Magnetic bead for extracting biological material
Magnetic beads with a multilayer structure address detachment and dispersibility issues, achieving enhanced extraction efficiency by stabilizing ligands and improving corrosion resistance.
Patent Information
- Application Number
- JP2023054844
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing magnetic beads for biological substance extraction face issues with detachment of bound biological materials and low dispersibility, leading to decreased extraction efficiency.
Magnetic beads with a multilayer structure comprising magnetic metal powder, an inorganic oxide layer, a gold layer, and an immobilization layer with ligand binding sites, enhancing stability and dispersibility.
The multilayer structure prevents detachment of ligands and improves corrosion resistance, ensuring high extraction efficiency and dispersibility of biological substances.
Smart Images

Figure 2024142624000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to magnetic beads for extracting biological substances. [Background technology]
[0002] In recent years, there has been an increasing demand for biological material testing in the fields of medical diagnosis and life science. Among biological material testing methods, the polymerase chain reaction (PCR) method is a method for extracting nucleic acids such as DNA (deoxyribonucleic acid) and RNA (ribonucleic acid) and specifically amplifying and detecting the nucleic acid. In the process of testing such biological materials, it is first necessary to extract the material to be tested from a specimen. To extract this biological material, for example, an extraction carrier having a binding ability to biological materials is used.
[0003] Patent Document 1 gives an example of a ligand as a binding species capable of binding to cell surface receptors or viruses. It discloses that a colloid carrying the ligand is used to detect a biomolecule. It also discloses that a self-assembled monolayer composed of thiols is formed on the surface of a gold-coated particle, and that the self-assembled monolayer presents a binding partner for the ligand. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-122728 A Summary of the Invention [Problem to be solved by the invention]
[0005] In the extraction of biological materials, various physical and chemical loads are applied to the extraction carrier. When such loads are applied to the colloid holding the ligand described in Patent Document 1, there is a concern that the biological material bound to the extraction carrier may be detached or the extraction carrier may aggregate, resulting in a decrease in the extraction efficiency of the biological material. In addition, the colloid described in Patent Document 1 has room for improvement in terms of dispersibility in the dispersion medium. When the dispersibility is low, the capture efficiency of the biological material decreases, and as a result, the extraction efficiency of the biological material decreases.
[0006] Therefore, the realization of magnetic beads for extracting biological substances that can extract biological substances efficiently has become an issue. [Means for solving the problem]
[0007] The magnetic beads for extracting biological material according to the application example of the present invention are: Magnetic metal powder; an inorganic oxide layer that covers the particle surfaces of the magnetic metal powder and contains an inorganic oxide; a base layer that covers a surface of the inorganic oxide layer and contains a reducing agent for gold ions or a catalyst for a reduction reaction of gold ions; a gold layer that covers a surface of the underlayer and contains gold; an immobilization layer comprising a ligand or a compound having a ligand binding site, which is bound to the surface of the gold layer via a Au-S bond; has. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a process diagram illustrating an example of a biological material extraction method. [Diagram 2] FIG. 2 is a schematic diagram for explaining the biological material extraction method shown in FIG. [Diagram 3] FIG. 2 is a schematic diagram for explaining the biological material extraction method shown in FIG. [Figure 4] FIG. 2 is a schematic diagram for explaining the biological material extraction method shown in FIG. [Diagram 5] FIG. 2 is a cross-sectional view showing a magnetic bead according to an embodiment. [Figure 6] FIG. 6 is a partial enlarged view of the coating film shown in FIG. [Figure 7] FIG. 6 is a cross-sectional view showing a modified example of the magnetic bead of FIG. [Figure 8] FIG. 2 is a schematic diagram showing a state in which a compound having a functional site is bound to a gold layer via an Au-S bond. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] BEST MODE FOR CARRYING OUT THE DISCLOSURE Preferred embodiments of the magnetic beads for extracting biological materials according to the present invention will now be described in detail with reference to the accompanying drawings.
[0010] The magnetic beads for extracting biological substances according to the embodiment are a group of particles that adsorb biological substances and are used in magnetic separation in that state. Magnetic separation is a technique for separating the solid phase and the liquid phase by applying an external magnetic field to a vessel containing a solid phase containing the magnetic beads for extracting biological substances and a liquid phase containing a dispersion medium, and magnetically attracting the solid phase. In the following description, the magnetic beads for extracting biological substances may be simply referred to as "magnetic beads."
[0011] Biological materials refer to materials such as nucleic acids such as DNA and RNA, proteins, sugars, various cells such as cancer cells, peptides, bacteria, viruses, etc. Nucleic acids may be present in biological samples such as cells and biological tissues, viruses, bacteria, etc. The biological material extraction method is a method for extracting such biological materials through the steps of dissolution / adsorption, washing, and elution, and the biological materials can be purified and extracted by utilizing the magnetic separation described above in the process.
[0012] 1. Biological material extraction method An example of a method for extracting a biological material using magnetic separation will be described below. Note that in the following description, the biological material is nucleic acid.
[0013] Fig. 1 is a process diagram for explaining an example of a biological material extraction method, Fig. 2 to Fig. 4 are schematic diagrams for explaining the biological material extraction method shown in Fig. 1.
[0014] The biological material extraction method shown in Fig. 1 includes a dissolving / adsorbing step S102, a washing step S108, and an elution step S110. Each step will be described below in order.
[0015] 1.1.Dissolution / adsorption process In the dissolution and adsorption step S102, a specimen containing nucleic acid, a liquid 3 containing a dissolution and adsorption solution, and magnetic beads 2 are placed in a container 1 shown in FIG. 2. The contents of the container 1 are then mixed. As a result, the magnetic beads 2 are dispersed in the liquid 3 in the container 1 as shown in FIG. 2. Since nucleic acids are usually encapsulated in cell membranes and nuclei, the dissolution action of the dissolution and adsorption solution dissolves and removes the so-called outer shell of the cell membrane and nucleus, and the nucleic acid is extracted. The nucleic acid is then adsorbed to the magnetic beads 2 by the adsorption action of the dissolution and adsorption solution.
[0016] As the dissolving / adsorbing liquid, for example, a liquid containing a chaotropic substance is used. The chaotropic substance has the effect of generating chaotropic ions in an aqueous solution, reducing the interaction of water molecules, thereby destabilizing the structure, and contributing to the adsorption of nucleic acids to the magnetic beads 2.
[0017] In addition, when extracting nucleic acids, particularly RNA, it is preferable to make the liquid 3 in the container 1 acidic by adding an acid or the like. Since RNA monomers contain ribose, they are more soluble in polar solvents than DNA. When using this difference to separate RNA and DNA, the outer shell may be dissolved and removed, and then the liquid 3 may be made acidic by adding an acid, for example. Then, a non-polar solvent such as phenol or chloroform is added to the liquid 3. This causes the DNA to move to the non-polar solvent, while the RNA remains in the polar solvent. As a result, the RNA and DNA can be separated, and the RNA can be extracted.
[0018] When extracting RNA, the pH of the liquid 3 in the container 1 is preferably 5.0 or less, more preferably 2.0 to 4.0. This causes the ionization equilibrium of the phosphate groups contained in the RNA to shift toward the hydroxyl groups, making the RNA particularly soluble in polar solvents. This can further increase the efficiency of RNA extraction.
[0019] 1.1.1.Magnetic separation operation In the dissolution / adsorption step S102, an external magnetic field is applied to the magnetic beads 2 with the nucleic acid adsorbed thereon, causing them to be magnetically attracted. This causes the magnetic beads 2 to move to the inner wall of the container 1 and be immobilized thereon. As a result, as shown in FIG. 3, the magnetic beads 2, which are a solid phase, can be separated from the liquid 3, which is a liquid phase. In this specification, the operation of immobilizing the magnetic beads 2 by applying such an external magnetic field is referred to as a "magnetic separation operation."
[0020] Before performing the magnetic separation operation, the contents of the container 1 are stirred as necessary. This increases the probability that the nucleic acid will be adsorbed onto the magnetic beads 2. For stirring, for example, a vortex mixer, manual shaking, pipetting, etc. can be used.
[0021] For example, a magnet 5 disposed on the side of the container is used to apply the external magnetic field. The magnet 5 may be an electromagnet or a permanent magnet. When an external magnetic field acts on the magnetic beads 2, the magnetic beads 2 move toward the magnet 5.
[0022] After the magnetic separation operation, an acceleration may be applied to the container as necessary. This allows the liquid 3 adhering to the magnetic beads 2 to be shaken off, thereby reducing the amount of liquid 3 that has not been separated. The acceleration may be centrifugal acceleration. A centrifuge may be used to apply the centrifugal acceleration.
