Transfer sheet, method of producing article, and article with release film
The transfer sheet with a release film having specific stiffness and peel strength characteristics addresses the issues of adherence and peeling during transfer, ensuring reliable and smooth peeling from adherends.
Patent Information
- Application Number
- JP2023055061
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-30
AI Technical Summary
The transfer sheet tends to adhere to the corners of adherends due to the stiffness of the release film, leading to lifting and partial peeling, and the release film peels off partially from the transfer layer due to springback, making it difficult to peel off completely.
The transfer sheet is designed with a release film having a loop stiffness of 0.18N/15mm or less and a peel strength of 0.7N/25mm or less, with a specific relationship between loop stiffness and peel strength (Y≧0.67X+0.17) to prevent lifting and partial peeling, allowing easy removal of the release film.
This design effectively suppresses lifting at corners and partial peeling, ensuring smooth peeling of the release film from the transfer layer, enhancing the reliability and quality of the transfer process.
Smart Images

Figure 2024142751000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a transfer sheet, a method for manufacturing an article, and an article with a release film. [Background technology]
[0002] It is known that a transfer layer (a layer transferred from a transfer sheet) of a transfer sheet is transferred to an adherend such as a metal member or a resin member to decorate the adherend. For example, Patent Document 1 discloses a rain gutter in which an oxide film layer is arranged on the outer surface of an aluminum base material, a decorative layer is arranged on the outer surface of the oxide film layer, and a pattern is applied to the surface of the decorative layer. Specifically, Patent Document 1 discloses forming a decorative layer by hydraulic transfer processing on the outer surface of an anodized aluminum base material. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-12283 A Summary of the Invention [Problem to be solved by the invention]
[0004] When the transfer layer of the transfer sheet is transferred to an adherend having multiple surfaces, the stiffness of the release film of the transfer sheet may cause the transfer sheet to float from the adherend at the corners of the adherend. In addition, after the transfer sheet is adhered to the adherend, the stiffness of the release film may cause the release film to partially peel off from the transfer layer (partial peeling of the release film due to springback). Furthermore, the transfer sheet is required to be able to easily peel off the release film from the transfer layer after the transfer sheet is adhered to the adherend.
[0005] The present disclosure has been made in consideration of the above-mentioned situation, and has as its main object to provide a transfer sheet that suppresses floating of the transfer sheet at the corner portions, suppresses partial peeling of the release film due to springback, and enables the release film to be easily peeled off from the transfer layer. [Means for solving the problem]
[0006] The present disclosure provides a transfer sheet having a release film and a transfer layer disposed on one side of the release film, wherein the loop stiffness of the release film is 0.18 N / 15 mm or less, the peel strength of the release film and the transfer layer is 0.7 N / 25 mm or less, and when the loop stiffness is X and the peel strength is Y, X and Y satisfy Y≧0.67X+0.17.
[0007] The present disclosure provides a method for manufacturing an article, comprising: a preparation step of preparing an adherend having multiple surfaces and the transfer sheet described above; and a wrapping step of sequentially bonding the transfer layer of the transfer sheet to the multiple surfaces of the adherend using a roller.
[0008] In the present disclosure, there is provided a method for producing a substrate comprising: an adherend having a plurality of surfaces; a transfer layer disposed so as to conform to the plurality of surfaces; and a release film disposed so as to conform to the transfer layer, The loop stiffness of the release film is 0.18 N / 15 mm or less, The peel strength between the release film and the transfer layer is 0.7 N / 25 mm or less; When the loop stiffness is X and the peel strength is Y, the X and Y satisfy Y≧0.67X+0.17. Effect of the Invention
[0009] The present disclosure has the effect of providing a transfer sheet that suppresses floating of the transfer sheet at the corners, suppresses partial peeling of the release film due to springback, and enables the release film to be easily peeled off from the transfer layer. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic cross-sectional view illustrating a transfer sheet according to the present disclosure. [Diagram 2] FIG. 2 is an explanatory diagram outlining a method for measuring loop stiffness in the present disclosure. [Diagram 3] 1 is a schematic side view illustrating a lapping process in the present disclosure; [Figure 4] 4A and 4B are cross-sectional views taken along lines AA, BB, CC, DD, and EE in FIG. [Diagram 5] FIG. 4 is an explanatory diagram illustrating the axial direction of each roller. [Figure 6] 1 is a schematic cross-sectional view illustrating a part of an article with a release film in the present disclosure, and a part of an article in the present disclosure. [Figure 7] 1 is a graph showing the relationship between loop stiffness and peel strength in Examples 1 to 5 and Comparative Examples 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The following describes the embodiments with reference to the drawings. However, the present disclosure can be implemented in many different forms and should not be limited to the description of the embodiments exemplified below. In addition, the drawings may show the width, thickness, and shape of each part in a schematic manner compared to the actual form in order to make the description clearer, but this is merely an example and should not be interpreted as being limiting.
