Support sheet and method for manufacturing workpiece processed product

The support sheet with a base material and energy ray-curable adhesive layer addresses non-uniform application and high-temperature issues, enabling easy peeling and reliable pickup of workpieces.

JP2024142716AInactive Publication Date: 2024-10-11LINTEC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023055007
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing support sheets for workpieces face issues with non-uniform application due to air bubbles, difficulty in peeling without deformation, and inability to withstand high temperatures during processing, leading to challenges in picking up workpieces from the support sheet.

Method used

A support sheet comprising a base material and an energy ray-curable adhesive layer, designed with specific adhesive forces and light transmittance properties, allowing easy peeling and reattachment while maintaining shape, even at high temperatures.

Benefits of technology

The support sheet enables easy peeling and reattachment of workpieces without deformation, and allows for normal pickup from the support sheet even at high temperatures, improving processing efficiency and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142716000001_ABST
    Figure 2024142716000001_ABST
Patent Text Reader

Abstract

To provide a support sheet which, for the purpose of reattachment, allows an adhesive layer in the support sheet to be easily peeled from a rear face of a workpiece while maintaining a shape, which can prevent occurrence of peeling of a chip in dicing, and which also allows a workpiece processed product to be picked up normally from the support sheet even if being heated at a high temperature of 140°C or above.SOLUTION: There is provided a support sheet 1. The support sheet 1 includes a base material 11 and an adhesive layer 12 formed on one surface 11a of the base material 11. An adhesive force (X0) between the adhesive layer 12 and a silicon mirror wafer is 8,000 mN / 25 mm or less, an adhesive force (X1) between an energy ray cured product of the adhesive layer 12 and the silicon mirror wafer is 500 mN / 25 mm or less, and an adhesive force (X01) between the adhesive layer 12 after reattachment and the silicon mirror wafer is 2,000 mN / 25 mm or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a support sheet and a method for manufacturing a workpiece. [Background technology]

[0002] A support sheet is used when processing a workpiece such as a wafer to manufacture a workpiece such as a chip. A typical support sheet includes a support sheet that includes a base material and an adhesive layer provided on one side of the base material. The adhesive layer in the support sheet is, for example, attached to the workpiece to be processed, and the support sheet fixes the workpiece during processing. When the processing is dicing, the support sheet functions as a dicing sheet. The obtained workpiece is finally separated from the support sheet and picked up for use in the intended application. At this time, when the adhesive layer is energy ray curable, the adhesive layer is cured with energy rays to reduce the adhesive force between the cured product and the workpiece, making it easier to pick up the workpiece.

[0003] A protective film-forming film for forming a protective film on the workpiece may be provided on the surface of the adhesive layer opposite to the substrate side to form a composite sheet for forming a protective film. The protective film-forming film in the composite sheet for forming a protective film is, for example, attached to the workpiece to be processed, and the composite sheet for forming a protective film fixes the workpiece during processing and forms a protective film on the workpiece or the workpiece. The obtained workpiece is finally separated from the support sheet with the protective film and picked up, and used for the intended purpose. Similarly to the above, when the adhesive layer is energy ray curable, the adhesive layer is energy ray cured to facilitate picking up the workpiece with the protective film.

[0004] On the other hand, the support sheet may be heated with the workpiece or workpiece attached thereto. This heating may be performed, for example, to remove foreign matter such as low molecular weight resin components attached to the surface of the workpiece. It may also be performed to dry the workpiece or the like after cleaning and removing fine foreign matter that is generated during processing such as dicing the workpiece and that is attached to the surface of the workpiece with water. These heating processes are usually performed with the upper limit of the heating temperature set to about 145°C. However, if the heat resistance of the support sheet is insufficient, when the support sheet to which the workpiece or workpiece is attached is heated at such a temperature, it may ultimately be impossible to pick up the workpiece from the support sheet.

[0005] As a support sheet that is heat resistant and suitable for heating, a support sheet (sheet for work processing) has been disclosed that has a base material and an adhesive layer, and in which the Young's modulus of the base material at 23°C after heating at 120°C for 4 hours and the storage modulus E' of the base material at 120°C are both specified within specific ranges (see Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2021-119592 A Summary of the Invention [Problem to be solved by the invention]

[0007] In the manufacture of workpieces, once a support sheet has been attached to the workpiece, an anomaly may occur in which the support sheet is not attached evenly over a portion or the entire surface of the workpiece due to air bubbles getting in between the workpiece and the support sheet, making it necessary to peel the support sheet near that portion or over the entire surface from the workpiece and reattach it.

[0008] However, when the adhesive layer is energy ray curable, the adhesive strength is relatively large before the energy ray curing, so when the support sheet is attached to the workpiece and the above-mentioned abnormality occurs, it becomes difficult to peel the support sheet from the workpiece without causing a large deformation of the support sheet, and the support sheet may stretch and deform to such an extent that it is difficult to reattach the support sheet. In addition, if the support sheet is reattached, there is a risk that the chip will peel off during the subsequent dicing process. The support sheet disclosed in Patent Document 1 does not aim to solve these problems.

[0009] In addition, as described above, the work with the support sheet or the workpiece with the support sheet may be heated at a high temperature of 140° C. or more. In the case where the adhesive layer is energy ray curable, even if the adhesive strength before the energy ray curing is relatively small, after washing and removing fine foreign matter adhering to the surface of the workpiece with water, the support sheet may be heated at a high temperature of 140° C. or more to dry the workpiece, and the workpiece may not be able to be picked up from the support sheet.

[0010] The present invention aims to provide a support sheet having a base material and an adhesive layer, which can be attached to the back surface of a workpiece, and then, for the purpose of reattachment, the adhesive layer in the support sheet can be easily peeled off from the back surface of the workpiece while maintaining its shape, which can prevent chip peeling when the support sheet is reattached to the back surface of the workpiece for dicing, and which allows the workpiece to be picked up normally from the support sheet even when the support sheet with the workpiece or workpiece attached thereto is heated at a high temperature of 140° C. or higher. Another object of the present invention is to provide a method for manufacturing a workpiece using the support sheet. [Means for solving the problem]

[0011] In order to solve the above problems, the present invention employs the following configuration. [1] A support sheet comprising a substrate and an energy ray-curable adhesive layer provided on one surface of the substrate, the support sheet is attached to the mirror surface of a silicon mirror wafer by the pressure-sensitive adhesive layer, and the silicon mirror wafer with the support sheet is left to stand for 30 minutes under a temperature condition of 23° C., and the adhesive strength (X0) between the pressure-sensitive adhesive layer and the silicon mirror wafer is measured. The adhesive strength (X0) is 8000 mN / 25 mm or less, the support sheet is attached to a mirror surface of a silicon mirror wafer by the pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer after attachment is heated at 140° C., the pressure-sensitive adhesive layer after heating is energy ray-cured, and an adhesive strength (X1) between the energy ray-cured product of the pressure-sensitive adhesive layer and the silicon mirror wafer is measured, and the adhesive strength (X1) is 500 mN / 25 mm or less; a support sheet in which the support sheet is attached to a mirror surface of a silicon mirror wafer by the adhesive layer, the silicon mirror wafer with the support sheet is left to stand for 30 minutes under a temperature condition of 23°C, the support sheet is peeled off at a peeling speed of 300 mm / min so that the surface of the silicon mirror wafer to which the adhesive layer was attached and the surface of the adhesive layer to which the silicon mirror wafer was attached form an angle of 180°, the support sheet is again attached to the same position of the mirror surface of the silicon mirror wafer by the same peeled surface of the adhesive layer, the silicon mirror wafer with the support sheet is left to stand for 30 minutes under a temperature condition of 23°C, and the adhesive strength (X01) between the adhesive layer and the silicon mirror wafer after re-attachment is measured, and the adhesive strength (X01) is 2000 mN / 25 mm or more. [2] The support sheet according to [1], wherein the pressure-sensitive adhesive layer contains a block type crosslinking agent (β1). [3] The support sheet according to [1] or [2], wherein the average light transmittance (L1) of the support sheet in the wavelength range of 400 to 800 nm is 80% or more. [4] The support sheet according to any one of [1] to [3], wherein when the support sheet is attached to the surface of a stainless steel plate by the pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer after attachment is heated at 140°C, and the adhesive strength (Y2) between the pressure-sensitive adhesive layer after heating and the stainless steel plate is measured, the adhesive strength (Y2) is 6000 mN / 25 mm or less.

[0012] [5] The support sheet according to any one of [1] to [4], wherein when the support sheet is attached to a mirror surface of a silicon mirror wafer by the adhesive layer, the silicon mirror wafer with the support sheet is left to stand for 30 minutes under a temperature condition of 23°C, and the adhesive strength (X0) between the adhesive layer and the silicon mirror wafer is measured, the adhesive strength (X0) is 2000 mN / 25 mm or more. [6] The support sheet is attached to the mirror surface of a silicon mirror wafer by the pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer after attachment is heated at 130°C, the pressure-sensitive adhesive layer after heating is energy ray-cured, and the adhesive strength (X11) between the energy ray-cured product of the pressure-sensitive adhesive layer and the silicon mirror wafer is measured, and the adhesive strength (X11) between the energy ray-cured product of the pressure-sensitive adhesive layer and the silicon mirror wafer is determined to be equal to or greater than the following formula (i): Adhesive strength change rate = Adhesive strength (X1) / Adhesive strength (X11) × 100 (i) The support sheet according to any one of [1] to [5], wherein the adhesive strength change rate calculated by the above formula is 90 to 150%. [7] The support sheet according to any one of [1] to [6], wherein when the support sheet is attached to a mirror surface of a silicon mirror wafer by the pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer after attachment is energy ray-cured, the energy ray-cured product of the pressure-sensitive adhesive layer is heated at 140°C, and an adhesive strength (X3) between the heated energy ray-cured product of the pressure-sensitive adhesive layer and the silicon mirror wafer is measured, the adhesive strength (X3) is 500 mN / 25 mm or less. [8] A support sheet described in any one of [1] to [7], wherein the difference between the average light transmittance (L1) of the support sheet in a wavelength range of 400 to 800 nm and the average light transmittance (L2) of the support sheet after heating at 140°C for 2 hours in a wavelength range of 400 to 800 nm is 30% or more.

[0013] [9] The support sheet according to any one of [1] to [8], wherein a second test piece having a thickness of 200±20 μm is prepared by laminating a plurality of first test pieces of the pressure-sensitive adhesive layer each having a thickness of less than 200 μm, and the second test piece is heated from -20°C to 150°C in a tensile mode under conditions of a frequency of 11 Hz, a heating rate of 3°C / min and a uniform heating rate, and the storage modulus E' of the second test piece is measured, wherein the storage modulus (E'23) when the temperature of the second test piece is 23°C is 4.0 MPa or more.

[10] A method for manufacturing a workpiece, the method comprising: an attachment step of attaching the adhesive layer in the support sheet described in any one of [1] to [9] to the workpiece and a fixing jig to fix a support sheet-attached workpiece, the workpiece including the support sheet and the support sheet provided on the workpiece, to the fixing jig; a heating step of heating the adhesive layer in the support sheet fixed to the fixing jig after the attachment step; a processing step of processing the workpiece in the support sheet-attached workpiece fixed to the fixing jig after the attachment step, to produce the workpiece; a curing step of curing the adhesive layer attached to the fixing jig with energy rays after the heating step and the processing step; and a picking up step of separating the workpiece from the cured product of the adhesive layer and picking it up after the curing step.

[11] The method for manufacturing a workpiece described in

[10] , wherein the fixing jig is made of stainless steel. Effect of the Invention

[0014] According to the present invention, there is provided a support sheet having a base material and an adhesive layer, which is attached to the back surface of a workpiece, and then, for the purpose of reattachment, the adhesive layer in the support sheet can be easily peeled off from the back surface of the workpiece while maintaining its shape, which can prevent chip peeling when the support sheet is reattached to the back surface of the workpiece for dicing, and which allows the workpiece to be picked up normally from the support sheet even when the support sheet with the workpiece or workpiece attached thereto is heated at a high temperature of 140° C. or higher. Also, according to the present invention, there is provided a method for manufacturing a workpiece using the support sheet. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a cross-sectional view illustrating an example of a support sheet according to an embodiment of the present invention. [Diagram 2] 1A to 1C are cross-sectional views for illustrating a schematic example of a method for manufacturing a workpiece (semiconductor chip) according to an embodiment of the present invention. [Figure 3A] 1A to 1C are cross-sectional views for illustrating a schematic diagram of a portion of an example of a method for recycling a support sheet according to one embodiment of the present invention, and a portion of an example of a method for reattaching the support sheet. [Figure 3B] 1A to 1C are cross-sectional views for illustrating a schematic diagram of a portion of an example of a method for recycling a support sheet according to one embodiment of the present invention, and a portion of an example of a method for reattaching the support sheet. [Figure 3C] 1A to 1C are cross-sectional views for illustrating a schematic diagram of a portion of an example of a method for recycling a support sheet according to one embodiment of the present invention, and a portion of an example of a method for reattaching the support sheet. [Figure 3D] 10A to 10C are cross-sectional views for illustrating a part of an example of a method for reattaching a support sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] ◇Support sheet A support sheet according to one embodiment of the present invention comprises a substrate and a pressure-sensitive adhesive layer provided on one surface of the substrate, the support sheet is attached to the mirror surface of a silicon mirror wafer by the adhesive layer, and the silicon mirror wafer with the support sheet is left to stand for 30 minutes under a temperature condition of 23° C., and the adhesive strength (X0) between the adhesive layer and the silicon mirror wafer (sometimes simply referred to as "adhesive strength (X0)" in this specification) is measured. The adhesive strength (X0) is 8000 mN / 25 mm or less, the support sheet is attached to a mirror surface of a silicon mirror wafer by the pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer after attachment is heated at 140° C., the pressure-sensitive adhesive layer after heating is energy ray-cured, and an adhesive strength (X1) (sometimes simply referred to as “adhesive strength (X1)” in this specification) between the energy ray-cured product of the pressure-sensitive adhesive layer and the silicon mirror wafer is measured, the adhesive strength (X1) is 500 mN / 25 mm or less, The support sheet is attached to the mirror surface of the silicon mirror wafer by the adhesive layer, and the silicon mirror wafer with the support sheet is left to stand for 30 minutes under a temperature condition of 23° C., and then peeled off at a peeling speed of 300 mm / min so that the surface of the silicon mirror wafer to which the adhesive layer was attached and the surface of the adhesive layer to which the silicon mirror wafer was attached form an angle of 180°. The support sheet is then attached again to the same position of the mirror surface of the silicon mirror wafer by the same peeled surface of the adhesive layer, and the silicon mirror wafer with the support sheet is left to stand for 30 minutes under a temperature condition of 23° C., and the silicon mirror wafer with the support sheet is then measured for adhesive strength (X01) (sometimes simply referred to as “adhesive strength (X01)” in this specification) between the adhesive layer and the silicon mirror wafer after re-attachment, and the adhesive strength (X01) is 2000 mN / 25 mm or more.

[0017] The support sheet of this embodiment can be used, for example, in the manufacture of workpieces, as described below. The support sheet of this embodiment can be laminated with a protective film-forming film, for example, as described below, to form a composite sheet for forming a protective film.

[0018] In the support sheet of this embodiment, the adhesive strength (X0) is 8000 mN / 25 mm or less, so that when the support sheet is attached to the back surface of a workpiece and the above-mentioned abnormality occurs, the adhesive layer in the support sheet can be easily peeled off from the back surface of the workpiece while maintaining its shape for the purpose of re-attachment.

[0019] In the support sheet of this embodiment, the adhesive strength (X1) is 500 mN / 25 mm or less. For example, even if the support sheet with the work or workpiece attached thereto is heated to about 130° C. as in the present invention, there are support sheets that can normally pick up the workpiece from the hardened support sheet, but cannot normally pick up the workpiece when the heating temperature is higher, such as about 140° C. In other words, the difficulty of picking up the workpiece from the hardened support sheet can be significantly higher when the heating temperature is about 130° C. than when the heating temperature is about 140° C. In contrast, the support sheet of this embodiment has an adhesive strength (X1) of 500 mN / 25 mm or less, and therefore has high pick-up properties that enable the workpiece to be normally picked up from the cured support sheet after the adhesive layer in the support sheet is cured to form a cured support sheet, even when the heating temperature is 140°C or higher, or even higher. The heating at this time may be, for example, heating for removing foreign matter such as low molecular weight resin components adhering to the surface of the workpiece, or heating for drying the workpiece after cleaning and removing fine foreign matter that is generated during processing such as dicing the workpiece and that is adhering to the surface of the workpiece with water.

[0020] In the support sheet of this embodiment, since the adhesive strength (X01) is 2000 mN / 25 mm or more, it is possible to prevent chip peeling when the support sheet is reattached to the back surface of the workpiece and diced.

[0021] In this specification, the support sheet after the adhesive layer has cured may be referred to as a "cured support sheet" particularly to distinguish it from a support sheet in which the adhesive layer is not cured.

[0022] In this embodiment, the workpiece may be, for example, a wafer, a semiconductor device panel, or the like.

[0023] Examples of the wafer include semiconductor wafers made of elemental semiconductors such as silicon, germanium, and selenium, and compound semiconductors such as GaAs, GaP, InP, CdTe, ZnSe, and SiC; and insulating wafers made of insulators such as sapphire and glass. A circuit is formed on one surface of the workpiece, which is typically a wafer, and in this specification, the surface of the workpiece on which the circuit is formed is referred to as the "circuit surface," and the surface of the workpiece opposite the circuit surface is referred to as the "rear surface." The wafer is divided into chips by dicing or other means. In this specification, as in the case of the wafer, the surface of the chip on which the circuit is formed is referred to as the "circuit surface," and the surface of the chip opposite the circuit surface is referred to as the "back surface." It is preferable that the circuit surface of each workpiece is provided with protruding electrodes such as bumps, pillars, etc. The protruding electrodes are preferably made of solder.

[0024] The semiconductor device panel is handled during the manufacturing process of a semiconductor device, and a specific example thereof is a configuration in which a semiconductor device in which one or more electronic components are sealed with sealing resin is used, and multiple such semiconductor devices are arranged in a planar manner within an area of ​​a circular, rectangular, or other shape.

[0025] In this embodiment, the workpiece is obtained by processing the workpiece. For example, if the workpiece is a wafer, the workpiece may be a chip, and if the workpiece is a semiconductor wafer, the workpiece may be a semiconductor chip.

[0026] In this specification, the term "energy rays" refers to electromagnetic waves or charged particle beams that have an energy quantum. Examples of energy rays include ultraviolet rays, radiation, and electron beams. Ultraviolet rays can be irradiated by using, for example, a high-pressure mercury lamp, a fusion lamp, a xenon lamp, a black light, or an LED lamp as an ultraviolet ray source. Electron beams can be irradiated by generating them using an electron beam accelerator or the like. In this specification, "energy ray curable" means a property that is cured by irradiation with energy rays, and "non-energy ray curable" means a property that is not cured even when irradiated with energy rays. In this specification, the term "non-curable" refers to a property that does not cure by any means, such as heating or irradiation with energy rays.

[0027] Fig. 1 is a cross-sectional view showing a schematic example of a support sheet according to an embodiment of the present invention. In addition, the drawings used in the following description may show essential parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may not necessarily be the same as in reality.

[0028] The support sheet 1 shown here is configured to include a substrate 11 and an adhesive layer 12 provided on one surface 11a of the substrate 11. The support sheet 1 further includes a release film 13 provided on a surface 12a of the adhesive layer 12 opposite the substrate 11 side.

[0029] The pressure-sensitive adhesive layer 12 may be non-curable, but is preferably energy ray-curable.

[0030] One surface 11a of the substrate 11 (the surface on the pressure-sensitive adhesive layer 12 side) does not have to be a matte surface, but is preferably a matte surface. When one surface 11a of the substrate 11 is a matte surface, the pressure-sensitive adhesive layer 12 preferably contains a block type crosslinking agent (β1) (sometimes simply referred to as "crosslinking agent (β1)" in this specification) described below. In that case, the content of the crosslinking agent (β1) in the pressure-sensitive adhesive layer 12 is preferably 3 mass% or more relative to the total mass of the pressure-sensitive adhesive layer 12. The pressure-sensitive adhesive layer containing the crosslinking agent (β1) will be described in detail later.

[0031] In this specification, the term "matte surface" refers to a surface that is relatively rough and uneven. Such a surface has a relatively low gloss and looks like it has been matte-treated, and is therefore called a "matte surface." In the matte surface of the substrate, it is usually difficult to fill the areas of the unevenness with a pressure-sensitive adhesive layer, and voids may occur. In contrast, the pressure-sensitive adhesive layer containing the crosslinking agent (β1) as described above can sufficiently fill the areas of the unevenness.

[0032] The support sheet of this embodiment is not limited to that shown in FIG. 1, and some of the configuration may be changed, deleted, or added to that shown in FIG. 1 as long as the effects of the present invention are not impaired. For example, the support sheet 1 shown in FIG. 1 has a release film 13, but in the support sheet of this embodiment, the release film is an optional configuration, and the support sheet of this embodiment does not necessarily have to have a release film. For example, the support sheet 1 shown in FIG. 1 includes a substrate 11, an adhesive layer 12, and a release film 13, but the support sheet of this embodiment may include other layers that do not fall under any of the substrate, adhesive layer, and release film. The other layers can be selected arbitrarily depending on the purpose, and are not particularly limited. However, in the support sheet of this embodiment, it is preferable that the substrate and the adhesive layer are provided in direct contact with each other, and the adhesive layer and the release film are provided in direct contact with each other.

[0033] Next, each layer constituting the support sheet of this embodiment will be described in detail.

[0034] <<Adhesive layer, adhesive composition (I)>> The pressure-sensitive adhesive layer is in the form of a sheet or film. The pressure-sensitive adhesive layer is preferably energy ray-curable. The energy ray-curable pressure-sensitive adhesive layer can adjust its physical properties before and after curing. The pressure-sensitive adhesive layer preferably contains the crosslinking agent (β1).

[0035] The adhesive layer may consist of one layer (single layer), or may consist of two or more layers. If it consists of multiple layers, these multiple layers may be the same or different, and the combination of these multiple layers is not particularly limited.

[0036] In this specification, not limited to the case of pressure-sensitive adhesive layers, "multiple layers may be the same or different" means "all layers may be the same, all layers may be different, or only some layers may be the same", and further, "multiple layers are different" means "at least one of the constituent materials and thicknesses of each layer is different from each other".

[0037] The thickness of the adhesive layer is not particularly limited, but is preferably 1 to 100 μm, more preferably 3 to 60 μm, even more preferably 5 to 30 μm, and particularly preferably 8 to 25 μm. When the thickness of the adhesive layer is within such a range, the properties of the adhesive layer become better. For example, the adhesive layer can embed the matte surface of the base material better, and the above-mentioned pick-up property of the workpiece from the cured support sheet becomes higher. Here, "the thickness of the adhesive layer" means the thickness of the entire adhesive layer. For example, the thickness of an adhesive layer consisting of multiple layers means the total thickness of all layers that make up the adhesive layer.

[0038] In this specification, the term "thickness", not limited to that of the adhesive layer, means, unless otherwise specified, a value expressed as the average of thicknesses measured at five randomly selected points on the object, and can be obtained using a constant pressure thickness gauge in accordance with JIS K7130.