[0023] 1.1.2.Liquid drain operation In the dissolution / adsorption step S102, while the magnetic beads 2 are fixed to the inner wall of the container 1, the liquid 3 accumulated at the bottom of the container 1 is aspirated and discharged using, for example, a pipette 6, as shown in Fig. 4. In this specification, such an operation of discharging the liquid 3 is referred to as a "liquid discharge operation." As a result of the liquid discharge operation, the magnetic beads 2 to which the nucleic acid is adsorbed remain in the container 1.
[0024] 1.2.Cleaning process In the washing step S108, the magnetic beads 2 to which the nucleic acid is adsorbed are washed. Washing refers to an operation of removing impurities adsorbed to the magnetic beads 2 by contacting the magnetic beads 2 to which the nucleic acid is adsorbed with a washing solution and then separating the magnetic beads 2 again to remove the impurities.
[0025] Specifically, after pouring a washing solution into the container 1 containing the magnetic beads 2 to which nucleic acid is adsorbed, the above-mentioned magnetic separation operation and liquid discharge operation are carried out again.
[0026] In the magnetic separation operation, first, a washing solution is supplied into the container 1 using a pipette or the like. Then, the magnetic beads 2 and the washing solution are stirred. As a result, the washing solution comes into contact with the magnetic beads 2, and the magnetic beads 2 to which the nucleic acid is adsorbed are washed. For stirring, for example, a vortex mixer, manual shaking, pipetting, or the like is used. At this time, the application of the external magnetic field may be temporarily turned off. This causes the magnetic beads 2 to be redispersed in the washing solution, thereby further increasing the washing efficiency.
[0027] Next, as a liquid discharge operation, the washing solution accumulated at the bottom of the container 1 is discharged while the magnetic beads 2 are fixed to the inner wall of the container 1. By supplying and discharging the washing solution as described above at least once, the magnetic beads 2 are washed. This makes it possible to remove impurities with high accuracy.
[0028] The washing liquid is not particularly limited as long as it does not promote the elution of nucleic acids and does not promote the binding of impurities to the magnetic beads 2, but examples include organic solvents such as ethanol, isopropyl alcohol, acetone, or aqueous solutions thereof, low salt concentration aqueous solutions, etc.
[0029] The washing solution may contain a surfactant such as Triton (registered trademark), Tween (registered trademark), SDS, etc. The washing solution may also contain a chaotropic substance such as guanidine hydrochloride.
[0030] Moreover, the cleaning step S108 may be performed as necessary, and may be omitted if cleaning is not necessary.
[0031] 1.3.Elution process In the elution step S110, the nucleic acid adsorbed to the magnetic beads 2 is eluted into an elution solution. Elution is an operation in which the magnetic beads 2 to which the nucleic acid is adsorbed are brought into contact with an elution solution and then separated again, thereby transferring the nucleic acid to the elution solution.
[0032] Specifically, after pouring the eluate into the container 1 containing the magnetic beads 2 to which nucleic acid is adsorbed, the above-mentioned magnetic separation operation and liquid discharge operation are carried out again.
[0033] In the magnetic separation operation, first, the elution solution is supplied into the container 1 using a pipette or the like. Then, the magnetic beads 2 and the elution solution are stirred. As a result, the elution solution comes into contact with the magnetic beads 2, and the nucleic acid is eluted into the elution solution. For stirring, for example, a vortex mixer, manual shaking, pipetting, or the like is used. At this time, the application of the external magnetic field may be temporarily turned off. This causes the magnetic beads 2 to disperse in the elution solution, thereby further increasing the elution efficiency.
[0034] Next, as a liquid discharging operation, the eluate that has accumulated at the bottom of the container 1 is discharged while the magnetic beads 2 are fixed to the inner wall of the container 1. This makes it possible to collect the eluate that contains nucleic acids.
[0035] The elution liquid is not particularly limited as long as it is a liquid that promotes the elution of nucleic acids from the magnetic beads 2 to which the nucleic acids are adsorbed. For example, in addition to water such as sterile water or pure water, a TE buffer solution, i.e., an aqueous solution containing 10 mM Tris-HCl buffer and 1 mM EDTA and having a pH of about 8, is preferably used.
[0036] The elution solution may contain a surfactant such as Triton (registered trademark), Tween (registered trademark), SDS, etc. In addition, it may contain sodium azide as a preservative.
[0037] In the elution step S110, the elution solution may be heated. This can promote the elution of the nucleic acid. The heating temperature of the elution solution is not particularly limited, but is preferably 70°C or higher and 200°C or lower, more preferably 80°C or higher and 150°C or lower, and even more preferably 95°C or higher and 125°C or lower.
[0038] 2. Magnetic beads for extracting biological materials Next, the magnetic beads 2 (magnetic beads for extracting a biological material according to the embodiment) will be described. The magnetic beads 2 are particles that are magnetic and have a binding ability to a biological material on their surfaces.
[0039] FIG. 5 is a cross-sectional view showing a magnetic bead 2 according to an embodiment. The magnetic bead 2 shown in FIG. 5 has a magnetic metal powder 22 and a coating film 24. A magnetic metal powder is used for the magnetic metal powder 22. At least the surface of the coating film 24 is composed of a substance or chemical structure that has a binding property with a biological substance. A particle group that is an aggregate of such magnetic beads 2 is used for the magnetic separation operation described above. In this specification, the magnetic bead 2 refers to the particle group or one of the particles that constitutes the particle group.
[0040] The saturation magnetization of the magnetic beads 2 is preferably 50 emu / g or more, more preferably 80 emu / g or more, and even more preferably 100 emu / g or more. The saturation magnetization is the value of magnetization when the magnetization of the magnetic material is constant regardless of the magnetic field when a sufficiently large magnetic field is applied from the outside. If the saturation magnetization is within the above range, the function as a magnetic material can be fully exerted. Specifically, the moving speed of the magnetic beads 2 in the magnetic field can be improved, so that the time required for magnetic separation can be shortened. In addition, the saturation magnetization of the magnetic beads 2 affects the adsorption force when fixed by an external magnetic field. If the saturation magnetization is within the above range, a sufficiently high adsorption force can be obtained, so that when the liquid 3 is discharged with the magnetic beads 2 fixed, the magnetic beads 2 can be prevented from being discharged together with the liquid 3. This can prevent a decrease in the yield of nucleic acid due to a decrease in the magnetic beads 2.
[0041] The upper limit of the saturation magnetization of the magnetic beads 2 is not particularly limited, but from the viewpoint of easiness in selecting a material that is suitable for balancing performance and cost, it is preferably 220 emu / g or less.
[0042] The saturation magnetization of the magnetic beads 2 can be measured by a vibrating sample magnetometer (VSM) or the like. An example of a vibrating sample magnetometer is TM-VSM1230-MHHL manufactured by Tamagawa Manufacturing Co., Ltd. The maximum applied magnetic field when measuring the saturation magnetization is, for example, 0.5 T or more.
[0043] The average particle diameter D50 of the magnetic beads 2 is preferably 0.5 μm or more and 50 μm or less, more preferably 1 μm or more and 30 μm or less, even more preferably 2 μm or more and 20 μm or less, and particularly preferably 3 μm or more and 15 μm or less. If the average particle diameter D50 of the magnetic beads 2 is within the above range, the specific surface area of the magnetic beads 2 can be sufficiently increased, and the magnetic beads 2 can generate an attractive force and an adsorption force suitable for magnetic separation. In addition, the aggregation of the magnetic beads 2 can be suppressed and the dispersibility can be increased. If the average particle diameter D50 of the magnetic beads 2 is below the lower limit, the magnetization value of the magnetic beads 2 becomes small and the magnetic beads 2 become more likely to aggregate, which may result in a decrease in the efficiency of nucleic acid extraction. In addition, the moving speed of the magnetic beads 2 may decrease, and the time required for magnetic separation may become longer. On the other hand, if the average particle diameter D50 of the magnetic beads 2 exceeds the upper limit, the specific surface area of the magnetic beads 2 becomes small, so that a sufficient amount of nucleic acid cannot be adsorbed, and the amount of nucleic acid extracted may decrease. Furthermore, the magnetic beads 2 are more likely to settle, and the magnetic beads 2 that can contribute to the extraction of nucleic acids are reduced, which may result in a decrease in the efficiency of nucleic acid extraction.