[0012] In this specification, when describing a mode in which another component is disposed on a certain component, the term "above" or "below" includes both cases in which another component is disposed directly above or below the certain component so as to be in contact with the component, and cases in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified. In addition, in this specification, when describing a mode in which another component is disposed on the surface of a certain component, the term "on the surface" includes both cases in which another component is disposed directly above or below the certain component so as to be in contact with the component, and cases in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified.
[0013] The transfer sheet, the method for producing an article, and the article with a release film according to the present disclosure will be described in detail below.
[0014] A. Transfer sheet Fig. 1(a) is a schematic cross-sectional view illustrating a transfer sheet in the present disclosure. As shown in Fig. 1(a), a transfer sheet 10 has a release film 1 and a transfer layer X arranged on one surface of the release film 1. The transfer layer X shown in Fig. 1(a) is a layer formed by applying a first protective layer 2 and a second protective layer 3 from the release film 1 side in a thickness direction D. T In this order, the transfer sheet 10 has the above-mentioned layers. Also, as shown in FIG. 1(b), the transfer sheet 10 may have a design layer 4 on the surface of the second protective layer 3 opposite to the first protective layer 2. In the present disclosure, the loop stiffness of the release film 1 is within a predetermined range. Also, the peel strength of the release film 1 and the transfer layer X is within a predetermined range. Furthermore, the loop stiffness of the release film 1 and the peel strength of the release film 1 and the transfer layer X satisfy a predetermined relationship.
[0015] According to the present disclosure, the loop stiffness and the peel strength are each within a specific range, and further, the loop stiffness and the peel strength satisfy a specific relationship, resulting in a transfer sheet that suppresses floating of the transfer sheet at the corners, suppresses partial peeling of the release film due to springback, and enables the release film to be easily peeled off from the transfer layer.
[0016] As described above, when the transfer layer of the transfer sheet is transferred to an adherend having multiple surfaces, the stiffness of the release film of the transfer sheet may cause the transfer sheet to not adhere sufficiently to the adherend at the corners of the adherend, causing the transfer sheet to float from the adherend. The corners of the adherend are the boundaries between adjacent surfaces. The lifting of the transfer sheet at the corners leads to product defects, so it is preferable that it does not occur. In addition, after the transfer sheet is adhered to the adherend, the release film may partially peel off from the transfer layer due to the stiffness of the release film (partial peeling of the release film due to springback). After the transfer sheet is adhered to the adherend, the release film functions as a protective film that protects the adherend and the transfer layer from external impact. Therefore, it is preferable that partial peeling of the release film due to springback does not occur. Furthermore, it is required that the transfer sheet be able to be easily peeled off from the transfer layer after the transfer sheet is adhered to the adherend.
[0017] In particular, immediately after the transfer sheet is attached to the adherend, it is required to suppress partial peeling of the release film from the transfer layer due to springback. On the other hand, it is required that the release film, which also functions as a protective film, can be peeled off well from the transfer layer. In response to such conflicting problems, the present inventors have conducted extensive research and found that the above conflicting problems can be solved by having the peel strength of the release film and the transfer layer in a specific range, and further, by having the above peel strength and the loop stiffness of the release film satisfy a specific relationship. Furthermore, the present inventors have found that by having the loop stiffness of the release film in a specific range, it is possible to suppress the lifting of the transfer sheet at the corners even when the transfer layer is attached to an adherend having multiple surfaces.
[0018] In addition, as described later, the transfer sheet in the present disclosure is preferably used for wrapping processing. The wrapping processing is a processing in which the transfer layer of the transfer sheet is sequentially laminated to multiple surfaces of the adherend using a roller. Since the peel strength of the release film and the transfer layer is, for example, lower than the peel strength of each layer constituting the transfer layer, when the transfer sheet is sequentially laminated to multiple surfaces as in the wrapping processing, partial peeling of the release film due to the above-mentioned springback is likely to occur. In contrast, in the present disclosure, the peel strength of the release film and the transfer layer is in a specific range, and further, the above-mentioned peel strength and the loop stiffness of the release film satisfy a specific relationship, thereby suppressing partial peeling of the release film from the transfer layer due to springback, and finally, the release film, which also functions as a protective film, can be satisfactorily peeled from the transfer layer.
[0019] In addition, as described later, the transfer sheet in the present disclosure is useful as a transfer sheet used in the manufacture of exterior products (items for outdoor use). Exterior products are exposed to harsh environments compared to interior products (items for indoor use), and therefore high weather resistance is required. For example, when an exterior product is manufactured using a decorative sheet, a transparent resin layer may be provided on the decorative sheet for the purpose of improving strength. In this case, since the transparent resin layer is a relatively thick layer, for example, high weather resistance is imparted by adding a sufficient amount of weather resistance agent to the transparent resin layer. In contrast, it is technically difficult to impart high weather resistance to a transfer sheet that does not have a layer corresponding to the transparent resin layer. In the present disclosure, as described later, it is preferable that the transfer layer has a first protective layer and a second protective layer, and both the first protective layer and the second protective layer contain a weather resistance agent. This makes it possible to impart high weather resistance while maintaining the properties required for the first protective layer (for example, surface properties such as scratch resistance) and the properties required for the second protective layer (for example, adhesion).
