Vehicle interior material reinforcement sheet and vehicle interior material
A reinforcing sheet made of natural and high-rigidity fibers with vinylon binder fibers addresses non-uniform rigidity and environmental issues in automobile interior materials, ensuring uniform rigidity and recyclability.
Patent Information
- Application Number
- JP2023054758
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing automobile interior materials face challenges in achieving uniform rigidity, are non-environmentally friendly due to glass fiber content, and have poor recyclability, leading to increased industrial waste.
A reinforcing sheet composed of natural fibers, high-rigidity fibers, and vinylon binder fibers, with specific mass percentages and properties, ensuring uniform rigidity and recyclability, and avoiding glass fiber usage.
The reinforcing sheet provides uniform rigidity, improved moldability, and environmental friendliness, allowing for thermal recycling and reducing industrial waste.
Smart Images

Figure 2024142572000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a reinforcing sheet for automobile interior materials and to an automobile interior material. [Background technology]
[0002] Automotive interior materials are required to have various performance characteristics such as strength, productivity, processing stability, etc. Furthermore, due to the recent growing interest in environmental protection, there is a demand for weight reduction to improve fuel efficiency and reduction of environmental load by reducing industrial waste. Conventionally, a product having a laminate in which a glass chopped strand mat is bonded to both sides of a polyurethane foam sheet has been used as an automobile interior material. While this product is excellent in strength, productivity, etc., it is difficult to reduce the weight while maintaining the strength because of the use of glass fiber. In addition, there are problems such as a deterioration of the working environment during the manufacturing process of the automobile interior material, and the inclusion of glass fiber makes thermal recycling impossible, so that the product must be landfilled as industrial waste.
[0003] Patent Document 1 proposes an automobile interior material that is lightweight and has shape stability by using a nonwoven fabric that uses vinylon fiber as a replacement for glass fiber as a reinforcing sheet. In Patent Document 1, long fiber vinylon fiber and low melting point polyester fiber are used as raw materials, but it is proposed to control the state of the strands of vinylon fiber bundled together to obtain shape stability, and also to adjust the fineness and fiber length of the vinylon fiber to enhance the reinforcing effect. However, the presence of vinylon fiber strands results in high rigidity in the part where the strands are present and low rigidity in the part where they are not, which causes the problem of non-uniform rigidity of the reinforcing sheet. Patent Document 2 proposes a nonwoven fabric made from natural fibers, polyester fibers, and vinylon fibers as a reinforcing sheet. This reinforcing sheet has a problem that it will tear when laminated with a polyurethane foam sheet and hot press molded as it is, but this is solved by making linear or other cuts in the reinforcing sheet to ensure elongation. However, when the reinforcing sheet is cut and then hot press molded, there are parts where the reinforcing sheet stretches during molding and the rigidity is reduced, resulting in a problem of non-uniform rigidity of the reinforcing sheet. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2010-188894 A [Patent Document 2] JP 2012-41657 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a reinforcing sheet for automobile interior materials made of environmentally friendly materials that allows the production of automobile interior materials having uniform rigidity, and to provide automobile interior materials having this reinforcing sheet. [Means for solving the problem]
[0006] The means for solving the problems of the present invention are as follows. 1. Contains natural fibers, high-rigidity fibers, and vinylon binder fibers. A reinforcing sheet for automobile interior materials, comprising 9 to 30 mass % of the vinylon binder fiber relative to all fibers. 2. The reinforcing sheet for automobile interior materials according to 1., wherein the high-rigidity fibers include vinylon fibers. 3. A reinforcing sheet for automobile interior materials according to 1., wherein the high stiffness fiber comprises vinylon fiber produced by a solvent-wet cooling gel spinning method. 4. The reinforcing sheet for automobile interior materials according to any one of 1. to 3., further comprising high melting point fibers. 5. The reinforcing sheet for automobile interior materials according to any one of 1. to 4., containing 10 to 40 mass % of the natural fibers and 20 to 60 mass % of the high stiffness fibers based on the total fibers. 6. Grammage is 20g / m 2 ~60g / m 2 6. The reinforcing sheet for automobile interior materials according to any one of 1. to 5., 7. An automobile interior material having a reinforcing sheet according to any one of 1. to 6. adhered to at least one surface of a sheet material. In this specification, the expression "A to B (A and B are numerical values)" means a numerical range including both ends, that is, A or more and B or less. Effect of the Invention
[0007] The reinforcing sheet for automobile interior materials of the present invention can be incinerated as industrial waste. The reinforcing sheet for automobile interior materials of the present invention has practical performance in terms of rigidity and moldability in addition to being lightweight and environmentally friendly. The reinforcing sheet for automobile interior materials of the present invention has uniform rigidity throughout the sheet, is not damaged (tear of the reinforcing sheet) during hot press molding for forming the automobile interior material, and has excellent processability and productivity. In addition, the automobile interior material using the reinforcing sheet for automobile interior materials of the present invention has uniform rigidity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Reinforcement sheet for automotive interior materials The reinforcing sheet for automobile interior materials (hereinafter also referred to as reinforcing sheet) of the present invention contains natural fibers, high-rigidity fibers, and vinylon binder fibers, and contains 9 to 30 mass % of the vinylon binder fibers based on the total fibers. The reinforcing sheet of the present invention is a component for automobile interior materials that is adhered to at least one surface of a sheet material made of a polyurethane foam sheet or the like, and is laminated, for example, in the following order: back surface protective material made of a film, nonwoven fabric, etc. / reinforcing sheet / sheet material / reinforcing sheet / surface layer made of urethane, cloth, woven fabric, nonwoven fabric, etc., and then hot press molded to form automobile interior materials such as ceiling materials and door trims.