[0039] The pressure-sensitive adhesive layer can be formed using a pressure-sensitive adhesive composition (I) containing components for constituting the pressure-sensitive adhesive layer. A preferred pressure-sensitive adhesive composition (I) is, for example, a pressure-sensitive adhesive composition containing a crosslinking agent (β1). For example, the pressure-sensitive adhesive composition (I) is applied to a surface on which a pressure-sensitive adhesive layer is to be formed, and then dried as necessary to form a pressure-sensitive adhesive layer at a desired site. The ratio of the contents of the components that do not vaporize at room temperature in the pressure-sensitive adhesive composition (I) is usually the same as the ratio of the contents of the components in the pressure-sensitive adhesive layer.

[0040] In this specification, "room temperature" means a temperature that is neither particularly cooled nor heated, that is, an ordinary temperature, and examples thereof include temperatures of 18 to 28°C.

[0041] In the pressure-sensitive adhesive layer, the proportion of the total content of one or more ingredients contained in the pressure-sensitive adhesive layer, which will be described later, relative to the total mass of the pressure-sensitive adhesive layer does not exceed 100 mass %. Similarly, in the pressure-sensitive adhesive composition (I), the ratio of the total content of one or more components contained in the pressure-sensitive adhesive composition (I), which will be described later, to the total mass of the pressure-sensitive adhesive composition (I) does not exceed 100 mass%.

[0042] The pressure-sensitive adhesive composition (I) may be applied by a known method, for example, a method using various coaters such as an air knife coater, a blade coater, a bar coater, a gravure coater, a roll coater, a roll knife coater, a curtain coater, a die coater, a knife coater, a screen coater, a Mayer bar coater, or a kiss coater.

[0043] The drying conditions for the pressure-sensitive adhesive composition (I) are not particularly limited. However, when the pressure-sensitive adhesive composition (I) contains a solvent described below, it is preferable to heat-dry it. The pressure-sensitive adhesive composition (I) containing the solvent is preferably heat-dried, for example, at 70 to 130° C. for 10 seconds to 5 minutes.

[0044] When the adhesive layer is provided on the substrate, for example, the adhesive composition (I) may be applied to the substrate and dried as necessary. Alternatively, for example, the adhesive composition (I) may be applied to a release film and dried as necessary to form an adhesive layer on the release film, and the exposed surface of the adhesive layer may be attached to one surface (e.g., a matte surface) of the substrate to laminate the adhesive layer on the substrate. In this case, the release film may be removed at any timing during the manufacturing process or the use process of the support sheet.

[0045] <Crosslinking agent (β1)> The crosslinking agent (β1) is a block type crosslinking agent and may be a known one. Examples of the crosslinking agent (β1) include compounds in which a crosslinkable group such as an isocyanate group reacts with a blocking agent, and the blocking agent masks the group so that the group cannot crosslink. Such crosslinking agents (β1) (blocked crosslinking agents) are relatively stable at room temperature and can be stored for a long period of time, but at high temperatures such as 130°C or higher, the blocking agent dissociates, the mask structure is eliminated, and the crosslinkable group such as an isocyanate group is regenerated and can act as a crosslinking agent.

[0046] More specifically, the crosslinking agent (β1) may be, for example, a crosslinking agent having both a nurate skeleton (isocyanurate skeleton) that can be considered to be formed by trimerization of diisocyanate and a skeleton derived from other diisocyanates. Such a crosslinking agent (β1) is preferably a crosslinking agent having both a nurate skeleton (isocyanurate skeleton) that can be considered to be formed by trimerization of hexamethylene diisocyanate and a skeleton derived from other hexamethylene diisocyanate.

[0047] The number average molecular weight (Mn) of the crosslinking agent (β1) is preferably 15,000 or less, more preferably 13,000 or less, and may be, for example, any of 9,000 or less, 5,000 or less, and 2,500 or less. By using such a crosslinking agent (β1), the embedding property of the adhesive layer on the matte surface of the substrate is improved. Furthermore, even if the support sheet with the work or workpiece attached thereto is heated at a high temperature of 140° C. or more, the effect of being able to normally pick up the workpiece from the cured support sheet is improved. On the other hand, the lower limit of the number average molecular weight (Mn) of the crosslinking agent (β1) is not particularly limited. For example, a crosslinking agent (β1) having a number average molecular weight of 1000 or more is easier to obtain or prepare. The crosslinking agent (β1) is preferably a crosslinking agent whose number average molecular weight is within any of the above ranges and which has both a nurate skeleton (isocyanurate skeleton) that can be considered to have been formed by trimerization of the above diisocyanate and a skeleton derived from another diisocyanate.

[0048] In this specification, the terms "number average molecular weight" and "weight average molecular weight" are polystyrene-equivalent values ​​measured by gel permeation chromatography (GPC) unless otherwise specified.

[0049] Preferred commercially available crosslinking agents (β1) include, for example, Asahi Kasei Corporation's "Duranate (registered trademark) MF-K60B" (number average molecular weight 12000, viscosity at 25°C 220 mPa·s (solids concentration 60 wt%)), Asahi Kasei Corporation's "Duranate (registered trademark) TPA-B80E" (number average molecular weight 2200, viscosity at 25°C 1800 mPa·s (solids concentration 80 wt%)), Asahi Kasei Corporation's "Duranate (registered trademark) SBN-70D" (number average molecular weight 3100, viscosity at 25°C 3300 mPa·s (solids concentration 70 wt%)), and the like.

[0050] In this specification, the viscosity of the crosslinking agent (β1), its solution or its dispersion is a value measured using an E-type viscometer, unless otherwise specified.

[0051] The crosslinking agent (β1) contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0052] In the pressure-sensitive adhesive layer, the content of the crosslinking agent (β1) relative to the total mass of the pressure-sensitive adhesive layer is preferably 3% by mass or more, and may be, for example, 7% by mass or more or 11% by mass or more, while the content is preferably 25% by mass or less, and may be, for example, 20% by mass or less. This is equivalent to saying that in the pressure-sensitive adhesive composition (I), the ratio of the content of the crosslinking agent (β1) to the total content of all components other than the solvent is preferably 3 mass% or more, and may be, for example, either 7 mass% or more or 11 mass% or more, while the ratio is preferably 25 mass% or less, and may be, for example, 20 mass% or less. This is based on the fact that in the process of removing the solvent from the resin composition containing the solvent and forming the resin film, the amount of components other than the solvent usually does not change, and the content ratio of the components other than the solvent is the same between the resin composition and the resin film.Therefore, in this specification, not only in the case of the pressure-sensitive adhesive layer, but also in the case of the resin film obtained by removing the solvent from the resin composition, the content of the components other than the solvent is described below.

[0053] In the adhesive layer, the content ratio of the crosslinking agent (β1) to the total mass of the adhesive layer is 3 mass% or more, so that the adhesive strength (X1) can be easily reduced, the workpiece can be easily picked up from the support sheet, and the matte surface of the substrate can be easily embedded by the adhesive layer. The larger the ratio, the higher the effect of the present invention. On the other hand, when the ratio is equal to or less than the upper limit, the other properties of the pressure-sensitive adhesive layer become better. In one embodiment, the ratio may be, for example, any one of 3 to 25 mass%, 7 to 25 mass%, and 11 to 25 mass%, or any one of 3 to 20 mass%, 7 to 20 mass%, and 11 to 20 mass%, although these are just examples of the ratio.

[0054] In this way, the adhesive layer on the matte surface of the substrate has a high embedding property, and therefore the average light transmittance of the support sheet in the visible light region is high. Therefore, when the workpiece obtained by processing the workpiece using the support sheet is held on the support sheet, the inspection accuracy is high when the workpiece is inspected for damage such as cracks and chips, so-called chipping, through the support sheet. Examples of the light transmittance in the visible light region include light transmittance in the wavelength range of 400 to 800 nm (sometimes referred to as "light transmittance (400 to 800 nm)" in this specification). Furthermore, the adhesive layer on the matte surface of the substrate has a high embedding property, and therefore the adhesive layer can be normally irradiated when the adhesive layer is cured by irradiating the adhesive layer with energy rays through the substrate, and the adhesive layer can be normally cured.

[0055] <Crosslinking agent (β2)> The pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) preferably further contain a non-blocking type crosslinking agent (β2) (sometimes simply referred to as "crosslinking agent (β2)" in this specification). The crosslinking agent (β2) is a non-blocking type crosslinking agent that does not fall under the category of the crosslinking agent (β1), and may be a known crosslinking agent. By containing not only the crosslinking agent (β1) but also the crosslinking agent (β2) in the adhesive layer, it becomes easier to set the adhesive strength (X0), adhesive strength (X1) and adhesive strength (X01) within the ranges described below, and the support sheet becomes more likely to exhibit the above-mentioned effects.

[0056] Furthermore, since the adhesive layer contains the crosslinking agent (β1) and the crosslinking agent (β2), the adhesive force (X1) described later can be made smaller, and even after the work with the support sheet (a work with a support sheet comprising a work and a support sheet provided on the work) or the workpiece with the support sheet (a workpiece with a support sheet comprising a workpiece and a support sheet provided on the workpiece) is heated at a high temperature of 140°C or higher, the adhesive layer in the support sheet is cured to form a cured support sheet, and the pick-up ability is easily improved so that the workpiece can be normally picked up from the cured support sheet. Examples of heating at this time include the same as those described above.

[0057] Examples of the crosslinking agent (β2) include isocyanate-based crosslinking agents (crosslinking agents having an isocyanate group) such as tolylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, and adducts of these diisocyanates; epoxy-based crosslinking agents (crosslinking agents having a glycidyl group) such as ethylene glycol glycidyl ether; aziridine-based crosslinking agents (crosslinking agents having an aziridinyl group) such as hexa[1-(2-methyl)-aziridinyl]triphosphatriazine; metal chelate-based crosslinking agents (crosslinking agents having a metal chelate structure) such as aluminum chelate; and isocyanurate-based crosslinking agents (crosslinking agents having an isocyanuric acid skeleton). Among these, the crosslinking agent (β2) is preferably an adduct of hexamethylene diisocyanate or an isocyanurate-modified product of hexamethylene diisocyanate, since it is easier to set the adhesive strength (X0), adhesive strength (X1) and adhesive strength (X01) within the ranges described below.

[0058] The crosslinking agent (β2) contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0059] In the pressure-sensitive adhesive layer, the content ratio of the crosslinking agent (β2) relative to the total mass of the pressure-sensitive adhesive layer is preferably 0.3% by mass or more, and may be, for example, any one of 0.6% by mass or more, 0.9% by mass or more, and 1.2% by mass or more. On the other hand, the content ratio is preferably 15% by mass or less, and may be, for example, 10% by mass or less, 5% by mass or less, or 3% by mass or less. When the content of the crosslinking agent (β2) is equal to or more than the lower limit, the effect obtained by using the crosslinking agent (β2) is enhanced. When the content of the crosslinking agent (β2) is equal to or less than the upper limit, excessive use of the crosslinking agent (β2) is suppressed. Furthermore, the embedding property of the matte surface of the substrate is improved. In one embodiment, the content of the crosslinking agent (β2) may be, for example, any one of 0.3 to 15 parts by mass, 0.6 to 15 parts by mass, 0.9 to 15 parts by mass, and 1.2 to 15 parts by mass, or any one of 0.3 to 10 parts by mass, 0.3 to 5 parts by mass, and 0.3 to 3 parts by mass, although these are only examples of the content of the crosslinking agent (β2).

[0060] In the adhesive layer, the ratio of the total content of the crosslinking agent (β1) and the crosslinking agent (β2) to the total mass of the adhesive layer is preferably 3% by mass or more, and may be, for example, any of 7% by mass or more, 11% by mass or more, and 13% by mass or more. When the ratio of the total content is equal to or more than the lower limit, the effect obtained by using the crosslinking agent (β1) and the crosslinking agent (β2) becomes higher. Furthermore, even when the support sheet with the work or the workpiece attached thereto is heated at a high temperature of 140°C or more, it becomes easier to set the adhesive strength (X1) to the range described below. On the other hand, the ratio of the total content is preferably 40% by mass or less, and may be, for example, 30% by mass or less. When the ratio of the total content is equal to or less than the upper limit, excessive use of the crosslinking agent (β1) and the crosslinking agent (β2) is suppressed. In one embodiment, the percentage of the total content may be, for example, any one of 3 to 40 mass%, 7 to 40 mass%, 11 to 40 mass%, and 13 to 40 mass%, or any one of 3 to 30 mass%, 7 to 30 mass%, 11 to 30 mass%, and 13 to 30 mass%, but these are only examples of the percentage of the total content.

[0061] <Energy ray curable acrylic resin (Ia)> The pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) preferably further contain an energy ray-curable acrylic resin (also referred to as "energy ray-curable acrylic resin (Ia)" in this specification). By using a pressure-sensitive adhesive layer containing the energy ray-curable acrylic resin (Ia) and the crosslinking agent (β1), and optionally the crosslinking agent (β2), it becomes easier to set the adhesive strength (X0), adhesive strength (X1) and adhesive strength (X01) within the ranges described below, and the support sheet becomes more likely to exhibit the above-mentioned effects.

[0062] The energy ray-curable acrylic resin (Ia) may, for example, be a resin having a structure in which an unsaturated group is introduced into the side chain of a non-energy ray-curable acrylic resin.

[0063] [Non-energy ray curable acrylic resin] The non-energy ray curable acrylic resin may be, for example, an acrylic polymer having a constituent unit derived from an alkyl (meth)acrylate ester and a constituent unit derived from a functional group-containing monomer.

[0064] In this specification, the term "(meth)acrylic acid" is a concept that includes both "acrylic acid" and "methacrylic acid". The same applies to terms similar to (meth)acrylic acid. For example, the term "(meth)acryloyl group" is a concept that includes both "acryloyl group" and "methacryloyl group", and the term "(meth)acrylate" is a concept that includes both "acrylate" and "methacrylate".

[0065] The (meth)acrylic acid alkyl ester may, for example, be one in which the carbon number of the alkyl group constituting the alkyl ester is 1 to 20. The alkyl group constituting the alkyl ester may be any one of linear, branched, and cyclic, but is preferably linear or branched.

[0066] Among the (meth)acrylic acid alkyl esters, examples of those in which the alkyl group is linear or branched include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), and the like.

[0067] Among the (meth)acrylic acid alkyl esters, examples in which the alkyl group is cyclic include isobornyl (meth)acrylate and dicyclopentanyl (meth)acrylate.

[0068] Among the above, the (meth)acrylic acid alkyl ester is preferably 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, dodecyl acrylate (lauryl acrylate), or dodecyl methacrylate (lauryl methacrylate), in terms of ease of adjusting the adhesive strength (X0), adhesive strength (X1), and adhesive strength (X01) to the desired values.

[0069] Examples of the functional group-containing monomer include those in which the functional group reacts with the crosslinking agent (β1) or the crosslinking agent (β2) to become a crosslinking starting point, and those in which the functional group reacts with a group in an unsaturated group-containing compound described below that can bond (react) with a non-energy ray-curable acrylic resin to enable the introduction of an unsaturated group into a side chain of an acrylic polymer.

[0070] Examples of the functional group-containing monomer include a hydroxyl group-containing monomer, a carboxyl group-containing monomer, an amino group-containing monomer, and an epoxy group-containing monomer.

[0071] Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and non-(meth)acrylic unsaturated alcohols (unsaturated alcohols not having a (meth)acryloyl skeleton) such as vinyl alcohol and allyl alcohol. Among these, the hydroxyl group-containing monomer is preferably a hydroxyalkyl methacrylate, and more preferably 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, or 2-hydroxybutyl methacrylate, in terms of ease of adjusting the adhesive strength (X0), adhesive strength (X1), and adhesive strength (X01) to the desired values.

[0072] Examples of the carboxy group-containing monomer include ethylenically unsaturated monocarboxylic acids (monocarboxylic acids having an ethylenically unsaturated bond) such as (meth)acrylic acid and crotonic acid; ethylenically unsaturated dicarboxylic acids (dicarboxylic acids having an ethylenically unsaturated bond) such as fumaric acid, itaconic acid, maleic acid and citraconic acid; anhydrides of the ethylenically unsaturated dicarboxylic acids; and (meth)acrylic acid carboxyalkyl esters such as 2-carboxyethyl methacrylate.

[0073] Examples of the epoxy group-containing monomer include glycidyl group-containing (meth)acrylic acid esters such as glycidyl (meth)acrylate.

[0074] The functional group-containing monomer is preferably a hydroxyl group-containing monomer.

[0075] The non-energy ray curable acrylic resin may have a constituent unit derived from another monomer which does not fall into either the constituent unit derived from an alkyl (meth)acrylate ester or the constituent unit derived from the functional group-containing monomer.

[0076] The other monomer is not particularly limited as long as it is copolymerizable with the (meth)acrylic acid alkyl ester and the like. Examples of the other monomers include styrene, α-methylstyrene, vinyl toluene, vinyl formate, vinyl acetate, acrylonitrile, and acrylamide.

[0077] The constituent units derived from the (meth)acrylic acid alkyl ester, the constituent units derived from the functional group-containing monomer, and the constituent units derived from the other monomers contained in the non-energy ray-curable acrylic resin may each be of only one type or of two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0078] In the non-energy ray-curable acrylic resin, the content of structural units derived from an alkyl (meth)acrylate is preferably 65 to 99 mass % based on the total amount of structural units.

[0079] In the non-energy ray-curable acrylic resin, the content of the structural unit derived from the functional group-containing monomer is preferably 1 to 35 mass % based on the total amount of the structural units.

[0080] In the non-energy ray-curable acrylic resin, the content of the structural units derived from the other monomers is preferably 0 to 10% by mass based on the total amount of the structural units.

[0081] The energy ray-curable acrylic resin (Ia) can be obtained, for example, by reacting the functional group in the non-energy ray-curable acrylic resin with an unsaturated group-containing compound having an energy ray-polymerizable unsaturated group.

[0082] [Unsaturated group-containing compound] The unsaturated group-containing compound is a compound that has, in addition to the energy ray-polymerizable unsaturated group, a group that can bond to the non-energy ray-curable acrylic resin by reacting with a functional group in the non-energy ray-curable acrylic resin. Examples of the energy ray-polymerizable unsaturated group include a (meth)acryloyl group, a vinyl group (ethenyl group), and an allyl group (2-propenyl group), and the like, with a (meth)acryloyl group being preferred. Examples of the group capable of bonding to the functional group in the non-energy ray-curable acrylic resin include an isocyanate group and a glycidyl group capable of bonding to a hydroxyl group or an amino group, and a hydroxyl group and an amino group capable of bonding to a carboxy group or an epoxy group.

[0083] Examples of the unsaturated group-containing compound include (meth)acryloyloxyethyl isocyanate, (meth)acryloyl isocyanate, and glycidyl (meth)acrylate.

[0084] When the functional group in the non-energy ray curable acrylic resin is reacted with an unsaturated group-containing compound having an energy ray polymerizable unsaturated group to obtain the energy ray curable acrylic resin (Ia), the total number of moles of the functional group-binding group in the unsaturated group-containing compound relative to the total number of moles of the functional group in the non-energy ray curable acrylic resin is preferably 0.35 to 0.75 times, and may be, for example, 0.5 to 0.75 times, 0.35 to 0.6 times, or 0.5 to 0.6 times. By having the total number of moles of the functional group-binding group in such a range, the adhesive strength (X1) described later can be made smaller, and the pick-up property of the workpiece from the cured support sheet tends to be made higher. On the other hand, the total number of moles of groups capable of bonding to the functional groups in the unsaturated group-containing compound is preferably 1 or less times the total number of moles of the functional groups in the non-energy ray-curable acrylic resin.

[0085] The energy ray-curable acrylic resin (Ia) contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0086] When the adhesive layer and the adhesive composition (I) contain the energy ray curable acrylic resin (Ia), the content ratio of the energy ray curable acrylic resin (Ia) in the adhesive layer relative to the total mass of the adhesive layer is preferably 50 to 95 mass%, and may be, for example, any of 65 to 95 mass% and 75 to 95 mass%, or any of 50 to 90 mass%, 50 to 85 mass%, and 60 to 85 mass%, or may be 65 to 85 mass%. When the ratio is equal to or greater than the lower limit, the pick-up property that allows the above-mentioned workpiece to be picked up from the support sheet without any abnormality is improved. When the ratio is equal to or less than the upper limit, the embedding property of the adhesive layer on the matte surface of the substrate is improved.

[0087] <Other ingredients> The pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may contain other components that do not fall under any of the energy ray-curable acrylic resin (Ia), the crosslinking agent (β1), and the crosslinking agent (β2), within a range that does not impair the effects of the present invention. Examples of the other components include an energy ray curable compound (α), a photopolymerization initiator (γ), and additives.

[0088] The other components contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type only, or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0089] [Energy ray curable compound (α)] The energy ray-curable compound (α) is not particularly limited as long as it is an energy ray-curable component that does not fall under the category of the energy ray-curable acrylic resin (Ia).

[0090] Examples of the energy ray-curable compound (α) include monomers or oligomers that have an energy ray-polymerizable unsaturated group and can be cured by irradiation with energy rays. One molecule of the energy ray-curable compound (α) has one or two or more, and may have three or more, energy ray-polymerizable unsaturated groups, but preferably has one or two. An example of the energy ray-polymerizable unsaturated group is a (meth)acryloyl group.

[0091] The molecular weight of the energy ray-curable compound (α) is not particularly limited, but is preferably not more than 500. By using such an energy ray-curable compound (α), the embedding property of the pressure-sensitive adhesive layer on the matte surface of the substrate is improved. The molecular weight of the energy ray curable compound (α) is preferably 100 to 500. When the molecular weight is equal to or more than the lower limit, the structure of the pressure-sensitive adhesive layer becomes more stable. However, these are only examples of the molecular weight of the energy ray curable compound (α).

[0092] The energy ray-curable compound (α) contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0093] In the adhesive layer, the content ratio of the energy ray curable compound (α) to the total mass of the adhesive layer is preferably 0 to 5 mass%. The higher the ratio, the higher the effect obtained by using the energy ray curable compound (α). When the ratio is equal to or less than the upper limit, the matte surface of the substrate is more easily embedded by the adhesive layer, and further, even when the support sheet with the work or workpiece attached thereto is heated at a high temperature of 140°C or more, the effect of being able to normally pick up the workpiece from the support sheet is improved.

[0094] [Photopolymerization initiator (γ)] When the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) contain either one or both of the energy ray-curable acrylic resin (Ia) and the energy ray-curable compound (α), the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) preferably contain a photopolymerization initiator (γ). The pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) containing the photopolymerization initiator (γ) sufficiently undergo a curing reaction even when irradiated with a relatively low-energy energy ray such as ultraviolet light.