[0044] The average particle size D50 of the magnetic beads 2 can be determined by measuring the volumetric particle size distribution by a laser diffraction / dispersion method and deriving an accumulated distribution curve from the particle size distribution. Specifically, the particle size (median diameter) at which the cumulative value from the small diameter side is 50% in the accumulated distribution curve is the average particle size D50 of the magnetic beads 2. Examples of devices for measuring particle size distribution by the laser diffraction / dispersion method include the MT3300 series manufactured by Microtrack Bell. Note that the method is not limited to the laser diffraction / dispersion method, and other methods such as image analysis may also be used.
[0045] Moreover, the 90% particle diameter of the magnetic beads 2 is defined as D90. In the magnetic beads 2, the ratio D90 / D50 of the 90% particle diameter D90 to the average particle diameter D50 is preferably 3.00 or less, more preferably 2.00 or less, and even more preferably 1.75 or less. This reduces the content of coarse particles, so that the coarse particles attract and aggregate with the surrounding relatively small particles, and the generation of aggregates can be suppressed. If aggregates are generated, they may settle due to their own weight, resulting in a decrease in extraction efficiency and an associated increase in the time required for testing the biological material. Therefore, if the ratio D90 / D50 is within the above range, the occurrence of these problems can be suppressed. Note that if the ratio D90 / D50 exceeds the upper limit, the content of coarse particles increases, so that even if the application of the external magnetic field is turned off, the dispersibility of the magnetic beads 2 may decrease and aggregation may occur more easily.
[0046] The 90% particle diameter D90 of the magnetic beads 2 can be determined from the cumulative distribution curve obtained from the particle size distribution measured by the volumetric particle size distribution using a laser diffraction / dispersion method. Specifically, the particle diameter at which the cumulative value from the small diameter side is 90% in the cumulative distribution curve is the 90% particle diameter D90 of the magnetic beads 2.
[0047] In addition, when the average thickness of the coating film 24 is t and the average particle size of the magnetic beads 2 is D50, the ratio of t to D50, t / D50, is preferably 0.0001 or more and 0.05 or less, more preferably 0.001 or more and 0.01 or less. If t / D50 is below the lower limit, the ratio of the thickness of the coating film 24 to the size of the magnetic metal powder 22 becomes too small, so that the coating film 24 may be destroyed or peeled off when the magnetic beads 2 collide with each other or with the inner wall of the container 1. For this reason, the amount of nucleic acid adsorbed to the surface of the coating film 24 and extracted may decrease, and the extraction efficiency may decrease. In addition, if the peeled coating film 24 or pieces of the magnetic metal powder 22 are present in the extraction liquid, they may be mixed in as impurities (contamination) when the nucleic acid is extracted. Furthermore, the magnetic metal powder 22 is exposed when the coating film 24 is destroyed or peeled off, and when the magnetic metal powder 22 comes into contact with an acidic solution, iron ions and the like are eluted, which may result in a decrease in the efficiency of nucleic acid extraction. On the other hand, when t / D50 exceeds the upper limit, the volume ratio of the coating film 24 to the total volume of the magnetic beads 2 increases, and the magnetization per volume of the magnetic beads 2 may decrease. This may decrease the movement speed when an external magnetic field is applied to the magnetic beads 2, and may increase the time required for magnetic separation.
[0048] The thickness of the coating film 24 can be measured from a cross-sectional observation image of the magnetic beads 2 by, for example, a transmission electron microscope or a scanning electron microscope. The average thickness t of the coating film 24 can be calculated by obtaining a plurality of observation images and averaging the measured values obtained by image processing or the like. For example, the average thickness t is a value obtained by measuring the thickness of the coating film 24 at five or more points on one magnetic bead 2, calculating the average value, and then averaging the average values for ten or more magnetic beads 2. Also, an analyzer such as EDX (Energy Dispersive X-ray spectroscopy) may be used to compare the intensities of, for example, Si-K characteristic X-rays and Fe-L characteristic X-rays, and the thickness of the coating film 24 may be calculated from the comparison result. That is, as described later, when the coating film 24 contains silicon and the magnetic metal powder 22 is made of an Fe-based alloy, the intensity ratio of the Si-K characteristic X-rays originating from the coating film 24 to the sum of the Fe-L characteristic X-rays originating from the magnetic metal powder 22 and the Si-K characteristic X-rays originating from the coating film 24 can be converted into the thickness of the coating film 24.
[0049] Moreover, the coercive force Hc of the magnetic beads 2 is preferably 1500 A / m or less, more preferably 800 A / m or less, even more preferably 400 A / m or less, and particularly preferably 100 A / m or less. The coercive force Hc refers to the value of the external magnetic field in the opposite direction required to return the magnetized magnetic body to an unmagnetized state. In other words, the coercive force Hc means the resistance to the external magnetic field. The smaller the coercive force Hc of the magnetic beads 2, the less likely the magnetic beads 2 are to aggregate together even when the magnetic field is switched from an applied state to an unapplied state, and the magnetic beads 2 can be uniformly dispersed in the dispersion liquid. Furthermore, even when the application of the magnetic field is repeatedly switched, the smaller the coercive force Hc, the better the redispersibility of the magnetic beads 2, so that the aggregation of the magnetic beads 2 can be further suppressed. The lower limit of the coercive force Hc of the magnetic beads 2 is not particularly limited, but is preferably 5 A / m or more from the viewpoint of ease of material selection suitable for the balance between performance and cost.
[0050] The coercive force Hc of the magnetic beads can be measured by a vibrating sample magnetometer, etc., in the same manner as the above-mentioned saturation magnetization. The maximum applied magnetic field when measuring the coercive force Hc is, for example, 15 kOe.
[0051] Moreover, the relative magnetic permeability of the magnetic beads 2 is preferably 5 or more. If the relative magnetic permeability of the magnetic beads 2 falls below the lower limit, the movement speed of the magnetic beads 2 decreases, and the time required for magnetic separation may become longer. The upper limit of the relative magnetic permeability of the magnetic beads 2 is not particularly limited, but since the magnetic beads 2 are in powder form, the relative magnetic permeability often takes a value of 100 or less due to the influence of the demagnetizing field.
[0052] 2.1.Magnetic metal powder The magnetic metal powder 22 is a particle having magnetism, and preferably contains at least one of Fe, Co, and Ni as a constituent element. In particular, from the viewpoint of obtaining high saturation magnetization, the composition of the magnetic metal powder 22 is preferably an alloy (Fe-based alloy) mainly composed of Fe. Specifically, it is more preferable that Fe is 50% or more in atomic ratio, and even more preferable that it is 70% or more. Examples of the Fe-based alloy include an Fe-Co-based alloy, an Fe-Ni-based alloy, an Fe-Co-Ni-based alloy, or a compound containing Fe, Co, and Ni. In addition, from the viewpoint of obtaining high magnetization, carbonyl iron powder, Fe-Si-based alloy powder, Fe-Si-Cr-based alloy powder, and the like, which are essentially made of 100% Fe by mass, are preferably used as the magnetic metal powder 22. With such an Fe-based alloy, it is possible to realize a magnetic metal powder 22 that has high saturation magnetization and high magnetic permeability even if the particle size is small. As a result, it is possible to realize a magnetic bead 2 that has a high moving speed due to the action of an external magnetic field and has a large attractive force when captured by an external magnetic field. As a result, the time required for magnetic separation can be shortened, and the magnetic beads 2 themselves can be prevented from being mixed into the eluate and becoming contaminants.
[0053] In addition to Fe, an element that exhibits ferromagnetism by itself, as described above, Fe-based alloys can contain one or more elements selected from the group consisting of Cr, Nb, Cu, Al, Mn, Mo, Si, Sn, B, C, P, Ti, and Zr, depending on the target properties. Si is a major constituent element of alloy powders, but it is also an element that promotes amorphization.
[0054] The Fe-based alloy may contain impurities to the extent that they do not impair the effect of the magnetic metal powder 22. In this embodiment, the impurities are elements that are unintentionally mixed into the raw materials of the magnetic metal powder 22 or during the manufacture of the magnetic beads 2. The impurities are not particularly limited, but examples thereof include O, N, S, Na, Mg, and K.
[0055] An example of an Fe-based alloy is an alloy with a Si content of preferably 1.0 atomic % or more and 30.0 atomic % or less, more preferably 1.5 atomic % or more and 13.0 atomic % or less, and further preferably 2.0 atomic % or more and 7.0 atomic % or less. Such an alloy has a high magnetic permeability and therefore tends to have a high saturation magnetization.
