Anti-ultraviolet breathable polyester fiber fabric and preparation method thereof
By adding anti-UV modifiers and hydroxyethyl methacrylate to polyester fibers and combining electrospinning technology, the problem of insufficient anti-UV performance and moisture absorption of polyester fibers in summer and outdoor applications is solved, and the fabric is realized. Excellent breathable and moisture permeability and antibacterial effects, improving the comfort and health and safety of clothing.
Patent Information
- Application Number
- CN202410662163.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-05-27
AI Technical Summary
Polyester fibers have insufficient UV resistance in summer and outdoor applications, poor hydrophilicity leads to insufficient moisture absorption and breathability, and are prone to adsorbing bacteria, posing a threat to human health and safety.
Using aqueous solution polymerization and electrospinning technology, the addition of anti-UV modifiers and copolymerization with hydroxyethyl methacrylate, the modified polyester fiber is prepared and blended with natural fibers, and the use of quaternary ammonium antibacterial monomers and mesoporous oxidation Zinc nano glue enhances the UV resistance, breathability and antibacterial properties of fabrics.
It achieves excellent breathable and moisture permeability of the fabric and anti-ultraviolet effect, while also having good antibacterial properties, improving the comfort and health and safety of the clothing.
Smart Images

Figure BDA0004860012950000081 
Figure BDA0004860012950000091 
Figure BDA0004860012950000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyester fiber fabrics, and particularly relates to an anti-ultraviolet breathable polyester fiber fabric and a preparation method thereof. Background Art
[0002] Polyester fiber is a synthetic fiber obtained by spinning polyester formed by the polycondensation of organic dibasic acid and diol, referred to as PET fiber. Due to its excellent modulus, strength, elasticity, shape retention and heat resistance, polyester fiber has become one of the most widely used and consumed chemical fiber varieties, accounting for more than 50% of the total textile fiber. It is often used in home furnishings, clothing, industrial textiles and other fields, and is also one of the commonly used fabrics for summer clothing.
[0003] When used as summer and outdoor fabrics, there are certain requirements for UV protection performance, but the anti-UV performance of polyester fiber itself is insufficient and cannot meet people's needs for summer and outdoor fabrics. Moreover, compared with natural fibers and some chemical fibers, polyester fiber has poor hydrophilicity, resulting in insufficient moisture absorption and breathability, which easily produces a stuffy feeling during wearing, reducing the comfort of clothing. In addition, due to the high surface area of the fiber, textiles made of polyester fiber are easy to absorb bacteria during wearing, and the bacteria will grow and multiply rapidly under nutritional conditions such as human sweat, causing harm to human health and safety. Summary of the invention
[0004] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide an anti-ultraviolet breathable polyester fiber fabric and a preparation method thereof. The modified polyester fiber is prepared by combining aqueous solution polymerization and electrospinning technology, and the added anti-ultraviolet modifier is copolymerized with hydroxyethyl methacrylate. The prepared fabric exhibits excellent air permeability and moisture permeability, and also has excellent anti-ultraviolet and antibacterial effects.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] An anti-ultraviolet breathable polyester fiber fabric, comprising modified polyester fiber and natural fiber, wherein the modified polyester fiber comprises the following components in parts by weight: 50-70 parts of PET chips, 10-25 parts of anti-ultraviolet modifier, 3-8 parts of hydroxyethyl methacrylate, 2-5 parts of polyvinyl alcohol, 0.5-5 parts of initiator, and 1-3 parts of crosslinking agent;
[0007] The anti-ultraviolet modifier is a composite anti-ultraviolet modifier prepared by grafting titanium dioxide nano-glue with quaternary ammonium salt antibacterial monomer and gamma-methacryloxypropyltrimethoxysilane and then combining with mesoporous zinc oxide.
[0008] Preferably, the natural fiber is any one of cotton and linen; the initiator is any one of potassium persulfate and ammonium persulfate; and the cross-linking agent is glutaraldehyde.