[0020] In addition, in the case of a transfer sheet, the adhesion of the first protective layer and the second protective layer is likely to be insufficient. Here, in the case of a decorative sheet, a design layer is usually formed on a base layer, then a second protective layer is formed on the design layer, and then the first protective layer is formed on the second protective layer. The first protective layer is typically prepared by curing a composition for forming the first protective layer formed on the second protective layer, so that the adhesion of the first protective layer and the second protective layer is good. In contrast, in the case of a transfer sheet, the first protective layer is typically formed on a release film, then a second protective layer is formed on the first protective layer, and then a design layer is formed on the second protective layer. The first protective layer is typically prepared by curing a composition for forming the first protective layer on a release film. Since the second protective layer is formed on the cured first protective layer, the adhesion of the first protective layer and the second protective layer is likely to be insufficient. In the present disclosure, it is preferable that the second protective layer is a layer having higher flexibility than the first protective layer. This can increase the adhesion of the first protective layer and the second protective layer.
[0021] 1. Loop stiffness and peel strength In the present disclosure, the loop stiffness of the release film is within a specific range. Also, in the present disclosure, the peel strength of the release film and the transfer layer is within a specific range. Furthermore, in the present disclosure, the loop stiffness and the peel strength satisfy a specific relationship.
[0022] (1) Loop stiffness In the present disclosure, the loop stiffness of the release film is in a specific range. The degree of stiffness of the release film is specified by the loop stiffness. FIG. 2 is an explanatory diagram for explaining an outline of the method for measuring loop stiffness in the present disclosure. As shown in FIG. 2, the release film 1 peeled off from the transfer sheet is cut to prepare a rectangular sample, and the ends of the release film 1 are overlapped to deform the release film 1 into a loop shape. Thereafter, the overlapped ends are fixed by a fixing jig 41 of a loop stiffness tester. A pressure jig 42 of the loop stiffness tester is pressed vertically against the loop-shaped release film 1 fixed by the fixing jig 41 to measure the stress during compression. In the present disclosure, the release film peeled off from the transfer sheet is cut into a rectangular shape with a width of 15 mm and a length of 150 mm to prepare a sample. Furthermore, the sample is fixed to a loop stiffness tester so that the loop length is 60 mm, and a pressure tool is pressed against it from the vertical direction to measure the stress during compression, and the maximum value of the stress is calculated as the loop stiffness.
[0023] The loop stiffness of the release film is usually 0.18N / 15mm or less, and may be 0.15N / 15mm or less. If the loop stiffness of the release film is too large, the transfer sheet is likely to float at the corners. On the other hand, the loop stiffness of the release film is, for example, 0.005N / 15mm or more, may be 0.010N / 15mm or more, or may be 0.012N / 15mm or more. The loop stiffness of the release film can be adjusted, for example, by the thickness of the release film. The thicker the release film, the higher the loop stiffness is usually.
[0024] (2) Peel strength In the present disclosure, the peel strength of the release film and the transfer layer is within a specific range. The peel strength of the release film and the transfer layer is measured by the following method. First, the transfer sheet is cut to a width of 25 mm, and a double-sided tape is attached to the entire surface of the release film opposite the transfer layer, and the release film is fixed to a metal plate with a width of 25 mm. Next, a 25 mm wide cellophane tape (registered trademark) made by Nichiban is attached to the entire surface of the transfer layer opposite the release film. Next, a peel strength tester is used to measure the peel strength under the conditions of a peel speed of 200 mm / min and a peel angle of 90°. After exceeding the upper yield point, the integral average value of the peel strength from the point where the lower yield point load is reached to 20 mm is taken, and the peel strength (N / 25 mm) is calculated.
[0025] The peel strength of the release film and the transfer layer is usually 0.7 N / 25 mm or less, and may be 0.6 N / 25 mm or less. If the peel strength of the release film and the transfer layer is too large, it becomes difficult to peel the release film well from the transfer layer. On the other hand, the peel strength of the release film and the transfer layer is, for example, 0.17 N / 25 mm or more, and may be 0.19 N / 25 mm or more. The peel strength of the release film and the transfer layer can be adjusted, for example, by the surface properties of the transfer layer side surface of the release film and the hardness of the transfer layer (e.g., protective layer). For example, the larger the surface roughness of the transfer layer side surface of the release film, the smaller the peel strength of the release film and the transfer layer will usually be. Also, the softer the transfer layer (e.g., protective layer), the greater the peel strength of the release film and the transfer layer will usually be.
[0026] (3) Relationship between loop stiffness and peel strength In the present disclosure, when the loop stiffness is X and the peel strength is Y, X and Y usually satisfy Y≧0.67X+0.17. When X and Y satisfy Relational Formula 1, partial peeling of the release film due to springback can be suppressed. As described in the examples described later, X and Y may satisfy Y≧0.67X+0.19. In addition, X and Y may satisfy Y≦2.99X+0.03.