[0056] The Fe-based alloy may contain at least one of B (boron) with a content of 5.0 atomic % or more and 16.0 atomic % or less, and C (carbon) with a content of 0.5 atomic % or more and 5.0 atomic % or less. These are elements that promote amorphization and contribute to the formation of a stable amorphous structure or nanocrystalline structure in the magnetic metal powder 22.
[0057] Furthermore, the Fe-based alloy preferably contains Cr (chromium) in an amount of 1.0 atomic % or more and 8.0 atomic % or less, which can enhance the corrosion resistance of the magnetic metal powder 22.
[0058] The total content of impurities is preferably 1.0 atomic % or less, so that the effect of the magnetic metal powder 22 is not impaired even if the impurities are contained.
[0059] A particularly preferred example of an Fe-based alloy is an alloy mainly composed of Fe, with a Si content of 2.0% by mass to 9.0% by mass, a B content of 1.0% by mass to 5.0% by mass, and a Cr content of 1.0% by mass to 3.0% by mass. Such an Fe-based alloy may contain a stable amorphous structure, and therefore has a low coercive force. In addition, the high Fe content results in a high saturation magnetization. Furthermore, the inclusion of Cr results in high corrosion resistance, and the elution of iron ions and the like can be suppressed. Since iron ions can have a negative effect on biological material testing, it is preferable that the elution be suppressed.
[0060] The constituent elements and composition of the magnetic metal powder 22 can be identified by ICP emission spectrometry as specified in JIS G 1258:2014, spark emission spectrometry as specified in JIS G 1253:2002, or the like. In addition, when the magnetic metal powder 22 is coated with a coating film 24, the coating film 24 can be removed by a chemical or physical method, and then the above-mentioned method can be used for measurement. In addition, when it is difficult to remove the coating film 24, for example, the magnetic beads 2 can be cut, and the core part of the magnetic metal powder 22 can be analyzed by an analyzer such as an EPMA (Electron Probe Micro Analyzer) or an EDX (Energy Dispersive X-ray spectroscopy).
[0061] The Vickers hardness of the magnetic metal powder 22 is preferably 100 or more, more preferably 300 or more, and even more preferably 800 or more. The method for measuring the hardness of the magnetic metal powder 22 is, for example, as follows. A plurality of particles of the magnetic metal powder 22 are taken out and embedded in resin to prepare a resin-embedded sample, and then the cross section of the magnetic metal powder 22 is made to appear on the surface of the resin-embedded sample by grinding and polishing. An indentation is made on this using a micro Vickers tester or a nano indenter, and the hardness is measured from the size of the indentation.
[0062] If the Vickers hardness of the magnetic metal powder 22 is less than the lower limit, the magnetic metal powder 22 may be plastically deformed due to the impact of the collision of the magnetic beads 2. If plastic deformation occurs, the coating film 24 may peel off or fall off. The upper limit of the Vickers hardness is not particularly limited, but is preferably 3000 or less from the viewpoint of ease of material selection suitable for the balance between performance and cost.
[0063] The main metal structure constituting the magnetic metal powder 22 can take various forms such as a crystalline structure, an amorphous structure, a nanocrystalline structure, and the like. The amorphous structure is a non-crystalline structure in which no crystals exist, and the nanocrystalline structure refers to a structure mainly composed of fine crystals with a crystal grain size of 100 nm or less. The amorphous structure and the nanocrystalline structure give the magnetic metal powder 22 high hardness. In addition, by making the magnetic beads 2 into an amorphous structure or a nanocrystalline structure, the coercive force Hc of the magnetic beads 2 becomes a particularly low value, which contributes to improving the redispersibility of the magnetic beads 2. The volume fraction of the amorphous structure or the nanocrystalline structure in the magnetic metal powder 22 is preferably 40% or more, more preferably 60% or more. This volume fraction is obtained from the results of crystal structure analysis by X-ray diffraction. In addition, the crystalline structure, the amorphous structure, and the nanocrystalline structure may each exist alone, or two or more of them may be mixed.
[0064] The metal structure of the magnetic metal powder 22 can be identified by performing crystal structure analysis on the magnetic metal powder 22 by X-ray diffraction. Furthermore, it can be specified by analyzing the structure observation image or diffraction pattern of the cut sample by a transmission electron microscope (TEM). For example, in the case of an amorphous structure, a diffraction peak derived from a metal crystal such as an α-Fe phase is not observed in a peak analysis by X-ray diffraction. In addition, in the case of an amorphous structure, a so-called halo pattern is formed in an electron beam diffraction pattern by TEM, and the formation of spots due to crystals is not observed. A nanocrystalline structure is composed of a crystalline structure with a grain size of, for example, 100 nm or less, and can be confirmed from a TEM observation image. More accurately, the average grain size can be calculated by image processing or the like from multiple TEM structure observation images in which multiple crystals exist. In addition, the crystal grain size can be estimated by the Sher method from the diffraction peak of the target crystalline phase by X-ray diffraction. Furthermore, for a crystalline structure with a large grain size, the crystal grain size can be measured by a method such as observing a cross section with an optical microscope or a scanning electron microscope (SEM).
[0065] In order to obtain the amorphous structure and nanocrystalline structure, it is effective to increase the cooling rate when pulverizing the molten raw material and then cooling it when manufacturing the magnetic metal powder 22. The ease of forming the amorphous structure and nanocrystalline structure also depends on the alloy composition. As a specific alloy system suitable for forming the amorphous structure and nanocrystalline structure, a composition in which one or more elements selected from the group consisting of Cr, Si, B, C, P, Nb, and Cu are added to Fe is preferable.
[0066] The magnetic metal powder 22 is manufactured by a method similar to a general method for manufacturing metal powder. Examples of manufacturing methods include a melting process in which a metal is melted and solidified to produce a powder, a chemical process in which a powder is produced by a reduction method or a carbonyl method, and a mechanical process in which a larger shape such as an ingot is mechanically crushed to obtain a powder. Of these, the melting process is suitable for manufacturing the magnetic metal powder 22.
[0067] Atomization is a typical manufacturing method using the melting process, in which a molten metal of a desired composition formed by melting is sprayed to form a powder.
[0068] The atomization method is a method of rapidly cooling and solidifying a molten metal by colliding it with a fluid (liquid or gas) sprayed at high speed to powderize it, and is divided into water atomization, high-pressure water atomization, rotating water flow atomization, gas atomization, etc., depending on the type of coolant and the configuration of the device. The atomization method makes it possible to efficiently manufacture magnetic metal powder 22. Furthermore, in the high-pressure water atomization method, rotating water flow atomization method, and gas atomization method, the particle shape of the metal powder becomes close to a spherical shape due to the action of surface tension.
[0069] 2.2.Coating film As shown in Fig. 5, the coating film 24 covers the particle surface of the magnetic metal powder 22. The coating film 24 may be formed on at least a part of the particle surface of the magnetic metal powder 22, but it is preferable that the coating film 24 covers the entire particle surface.
[0070] FIG. 6 is a partial enlarged view of the coating film 24 shown in FIG. 6, the coating film 24 has an inorganic oxide layer 242, an underlayer 244, a gold layer 246, and an immobilization layer 248. That is, the coating film 24 has a multilayer structure having these layers. Note that each layer preferably covers its entire underlayer, but may have discontinuous portions.
[0071] 2.2.1. Inorganic oxide layer The inorganic oxide layer 242 coats the particle surfaces of the magnetic metal powder 22 and contains an inorganic oxide. Examples of the inorganic oxide include silicon oxide, magnesium oxide, calcium oxide, aluminum oxide, titanium oxide, zirconium oxide, boron oxide, yttrium oxide, etc., and one or a mixture of two or more of these is used. Since the inorganic oxide layer 242 containing such an inorganic oxide is porous, a large contact area with the underlying layer 244 can be ensured. Thereby, the adhesion of the underlying layer 244 to the inorganic oxide layer 242 can be enhanced.
[0072] Among these, the inorganic oxide is preferably silicon oxide or titanium oxide. Since these are chemically stable, oxidation and corrosion of the magnetic metal powder 22 can be particularly suppressed, and the corrosion resistance of the magnetic beads 2 can be particularly enhanced.
[0073] Silicon oxide is represented by the compositional formula SiOx (0 < x ≤ 2), and is preferably SiO2. Further, silicon oxide may form a composite oxide or a composite with one or two or more selected from the group consisting of Al, Ti, V, Nb, Cr, Mn, Sn, and Zr.
