Polycarbonate resin and method for producing the same and polycarbonate resin molded product

A polycarbonate resin with specific structural units and production methods enhances optical properties, heat resistance, and mechanical strength, addressing the limitations of conventional resins for high-temperature applications.

JP2024142583AInactive Publication Date: 2024-10-11MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2023054783
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional polycarbonate resins made from bisphenol A fail to meet the requirements of high optical properties, heat resistance, and mechanical strength needed for applications in high-temperature environments, such as automotive lenses.

Method used

A polycarbonate resin containing a structural unit represented by formula (1) with an intrinsic viscosity of 0.30 or more, a refractive index of 1.590 or more, and a glass transition temperature of 145°C or higher, produced using a dihydroxy compound like bis(4-hydroxyphenyl)diphenylsilane through a melt transesterification method.

Benefits of technology

The resin achieves excellent optical properties, heat resistance, and mechanical strength, making it suitable for high-temperature applications like automotive lenses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142583000001
    Figure 2024142583000001
  • Figure 2024142583000002
    Figure 2024142583000002
  • Figure 2024142583000003
    Figure 2024142583000003
Patent Text Reader

Abstract

To provide a polycarbonate resin that exhibits superior optical properties and delivers superior heat resistance and mechanical strength, and a polycarbonate resin molded product.SOLUTION: A polycarbonate resin is synthesized through an ester exchange reaction, for example, between a carbonate ester and a dihydroxy compound, such as bis(4-hydroxyphenyl)diphenylsilane and bis(4-hydroxyphenyl)diphenylgermane in molten conditions. The polycarbonate resin has an intrinsic viscosity [η] of 0.30 or more as measured in chloroform at 25°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polycarbonate resin having excellent optical properties, heat resistance and mechanical strength, a method for producing the same, and a polycarbonate resin molded article. [Background technology]

[0002] Polycarbonate resin has excellent mechanical strength, electrical properties, transparency, etc., and is widely used as an engineering plastic in various fields such as electrical and electronic equipment and the automotive field. For example, due to its excellent transparency, dimensional stability, mechanical properties, etc., it is used as an optical molding material.

[0003] In recent years, in these application fields, there is a demand for materials that are excellent in optical properties, heat resistance, and mechanical strength. Currently, the most commonly used polycarbonate resin is a polycarbonate resin made from bisphenol A, but it is difficult for conventional polycarbonate resins made from bisphenol A to meet these requirements. In order to meet various requirements, various polycarbonate resins made from monomers other than bisphenol A have also been proposed.

[0004] Patent Document 1 discloses a polycarbonate resin that mainly contains repeating units having a 9,9-bisphenylfluorene skeleton as a polycarbonate resin having excellent optical properties.

[0005] On the other hand, Non-Patent Documents 1 to 3 disclose methods for synthesizing polymers from bisphenols having specific structures containing Si or Ge using various phase transfer catalysts under phase transfer conditions. Non-Patent Documents 1 and 2 discuss differences in phase transfer catalysts in polymer synthesis. Non-Patent Document 3 also discusses the thermal behavior of polymers synthesized from bisphenols having specific structures containing Si or Ge. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 10-101787 [Non-patent literature]

[0007] [Non-Patent Document 1] Journal of Macromolecular Science, Pure and Applied Chemistry, A37(9), 997-1008 (2000). [Non-Patent Document 2] Journal of Inorganic and Organometallic Polymers, 13(1), 21-28 (2003). [Non-Patent Document 3] International Journal of Polymeric Materials, 52(5), 373-386 (2003). Summary of the Invention [Problem to be solved by the invention]

[0008] In the examples of Patent Document 1, a polycarbonate resin is prepared using 2,2'-[9H-fluoren-9-ylidenebis(4,1-phenyleneoxy)]-bisethanol [9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (abbreviation: BPEF)] as a polymerization component. The glass transition temperature of the polycarbonate resin described in Patent Document 1 is about 140 to 145°C. However, it may not be applicable to applications (for example, vehicle-mounted lenses, etc.) where production or use in a high-temperature environment is expected.

[0009] Non-Patent Document 1 discloses a method for synthesizing a polymer using a bisphenol compound having a specific structure containing Si or Ge, and Non-Patent Document 2 discloses a method for synthesizing a copolymer polycarbonate of bisphenol A and a bisphenol compound having a specific structure containing Si or Ge. However, the intrinsic viscosity of the obtained polymer is relatively small, and no mention is made of the heat resistance or optical properties.

[0010] Non-Patent Document 3 discloses the glass transition temperature of a polymer using a bisphenol compound having a specific structure containing Si or Ge, but the heat resistance is not sufficient and there is no mention of the optical properties.

[0011] The present invention has been made in view of the above problems, and an object of the present invention is to provide a polycarbonate resin having excellent optical properties, as well as excellent heat resistance and mechanical strength, a production method thereof, and a polycarbonate resin molded article. [Means for solving the problem]

[0012] The present inventors have conducted extensive research to solve the above problems, and have found that the following invention meets the above object, thereby completing the present invention. That is, the present invention resides in the following [1] to

[12] .