[0027] 2. Transfer layer The transfer layer in the present disclosure is a layer transferred from a transfer sheet. The transfer layer preferably has a protective layer that protects the surface of the adherend. In addition, the transfer layer preferably has a design layer on the side of the protective layer opposite to the release film.
[0028] (1) Protective layer The transfer layer in the present disclosure preferably has a protective layer. The protective layer is not particularly limited. The transfer layer may have only one protective layer, or may have two or more protective layers. For example, the transfer layer may be a single layer of the first protective layer described later, or a single layer of the second protective layer described later. In particular, the transfer layer preferably has the first protective layer and the second protective layer described later in this order in the thickness direction from the release film side. This is because it is particularly useful as a transfer sheet used for exterior products (items for outdoor use).
[0029] (i) First protective layer The transfer layer in the present disclosure preferably has a first protective layer. The first protective layer contributes to improving the surface properties (e.g., scratch resistance) of the article. The first protective layer and the release film may be arranged so as to be in direct contact with each other, or may be arranged via another layer.
[0030] The first protective layer preferably contains a cured product (crosslinked structure) of a curable resin composition as a resin component. The proportion of the cured product of the curable resin composition is, for example, 70% by mass or more, 90% by mass or more, 95% by mass or more, or 100% by mass, based on the total resin components constituting the first protective layer.
[0031] Examples of the curable resin composition used in the first protective layer include an ionizing radiation curable resin composition and a heat curable resin composition. Examples of the ionizing radiation curable resin composition include an electron beam curable resin composition and an ultraviolet ray curable resin composition. Among these, an electron beam curable resin composition is preferred because it does not require a polymerization initiator, has little odor, and is less likely to cause coloring.
[0032] The ionizing radiation curable resin composition is a composition containing a compound having an ionizing radiation curable functional group (hereinafter, also referred to as "ionizing radiation curable compound"). The ionizing radiation curable functional group is a group that crosslinks and cures when irradiated with ionizing radiation, and examples of such functional groups include functional groups having an ethylenic double bond, such as a (meth)acryloyl group, a vinyl group, and an allyl group. In the present disclosure, the (meth)acryloyl group refers to an acryloyl group or a methcroyl group.
[0033] Ionizing radiation refers to electromagnetic waves or charged particle beams that have an energy quantum capable of polymerizing or crosslinking molecules. Examples of ionizing radiation include electron beams (EB) and ultraviolet rays (UV). Other examples of ionizing radiation include electromagnetic waves such as X-rays and gamma rays, and charged particle beams such as alpha rays and ion beams.
[0034] The ionizing radiation curable resin composition preferably contains, as the ionizing radiation curable compound, one or more selected from, for example, urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, polycarbonate (meth)acrylate, and acrylic (meth)acrylate. Among them, the ionizing radiation curable resin composition preferably contains at least urethane (meth)acrylate as the ionizing radiation curable compound. In the present disclosure, urethane (meth)acrylate refers to urethane acrylate or urethane methacrylate. The urethane (meth)acrylate is preferably a caprolactane-based urethane (meth)acrylate.
[0035] When the ionizing radiation curable resin composition contains a caprolactane-based urethane (meth)acrylate, the caprolactane-based urethane (meth)acrylate preferably has 2 or more and 4 or less functional groups, more preferably 2 or more and 3 or less functional groups.
[0036] The ionizing radiation curable resin composition may contain a caprolactane-based urethane (meth)acrylate and a non-caprolactane-modified urethane (meth)acrylate. In this case, the content of the caprolactane-based urethane (meth)acrylate contained in the first protective layer is M CLUA The content of urethane (meth)acrylate not modified with caprolactone is M UA Let us assume that UA and M. CLUA M for the sum of CLUA Mass ratio (M CLUA / (M UA +M CLUA )) is, for example, 40% by mass or more and 90% by mass or less, alternatively 45% by mass or more and 80% by mass or less, or 50% by mass or more and 70% by mass or less.
[0037] Caprolactan-based urethane (meth)acrylate can usually be obtained by reacting caprolactan-based polyol, organic isocyanate, and hydroxy (meth)acrylate. For example, a method of synthesis includes reacting polycaprolactan-based polyol with organic polyisocyanate to generate a polyurethane prepolymer containing -NCO groups (isocyanate groups) at both ends, and then reacting it with hydroxy (meth)acrylate.
[0038] Caprolactane polyols may be commercially available, preferably having two hydroxyl groups and a number average molecular weight of 500 to 3000, more preferably 750 to 2000. In addition, polyols other than caprolactane polyols, such as ethylene glycol, diethylene glycol, 1,4-butanediol, 1,6-hexanediol, etc., may be used in combination in any ratio. As the organic polyisocyanate, a diisocyanate having two isocyanate groups is preferred, and from the viewpoint of suppressing yellowing, isophorone diisocyanate, hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, trimethylhexamethylene diisocyanate, etc. are preferred. As the hydroxy(meth)acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, caprolactane-modified 2-hydroxyethyl acrylate, etc. are preferred.