[0074] Titanium oxide is represented by the compositional formula TiOx (0 < x ≤ 2), and is preferably TiO2. Further, titanium oxide may form a composite oxide or a composite with one or two or more selected from the group consisting of Si, Al, V, Nb, Cr, Mn, Sn, and Zr.
[0075] The inorganic oxide may contain a substance (impurity) other than the inorganic oxide, for example, at a ratio of 50% by mass or less of the above-described inorganic oxide, within a range that does not impair its effect. For example, when silicon oxide is used as the inorganic oxide, examples of the impurity include C, N, P, etc. The composition of the inorganic oxide can be confirmed, for example, by EDX analysis, Auger electron spectroscopy measurement, etc.
[0076] The inorganic oxide layer 242 may cover the surface of one particle of the magnetic metal powder 22, but may also cover a plurality of particles collectively.
[0077] FIG. 7 is a cross-sectional view showing a modified example of the magnetic bead 2 of FIG. The magnetic beads 2A shown in FIG. 7 include a plurality of particles of the magnetic metal powder 22. An inorganic oxide layer 242 is provided so as to cover the plurality of particles. A base layer 244, a gold layer 246, and an immobilization layer 248 are also laminated on the inorganic oxide layer 242. In this manner, the coating film 24 shown in FIG. 7 is configured. With such magnetic beads 2A, the same effect as that of the magnetic beads 2 shown in FIG. 5 can be obtained. The inorganic oxide layer 242 may cover each particle. The base layer 244, the gold layer 246, and the immobilization layer 248 may be provided across a plurality of particles. The base layer 244 may also cover each particle, and the gold layer 246 and the immobilization layer 248 may be provided across a plurality of particles.
[0078] The number of particles of the magnetic metal powder 22 in the magnetic beads 2A is not particularly limited, but is set to be 2 or more and 100 or less.
[0079] The average thickness of the inorganic oxide layer 242 is preferably 10 nm or more and 200 nm or less, more preferably 20 nm or more and 150 nm or less, and even more preferably 30 nm or more and 100 nm or less. This makes it possible to prevent the inorganic oxide layer 242 from being destroyed or peeled off even if the magnetic beads 2 collide with each other or with the inner wall of the container. As a result, it is possible to prevent the elution of iron ions and the like that accompanies the exposure of the magnetic metal powder 22. In addition, it is possible to prevent the magnetization per volume of the magnetic beads 2 from decreasing, and to prevent the movement speed of the magnetic beads 2 from decreasing.
[0080] The average thickness of the inorganic oxide layer 242 is measured in the same manner as the method for measuring the average thickness of the coating film 24 described above.
[0081] The inorganic oxide layer 242 can be formed, for example, by a wet method such as a sol-gel method, or by a dry method such as a vapor phase deposition method. Among these, the Stöber method, which is a type of sol-gel method, or the ALD (Atomic Layer Deposition) method can be preferably used. The Stöber method is a method for forming monodisperse particles by hydrolysis of metal alkoxide. For example, when the inorganic oxide layer 242 is formed of silicon oxide, silicon oxide can be produced by hydrolysis reaction of silicon alkoxide. Before forming the inorganic oxide layer 242, the base, for example, the surface of the particles of the magnetic metal powder 22, may be cleaned with water or an organic solvent.
[0082] 2.2.2. Base layer The underlayer 244 is a layer that can be a base for the gold layer 246 described later. The base for the gold layer 246 refers to a surface on which gold can be favorably deposited when the gold layer 246 is formed by electroless gold plating. Specifically, the underlayer 244 contains a reducing agent that reduces gold ions to gold, or a catalyst for a reduction reaction that reduces gold ions to gold. Such an underlayer 244 enhances the adhesion of the gold layer 246. As a result, the adhesion of the immobilization layer 248 formed on the gold layer 246 can be enhanced.
[0083] The reducing agent dissolves in the electroless gold plating solution, ionizes, and releases electrons, thereby reducing the gold ions to gold. Therefore, the underlayer 244 containing the reducing agent enables the formation of the gold layer 246 by a displacement plating method. Examples of the reducing agent include metals such as nickel, palladium, and copper, which have a higher ionization tendency than gold, and alloys containing these metals.
[0084] The catalyst has catalytic activity to catalyze the reduction reaction of gold ions when the reducing agent contained in the electroless gold plating solution causes the reduction reaction. Therefore, the base layer 244 containing the catalyst enables the formation of the gold layer 246 by a self-catalytic reduction plating method. Examples of the catalyst include simple metals such as nickel, palladium, and copper, and alloys containing these metals. The content of these metals in the base layer 244 is preferably more than 50% by mass, and more preferably 70% by mass or more.
[0085] Of these, it is preferable that the underlayer 244 contains nickel. When the underlayer 244 contains nickel or a nickel alloy, the gold layer 246 can be favorably formed by an electroless gold plating method such as a displacement plating method or an autocatalytic reduction plating method.
[0086] These reducing agents and catalysts may be present in any form. For example, the underlayer 244 may be a plating film, a film formed by a vapor phase film formation method, or a film formed by a liquid phase film formation method. Examples of the plating film include an electroless plating film. Before the underlayer 244 is formed, the surface of the underlayer, for example, the inorganic oxide layer 242, may be subjected to a surface treatment such as a degreasing treatment or an acid immersion treatment, or a cleaning treatment using water or an organic solvent.
[0087] The average thickness of the underlayer 244 is not particularly limited, but is preferably 10 nm to 500 nm, more preferably 30 nm to 300 nm, and even more preferably 50 nm to 200 nm, which ensures that the underlayer 244 has a sufficient thickness to function as a base.
[0088] The average thickness of the underlayer 244 is measured in the same manner as the method for measuring the average thickness of the coating film 24 described above.
[0089] Moreover, the average total thickness of the inorganic oxide layer 242 and the underlayer 244 is preferably 10 nm or more and 600 nm or less, more preferably 50 nm or more and 450 nm or less, and even more preferably 100 nm or more and 300 nm or less. This makes it possible to sufficiently ensure the corrosion resistance of the magnetic beads 2. Also, it is possible to optimize the volume ratio of the coating film 24 to the total volume of the magnetic beads 2, and to suppress a decrease in the magnetization per volume of the magnetic beads 2.
[0090] The average thickness of the underlayer 244 may be thinner than the average thickness of the inorganic oxide layer 242, but is preferably set to be thicker. More preferably, the average thickness of the underlayer 244 is set to be 1.2 to 4.0 times, and even more preferably 1.5 to 3.0 times, of the average thickness of the inorganic oxide layer 242. This enhances the function of the underlayer 244 as a base for stably forming the gold layer 246, and improves the corrosion resistance of the magnetic beads 2. As a result, the immobilization layer 248 can be stabilized, and oxidation and corrosion of the magnetic metal powder 22 can be suppressed, resulting in magnetic beads 2 with particularly good nucleic acid extraction efficiency.
[0091] The underlayer 244 may have a multi-layer structure. For example, the first layer may be a nickel-containing layer and the second layer may be a palladium-containing layer. By using such a multi-layer structure, oxidation and corrosion of the underlayer 244 can be more reliably suppressed. As a result, the corrosion resistance of the magnetic beads 2 can be further improved.
[0092] 2.2.3. Gold layer The gold layer 246 is a layer that can serve as a base for the immobilization layer 248. The base for the immobilization layer 248 refers to a surface that can favorably bind the compounds contained in the immobilization layer 248. Specifically, the material constituting the gold layer 246 can be simple gold or an alloy containing gold. The gold layer 246 has high corrosion resistance, and therefore has a high function of suppressing oxidation and corrosion of the magnetic metal powder 22. This can suppress the decrease in magnetization of the magnetic metal powder 22 and the decrease in the extraction efficiency of nucleic acids due to the elution of iron ions, etc.
[0093] The gold content of the magnetic beads 2 is preferably 1% by mass or more and 30% by mass or less, more preferably 3% by mass or more and 25% by mass or less, and even more preferably 5% by mass or more and 20% by mass or less. This ensures a sufficient coverage rate of the gold layer 246, and allows the immobilization layer 248 to be formed evenly.
[0094] The average thickness of the gold layer 246 is preferably 0.5 nm to 50 nm, more preferably 1 nm to 30 nm, and even more preferably 2 nm to 20 nm, which ensures particularly good corrosion resistance of the magnetic beads 2.
[0095] As described above, the gold layer 246 can be formed by electroless gold plating such as displacement plating or autocatalytic reduction plating. Before the gold layer 246 is formed, the surface of the base layer, for example, the base layer 244, may be subjected to a surface treatment such as degreasing or acid immersion, or a cleaning treatment using water or an organic solvent.