[0013] [1] A polycarbonate resin containing a structural unit (A) represented by the following formula (1), and having an intrinsic viscosity [η] measured in chloroform at 25°C of 0.30 or more: [ka] (In formula (1), R 1 ~R 18 each independently represents a hydrogen atom or an alkyl group having 1 to 15 carbon atoms. X represents Si or Ge. [2] In the formula (1), R 9 ~R 18 is a hydrogen atom. [3] In the formula (1), R 1 ~R8 are each independently a hydrogen atom or a methyl group. [4] In the formula (1), R 1 ~R 8 is a hydrogen atom. [5] The polycarbonate resin according to any one of [1] to [4] above, wherein in formula (1), X is Si. [6] The polycarbonate resin according to any one of [1] to [5] above, which contains 20 mol % or more of the structural unit (A). [7] The polycarbonate resin according to any one of [1] to [6] above, having a refractive index nD of 1.590 or more. [8] The polycarbonate resin according to any one of [1] to [7] above, having a glass transition temperature of 145°C or higher. [9] The polycarbonate resin according to any one of [1] to [8] above, further comprising a structural unit (B) represented by the following formula (2): [ka] (In formula (2), R 20 ~R 21 each independently represents a hydrogen atom, an alkyl group having 1 to 15 carbon atoms, or an aryl group having 6 to 26 carbon atoms; Y represents -CR 22 R 23 -(R 22 , R 23 each independently represents a hydrogen atom, an alkyl group having 1 to 15 carbon atoms, or an aryl group having 6 to 26 carbon atoms, a cycloalkylidene group having 3 to 15 carbon atoms, or a 9,9-fluorenylidene group.

[10] A method for producing a polycarbonate resin, comprising producing the polycarbonate resin according to any one of [1] to [9] above using a dihydroxy compound represented by the following formula (1a): [ka] (In formula (1a), R 1 ~R 18each independently represents a hydrogen atom or an alkyl group having 1 to 15 carbon atoms. X represents Si or Ge.

[11] A polycarbonate resin molded product comprising the polycarbonate resin according to any one of [1] to [9] above.

[12] The polycarbonate resin molded article according to

[11] above, which is an optical component. Effect of the Invention

[0014] According to the present invention, there are provided a polycarbonate resin having excellent optical properties, heat resistance and mechanical strength, a production method thereof, and a polycarbonate resin molded article. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The following describes in detail an embodiment of the present invention. The following description of the constituent elements is an example (representative example) of an embodiment of the present invention, and the present invention is not limited to the following content unless the gist of the present invention is changed.

[0016] <Polycarbonate resin> The present invention relates to a polycarbonate resin (hereinafter, sometimes referred to as the "polycarbonate resin of the present invention") that contains a structural unit (A) represented by the following formula (1) and has an intrinsic viscosity [η] measured in chloroform at 25°C of 0.30 or more.

[0017] [ka]

[0018] In formula (1), R 1 ~R 18 each independently represents a hydrogen atom or an alkyl group having 1 to 15 carbon atoms. X represents Si or Ge.

[0019] Structural units The structural unit (A) is a structural unit represented by the above formula (1). In the above formula (1), R 1 ~R 18each independently represents a hydrogen atom or an alkyl group having 1 to 15 carbon atoms.

[0020] In the above formula (1), R 1 ~R 18 The alkyl group represented by the formula (I) may be linear, branched, or cyclic. The alkyl group may be unsubstituted or may have a substituent. The number of carbon atoms in the alkyl group is 1 to 15, preferably 1 to 10, and more preferably 1 to 5. The number of carbon atoms in the alkyl group means the number of carbon atoms in the alkyl group including the substituent, and when the alkyl group has a substituent, it is the total number of carbon atoms in the substituent and the number of carbon atoms in the alkyl group.

[0021] R 1 ~R 18 Examples of the alkyl group represented by the formula (I) include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an n-hexyl group, a cyclohexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, an n-pentadecyl group, and the like, as well as these groups having a substituent.

[0022] Among these, in order to improve the refractive index of the resulting polycarbonate resin, R 9 ~R 18 is preferably a hydrogen atom.

[0023] In order to improve the refractive index of the resulting polycarbonate resin, R 1 ~R 8 is preferably each independently a hydrogen atom or a methyl group, and more preferably all of them are hydrogen atoms.

[0024] In the above formula (1), X represents Si or Ge, with Si being preferred.

[0025] The polycarbonate resin of the present invention may be a homopolymer of the structural unit (A) or a copolymer containing the structural unit (A) and a structural unit other than the structural unit (A). In addition, the other structural unit may be a single structure or may contain two or more different structures.

[0026] The content of the structural unit (A) (the ratio of the structural unit (A) to the total structural units in the polycarbonate resin of the present invention) may be determined depending on the form of the polycarbonate resin, etc., but is preferably 20 mol% or more, more preferably 30 mol% or more. If the structural unit (A) is too small, the optical properties may be insufficient. The upper limit of the content of the structural unit (A) is not particularly limited, but is usually 100 mol% or less, 90 mol% or less, etc.

[0027] The structural unit (A) may be a single structure or may contain two or more different structures represented by the above (1). When the structural unit (A) contains two or more different structures represented by the above (1), the content of the structural unit (A) is the total content of the two or more different structural units represented by the above (1).