[0095] Examples of the photopolymerization initiator (γ) include benzoin compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin methyl benzoate, and benzoin dimethyl ketal; acetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2,2-dimethoxy-1,2-diphenylethane-1-one, 2-hydroxy-1-(4-(4- Acetophenone compounds such as (2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-(dimethylamino)-4'-morpholinobutylphenone, 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)butan-1-one; bis(2,4,6-trimethylbenzoyl)phenyl acylphosphine oxide compounds such as phenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; oxime ester compounds such as ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime); sulfide compounds such as benzyl phenyl sulfide and tetramethylthiuram monosulfide; α-ketol compounds such as 1-hydroxycyclohexyl phenyl ketone Examples of suitable amines include azo compounds such as azobisisobutyronitrile, titanocene compounds such as titanocene, thioxanthone compounds such as thioxanthone, peroxide compounds, diketone compounds such as diacetyl, benzyl, dibenzyl, benzophenone, 2,4-diethylthioxanthone, 1,2-diphenylmethane, 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone, and quinone compounds such as 1-chloroanthraquinone and 2-chloroanthraquinone. As the photopolymerization initiator (γ), for example, a photosensitizer such as an amine can be used.

[0096] The photopolymerization initiator (γ) contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0097] The photopolymerization initiator (γ) has high heat resistance even under heating conditions of 140° C. or more, and exhibits a stronger effect. In this respect, it is preferable that the photopolymerization initiator (γ) is one or more selected from the group consisting of 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone, 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)butan-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime).

[0098] As these photopolymerization initiators (γ), the following are commercially available products. 2-Hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one: "Omnirad (registered trademark) 127" manufactured by IGM Resins 2-Methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one: "Omnirad (registered trademark) 907" manufactured by IGM Resins 2-Benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone: "Omnirad (registered trademark) 369" manufactured by IGM Resins 2-Dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)butan-1-one: "Omnirad (registered trademark) 379EG" manufactured by IGM Resins 2,4,6-trimethylbenzoyldiphenylphosphine oxide: "Omnirad (registered trademark) TPO H" manufactured by IGM Resins Ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) "Omnirad (registered trademark) OXE02" manufactured by IGM Resins

[0099] When the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) contain a photopolymerization initiator (γ), the content of the photopolymerization initiator (γ) in the pressure-sensitive adhesive layer is preferably 1 to 5 parts by mass relative to 100 parts by mass of the total content of the energy ray curable acrylic resin (Ia) and the energy ray curable compound (α), and may be, for example, any of 1.5 to 4.5 parts by mass and 2 to 4 parts by mass. When the content of the photopolymerization initiator (γ) is equal to or more than the lower limit, the effect obtained by using the photopolymerization initiator (γ) is further enhanced. When the content of the photopolymerization initiator (γ) is equal to or less than the upper limit, excessive use of the photopolymerization initiator (γ) is suppressed. Here, when the adhesive layer does not contain the energy ray curable acrylic resin (Ia), the content of the energy ray curable acrylic resin (Ia) in the adhesive layer is set to 0 parts by mass, and when the adhesive layer does not contain the energy ray curable compound (α), the content of the energy ray curable compound (α) in the adhesive layer is set to 0 parts by mass.

[0100] [Additives] Examples of the additives include known additives such as antistatic agents, antioxidants, softeners (plasticizers), fillers, rust inhibitors, colorants (pigments, dyes), sensitizers, tackifiers, reaction retarders, and crosslinking accelerators (catalysts). The reaction retarder is, for example, a component that suppresses the progress of unintended crosslinking reaction in the pressure-sensitive adhesive composition (I) during storage due to the action of a catalyst mixed in the pressure-sensitive adhesive composition (I). Examples of reaction retarders include those that form a chelate complex by chelating with a catalyst, and more specifically, components having two or more carbonyl groups (-C(=O)-) in one molecule.

[0101] The additives contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0102] The content of the additive in the pressure-sensitive adhesive composition (I) is not particularly limited and may be appropriately selected depending on the type of additive.

[0103] [solvent] The pressure-sensitive adhesive composition (I) may contain a solvent. By containing a solvent, the pressure-sensitive adhesive composition (I) has improved suitability for application to a surface to be coated.

[0104] The solvent is preferably an organic solvent, and examples of the organic solvent include ketones such as methyl ethyl ketone and acetone; esters (carboxylates) such as ethyl acetate; ethers such as tetrahydrofuran and dioxane; aliphatic hydrocarbons such as cyclohexane and n-hexane; aromatic hydrocarbons such as toluene and xylene; and alcohols such as 1-propanol and 2-propanol.

[0105] The pressure-sensitive adhesive composition (I) may contain only one type of solvent, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0106] The content of the solvent in the pressure-sensitive adhesive composition (I) is not particularly limited and may be appropriately adjusted.

[0107] [Gas Generator] The pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) preferably do not contain a gas generating agent as the other component. The gas generating agent is a component that generates gas by an external stimulus such as heating or light irradiation. By using a pressure-sensitive adhesive layer containing a gas generating agent, gas is generated at the interface between the pressure-sensitive adhesive layer and the adherend, and the peeling force (adhesive force) between the pressure-sensitive adhesive layer or its energy ray cured product and the adherend can be reduced by the pressure of the gas. Therefore, by using a pressure-sensitive adhesive layer containing a gas generating agent, it may be possible to easily pick up the workpiece from the cured product of the pressure-sensitive adhesive layer in the pick-up step in the manufacturing method of the workpiece described later. However, when an adhesive layer containing a gas generating agent is used, it may be difficult to adjust the peeling force (adhesive force) between the adhesive layer or its energy ray cured product and the adherend, and excessive fluctuations in the peeling force may not be suppressed. In such a case, the pick-up of the workpiece from the cured product of the adhesive layer in the pick-up process may become unstable. Furthermore, the gas generating agent may remain at the part of the workpiece that was in contact with the cured product of the adhesive layer. In such a case, the gas generating agent may be taken into the interior of the semiconductor device, which is the final target, and the reliability of the semiconductor device may be reduced. Therefore, it is preferable that the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) do not contain a gas-generating agent.

[0108] Among the gas generating agents, examples of components that generate gas when irradiated with light include carboxylic acid compounds (compounds having a carboxy group), salts of the carboxylic acid compounds, tetrazole, salts of tetrazole, tetrazole derivatives (compounds having a structure in which one or two hydrogen atoms in tetrazole are replaced with groups other than hydrogen atoms), and salts of the tetrazole derivatives. The carboxylic acid compound and its salt generate carbon dioxide gas in response to an external stimulus, and the tetrazole and its salt, and the tetrazole derivative and its salt generate nitrogen gas in response to an external stimulus.

[0109] In this specification, unless otherwise specified, the term "group" includes not only an atomic group formed by bonding multiple atoms, but also a single atom.

[0110] The gas generating agent may be, for example, a component that has heat resistance and does not decompose under temperature conditions of about 200° C. or less, but generates gas when irradiated with light such as ultraviolet light.

[0111] <One embodiment of the pressure-sensitive adhesive layer> An example of a preferred pressure-sensitive adhesive layer and pressure-sensitive adhesive composition (I) is a pressure-sensitive adhesive layer containing a crosslinking agent (β1), a crosslinking agent (β2), an energy ray-curable acrylic resin (Ia), and a photopolymerization initiator (γ).

[0112] In terms of obtaining the effects of the present invention more remarkably, a more preferred pressure-sensitive adhesive layer is, for example, a pressure-sensitive adhesive layer that contains a crosslinking agent (β1) and a crosslinking agent (β2) and is energy ray curable. Such a pressure-sensitive adhesive layer may further contain an energy ray curable acrylic resin (Ia) and a photopolymerization initiator (γ). For the same reason, a more preferred pressure-sensitive adhesive layer is, for example, a pressure-sensitive adhesive layer that contains a crosslinking agent (β1) and a crosslinking agent (β2) and is energy ray curable, the number average molecular weight of the crosslinking agent (β1) being 15000 or less, and the content of the crosslinking agent (β1) relative to the total mass of the pressure-sensitive adhesive layer being 3 mass% or more. Such a pressure-sensitive adhesive layer may further contain an energy ray curable acrylic resin (Ia) and a photopolymerization initiator (γ).

[0113] In the adhesive layer, the ratio of the total content of the crosslinking agent (β1), the crosslinking agent (β2), the energy ray curable acrylic resin (Ia), and the photopolymerization initiator (γ) to the total mass of the adhesive layer is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and may be, for example, any of 97% by mass or more and 99% by mass or more. When the ratio is equal to or more than the lower limit, the adhesive strength (X0), adhesive strength (X1), and adhesive strength (X01) can be more easily reduced to the range described below, and the adhesive layer in the support sheet can be more easily peeled off from the back surface of the workpiece while maintaining its shape, and the workpiece can be more easily picked up normally from the support sheet. Furthermore, other properties of the adhesive layer that are different from this become better. On the other hand, the ratio is 100% by mass or less.

[0114] <Method for producing pressure-sensitive adhesive composition (I)> The adhesive composition (I) can be obtained by blending the components for constituting the adhesive composition (I), such as a crosslinking agent (β1), optionally a crosslinking agent (β2), optionally an energy ray-curable acrylic resin (Ia), and optionally the other components (e.g., one or more selected from the group consisting of an energy ray-curable compound (α), a photopolymerization initiator (γ), an additive, and a solvent). The order of addition of the components when blending is not particularly limited, and two or more components may be added simultaneously. The method for mixing the components during blending is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or stirring blade, a method of mixing using a mixer, a method of mixing by adding ultrasound, etc. The temperature and time during addition and mixing of each component are not particularly limited as long as the components do not deteriorate, and may be adjusted appropriately. A temperature of 15 to 30°C is preferred.

[0115] <<Base material>> The substrate is in the form of a sheet or film, and examples of the constituent materials thereof include various resins. Examples of the resin include polyethylenes such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and high-density polyethylene (HDPE); polyolefins other than polyethylene such as polypropylene, polybutene, polybutadiene, polymethylpentene, and norbornene resin; ethylene-based copolymers (copolymers obtained by using ethylene as a monomer) such as ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester copolymer, and ethylene-norbornene copolymer; vinyl chloride-based resins (copolymers obtained by using vinyl chloride as a monomer) such as polyvinyl chloride and vinyl chloride copolymer. resins having aromatic ring groups); polystyrene; polycycloolefins; polyesters such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polyethylene isophthalate, polyethylene-2,6-naphthalenedicarboxylate, and wholly aromatic polyesters in which all constituent units have aromatic cyclic groups; copolymers of two or more of the above polyesters; poly(meth)acrylic acid esters; polyurethanes; polyurethane acrylates; polyimides; polyamides; polycarbonates; fluororesins; polyacetals; modified polyphenylene oxides; polyphenylene sulfides; polysulfones; and polyether ketones. The resin may be, for example, a polymer alloy such as a mixture of the polyester and other resins. The polymer alloy of the polyester and other resins is preferably one in which the amount of the resin other than the polyester is relatively small. Examples of the resin include crosslinked resins in which one or more of the resins exemplified above are crosslinked; and modified resins such as ionomers using one or more of the resins exemplified above.

[0116] Among the above, the resin constituting the substrate is preferably polypropylene or polybutylene terephthalate, in that it provides the substrate with higher heat resistance at high temperatures (eg, 140° C. or higher) and flexibility.

[0117] The resin constituting the substrate may be of only one type, or of two or more types. When two or more types are used, the combination and ratio thereof can be selected arbitrarily.

[0118] The substrate may contain, in addition to the main constituent materials such as the resin, various known additives such as fillers, colorants, antioxidants, organic lubricants, catalysts, and softeners (plasticizers).

[0119] In the support sheet, since the pressure-sensitive adhesive layer is energy ray curable, the substrate is preferably one that transmits energy rays, and is preferably transparent.

[0120] It is preferable that at least one surface of the substrate is a matte surface, and both surfaces may be matte surfaces, or one surface may be a matte surface and the other surface may be a glossy surface with a small degree of unevenness. When at least one surface of the substrate is a matte surface, the support sheet preferably has an adhesive layer provided on the matte surface of the substrate, and when both surfaces of the substrate are matte surfaces, the adhesive layer is preferably provided on the matte surface having a larger surface roughness (Ra).

[0121] The matte surface of the substrate is a surface of the substrate having a roughness of a certain value or more, and has a low gloss, so that it can be clearly identified by its appearance. Substrates having at least one matte surface are commercially available, and can also be prepared by known methods.

[0122] The surface roughness (Ra) of the matte surface of the substrate is preferably 0.05 μm or more, and may be, for example, any of 0.1 μm or more, 0.4 μm or more, and 0.7 μm or more. When the surface roughness is equal to or more than the lower limit, the effect of the present invention that the matte surface of the substrate is highly embedded by the adhesive layer can be obtained more significantly. In addition, blocking of the substrate when the substrates are stored in a stacked state is more suppressed. The upper limit of the surface roughness (Ra) of the matte surface of the substrate is not particularly limited. For example, the surface roughness is preferably 2 μm or less so that the surface irregularity does not become excessively large. In one embodiment, the surface roughness (Ra) of the matte surface of the substrate may be, for example, any one of 0.05 to 2 μm, 0.1 to 2 μm, 0.4 to 2 μm, and 0.7 to 2 μm, although these are just examples of the surface roughness.

[0123] In this specification, the term "surface roughness (Ra)" is not limited to the matte surface of the substrate, but means the so-called arithmetic mean roughness determined in accordance with JIS B0601:2001.

[0124] The surface roughness (Ra) of the glossy surface of the substrate is preferably less than 0.05 μm, and may be, for example, 0.04 μm or less. When the surface roughness is in this range, the average light transmittance of the support sheet described below in the wavelength range of 400 to 800 nm becomes higher. The lower limit of the surface roughness (Ra) of the glossy surface of the substrate is not particularly limited. For example, the surface roughness is preferably 0.01 μm or more in order to prevent blocking of the substrate when the substrates are stored in a stacked state. In one embodiment, the surface roughness (Ra) of the glossy surface of the substrate may be, for example, any one of 0.01 μm or more and less than 0.05 μm, and 0.01 to 0.04 μm, although these are just examples of the surface roughness.

[0125] The surface roughness (Ra) of both sides of the substrate can be adjusted, for example, by the molding conditions of the substrate, the surface treatment conditions, etc. Examples of the surface treatment include a roughening treatment such as sandblasting or solvent treatment, and a smoothing treatment such as polishing.

[0126] In order to adjust the adhesiveness with the pressure-sensitive adhesive layer provided thereon, the surface of the substrate may be subjected to oxidation treatment such as corona discharge treatment, electron beam irradiation treatment, plasma treatment, ozone / ultraviolet irradiation treatment, flame treatment, chromic acid treatment, hot air treatment, lipophilic treatment, hydrophilic treatment, etc. The surface of the substrate may be treated with a primer.

[0127] The substrate may consist of one layer (single layer), or may consist of two or more layers. When the substrate consists of multiple layers, the multiple layers may be the same or different, and the combination of the multiple layers is not particularly limited.

[0128] The thickness of the substrate is preferably 50 to 300 μm, and more preferably 60 to 100 μm. By setting the thickness of the substrate within this range, the heat resistance (e.g., 140° C. or higher), flexibility, and suitability for attachment to a workpiece of the support sheet are improved. Here, the "thickness of the substrate" means the thickness of the entire substrate. For example, the thickness of a substrate consisting of multiple layers means the total thickness of all layers constituting the substrate.

[0129] The substrate can be produced by a known method. For example, a substrate containing a resin can be produced by molding a resin composition containing the resin.

[0130] <<Release film>> The release film may be a known one. More specifically, the release film may be, for example, a release film substrate having one or both sides treated for release. The release film substrate is preferably a polyethylene terephthalate film. The release treated surface can be formed by subjecting the surface of the substrate for the release film to a release treatment with a known release treating agent. The thickness of the release film may be, for example, from 2 to 300 μm, and is preferably from 20 to 100 μm.

[0131] Next, the physical properties of the support sheet (adhesive layer) will be described.

[0132] <Adhesive strength (X0)> The adhesive strength (X0) is 8000 mN / 25 mm or less, may be 7500 mN / 25 mm or less, may be 7000 mN / 25 mm or less, or may be 6800 mN / 25 mm or less. By using a support sheet with a small adhesive strength (X0), when an abnormality occurs when the support sheet is attached to the back surface of a workpiece, the adhesive layer in the support sheet can be easily peeled off from the back surface of the workpiece while maintaining its shape for the purpose of reattachment.

[0133] The adhesive strength (X0) is preferably 2000 mN / 25 mm or more, more preferably 3000 mN / 25 mm or more, even more preferably 4000 mN / 25 mm or more, and particularly preferably 5000 mN / 25 mm or more. By using a support sheet with a large adhesive strength (X0), even if a force is applied by the workpiece in a state where the workpiece or workpiece is attached to the support sheet, such as processing that places a load on the workpiece (e.g., dicing of a semiconductor wafer) or washing with water that places a load on the workpiece (e.g., washing with water of a semiconductor chip after dicing), peeling of the workpiece from the support sheet is suppressed.

[0134] In one embodiment, the adhesive strength (X0) may be, for example, any one of 2000 to 8000 mN / 25 mm, 3000 to 7500 mN / 25 mm, 4000 to 7000 mN / 25 mm, and 5000 to 6800 mN / 25 mm, although these are only examples of the adhesive strength (X0).

[0135] The adhesive strength (X0) can be measured, for example, by the following method. That is, a silicon mirror wafer with a test piece is prepared in the same manner as in the measurement of the adhesive strength (X1), and this silicon mirror wafer with the test piece is left to stand and stored at a temperature of 23° C. for 30 minutes. Next, at room temperature, the test piece is peeled off from the silicon mirror wafer after the static storage at a peeling speed of 300 mm / min. At this time, the test piece is peeled off in its length direction so that the surface of the silicon mirror wafer to which the test piece was attached forms an angle of 180° with the surface of the test piece to which the silicon mirror wafer was attached, that is, a so-called 180° peeling is performed. Then, the load (peeling force) at this 180° peeling is measured, and the measurement length is set to 50 mm, and the measurement value at the first 5 mm length and the measurement value at the last 5 mm length are excluded from the effective value. Then, the average value of the measured values ​​is adopted as the adhesive strength (X0) (mN / 25 mm). In this embodiment, such measurement of the peel strength may be performed on two or more test pieces (support sheets), and the average value of the obtained measured values ​​may be used as the adhesive strength (X0).

[0136] <Adhesive strength (X1)> The adhesive strength (X1) is 500 mN / 25 mm or less, and may be, for example, any of 400 mN / 25 mm or less, 350 mN / 25 mm or less, and 310 mN / 25 mm or less. The smaller the adhesive strength (X1), the higher the pick-up ability, which allows the workpiece or workpiece to be normally picked up from the cured support sheet, even when the support sheet with the workpiece or workpiece attached thereto is heated at a high temperature of 140° C. or more. The lower limit of the adhesive strength (X1) is not particularly limited. For example, an adhesive layer having an adhesive strength (X1) of 30 mN / 25 mm or more can be formed more easily. In one embodiment, the adhesive strength (X1) may be, for example, any one of 30 to 500 mN / 25 mm, 30 to 400 mN / 25 mm, 30 to 350 mN / 25 mm, and 30 to 310 mN / 25 mm, although these are only examples of the adhesive strength (X1).

[0137] The adhesive strength (X1) can be measured, for example, by the method shown below. That is, first, a test piece having a width of 25 mm is cut out from the support sheet. Next, the test piece (support sheet) is attached to the mirror surface of the silicon mirror wafer by the adhesive layer therein to prepare a silicon mirror wafer with the test piece attached. The attachment is preferably performed at room temperature, at an attachment speed of 290 to 310 mm / min, and with an attachment pressure of 0.3 MPa, using a laminating roller. Next, the obtained silicon mirror wafer with the test piece is heated at 140° C. for 2 hours. Next, the silicon mirror wafer with the test piece was cooled down to 23°C by standing, and then exposed to an illumination of 230mW / cm 2 , light intensity 200mJ / cm 2 Under the above condition, the adhesive layer in the silicon mirror wafer with the test piece after cooling is irradiated with energy rays through the substrate to harden the adhesive layer in the test piece. Next, the test piece is peeled off from the silicon mirror wafer at room temperature with a peeling speed of 300 mm / min. At this time, the test piece is peeled off in its length direction so that the surface of the silicon mirror wafer to which the test piece was attached forms an angle of 180° with the surface of the test piece to which the silicon mirror wafer was attached, that is, a so-called 180° peeling is performed. Then, the load (peeling force) at this 180° peeling is measured, and the measurement length is set to 50 mm, and the measurement value at the first 5 mm length and the measurement value at the last 5 mm length are excluded from the effective value. Then, the average value of the measured values ​​is adopted as the adhesive strength (X1) (mN / 25 mm). In this embodiment, such measurement of the peel strength may be performed on two or more test pieces (support sheets), and the average value of the obtained measured values ​​may be used as the adhesive strength (X1).

[0138] <Adhesive strength (X01)> The adhesive strength (X01) is 2000 mN / 25 mm or more, and may be, for example, 3000 mN / 25 mm or more, 4000 mN / 25 mm or more, or 5000 mN / 25 mm or more. The greater the adhesive strength (X01), the more likely it is that chip peeling will be prevented when the support sheet is reattached to the back surface of the workpiece and diced. The upper limit of the adhesive strength (X01) is not particularly limited. For example, a pressure-sensitive adhesive layer having an adhesive strength (X01) of 12000 mN / 25 mm or less can be formed more easily. In one embodiment, the adhesive strength (X01) may be, for example, any one of 2000 to 12000 mN / 25 mm, 3000 to 10000 mN / 25 mm, 4000 to 8500 mN / 25 mm, and 5000 to 7500 mN / 25 mm, although these are just examples of the adhesive strength (X01).

[0139] The adhesive strength (X01) can be measured, for example, by the method shown below. That is, first, a test piece having a width of 25 mm is cut out from the support sheet. Next, the test piece (support sheet) is attached to the mirror surface of the silicon mirror wafer by the adhesive layer therein to prepare a silicon mirror wafer with the test piece attached. The attachment is preferably performed at room temperature, at an attachment speed of 290 to 310 mm / min, and with an attachment pressure of 0.3 MPa, using a laminating roller. Next, the silicon mirror wafer with the test piece attached is left to stand for 30 minutes under a temperature condition of 23° C., and then the test piece is peeled off from the silicon mirror wafer at a peeling speed of 300 mm / min under room temperature. At this time, the test piece is peeled off in its length direction so that the surface of the silicon mirror wafer to which the test piece was attached forms an angle of 180° with the surface of the silicon mirror wafer to which the silicon mirror wafer was attached, that is, a so-called 180° peeling is performed. Next, the same test piece is attached again to the same position of the mirror surface of the same silicon mirror wafer by the same peeled surface of the adhesive layer of the same test piece, to prepare a silicon mirror wafer with the test piece. The attachment is also preferably performed at room temperature, at an attachment speed of 290 to 310 mm / min, and with an attachment pressure of 0.3 MPa, using a laminating roller. Next, the silicon mirror wafer with the test piece attached is left to stand for 30 minutes under a temperature condition of 23° C., and then the test piece is peeled off from the silicon mirror wafer at room temperature at a peeling speed of 300 mm / min. At this time, the test piece is peeled in its length direction so that the surface of the silicon mirror wafer to which the test piece was attached forms an angle of 180° with the surface of the test piece to which the silicon mirror wafer was attached, i.e., a so-called 180° peel is performed. Then, the load (peel force) at this 180° peel is measured, and the measurement length is set to 50 mm, and the measurement value at the first 5 mm length and the measurement value at the last 5 mm length are excluded from the effective value. Then, the average value of the measurements is adopted as the adhesive strength (X01) (mN / 25 mm). In this embodiment, such measurement of the peel strength may be performed on two or more test pieces (support sheets), and the average value of the obtained measured values ​​may be used as the adhesive strength (X01).