[0009] Preferably, the preparation method of the anti-ultraviolet modifier comprises the following steps:
[0010] A. Mix tetrabutyl titanate, ethanol and deionized water and stir for 15 to 30 minutes, then add acetic acid and continue stirring for 8 to 12 hours to obtain titanium dioxide nanogel;
[0011] B. Place N,N-dimethyloctylamine and toluene solvent in a reactor, pass nitrogen protection, then add 3-chloropropyltrimethoxysilane, place at 75-90°C and stir to react for 24-36 hours. After the reaction is completed, rotary distillation and drying are performed to obtain a quaternary ammonium salt antibacterial monomer;
[0012] C. Add quaternary ammonium salt antibacterial monomer, mesoporous nano zinc oxide and γ-methacryloxypropyltrimethoxysilane to the titanium dioxide nanogel, and react at 40-55° C. for 4-6 hours to obtain an anti-ultraviolet modifier.
[0013] Preferably, the preparation method of the mesoporous nano zinc oxide is specifically as follows: zinc acetate and urea are dissolved in deionized water, sodium dodecyl sulfate is added and stirred, and then acetic acid is added to adjust the pH of the solution to 4-5, and after stirring and mixing for 2-3 hours, the solution is transferred to a hydrothermal kettle and reacted at 80-95°C for 12-24 hours. After the reaction is completed, the solution is filtered, washed, dried and calcined to obtain mesoporous nano zinc oxide.
[0014] Preferably, in step B, the mass ratio of N,N-dimethyloctylamine to 3-chloropropyltrimethoxysilane is 1:1 to 1.4.
[0015] Preferably, in step C, the mass ratio of titanium dioxide nano-gel, quaternary ammonium salt antibacterial monomer, mesoporous nano zinc oxide and γ-methacryloxypropyltrimethoxysilane is 8-12:1-2:2-5:2-4.
[0016] Preferably, the method for preparing the modified polyester fiber comprises the following steps:
[0017] S1, mixing an anti-ultraviolet modifier and hydroxyethyl methacrylate, and then adding polyvinyl alcohol and an initiator to obtain a mixed solution;
[0018] S2, placing the mixed solution at 40-80° C. for polymerization reaction, cooling, and obtaining a polymerization solution;
[0019] S3, using trifluoroacetic acid and dichloromethane as solvent, adding PET slices to dissolve to obtain PET spinning solution;
[0020] S4, adding a polymer solution and a cross-linking agent to the PET spinning solution, and obtaining a mixed spinning solution by degassing;
[0021] S5, subjecting the mixed spinning solution to electrostatic spinning and thermal cross-linking treatment to obtain modified polyester fibers.
[0022] Preferably, the volume ratio of trifluoroacetic acid to dichloromethane is 4:1, and the concentration of the PET spinning solution is 16-25%.
[0023] Preferably, in the electrospinning operation, the voltage is set at 30-34 kV, the propulsion rate is 0.4-0.7 mL / h, and the distance between the nozzle and the receiving roller is 13-17 cm; the thermal crosslinking treatment temperature is 120-160° C., and the time is 30-120 min.
[0024] Preferably, the preparation method of the anti-ultraviolet breathable polyester fiber fabric as described above has the specific operation steps of: blending the modified polyester fiber and the natural fiber to form a double-layer weaving, and the mass ratio of the modified polyester fiber to the natural fiber is 80:10-20.