[0096] 2.2.4. Fixed layer The immobilization layer 248 contains a compound having a ligand or a ligand-binding site. A ligand is a site that has the function of specifically binding to a target biological substance. A ligand-binding site is a site (ligand-reactive group) that can bind such a ligand. By having such an immobilization layer 248, the magnetic beads 2 can efficiently adsorb the target biological substance.
[0097] Specific examples of the ligand include multidentate ligands such as nitrilotriacetic acid (NTA), iminodiacetic acid (IDA), phenanthroline, terpyridine, bipyridine, triethylenetetraamine, tris(carboxymethyl)ethylenediamine, diethylenetriaminepentaacetic acid, polypyrazolylboric acid, 1,4,7-triazocyclononane, dimethylglyoxime, diphenylglyoxime, and derivatives thereof.
[0098] Of these, nitrilotriacetic acid (NTA) or iminodiacetic acid (IDA) is preferably used as the ligand.
[0099] Specific examples of the ligand binding site include an aldehyde group, a carboxy group, an amide group, N-hydroxysuccinimide (NHS), an amino group, a hydroxy group, -CH=CH-, -(C=O)-CH=CH-, and the like.
[0100] Among these, an aldehyde group, a carboxy group, an amide group, or N-hydroxysuccinimide (NHS) is preferably used for the ligand binding site.
[0101] These ligands or ligand binding sites are bonded to the gold layer 246 via a spacer, which is provided as necessary, and an Au-S bond. The Au-S bond is a strong bond, and contributes to strong fixation of the ligands and the ligand binding sites to the gold layer 246. This makes it possible to prevent the ligands from being detached even when various physical and chemical loads are applied to the magnetic beads 2 to which nucleic acid is adsorbed. As a result, it is possible to prevent a decrease in the efficiency of capturing nucleic acid, and thus to realize magnetic beads 2 with good nucleic acid extraction efficiency.
[0102] Further, in the magnetic beads 2, an underlayer 244 is provided as a base for the gold layer 246. The underlayer 244 enhances the adhesion of the gold layer 246. This makes it possible to suppress peeling of the gold layer 246, and therefore from this point of view, it is possible to suppress detachment of the ligand. Further, in the magnetic beads 2, an inorganic oxide layer 242 is provided as a base for the underlayer 244. The inorganic oxide layer 242 enhances the adhesion of the underlayer 244. This makes it possible to suppress peeling of the underlayer 244, and therefore from this point of view, it is possible to suppress detachment of the ligand. Therefore, the coating film 24 having the above-mentioned multilayer structure can suppress detachment of the ligand, and realize magnetic beads 2 with good nucleic acid extraction efficiency.
[0103] A compound having a ligand or a ligand binding site is a compound having a thiol group or a disulfide group capable of forming a Au-S bond, and is a reaction product of a reaction between a thiol derivative or its salt described below and the gold layer 246.
[0104] Fig. 8 is a schematic diagram showing a state in which a compound 10 having a functional site X is bound to a gold layer 246 via an Au-S bond. In Fig. 8, a ligand or a ligand binding site is referred to as a "functional site X".
[0105] Compound 10 shown in FIG. 8 is composed of a Au—S bond, a spacer L and a functional moiety X.
[0106] Spacer L is a moiety that links an -S- bond and a functional moiety X. Examples of unit structures constituting spacer L include PEG (polyethylene glycol), PPG (polypropylene glycol), PBG (polybutylene glycol), a composite structure of a carbonate bond and PEG, a composite structure of an amide bond and PEG, methylene, and the like, and a structure in which one or more of these are mixed is included.
[0107] Furthermore, as shown in Fig. 8, between adjacent compounds 10, self-organization occurs due to the interaction between spacers L, and the compounds 10 tend to be oriented. This makes it possible to realize an immobilization layer 248 in which functional sites X are densely arranged. In such an immobilization layer 248, the amount of biomaterial adsorbed per unit amount of magnetic beads 2 can be increased. The structure of compound 10 shown in Fig. 8 may include a branched structure of molecular chains (not shown). The following formula (1) is an example of the structure of a thiol derivative that produces compound 10.
[0108] R 1 -(CH2) x -(C2H5O) y -R 2 … (1) [In the above formula (1), x is an integer of 2 or more and 18 or less, and y is an integer of 0 or more and 100 or less. In addition, in the above formula (1), R 1 is a thiol group or a disulfide bond, and R 2 is a ligand or ligand-binding site.
[0109] The thiol derivative having the structure represented by the above formula (1) or its salt can generate compound 10 capable of arranging ligands or ligand binding sites at a high density by reacting with gold layer 246. This allows magnetic beads 2 with particularly good nucleic acid extraction efficiency to be obtained.
[0110] The structure represented by the above formula (1) is the whole or a part of the molecular structure of the thiol derivative. Therefore, the molecular structure of the thiol derivative may include the structure represented by the above formula (1) and another structure.
[0111] Examples of the salts of thiol derivatives include alkali metal salts such as lithium salts, sodium salts, and potassium salts, and alkaline earth metal salts such as magnesium salts and calcium salts.
[0112] A thiol group is a reactive functional group represented by -SH. A disulfide bond is a functional group represented by -SS-, which is converted to a thiol group by reduction. Therefore, R in the above formula (1) 1 is a disulfide bond, the thiol derivative is represented by the above formula (1) 1 The thiol group reacts with gold to form a strong Au-S bond. The product of this reaction is compound 10 shown above.
[0113] Also, -(CH2) x -(C2H5O) y The - corresponds to the above-mentioned spacer L. The thiol derivative represented by the above formula (1) contains methylene or PEG as the spacer L, and therefore when bonded to the gold layer 246, the compound 10 is easily self-assembled. This allows the compound 10 to be oriented, enabling the functional site X to be arranged at a high density.
[0114] In the above formula (1), x, which represents the number of methylenes, is set to 2 or more and 18 or less, preferably 3 or more and 10 or less, and more preferably 4 or more and 6 or less. This stabilizes the compound 10, and can suppress deterioration of the immobilization layer 248 accompanying magnetic separation and liquid discharge operations. If x is below the lower limit, the length of the spacer L is shortened, and the functionality of the functional site X may decrease, that is, the ligand or the ligand binding site may become difficult to function. In addition, the shortening of the length of the spacer L may make it difficult to achieve self-organization of the compound 10. On the other hand, if x exceeds the upper limit, the molecular chain of the compound 10 may become too long, and the compound 10 may become difficult to orient, and the density of the functional site X may not be sufficiently increased.
[0115] In the above formula (1), y, which represents the number of PEGs, is 0 to 100, preferably 1 to 30, and more preferably 2 to 10. This stabilizes the compound 10. If y is below the lower limit, the length of the spacer L is shortened, which may reduce the functionality of the functional moiety X. In addition, the shortening of the length of the spacer L may make it difficult to achieve self-organization of the compound 10. On the other hand, if y is above the upper limit, the molecular chain of the compound 10 may become too long, which may make it difficult for the compound 10 to be oriented, and may not be able to sufficiently increase the density of the functional moiety X.
[0116] Specific examples of the thiol derivative having a ligand include compounds represented by the following formulas (A-1) to (A-7).
[0117] [ka]
[0118] [ka]
[0119] [ka]
[0120] [ka]
[0121] [ka]
[0122] [ka]
[0123] [ka]
[0124] Specific examples of the thiol derivative having a ligand binding site include compounds represented by the following formulas (B-1) to (B-4).
[0125] [ka]
[0126] [ka]
[0127] [ka]
[0128] [ka]
[0129] Such compounds are synthesized, for example, by using a linker compound in which various functional groups are added to a PEG chain or an alkyl chain, and linking them via the PEG chain or the alkyl chain.
[0130] 3. Advantages of the above embodiment As described above, the magnetic beads 2, which are magnetic beads for extracting biological substances according to the embodiment, have the magnetic metal powder 22, the inorganic oxide layer 242, the underlayer 244, the gold layer 246, and the immobilization layer 248. The inorganic oxide layer 242 covers the particle surface of the magnetic metal powder 22 and contains an inorganic oxide. The underlayer 244 covers the surface of the inorganic oxide layer 242 and contains a reducing agent for gold ions or a catalyst for the reduction reaction of gold ions. The gold layer 246 covers the surface of the underlayer 244 and contains gold. The immobilization layer 248 contains a compound 10 having a ligand or a ligand binding site, which is bound to the surface of the gold layer 246 via an Au-S bond.