[0140] <Adhesive strength (X3)> The support sheet is attached to the mirror surface of the silicon mirror wafer by the adhesive layer, the adhesive layer after attachment is energy ray cured, the energy ray cured product of the adhesive layer is heated at 140°C, and the adhesive force (X3) (sometimes simply referred to as "adhesive force (X3)" in this specification) between the heated product of the energy ray cured product of the adhesive layer and the silicon mirror wafer is measured. In the manufacturing method of the workpiece to be described later, the support sheet (adhesive layer) is heated and the adhesive layer in the support sheet is energy ray cured in this order. However, by using such a support sheet, even if the adhesive layer in the support sheet is energy ray cured and the cured support sheet (energy ray cured product of the adhesive layer) is heated in this order, the pick-up ability is improved so that the workpiece can be normally picked up from the cured support sheet when the support sheet with the workpiece or workpiece attached thereto is heated at a high temperature of 140°C or higher. Therefore, the support sheet can be applied to a wide variety of methods for manufacturing workpieces, and is highly versatile in terms of usage.

[0141] The adhesive strength (X3) may be, for example, 400 mN / 25 mm or less, 350 mN / 25 mm or less, or 310 mN / 25 mm or less. The smaller the adhesive strength (X3), the higher the pick-up ability, which allows the workpiece to be picked up from the cured support sheet without any problems, as described above. The lower limit of the adhesive strength (X3) is not particularly limited. For example, an adhesive layer having an adhesive strength (X3) of 30 mN / 25 mm or more can be formed more easily. In one embodiment, the adhesive strength (X3) may be, for example, any one of 30 to 500 mN / 25 mm, 30 to 400 mN / 25 mm, 30 to 350 mN / 25 mm, and 30 to 310 mN / 25 mm, although these are just examples of the adhesive strength (X3).

[0142] The adhesive strength (X3) can be measured, for example, by the method shown below. That is, a silicon mirror wafer with a test piece was prepared in the same manner as when measuring the adhesive strength (X1), and the illuminance was 230 mW / cm 2 , light intensity 200mJ / cm 2 Under the above conditions, the adhesive layer in the silicon mirror wafer with the test piece is irradiated with energy rays through the substrate, thereby hardening the adhesive layer in the test piece. Next, the silicon mirror wafer with the test piece attached thereto after being irradiated with the energy rays (after the adhesive layer is cured with the energy rays) is heated at 140° C. for 2 hours. Next, the silicon mirror wafer with the heated test piece is allowed to cool until its temperature reaches 23°C. Next, the test piece is peeled off from the silicon mirror wafer at room temperature with a peeling speed of 300 mm / min. At this time, the test piece is peeled off in its length direction so that the surface of the silicon mirror wafer to which the test piece was attached forms an angle of 180° with the surface of the test piece to which the silicon mirror wafer was attached, that is, a so-called 180° peeling is performed. Then, the load (peeling force) at this 180° peeling is measured, and the measurement length is set to 50 mm, and the measurement value at the first 5 mm length and the measurement value at the last 5 mm length are excluded from the effective value. Then, the average value of the measured values ​​is adopted as the adhesive strength (X3) (mN / 25 mm). In this embodiment, such measurement of the peel strength may be performed on two or more test pieces (support sheets), and the average value of the obtained measured values ​​may be used as the adhesive strength (X3).

[0143] <Adhesive strength change rate> The support sheet is attached to the mirror surface of a silicon mirror wafer by the pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer after attachment is heated at 130° C., the pressure-sensitive adhesive layer after heating is energy ray-cured, and the adhesive strength (X11) (sometimes simply referred to as “adhesive strength (X11)” in this specification) between the energy ray-cured product of the pressure-sensitive adhesive layer and the silicon mirror wafer is measured, and the adhesive strength (X11) (sometimes simply referred to as “adhesive strength (X11)” in this specification) between the energy ray-cured product of the pressure-sensitive adhesive layer and the silicon mirror wafer is expressed by the following formula (i): Adhesive strength change rate = Adhesive strength (X1) / Adhesive strength (X11) × 100 (i) It is preferable that the adhesive strength change rate calculated by (sometimes simply referred to as "adhesive strength change rate" in this specification) is 90 to 150%. In the manufacturing method of the workpiece described later, it is assumed that the support sheet (adhesive layer) is heated at a temperature of 140°C or more and the adhesive layer in the support sheet after heating is cured with energy rays. By using such a support sheet, even if the support sheet (adhesive layer) is heated at 130°C, the workpiece can be picked up from the cured support sheet without any abnormality under the same conditions as when the support sheet is heated at a temperature of 140°C or more. Therefore, the support sheet does not require any change in the condition settings of the device when the workpiece is manufactured, and is highly versatile in terms of setting the heating temperature.

[0144] The rate of change in adhesive strength may be, for example, any one of 100 to 150%, 120 to 150%, and 130 to 150%, any one of 90 to 140%, 90 to 130%, and 90 to 120%, or may be 100 to 140%.

[0145] The rate of change in adhesive strength can be calculated, for example, by the following method. That is, the adhesive force (X11) between the energy ray-cured product of the adhesive layer after heating and the silicon mirror wafer is measured in the same manner as in measuring the adhesive force (X1), except that the heating temperature of the silicon mirror wafer with the test piece is 130° C. instead of 140° C. In this case, as in the case of the adhesive force (X1), the peel force between the silicon mirror wafer and the test piece is measured for two or more test pieces (support sheets), and the average value of the obtained multiple measured values ​​may be used as the adhesive force (X11). Then, the adhesive strength change rate is calculated according to the formula (i) using the adhesive strength (X1) value measured by the method described above and the adhesive strength (X11) value.

[0146] <Adhesive strength (X11)> The adhesive strength (X11) is not particularly limited as long as it does not impair the effects of the present invention, but is preferably a value that causes the adhesive strength change rate to be in the above-mentioned range. The adhesive strength (X11) is preferably, for example, 30 to 560 mN / 25 mm, and may be, for example, any one of 30 to 500 mN / 25 mm, 70 to 450 mN / 25 mm, and 100 to 400 mN / 25 mm.

[0147] <Adhesive strength (Y2)> When the support sheet is attached to the surface of a stainless steel (SUS) plate by the adhesive layer, the adhesive layer after attachment is heated at 140° C., and the adhesive strength (Y2) between the adhesive layer after heating and the stainless steel plate (sometimes simply referred to as "adhesive strength (Y2)" in this specification) is measured, the adhesive strength (Y2) is preferably 6000 mN / 25 mm or less. In the manufacturing method of a workpiece processed product described later, a workpiece with a support sheet is produced in an intermediate step, and the workpiece with the support sheet is fixed to a fixing jig by the adhesive layer therein. By using the support sheet as described above, when the workpiece with the support sheet fixed to the fixing jig is heated at a high temperature of 140° C. or more, the workpiece with the support sheet can be peeled off from the fixing jig without further curing the adhesive layer with energy rays, and furthermore, the adhesive layer can be suppressed from remaining on the fixing jig. Therefore, the support sheet enables the adoption of a highly versatile method as a manufacturing method of a workpiece processed product, and is highly versatile in terms of use.

[0148] Fixing jigs such as ring frames are usually made of metal such as SUS. The support sheet of the present embodiment is also effective for fixing jigs made of metals other than SUS.

[0149] The adhesive strength (Y2) may be, for example, any one of 5000 mN / 25 mm or less, 3800 mN / 25 mm or less, and 2600 mN / 25 mm or less. The smaller the adhesive strength (Y2), the easier it is to peel off the work with the support sheet from the fixing jig, as described above. On the other hand, the adhesive strength (Y2) is preferably 2000 mN / 25 mm or more. By using such a support sheet, when the workpiece with the support sheet is heated in a state where it is fixed to the fixing jig in the heating step of the manufacturing method of the workpiece to be described later, unintended peeling of the workpiece with the support sheet from the fixing jig is suppressed. In one embodiment, the adhesive strength (Y2) may be, for example, any one of 2000 to 6000 mN / 25 mm, 2000 to 5000 mN / 25 mm, 2000 to 3800 mN / 25 mm, and 2000 to 2600 mN / 25 mm, although these are just examples of the adhesive strength (Y2).

[0150] The adhesive strength (Y2) can be measured, for example, by the following method. That is, first, a test piece having a width of 25 mm is cut out from the support sheet. Next, the test piece (support sheet) is attached to one side of a 1000 μm thick SUS plate by the adhesive layer in the support sheet to prepare a SUS plate with a test piece attached. The attachment is preferably performed at room temperature, at an attachment speed of 290 to 310 mm / min, and with an attachment pressure of 0.3 MPa, using a laminating roller. Next, the obtained SUS plate with the test piece attached is heated at 140°C for 2 hours. Next, the SUS plate with the test piece is cooled to 23°C by natural cooling, and then the test piece is peeled off from the SUS plate at room temperature at a peeling speed of 300mm / min. At this time, the test piece is peeled off in its length direction so that the surface of the SUS plate to which the test piece was attached forms an angle of 180° with the surface of the SUS plate to which the test piece was attached, that is, a so-called 180° peeling is performed. Then, the load (peel force) at this 180° peeling is measured, and the measurement length is set to 50mm, and the measurement value at the first 5mm length and the measurement value at the last 5mm length are excluded from the effective value. Then, the average value of the measured values ​​is adopted as the adhesive strength (Y2) (mN / 25mm). In this embodiment, such measurement of the peel strength may be performed on two or more test pieces (support sheets), and the average value of the obtained measured values ​​may be used as the adhesive strength (Y2).

[0151] <Method of adjusting adhesive strength of adhesive layer> The various adhesive strengths of the adhesive layer described above, i.e., the adhesive strength (X1) between the energy ray-cured product of the adhesive layer after heating at 140°C and the silicon mirror wafer; the adhesive strength (X3) between the heated energy ray-cured product of the adhesive layer and the silicon mirror wafer; the adhesive strength (X0) between the adhesive layer and the silicon mirror wafer; the adhesive strength (X11) between the energy ray-cured product of the adhesive layer after heating at 130°C and the silicon mirror wafer; and the adhesive strength (Y2) between the adhesive layer after heating at 140°C and a SUS plate, can be adjusted by adjusting the types and contents of the components contained in the adhesive layer.

[0152] For example, the adhesive strength (X1) can be reduced by incorporating an energy ray-curable acrylic resin (Ia) having a structural unit derived from a functional group-containing monomer having a methacryloyl group into the pressure-sensitive adhesive layer. For example, the adhesive strength (X1) can be reduced by including an energy ray-curable acrylic resin (Ia) having a relatively high glass transition temperature in the adhesive layer. For example, when a functional group in the acrylic polymer (e.g., a hydroxyl group) is reacted with a group capable of bonding to the functional group in the unsaturated group-containing compound (e.g., an isocyanate group in (meth)acryloyloxyethyl isocyanate), the total number of moles of groups capable of bonding to the functional group in the unsaturated group-containing compound is increased relative to the total number of moles of the functional groups in the acrylic polymer to prepare an energy ray-curable acrylic resin (Ia). By incorporating such an energy ray-curable acrylic resin (Ia) in the pressure-sensitive adhesive layer, the adhesive strength (X1) can be reduced. For example, in an adhesive layer containing an energy ray-curable acrylic resin (Ia) and a crosslinking agent (β2), by using a crosslinking agent (β2) having a ring structure, the adhesive strength (X1) tends to be smaller than when a crosslinking agent having a chain structure without a ring structure is used. For example, in a pressure-sensitive adhesive layer containing an energy ray-curable acrylic resin (Ia) and a crosslinking agent (β2), by using a crosslinking agent (β2) that does not have a urethane bond, the adhesive strength (X1) tends to be smaller than when a crosslinking agent having a urethane bond, such as a trimethylolpropane adduct of diisocyanate, is used.

[0153] For example, when the pressure-sensitive adhesive layer does not contain the energy ray-curable compound (α), the adhesive strength (Y2) can be made smaller than when the pressure-sensitive adhesive layer contains the energy ray-curable compound (α). For example, when using an energy ray-curable acrylic resin (Ia) obtained by reacting a functional group (e.g., a hydroxyl group) in the acrylic polymer with a group capable of bonding to the functional group in the unsaturated group-containing compound (e.g., an isocyanate group in (meth)acryloyloxyethyl isocyanate), the adhesive strength (Y2) can be reduced by incorporating into the adhesive layer an energy ray-curable acrylic resin (Ia) having a large amount of unreacted functional groups derived from the acrylic polymer (in other words, having a large amount of functional groups capable of reacting with the crosslinking agent (β1) or the crosslinking agent (β2)). For example, by increasing the total content of the crosslinking agent (β1) and the crosslinking agent (β2) in the pressure-sensitive adhesive layer, the adhesive strength (Y2) can be reduced. For example, in an adhesive layer containing an energy ray-curable acrylic resin (Ia) and a crosslinking agent (β2), by using a crosslinking agent (β2) having a ring structure, the adhesive strength (Y2) tends to be smaller than when a crosslinking agent having a chain structure without a ring structure is used. For example, in an adhesive layer containing an energy ray-curable acrylic resin (Ia) and a crosslinking agent (β2), by using a crosslinking agent (β2) that does not have a urethane bond, the adhesive strength (Y2) tends to be smaller than when a crosslinking agent having a urethane bond, such as a trimethylolpropane adduct of diisocyanate, is used.

[0154] For example, when using an energy ray-curable acrylic resin (Ia) obtained by reacting a functional group (e.g., a hydroxyl group) in the acrylic polymer with a group capable of bonding to the functional group in the unsaturated group-containing compound (e.g., an isocyanate group in (meth)acryloyloxyethyl isocyanate), the adhesive strength (X0) can be reduced by including in the adhesive layer an energy ray-curable acrylic resin (Ia) having a large amount of unreacted functional groups derived from the acrylic polymer (in other words, having a large amount of functional groups capable of reacting with the crosslinking agent (β2)). For example, by increasing the content of the crosslinking agent (β2) in the pressure-sensitive adhesive layer, the adhesive strength (X0) can be reduced.

[0155] For example, the adhesive strength (X3) can be reduced by incorporating an energy ray-curable acrylic resin (Ia) having a structural unit derived from a functional group-containing monomer having a methacryloyl group into the pressure-sensitive adhesive layer. For example, the adhesive strength (X3) can be reduced by including in the adhesive layer an energy ray-curable acrylic resin (Ia) having a relatively high glass transition temperature. For example, when a functional group in the acrylic polymer (e.g., a hydroxyl group) is reacted with a group capable of bonding to the functional group in the unsaturated group-containing compound (e.g., an isocyanate group in (meth)acryloyloxyethyl isocyanate), the total number of moles of groups capable of bonding to the functional group in the unsaturated group-containing compound is increased relative to the total number of moles of the functional groups in the acrylic polymer to prepare an energy ray-curable acrylic resin (Ia). By incorporating such an energy ray-curable acrylic resin (Ia) in the pressure-sensitive adhesive layer, the adhesive strength (X3) can be reduced. For example, in an adhesive layer containing an energy ray-curable acrylic resin (Ia) and a crosslinking agent (β2), by using a crosslinking agent (β2) having a ring structure, the adhesive strength (X3) tends to be smaller than when a crosslinking agent having a chain structure without a ring structure is used. For example, in a pressure-sensitive adhesive layer containing an energy ray-curable acrylic resin (Ia) and a crosslinking agent (β2), by using a crosslinking agent (β2) that does not have a urethane bond, the adhesive strength (X3) tends to be smaller than when a crosslinking agent having a urethane bond, such as a trimethylolpropane adduct of diisocyanate, is used.

[0156] For example, the adhesive strength (X11) can be reduced by incorporating an energy ray-curable acrylic resin (Ia) having a structural unit derived from a functional group-containing monomer having a methacryloyl group into the pressure-sensitive adhesive layer. For example, by incorporating an energy ray-curable acrylic resin (Ia) having a relatively high glass transition temperature into the pressure-sensitive adhesive layer, the adhesive strength (X11) can be reduced. For example, when a functional group in the acrylic polymer (e.g., a hydroxyl group) is reacted with a group capable of bonding to the functional group in the unsaturated group-containing compound (e.g., an isocyanate group in (meth)acryloyloxyethyl isocyanate), the total number of moles of groups capable of bonding to the functional group in the unsaturated group-containing compound is increased relative to the total number of moles of the functional groups in the acrylic polymer to prepare an energy ray-curable acrylic resin (Ia). By incorporating such an energy ray-curable acrylic resin (Ia) in the pressure-sensitive adhesive layer, the adhesive strength (X11) can be reduced.

[0157] For example, when using an energy ray-curable acrylic resin (Ia) obtained by reacting a functional group (e.g., a hydroxyl group) in the acrylic polymer with a group capable of bonding to the functional group in the unsaturated group-containing compound (e.g., an isocyanate group in (meth)acryloyloxyethyl isocyanate), the adhesive strength (X01) can be increased by including in the adhesive layer an energy ray-curable acrylic resin (Ia) having fewer unreacted functional groups derived from the acrylic polymer (in other words, having fewer functional groups capable of reacting with the crosslinking agent (β2)). For example, by reducing the content of the crosslinking agent (β2) in the pressure-sensitive adhesive layer, the adhesive strength (X01) can be increased.

[0158] <Storage modulus (E'23)> The storage modulus (E'23) is the storage modulus when a second test piece having a thickness of 200±20 μm is prepared by stacking a plurality of first test pieces of the pressure-sensitive adhesive layer, and the storage modulus E' of the second test piece is measured while heating the second test piece from -20°C to 150°C in a tensile mode under conditions of a frequency of 11 Hz, a heating rate of 3°C / min and a uniform heating rate, and the temperature of the second test piece is 23°C.

[0159] The storage modulus (E'23) is preferably 4.0 MPa or more, and may be, for example, any one of 4.5 MPa or more, 4.8 MPa or more, and 5.0 MPa or more. The larger the storage modulus (E'23), the more the deformation of the support sheet can be suppressed when an abnormality occurs in the support sheet attached to the workpiece and the support sheet is peeled off from the workpiece, and the roughness of the surface of the adhesive layer can be prevented. Therefore, uniform re-attachment is possible within the plane of the adhesive layer, and the support sheet has excellent reusability. In addition, the adhesive layer can be suppressed from remaining on the workpiece, and the reworkability is excellent.

[0160] The upper limit of the storage modulus (E'23) is not particularly limited. The storage modulus (E'23) may be 12 MPa or less, 10 MPa or less, 8 MPa or less, or 7 MPa or less. In one embodiment, the storage modulus (E'23) may be, for example, any one of 4.0 to 12 MPa, 4.5 to 20 MPa, 4.8 to 8 MPa, and 5.0 to 7 MPa, although these are only examples of the storage modulus (E'23).

[0161] The storage modulus (E'23) can be measured, for example, by the following method. That is, first, a plurality of pressure-sensitive adhesive layers each having a thickness of less than 200 μm are prepared, and these are used as the first test pieces. The first test pieces may be, for example, slices cut to a desired size from the pressure-sensitive adhesive layer to be measured. Next, these first test pieces (adhesive layers) are laminated together in the thickness direction to produce a laminate having a thickness of 200±20 μm (i.e., 180 to 220 μm). Further, a piece having a width of 4 mm is cut out from the laminate to serve as a second test piece. Next, the second test piece is held at two points with an interval of 20 mm, and in this state, the storage modulus E' of the second test piece is measured under the condition of a frequency of 11 Hz while the temperature of the second test piece is raised uniformly from -20°C to 150°C at a rate of 3°C / min. Then, the storage modulus E' of the second test piece when the temperature is 23°C is adopted as the storage modulus (E'23). The second test piece is held at two points spaced 20 mm apart, which means that the length of the portion of the second test piece subject to measurement of the storage modulus E' is 20 mm.

[0162] The second test piece can be held at the two locations using, for example, a known holding means such as a gripping tool.

[0163] The number of first test pieces after heating that constitute the second test piece is not particularly limited as long as it is two or more, and can be selected arbitrarily depending on the thickness of each first test piece (adhesive layer). For example, five heated first test pieces each having a thickness of 40 μm can be used to prepare the second test piece having a thickness of 200 μm. Also, fourteen heated first test pieces each having a thickness of 15 μm can be used to prepare the second test piece having a thickness of 210 μm. However, these are merely examples, and the number and thickness of the first test pieces used are not limited to these.

[0164] The storage modulus (E'23) can be adjusted by adjusting the types and contents of the components contained in the pressure-sensitive adhesive layer. For example, by reducing the content of the energy ray-curable compound (α) in the pressure-sensitive adhesive layer, the storage modulus (E'23) can be increased. For example, when using an energy ray-curable acrylic resin (Ia) obtained by reacting a functional group (e.g., a hydroxyl group) in the acrylic polymer with a group capable of bonding to the functional group in the unsaturated group-containing compound (e.g., an isocyanate group in (meth)acryloyloxyethyl isocyanate), the storage modulus (E'23) can be increased by incorporating into the adhesive layer an energy ray-curable acrylic resin (Ia) having a large amount of unreacted functional groups derived from the acrylic polymer (in other words, having a large amount of functional groups capable of reacting with the crosslinking agent (β2)). For example, by increasing the content of the crosslinking agent (β2) in the pressure-sensitive adhesive layer, the storage modulus (E′23) can be increased. For example, in an adhesive layer containing an energy ray-curable acrylic resin (Ia) and a crosslinking agent (β2), the storage modulus (E'23) tends to be greater when a crosslinking agent (β2) having a chain structure and no ring structure is used than when a crosslinking agent having a ring structure is used. For example, in an adhesive layer containing an energy ray-curable acrylic resin (Ia) and a crosslinking agent (β2), the storage modulus (E'23) tends to be greater when a crosslinking agent (β2) having a urethane bond, such as a trimethylolpropane adduct of diisocyanate, is used than when a crosslinking agent not having a urethane bond is used.

[0165] <Average light transmittance (400-800 nm) of support sheet (L1)> The average value (L1) of the light transmittance (400-800 nm) of the support sheet (sometimes simply referred to in this specification as the "average value (L1) of the light transmittance of the support sheet" or the "average value (L1)") is preferably 80% or more, and may be, for example, either 82% or more or 83.5% or more. When the average value (L1) of the light transmittance (400-800 nm) is equal to or more than the lower limit, the inspection accuracy is improved when inspecting the workpiece for damage such as cracks or chips (e.g., chipping) through the support sheet while the workpiece is held on the support sheet.

[0166] The upper limit of the average light transmittance (L1) of the support sheet is not particularly limited. For example, a support sheet having an average light transmittance (L1) of 95% or less can be more easily manufactured. In one embodiment, the average light transmittance (L1) of the support sheet may be, for example, any one of 80 to 95%, 82 to 95%, and 83.5 to 95%, although these are just examples of the average value (L1). However, in this specification, unless otherwise specified, the light transmittance of the support sheet is not limited to the light transmittance in the wavelength range of 400 to 800 nm, but means the light transmittance of the support sheet in a state in which no release film is provided.