[0009] (Natural Fibers) Natural fibers improve the dispersibility of the raw material slurry in the raw material composition of the reinforcing sheet, enabling stable production. The content of natural fibers relative to the total fibers constituting the reinforcing sheet is not particularly limited, but is preferably 10% by mass or more and 40% by mass or less. If the content of natural fibers is less than 10% by mass, the papermaking properties may be affected, such as the transfer of wet paper during papermaking of the reinforcing sheet may be deteriorated, and in addition, bundling fibers may be easily generated in the raw material slurry, which may affect the formability due to the deterioration of the texture of the reinforcing sheet and the decrease in strength uniformity. If the content of natural fibers is more than 40% by mass, the blending rate of synthetic fibers (fibers other than natural fibers) is low, so the stiffness of the reinforcing sheet may decrease and the reinforcing sheet may be damaged by tensile stress during hot press molding. The content of natural fibers is more preferably 15% by mass or more, and more preferably 30% by mass or less.
[0010] As the natural fiber, fibers derived from plants, microorganisms, and animals can be used without any particular limitation.Specific examples include natural cellulose such as pulp, cellulose produced by microorganisms such as acetic acid bacteria, mercerized pulp obtained by treating cellulose with a high concentration alkali, regenerated cellulose obtained by dissolving cellulose in a solvent such as a cuprammonium solution or a morpholine derivative and then reprecipitating, cellulose-based fibers such as various cellulose derivatives such as acetylated modified cellulose and carboxylated modified cellulose, and animal hair such as silk, wool, and goat hair, and one or more of these can be used.
[0011] The natural fibers used in the present invention are preferably cellulosic fibers, and more preferably pulp. Examples of pulp include chemical pulp of wood pulp, mechanical pulp of wood pulp, and non-wood pulp obtained from sisal, Manila hemp, and kenaf. Examples of chemical pulp include bleached hardwood kraft pulp (LBKP), bleached softwood kraft pulp (NBKP), unbleached hardwood kraft pulp (LUKP), and unbleached softwood kraft pulp (NUKP). Examples of mechanical pulp include refiner ground pulp (RGP), chemi-ground pulp (CGP), thermo-ground pulp (TGP), and ground pulp (GP). Among pulps, chemical pulp is preferred because it is easy to obtain and process, and relatively high paper strength can be obtained, and bleached softwood kraft pulp (NBKP) is more preferred. In addition, the Canadian standard freeness of the pulp is preferably 300 ml or more and 500 ml or less. The ratio of pulp to all natural fibers is preferably 60% by mass or more, the ratio of chemical pulp to all natural fibers is preferably 60% by mass or more, and the ratio of NBKP to all natural fibers is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more.
[0012] (High stiffness fiber) In this specification, a high-rigidity fiber means a fiber having an elastic modulus of 200 cN / dtex or more. The elastic modulus of the high-rigidity fiber is preferably 210 cN / dtex or more, more preferably 220 cN / dtex or more, even more preferably 230 cN / dtex or more, even more preferably 250 cN / dtex or more, and even more preferably 300 cN / dtex or more. High-rigidity fibers have excellent rigidity in themselves and do not melt during heat press molding. High-rigidity fibers are blended as an alternative to glass fibers, and do not melt or soften under the heating conditions when the reinforcing sheet and the sheet material are bonded and molded by heat press, providing rigidity to the reinforcing sheet and the automobile interior material.