[0039] When the ionizing radiation curable resin composition contains a caprolactane polyol, the caprolactane urethane (meth)acrylate is preferably a caprolactane diol urethane (meth)acrylate. The caprolactane diol urethane (meth)acrylate refers to a urethane (meth)acrylate having a diethylene glycol terminal, among caprolactane urethane (meth)acrylates. By using the caprolactane diol urethane (meth)acrylate, it is possible to suppress the occurrence of cracks and whitening in the first protective layer.
[0040] The ionizing radiation curable resin composition may contain a hydroxyl group-containing (meth)acrylate as an ionizing radiation curable compound. Examples of the hydroxyl group-containing (meth)acrylate include hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, 1,4-cyclohexane dimethanol monoacrylate, polyethylene glycol monoacrylate, polyethylene glycol monomethacrylate, trimethylolpropane diacrylate, trimethylolpropane dimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, dipentaerythritol hexaacrylate, dipentaerythritol hexamethacrylate, glycidyl acrylate, glycidyl methacrylate, isocyanuric acid monoacrylate, isocyanuric acid monomethacrylate, isocyanuric acid diacrylate, isocyanuric acid dimethacrylate, glycerin diacrylate, and glycerin dimethacrylate. The hydroxyl group-containing (meth)acrylate may be a hydroxyl group-containing (meth)acrylate modified with ethylene oxide (EO), propylene oxide (PO), caprolactone, etc. The proportion of the hydroxyl group-containing (meth)acrylate in the ionizing radiation curable resin composition is, for example, 10% by mass or more and 90% by mass or less.
[0041] The number average molecular weight of the ionizing radiation curable compound is, for example, from 200 to 10,000, may be from 1,000 to 10,000, or may be from 2,000 to 10,000. The number average molecular weight is an average molecular weight measured by GPC analysis and converted into standard polystyrene.
[0042] For example, when the ionizing radiation curable compound is an ultraviolet ray curable compound, the ionizing radiation curable compound preferably contains at least one of a photopolymerization initiator and a photopolymerization accelerator. Examples of the photopolymerization initiator include acetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzyl dimethyl ketal, benzoyl benzoate, α-acyloxime ester, acylphosphine oxide, and thioxanthones. Examples of the photopolymerization accelerator include p-dimethylaminobenzoic acid isoamyl ester and p-dimethylaminobenzoic acid ethyl ester.
[0043] The first protective layer preferably contains a weathering agent. Examples of the weathering agent include an ultraviolet absorbing agent and a light stabilizer. The first protective layer preferably contains at least one of an ultraviolet absorbing agent and a light stabilizer. The first protective layer may contain one or more ultraviolet absorbing agents. Similarly, the first protective layer may contain one or more light stabilizers.
[0044] Examples of the ultraviolet absorbing agent contained in the first protective layer include organic ultraviolet absorbing agents such as triazine-based ultraviolet absorbing agents, benzotriazole-based ultraviolet absorbing agents, benzophenone-based ultraviolet absorbing agents, oxybenzophenone-based ultraviolet absorbing agents, salicylic acid ester-based ultraviolet absorbing agents, and cyano(meth)acrylate-based ultraviolet absorbing agents, and inorganic ultraviolet absorbing agents such as titanium dioxide, cerium oxide, and zinc oxide. Among these, triazine-based ultraviolet absorbing agents are more preferable.
[0045] Examples of triazine-based ultraviolet absorbers include hydroxyphenyl triazine-based ultraviolet absorbers. Examples of hydroxyphenyl triazine-based ultraviolet absorbers include 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, azine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5[2-(2-ethylhexanoyloxy)ethoxy]phenol.
[0046] The content of the ultraviolet absorber in the first protective layer is, for example, 0.5 parts by mass to 10 parts by mass, alternatively 0.8 parts by mass to 8 parts by mass, or alternatively 1 part by mass to 5 parts by mass, relative to 100 parts by mass of the ionizing radiation curable compound. If the content of the ultraviolet absorber is high, bleeding out of the ultraviolet absorber may occur, whereas if the content of the ultraviolet absorber is low, sufficient ultraviolet absorbing performance may not be obtained.
[0047] The light stabilizer contained in the first protective layer may be, for example, a hindered amine light stabilizer. Examples of the hindered amine light stabilizer include 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, methyl(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, and 2,4-bis[N-butyl-N-(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)amino]-6-(2-hydroxyethylamine)-1,3,5-triazine).
[0048] The content of the light stabilizer in the first protective layer is, for example, 1 part by mass to 10 parts by mass, or may be 1.5 parts by mass to 8 parts by mass, or may be 2 parts by mass to 5 parts by mass, relative to 100 parts by mass of the ionizing radiation curable compound. If the content of the light stabilizer is high, bleeding out of the light stabilizer may occur, and if the content of the light stabilizer is low, sufficient light stability may not be obtained.