[0167] The average light transmittance (L1) of the support sheet can be calculated, for example, by the method shown below. That is, the support sheet is irradiated with light from the outside of the substrate side, and the light transmittance is measured by direct light reception without using an integrating sphere. The light transmittance value T(1) at a wavelength of n (nm) in 1 nm increments in the wavelength range of 400 to 800 nm is calculated. n (wherein n is an integer of 400 to 800) is measured. Then, T(1) when n is 400 to 800 is measured. n Add up all the values ​​and get the total value T(1) 400-800 Calculate the obtained T(1) 400-800 , T(1) n Divide by the number of measurements (i.e., 800-400+1=401) (T(1) 400-800 / 401), the average light transmittance (L1) of the support sheet can be calculated.

[0168] The average light transmittance (L1) of the support sheet can be adjusted, for example, by adjusting the types and contents of the components contained in the substrate, the roughness of both surfaces of the substrate (for example, surface roughness (Ra)), and the like. The average light transmittance (L1) of the support sheet can also be adjusted by adjusting the types and contents of the components contained in the pressure-sensitive adhesive layer.

[0169] <Light transmittance difference> The difference between the average light transmittance (L1) of the support sheet (400-800 nm) and the average light transmittance (L2) of the support sheet after heating at 140° C. for 2 hours (hereinafter, sometimes simply referred to as the “average light transmittance (L2) of the support sheet after heating” or “average light transmittance (L2)”) (hereinafter, sometimes referred to as the “light transmittance difference”) is preferably 30% or more, and may be, for example, any of 34% or more, 38% or more, and 42% or more. When the light transmittance difference ([average light transmittance (L1) of the support sheet)]-[average light transmittance (L2) of the support sheet after heating)]) is the lower limit or more, the support sheet clearly discolors (more specifically, whitens) and changes in appearance when heated at a high temperature of 140° C. or more. Therefore, when the support sheet is heated at such a high temperature, the support sheet becomes more identifiable (the support sheet can be more easily identified), and the history of the support sheet being heated at such a high temperature can be easily confirmed. The upper limit of the light transmittance difference of the support sheet is not particularly limited. For example, a support sheet having a light transmittance difference of 60% or less can be more easily manufactured. In one embodiment, the light transmittance difference may be, for example, any one of 30 to 60%, 34 to 60%, 38 to 60%, and 42% to 60%, although these are just examples of the light transmittance difference.

[0170] The reason why the support sheet heated at a higher temperature turns white is unclear, but it is speculated that this is because the relatively low molecular weight component and the high molecular weight component coexist in the pressure-sensitive adhesive layer after heating, causing phase separation of these components. For example, the relatively low molecular weight component is assumed to be an oligomer, which is a reaction product between crosslinkers (β1), a blocking agent separated from the crosslinker (β1), etc., and for example, the high molecular weight component is assumed to be a crosslinked energy ray curable acrylic resin (Ia), etc.

[0171] The average light transmittance (L2) of the support sheet after heating can be calculated, for example, by the method shown below. That is, the support sheet is heated at 140° C. for 2 hours. Next, the support sheet is cooled to a temperature of 23°C by natural cooling, and then the support sheet after cooling is irradiated with light from the outside of the substrate side, and the light transmittance is measured by direct light reception without using an integrating sphere. Then, in the same manner as in the case of the average light transmittance (L1) of the support sheet, that is, in the wavelength range of 400 to 800 nm, the light transmittance value T(2) at a wavelength of n (nm) at 1 nm intervals is measured. n (wherein n is an integer of 400 to 800) is measured. Then, T(2) when n is 400 to 800 is measured. n Add up all the values ​​and get the total T(2) 400-800 Calculate the obtained T(2) 400-800 , T(2) n Divide by the number of measurements (i.e., 800-400+1=401) (T(2) 400-800 / 401), the average light transmittance (L2) of the support sheet after heating can be calculated. Next, the difference between the average light transmittance (L1) of the support sheet and the average light transmittance (L2) of the support sheet after heating is calculated, thereby making it possible to calculate the light transmittance difference.

[0172] The average light transmittance (L2) of the support sheet after heating can be adjusted, for example, by adjusting the types and contents of the components contained in the substrate and the roughness of both surfaces of the substrate (for example, surface roughness (Ra)). The average light transmittance (L2) of the support sheet after heating can also be adjusted by adjusting the types and contents of the components contained in the pressure-sensitive adhesive layer.

[0173] <Example of support sheet> In addition to the upper limit of the adhesive strength (X0), the adhesive strength (X1), and the adhesive strength (X01), it is preferable that the support sheet further has one or more selected from the group consisting of the average light transmittance (L1), the adhesive strength (Y2), the lower limit of the adhesive strength (X0), the adhesive strength change rate (=adhesive strength (X1) / adhesive strength (X11)×100), the adhesive strength (X3), the light transmittance difference (=[the average light transmittance of the support sheet (L1)]−[the average light transmittance of the support sheet after heating (L2)]) and the storage modulus (E'23) within any of the numerical ranges described above. That is, an example of a preferable support sheet is, for example, a support sheet that satisfies the following conditions (1-1), (1-2), and (1-3): (1-1) The adhesive strength (X0) between the adhesive layer and the silicon mirror wafer is 8000 mN / 25 mm or less. (1-2) The adhesive strength (X1) between the energy ray-cured product of the pressure-sensitive adhesive layer and the silicon mirror wafer is 500 mN / 25 mm or less. (1-3) After re-attachment, the adhesive strength (X01) between the pressure-sensitive adhesive layer and the silicon mirror wafer is 2000 mN / 25 mm or more. and the following conditions (1-4) to (1-10): (1-4) The average light transmittance (L1) in the wavelength range of 400 to 800 nm is 80% or more. (1-5) The adhesive strength (Y2) between the pressure-sensitive adhesive layer and the stainless steel plate after heating is 6000 mN / 25 mm or less. (1-6) When the adhesive strength (X0) between the adhesive layer and the silicon mirror wafer is measured, the adhesive strength (X0) is 2000 mN / 25 mm or more. (1-7) The adhesive strength change rate is 90 to 150%. (1-8) The adhesive strength (X3) between the heated energy ray-cured product of the pressure-sensitive adhesive layer and the silicon mirror wafer is 500 mN / 25 mm or less. (1-9) The light transmittance difference is 30% or more. (1-10) The storage modulus (E'23) is 4.0 MPa or more. and a support sheet satisfying one or more of the following requirements: An example of a more preferable support sheet is one that satisfies all of the above conditions (1-1) to (1-10). In the support sheet exemplified here, in addition to the upper limit of the adhesive strength (X0), the adhesive strength (X1) and the adhesive strength (X01), it is particularly preferable that one or more selected from the group consisting of the average light transmittance (L1), the adhesive strength (Y2), the lower limit of the adhesive strength (X0), the adhesive strength change rate, the adhesive strength (X3), the light transmittance difference and the storage modulus (E'23) are further limited to any of the numerical ranges described above.

[0174] ◇ Manufacturing method of support sheet The support sheet can be manufactured by laminating the above-mentioned layers constituting the support sheet so as to have a corresponding positional relationship, and adjusting the shape of some or all of the layers as necessary. The method of forming each layer is as described above. For example, when at least one surface of the substrate is a matte surface and an adhesive layer is provided on the matte surface, the above-mentioned adhesive composition (I) can be applied to the matte surface and dried as necessary to produce a support sheet.

[0175] The support sheet can also be produced by applying the pressure-sensitive adhesive composition (I) to one side of a release film, drying it as necessary to form a pressure-sensitive adhesive layer on the release film, and bonding the exposed surface of the pressure-sensitive adhesive layer to one side of a substrate. In this case, the pressure-sensitive adhesive composition (I) is preferably applied to the release-treated surface of the release film.

[0176] The pressure applied when bonding the adhesive layer to the substrate in this manner (application pressure) is preferably 0.2 to 0.6 MPa. When the pressure is equal to or greater than the lower limit, the adhesive strength between the adhesive layer and the substrate can be sufficiently increased, and the adhesive layer can be more easily embedded into the matte surface of the substrate. When the pressure is equal to or less than the upper limit, excessive pressure can be avoided. Such bonding of the pressure-sensitive adhesive layer and the substrate is preferably carried out under temperature conditions of, for example, 15° C. or higher, but may be carried out at room temperature.

[0177] The support sheet having the other layer can be produced, for example, by applying a composition for forming the other layer to an appropriate location on the substrate or the pressure-sensitive adhesive layer, drying the composition as necessary to form the other layer, and laminating a further required layer as necessary. The support sheet can also be produced by laminating a film-like other layer to an appropriate location on the substrate or the pressure-sensitive adhesive layer to provide the other layer, and laminating a further required layer as necessary.

[0178] ◇Composite sheet for forming protective film The support sheet can be laminated with a protective film-forming film to form a composite sheet for forming a protective film. That is, the composite sheet for forming a protective film includes the support sheet and a protective film-forming film provided on the surface of the pressure-sensitive adhesive layer in the support sheet opposite to the substrate side. More specifically, the composite sheet for forming a protective film includes a substrate, a pressure-sensitive adhesive layer provided on one surface of the substrate, and a protective film-forming film provided on the surface of the pressure-sensitive adhesive layer opposite to the substrate side. The composite sheet for forming a protective film may further include a release film provided on the surface of the protective film-forming film opposite to the pressure-sensitive adhesive layer side.

[0179] <<Protective film forming film>> The protective film forming film is a film for forming a protective film at any location of the workpiece. By using the composite sheet for forming a protective film, a workpiece with a protective film can be manufactured, which includes a workpiece and a protective film provided at any location of the workpiece. For example, when the workpiece is a wafer, the composite sheet for forming a protective film can be used to manufacture a chip with a protective film, which includes a chip and a protective film provided on the back surface of the chip.

[0180] The protective film-forming film may be curable or non-curable. That is, the protective film-forming film may function as a protective film by being cured, or may function as a protective film in an uncured state. The curable protective film-forming film may be either heat-curable or energy ray-curable, or may have both heat-curable and energy ray-curable properties.

[0181] The protective film-forming film may be made of one layer (single layer) or may be made of two or more layers. When the protective film-forming film is made of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited.

[0182] The thermosetting protective film-forming film may, for example, contain a polymer component (A) and a thermosetting component (B). Examples of the polymer component (A) include acrylic resins, urethane resins, phenoxy resins, silicone resins, and saturated polyester resins. Examples of the thermosetting component (B) include epoxy-based thermosetting resins, thermosetting polyimide resins, and unsaturated polyester resins. In this specification, the thermosetting polyimide resin is a general term for a polyimide precursor that forms a polyimide resin by thermal curing, and a thermosetting polyimide. The epoxy thermosetting resin is composed of an epoxy resin (B1) and a thermosetting agent (B2).

[0183] In addition to these components, the thermosetting protective film-forming film may further contain one or more selected from the group consisting of a curing accelerator (C), a filler (D), a coupling agent (E), a crosslinking agent (F), an energy ray curable resin (G), a photopolymerization initiator (H), a colorant (I) and a general-purpose additive (J).

[0184] The energy ray-curable protective film-forming film may, for example, contain an energy ray-curable component (a). Examples of the energy ray-curable component (a) include a polymer (a1) having an energy ray-curable group and a weight average molecular weight of 80,000 to 2,000,000, and a compound (a2) having an energy ray-curable group and a molecular weight of 100 to 80,000.

[0185] The energy ray-curable protective film-forming film preferably contains, in addition to the energy ray-curable component (a), a polymer (b) having no energy ray-curable group. Examples of the polymer (b) having no energy ray-curable group include acrylic resins, urethane resins, phenoxy resins, silicone resins, and saturated polyester resins.

[0186] The energy ray-curable protective film-forming film may further contain, in addition to the energy ray-curable component (a) and the polymer (b) having no energy ray-curable group, one or more selected from the group consisting of a colorant, a thermosetting component, a thermosetting agent, a filler, a coupling agent, a crosslinking agent, a photopolymerization initiator, and a general-purpose additive.

[0187] An example of the non-curable protective film-forming film is one that contains a polymer component. Examples of the polymer component include the same non-curable resins as the polymer component (A) listed as a component contained in the above-mentioned thermosetting protective film-forming film.

[0188] The non-curable protective film-forming film may further contain, in addition to the polymer component, one or more selected from the group consisting of colorants, fillers, coupling agents, crosslinking agents, and general-purpose additives.

[0189] The thickness of the protective film-forming film is preferably 1 to 100 μm. When the thickness of the protective film-forming film is equal to or greater than the lower limit, a protective film having higher protective ability can be formed. When the thickness of the protective film-forming film is equal to or less than the upper limit, the protective film can be prevented from becoming excessively thick. Here, "thickness of the protective film-forming film" means the thickness of the entire protective film-forming film, for example, the thickness of a protective film-forming film consisting of multiple layers means the total thickness of all layers that constitute the protective film-forming film.

[0190] The protective film-forming film can be formed using a protective film-forming composition containing its constituent materials (a thermosetting protective film-forming composition for forming a thermosetting protective film-forming film, an energy ray curable protective film-forming composition for forming an energy ray curable protective film-forming film, and a non-curable protective film-forming composition for forming a non-curable protective film-forming film). For example, the protective film-forming film can be formed by applying the protective film-forming composition to the surface to be formed and drying it as necessary. The ratio of the contents of the components that do not vaporize at room temperature in the protective film-forming composition is usually the same as the ratio of the contents of the components in the protective film-forming film.

[0191] ◇Manufacturing method of composite sheet for forming protective film The composite sheet for forming a protective film can be produced by laminating the above-mentioned layers constituting the composite sheet so as to have a corresponding positional relationship, and adjusting the shape of some or all of the layers as necessary. The method for forming each layer is as described above. For example, a protective film-forming composite sheet can be produced by applying a protective film-forming composition to one side of a release film and drying it as necessary to form a protective film-forming film on the release film, and then bonding the exposed surface of this protective film-forming film (the surface opposite to the release film side) to the exposed surface of the pressure-sensitive adhesive layer in the support sheet (the surface opposite to the substrate side). The protective film-forming composition is preferably applied to the release-treated surface of the release film.

[0192] ◇ Manufacturing method of workpiece (How to use the support sheet) The support sheet may be used in the manufacture of a work piece. That is, a manufacturing method of a workpiece according to one embodiment of the present invention includes an attachment step of fixing a workpiece with a support sheet, comprising the workpiece and the support sheet provided on the workpiece, to the fixing jig by attaching the adhesive layer in the support sheet to the workpiece and the fixing jig; a heating step of heating the adhesive layer in the support sheet fixed to the fixing jig after the attachment step; a processing step of producing the workpiece by processing the workpiece in the workpiece with a support sheet fixed to the fixing jig after the attachment step; a curing step of curing the adhesive layer attached to the fixing jig with energy rays after the heating step and the processing step; and a picking up step of separating the workpiece from the cured product of the adhesive layer and picking it up after the curing step. As explained above, the fixing jig is a known one, and is preferably made of, for example, stainless steel.

[0193] Examples of a method for manufacturing a workpiece when the work is a semiconductor wafer, i.e., a method for manufacturing a semiconductor chip, include a manufacturing method having a bonding step of bonding the adhesive layer in the support sheet to a semiconductor wafer and a fixing jig, thereby fixing a semiconductor wafer with a support sheet, which includes the semiconductor wafer and the support sheet provided on the semiconductor wafer, to the fixing jig; a heating step of heating the adhesive layer in the support sheet fixed to the fixing jig after the bonding step; a processing step of producing the semiconductor chip by dividing the semiconductor wafer in the semiconductor wafer with support sheet fixed to the fixing jig after the bonding step; a curing step of curing the adhesive layer attached to the fixing jig with energy rays after the heating step and the processing step; and a picking up step of detaching the semiconductor chip from the cured product of the adhesive layer and picking it up after the curing step.

[0194] After the pasting step, the order of performing the processing step and the heating step can be arbitrarily selected according to the purpose. For example, the processing step may be performed before the heating step, or the heating step may be performed before the processing step. For example, in the manufacturing method, the heating step can be performed to remove foreign matter such as low molecular weight resin components attached to the surface of the workpiece by volatilization. In this case, the heating step can be performed either before or after the processing step. In addition, in the manufacturing method, the heating step can be performed to dry the workpiece after cleaning and removing fine foreign matter that is generated during processing such as dicing of the workpiece and that is attached to the surface of the workpiece with water. In this case, the heating step is performed after the processing step. In the manufacturing method, the heating step for removing the foreign matter and the heating step for drying may be performed together, or these heating steps may be performed at the same time.

[0195] <<An example of a manufacturing method for a workpiece>> ◎Manufacturing method (1-1) Fig. 2 is a cross-sectional view for explaining an example of the manufacturing method when the workpiece is a semiconductor wafer. Here, a manufacturing method (sometimes referred to as "manufacturing method (1-1)" in this specification) is explained in which the support sheet 1 shown in Fig. 1 is used and a heating step is performed after a processing step.

[0196] <Attachment process> In the attachment step of manufacturing method (1-1), the adhesive layer 12 in the support sheet 1 is attached to the semiconductor wafer 9 (more specifically, the back surface 9b of the semiconductor wafer 9), which is a workpiece, and to the ring frame 8, which is a fixing jig, to fix a support sheet-attached semiconductor wafer 109, which includes the semiconductor wafer 9 and the support sheet 1 provided on the back surface 9b of the semiconductor wafer 9, to the ring frame 8, as shown in Fig. 2(a). The support sheet-attached semiconductor wafer 109 is the support sheet-attached workpiece. The support sheet 1 is used after removing the release film 13. A surface 12a of the adhesive layer 12 opposite to the substrate 11 side is the same as one surface 1a of the support sheet 1 (the surface on the adhesive layer 12 side). In FIG. 2, bumps and the like on the circuit surface 9a of the semiconductor wafer 9 are omitted.

[0197] In the attachment step of the manufacturing method (1-1), a region of the adhesive layer 12 near the center in the width direction is attached to the semiconductor wafer 9, and a region surrounding this attachment region to the semiconductor wafer 9 is attached to the ring frame 8.

[0198] The support sheet 1 (adhesive layer 12) can be attached to the semiconductor wafer 9 and the ring frame 8 at room temperature. The speed at which the support sheet 1 (adhesive layer 12) is attached to the semiconductor wafer 9 and the ring frame 8 is not particularly limited, but is preferably 200 to 400 mm / min.

[0199] <Processing process> After the attachment step of the manufacturing method (1-1), in the processing step, as shown in Fig. 2(b), the semiconductor wafer 9 in the semiconductor wafer 109 with a support sheet fixed to the ring frame 8 is divided to produce semiconductor chips 90, which are workpieces. Through the processing step, a group of semiconductor chips with a support sheet 901 is obtained, in which a plurality of semiconductor chips 90 are aligned and held on one support sheet 1.

[0200] The circuit surface 90 a of the semiconductor chip 90 corresponds to the circuit surface 9 a of the semiconductor wafer 9 . The back surface 90 b of the semiconductor chip 90 corresponds to the back surface 9 b of the semiconductor wafer 9 .

[0201] The semiconductor wafer 9 can be divided by a known method, such as blade dicing using a blade, laser dicing by laser irradiation, or water dicing by spraying water containing an abrasive. The semiconductor wafer 9 can also be divided by using a semiconductor wafer 9 on which a modified layer has been formed by Stealth Dicing (registered trademark) and which has not been divided, and expanding the semiconductor wafer 9 in a direction parallel to its circuit surface 9a or back surface 9b.

[0202] Stealth Dicing (registered trademark) is a method as follows. That is, first, a planned division location is set inside the semiconductor wafer, and a laser beam is irradiated so as to converge on this location as a focal point, thereby forming a modified layer inside the semiconductor wafer. The modified layer of the semiconductor wafer is different from other locations of the semiconductor wafer, and is altered by the irradiation of the laser beam, and has a weaker strength. Therefore, when a force is applied to the semiconductor wafer, a crack is generated in the modified layer inside the semiconductor wafer, which extends in the direction of both sides of the semiconductor wafer, and becomes the starting point for dividing (cutting) the semiconductor wafer. Next, a force is applied to the semiconductor wafer to divide the semiconductor wafer at the site of the modified layer, and semiconductor chips are produced.

[0203] In the case where the adhesive strength (X0) of the support sheet 1 is 2000 mN / 25 mm or more, in the processing step, when the semiconductor wafer 9 is divided into small-sized semiconductor chips 90, and the small-sized semiconductor chips 90 obtained by such division and having a large amount of cutting debris attached thereto are washed with water, peeling of the semiconductor chips 90 from the support sheet 1 (adhesive layer 12) is suppressed even if force is applied by the semiconductor chips 90.

[0204] When the average light transmittance (L1) of the support sheet is 80% or more, the inspection accuracy is improved when inspecting the semiconductor chips with support sheets obtained in the processing step for damage such as cracks or chips (e.g., chipping) through the support sheet.

[0205] <Heating process> After the attachment step and processing step of the manufacturing method (1-1), in the heating step, the adhesive layer 12 in the support sheet 1 fixed to the ring frame 8 is heated as shown in Fig. 2(c). In this case, the heating of the adhesive layer 12 is accompanied by heating of the entire semiconductor chip group 901 with the support sheet, and this heating can remove, for example, foreign matter such as low molecular weight resin components adhering to the surface (for example, the circuit surface 90a) of the semiconductor chip 90 by volatilization. In addition, after fine foreign matter generated during dicing of the semiconductor wafer and adhering to the surface of the semiconductor chip is washed and removed with water, the semiconductor chip, etc. can be dried by this heating.

[0206] The temperature (heating temperature) during heating of the adhesive layer 12 in the semiconductor chip group 901 with the support sheet is preferably 130 to 145°C, and may be 130°C or higher and lower than 140°C, but is more preferably 140 to 145°C. When the heating temperature is equal to or higher than the lower limit, the effect of heating can be sufficiently obtained. When the heating temperature is equal to or lower than the upper limit, excessive heating can be avoided, and, for example, deterioration of the semiconductor chip group 901 with the support sheet can be suppressed. In particular, when the heating temperature is 140 to 145°C, the effect obtained by using the support sheet 1 is particularly high.

[0207] In the case where the adhesive strength (Y2) of the support sheet 1 is 6000 mN / 25 mm or less, the semiconductor chip group 901 with the support sheet is heated in a state fixed to the ring frame 8 in the heating step, so that the semiconductor chip group 901 with the support sheet can be peeled off from the ring frame 8 without further energy ray curing of the adhesive layer 12 in the semiconductor chip group 901 with the support sheet after heating. Furthermore, when the semiconductor chip group 901 with the support sheet is peeled off from the ring frame 8, the adhesive layer 12 remaining on the ring frame 8 can be suppressed. Therefore, for example, after the semiconductor chip group 901 with the support sheet after heating is peeled off from the ring frame 8, it can be attached to the ring frame 8 again and fixed. In this way, a highly versatile method can be adopted as a method for manufacturing a workpiece.

[0208] When the light transmittance difference of the support sheet 1 is 30% or more, the support sheet 1 clearly whitens when heated at a high temperature of 140° C. or more in the heating step, and therefore the distinguishability of the support sheet 1 becomes high when the support sheet 1 is heated at such a high temperature.