[0028] [Other structural units] As described above, the polycarbonate resin of the present invention may contain other structural units than the structural unit (A), and the structure is not particularly limited. The other structural units may be structures other than carbonate structural units, but the other structural units are preferably carbonate structural units derived from aliphatic and / or aromatic dihydroxy compounds other than the dihydroxy compound that is the raw material of the structural unit (A). For example, the other structural units may include the structural unit (B) represented by the following formula (2).

[0029] [ka]

[0030] In the above formula (2), R 20 ~R 21each independently represents a hydrogen atom, an alkyl group having 1 to 15 carbon atoms, or an aryl group having 6 to 26 carbon atoms; Y represents -CR 22 R 23 -(R 22 , R 23 each independently represents a hydrogen atom, an alkyl group having 1 to 15 carbon atoms, or an aryl group having 6 to 26 carbon atoms; ), a cycloalkylidene group having 3 to 15 carbon atoms, or a 9,9-fluorenylidene group.

[0031] The number of carbon atoms in an alkyl group, an aryl group, or a cycloalkylidene group means the number of carbon atoms in the group including the substituent, and when the group has a substituent, the number of carbon atoms in the substituent is the total of the number of carbon atoms in the group.

[0032] In the above formula (2), R 20 ~R 21 The alkyl group represented by the formula (I) may be unsubstituted or substituted. It may be linear, branched, or cyclic. The number of carbon atoms in the alkyl group is 1 to 15, preferably 1 to 10, and more preferably 1 to 5.

[0033] R 20 ~R 21 Examples of the alkyl group represented by the formula (I) include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an n-hexyl group, a cyclohexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, an n-pentadecyl group, and the like, as well as these groups having a substituent.

[0034] In the above formula (2), R 20 , R 21 The aryl group represented by the following formula may be unsubstituted or may have a substituent. The number of carbon atoms in the aryl group is 6 to 26, preferably 6 to 20, and more preferably 6 to 15. Examples of the aryl group include groups such as a phenyl group and a naphthyl group, and these groups having a substituent, and are preferably substituted or unsubstituted phenyl groups.

[0035] In the above formula (2), "-CR 22 R 23 -"R 22 , R 23 R each independently represents a hydrogen atom, an alkyl group having 1 to 15 carbon atoms, or an aryl group having 6 to 26 carbon atoms. 22 , R 23 The alkyl group represented by the formula (2) is R 20 , R 21 The alkyl group represented by R 22 , R 23 The aryl group represented by R 20 , R 21 The above is the same as the aryl group represented by the following formula:

[0036] In the above formula (2), the cycloalkylidene group represented by Y may have a branched structure and may be unsubstituted or substituted. The number of carbon atoms in the cycloalkylidene group is 3 to 15, and preferably 5 to 10. Examples of the cycloalkylidene group represented by Y include a cyclopentylidene group and a cyclohexylidene group.

[0037] In the above formula (2), the 9,9-fluorenylidene group represented by Y may be unsubstituted or may have a substituent.

[0038] In the above formula (2), R 20 , R 21 are each preferably independently a hydrogen atom or a methyl group, and R 20 is a hydrogen atom, and R 21 More preferably, is a hydrogen atom or a methyl group.

[0039] In the above formula (2), Y is -CR 22 R 23 - is preferably a 2,2-propylidene group (-CR 22 R 23 -R 22 and R 23 is a methyl group) is more preferred.

[0040] (Resin additives) The polycarbonate resin of the present invention may contain various resin additives as necessary, and may contain one type or two or more types of resin additives, so long as the desired physical properties are not significantly impaired. Examples of resin additives include heat stabilizers, antioxidants, release agents, light resistance agents (HALS), flame retardants, antistatic agents, antifogging agents, lubricants, antiblocking agents, flow improvers, plasticizers, dispersants, antibacterial agents, dyes, pigments, etc.

[0041] (intrinsic viscosity) The polycarbonate resin of the present invention has an intrinsic viscosity [η] (hereinafter simply referred to as "intrinsic viscosity") of 0.30 or more, measured in chloroform at 25°C. By including the structural unit (A) represented by the above formula (1) and having an intrinsic viscosity of 0.30 or more, the polycarbonate resin can have excellent optical properties, heat resistance, and mechanical strength. The intrinsic viscosity is preferably 0.35 or more, more preferably 0.40 or more. The upper limit is not particularly limited, but is preferably 0.85 or less, more preferably 0.70 or less. The method for measuring the intrinsic viscosity is as described in the examples below.

[0042] (Refractive Index) The refractive index (nD) of the polycarbonate resin of the present invention is preferably 1.590 or more, more preferably 1.600 or more, and even more preferably 1.605 or more. There is no particular upper limit, but it can be 1.700 or less, 1.650 or less, etc. The refractive index (nD) is a refractive index at a wavelength of 589 nm measured at 20°C, and the measurement method is as described in the examples below.

[0043] (glass transition temperature) The glass transition temperature (Tg) of the polycarbonate resin of the present invention is preferably 145 to 170°C, more preferably 145 to 165°C. If the glass transition temperature is too low, the heat resistance may be insufficient depending on the usage environment. On the other hand, if the glass transition temperature is too high, the melting temperature becomes high, and the resin is easily decomposed or discolored during molding, which is not preferable. Therefore, the glass transition temperature is preferably within the above range. The method for measuring the glass transition temperature is as described in the examples below.