[0025] Beneficial effects of the present invention:
[0026] The invention uses N, N-dimethyl n-octylamine and 3-chloropropyltrimethoxysilane to synthesize a quaternary ammonium salt antibacterial monomer, and then adds the quaternary ammonium salt antibacterial monomer, mesoporous nano zinc oxide and γ-methacryloxypropyltrimethoxysilane to titanium dioxide nano glue, and the silicon hydroxyl groups in the quaternary ammonium salt antibacterial monomer and the γ-methacryloxypropyltrimethoxysilane structure are hydrolyzed to generate hydroxyl groups, which then undergo a condensation reaction with the hydroxyl groups on the surface of nano titanium dioxide, so that the quaternary ammonium salt antibacterial monomer is grafted on the surface of the nano titanium dioxide and a double bond structure is combined, and at the same time, the hydroxyl groups on the surface of the mesoporous nano zinc oxide are combined with the γ-methacryloxypropyltrimethoxysilane, so that the mesoporous nano zinc oxide is bonded to the nano titanium dioxide. The surface of mesoporous nano zinc oxide is grafted with double bonds, and the grafted double bond structure can serve as a bridge for polymerization with hydroxyethyl methacrylate. Nano titanium dioxide and nano zinc oxide, as commonly used inorganic UV shielding agents, can absorb and scatter ultraviolet rays and effectively resist the harm of ultraviolet rays. In addition, the synthesized mesoporous nano zinc oxide has the advantages of being porous and having a large specific surface area, and has good air permeability and moisture permeability, which helps the body to sweat. At the same time, the quaternary ammonium salt functional group in the quaternary ammonium salt antibacterial monomer structure has a broad-spectrum antibacterial effect. Introducing it into the nano titanium dioxide structure can give the fabric a good antibacterial effect. At the same time, the precipitation problem of the antibacterial monomer is avoided due to the strong combination of chemical bonds.
[0027] The present invention uses hydroxyethyl methacrylate, anti-ultraviolet modifier and polyvinyl alcohol as raw materials, adds initiator and crosslinking agent, prepares polymer solution by aqueous solution method, polyvinyl alcohol runs through polymer chain segments to form semi-interpenetrating network structure, improves the spinnability of polymer, and introduces hydroxyethyl methacrylate into the molecular chain of copolymer as hydrophilic component to enhance the hygroscopicity of fabric. The present invention prepares modified polyester fiber by combining aqueous solution polymerization method and electrostatic spinning technology, and then blends the obtained modified polyester fiber with natural fiber. The fabric prepared by the present invention shows excellent air permeability and moisture permeability, and has excellent anti-ultraviolet and antibacterial effects. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The intrinsic viscosity of the PET chips in the embodiments and comparative examples of the present invention is 0.675 dL / g, and they are produced by Jiangsu Silk Group Co., Ltd.
[0030] Example 1 A method for preparing mesoporous nano zinc oxide is specifically as follows:
[0031] Take 1.10g of zinc acetate and 6.01g of urea and dissolve them in 100mL of deionized water, add 0.12g of sodium dodecyl sulfate and stir to mix, then add acetic acid to adjust the pH of the solution to 5, stir and mix for 2h, then move to a hydrothermal autoclave and react at 90°C for 24h. After the reaction is completed, filter, wash, dry, and calcine at 300°C for 0.5h to obtain mesoporous nano zinc oxide.
[0032] Embodiment 2 A method for preparing an anti-ultraviolet modifier comprises the following steps:
[0033] A. Take 24 mL of tetrabutyl titanate, 200 mL of ethanol and 5 mL of deionized water, mix and stir for 30 min, then add 16 mL of acetic acid and continue stirring for 12 h to obtain titanium dioxide nanogel;
[0034] B. Take 10g N, N-dimethyl-n-octylamine and 7.5mL toluene solvent in a reactor, pass nitrogen protection, then add 12g 3-chloropropyltrimethoxysilane, place it at 80°C and stir to react for 36h. After the reaction is completed, rotary distillation and drying are carried out to obtain a quaternary ammonium salt antibacterial monomer;
[0035] C. Add 2g of quaternary ammonium salt antibacterial monomer, 3g of mesoporous nano zinc oxide and 2g of γ-methacryloxypropyltrimethoxysilane to 10g of titanium dioxide nanogel, and react at 45°C for 6h to obtain an anti-ultraviolet modifier.