[0209] <Curing process> After the processing step and the heating step of the manufacturing method (1-1), in the curing step, the adhesive layer 12 attached to the ring frame 8 is cured with energy rays as shown in Fig. 2(d) . By the curing step, a group of semiconductor chips 901' with a cured support sheet is obtained, in which a plurality of semiconductor chips 90 are aligned and held on one cured support sheet 1'. The support sheet 1 becomes a cured support sheet 1' when the pressure-sensitive adhesive layer 12 is cured with energy rays to become an energy-ray-cured product 12'. Group of semiconductor chips with cured support sheet 901' is a laminate of a group of workpieces and a cured support sheet (in other words, a group of workpieces with a cured support sheet), and is the same as group of semiconductor chips with support sheet 901 except that adhesive layer 12 is an energy ray-cured material 12'.

[0210] When the adhesive layer 12 is cured with energy rays (when the adhesive layer 12 is irradiated with energy rays), the illuminance of the energy rays is 60 to 320 mW / cm 2 The light amount of the energy beam is preferably 100 to 1000 mJ / cm. 2 It is preferable that: The energy rays are preferably irradiated onto the pressure-sensitive adhesive layer 12 from outside the support sheet 1 through the substrate 11 (via the substrate 11).

[0211] <Pickup process> In the pick-up step after the curing step of the manufacturing method (1-1), the semiconductor chip 90 can be removed from the group of semiconductor chips 901' with the cured support sheet by detaching and picking up the semiconductor chip 90 from the energy ray-cured product 12' of the adhesive layer in the cured support sheet 1' as shown in Fig. 2(e). Here, the pick-up direction is indicated by the arrow P.

[0212] When the semiconductor chip 90 is picked up, peeling occurs between the back surface 90b of the semiconductor chip 90 and the surface 12a' of the energy ray-cured product 12' of the adhesive layer opposite the substrate 11. At this time, since the adhesive force between the energy ray-cured product 12' of the adhesive layer and the semiconductor chip 90 is smaller than the adhesive force between the adhesive layer 12 and the semiconductor chip 90, the semiconductor chip 90 is easily peeled from the energy ray-cured product 12' of the adhesive layer and can be easily picked up. The surface 12a' opposite the substrate 11 side of the energy ray-cured product 12' of the adhesive layer corresponds to the surface 12a opposite the substrate 11 side of the adhesive layer 12, and is the same as one surface 1a' of the cured support sheet 1' (the surface of the adhesive layer facing the energy ray-cured product 12').

[0213] A known method can be used to pick up the semiconductor chip 90. For example, a vacuum collet or the like can be used as a separating means 7 for separating the semiconductor chip 90 from the cured support sheet 1' (the energy ray-cured product 12' of the pressure-sensitive adhesive layer).

[0214] Since the adhesive strength (X1) of the support sheet 1 is 500 mN / 25 mm or less, the pick-up ability is enhanced so that the semiconductor chip 90 can be normally picked up from the hardened support sheet 1' even after the support sheet 1 holding the semiconductor chip group (in other words, the semiconductor chip group 901 with support sheet) is heated to a high temperature of 140°C or higher, with an upper limit of approximately 145°C, in the heating process.

[0215] In the support sheet 1, when the adhesive strength change rate is 90-150%, even if the heating temperature in the heating step is 130° C. or higher and lower than 140° C., particularly 130° C., the semiconductor chip 90 (corresponding to the workpiece) can be normally picked up from the cured support sheet 1' under the same conditions as when the heating temperature is 140-145° C., and the pick-up property is high. Therefore, even if the heating temperature is set low in this way, it is not necessary to change the device condition settings when manufacturing the semiconductor chip 90, and versatility in terms of setting the heating temperature is increased.

[0216] <Other processes> The manufacturing method (1-1) may include a step other than any of the attaching step, the processing step, the heating step, the curing step, and the pick-up step. The type of the other steps, the number of the other steps, and the timing of performing the other steps can all be selected arbitrarily depending on the purpose, and are not particularly limited.

[0217] <<Other examples of manufacturing methods for workpieces>> ◎Manufacturing method (1-2) So far, a method for manufacturing a workpiece has been described in which the adhering step, processing step, heating step, curing step, and pick-up step are performed in this order (manufacturing method (1-1)). However, the manufacturing method for a workpiece in this embodiment is not limited to this. For example, in the manufacturing method, as described above, the order of the processing step and heating step may be reversed (in this specification, such a manufacturing method may be referred to as "manufacturing method (1-2)"). The manufacturing method (1-2) will be described when the workpiece is a semiconductor wafer.

[0218] <Attachment process> In the manufacturing method of such a workpiece (manufacturing method (1-2)), a bonding step is first performed. The bonding step of the manufacturing method (1-2) is the same as the bonding step of the manufacturing method (1-1).

[0219] <Heating process> In the heating step after the laminating step of the manufacturing method (1-2), the adhesive layer in the support sheet fixed to the ring frame is heated. In this case, the heating of the adhesive layer is accompanied by the heating of the entire semiconductor wafer with the support sheet. By this heating, for example, foreign matter such as low molecular weight resin components adhering to the surface (for example, the circuit surface) of the semiconductor wafer can be removed by volatilization.

[0220] The temperature (heating temperature) at which the pressure-sensitive adhesive layer (semiconductor wafer with support sheet) is heated is the same as the temperature (heating temperature) at which the pressure-sensitive adhesive layer (semiconductor chip group with support sheet) is heated in the heating step of production method (1-1).

[0221] When the light transmittance difference of the support sheet is 30% or more, the support sheet is clearly whitened when heated at a high temperature of 140° C. or more in the heating step, and therefore the support sheet is highly distinguishable when heated at such a high temperature.

[0222] <Processing process> After the attachment step and the heating step of manufacturing method (1-2), in the processing step, the semiconductor wafer in the heated semiconductor wafer with support sheet fixed to the ring frame is divided to produce semiconductor chips, which are workpieces. The semiconductor wafer can be divided in the same manner as in manufacturing method (1-1). Except for the fact that it is heated, the processing step produces a group of semiconductor chips with support sheet that is the same as in manufacturing method (1-1).

[0223] In the case where the adhesive strength (Y2) of the support sheet is 6000 mN / 25 mm or less, when the workpiece with the support sheet fixed to the fixing jig is heated at a high temperature of 140° C. or more in the heating step of the manufacturing method (1-2), the workpiece with the support sheet can be peeled off from the fixing jig without further curing the adhesive layer with energy rays, and furthermore, the adhesive layer can be prevented from remaining on the fixing jig. Therefore, for example, after peeling off the support sheet in the semiconductor chip group with the support sheet after heating from the ring frame, it can be attached to the ring frame again and fixed. In this way, a highly versatile method can be adopted as a manufacturing method for the workpiece.

[0224] <Curing process> After the heating step and processing step of manufacturing method (1-2), the curing step can be carried out in the same manner as in manufacturing method (1-1), and the curing step produces a group of semiconductor chips with a cured support sheet similar to that of manufacturing method (1-1).

[0225] <Pickup process> After the hardening step in manufacturing method (1-2), the pick-up step can be carried out in the same manner as in manufacturing method (1-1), and the target semiconductor chip can be extracted by the pick-up step in the same manner as in manufacturing method (1-1).

[0226] Since the adhesive strength (X1) of the support sheet is 500 mN / 25 mm or less, even after the semiconductor wafer with the support sheet is heated to a high temperature of 140°C or more, with an upper limit of approximately 145°C, in the heating process, the semiconductor chip can be picked up normally from the hardened support sheet, as in the manufacturing method (1-1), and the pick-up ability is high.

[0227] In the case of a support sheet, when the adhesive strength change rate is 90 to 150%, even if the heating temperature in the heating step is 130° C. or more and less than 140° C., particularly 130° C., the semiconductor chip (corresponding to the workpiece) can be normally picked up from the cured support sheet under the same conditions as when the heating temperature is 140 to 145° C., and the pick-up property is high. Therefore, as in the case of manufacturing method (1-1), even if the heating temperature is set low, there is no need to change the device condition settings when manufacturing the semiconductor chip, and versatility in terms of setting the heating temperature is increased.

[0228] <Other processes> The production method (1-2) may include other steps similar to those in the production method (1-1). In the production method (1-2), the type of the other steps, the number of the other steps, and the timing of performing the other steps can all be selected arbitrarily depending on the purpose, and are not particularly limited.

[0229] <<Examples of other manufacturing methods for workpieces>> ◎Other manufacturing methods (01) In the manufacturing method of this embodiment, whether it is manufacturing method (1-1) or manufacturing method (1-2), the heating step and the curing step are performed in this order, and the support sheet (adhesive layer) is heated, and then the adhesive layer in the support sheet is cured with energy rays. In contrast, when the adhesive strength (X3) is 500 mN / 25 mm or less, the adhesive layer in the support sheet is cured with energy rays, which is the opposite to the above, so that even if a workpiece with a cured support sheet including a workpiece and a cured support sheet provided on the workpiece is produced and then the cured support sheet (energy ray cured product of the adhesive layer) is heated, the pick-up ability is improved so that the workpiece can be picked up without abnormality from the cured support sheet. That is, a method for manufacturing a workpiece having an adhesive strength (X3) of 500 mN / 25 mm or less includes a bonding step (sometimes referred to as a "bonding step (01)" in this specification) of bonding the adhesive layer in the support sheet to the workpiece and a fixing jig to fix a support sheet-attached workpiece including the workpiece and the support sheet provided on the workpiece to the fixing jig, a curing step (sometimes referred to as a "curing step (01)" in this specification) of producing a cured support sheet by curing the adhesive layer in the support sheet fixed to the fixing jig with energy rays after the bonding step (01), and a curing step (sometimes referred to as a "curing step (01)" in this specification) of curing the adhesive layer in the support sheet fixed to the fixing jig with energy rays after the bonding step (01). An example of such a manufacturing method (sometimes referred to in this specification as "another manufacturing method (01)") includes a processing step (sometimes referred to in this specification as "processing step (01)") of producing the workpiece by processing the workpiece in the workpiece with the cured support sheet, a heating step (sometimes referred to in this specification as "heating step (01)") of heating the energy ray-cured product of the adhesive layer affixed to the fixing jig after the curing step (01) and the processing step (01), and a pick-up step (sometimes referred to in this specification as "pick-up step (01)") of detaching the workpiece from the heated product of the energy ray-cured product of the adhesive layer and picking it up after the heating step (01).

[0230] The attaching step (01) of the other manufacturing method (01) is the same as the attaching step of the manufacturing method (1-1).

[0231] In another manufacturing method (01), when the curing step (01) and the processing step (01) are performed in this order, the curing step (01) is the same as the curing step in the manufacturing method (1-1) or (1-2) except that the target of energy ray curing is the unheated adhesive layer in the workpiece with a support sheet, instead of the heated adhesive layer in the workpiece with a support sheet. In the other manufacturing method (01), when the processing step (01) and the curing step (01) are carried out in this order, the processing step (01) is the same as the processing step of the manufacturing method (1-1).

[0232] In another manufacturing method (01), when the hardening step (01) and the processing step (01) are performed in this order, the processing step (01) is the same as the processing step in the manufacturing method (1-1) except that the processing target is a workpiece in a hardened workpiece with a support sheet instead of a workpiece in a workpiece with a support sheet. In another manufacturing method (01), when the processing step (01) and the curing step (01) are performed in this order, the curing step (01) is the same as the curing step of the manufacturing method (1-1) or the manufacturing method (1-2) except that the target of energy ray curing is the unheated adhesive layer in the workpiece with a support sheet instead of the heated adhesive layer in the workpiece with a support sheet.

[0233] The heating step (01) of the other manufacturing method (01) is the same as the heating step of the manufacturing method (1-1) except that the target of heating is the adhesive layer in the cured workpiece with the support sheet instead of the adhesive layer in the workpiece with the support sheet. By heating the adhesive layer in this case, for example, foreign matter such as low molecular weight resin components adhering to the surface of the workpiece can be removed by volatilization. In addition, after fine foreign matter adhering to the surface of the workpiece is washed and removed with water, the workpiece can be dried by this heating. The heating step (01) produces a group of workpieces with a hardened support sheet, similar to the case of the above-mentioned manufacturing method (for example, manufacturing method (1-1) or manufacturing method (1-2)).

[0234] The pick-up step (01) of the other manufacturing method (01) is the same as the pick-up step of the manufacturing method (1-1) or the manufacturing method (1-2).

[0235] In the support sheet, when the adhesive strength (X1) is 500 mN / 25 mm or less and the adhesive strength (X3) is 500 mN / 25 mm or less, even after the adhesive layer in the workpiece with the cured support sheet is heated to a high temperature of up to about 145°C in the heating step (01), the semiconductor chip can be picked up normally from the cured support sheet, and the pick-up ability is high.

[0236] The other manufacturing method (01) may include other steps similar to those in the manufacturing method (1-1) or the manufacturing method (1-2). In the production method (01), the type of the other steps, the number of the other steps, and the timing of performing the other steps can all be selected arbitrarily depending on the purpose, and are not particularly limited. In manufacturing method (01), the adhesive layer in the support sheet can also be easily peeled off from the back surface of the workpiece while maintaining its shape for the purpose of re-attachment, which prevents chips from peeling off during dicing and enables the workpiece to be properly picked up from the support sheet.

[0237] ◇How to regenerate the support sheet By using the support sheet according to one embodiment of the present invention described above, the support sheet can be regenerated by attaching the adhesive layer in the support sheet to the back surface of a workpiece, and then peeling the adhesive layer in the support sheet from the back surface of the workpiece, making it possible to reattach the support sheet to the back surface of the workpiece.

[0238] For example, after the adhesive layer in the support sheet is attached to the back surface of the workpiece, if an abnormality occurs on a part or the entire surface of the workpiece, such as the support sheet not being attached evenly due to air bubbles being mixed between the workpiece and the support sheet, the adhesive layer in the support sheet is peeled off from the back surface of the workpiece in the vicinity of the part or the entire surface. At this time, the support sheet is only slightly stretched during peeling, and the deformation of the support sheet is small enough to allow the support sheet to be reattached, so the support sheet can be regenerated. Furthermore, the workpiece can be regenerated by making the back surface of the workpiece into a state in which the support sheet can be reattached.

[0239] 3A to 3C are cross-sectional views for illustrating an example of a method for regenerating a support sheet. Here, the case where the workpiece is a semiconductor wafer will be described by taking the support sheet 1 shown in FIG. 1 as an example.

[0240] In the method for regenerating a support sheet according to this embodiment, as shown in Fig. 3A, a support sheet 1 is attached to the back surface 9b of a semiconductor wafer 9. Here, the release film 13 is removed from the support sheet 1 with the release film, and the first surface 12a of the pressure-sensitive adhesive layer 12 of the support sheet 1 thus exposed is attached to the back surface 9b of the semiconductor wafer 9.

[0241] In the support sheet regenerating method according to this embodiment, next, as shown in Figures 3B and 3C, the support sheet 1 is peeled off from a part or the entire back surface 9b of the semiconductor wafer 9. In the regenerating method according to this embodiment, since the support sheet 1 shown in Figure 1 is used as the support sheet 1, the support sheet 1 can be easily peeled off from the back surface 9b of the semiconductor wafer 9, and the support sheet 1 can be regenerated to a state in which the support sheet 1 can be reattached to the back surface 9b of the semiconductor wafer 9. Also, the semiconductor wafer 9 can be regenerated to a state in which the support sheet 1 can be reattached.

[0242] 3A to 3D are cross-sectional views for explaining an example of a method for reattaching a support sheet. After the semiconductor wafer 9 and the support sheet 1 are regenerated by the regeneration method according to this embodiment, the regenerated support sheet 1 can be reattached to the back surface 9b of the regenerated semiconductor wafer 9, for example, as shown in FIG. 3D.

[0243] The support sheet 1 can be reattached to the semiconductor wafer 9 in the same manner as described above for the initial attachment of the support sheet 1 to the semiconductor wafer 9. Thereafter, the method for manufacturing the workpiece, i.e., the method for manufacturing the semiconductor chips, can be carried out in the same manner as described above. EXAMPLES

[0244] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the following examples.

[0245] The ring frame used in the following Examples, Comparative Examples, and Reference Examples is made of SUS. The shape of the ring frame is a substantially circular ring shape in which two arcs in a part of the outer periphery of the ring, which are symmetrical with respect to the center of the ring, are both cut into straight lines. The ring frame for 8-inch wafers has an outer diameter of 296 mm, a width of the straight line part of 276 mm, an inner diameter of 250 mm, and a thickness of 1.2 mm.

[0246] <Raw materials for resin production> The full names of the raw materials for producing the resins, which are abbreviated in the present examples and comparative examples, are shown below. 2EHA: 2-ethylhexyl acrylate 2EHMA: 2-Ethylhexyl methacrylate HEA: 2-hydroxyethyl acrylate HEMA: 2-hydroxyethyl methacrylate MOI: 2-Methacryloyloxyethyl isocyanate

[0247] <Raw materials for producing adhesive composition> In the present examples and comparative examples, the raw materials used in producing the pressure-sensitive adhesive compositions are shown below. [Energy ray curable compound (α)] (α)-1: 2-(2-phenoxyethoxy)ethyl acrylate ("AMP-20GY" manufactured by Shin-Nakamura Chemical Co., Ltd., viscosity 18 mPa·s at 23°C (measured using a single-cylinder B-type (Brookfield type) rotational viscometer), molecular weight 236.1) [Crosslinker (β1)] (β1)-1: A block-type crosslinking agent having both a nurate skeleton formed by the trimerization of hexamethylene diisocyanate and a skeleton derived from other hexamethylene diisocyanate ("Duranate (registered trademark) MF-K60B" manufactured by Asahi Kasei Corporation, number average molecular weight 12000, viscosity at 25°C 220 mPa s). [Crosslinker (β2)] (β2)-1: Isocyanurate modified hexamethylene diisocyanate ("Coronate HX" manufactured by Tosoh Corporation) (β2)-2: Trimethylolpropane adduct of 1,6-hexamethylene diisocyanate ("Coronate HL" manufactured by Tosoh Corporation) [Photopolymerization initiator (γ)] (γ)-1: 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one (Omnirad® 127, manufactured by IGM Resins)

[0248] The viscosity of the above crosslinking agent (β1) is a value measured by an E-type viscometer.

[0249] [Example 1] <<Manufacture of support sheet>> <Production of energy ray curable acrylic resin (Ia)> The acrylic polymer (1) was added with MOI, and the addition reaction was carried out in an air stream at 50°C for 48 hours to obtain an energy beam curable acrylic resin (Ia)-1. The acrylic polymer (1) was a copolymer of 2EHA (35 parts by mass), 2EHMA (45 parts by mass), and HEMA (20 parts by mass). The amount of MOI used was such that the total number of moles of isocyanate groups in the MOI was 0.55 times the total number of moles of hydroxyl groups derived from HEMA in the acrylic polymer (1). The weight average molecular weight of the obtained energy beam curable acrylic resin (Ia)-1 was 400,000, and the glass transition temperature was -26°C.

[0250] <Production of Pressure-Sensitive Adhesive Composition (I)> The energy ray curable adhesive composition (I)-1 was prepared at room temperature, containing energy ray curable acrylic resin (Ia)-1 (100 parts by mass), crosslinking agent (β1)-1 (13.5 parts by mass), crosslinking agent (β2)-1 (2 parts by mass), and photopolymerization initiator (γ)-1 (3 parts by mass), and further containing methyl ethyl ketone as a solvent, and the total concentration of all components other than the solvent was 25% by mass. Note that the contents of all components other than methyl ethyl ketone shown here are the contents of the target product excluding the solvent.

[0251] <Formation of adhesive layer> A release film ("SP-PET381031", manufactured by Lintec Corporation, thickness 38 μm) made of polyethylene terephthalate film, one side of which had been treated for release by silicone treatment, was used. The adhesive composition (I)-1 obtained above was applied to the release-treated surface, and the adhesive was dried by heating at 100°C for 2 minutes to form an energy ray-curable adhesive layer having a thickness of 15 μm, giving an adhesive layer with a release film.

[0252] <Manufacture of Support Sheet> Next, at room temperature, a polypropylene film (manufactured by Diaplus Film Co., Ltd., thickness 80 μm) was attached as a substrate to the exposed surface of the pressure-sensitive adhesive layer at a sticking speed of 5 m / min and a pressure of 0.4 MPa. One surface of the polypropylene film was a matte surface with a surface roughness (Ra) of 0.90 μm, and the other surface was a slightly matte surface with a surface roughness (Ra) of 0.12 μm, and the pressure-sensitive adhesive layer was attached to the matte surface of the polypropylene film. In this manner, the desired support sheet was obtained.

[0253] <<Evaluation of the support sheet>> In the following evaluations of the support sheet, the release film on the adhesive layer was peeled off as appropriate before evaluation. For example, when the support sheet was attached to each adherend to measure the adhesive strength, when the light transmittance was measured, and when evaluations were performed to confirm each effect, the release film was peeled off before use in the evaluations.

[0254] <Measurement of adhesive strength (X1) between the energy ray cured adhesive layer after heating at 140℃ and a silicon mirror wafer> A test piece measuring 70 mm in length and 25 mm in width was cut out from the support sheet obtained above. The test piece was attached to the mirror surface of a silicon mirror wafer (thickness 650 μm) by the adhesive layer therein under the attachment temperature condition of 23° C. (laminating roller temperature 23° C., silicon mirror wafer temperature 23° C.), attachment speed 300 mm / min, and attachment pressure 0.3 MPa to obtain a silicon mirror wafer with a test piece attached. This silicon mirror wafer with a test piece attached was placed in an oven whose temperature was adjusted to 140° C., and heated at this temperature (140° C.) for 2 hours. Next, the silicon mirror wafer with the test piece was removed from the oven and allowed to cool until its temperature reached 23° C. Then, an ultraviolet ray irradiation device ("RAD-2000UV" manufactured by Lintec Corporation) was used to irradiate the wafer with an illuminance of 230 mW / cm 2 , light intensity 200mJ / cm 2Under the above conditions, the adhesive layer in the silicon mirror wafer with the test piece taken out was irradiated with ultraviolet light through the substrate, thereby curing the adhesive layer in the test piece with ultraviolet light.

[0255] Next, the test piece was peeled off from the silicon mirror wafer at a peeling speed of 300 mm / min in an environment of 23°C. At this time, the test piece was peeled off in its length direction so that the surface of the silicon mirror wafer to which the test piece was attached and the surface of the test piece to which the silicon mirror wafer was attached formed an angle of 180° (180° peeling was performed). Then, the load (peeling force) at this 180° peeling was measured, and the measurement length was set to 50 mm, and the measurement value at the first 5 mm length and the measurement value at the last 5 mm length were excluded from the effective value. Then, the average value of the measured values ​​was adopted as the adhesive strength (mN / 25 mm). The adhesive strength was measured twice, and the average value was used as the adhesive strength (X1) (mN / 25 mm) between the energy ray-cured adhesive layer and the silicon mirror wafer after heating at 140° C. The results are shown in Table 1.

[0256] In Table 1, "content (mass%) of crosslinking agent (β1) in pressure-sensitive adhesive layer" means "proportion (mass%) of the content of crosslinking agent (β1) in the pressure-sensitive adhesive layer relative to the total mass of the pressure-sensitive adhesive layer." This also applies to the following tables.