[0013] The content of the high-rigidity fibers in the total fibers constituting the reinforcing sheet is not particularly limited, but is preferably 20% by mass or more and 60% by mass or less. If the content of the high-rigidity fibers is less than 20% by mass, the rigidity required for the reinforcing sheet may not be ensured. If the content is more than 60% by mass, bundling fibers are likely to occur in the raw material slurry, which may deteriorate the texture of the reinforcing sheet and affect the moldability. The content of the high-rigidity fibers is more preferably 30% by mass or more, and more preferably 50% by mass or less.
[0014] The type of high-rigidity fiber is not particularly limited, and examples thereof include aramid fibers such as Kevlar (registered trademark), carbon fibers, and vinylon fibers. One or more of these can be used. Among these, it is preferable to use vinylon fibers. Vinylon fibers are synthetic fibers obtained by acetalizing polyvinyl alcohol, and are manufactured by wet spinning and dry spinning. Vinylon fibers have excellent strength and heat resistance, and do not melt during hot press molding due to their high softening temperature. As vinylon fibers, any known fiber can be used without any particular limitation, but vinylon fibers manufactured by the solvent wet cooling gel spinning method, which is a spinning method developed by Kuraray Co., Ltd., are preferred because they have a uniform structure with a perfectly circular cross section and are stronger.
[0015] The proportion of vinylon fibers to the total high-rigidity fibers is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more. Also, the proportion of vinylon fibers produced by solvent-wet cooling gel spinning to the total high-rigidity fibers is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more.
[0016] The fiber diameter of the vinylon fiber (solvent wet cooling gel spinning vinylon fiber) is preferably 10 dtex or more and 30 dtex or less. If the fiber diameter is less than 10 dtex, it may be difficult to ensure the rigidity of the fiber, and if the fiber diameter exceeds 30 dtex, the total number of fibers may be reduced, resulting in a decrease in the rigidity of the reinforcing sheet. The fiber diameter is more preferably 15 dtex or more, and more preferably 25 dtex or less. The fiber length of the vinylon fiber (solvent wet cooling gel spinning vinylon fiber) is preferably 5 mm or more and 20 mm or less. If the fiber length is less than 5 mm, it may be difficult to increase the rigidity of the reinforcing sheet, and if it exceeds 20 mm, the fibers may become entangled and the uniformity of the reinforcing sheet may decrease. The fiber length is more preferably 7 mm or more and more preferably 18 mm or less.
[0017] (Vinylon binder fiber) The present invention includes at least vinylon binder fibers as binder fibers, which can be produced by injecting an aqueous solution of polyvinyl alcohol into a saturated solution of sodium sulfate, followed by dehydration and coagulation. When the reinforcing sheet is made into paper, the vinylon binder fiber melts due to the moist heat of the dryer part and forms bonds with other fibers. Also, when the reinforcing sheet is hot-press molded, the vinylon binder fiber softens and stretches, supporting the deformation of the reinforcing sheet, preventing the rising parts of the molded body (parts with high tensile stress) from becoming see-through or breaking, resulting in an automobile interior material with uniform rigidity.
[0018] The content of vinylon binder fiber in the total fibers constituting the reinforcing sheet is 9% by mass or more and 30% by mass or less. If the content of vinylon binder fiber is less than 9% by mass, the number of bonding points with natural fibers or high-rigidity fibers decreases, resulting in a decrease in tensile strength. In addition, the reinforcing sheet does not stretch sufficiently at the rising portion of the molded body during press molding, making it easy for "see-through" and "tears" to occur. If the content of vinylon binder fiber is more than 30% by mass, the vinylon binder fiber sticks to the dryer surface of the papermaking machine during papermaking of the reinforcing sheet, making it difficult to papermake the reinforcing sheet. The content of vinylon binder fiber is more preferably 13% by mass or more, and more preferably 25% by mass or less.
[0019] In the present invention, binder fibers other than vinylon binder fibers may be included. As other binder fibers, known binder fibers such as PVA-based binder fibers and polyester-based binder fibers can be used without any particular restrictions. However, the proportion of vinylon binder fibers to the total binder fibers is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more.