[0044] (Production of polycarbonate resin) The method for producing the polycarbonate resin of the present invention is not particularly limited as long as it can produce the polycarbonate resin of the present invention, and it can be produced by a known polymerization method. The polymerization method is not particularly limited, but examples thereof include melt transesterification, interfacial polymerization, pyridine method, ring-opening polymerization of cyclic carbonate compounds, and solid-phase transesterification of prepolymers.

[0045] The polycarbonate resin of the present invention can usually be produced using a dihydroxy compound represented by the formula (1a) described later. Among them, the melt transesterification method is one of the preferred methods for producing the polycarbonate resin of the present invention, since it is easy to obtain a resin having an intrinsic viscosity of 0.30 or more.

[0046] The melt transesterification method will be specifically described below.

[0047] (Melt transesterification method) In the melt transesterification method, for example, a carbonate ester and a dihydroxy compound are subjected to a transesterification reaction in a molten state to obtain a polycarbonate resin. That is, the polycarbonate resin of the present invention can be produced by reacting a dihydroxy compound including a dihydroxy compound represented by the following formula (1a) with a carbonate ester by the melt transesterification method.

[0048] (Dihydroxy Compounds) The polycarbonate resin of the present invention can be produced by using a dihydroxy compound represented by the following formula (1a) as the dihydroxy compound.

[0049] [ka]

[0050] The dihydroxy compound represented by the above formula (1a) is a dihydroxy compound corresponding to the structural unit (A) represented by the above formula (1), and R 1 ~R 18 and X have the same meaning as in the above formula (1), and the preferred embodiments are also the same.

[0051] Specific examples of the dihydroxy compound represented by the above formula (1a) include bis(4-hydroxyphenyl)diphenylsilane and bis(4-hydroxyphenyl)diphenylgermane.

[0052] In addition, when a copolymer containing a structural unit other than the structural unit (A) is to be obtained, the copolymer can be produced by using a dihydroxy compound corresponding to the other structural unit in addition to the dihydroxy compound represented by the above formula (1a). Examples of the dihydroxy compound used to introduce the other structural unit include the dihydroxy compound represented by the following formula (2a).

[0053] [ka]

[0054] The dihydroxy compound represented by the above formula (2a) is a dihydroxy compound corresponding to the structural unit (B) represented by the above formula (2), and R 20 , R 21 and Y have the same meaning as in formula (2) above, and the preferred embodiments are also the same.

[0055] Specific examples of the dihydroxy compound represented by the above formula (2a) include 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane, 9,9-bis(4-hydroxyphenyl)fluorene, and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene.

[0056] (carbonate ester) The carbonate ester is not particularly limited, but examples thereof include diaryl carbonates, dialkyl carbonates, biscarbonates of dihydroxy compounds, monocarbonates of dihydroxy compounds, and carbonates of dihydroxy compounds such as cyclic carbonates. Of these, the compound represented by the following formula (3) is preferred.

[0057] [ka]

[0058] In the above formula (3), R 30 and R 31 each independently represents an alkyl group having 1 to 15 carbon atoms or an aryl group having 6 to 26 carbon atoms.

[0059] In the above formula (3), R 30 and R 31 The alkyl group represented by the formula (I) may be linear, branched, or cyclic. The alkyl group may be unsubstituted or may have a substituent. The number of carbon atoms in the alkyl group (including the number of carbon atoms in the substituent when the alkyl group has a substituent) is 1 to 15, preferably 1 to 10, and more preferably 1 to 5.

[0060] In the above formula (3), R 30 and R 31 The aryl group represented by the following formula (1) may be unsubstituted or substituted. The aryl group has 6 to 26 carbon atoms (including the carbon number of the substituent when the aryl group has a substituent), preferably 6 to 20 carbon atoms, and more preferably 6 to 15 carbon atoms.

[0061] Among these, from the viewpoint of reactivity with a dihydroxy compound, the carbonate ester is more preferably a diaryl carbonate which may have a substituent and is represented by the following formula (4).

[0062] [ka]

[0063] In the above formula (4), R 32 and R 33 each independently represents a halogen atom, a nitro group, a cyano group, a linear alkyl group having 1 to 15 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, a cycloalkyl group having 4 to 15 carbon atoms, an aryl group having 6 to 20 carbon atoms, a carboxylic acid group, an alkoxycarbonyl group having 2 to 20 carbon atoms, or an acyloxy group having 1 to 20 carbon atoms. p and q each independently represent an integer of 0 to 5, each independently being preferably an integer of 0 to 3, and more preferably an integer of 0 to 2.

[0064] Specific examples of the carbonate ester represented by the above formula (3) or (4) include dimethyl carbonate, diethyl carbonate, di-t-butyl carbonate, diphenyl carbonate, bis(4-methylphenyl) carbonate, bis(4-chlorophenyl) carbonate, bis(4-fluorophenyl) carbonate, bis(2-chlorophenyl) carbonate, bis(2,4-difluorophenyl) carbonate, bis(4-nitrophenyl) carbonate, bis(2-nitrophenyl) carbonate, bis(methylsalicylphenyl) carbonate, and ditolyl carbonate, with diphenyl carbonate being preferred. These carbonate esters may be used alone or in combination of two or more.