[0257] <Measurement of adhesive strength (X0) between adhesive layer and silicon mirror wafer> A silicon mirror wafer with a test piece was prepared in the same manner as in the measurement of the adhesive strength (X1) described above. Next, the silicon mirror wafer with the test piece was left to stand and stored at a temperature of 23° C. for 30 minutes. Next, the test piece was peeled off from the silicon mirror wafer after the static storage at a peeling speed of 300 mm / min in an environment of 23°C. At this time, the test piece was peeled off in its length direction so that the surface of the silicon mirror wafer to which the test piece was attached and the surface of the test piece to which the silicon mirror wafer was attached made an angle of 180° (180° peeling was performed). Then, the load (peeling force) at this 180° peeling was measured, and the measurement length was set to 50 mm, and the measurement value at the first 5 mm length and the measurement value at the last 5 mm length were excluded from the effective value. Then, the average value of the measured values ​​was adopted as the adhesive strength (mN / 25 mm). The adhesive strength was measured twice, and the average value was used as the adhesive strength (X0) (mN / 25 mm) between the adhesive layer and the silicon mirror wafer. The results are shown in Table 1.

[0258] <Measurement of adhesive strength (X01) between adhesive layer and silicon mirror wafer after reattachment> A silicon mirror wafer with a test piece was prepared in the same manner as in the measurement of the adhesive strength (X0) above, except that a test piece with a length of 70 mm and a width of 25 mm was used, and then this silicon mirror wafer with the test piece was left to stand for 30 minutes under a temperature condition of 23° C. Next, in an environment of 23° C., a 60 mm long portion of the test piece was peeled off in the length direction from the silicon mirror wafer after this standing storage at a peeling speed of 300 mm / min so that the surface of the silicon mirror wafer to which the test piece was attached and the surface of the test piece to which the silicon mirror wafer was attached made an angle of 180° (180° peeling was performed). Again, under attachment temperature conditions of 23°C (laminating roller temperature 23°C, silicon mirror wafer temperature 23°C), attachment speed 300 mm / min, and attachment pressure 0.3 MPa, this test piece was attached to the same position on the mirror surface of the same silicon mirror wafer with the same peeled surface of the adhesive layer therein, to obtain a silicon mirror wafer with the test piece attached. Next, the silicon mirror wafer with the test piece was left to stand and stored at a temperature of 23° C. for 30 minutes. Next, the test piece was peeled off from the silicon mirror wafer after the static storage at a peeling speed of 300 mm / min in an environment of 23°C. At this time, the test piece was peeled off in its length direction so that the surface of the silicon mirror wafer to which the test piece was attached and the surface of the test piece to which the silicon mirror wafer was attached made an angle of 180° (180° peeling was performed). Then, the load (peeling force) at this 180° peeling was measured, and the measurement length was set to 50 mm, and the measurement value at the first 5 mm length and the measurement value at the last 5 mm length were excluded from the effective value. Then, the average value of the measured values ​​was adopted as the adhesive strength (mN / 25 mm). The adhesive strength was measured twice, and the average value was used as the adhesive strength (X01) (mN / 25 mm) between the adhesive layer and the silicon mirror wafer after re-attachment. The results are shown in Table 1.

[0259] <Measurement of adhesive strength (X3) between the heated energy ray cured adhesive layer and a silicon mirror wafer> A silicon mirror wafer with a test piece was prepared using the same method as in the measurement of adhesive strength (X1) above. An ultraviolet irradiation device (Rintec Corporation's "RAD-2000UV") was used, with an illuminance of 230 mW / cm 2 , light intensity 200mJ / cm 2 Under the above conditions, the adhesive layer in the silicon mirror wafer with the test piece was irradiated with ultraviolet light through the substrate, thereby curing the adhesive layer in the test piece with ultraviolet light. Next, the silicon mirror wafer with the test piece after irradiation with ultraviolet light was placed inside an oven whose temperature was adjusted to 140° C., and heated at this temperature (140° C.) for 2 hours. Next, the silicon mirror wafer with the test piece attached was taken out of the oven and allowed to cool until its temperature reached 23°C. Next, the test piece was peeled off from the silicon mirror wafer at a peeling speed of 300 mm / min in an environment of 23°C. At this time, the test piece was peeled off in its length direction so that the surface of the silicon mirror wafer to which the test piece was attached and the surface of the test piece to which the silicon mirror wafer was attached formed an angle of 180° (180° peeling was performed). Then, the load (peeling force) at this 180° peeling was measured, and the measurement length was set to 50 mm, and the measurement value at the first 5 mm length and the measurement value at the last 5 mm length were excluded from the effective value. Then, the average value of the measured values ​​was adopted as the adhesive strength (mN / 25 mm). The adhesive strength was measured twice, and the average value was used as the adhesive strength (X3) (mN / 25 mm) between the heated energy ray-cured adhesive layer and the silicon mirror wafer. The results are shown in Table 1.

[0260] <Calculation of adhesive strength change rate> A silicon mirror wafer with a test piece was prepared in the same manner as in the measurement of the adhesive strength (X1) above. Then, the adhesive strength (X11) between the energy ray-cured product of the adhesive layer and the silicon mirror wafer after heating at 130°C was measured in the same manner as in the measurement of the adhesive strength (X1) above, except that the heating temperature of the silicon mirror wafer with the test piece was changed from 140°C to 130°C. Using the measured value of the adhesive strength (X1) and the measured value of the adhesive strength (X11), the rate of change in adhesive strength was calculated according to the above formula (i) (rate of change in adhesive strength = adhesive strength (X1) / adhesive strength (X11) x 100). The results are shown in Table 1 together with the measured value of the adhesive strength (X11).

[0261] <Measurement of adhesive strength (Y2) between adhesive layer and SUS plate after heating at 140℃> A SUS plate with a test piece was obtained in the same manner as in measuring the adhesive strength (X1) above, except that the test piece was attached to the #1200 polished surface of a SUS plate ("SUS304 #1200HL, thickness 1000 μm, size 70 mm x 150 mm" manufactured by Paltec) instead of the mirror surface of the silicon mirror wafer. Next, this SUS plate with the test piece was heated at 140°C for 2 hours in the same manner as in the case of the silicon mirror wafer with the test piece when measuring the adhesive strength (X1) above, and then allowed to cool until the temperature reached 23°C.

[0262] Next, the test piece was peeled off from the cooled SUS plate at a peeling speed of 300 mm / min in an environment of 23°C. At this time, the test piece was peeled off in its length direction so that the surface of the SUS plate to which the test piece was attached and the surface of the test piece to which the SUS plate was attached formed an angle of 180° (180° peeling was performed). Then, the load (peeling force) at this 180° peeling was measured, and the measurement length was set to 50 mm, and the measurement value at the first 5 mm length and the measurement value at the last 5 mm length were excluded from the effective value. Then, the average value of the measured values ​​was adopted as the adhesive strength (mN / 25 mm). The adhesive strength was measured twice, and the average value was used as the adhesive strength (Y2) (mN / 25 mm) between the adhesive layer and the SUS plate after heating at 140° C. The results are shown in Table 1.

[0263] <Calculation of the average light transmittance (L1) of the support sheet, and evaluation of embeddability of the adhesive layer on the matte surface of the substrate> Using a UV-vis measurement device (Shimadzu Corporation's "UV-vis-NIR3600"), the support sheet obtained above was irradiated with light from the outside of the substrate side, and the light transmittance was measured by direct light reception without using an integrating sphere. The wavelength range of the measurement was 190 to 2000 nm. Then, in the wavelength range of 400 to 800 nm in the visible light region, the light transmittance values ​​were summed up every 1 nm, and the sum was divided by the number of summed light transmittance values ​​(i.e., 800-400+1=401) to calculate the average light transmittance (400 to 800 nm) (L1) (%) of the support sheet. Then, from this average value (L1), the embeddability of the adhesive layer on the matte surface of the substrate was evaluated according to the following criteria. These results are shown in Table 1. (Evaluation Criteria) A: The average light transmittance (L1) of the support sheet is 80% or more, and the matte surface of the substrate has a high embedding property with the adhesive layer. B: The average light transmittance (L1) of the support sheet is less than 80%, and the matte surface of the substrate is not sufficiently embedded by the adhesive layer.

[0264] <Calculation of light transmittance difference> The pressure-sensitive adhesive layer in the support sheet obtained above was attached to the mirror surface of a silicon mirror wafer (thickness 650 μm) in the width direction of the central region, and the region surrounding the region attached to the silicon mirror wafer was attached to a ring frame. The pressure-sensitive adhesive layer was attached to the silicon wafer and the ring frame at a temperature of 23° C. (laminating roller temperature 23° C., silicon mirror wafer temperature 23° C.), at a bonding speed of 300 mm / min, and at a bonding pressure of 0.3 MPa. As a result, a silicon mirror wafer with a support sheet, which includes a silicon mirror wafer and a support sheet provided on one side of the silicon mirror wafer, was fixed to the ring frame. The silicon mirror wafer with the support sheet was then placed inside an oven whose temperature was adjusted to 140° C., and heated at this temperature (140° C.) for 2 hours. The silicon mirror wafer with the support sheet was then removed from the oven and allowed to cool until its temperature reached 23° C. A test piece was cut out from a region of the support sheet in the silicon mirror wafer with the support sheet after cooling, where the adhesive layer was exposed, between the region where the adhesive layer was attached to the ring frame and the region where the adhesive layer was attached to the silicon mirror wafer.

[0265] Using a UV-vis measuring device (Shimadzu Corporation's "UV-vis-NIR3600"), the light transmittance of the test piece (i.e., the support sheet after heating) was measured and the average light transmittance (L2) was calculated in the same manner as when calculating the average light transmittance (L1) of the support sheet above, except that the test piece obtained above was used instead of the support sheet. From the obtained values, the light transmittance difference ([average light transmittance of the support sheet (L1)] - [average light transmittance of the support sheet after heating (L2)]) was calculated. The results are shown in Table 1.

[0266] <Evaluation of the discernibility of support sheets heated at 140°C> Before being placed inside an oven whose temperature was adjusted to 140° C., the color of the support sheet of the silicon mirror wafer with the support sheet was visually observed by 10 judges under fluorescent lighting for 3 seconds. Furthermore, among the silicon mirror wafers with support sheets after heating at 140° C. and cooling, the color of the support sheet was visually observed by 10 judges under fluorescent light for 3 seconds. Ten judges judged the appearance of the support sheet before and after heating in terms of color change, and evaluated the distinctiveness of the support sheet heated at 140° C. according to the following criteria. The results are shown in Table 1. (Evaluation Criteria) A: All 10 judges judged that the appearance of the support sheet had changed due to heating. B: 8 to 9 judges determined that the appearance of the support sheet had changed due to heating, and 1 to 2 judges determined that the appearance of the support sheet had not changed due to heating. C: Three or more judges judged that the appearance of the support sheet was not changed by heating.

[0267] <Evaluation of chipping inspection accuracy of support sheet> (Manufacture of silicon chips with support sheets) An 8-inch silicon wafer (thickness 350 μm) with one surface polished with #2000 was prepared. The pressure-sensitive adhesive layer in the support sheet obtained above was attached to the silicon wafer in a central region in the width direction, and the region surrounding the region attached to the silicon wafer was attached to a ring frame. The pressure-sensitive adhesive layer was attached to the silicon wafer and the ring frame at a temperature of 23° C. (laminating roller temperature 23° C., silicon wafer temperature 23° C.), at a bonding speed of 300 mm / min, and at a bonding pressure of 0.3 MPa. As a result, a silicon wafer with a support sheet, which includes a silicon wafer and a support sheet provided on one surface of the silicon wafer, was fixed to the ring frame (bonding process). Next, a dicing device (DISCO Corp. "DFD6362") was used to dice the silicon wafer in the silicon wafer with the support sheet fixed to the ring frame, to produce multiple silicon chips with a size of 1 mm x 1 mm (processing step). At this time, a dicing blade "ZH05-SD2000-N1-90 CC" manufactured by DISCO Corp. was used as the dicing blade, the blade rotation speed was 35000 rpm, the blade feed speed was 30 mm / s, and the blade height was 0.06 mm. The blade was inserted into the silicon wafer with the support sheet from the surface on the silicon wafer side, and cut into the base material to a depth of 20 μm from the surface on the adhesive layer side. In this manner, a group of silicon chips with a support sheet was produced, in which a plurality of silicon chips were aligned and held on one support sheet.

[0268] (Evaluation of chipping inspection accuracy of support sheet) Using an automatic wafer appearance inspection device (Canon's "Eagle-i"), the silicon chips in this group of silicon chips with support sheets were observed through the support sheet, and the number C1 of silicon chips that had cracks or chips (chipping) measuring 100 μm or more on the attachment surface of the silicon chip to the support sheet was confirmed. Next, an adhesive tape ("PET50 PL Thin" manufactured by Lintec Corporation) was attached to the exposed surfaces (the surfaces opposite to the support sheet) of all the silicon chips in the group of silicon chips with support sheets at a temperature of 23° C. This adhesive tape was composed of a substrate having a thickness of 50 μm and an acrylic adhesive layer provided on one surface of the substrate. Next, using an ultraviolet ray irradiation device ("RAD-2000UV" manufactured by Lintec Corporation), the adhesive layer in the group of silicon chips with the support sheet after the adhesive tape was attached was irradiated with an illuminance of 230 mW / cm from the outside of the substrate side through the substrate. 2 , light intensity 200mJ / cm 2 The pressure-sensitive adhesive layer was cured by irradiating it with ultraviolet light under the conditions of: Next, the cured support sheet was removed from the resulting group of silicon chips with the cured support sheet, and the silicon chips in the group of silicon chips exposed as a result were directly observed using the automatic wafer appearance inspection device, and the number C2 of silicon chips with cracks or chipping (chipping) of 100 μm or more in size was confirmed on the exposed surface of the silicon chip (the surface that was attached to the cured support sheet).

[0269] The chipping inspection accuracy value was calculated according to the following formula (ii), and the chipping inspection accuracy of the support sheet was evaluated according to the following criteria. The results are shown in Table 1. [Chipping inspection accuracy value]=C2 / C1 (ii) (Evaluation Criteria) A: The inspection accuracy value is less than 1.2, the chipping inspection accuracy of the support sheet is high, and the inspection accuracy is acceptable. B: The inspection accuracy value is 1.2 or more, the chipping inspection accuracy of the support sheet is poor, and the inspection accuracy is unacceptable.

[0270] <Measurement of elongation rate of support sheet before and after peeling off silicon wafer> When a support sheet was attached to a silicon wafer and then peeled off, the ratio of the amount of elongation of the support sheet after peeling to the length of the support sheet before peeling, i.e., the elongation rate of the support sheet before and after peeling off the silicon wafer, was measured using the following procedure. (1) The support sheet of Example 1 was applied to the entire ground surface of a circular 6-inch silicon wafer (thickness 580 μm) with one side ground with #6000, at a temperature of 23° C. (laminating roller temperature 23° C., silicon wafer temperature 23° C.) at a speed of 300 mm / min and a pressure of 0.3 MPa under conditions of 23° C. and 50% humidity, and left to stand for 30 minutes under conditions of 23° C. and 50% humidity. (2) A radius line (length L1 = 75 mm) connecting the center and the arc was drawn on the side of the support sheet. (3) The support sheet was peeled off from the side opposite the arc of the drawn radius line to the center (halfway down the silicon wafer). (4) A chuck (width 33 mm) of an autograph ("AG-IS" manufactured by Shimadzu Corporation) was attached to the edge of the peeled support sheet. (5) Under conditions of 23° C. and 50% humidity, the support sheet was peeled off from the entire surface of the silicon wafer at a constant speed using an autograph (peel speed: 300 mm / min, peel angle: 180°). (6) After peeling, the length L2 [mm] of the marked radius line on the support sheet was measured.

[0271] The elongation rate of the support sheet was calculated according to the following formula (i), and the recyclability of the support sheet was evaluated according to the following evaluation criteria. The results are shown in Table 1. Elongation rate [%]=(L2-L1) / L1×100 (i)

[0272] (Evaluation criteria for recyclability of support sheets) A: The elongation rate of the support sheet is small at 3% or less, and the support sheet has excellent recyclability, so it is acceptable. B: The elongation rate of the support sheet is greater than 3% and less than 6%, and the recyclability of the support sheet is good and pass. C: The elongation rate of the support sheet is 6% or more, and the recyclability of the support sheet is poor, and the sheet is unacceptable.

[0273] <Evaluation of chip peeling resistance during dicing> (Manufacture of silicon chips with support sheets) An 8-inch silicon wafer (thickness 200 μm) with one surface polished with #2000 was prepared. The pressure-sensitive adhesive layer in the support sheet obtained above was attached to the silicon wafer in a central region in the width direction, and the region surrounding the region attached to the silicon wafer was attached to a ring frame. The pressure-sensitive adhesive layer was attached to the silicon wafer and the ring frame at a temperature of 23° C. (laminating roller temperature 23° C., silicon wafer temperature 23° C.), at a bonding speed of 300 mm / min, and at a bonding pressure of 0.3 MPa. As a result, a silicon wafer with a support sheet, which includes a silicon wafer and a support sheet provided on one surface of the silicon wafer, was fixed to the ring frame (bonding process).

[0274] Next, a dicing device (DISCO Corp. "DFD6362") was used to dice the silicon wafer in the silicon wafer with the support sheet fixed to the ring frame, to produce multiple silicon chips with a size of 0.9 mm x 1.5 mm (processing step). At this time, a dicing blade "ZH05-SD2000-N1-90 CC" manufactured by DISCO Corp. was used as the dicing blade, the blade rotation speed was 35000 rpm, the blade feed speed was 60 mm / s, and the blade height was 0.06 mm. The blade was inserted into the silicon wafer with the support sheet from the surface on the silicon wafer side, and cut into the base material to a depth of 20 μm from the surface on the adhesive layer side. In this manner, a group of silicon chips with a support sheet was produced, in which a plurality of silicon chips were aligned and held on one support sheet.

[0275] (Evaluation of chip peel resistance during dicing) At this time, the number of peeled silicon chips was counted. In this case, not only chips of 0.9 mm x 1.5 mm (rectangular) but also corner chips (e.g. triangular) were counted as one chip if they peeled off. The following criteria were used for judgment. (Evaluation Criteria) A: The number of peeled silicon chips was 3 or less. B: The number of peeled silicon chips was 4 or more and 5 or less. C: Six or more silicon chips were peeled off.

[0276] <Evaluation of chip peel resistance during dicing when reattaching> (Manufacture of silicon chips with support sheets) An 8-inch silicon wafer (thickness 200 μm) with one surface polished with #2000 was prepared. The pressure-sensitive adhesive layer in the support sheet obtained above was attached to the silicon wafer in a central region in the width direction, and the region surrounding the region attached to the silicon wafer was attached to a ring frame. The pressure-sensitive adhesive layer was attached to the silicon wafer and the ring frame at a temperature of 23° C. (laminating roller temperature 23° C., silicon wafer temperature 23° C.), at a bonding speed of 300 mm / min, and at a bonding pressure of 0.3 MPa. As a result, a silicon wafer with a support sheet, which includes a silicon wafer and a support sheet provided on one surface of the silicon wafer, was fixed to the ring frame (bonding process). Next, while fixing the silicon wafer and the ring frame so as not to change their positional relationship, the support sheet was peeled off from the silicon wafer with the support sheet at a peel speed of approximately 300 mm / min (260 to 340 mm / min) and a peel angle of 180°. The same support sheet was again attached to the same silicon wafer, and the area surrounding the attached area to the silicon wafer was attached to the ring frame. At this time, the adhesive layer was attached to the silicon wafer and the ring frame under the attachment temperature condition of 23°C (laminating roller temperature 23°C, silicon wafer temperature 23°C), attachment speed 300mm / min, and attachment pressure 0.3MPa. As a result, the silicon wafer with the support sheet, which includes the silicon wafer and the support sheet provided on one side of the silicon wafer, was fixed to the ring frame (re-attachment process). The obtained silicon wafer with support sheet was diced under the same conditions as those described above in <Evaluation of chip peeling resistance during dicing> to produce multiple silicon chips measuring 0.9 mm x 1.5 mm by dicing the silicon wafer in the silicon wafer with support sheet fixed to a ring frame (processing step). In this manner, a group of silicon chips with a support sheet was produced, in which a plurality of silicon chips were aligned and held on one support sheet.

[0277] (Evaluation of chip peel resistance during dicing when reattached) At this time, the number of peeled silicon chips was counted. In this case, not only chips of 0.9 mm x 1.5 mm (rectangular) but also corner chips (e.g. triangular) were counted as one chip if they peeled off. The following criteria were used for judgment. (Evaluation Criteria) A: The number of peeled silicon chips was 3 or less. B: The number of peeled silicon chips was 4 or more and 5 or less. C: Six or more silicon chips were peeled off.

[0278] <Evaluation of silicon chip pick-up ability of support sheet> (Manufacture of silicon chips with support sheets) The silicon wafer with the support sheet was fixed to a ring frame (attachment process) using the same method as in the "Evaluation of chipping inspection accuracy of the support sheet" above. The silicon wafer with the support sheet fixed to the ring frame was placed in an oven and heated at 140°C for 2 hours (heating process). Next, the silicon wafer with the support sheet fixed to the ring frame was removed from the oven and allowed to cool until its temperature reached 23° C. Then, a group of silicon chips with support sheets were produced (processing step) in the same manner as in the above “Evaluation of chipping inspection accuracy of support sheet” except that the size of the silicon chips was changed from 1 mm × 1 mm to 2.5 mm × 2.5 mm.

[0279] (Evaluation of silicon chip pick-up ability of support sheet) Next, an ultraviolet ray irradiation device ("RAD-2000UV" manufactured by Lintec Corporation) was used to irradiate the adhesive layer in the group of silicon chips with support sheets with an illuminance of 230 mW / cm from the outside of the substrate side through the substrate. 2 , light intensity 200mJ / cm 2 The adhesive layer attached to the ring frame was cured by irradiating it with ultraviolet light under the above conditions (curing step). Next, using a pick-up die bonding device (Canon Machinery's "BESTEM D-510"), the silicon chips of the group of silicon chips with the cured support sheet were picked up by detaching them from the cured product of the adhesive layer under the following pick-up conditions (pick-up process). This pick-up was performed on a total of 100 silicon chips in 10 rows in two orthogonal directions divided from the center and the area near the center of the silicon wafer before dicing, among the silicon chips of the group of silicon chips with the cured support sheet, by pushing up one silicon chip with one pin from the support sheet side. Then, the pick-up property of the support sheet was evaluated according to the following criteria. The results are shown in Table 1.

[0280] (Pickup conditions) Push-up speed: 5mm / s Expanded amount: 4mm Curvature radius of the pin tip: 0.75 mm (Evaluation Criteria) A: All (100) silicon chips were picked up successfully. B: 1-4 silicon chips could not be picked up successfully, but all other silicon chips (96-99) could be picked up successfully. C: Five or more silicon chips could not be picked up normally.

