] (2) Amount and rate of adhesion The amount of antiviral agent, dispersion aid, other functional agent, dye, or pigment attached to the fiber layer was calculated by subtracting the basis weight of the fiber layer, i.e., the substrate, before the agent-impregnating process from the basis weight of the fiber layer after the agent-impregnating process, and then the total attachment amount was multiplied by the content of each component to calculate the attachment amount of each component.
[0044] The adhesion rate was calculated by dividing the adhesion amount of each component by the basis weight of the substrate.
[0045] (3) Content rate When antiviral agents, dispersion aids, other functional agents, electret additives, etc. are kneaded into the raw resin of fibers, the content is calculated by dividing the weight of the target component in the agent / additive kneaded into the raw material by the weight of the raw resin containing the agent / additive.
[0046] (4) Collection efficiency The filter media was set by sandwiching it between the upper and lower wind tunnels of the measuring device, and the gap between the filter media and the wind tunnel was closed to prevent air leaking. Air was passed through at a suction processing speed of 3.2 m / min, and the number of airborne dust particles with particle sizes of 0.3 μm to 0.5 μm upstream and downstream of the filter media was measured using a particle counter, and the collection efficiency was calculated using the following formula. Collection efficiency (%) = 1-(number of downstream particles / number of upstream particles) x 100 (5) Antiviral test According to JIS L 1922 (2016) (Testing method for antiviral performance of textile products (plaque measurement method)), 0.4 g of sample was placed in a vial, inoculated with 0.2 ml of virus liquid, and left at 25°C for 2 hours. 20 ml of SCDLP medium was then added to wash out the virus from the sample, and the virus infectivity of the washed-out liquid was measured by the plaque measurement method. The antiviral activity value was calculated according to the following formula. For the blank, the same operation as above was carried out without using the sample, and the virus infectivity was calculated. Antiviral activity value = log (blank infectivity after 2 hours of action) - log (sample infectivity after 2 hours of action) A standard cloth (cotton) is generally used as the blank. The type of virus used in the test is influenza virus (H1N1).
[0047] The calculated antiviral activity value was evaluated according to the following criteria. ◎: Antiviral activity value is 3.0 or higher ○: Antiviral activity value is 2.0 or more and less than 3.0 △: Antiviral activity value is 1.0 or more and less than 2.0 ×: Antiviral activity value is less than 1.0 (6) Mold resistance test According to ASTM G 21-15(2021)e1, the samples were inoculated with a mixed spore suspension of mold and incubated at a temperature of 28-30°C and a humidity of 85% or higher for 28 days, after which the growth of mycelium on the surface of the samples was observed with the naked eye and a microscope. Five species of fungi were used for the test: Aspergillus brasiliensis, Talaromyces pinophilus, Chaetomium globosum, Trichoderma virens, and Aureobasidium pullulans.
[0048] The observation results were evaluated according to the following criteria. 0: No mycelial growth observed in sample 1: The sample shows signs of mycelial growth (less than 10% of the total area) 2: The sample has slight mycelial growth (greater than 10% and less than 30% of the total area) 3: Sample has moderate hyphae growth (greater than 30% and less than 60% of the total area) 4: The sample has a large growth of mycelium (greater than 60% of the total area but less than 100%) [Example 1] (Upstream fiber layer) A mixture of 30 parts by mass of polyester staple fiber with a fineness of 17 dtex (polyethylene terephthalate, melting point 265°C), 10 parts by mass of heat-bonded polyester staple fiber with a fineness of 15 dtex (core: polyethylene terephthalate, melting point 265°C, sheath: modified polyester, melting point 110°C), and 60 parts by mass of heat-bonded polyester staple fiber with a fineness of 4.4 dtex (core: polyethylene terephthalate, melting point 265°C, sheath: modified polyester, melting point 180°C) was mixed and passed through a cotton opener and carding machine to spin a web. The web was then cross-lapped and adjusted to the desired basis weight, and passed through an air-through heating furnace on a transport conveyor to produce a web with a basis weight of 80 g / m. 2 Thus, a thermally bonded nonwoven fabric having a thickness of 0.3 mm was obtained.
[0049] A slurry containing silver-copper-supported zeolite and silver-zinc-supported zeolite as antiviral agents ("Agion" (registered trademark) AM Slurry manufactured by Sciessent LLC) was mixed with water to prepare a processing solution, which was then placed in an impregnation tank. The thermal bond nonwoven fabric was passed through the impregnation tank to be impregnated with the processing solution, and then passed through an air-through heating furnace and dried to prepare an upstream fiber layer. The concentration of the processing solution was such that the amount of antiviral agent attached was 1.1 g / m 2 The deposition rate was adjusted to 1.4% by mass. In this case, the deposition rate of the silver-copper-supported zeolite was 0.82% by mass, and the deposition rate of the silver-zinc-supported zeolite was 0.59% by mass.
[0050] (Downstream fiber layer) The fiber raw material is polypropylene resin containing copper iodide (I) dispersed as an antiviral agent, and the fiber is melt-blown to produce a fiber with an average fiber diameter of 2.0 μm and a basis weight of 20 g / m. 2 A nonwoven fabric having the above structure was obtained. Next, the nonwoven fabric was immersed in a water tank to which pure water was supplied, and while the nonwoven fabric was being run, a slit-shaped suction nozzle was brought into contact with the surface of the nonwoven fabric to suck in the water, thereby allowing the water to penetrate the entire surface of the fiber layer, and the fiber layer was dried after draining to obtain an electret downstream fiber layer. The copper (I) iodide content was adjusted to 0.54 mass%, and the copper content was adjusted to 0.18 mass%.