[0065] The ratio of the dihydroxy compound and the carbonate ester is arbitrary as long as the desired polycarbonate resin can be obtained, but it is preferable to use the carbonate ester in excess of the dihydroxy compound when polymerizing with the dihydroxy compound. The carbonate ester is preferably 1.00 to 1.30 mol, more preferably 1.02 to 1.20 mol, per 1 mol of the dihydroxy compound. If this molar ratio is too small, the terminal OH group of the obtained polycarbonate resin increases, and the thermal stability of the resin tends to deteriorate. On the other hand, if this molar ratio is too large, the reaction rate of the ester exchange decreases, making it difficult to produce a polycarbonate resin having a desired intrinsic viscosity, or the amount of carbonate ester remaining in the resin increases, which may cause odor during molding or when the molded product is formed.

[0066] In addition to the carbonate ester, a dicarboxylic acid or a dicarboxylic acid ester may be used. In this case, it is preferable to use the carbonate ester so that 50 mol % or less is replaced with the dicarboxylic acid or the dicarboxylic acid ester, and it is more preferable to use the carbonate ester so that 30 mol % or less is replaced with the dicarboxylic acid or the dicarboxylic acid ester. Representative dicarboxylic acids or dicarboxylic acid esters include terephthalic acid, isophthalic acid, diphenyl terephthalate, diphenyl isophthalate, etc. When the dicarboxylic acid or dicarboxylic acid ester is replaced, a polyester carbonate is obtained.

[0067] When producing a polycarbonate resin by the melt transesterification method, a transesterification catalyst is usually used. That is, in the presence of the transesterification catalyst, a carbonate ester and a dihydroxy compound are reacted to obtain a polycarbonate resin. The transesterification catalyst is not particularly limited, and a conventionally known catalyst can be used. For example, it is preferable to use an alkali metal compound and / or an alkaline earth metal compound. In addition, a basic compound such as a basic boron compound, a basic phosphorus compound, a basic ammonium compound, or an amine compound may be used in combination as an auxiliary. The transesterification catalyst may be used alone or in combination.

[0068] In the melt transesterification method, the reaction temperature is not particularly limited, but is usually 100 to 300°C. The pressure during the reaction is not particularly limited, but is usually reduced pressure of 2 mmHg or less. In the presence of an alkali catalyst, the polycarbonate resin of the present invention is significantly affected by thermal history and oxidation, which may lead to deterioration of the hue, so it is preferable to select a reaction temperature of 300°C or less, and a reduced pressure condition with a lower limit of about 0.05 mmHg to prevent oxygen from leaking from the equipment due to excessive reduced pressure. As a specific operation, a melt polycondensation reaction may be performed under the above conditions while removing by-products.

[0069] The reaction can be carried out in either a batch or continuous manner. In the case of a batch reaction, the order of mixing the reaction substrate (reaction raw material), catalyst, additives, etc. is arbitrary as long as the desired polycarbonate resin can be obtained, and an appropriate order may be arbitrarily set.

[0070] In the melt transesterification method, a catalyst deactivator may be used as necessary. As the catalyst deactivator, any compound that neutralizes the transesterification catalyst may be used. Examples of the catalyst deactivator include sulfur-containing acidic compounds and their derivatives, phosphorus-containing acidic compounds and their derivatives, etc. One type of catalyst deactivator may be used, or two or more types may be used.

[0071] The amount of the catalyst deactivator used is not particularly limited, but is usually 0.5 equivalents or more, preferably 1 equivalent or more, more preferably 3 equivalents or more, and is usually 50 equivalents or less, preferably 10 equivalents or less, more preferably 8 equivalents or less, relative to the ester exchange catalyst.

[0072] <Polycarbonate resin composition> The polycarbonate resin of the present invention may be used alone, or two or more kinds of the polycarbonate resins of the present invention may be mixed, or the polycarbonate resin of the present invention may be mixed with a resin other than the polycarbonate resin of the present invention, and used as a polycarbonate resin composition.

[0073] Examples of other resins include polycarbonate resins other than the polycarbonate resin of the present invention; thermoplastic polyester resins such as polyethylene terephthalate resin, polytrimethylene terephthalate, and polybutylene terephthalate resin; styrene resins such as polystyrene resin, high impact polystyrene resin (HIPS), acrylonitrile-styrene copolymer (AS resin), acrylonitrile-styrene-acrylic rubber copolymer (ASA resin), and acrylonitrile-ethylene propylene rubber-styrene copolymer (AES resin); polyolefin resins such as polyethylene resin and polypropylene resin; polyamide resins; polyimide resins; polyetherimide resins; polyurethane resins; polyphenylene ether resins; polyphenylene sulfide resins; polysulfone resins; and polymethacrylate resins.

[0074] The polycarbonate resin composition of the present invention is a composition containing two or more of the polycarbonate resins of the present invention or a composition containing the polycarbonate resin of the present invention and another resin. In addition, when the polycarbonate resin of the present invention and another resin are contained, the composition may contain one type of the polycarbonate resin of the present invention or two or more types. The other resin may also contain one type or two or more types. These can be used in any combination or ratio.

[0075] The content of the polycarbonate resin of the present invention in the polycarbonate resin composition of the present invention is not particularly limited, but it is preferable to adjust the ratio according to the proportion of the structural unit (A) in the polycarbonate resin of the present invention. It is preferable that the content of the structural unit (A) of the polycarbonate resin of the present invention in the polycarbonate resin composition of the present invention is 20 mol% or more.