[0281] <Measurement of storage modulus (E'23) of the second test piece of the adhesive layer> Using the same method as in the production of the support sheet, an energy ray-curable adhesive layer having a thickness of 15 μm was formed on the release-treated surface of the release film. A release film ("SP-PET381031" manufactured by Lintec Corporation) made of polyethylene terephthalate with one side treated for release by silicone treatment was used as the release film for processing, and the exposed surface of the pressure-sensitive adhesive layer was attached to the release-treated surface. The attachment was performed at room temperature, at a sticking speed of 5 m / min, and with a pressure of 0.4 MPa. As a result, a laminate (adhesive layer provided with release film and release film for process) in which a release film, a pressure-sensitive adhesive layer, and a release film for process were laminated in this order was produced. The pressure-sensitive adhesive layer in the laminate was used as a first test piece, and was used to produce the second test piece thereafter. Using the 14 laminates obtained above, the exposed surfaces of the pressure-sensitive adhesive layers (first test pieces) were sequentially bonded together while removing the release film and the release film for processing, to prepare a laminate having a thickness of 210 μm. Furthermore, a piece having a width of 4 mm was cut out from the laminate, and this was used as the second test piece. Next, the storage modulus E' of the second test piece was measured in the temperature range from -20°C to 150°C using an automatic dynamic viscoelasticity measuring device (A&D's "Rheovibron DDV-01FP") under the conditions of a chuck distance of 20 mm, a frequency of 11 Hz, a temperature rise rate of 3°C / min, and a constant rate of temperature rise, by the tensile method (tensile mode). Among these, the storage modulus (E'23) at a temperature of 23°C is shown in Table 1.

[0282] [Example 2] <<Manufacture and evaluation of support sheet>> An energy ray curable adhesive composition (I)-2 was prepared, which had the same composition as in Example 1, except that the crosslinking agent (β2)-2 (2 parts by mass) was used instead of the crosslinking agent (β2)-1 (2 parts by mass). A support sheet was produced and evaluated in the same manner as in Example 1, except that the adhesive composition (I)-2 was used instead of the adhesive composition (I)-1. The results are shown in Table 1.

[0283] [Reference example 1] <<Manufacture of support sheet>> <Production of energy ray curable acrylic resin (Ia)> The same acrylic polymer (1) as used in Example 1 was added with MOI, and an addition reaction was carried out in an air stream at 50°C for 48 hours to obtain an energy beam curable acrylic resin (Ia)-2. The amount of MOI used was such that the total number of moles of isocyanate groups in the MOI was 0.785 times the total number of moles of hydroxyl groups derived from HEMA in the acrylic polymer (1). The weight average molecular weight of the obtained energy beam curable acrylic resin (Ia)-2 was 500,000, and the glass transition temperature was -26°C.

[0284] <Production of Pressure-Sensitive Adhesive Composition (R)> The energy ray curable adhesive composition (R)-1 was prepared, which contains energy ray curable acrylic resin (Ia)-2 (100 parts by mass), energy ray curable compound (α)-1 (25 parts by mass), crosslinking agent (β2)-1 (4.12 parts by mass), and photopolymerization initiator (γ)-1 (3 parts by mass), and further contains methyl ethyl ketone as a solvent, and the total concentration of all components other than the solvent is 25% by mass. Note that the contents of all components other than methyl ethyl ketone shown here are the contents of the target product excluding the solvent.

[0285] <Formation of adhesive layer, production of support sheet> An adhesive layer (thickness 15 μm) was formed and a support sheet was produced in the same manner as in Example 1, except that the adhesive composition (R)-1 obtained above was used instead of the adhesive composition (I)-1.

[0286] <<Evaluation of the support sheet>> The support sheet obtained above was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0287] [Reference example 2] <<Manufacture and evaluation of support sheet>> An energy ray curable adhesive composition (R)-2 was prepared, which had the same composition as in Example 1, except that the content of the crosslinking agent (β1)-1 was 15.5 parts by mass instead of 13.5 parts by mass, and that the crosslinking agent (β2)-1 was not contained. A support sheet was produced and evaluated in the same manner as in Example 1, except that the adhesive composition (R)-2 was used instead of the adhesive composition (I)-1. The results are shown in Table 2.

[0288] [Reference example 3] <<Manufacture of support sheet>> <Production of energy ray curable acrylic resin (Ia)> The same acrylic polymer (1) as used in Example 1 was added with MOI, and an addition reaction was carried out in an air stream at 50°C for 48 hours to obtain an energy beam curable acrylic resin (Ia)-3. The amount of MOI used was such that the total number of moles of isocyanate groups in the MOI was 0.95 times the total number of moles of hydroxyl groups derived from HEMA in the acrylic polymer (1). The weight average molecular weight of the obtained energy beam curable acrylic resin (Ia)-3 was 440,000, and the glass transition temperature was -26°C.

[0289] <Production of Pressure-Sensitive Adhesive Composition (R)> The energy ray curable adhesive composition (R)-3 was prepared containing energy ray curable acrylic resin (Ia)-3 (100 parts by mass), energy ray curable compound (α)-1 (5.7 parts by mass), crosslinking agent (β2)-2 (0.59 parts by mass), and photopolymerization initiator (γ)-1 (3 parts by mass), and further containing methyl ethyl ketone as a solvent, and the total concentration of all components other than the solvent was 25% by mass. Note that the contents of all components other than methyl ethyl ketone shown here are the contents of the target product excluding the solvent.

[0290] <Formation of adhesive layer, production of support sheet> An adhesive layer (thickness 15 μm) was formed and a support sheet was produced in the same manner as in Example 1, except that the adhesive composition (R)-3 obtained above was used instead of the adhesive composition (I)-1.

[0291] <<Evaluation of the support sheet>> The support sheet obtained above was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0292] [Comparative Example 1] <<Manufacture and evaluation of support sheet>> An energy ray curable adhesive composition (R)-4 was prepared, which has the same composition as in Reference Example 3, except that the content of the crosslinking agent (β2)-2 is 0.53 parts by mass instead of 0.59 parts by mass, and that the energy ray curable compound (α)-1 is not contained. Then, a support sheet was produced and evaluated in the same manner as in Example 1, except that the adhesive composition (R)-4 was used instead of the adhesive composition (I)-1. The results are shown in Table 2.

[0293] [Comparative Example 2] <<Manufacture of support sheet>> <Production of energy ray curable acrylic resin (Ia)> The MOI was added to the acrylic polymer (2) and subjected to an addition reaction in an air stream at 50°C for 48 hours to obtain an energy beam curable acrylic resin (Ia)-4. The acrylic polymer (2) is a copolymer of 2EHA (35 parts by mass), 2EHMA (45 parts by mass), and HEA (20 parts by mass). The amount of MOI used was such that the total number of moles of isocyanate groups in the MOI was 0.7 times the total number of moles of hydroxyl groups derived from HEA in the acrylic polymer (2). The weight average molecular weight of the obtained energy beam curable acrylic resin (Ia)-4 was 880,000, and the glass transition temperature was -35°C.

[0294] <Production of Pressure-Sensitive Adhesive Composition (R)> An energy ray curable pressure sensitive adhesive composition (R)-5 was prepared, which contains energy ray curable acrylic resin (Ia)-4 (100 parts by mass), crosslinking agent (β2)-2 (9.26 parts by mass), and photopolymerization initiator (γ)-1 (3 parts by mass), and further contains methyl ethyl ketone as a solvent, and the total concentration of all components other than the solvent is 25% by mass. Note that the contents of all components other than methyl ethyl ketone shown here are the contents of the target product excluding the solvent.

[0295] <Formation of adhesive layer, production of support sheet> An adhesive layer (thickness 15 μm) was formed and a support sheet was produced in the same manner as in Example 1, except that the adhesive composition (R)-5 obtained above was used instead of the adhesive composition (I)-1.

[0296] <<Evaluation of the support sheet>> The support sheet obtained above was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0297] [Table 1]

[0298] [Table 2]

[0299] As is clear from the above results, in Examples 1 and 2, the adhesive layer in the support sheet could be easily peeled off from the back surface of the workpiece while maintaining its shape, i.e., the support sheet could be regenerated, and even after re-attachment, chip peeling could be prevented during dicing. Furthermore, even when heated at high temperatures of 140°C or higher, the workpiece could be properly picked up from the support sheet.

[0300] In Examples 1 and 2, the adhesive strength (X1) was 480 mN / 25 mm or less, and by using the support sheets of Examples 1 and 2, the pick-up properties were good enough to enable the silicon chip to be picked up normally even after the support sheet with the silicon mirror wafer attached was heated at 140°C for 2 hours.

[0301] Furthermore, in Examples 1 and 2, the adhesive strength (X0) was 7200 mN / 25 mm or less, and the adhesive layer in the support sheet could be peeled off from the back surface of the work while maintaining its shape, that is, the support sheet could be recycled.

[0302] Furthermore, in Examples 1 and 2, the adhesive strength (X01) was 6300 mN / 25 mm or more, which was sufficiently large. Therefore, by using the support sheets of Examples 1 and 2, it was possible to prevent chip peeling when the support sheet was peeled off from the back surface of the silicon wafer for the purpose of re-attachment, and the support sheet was re-attached to the back surface of the silicon wafer and diced.

[0303] Thus, the support sheets of Examples 1 and 2 had the desired properties. In Examples 1 and 2, the adhesive layer contained crosslinker (β1) and crosslinker (β2), and the content of crosslinker (β1) in the adhesive layer relative to the total mass of the adhesive layer was 11.4 mass%, which was presumably what made it easier to achieve the above-mentioned characteristics.

[0304] In addition, in Examples 1 and 2, the adhesive strength (X0) was 6600 mN / 25 mm or more, which was sufficiently large. Therefore, it was possible to prevent the chip from peeling off during dicing. Furthermore, it was presumed that by using the support sheets of Examples 1 and 2, it is possible to suppress the peeling of the silicon chip from the support sheet even if a significantly large force is applied to the silicon chip, for example, by dicing a silicon wafer at high speed or washing the silicon chip with high pressure after dicing.

[0305] Furthermore, the matte surface of the substrate had high embedding ability with the adhesive layer in Examples 1 and 2. As a result, in Examples 1 and 2, the average light transmittance (400 to 800 nm) of the support sheet (L1) was 82.6% or more, which was sufficiently high, and the chipping inspection accuracy of the support sheet was high.

[0306] Furthermore, in Examples 1 and 2, the adhesive strength (Y2) was 4600 mN / 25 mm or less, which was appropriately small. Therefore, it was presumed that by using the support sheets of Examples 1 and 2, when the silicon wafer with the support sheet fixed to the ring frame was heated at 140° C., the silicon wafer with the support sheet could be peeled off from the ring frame without further curing the adhesive layer with energy rays, and furthermore, the adhesive layer could be prevented from remaining on the ring frame.

[0307] Furthermore, in Examples 1 and 2, the adhesive strength change rate of the adhesive layer was 103 to 137%, which was within a preferable range. Therefore, it was presumed that by using the support sheets of Examples 1 and 2, even if the heating temperature of the support sheet (adhesive layer) was 130°C, the silicon chip could be picked up normally under the same conditions as when it was 140°C. In other words, the support sheets of Examples 1 and 2 did not require any changes to the device condition settings when picking up the silicon chip, regardless of whether the heating temperature was 140°C or 130°C, and were highly versatile in terms of setting the heating temperature.

[0308] Furthermore, in Examples 1 and 2, the adhesive strength (X3) was 360 mN / 25 mm or less, which was sufficiently small. Therefore, it was presumed that by using the support sheets of Examples 1 and 2, even if the energy ray curing of the adhesive layer in the support sheet and the heating of the support sheet are performed in this order, the silicon chip can be picked up normally in the same manner as when the heating of the support sheet and the energy ray curing of the adhesive layer in the support sheet are performed in this order. In other words, the support sheets of Examples 1 and 2 have many applicable variations as a manufacturing method for workpieces such as semiconductor chips, and are highly versatile in terms of usage.

[0309] Furthermore, in Examples 1 and 2, the difference between the average light transmittance (L1) of the unheated support sheet and the average light transmittance (L2) of the heated support sheet was 45.4% or more, which was sufficiently large. The support sheets of Examples 1 and 2 were clearly whitened when heated at 140°C, and these support sheets were highly distinguishable when heated at 140°C.

[0310] Furthermore, in Examples 1 and 2, the storage modulus (E'23) was sufficiently large at 5.2 MPa or more. Therefore, by using the support sheets of Examples 1 and 2, when an abnormality occurs during application of the support sheet and the support sheet is peeled off from the silicon wafer, deformation of the support sheet can be suppressed, roughness of the surface of the adhesive layer can be prevented, and uniform reapplication within the surface of the adhesive layer becomes possible, and it was presumed that the support sheet has excellent reusability. In addition, it was presumed that the adhesive layer can be suppressed from remaining on the workpiece, and that the reworkability is excellent.

[0311] Thus, the support sheets of Examples 1 and 2 were also excellent in unintended properties.

[0312] In contrast to these, in the support sheets of Reference Example 2 and Comparative Example 1, the adhesive layer in the support sheet could not be easily peeled off from the back surface of the workpiece while maintaining its shape, while in the support sheets of Reference Example 1 and Comparative Example 2, chips peeled off when the support sheet was reattached and diced, and in the support sheets of Reference Examples 1 to 3 and Comparative Examples 1 to 2, when heated to a high temperature of 140°C or higher, the workpiece could not be properly picked up from the support sheet.

[0313] In Reference Examples 1 to 3 and Comparative Examples 1 and 2, the adhesive strength (X1) was 600 mN / 25 mm or more, and after the support sheet with the silicon mirror wafer attached was heated at 140°C for 2 hours, many of the silicon chips could not be picked up normally, and the pickup performance was significantly poor.

[0314] In Reference Example 2 and Comparative Example 1, the support sheets had high adhesive strengths (X0) of 11000 mN / 25 mm or more, and therefore the adhesive layer in the support sheet could not be easily peeled off from the back surface of the workpiece while maintaining its shape.

[0315] In Reference Example 1 and Comparative Example 2, the adhesive strength (X01) was small, being 1500 mN / 25 mm or less. Therefore, when the support sheet of Reference Example 1 or Comparative Example 2 was used and the support sheet was reattached, chip peeling occurred during dicing.

[0316] Thus, none of the support sheets of Comparative Examples 1 and 2 and Reference Examples 1 to 3 had the desired properties.

[0317] Furthermore, in Reference Example 1, the adhesive strength (X0) was small at 160 mN / 25 mm. Therefore, by using the support sheet of Reference Example 1, chip peeling occurred during dicing.

[0318] Furthermore, the matte surface of the substrate was not sufficiently embedded by the adhesive layer in Comparative Examples 1 and 2. As a result, the average light transmittance (400-800 nm) (L1) of the support sheet in Comparative Examples 1 and 2 was low, being 79.1% or less, and the chipping inspection accuracy of the support sheet was poor.

[0319] Furthermore, the adhesive strength (Y2) was too large, being 7900 mN / 25 mm or more, in Comparative Examples 1 and 2 and Reference Examples 1 and 3. Therefore, it was presumed that by using the support sheets of Comparative Examples 1 and 2 and Reference Examples 1 and 3, when the silicon wafer with the support sheet fixed to the ring frame was heated at 140° C., the silicon wafer with the support sheet could not be peeled off from the ring frame unless the adhesive layer was further cured with energy rays.

[0320] Furthermore, in Comparative Example 1 and Reference Examples 1 to 3, the adhesive strength change rate of the adhesive layer was 171% or more, which was too large. Therefore, it was presumed that by using the support sheets of Comparative Example 1 and Reference Examples 1 to 3, when the heating temperature of the support sheet (adhesive layer) was 130° C., the silicon chip could not be picked up normally under the same conditions as in the case of 140° C. In other words, the support sheets of Comparative Example 1 and Reference Examples 1 to 3 could not be said to be highly versatile in terms of setting the heating temperature.

[0321] Furthermore, in Comparative Examples 1-2 and Reference Example 2, the adhesive strength (X3) was 580 mN / 25 mm or more, which was too large. Therefore, it was presumed that when the support sheets of Comparative Examples 1-2 and Reference Example 2 are used, and the energy ray curing of the adhesive layer in the support sheet and the heating of the support sheet are performed in this order, the silicon chip cannot be picked up normally, unlike the case where the support sheet is heated and the energy ray curing of the adhesive layer in the support sheet are performed in this order. In other words, the support sheets of Comparative Examples 1-2 and Reference Example 2 cannot be said to be highly versatile in terms of usage.

[0322] Furthermore, in Comparative Examples 1 and 2 and Reference Examples 1 and 3, the difference between the average light transmittance (L1) of the unheated support sheet and the average light transmittance (L2) of the heated support sheet was small, being 12.2% or less. The support sheets of Comparative Examples 1 and 2 and Reference Examples 1 and 3 showed a low degree of whitening when heated at 140°C, and these support sheets showed low discernibility when heated at 140°C.

[0323] Furthermore, in Comparative Examples 1-2 and Reference Examples 1-3, the storage modulus (E'23) was as small as 3.3 MPa or less. Therefore, when the support sheets of Comparative Examples 1-2 and Reference Examples 1-3 are applied and peeled off, the support sheet is deformed and the surface of the adhesive layer is roughened, so that the adhesive layer cannot be uniformly reapplied within its plane, and it is presumed that the reusability of the support sheet is poor. In addition, the adhesive layer remains on the workpiece, so that the reworkability is also presumed to be poor. [Industrial Applicability]

[0324] The present invention may be utilized in the manufacture of workpieces such as semiconductor chips. [Explanation of symbols]

[0325] DESCRIPTION OF SYMBOLS 1...support sheet, 11...substrate, 11a...one surface of substrate (surface on which adhesive layer is formed), 12...adhesive layer, 12'...energy ray cured product of adhesive layer, 8...ring frame, 9...semiconductor wafer, 90...semiconductor chip, 109...semiconductor wafer with support sheet

Claims

1. A support sheet comprising a substrate and an energy ray-curable adhesive layer provided on one surface of the substrate, the support sheet is attached to the mirror surface of a silicon mirror wafer by the pressure-sensitive adhesive layer, and the silicon mirror wafer provided with the support sheet is left to stand for 30 minutes under a temperature condition of 23° C., and the adhesive strength (X0) between the pressure-sensitive adhesive layer and the silicon mirror wafer is measured. The adhesive strength (X0) is 8000 mN / 25 mm or less, the support sheet is attached to a mirror surface of a silicon mirror wafer by the pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer after attachment is heated at 140° C., the pressure-sensitive adhesive layer after heating is energy ray-cured, and an adhesive strength (X1) between the energy ray-cured product of the pressure-sensitive adhesive layer and the silicon mirror wafer is measured; the adhesive strength (X1) is 500 mN / 25 mm or less; a support sheet in which the support sheet is attached to a mirror surface of a silicon mirror wafer by the adhesive layer, the silicon mirror wafer with the support sheet is left to stand for 30 minutes under a temperature condition of 23° C., the support sheet is peeled off at a peeling speed of 300 mm / min so that the surface of the silicon mirror wafer to which the adhesive layer was attached and the surface of the adhesive layer to which the silicon mirror wafer was attached form an angle of 180°, the support sheet is again attached to the same position of the mirror surface of the silicon mirror wafer by the same peeled surface of the adhesive layer, the silicon mirror wafer with the support sheet is left to stand for 30 minutes under a temperature condition of 23° C., and the adhesive strength (X01) between the adhesive layer and the silicon mirror wafer after re-attachment is measured, and the adhesive strength (X01) is 2000 mN / 25 mm or more.

2. The support sheet according to claim 1 , wherein the pressure-sensitive adhesive layer contains a block type crosslinking agent (β1).

3. The support sheet according to claim 1 or 2, wherein the average light transmittance (L1) of the support sheet in the wavelength range of 400 to 800 nm is 80% or more.

4. The support sheet according to claim 1 or 2, wherein when the support sheet is attached to the surface of a stainless steel plate by the adhesive layer, the adhesive layer after attachment is heated at 140°C, and the adhesive strength (Y2) between the adhesive layer after heating and the stainless steel plate is measured, the adhesive strength (Y2) is 6000 mN / 25 mm or less.

5. 3. The support sheet according to claim 1 or 2, wherein when the support sheet is attached to a mirror surface of a silicon mirror wafer by the adhesive layer, the silicon mirror wafer provided with the support sheet is left to stand for 30 minutes under a temperature condition of 23°C, and an adhesive strength (X0) between the adhesive layer and the silicon mirror wafer is measured, the adhesive strength (X0) is 2000 mN / 25 mm or more.

6. The support sheet was attached to the mirror surface of a silicon mirror wafer by the pressure-sensitive adhesive layer, and the pressure-sensitive adhesive layer after attachment was heated at 130° C. and the pressure-sensitive adhesive layer after heating was energy ray-cured. When the adhesive strength (X11) between the energy ray-cured product of the pressure-sensitive adhesive layer and the silicon mirror wafer was measured, the adhesive strength (X11) was found to be equal to or greater than the adhesive strength (X11) of the silicon mirror wafer. Adhesive strength change rate=Adhesive strength (X1) / Adhesive strength (X11)×100 (i) The support sheet according to claim 1 or 2, wherein the adhesive strength change rate calculated by is 90 to 150%.

7. 3. The support sheet according to claim 1 or 2, wherein when the support sheet is attached to a mirror surface of a silicon mirror wafer by the pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer after attachment is energy ray-cured, the energy ray-cured product of the pressure-sensitive adhesive layer is heated at 140°C, and an adhesive force (X3) between the heated energy ray-cured product of the pressure-sensitive adhesive layer and the silicon mirror wafer is measured, the adhesive force (X3) is 500 mN / 25 mm or less.

8. The support sheet according to claim 1 or 2, wherein the difference between the average light transmittance (L1) of the support sheet in the wavelength range of 400 to 800 nm and the average light transmittance (L2) of the support sheet after heating in the wavelength range of 400 to 800 nm when the support sheet is heated at 140° C. for 2 hours is 30% or more.

9. 3. The support sheet according to claim 1 or 2, wherein a second test piece having a thickness of 200±20 μm is prepared by laminating a plurality of first test pieces of the pressure-sensitive adhesive layer having a thickness of less than 200 μm, and the second test piece is heated from −20° C. to 150° C. in a tensile mode under conditions of a frequency of 11 Hz, a temperature increase rate of 3° C. / min, and a uniform heating rate, and the storage modulus E′ of the second test piece is measured, and the storage modulus (E′23) when the temperature of the second test piece is 23° C. is 4.0 MPa or more.

10. A method for manufacturing a workpiece, the method comprising: an attachment step of attaching the adhesive layer in the support sheet described in claim 1 or 2 to the workpiece and a fixing jig to fix a workpiece with a support sheet, the workpiece including the workpiece and the support sheet provided on the workpiece, to the fixing jig; a heating step of heating the adhesive layer in the support sheet fixed to the fixing jig after the attachment step; a processing step of producing the workpiece by processing the workpiece in the workpiece with the support sheet fixed to the fixing jig after the attachment step; a curing step of curing the adhesive layer attached to the fixing jig with energy rays after the heating step and the processing step; and a picking up step of separating the workpiece from the cured product of the adhesive layer and picking it up after the curing step.

11. The method of claim 10, wherein the fixture is made of stainless steel.

Citation Information

Patent Citations

  • Method for manufacturing semiconductor device and protective tape

    JP2018082131A

  • Adhesive sheet

    JP2019065113A

  • Semiconductor-processing sheet

    JP2019179841A

  • Pressure-sensitive adhesive sheet for semiconductor processing

    JP2021097075A

  • Adhesive composition, cured product, and adhesive sheet

    JP2022038777A