[0051] (Lamination) The upstream fiber layer is coated with a polyethylene hot melt resin at 7.0 g / m 2 After applying heat to melt the mixture, the mixture was brought into contact with the upstream fiber layer, and the fiber layers were bonded together to obtain a filter medium for air filters.
[0052] [Example 2] (Upstream fiber layer) Antiviral agent applied at 1.8g / m 2 An upstream fiber layer was obtained in the same manner as in Example 1, except that the deposition rate of the silver-copper-supported zeolite was 2.3 mass %, the deposition rate of the silver-zinc-supported zeolite was 1.31 mass %, and the deposition rate of the silver-zinc-supported zeolite was 0.94 mass %.
[0053] (Downstream fiber layer) The downstream fiber layer was obtained in the same manner as in Example 1.
[0054] (Lamination) The lamination process was carried out in the same manner as in Example 1.
[0055] [Example 3] (Upstream fiber layer) Thiabendazole (Sumika Environmental Science Co., Ltd.'s Synthol M-30) was used as a fungicide, and was added to the antiviral agent processing solution before processing the substrate, resulting in an antifungal agent adhesion of 0.50 g / m 2 An upstream fiber layer was obtained in the same manner as in Example 1, except that the deposition rate was adjusted to 0.62 mass %.
[0056] (Downstream fiber layer) The downstream fiber layer was obtained in the same manner as in Example 1.
[0057] (Lamination) The lamination process was carried out in the same manner as in Example 1.
[0058] [Example 4] (Upstream fiber layer) Antiviral agent applied at 1.8g / m 2 An upstream fiber layer was obtained in the same manner as in Example 3, except that the deposition rate of the silver-copper-supported zeolite was 2.3 mass %, the deposition rate of the silver-zinc-supported zeolite was 1.31 mass %, and the deposition rate of the silver-zinc-supported zeolite was 0.94 mass %.
[0059] (Downstream fiber layer) The downstream fiber layer was obtained in the same manner as in Example 1.
[0060] (Lamination) The lamination process was carried out in the same manner as in Example 1.
[0061] [Comparative Example 1] (Upstream fiber layer) An upstream fiber layer was obtained in the same manner as in Example 1, except that the post-treatment of the antiviral agent, i.e., the steps of impregnation in a liquid containing an antiviral agent and drying, was not performed.
[0062] (Downstream fiber layer) The downstream fiber layer was obtained in the same manner as in Example 1.
[0063] (Lamination) The lamination process was carried out in the same manner as in Example 1.
[0064] [Comparative Example 2] (Upstream fiber layer) The upstream fiber layer was obtained in the same manner as in Example 1.
[0065] (Downstream fiber layer) A downstream fiber layer was obtained in the same manner as in Example 1, except that no antiviral agent was added to the fiber raw material.
[0066] (Lamination) The lamination process was carried out in the same manner as in Example 1.
[0067] Table 1 shows the results of collection efficiency, antiviral test, and mold resistance test carried out using the upstream fiber layer, downstream fiber layer, and filter media of the examples and comparative examples.
[0068] In Examples 1 to 4, antiviral properties were obtained in the upstream fiber layer and the downstream fiber layer. In Comparative Example 1, antiviral properties were obtained in the downstream fiber layer, but not in the upstream fiber layer. In Comparative Example 2, antiviral properties were obtained in the upstream fiber layer, but not in the downstream fiber layer.
[0069] The upstream fiber layers of Examples 1 to 4 and Comparative Example 2 were given a mold resistance of "0." The upstream fiber layers of Examples 1 and 2 and Comparative Example 2 did not contain thiabendazole, but contained silver-copper zeolite and silver-zinc zeolite, and thus obtained mold resistance.
[0070] Moreover, the downstream fiber layers of Examples 1 to 4 and Comparative Example 1 contained copper (I) iodide, and thus obtained a mold resistance of "0."
[0071] [Table 1] [Explanation of symbols]
[0072] 10: Upstream fiber layer 20: downstream fiber layer P: Wind direction [Industrial Applicability]
[0073] The filter of the present invention can be used as an air filter material for air purifiers, home air conditioners, commercial air conditioners, air conditioners for automobile cabins, air conditioners, and the like.
Claims
1. A laminated filter material for air filters comprising: an upstream fiber layer having antiviral properties and a particle collection efficiency of 10% or less for particles with a particle diameter of 0.3 μm or more and 0.5 μm or less; and a downstream fiber layer having antiviral properties and a particle collection efficiency of 90% or more for particles with a particle diameter of 0.3 μm or more and 0.5 μm or less.
2. 2. The laminated filter medium for air filters according to claim 1, wherein the downstream fiber layer contains a copper compound, and the copper content of the downstream fiber layer is 0.05% by mass or more and 1.0% by mass or less.
3. 3. The laminated filter material for air filters according to claim 1, wherein the upstream fiber layer contains silver-copper zeolite and silver-zinc zeolite, and the total adhesion rate of the silver-copper zeolite and silver-zinc zeolite in the upstream fiber layer is 0.3 mass% or more and 10 mass% or less.
4. The upstream fiber layer has a constituent fiber having an average fiber diameter of 20 μm or more and 60 μm or less and a basis weight of 40 g / m 2 110g / m or more 2 The laminated filter material for air filters according to any one of claims 1 to 3, characterized in that:
Citation Information
Patent Citations
Antiviral substance, antiviral fiber and antiviral fiber structure
JP2011042615A