[0076] The polycarbonate resin composition of the present invention may contain one or more resin additives as necessary, so long as the desired physical properties are not significantly impaired. Examples of the resin additives include heat stabilizers, antioxidants, release agents, light resistance agents (HALS), flame retardants, antistatic agents, antifogging agents, lubricants, antiblocking agents, flow improvers, plasticizers, dispersants, antibacterial agents, dyes, pigments, etc.

[0077] (Production of polycarbonate resin composition) The polycarbonate resin composition of the present invention can be produced by a known method. The method for producing the composition is not particularly limited, but methods such as dry blending, melt mixing, and solution mixing can be used.

[0078] <Polycarbonate resin molding> The present invention also relates to a polycarbonate resin molded article containing the polycarbonate resin of the present invention (hereinafter, may be referred to as "molded article of the present invention"). The molded article of the present invention can be obtained by molding the polycarbonate resin of the present invention or the polycarbonate resin composition of the present invention. The molding method is not particularly limited, and known methods such as injection molding and extrusion molding can be used. By selecting a molding method according to the shape, a molded article of any shape can be obtained, such as an injection molded article molded into the shape of various members such as a lens, or an extrusion molded article molded into the shape of a sheet, film, etc.

[0079] The molded article of the present invention is not particularly limited in the form in which it contains the polycarbonate resin of the present invention. The molded article of the present invention may contain the polycarbonate resin of the present invention alone or in combination with another polycarbonate resin.

[0080] The molded article of the present invention can be used for various applications such as electrical and electronic equipment and automobile parts. In particular, the molded article of the present invention has excellent optical properties, heat resistance, and mechanical strength, and is therefore suitable for optical components and components for applications expected to be used in high-temperature environments. Specifically, it can be used as a lens for an in-vehicle camera, a lens for a smartphone camera, a lens for an action camera, and the like. EXAMPLES

[0081] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0082] The physical properties of the polycarbonate resins obtained in the following Examples and Comparative Examples were evaluated by the following methods.

[0083] [1] Intrinsic viscosity ([η]) The polycarbonate resin was dissolved in chloroform (concentration: 3.0 g / L), and the intrinsic viscosity (limiting viscosity) [η] (unit: dL / g) at 25° C. was determined using an Ubbelohde viscosity tube (manufactured by Moritomo Rika Kogyo Co., Ltd.).

[0084] [2] Glass transition temperature (Tg) Using a differential scanning calorimeter (DSC6220 manufactured by SII), about 10 mg of a polycarbonate resin sample was heated at a heating rate of 20°C / min to measure the calorific value, and the extrapolated glass transition onset temperature was determined, which is the temperature at the intersection of a straight line extending the low-temperature baseline to the high-temperature side and a tangent drawn at the point where the gradient of the curve of the stepwise change in the glass transition is maximum, in accordance with ISO 3146. The extrapolated glass transition onset temperature was taken as the glass transition temperature (Tg).

[0085] [3] Refractive index (nD) Approximately 4 g of the resin sample, which had been vacuum-dried at 100°C for 2 hours, was pressed in a heat press using a spacer 8 cm wide, 8 cm long, and 0.5 mm thick at a heat press temperature of 200-250°C, preheated for 1-3 minutes, and pressurized at a pressure of 20 MPa for 1 minute, then removed from the heat press and cooled at room temperature to produce a film with a thickness of 100-300 μm. A rectangular test piece with a length of 40 mm and a width of 8 mm was cut out from this film to be used as a measurement sample. The refractive index nD was measured using a multi-wavelength Abbe refractometer (DRM4 / 1550, manufactured by Atago Co., Ltd.) and an interference filter with a wavelength of 589 nm (D line). The measurement was performed at 20°C using monobromonaphthalene as the interface liquid.

[0086] [Synthesis Example 1] [Synthesis example: Synthesis of bis(4-benzyloxyphenyl)-diphenylsilane (2)]

[0087] [ka]

[0088] A solution of 1-benzyloxy-4-bromobenzene (1) (50 g, 190.02 mmol) in tetrahydrofuran (200 mL) was cooled to -78 °C while stirring under nitrogen atmosphere, and n-butyllithium (2.5 M in hexane, 83.61 mL) was added and stirred at -78 °C for 1 hour. Next, a solution of dichloro(diphenyl)silane (19.25 g, 76.01 mmol) in tetrahydrofuran (100 mL) was added, and the resulting mixture was stirred at 25 °C for 16 hours under nitrogen atmosphere. The progress of the reaction was monitored by TLC (petroleum ether: ethyl acetate = 20:1), and it was found that almost no spots of 1-benzyloxy-4-bromobenzene remained, and several other spots had formed. The reaction mixture was then quenched with 2 L of demineralized water at 0 °C, extracted with 2 L of ethyl acetate, and the organic layer was separated. The resulting organic layer was washed twice with 2 L of demineralized water and then with 200 mL of saturated aqueous sodium chloride solution, and the resulting organic layer was dried by adding anhydrous sodium sulfate. Next, sodium sulfate was removed by filtration, and the filtrate was concentrated under reduced pressure to obtain a crude product. 100 mL of ethyl acetate and 500 mL of n-heptane were added to the crude product, and the mixture was stirred at 25°C for 16 hours. The precipitated crystals were filtered off and dried under reduced pressure at 50°C to obtain a white solid of bis(4-benzyloxyphenyl)-diphenyl-silane (2) (35.8 g, yield 83.26%, HPLC purity 97%).