[0131] According to such a configuration, even when a load is applied, it is possible to suppress the detachment of the ligand and the oxidation and corrosion of the magnetic metal powder 22. This makes it possible to obtain magnetic beads 2 with good efficiency in extracting biological materials.
[0132] Moreover, the above compound 10 is preferably a reaction product between a thiol derivative represented by the following formula (1) or a salt thereof and the gold layer 246.
[0133] R 1 -(CH2) x -(C2H5O) y -R 2 … (1) [In the above formula (1), x is an integer of 2 or more and 18 or less, and y is an integer of 0 or more and 100 or less. In addition, in the above formula (1), R 1 is a thiol group or a disulfide bond, and R 2 is the ligand or the ligand binding site. The thiol derivative having the structure represented by the above formula (1) or its salt can generate compound 10 in which ligands or ligand binding sites can be arranged at a high density by reacting with gold layer 246. This allows magnetic beads 2 with particularly good extraction efficiency for biological materials to be obtained.
[0134] The inorganic oxide is preferably silicon oxide or titanium oxide. These are chemically stable, and therefore can particularly inhibit the oxidation and corrosion of the magnetic metal powder 22, and can particularly enhance the corrosion resistance of the magnetic beads 2.
[0135] Moreover, the underlayer 244 preferably contains nickel. By including nickel or a nickel alloy in the underlayer 244, the gold layer 246 can be formed satisfactorily by electroless gold plating such as displacement plating or autocatalytic reduction plating.
[0136] The combined average thickness of the inorganic oxide layer 242 and the underlayer 244 is preferably 10 nm or more and 600 nm or less.
[0137] This makes it possible to sufficiently ensure the corrosion resistance of the magnetic beads 2. In addition, it is possible to optimize the volume ratio of the coating film 24 to the total volume of the magnetic beads 2, thereby preventing the magnetization per volume of the magnetic beads 2 from decreasing.
[0138] Moreover, the average particle size D50 of the magnetic beads 2 is preferably 0.5 μm or more and 50 μm or less.
[0139] This allows the specific surface area of the magnetic beads 2 to be sufficiently large, and allows the magnetic beads 2 to generate attractive and adsorbing forces suitable for magnetic separation. In addition, aggregation of the magnetic beads 2 can be suppressed, and dispersibility can be improved.
[0140] Moreover, it is preferable that the saturation magnetization of the magnetic metal powder 22 is 80 emu / g or more, and the coercive force of the magnetic metal powder 22 is 100 A / m or less.
[0141] This makes it possible to improve the moving speed of the magnetic beads 2 in the magnetic field, thereby shortening the time required for magnetic separation. In addition, since a sufficiently high adsorptive force is obtained, when the liquid 3 is discharged with the magnetic beads 2 fixed, the magnetic beads 2 can be prevented from being discharged together with the liquid 3. This makes it possible to prevent a decrease in the yield of the biological material due to a decrease in the magnetic beads 2. Furthermore, even when the application of the magnetic field is repeatedly switched, aggregation of the magnetic beads 2 can be prevented.
[0142] Moreover, the average thickness of the underlayer 244 is preferably 1.2 times or more and 4.0 times or less the average thickness of the inorganic oxide layer 242 .
[0143] This enhances the function of the base layer 244 as a base for stably forming the gold layer 246, and improves the corrosion resistance of the magnetic beads 2. As a result, the immobilization layer 248 can be stabilized, and oxidation and corrosion of the magnetic metal powder 22 can be suppressed, resulting in magnetic beads 2 with particularly good extraction efficiency for biological materials.
[0144] Although the magnetic beads for extracting biological material of the present invention have been described above based on the illustrated embodiment, the present invention is not limited thereto. For example, the magnetic beads for extracting biological material of the present invention may be those having any component added thereto in the above embodiment. EXAMPLES
[0145] Next, specific examples of the present invention will be described. 4. Preparation of Magnetic Beads 4.1. Example 1 First, a metal powder mainly composed of an amorphous structure produced by a water atomization method was prepared as a magnetic metal powder, and the prepared metal powder was washed with ultrapure water and ethanol.
[0146] Next, a silicon oxide (SiO2) film was formed on the particle surface of the magnetic metal powder by the Stöber method to obtain an inorganic oxide layer. Tetraethoxysilane (TEOS) was used as the silicon alkoxide. The magnetic metal powder with the inorganic oxide layer formed was subjected to a degreasing process and an acid immersion process.
[0147] Next, a nickel film was formed on the surface of the inorganic oxide layer by electroless nickel plating to obtain an underlayer. The magnetic metal powder on which the underlayer was formed was subjected to a degreasing treatment.
[0148] Next, a gold film was formed on the surface of the underlayer by a displacement type electroless gold plating method to obtain a gold layer. The magnetic metal powder on which the gold layer was formed was washed with ultrapure water and ethanol.
[0149] Next, a thiol derivative having a structure represented by the symbol in Table 1 was dissolved in ethanol to prepare an ethanol solution. Then, the magnetic metal powder on which the gold layer was formed was immersed in the ethanol solution and subjected to a stirring process. This caused the thiol derivative to react with the gold layer, resulting in an immobilized layer.
[0150] The average particle size, saturation magnetization and coercive force of the magnetic metal powder, as well as the conditions for forming the coating film, are as shown in Table 1. The symbols representing the thiol derivatives shown in Table 1 correspond to the above-mentioned formula (A-1).
[0151] 4.2. Examples 2 to 11 Magnetic beads were obtained in the same manner as in Example 1, except that the composition of the magnetic metal powder and the conditions for forming the coating film were as shown in Table 1. The symbols representing the thiol derivatives shown in Table 1 correspond to the thiol derivatives represented by the above-mentioned formulas (A-2) to (A-7) and formulas (B-1) to (B-4).
[0152] 4.3. Comparative Example 1 Except for using gold colloid particles instead of magnetic metal powder, magnetic beads were obtained in the same manner as in Example 1. Note that the gold colloid particles are particles composed only of gold and do not include an inorganic oxide layer or an underlayer.
[0153] 4.4. Comparative Examples 2 and 3 Except for forming the immobilization layer using a silane coupling agent instead of a thiol derivative, magnetic beads were obtained in the same manner as in Example 1. The symbols representing the silane coupling agents shown in Table 1 correspond to the silane coupling agents represented by the following formulas (C-1) and (D-1).
[0154] [ka]
[0155] [ka]
[0156] 4.5. Examples 12 to 25 Magnetic beads were obtained in the same manner as in Example 1, except that the composition of the magnetic metal powder and the conditions for forming the coating film were as shown in Table 2. The symbols representing the thiol derivatives shown in Table 2 correspond to the above-mentioned formula (A-1).
[0157] 4.6. Comparative Example 4 Magnetic beads were obtained in the same manner as in Example 1, except that the inorganic oxide layer was omitted and the conditions for forming the coating layer were as shown in Table 2.
[0158] 4.7. Comparative Example 5 Magnetic beads were obtained in the same manner as in Example 1, except that the underlayer was omitted and the conditions for forming the coating layer were as shown in Table 2.
[0159] 4.8. Comparative Example 6 Magnetic beads were obtained in the same manner as in Example 1, except that ferrite-containing particles were used instead of the magnetic metal powder, and the coating layer formation conditions were set as shown in Table 2. The ferrite-containing particles are particles in which ferrite particles are dispersed in silica.
[0160] 5. Evaluation of Magnetic Beads 5.1. Purification yield of biological material First, protein A was dispersed in pure water as a target biological material to prepare a sample aqueous solution in a microtube. The concentration of protein A was 50 μg / mL.
[0161] Next, the magnetic beads of each Example and Comparative Example were dispersed in the sample aqueous solution to a concentration of 30% by mass.
[0162] Next, a magnet was brought close to the side of the microtube, a magnetic field was applied, and the supernatant was removed. The magnetic beads remaining in the microtube were then collected. This allowed the target biological material to be adsorbed onto the magnetic beads. The collected magnetic beads were then dispersed in a PBS buffer solution to prepare a dispersion. The PBS buffer solution was a phosphate buffer solution containing NaCl at a concentration of 137 mmol / L, Na2HPO4 at a concentration of 8.1 mmol / L, KCl at a concentration of 2.7 mmol / L, and KH2PO4 at a concentration of 1.5 mmol / L.