[0049] The first protective layer may contain additives such as silicone compounds, polymerization inhibitors, crosslinking agents, antistatic agents, adhesion improvers, antioxidants, leveling agents, thixotropy imparting agents, coupling agents, plasticizers, antifouling agents, defoamers, and fillers. The thickness of the first protective layer is, for example, 2 μm or more and 20 μm or less, 3 μm or more and 15 μm or less, or 4 μm or more and 10 μm or less. If the first protective layer is thin, sufficient weather resistance may not be obtained, and if the first protective layer is thick, cracks may easily occur in the first protective layer, and good adhesion may not be obtained.
[0050] (ii) Second protective layer The transfer layer in the present disclosure preferably has a second protective layer on the side opposite to the release film of the first protective layer. The second protective layer is preferably a layer that is softer than the first protective layer. The second protective layer and the first protective layer may be disposed so as to be in direct contact with each other, or may be disposed via another layer.
[0051] The second protective layer preferably contains a cured product (crosslinked structure) of a curable resin composition as a resin component. The proportion of the cured product of the curable resin composition is, for example, 70% by mass or more, 90% by mass or more, 95% by mass or more, or 100% by mass, based on the total resin components constituting the second protective layer.
[0052] The curable resin composition used in the second protective layer may be, for example, a thermosetting resin composition. The thermosetting resin composition is a composition that contains at least a thermosetting resin, and is a composition that is cured by heating. Examples of the thermosetting resin include (meth)acrylic resins, phenolic resins, urea melamine resins, epoxy resins, unsaturated polyester resins, and silicone resins. The thermosetting resin composition preferably contains a urethane (meth)acrylic resin as the thermosetting resin. The thermosetting resin composition may further contain a curing agent such as an isocyanate curing agent or an epoxy curing agent.
[0053] In addition, when the curable resin composition contains a urethane (meth)acrylic resin, the urethane (meth)acrylic resin is preferably a urethane (meth)acrylic copolymer, more preferably a polycarbonate-based urethane (meth)acrylic copolymer. The polycarbonate-based urethane (meth)acrylic copolymer is a resin obtained by radically polymerizing a (meth)acrylic monomer with a polycarbonate-based polyurethane polymer obtained by reacting a polycarbonate diol with a (di)isocyanate.
[0054] Examples of the (di)isocyanate include aromatic isocyanates such as 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 1,5-naphthalene diisocyanate, n-isocyanate phenylsulfonyl isocyanate, o-isocyanate phenylsulfonyl isocyanate, and p-isocyanate phenylsulfonyl isocyanate; aliphatic isocyanates such as 1,6-hexamethylene diisocyanate; and alicyclic isocyanates such as isophorone diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated diphenylmethane diisocyanate.
[0055] Examples of the (meth)acrylic monomer include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate.
[0056] In the polycarbonate-based urethane (meth)acrylic copolymer, the mass ratio of the urethane component to the total of the (meth)acrylic component and the urethane component ([urethane component] / ([(meth)acrylic component]+[urethane component]) is, for example, 70 mass% or more and 95 mass% or less, alternatively 75 mass% or more and 95 mass% or less, or alternatively 80 mass% or more and 90 mass% or less.
[0057] The second protective layer preferably contains a weathering agent. Examples of weathering agents include ultraviolet absorbers and light stabilizers. The second protective layer preferably contains at least one of an ultraviolet absorber and a light stabilizer. The preferred types and modes of the weathering agent are the same as those described in "(i) First Protective Layer" above, and therefore will not be described here. In particular, the second protective layer preferably contains a triazine-based ultraviolet absorber. The second protective layer preferably contains a hindered amine-based light stabilizer.
[0058] The content of the ultraviolet absorber in the second protective layer is, for example, 0.1 parts by mass or more and 50 parts by mass or less, or may be 3 parts by mass or more and 40 parts by mass or less, or may be 10 parts by mass or more and 35 parts by mass or less, relative to 100 parts by mass of the resin component. The content of the ultraviolet absorber in the second protective layer (content relative to 100 parts by mass of the resin component) may be greater than the content of the ultraviolet absorber in the first protective layer (content relative to 100 parts by mass of the resin component).
[0059] The content of the light stabilizer in the second protective layer is, for example, 0.1 to 15 parts by mass, or 1 to 15 parts by mass, or 3 to 10 parts by mass, relative to 100 parts by mass of the resin component. The content of the light stabilizer in the second protective layer (content relative to 100 parts by mass of the resin component) may be greater than the content of the light stabilizer in the first protective layer (content relative to 100 parts by mass of the resin component).
[0060] The second protective layer may contain additives such as silicone compounds, polymerization inhibitors, crosslinking agents, antistatic agents, adhesion improvers, antioxidants, leveling agents, thixotropy imparting agents, coupling agents, plasticizers, antifouling agents, defoamers, and fillers. The thickness of the second protective layer is, for example, 2 μm to 10 μm, or 3 μm to 8 μm, or 3 μm to 5 μm. If the second protective layer is thin, the adhesion (particularly initial adhesion) with the relatively hard first protective layer may be reduced. On the other hand, if the second protective layer is thick, the movement of the second protective layer due to heat becomes large, and cracks are likely to occur in the first protective layer.