[0089] Proton Nuclear Magnetic Resonance (hereinafter referred to as " 1 1 H NMR) spectrum was consistent with the desired product.

[0090] 1 H NMR(400MHz,CDCl3) δ=7.59(d,J=6.5Hz,4H),7.52(d,J=8.1Hz,4H),7.49-7.32(m,16H),7.03(d,J=8.3Hz,4H),5.11(s,4H)

[0091] [Synthesis example: Synthesis of bis(4-hydroxyphenyl)diphenylsilane (3)]

[0092] [ka]

[0093] A solution of sodium hydride (10.5 g, 262.42 mmol, 60% purity) and palladium(II) acetate (1.18 g, 5.25 mmol) in N,N-dimethylacetamide (150 mL) was stirred at 25 °C for 5 min under nitrogen atmosphere, and then a solution of bis(4-benzyloxyphenyl)-diphenyl-silane (28.8 g, 52.48 mmol) in N,N-dimethylacetamide (200 mL) was added to the solution. The reaction was then stirred at 50 °C for 16 h. The reaction progress was monitored by TLC (petroleum ether:ethyl acetate=3:1), which showed that bis(4-benzyloxyphenyl)-diphenyl-silane (2) was completely consumed and two new spots were formed. The reaction mixture was then quenched with 2 L of demineralized water, adjusted to pH=4-6 by adding 4 M aqueous HCl, and then extracted twice with 3 L of ethyl acetate. The organic layer was washed three times with 2 L of desalted water and once with 500 mL of saturated aqueous sodium chloride solution, and then anhydrous sodium sulfate was added to the organic layer to dry it. Next, sodium sulfate was removed by filtration, and the filtrate was concentrated under reduced pressure to obtain a crude product. This crude product was purified by silica gel column chromatography (developing solvent n-hexane:ethyl acetate = 80:20), and the resulting solution was concentrated under reduced pressure to obtain a crude product. 450 mL of n-heptane and 90 mL of ethyl acetate were added to this crude product, and after stirring at 25 ° C for 16 hours, the precipitated crystals were filtered off and dried under reduced pressure at 50 ° C to obtain bis(4-hydroxyphenyl)diphenylsilane (3) (17.54 g, yield 90.69%, HPLC purity 99%) as an off-white solid.

[0094] 1 The 1 H NMR spectrum was consistent with the desired product.

[0095] 1 H NMR(400MHz,DMSO-d6)δ=9.70(s,2H),7.51-7.32(m,10H),7.26(d,J=8.4Hz,4H),6.83(d,J=8.4,4H)

[0096] [Example 1] A raw material mixture was prepared by adding 5.18 g (about 0.014 mol) of bis(4-hydroxyphenyl)-diphenylsilane (3) (hereinafter, sometimes abbreviated as "BPPSi") obtained in Synthesis Example 1 above, 4.82 g (about 0.021 mol) of 2,2-bis(4-hydroxyphenyl)propane (BPA) (manufactured by Mitsubishi Chemical Corporation), 7.72 g (about 0.036 mol) of diphenyl carbonate (DPC), and a 0.4 mass% aqueous solution of cesium carbonate as a catalyst to a glass reactor with a capacity of 150 ml equipped with a reactor stirrer, a reactor heating device, and a reactor pressure adjusting device.

[0097] Next, the pressure in the glass reactor was reduced to about 50 Pa (0.38 Torr), and then the operation of returning the pressure to atmospheric pressure with nitrogen was repeated three times to replace the inside of the reactor with nitrogen. After nitrogen replacement, the temperature outside the reactor was set to 220°C, and the temperature inside the reactor was gradually increased to dissolve the mixture. Then, the stirrer was rotated at 100 rpm. Then, the pressure inside the reactor was reduced from 101.3 kPa (760 Torr) to 13.3 kPa (100 Torr) in absolute pressure over 40 minutes while distilling off phenol by-produced by the oligomerization reaction of the dihydroxy compound and DPC inside the reactor.

[0098] Next, the pressure in the reactor was kept at 13.3 kPa, and the transesterification reaction was carried out for 80 minutes while further distilling off phenol. Thereafter, the temperature outside the reactor was raised to 250°C, and the pressure inside the reactor was reduced from 13.3 kPa (100 Torr) to 399 Pa (3 Torr) in absolute pressure over 40 minutes, and the distilled phenol was removed from the system. Furthermore, the temperature outside the reactor was raised to 285°C, and the absolute pressure inside the reactor was reduced to 30 Pa (about 0.2 Torr), and a polycondensation reaction was carried out. The polycondensation reaction was terminated when the agitator of the reactor reached a predetermined stirring power.

[0099] Next, the pressure inside the reactor was restored to 101.3 kPa absolute pressure with nitrogen, and then increased to 0.2 MPa gauge pressure, and the polycarbonate resin was extracted from the reactor.

[0100] The polycarbonate resin thus obtained was subjected to the evaluations according to the procedures described above. The results are shown in Table 1.