[0020] The fiber diameter of the vinylon binder fiber is preferably 0.3 dtex or more and 5 dtex or less, more preferably 0.44 dtex or more, and more preferably 3 dtex or less, from the viewpoints of dispersibility, papermaking property, etc. The fiber length of the vinylon binder fiber is preferably from 1 mm to 8 mm, more preferably from 2 mm or more, and more preferably from 4 mm or less, from the viewpoints of dispersibility, papermaking properties, etc.
[0021] (High melting point fiber) In the present invention, in addition to the natural fiber, the high-rigidity fiber, and the vinylon binder fiber, a high-melting fiber can be further blended. As the high-melting fiber, one that does not melt under the heating and pressure treatment conditions during the hot press processing of the reinforcing sheet and the sheet material and does not reduce the thickness (bulk) of the reinforcing sheet can be used, and for example, one or more of main polyester fiber (PET fiber), main polypropylene fiber (PP fiber), polyphenylene sulfide fiber (PPS fiber), rayon fiber, etc. can be used. The melting point of the high-melting fiber is preferably 160°C or higher, more preferably 200°C or higher, and even more preferably 230°C or higher. As the high-melting fiber, one having a fiber diameter of 1 to 5 dtex and a fiber length of about 4 to 10 mm can be used. In addition, the high-melting fiber can be blended within a range that does not reduce the rigidity of the reinforcing sheet. The reinforcing sheet of the present invention may contain fibers other than those described above, but the proportion of glass fibers to the total fibers constituting the reinforcing sheet is preferably 1 mass % or less, more preferably 0.5 mass % or less, and most preferably zero.
[0022] (optional ingredient) The reinforcing sheet of the present invention may contain optional components within a range that does not impair the intended effects of the present invention, in addition to fibers such as natural fibers, high-rigidity fibers, vinylon binder fibers, and any high-melting-point fibers. Examples of the optional components include dry strength agents such as polyacrylamide, wet strength agents such as polyamide epichlorohydrin and melamine resin, retention aids such as polyethylene oxide, fixing agents such as aluminum sulfate, dispersants, defoamers, release agents, flame retardants, preservatives, antifungal agents, and deodorizers.
[0023] (Basic weight) The basis weight of the reinforcing sheet can be appropriately adjusted depending on the desired performance of the interior material. For example, 2 More than 60g / m 2 A low basis weight is preferred for reducing the weight of automotive interior materials, but a basis weight of 20 g / m or less is preferred. 2 If the basis weight is lower than 60 g / m, the reinforcing sheet may break during press molding due to a decrease in strength.2 A basis weight higher than this is disadvantageous in terms of reducing the weight of automotive interior materials. 2 More preferably, 55 g / m 2 The following is more preferred: (Thickness) The thickness of the reinforcing sheet can be adjusted appropriately depending on the desired performance of the interior material, but for example, a thickness of 100 μm or more and 300 μm or less is preferable. In order to reduce the thickness of the automobile interior material, a thin thickness is preferable, but if the thickness is thinner than 100 μm, the reinforcing sheet may break during press molding due to a decrease in strength. Furthermore, if the thickness is thicker than 300 μm, when bonding with an adhesive, the amount of adhesive required increases, resulting in high costs. The thickness of the reinforcing sheet is more preferably 120 μm or more, and more preferably 250 μm or less.
[0024] (Tensile strength) The tensile strength of the reinforcing sheet, measured according to JIS-P8113 (2006) "Paper and paperboard -- Test methods for tensile properties, Part 2: Constant speed extension method", is preferably 20N / 50mm or more. If the tensile strength is less than 20N / 50mm, the reinforcing sheet may be prone to "see-through" or "tears" at the rising part of the molded product due to the tensile stress during heat press molding. (Tensile elongation at break) The tensile breaking elongation of the reinforcing sheet, measured in accordance with JIS-P8113 (2006) "Testing method for tensile strength of paper and paperboard", is preferably 2.0% or more. If the tensile breaking elongation is less than 2.0%, the reinforcing sheet may be prone to "see-through" or "tears" at the rising portion of the molded product due to the tensile stress during hot press molding. (Clark is scary) The Clark stiffness of the reinforcing sheet measured in accordance with JIS-P8143 (2009) "Paper - Stiffness test method - Clark stiffness tester method" is 30 cm 3 Clark's fear is 30cm. 3 If the ratio is less than 100 / 100, the rigidity of the automobile interior material after hot press molding cannot be ensured, and the shape stability may deteriorate.