[0163] Next, the prepared dispersion was stirred by inversion stirring for 30 minutes, the supernatant was collected, and the BCA assay test solution was added. Then, the absorbance of the dispersion to which the test solution was added was measured using a UV-vis meter (U-3900H type spectrophotometer). The abs.-562 nm value of the imidazole solution alone was set as the reference value, and the ratio of the abs.-562 nm value of the supernatant obtained using the magnetic beads of each Example and Comparative Example was calculated. The closer this ratio is to 1.0, the greater the amount of biological material purified by the magnetic beads. The calculated ratio was then evaluated in light of the following evaluation criteria. The evaluation results are shown in Tables 1 and 2.
[0164] A: The ratio of the abs.-562nm value of the supernatant to the reference value is 0.8 or more. B: The ratio of the abs.-562 nm value of the supernatant to the reference value is 0.7 or more and less than 0.8. C: The ratio of the abs.-562 nm value of the supernatant to the reference value is 0.6 or more and less than 0.7. D: The ratio of the abs.-562 nm value of the supernatant to the reference value is 0.3 or more and less than 0.6. E: The ratio of the abs.-562 nm value of the supernatant to the reference value is less than 0.3.
[0165] 5.2. Redispersibility First, the magnetic beads of each Example and Comparative Example were dispersed in a PBS buffer solution to a concentration of 30% by mass to prepare a dispersion. The PBS buffer solution was the same as that used in 5.1.
[0166] Next, the prepared dispersion was placed in a laser diffraction / scattering particle size distribution analyzer, and the volumetric average particle size D50 was measured. The measured average particle size D50 was taken as the value before the separation of the target biological material, and this was used as the reference value.
[0167] Next, the magnetic beads were dispersed in the same manner as in 5.1. in the sample aqueous solution prepared in the same manner as in 5.1., magnetic separation was performed, and the magnetic beads adsorbing the biological material were recovered. After that, the recovered magnetic beads were dispersed in a PBS buffer aqueous solution in the same manner as in 5.1. to prepare a dispersion. Then, the average particle size D50 on a volume basis was measured in the same manner as above, and the measured value was used as the value after the separation work of the target biological material.
[0168] Next, the ratio of the value after the separation process to the reference value was calculated. The closer this ratio is to 1.0, the better the redispersibility of the magnetic beads is. The calculated ratio was then evaluated against the following evaluation criteria. The evaluation results are shown in Tables 1 and 2. A: The ratio of the value after separation to the standard value is less than 1.1. B: The ratio of the value after separation to the standard value is 1.1 or more and less than 1.3. C: The ratio of the value after separation to the standard value is 1.3 or more and less than 1.5. D: The ratio of the value after separation to the reference value is 1.5 or more and less than 2.0. E: The ratio of the value after separation to the reference value is 2.0 or more.
[0169] 5.3.Corrosion Resistance First, the magnetic beads of each Example and Comparative Example were dispersed in a PBS buffer solution to a concentration of 30% by mass to prepare a dispersion. The PBS buffer solution was the same as that used in 5.1.
[0170] Next, the prepared dispersion was left to stand for 10 days under conditions of an atmospheric pressure of 1013 hPa and a temperature of 70°C, and then the elemental concentration of the supernatant was measured using an ICP analyzer, 5100 ICP-OES, manufactured by Agilent Technologies.
[0171] The element concentration of the PBS buffer solution alone was used as the reference value, and the difference between this and the element concentration of the supernatant was calculated. The smaller the difference between the ion concentration of the supernatant and the reference value, the smaller the amount of magnetic component elution. The evaluation results are shown in Tables 1 and 2.
[0172] A: The difference in ion concentration is less than 10 ppm. B: The difference in ion concentration is 10 ppm or more and less than 20 ppm. C: The difference in ion concentration is 20 ppm or more and less than 35 ppm. D: The difference in ion concentration is 35 ppm or more and less than 100 ppm. E: The difference in ion concentration is 100 ppm or more.
[0173] 5.4.Magnetic separation speed First, the magnetic beads of each Example and Comparative Example were dispersed in pure water at 25°C to a concentration of 0.1% by mass to prepare a dispersion. Next, the dispersion was placed in a spectroscopic cell, and stirred by ultrasonic irradiation or by a vortex mixer. The stirring time was 1 minute. Next, the spectroscopic cell that had been subjected to the stirring process was quickly set in the cell holder of the spectrophotometer. Note that a magnet was attached to the cell holder in advance in accordance with the position where the spectroscopic cell was to be placed. In addition, the shortest distance between the outer wall of the spectroscopic cell set in the cell holder and the magnet was 2.0 mm, and a magnet with a surface magnetic flux density of 180 mT was used as the magnet.
[0174] Next, at the same time as starting to leave the spectroscopic cell, measurement of the absorbance at a wavelength of 550 nm was started for the spectroscopic cell. The time until the measured absorbance decayed to 10% of the initial absorbance was measured, and the measurement result was used as an evaluation index for evaluating the magnetic separation speed. The obtained evaluation index was evaluated against the following evaluation criteria. The evaluation results are shown in Tables 1 and 2.
[0175] A: The evaluation index for magnetic separation speed is less than 20 seconds. B: The evaluation index for magnetic separation speed is 20 seconds or more and less than 30 seconds. C: The evaluation index for magnetic separation speed is 30 seconds or more and less than 45 seconds. D: The evaluation index of the magnetic separation speed is 45 seconds or more and less than 60 seconds. E: The evaluation index for magnetic separation speed is 60 seconds or more.
[0176] [Table 1]
[0177] [Table 2]
[0178] As shown in Tables 1 and 2, the magnetic beads of each Example had a large amount of purified biological material and good redispersibility even after magnetic separation. The magnetic beads of each Example also had good corrosion resistance even after immersing in an acid-containing PBS buffer solution for 10 days. Furthermore, it was confirmed that the magnetic beads of each Example had a sufficiently high magnetic separation speed.
[0179] From the above results, it is evident that the present invention can provide magnetic beads with good extraction efficiency for biological materials. [Explanation of symbols]
[0180] 1...container, 2...magnetic beads, 2A...magnetic beads, 3...liquid, 5...magnet, 6...pipette, 10...compound, 22...magnetic metal powder, 24...coating film, 242...inorganic oxide layer, 244...underlayer, 246...gold layer, 248...immobilization layer, S102...dissolution / adsorption step, S108...washing step, S110...elution step, L...spacer, X...functional site
Claims
1. Magnetic metal powder; an inorganic oxide layer that covers the particle surfaces of the magnetic metal powder and contains an inorganic oxide; a base layer that covers a surface of the inorganic oxide layer and contains a reducing agent for gold ions or a catalyst for a reduction reaction of gold ions; a gold layer that covers a surface of the underlayer and contains gold; an immobilization layer comprising a ligand or a compound having a ligand binding site, which is bound to the surface of the gold layer via a Au—S bond; 1. A magnetic bead for extracting a biological material, comprising:
2. 2. The magnetic beads for extracting biological substances according to claim 1, wherein the compound is a reaction product between a thiol derivative represented by the following formula (1) or a salt thereof and the gold layer: R 1 - (CH 2 ) x - (C 2 H 5 O) y -R 2 … (1) [In the above formula (1), x is an integer of 2 or more and 18 or less, and y is an integer of 0 or more and 100 or less. 1 is a thiol group or a disulfide bond, R 2 is the ligand or the ligand binding site.
3. 3. The magnetic beads for extracting a biological material according to claim 1, wherein the inorganic oxide is silicon oxide or titanium oxide.
4. 3. The magnetic beads for extracting a biological material according to claim 1, wherein the underlayer contains nickel.
5. 3. The magnetic beads for extracting a biological material according to claim 1, wherein the total average thickness of said inorganic oxide layer and said underlayer is 10 nm or more and 600 nm or less.
6. 3. Magnetic beads for extracting biological substances according to claim 1 or 2, having an average particle size of 0.5 μm or more and 50 μm or less.
7. The saturation magnetization of the magnetic metal powder is 80 emu / g or more; 3. The magnetic beads for extracting biological substances according to claim 1, wherein the magnetic metal powder has a coercive force of 100 A / m or less.
8. 3. The magnetic beads for extracting a biological material according to claim 1, wherein the average thickness of the underlayer is 1.2 to 4.0 times the average thickness of the inorganic oxide layer.
Citation Information
Patent Citations
Two-dimensional cell scratch chip and preparation method and application thereof
CN106282016A
Nanoparticle biosensors and methods of making and using the same
JP2009509132A
Metallic microparticle, manufacturing method therefor, and magnetic bead
JP2010156054A
Functional particle containing gold component
JP2010249729A
Electrochemical detection method
JP2015516067A