[0101] [Example 2] The procedure described in Example 1 was repeated except that the predetermined stirring power was set higher than that in Example 1. The polycarbonate resin thus obtained was subjected to the evaluations according to the procedures described above. The results are shown in Table 1.

[0102] [Example 3] The procedure was the same as in Example 1, except that the raw material mixture was prepared by adding 10.01 g (approximately 0.0271 mol) of BPPSi, 5.96 g (approximately 0.028 mol) of DPC, and a 0.4 mass% aqueous solution of cesium carbonate as a catalyst such that the amount of cesium carbonate was 20 μmol per 1 mol of the total dihydroxy compounds. The polycarbonate resin thus obtained was subjected to the evaluations according to the procedures described above. The results are shown in Table 1.

[0103] [Example 4] The procedure described in Example 3 was repeated except that the predetermined stirring power was set higher than that in Example 3. The polycarbonate resin thus obtained was subjected to the evaluations according to the procedures described above. The results are shown in Table 1.

[0104] [Comparative Example 1] A raw material mixture was prepared by adding 4.94 g (about 0.013 mol) of BPPSi, 3.06 g (about 0.013 mol) of BPA, 5.89 g (about 0.028 mol) of DPC, and a 0.4 mass% aqueous solution of cesium carbonate as a catalyst such that the amount of cesium carbonate was 15 μmol per 1 mol of total dihydroxy compounds. The procedure described in Example 1 was repeated except that the predetermined stirring power was set lower than that in Example 1. The polycarbonate resin thus obtained was subjected to the evaluations according to the procedures described above. The results are shown in Table 2.

[0105] [Comparative Example 2] The procedure described in Example 3 was repeated except that the predetermined stirring power was set lower than that in Example 3. The polycarbonate resin thus obtained was subjected to the evaluations according to the procedures described above. The results are shown in Table 2.

[0106] [Comparative Example 3] The procedure was the same as in Example 1, except that the raw material mixture was prepared by adding 10.00 g (approximately 0.044 mol) of BPA, 9.95 g (approximately 0.046 mol) of DPC, and a 0.4 mass% aqueous solution of cesium carbonate as a catalyst, so that the amount of cesium carbonate was 0.5 μmol per 1 mol of the total dihydroxy compounds. The polycarbonate resin thus obtained was subjected to the evaluations according to the procedures described above. The results are shown in Table 2.

[0107] Tables 1 and 2 show the results of the content of the structural unit (A), the intrinsic viscosity ([η]), the glass transition temperature (Tg), and the refractive index (nD) of Examples 1 to 4 and Comparative Examples 1 to 3. Note that "Not measurable" for the refractive index in Table 2 means that the strength of the film was extremely low and the refractive index could not be measured.

[0108] [Table 1]

[0109] [Table 2]

Claims

1. A polycarbonate resin containing a structural unit (A) represented by the following formula (1), and having an intrinsic viscosity [η] measured in chloroform at 25° C. of 0.30 or more: [Formula 1] (In formula (1), R 1 ~R 18 each independently represents a hydrogen atom or an alkyl group having 1 to 15 carbon atoms; and X represents Si or Ge.

2. In the formula (1), R 9 ~R 18 The polycarbonate resin according to claim 1 , wherein is a hydrogen atom.

3. In the formula (1), R 1 ~R 8 The polycarbonate resin according to claim 1 or 2, wherein each independently represents a hydrogen atom or a methyl group.

4. In the formula (1), R 1 ~R 8 The polycarbonate resin according to claim 3 , wherein is a hydrogen atom.

5. The polycarbonate resin according to claim 1 or 2, wherein in the formula (1), X is Si.

6. The polycarbonate resin according to claim 1 or 2, comprising 20 mol % or more of the structural unit (A).

7. The polycarbonate resin according to claim 1 or 2, having a refractive index nD of 1.590 or more.

8. The polycarbonate resin according to claim 1 or 2, which has a glass transition temperature of 145° C. or higher.

9. The polycarbonate resin according to claim 1 or 2, further comprising a structural unit (B) represented by the following formula (2): [chemical 2] (In formula (2), R 20 ~R 21each independently represents a hydrogen atom, an alkyl group having 1 to 15 carbon atoms, or an aryl group having 6 to 26 carbon atoms; Y is -CR 22 R 23 - (R 22 , R 23 each independently represents a hydrogen atom, an alkyl group having 1 to 15 carbon atoms, or an aryl group having 6 to 26 carbon atoms; ) represents a cycloalkylidene group having 3 to 15 carbon atoms, or a 9,9-fluorenylidene group.

10. A method for producing a polycarbonate resin, comprising producing the polycarbonate resin according to claim 1 or 2 by using a dihydroxy compound represented by the following formula (1a): [C3] (In formula (1a), R 1 ~R 18 each independently represents a hydrogen atom or an alkyl group having 1 to 15 carbon atoms; and X represents Si or Ge.

11. A polycarbonate resin molded article comprising the polycarbonate resin according to claim 1 or 2.

12. The polycarbonate resin molded article according to claim 11, which is an optical member.

Citation Information

Patent Citations

  • Copolycarbonate and its production

    JP1998101787A

Cited By

  • Intrinsic flame-retardant deoxybenzoin-based polycarbonate and preparation method thereof

    CN122255439A