[0025] Manufacturing method of reinforcing sheet The method for producing the reinforcing sheet is not particularly limited, and a method used in known papermaking applications can be used. Specifically, the reinforcing sheet can be produced using a Fourdrinier paper machine, a cylinder paper machine, a short wire paper machine, a twin-wire paper machine, an on-top hybrid paper machine, a gap former machine, or the like. The reinforcing sheet exerts its strength by the binder fibers being melted by heat treatment in the drying step to bond between the fibers, or by forming bonding points with other fibers in the case of vinylon binder fibers by melting with moist heat.
[0026] "Automotive interior materials" The reinforcing sheet of the present invention is used for automobile interior materials. In the case of automobile interior materials, reinforcing sheets are attached to both sides of a sheet material, and the reinforcing sheet of the present invention only needs to be attached to at least one side of the sheet material, and is preferably attached to both sides. Adhesion can be performed using an adhesive, or heat sealing can be performed using the heat amount of the vinylon binder fiber during heat pressing and the moisture of the constituent materials, or a hot melt film or hot melt nonwoven fabric can be sandwiched between the sheet material and the reinforcing sheet and heat fused.
[0027] Sheet material As the sheet material, any sheet material used for automobile interior materials can be used without any particular limitation, and examples thereof include foamed polyurethane sheets, foamed polyethylene sheets, foamed polypropylene sheets, foamed polystyrene sheets, rubber sponges, etc. ·glue When an adhesive is used, any adhesive used in automotive interior materials applications can be used without any particular limitation. For example, an isocyanate adhesive, a phenol adhesive, a melamine adhesive, a synthetic rubber-based solvent-type adhesive, an acrylic emulsion adhesive, a synthetic rubber-based hot melt adhesive, a urethane emulsion adhesive, or a heat seal adhesive containing a thermoplastic resin such as an ethylene-vinyl acetate copolymer, vinyl acetate or a copolymer thereof, a polyolefin-based copolymer, or a polyester-based copolymer can be used. EXAMPLES
[0028] Example 1 The fibers used were 18% by mass of bleached softwood kraft pulp (NBKP, freeness 370mlCSF), a natural fiber, 32% by mass of vinylon fiber (VPKW1702, 17dtex, 12mm, manufactured by Kuraray Co., Ltd.) produced by solvent wet cooling gel spinning as a high-rigidity fiber, 15% by mass of vinylon binder fiber (VPB107-1Hx3, 1.2dtex, 3mm, manufactured by Kuraray Co., Ltd.), and 35% by mass of main PET fiber (3.3dtex, 5mm, manufactured by Teijin Co., Ltd.) as a high-melting-point fiber. In addition, 3% of a dispersant was added to the synthetic fiber (fiber other than natural fiber), and 4% of an antifoaming agent was added to the synthetic fiber to adjust the raw material slurry. From this raw material slurry, the target basis weight after drying is 30 g / m 2 Wet paper was hand-made to obtain a sheet with a thickness of 100 mm, which was then pressed and dried in a cylindrical dryer at 105°C to produce a reinforcing sheet.
[0029] Example 2 A reinforcing sheet was produced in the same manner as in Example 1, except that the blending amount of the vinylon binder fiber was 20 mass % and the blending amount of the high melting point fiber was 30 mass %.
[0030] Comparative Example 1 A reinforcing sheet was produced in the same manner as in Example 1, except that the blending amount of the vinylon binder fiber was 5 mass % and the blending amount of the high melting point fiber was 45 mass %. Comparative Example 2 A reinforcing sheet was produced in the same manner as in Example 1, except that the blending amount of the vinylon binder fiber was 8 mass % and the blending amount of the high melting point fiber was 42 mass %.
[0031] Comparative Example 3 A reinforcing sheet was produced in the same manner as in Example 1, except that 40% by mass of core-sheath polyester binder fiber (Melty 4080, 2.2 dtex, 5 mm, manufactured by Unitika Ltd.) was used instead of the vinylon binder fiber, and the amount of polyester fiber was 10% by mass. Comparative Example 4 A reinforcing sheet was produced in the same manner as in Comparative Example 3, except that 25% by mass of core-sheath polyester binder fiber (Melty 4080) was blended and 25% by mass of polyethylene / polypropylene composite fiber (RCE, 1.7 dtex, 5 mm, manufactured by Ube Exsymo Co., Ltd.) was used instead of the high melting point fiber. This reinforcing sheet was further heat-treated in a cylindrical dryer at 160°C.