[0061] (2) Other layers The transfer layer in the present disclosure may or may not have a design layer on the side opposite to the release film of the protective layer. By providing a design layer, the design of the article is improved. The design layer and the protective layer may be arranged so as to be in direct contact with each other, or may be arranged via another layer.
[0062] Examples of the design layer include a solid layer (a layer coated with ink) and a pattern layer (a layer printed with ink). The transfer sheet may have a pattern layer and a solid layer in this order from the release film side as the design layer. Examples of the pattern in the pattern layer include wood grain, stone grain, sand grain, tiled pattern, brickwork pattern, cloth grain pattern, leather-squeezed pattern, geometric figures, letters, symbols, abstract patterns, and floral patterns.
[0063] The design layer usually contains a colorant and a binder resin. Examples of the colorant include inorganic pigments such as carbon black (ink), iron black, titanium white, antimony white, yellow lead, titanium yellow, red iron oxide, cadmium red, ultramarine blue, and cobalt blue, organic pigments (including dyes) such as quinacridone red, isoindolinone yellow, nickel azo complex, phthalocyanine blue, and azomethine azo black, metal pigments such as aluminum and brass, and pearl pigments such as titanium dioxide-coated mica and basic lead carbonate.
[0064] Examples of binder resins include urethane-based resins, acrylic polyol-based resins, (meth)acrylic resins, ester-based resins, amide-based resins, butyral-based resins, styrene-based resins, urethane-acrylic copolymers, vinyl chloride-vinyl acetate copolymers, vinyl chloride-vinyl acetate-acrylic copolymers, chlorinated propylene-based resins, nitrocellulose-based resins, and cellulose acetate-based resins.
[0065] The design layer may contain additives such as ultraviolet absorbers, light stabilizers, hardeners, plasticizers, catalysts, etc., as necessary. The thickness of the design layer is, for example, 0.5 μm or more and 20 μm or less, or may be 1 μm or more and 10 μm or less, or may be 2 μm or more and 5 μm or less.
[0066] The transfer layer in the present disclosure may or may not have an adhesive layer on the surface of the protective layer opposite to the release film. The adhesive layer and the protective layer may be arranged so as to be in direct contact with each other, or may be arranged via another layer (e.g., a design layer). The adhesive layer may contain a component having adhesive properties. Examples of the component having adhesive properties include (meth)acrylic resins, vinyl chloride-vinyl acetate copolymers, vinyl acetate resins, ester resins, epoxy resins, imide resins, and rubber resins.
[0067] The adhesive layer may be a so-called pressure-sensitive adhesive layer. The adhesive layer has pressure-sensitive adhesiveness at room temperature. Examples of the resin contained in the adhesive layer include (meth)acrylic resin, vinyl resin, ester resin, urethane resin, amide resin, epoxy resin, rubber resin, and ionomer resin. The adhesive layer may be a so-called heat seal layer. The heat seal layer exhibits pressure-sensitive adhesiveness by heat. Examples of the resin contained in the heat seal layer include (meth)acrylic resin, urethane resin, olefin resin, ester resin, epoxy resin, urea resin, melamine resin, phenol resin, and vinyl resin. The thickness of the adhesive layer is, for example, 1 μm or more and 30 μm or less.
[0068] (3) Transfer layer The thickness of the transfer layer is, for example, 8 μm or more, and may be 10 μm or more, 12 μm or more, or 14 μm or more, while the thickness of the transfer layer is, for example, 50 μm or less, and may be 40 μm or less, or 30 μm or less.
[0069] 3.Release film The transfer sheet in the present disclosure has a release film facing the transfer layer.
[0070] The release film is preferably a resin film. Examples of the resin contained in the resin film include ester resins, olefin resins, styrene resins, vinyl resins, (meth)acrylic resins, amide resins, imide resins, and carbonate resins.
[0071] The release film preferably contains an ester-based resin or an olefin-based resin. Examples of ester-based resins include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), and polyethylene terephthalate-isophthalate copolymers. Among these, PET or PBT is preferred, and PET is more preferred, from the viewpoint of being less susceptible to thermal shrinkage during the production of the transfer sheet and shrinkage due to irradiation with ionizing radiation.
[0072] Examples of olefin resins include polyethylene, polypropylene, polybutene, ethylene-propylene copolymer, and ethylene-propylene-butene copolymer. Among these, polypropylene is preferred from the viewpoint of being less susceptible to thermal shrinkage during the production of the transfer sheet and to shrinkage due to irradiation with ionizing radiation. The release film may be, for example, a paper processed with polypropylene (PP).
[0073] The release film may be a stretched film or an unstretched film. The stretch ratio in the machine direction (MD) of the stretched film is, for example, 5 times or more and 30 times or less. The stretch ratio in the width direction (TD) of the stretched film is, for example, 5 times or more and 30 times or less. The thickness of the release film is, for example, 10 μm or more and 200 μm or less, may be 15 μm or more and 150 μm or less, or may be 20 μm or more and 100 μm or less.