[0036] Example 3 A modified polyester fiber includes the following components in parts by weight: 50 parts of PET chips, 12 parts of anti-ultraviolet modifier, 3 parts of hydroxyethyl methacrylate, 2 parts of polyvinyl alcohol, 1 part of initiator potassium persulfate, and 1 part of cross-linking agent glutaraldehyde.
[0037] The preparation method of the modified polyester fiber comprises the following steps:
[0038] S1, mixing an anti-ultraviolet modifier and hydroxyethyl methacrylate, and then adding polyvinyl alcohol and an initiator to obtain a mixed solution;
[0039] S2, placing the mixed solution at 65° C. for polymerization reaction, cooling, and obtaining a polymerization solution;
[0040] S3, preparing trifluoroacetic acid-dichloromethane solvent at a volume ratio of 4:1, adding PET slices to dissolve to obtain a PET spinning solution with a concentration of 18%;
[0041] S4, adding a polymer solution and a cross-linking agent to the PET spinning solution, and obtaining a mixed spinning solution by degassing;
[0042] S5. Place the mixed spinning solution in an electrospinning machine, set the voltage to 32 kV, the propulsion rate to 0.5 mL / h, adjust the distance between the nozzle and the receiving roller to 15 cm, perform electrospinning to obtain spun fibers, place the spun fibers at 140° C. for thermal crosslinking treatment for 60 min, and obtain modified polyester fibers.
[0043] A method for preparing an anti-ultraviolet breathable polyester fiber fabric comprises the following specific steps: the modified polyester fiber and cotton fiber are blended and spun into a double-layer fabric, the mass ratio of the modified polyester fiber to the cotton fiber is 80:20, the machine specification of the grey cloth is a warp density of 26 strands / cm, a weft density of 21 strands / cm, and the cotton fiber fineness is 148×2dtex.
[0044] Example 4 A modified polyester fiber includes the following components in parts by weight: 57 parts of PET chips, 20 parts of anti-ultraviolet modifier, 5 parts of hydroxyethyl methacrylate, 3 parts of polyvinyl alcohol, 2 parts of initiator ammonium persulfate, and 2 parts of cross-linking agent glutaraldehyde.
[0045] The preparation method of the modified polyester fiber is the same as that in Example 3.
[0046] A method for preparing an anti-ultraviolet breathable polyester fiber fabric comprises the following specific steps: the modified polyester fiber and cotton fiber are blended and spun into a double-layer fabric, the mass ratio of the modified polyester fiber to the cotton fiber is 80:15, the machine specification of the grey cloth is a warp density of 26 strands / cm, a weft density of 21 strands / cm, and the cotton fiber fineness is 148×2dtex.
[0047] Example 5 A modified polyester fiber includes the following components in parts by weight: 68 parts of PET chips, 25 parts of anti-ultraviolet modifier, 8 parts of hydroxyethyl methacrylate, 4 parts of polyvinyl alcohol, 4 parts of initiator ammonium persulfate, and 3 parts of cross-linking agent glutaraldehyde.
[0048] The preparation method of the modified polyester fiber is the same as that in Example 3.
[0049] A method for preparing an anti-ultraviolet breathable polyester fiber fabric comprises the following specific steps: the modified polyester fiber and cotton fiber are blended and spun into a double-layer fabric, the mass ratio of the modified polyester fiber to the cotton fiber is 80:10, the machine specification of the grey cloth is a warp density of 26 strands / cm, a weft density of 21 strands / cm, and the cotton fiber fineness is 148×2dtex.