[0032] <Physical property evaluation> The physical properties of the reinforcing sheets obtained in the examples and comparative examples were measured by the following methods. The results are shown in Table 1. ·Basic weight Measurements were made in accordance with JIS-P8124 (2011) "Paper and paperboard -- Method of measurement of basis weight." Thickness Measurements were performed in accordance with JIS-P8118 (2014) "Paper and paperboard -- Test methods for thickness, density and specific volume." ·density Measurements were made in accordance with JIS-P8124 (2011) "Paper and paperboard -- Determination of basis weight" and JIS-P8118 (2014) "Paper and paperboard -- Determination of thickness, density and specific volume".
[0033] Tensile strength Measurements were performed in accordance with JIS-P8113 (2006) "Paper and paperboard - Test methods for tensile properties, Part 2: Constant speed extension method." Measurement conditions: Test speed 20 mm / min, initial span 180 mm, test piece width 50 mm. Tensile elongation at break Measurements were performed in accordance with JIS-P8113 (2006) "Testing method for tensile strength of paper and paperboard." Measurement conditions: test speed 20 mm / min, initial span 180 mm, test piece width 50 mm. Clark is scared Measurements were made in accordance with JIS-P8143 (2009) "Paper - Stiffness test method - Clark stiffness tester method." Measurement conditions: Test piece width 15 mm
[0034] ·Processability (formability) Circular samples with a diameter of 60 mm were cut out from each of the reinforcing sheets obtained in the examples and comparative examples and from the sheet material (foamed polyurethane sheet, thickness 5 mm). These were laminated in the order of reinforcing sheet / sheet material / reinforcing sheet, sandwiched between a metal holder having a circular die hole with a diameter of 47 mm, and heat-treated for 15 minutes in a hot air dryer at 130°C or 160°C. At this time, the reinforcing sheet and the sheet material were thermally fused by the binder fibers in the reinforcing sheet. Immediately after the heat treatment, a punch with a diameter of 45 mm was pressed into the die hole to a depth of 7 mm for press molding. The obtained molded article was visually observed for tears due to breakage at the rising portion of the molded article and transparency caused by stretching, and was evaluated according to the following criteria. ◯: No cracks or transparency in the molded product. ×: The molded product has cracks or is transparent.
[0035] [Table 1]
[0036] The reinforcing sheet of the present invention had a low basis weight and was lightweight, yet had good moldability in thermocompression molding. [Industrial Applicability]
[0037] Automotive interior materials using the reinforcing sheet of the present invention can provide molded articles having uniform stiffness without breaking during hot press molding. In addition, since the reinforcing sheet of the present invention does not use glass fibers, it can be suitably used for applications such as lightweight and environmentally friendly automotive interior materials.
Claims
1. Contains natural fibers, high-rigidity fibers, and vinylon binder fibers. A reinforcing sheet for automobile interior materials, comprising 9 to 30 mass % of the vinylon binder fiber relative to the total mass of the fibers.
2. 2. The reinforcing sheet for automobile interior materials according to claim 1, wherein the high-rigidity fiber comprises vinylon fiber.
3. 2. The reinforcing sheet for automobile interior materials according to claim 1, wherein the high-rigidity fiber comprises vinylon fiber produced by a solvent-wet cooling gel spinning method.
4. 2. The reinforcing sheet for automobile interior materials according to claim 1, further comprising high melting point fibers.
5. 2. The reinforcing sheet for automobile interior materials according to claim 1, comprising 10 to 40 mass % of said natural fibers and 20 to 60 mass % of said high-rigidity fibers based on the total amount of fibers.
6. Basis weight: 20 g / m 2 ~60g / m 2 2. The reinforcing sheet for automobile interior materials according to claim 1, which is
7. 7. An automobile interior material comprising a sheet material and the reinforcing sheet according to claim 1 adhered to at least one surface of the sheet material.
Citation Information
Patent Citations
Method for producing greenhouse rear wall board by using automobile interior trimming leftover materials
CN109183206A
High-strength special paper processing technology
CN110373926A
Sheet for molding, molded article produced from said sheet and production thereof
JP1989056738A
Filter medium for liquid filtration and production process of the same
JP2002085918A
Nonwoven fabric, interior materials and method for producing the same