[0050] Comparative Example 1 A method for preparing an anti-ultraviolet modifier comprises the following steps:
[0051] A. Take 24 mL of tetrabutyl titanate, 200 mL of ethanol and 5 mL of deionized water, mix and stir for 30 min, then add 16 mL of acetic acid and continue stirring for 12 h to obtain titanium dioxide nanogel;
[0052] B. Take 10g N, N-dimethyl-n-octylamine and 7.5mL toluene solvent in a reactor, pass nitrogen protection, then add 12g 3-chloropropyltrimethoxysilane, place it at 80°C and stir to react for 36h. After the reaction is completed, rotary distillation and drying are carried out to obtain a quaternary ammonium salt antibacterial monomer;
[0053] C. Add 2 g of quaternary ammonium salt antibacterial monomer and 2 g of γ-methacryloxypropyltrimethoxysilane to 10 g of titanium dioxide nanogel, and react at 45° C. for 6 h to obtain an anti-ultraviolet modifier.
[0054] Comparative Example 2 A method for preparing an anti-ultraviolet modifier comprises the following steps:
[0055] A. Take 24 mL of tetrabutyl titanate, 200 mL of ethanol and 5 mL of deionized water, mix and stir for 30 min, then add 16 mL of acetic acid and continue stirring for 12 h to obtain titanium dioxide nanogel;
[0056] B. Take 10g N, N-dimethyl-n-octylamine and 7.5mL toluene solvent in a reactor, pass nitrogen protection, then add 12g 3-chloropropyltrimethoxysilane, place it at 80°C and stir to react for 36h. After the reaction is completed, rotary distillation and drying are carried out to obtain a quaternary ammonium salt antibacterial monomer;
[0057] C. Add 3g of mesoporous nano zinc oxide and 2g of γ-methacryloxypropyltrimethoxysilane to 10g of titanium dioxide nanogel, and react at 45°C for 6h to obtain an anti-ultraviolet modifier.
[0058] Comparative Example 3: A modified polyester fiber includes the following components in parts by weight: 68 parts of PET chips, 25 parts of the anti-UV modifier prepared in Comparative Example 1, 8 parts of hydroxyethyl methacrylate, 4 parts of polyvinyl alcohol, 4 parts of initiator ammonium persulfate, and 3 parts of cross-linking agent glutaraldehyde.
[0059] The preparation method of the modified polyester fiber is the same as that in Example 3.
[0060] The preparation method of a UV-resistant breathable polyester fiber fabric is the same as that of Example 5.
[0061] Comparative Example 4: A modified polyester fiber includes the following components in parts by weight: 68 parts of PET chips, 25 parts of the anti-UV modifier prepared in Comparative Example 2, 8 parts of hydroxyethyl methacrylate, 4 parts of polyvinyl alcohol, 4 parts of initiator ammonium persulfate, and 3 parts of cross-linking agent glutaraldehyde.
[0062] The preparation method of the modified polyester fiber is the same as that in Example 3.
[0063] The preparation method of a UV-resistant breathable polyester fiber fabric is the same as that of Example 5.
[0064] Performance Testing
[0065] The fabrics prepared in Examples 3-5 and Comparative Examples 3-4 were subjected to the following performance tests:
[0066] (1) UV protection performance test: UV-2000F ultraviolet transmittance analyzer was used to perform UV protection test in accordance with GB / T6505-2009 standard. Test method: Select a flat part of fabric at least 5 cm away from the edge of the fabric, cut a 5 cm × 5 cm sample, test its ultraviolet protection factor (UPF), and adjust the sample position so that each sample is tested 5-10 times to obtain the average value. Similarly, the UV protection performance under immersion conditions was tested to simulate the effect of human sweating on the fabric's anti-ultraviolet performance. The data results are shown in Table 1.
[0067] Table 1 Test results of anti-ultraviolet performance of samples
[0068]
[0069] It can be seen from the data in Table 1 that the fabric prepared by the present invention has excellent anti-ultraviolet performance. In comparative example 3, mesoporous nano zinc oxide is not added, and its anti-ultraviolet performance is slightly worse than that of examples 3-5, indicating that the synergistic effect of mesoporous nano zinc oxide and nano titanium dioxide can achieve a more excellent anti-ultraviolet effect.
[0070] (2) Air permeability test: The sample was humidified for 24 h under standard atmospheric pressure (20 ± 2 °C, relative humidity 62% to 68%), and then tested using a YG461E air permeability tester (Wenzhou Fangyuan Instrument Co., Ltd.) in accordance with GB / T5453-1997 “Determination of Air Permeability of Textile Fabrics”. The test was repeated 10 times, and the average value was calculated. The data results are shown in Table 2.
[0071] (3) Moisture permeability test: The moisture permeability is measured according to GB / T 12704.1-2009 “Test method for moisture permeability of textile fabrics - Part 1: Moisture absorption method”. A moisture permeability cup filled with desiccant (anhydrous calcium chloride dried at 160°C for 3h) and sealed with a sample is placed in a sealed environment with a temperature of (38±2)°C, a relative humidity of (90±2)% and a certain circulating airflow of (0.3-0.5) m / s. The moisture permeability of the sample is calculated based on the change in the mass of the moisture permeability cup within a specific time. The calculation method is shown in the following formula: T = (Δm-Δm0) / A·t, where: T is the moisture permeability, g / m 2 ·24h; Δm is the difference in mass between two consecutive weighings of the same sample, g; Δm0 is the mass difference of the blank sample, g; A is the effective test area in the sample test, m 2 , this test is 0.00283m 2 , t is the test time, s, and the data results are shown in Table 2.
[0072] Table 2 Test results of air and moisture permeability of samples
[0073]
[0074] It can be seen from the data in Table 2 that the fabric prepared by the present invention has excellent air permeability and moisture permeability. In comparative example 3, no mesoporous nano zinc oxide was added, and its air permeability and moisture permeability were slightly worse than those of examples 3-5, indicating that the porous structure of nano zinc oxide helps the human body to perspire.
[0075] (4) Antibacterial performance test: According to the test standard "GB / T 20944.3-2008-Evaluation of antibacterial properties of textiles Part 3 Oscillation method", the antibacterial rate calculation formula is: Y = (Wt-Qt) / Wt×100%, where: Y-inhibition rate, %; Wt-the number of viable bacteria in the control sample, CFU / mL; Qt-the number of viable bacteria in the test sample, CFU / mL. The data results are shown in Table 3.
[0076] (5) Washing resistance test: According to the 5A procedure of GB / T 8629-2001 standard, the drying procedure was oven drying method, and the data results were shown in Table 3.
[0077] Table 3 Test results of antibacterial properties of samples
[0078]
[0079] It can be seen from the data in Table 3 that the fabric prepared by the present invention has excellent antibacterial properties and water-washing resistance. In Comparative Example 4, no quaternary ammonium salt antibacterial monomer was added, and the measured antibacterial rates of Escherichia coli and Staphylococcus aureus were significantly lower than those of Examples 3-5, indicating that the addition of quaternary ammonium salt antibacterial monomers improved the antibacterial properties and water-washing resistance of the fabric.
[0080] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0081] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A UV-resistant breathable polyester fabric, It is characterized in that The invention comprises modified polyester fiber and natural fiber, wherein the modified polyester fiber comprises the following components in parts by weight: 50-70 parts of PET chips, 10-25 parts of anti-ultraviolet modifier, 3-8 parts of hydroxyethyl methacrylate, 2-5 parts of polyvinyl alcohol, 0.5-5 parts of initiator, and 1-3 parts of crosslinking agent; The anti-ultraviolet modifier is a composite anti-ultraviolet modifier obtained by grafting titanium dioxide nano-gel with quaternary ammonium salt antibacterial monomer and γ-methacryloxypropyltrimethoxysilane and then combining with mesoporous zinc oxide; The preparation method of the anti-ultraviolet modifier comprises the following steps: A. Mix tetrabutyl titanate, ethanol and deionized water and stir for 15-30 min, then add acetic acid and continue stirring for 8-12 h to obtain titanium dioxide nanogel; B. Place N,N-dimethyloctylamine and toluene solvent in a reactor, pass nitrogen protection, then add 3-chloropropyltrimethoxysilane, place at 75-90°C and stir to react for 24-36 hours. After the reaction is completed, rotary distillation and drying are performed to obtain a quaternary ammonium salt antibacterial monomer; C. Add quaternary ammonium salt antibacterial monomer, mesoporous nano zinc oxide and γ-methacryloxypropyltrimethoxysilane to the titanium dioxide nanogel, and react at 40-55° C. for 4-6 hours to obtain an anti-ultraviolet modifier.
2. The UV-resistant breathable polyester fiber fabric according to claim 1, It is characterized in that The natural fiber is any one of cotton and linen; the initiator is any one of potassium persulfate and ammonium persulfate; and the cross-linking agent is glutaraldehyde.
3. The UV-resistant breathable polyester fiber fabric according to claim 1, It is characterized in that The preparation method of the mesoporous nano zinc oxide is specifically as follows: zinc acetate and urea are dissolved in deionized water, sodium dodecyl sulfate is added and stirred, and then acetic acid is added to adjust the pH of the solution to 4-5, and the mixture is stirred for 2-3 hours, then transferred to a hydrothermal kettle and reacted at 80-95° C. for 12-24 hours, and after the reaction is completed, filtered, washed, dried, and calcined to obtain the mesoporous nano zinc oxide.
4. The anti-ultraviolet breathable polyester fiber fabric according to claim 1, It is characterized in that In the step B, the mass ratio of N,N-dimethyl-n-octylamine to 3-chloropropyltrimethoxysilane is 1:1-1.
4.
5. The UV-resistant breathable polyester fiber fabric according to claim 1, It is characterized in that In the step C, the mass ratio of titanium dioxide nano-gel, quaternary ammonium salt antibacterial monomer, mesoporous nano zinc oxide and gamma-methacryloxypropyltrimethoxysilane is 8-12:1-2:2-5:2-4.
6. The UV-resistant breathable polyester fiber fabric according to claim 1, It is characterized in that The preparation method of the modified polyester fiber comprises the following steps: S1, mixing an anti-ultraviolet modifier and hydroxyethyl methacrylate, and then adding polyvinyl alcohol and an initiator to obtain a mixed solution; S2, placing the mixed solution at 40-80° C. for polymerization reaction, cooling, and obtaining a polymerization solution; S3, using trifluoroacetic acid and dichloromethane as solvent, adding PET slices to dissolve to obtain PET spinning solution; S4, adding a polymer solution and a cross-linking agent to the PET spinning solution, and obtaining a mixed spinning solution by degassing; S5, subjecting the mixed spinning solution to electrostatic spinning and thermal cross-linking treatment to obtain modified polyester fibers.
7. The anti-ultraviolet breathable polyester fiber fabric according to claim 6, It is characterized in that The volume ratio of trifluoroacetic acid to dichloromethane is 4:1, and the concentration of the PET spinning solution is 16-25%.
8. The UV-resistant breathable polyester fiber fabric according to claim 6, It is characterized in that The voltage in the electrospinning operation is set to 30-34 kV, the propulsion rate is 0.4-0.7 mL / h, and the distance between the nozzle and the receiving roller is 13-17 cm; the thermal crosslinking treatment temperature is 120-160° C., and the time is 30-120 min.
9. The method for preparing the UV-resistant breathable polyester fiber fabric according to claim 1, It is characterized in that The specific operation steps are: the modified polyester fiber and the natural fiber are blended and spun into double-layer yarns, and the mass ratio of the modified polyester fiber and the natural fiber blend is 80:10-20.
Citation Information
Cited By
Preparation method of high-performance anti-ultraviolet water-repellent polyester fiber
CN122039429A