[0074] The release film may contain a matting agent kneaded therein. A part of the kneaded matting agent is usually exposed from the release film. By adding a matting agent to the release film, the peel strength of the release film and the transfer layer can be adjusted. Examples of the matting agent include inorganic particles and organic particles. Examples of the inorganic particles include silica, alumina, calcium carbonate, magnesium carbonate, calcium sulfate, barium sulfate, and kaolin. Examples of the organic particles include acrylic beads, urethane beads, nylon beads, silicone beads, silicone rubber beads, polycarbonate beads, and polyolefin wax (e.g., polypropylene wax, polyethylene wax). The average particle size of the matting agent is, for example, 1.0 μm or more and 10 μm or less, and may be 2.0 μm or more and 8.0 μm or less. The average particle size of the matting agent is determined by the D 50 This refers to.
[0075] The release film may have a mat layer containing a mat agent on the surface on the transfer layer side. The mat agent used in the mat layer is the same as described above. The mat layer may also contain a cured product (crosslinked structure) of a curable resin composition as a resin component. Examples of the curable resin composition used in the mat layer include an ionizing radiation curable resin composition and a thermosetting resin composition. Details of the ionizing radiation curable resin composition and the thermosetting resin composition are the same as described above. The mat layer may also contain a thermoplastic resin as a resin component. The mat layer may contain additives such as a release agent, an ultraviolet absorber, an infrared absorber, a light stabilizer, a polymerization inhibitor, a crosslinking agent, an antistatic agent, an antioxidant, a leveling agent, a coupling agent, a plasticizer, a defoamer, a filler, a thermal radical generator, and an aluminum chelating agent, as necessary. The thickness of the mat layer is not particularly limited, but is, for example, 0.1 μm or more and 10 μm or less.
[0076] 4. Transfer sheet The transfer sheet in the present disclosure has a release film (first release film) and a transfer layer. The transfer sheet may have a second release film on the side of the transfer layer opposite to the release film. For example, when the transfer sheet is wound into a roll to produce it, the occurrence of blocking can be suppressed. Details of the second release film are the same as those described above for the first release film, so the description here is omitted. In addition, the transfer sheet in the present disclosure is preferably used for wrapping processing. Details of the wrapping processing will be described in "B. Method for producing an article" below.
[0077] 5. How to make a transfer sheet The method of producing the transfer sheet in the present disclosure is not particularly limited. For example, when producing the transfer sheet shown in FIG. 1(a), it is preferable to form a first protective layer 2 on one side of a release film 1, and then form a second protective layer 3 on the side of the first protective layer 2 opposite to the release film 1. Also, when producing the transfer sheet shown in FIG. 1(b), it is preferable to form a first protective layer 2 on one side of a release film 1, then form a second protective layer 3 on the side of the first protective layer 2 opposite to the release film 1, and then form a design layer 4 on the side of the second protective layer 3 opposite to the first protective layer 2.
[0078] The method for forming the first protective layer may be, for example, a method of applying a composition for forming the first protective layer to the surface of a release film and curing the composition. The method for applying the composition may be, for example, a gravure printing method, a bar coating method, a roll coating method, a reverse roll coating method, or a comma coating method. The curing method may be, for example, a method of irradiating ionizing radiation such as an electron beam or ultraviolet light.
[0079] The method for forming the second protective layer may, for example, be a method of applying a composition for forming the second protective layer to the surface of the first protective layer opposite to the release film, and curing it as necessary. The method for applying the composition may, for example, be a gravure printing method, a bar coating method, a roll coating method, a reverse roll coating method, or a comma coating method. The curing method may, for example, be heat. The method for forming the design layer may, for example, be a method of applying an ink containing a colorant, a binder resin, and a solvent to the surface of the second protective layer opposite to the first protective layer.
[0080] B. Method of Manufacturing the Article The method for manufacturing an article in the present disclosure includes a preparation step of preparing an adherend having multiple sides and the above-mentioned transfer sheet, and a wrapping step of sequentially bonding the transfer layer of the transfer sheet to the multiple sides of the adherend using a roller.
[0081] 3 is a schematic cross-sectional view illustrating a lapping process in the present disclosure. In FIG. 3, the adherend 20 is wrapped in a wrapping material in the longitudinal direction D L While conveying the adherend 20 along the axis, the transfer layer X of the transfer sheet 10 is sequentially bonded to multiple surfaces of the adherend 20 using multiple rollers 60 (60a to 60e).
[0082] According to the present disclosure, by using the above-mentioned transfer sheet, it is possible to achieve both suppressing floating of the transfer sheet at the corners, suppressing partial peeling of the release film due to springback, and enabling the release film to be easily peeled off from the transfer layer.
[0083] 1. Preparation process The preparation step in the present disclosure is a step of preparing an adherend having multiple surfaces and the above-mentioned transfer sheet. The transfer sheet is the same as that described in "A. Transfer sheet" above, so the description here is omitted.
[0084] An example of the adherend in the present disclosure is a metal member. The metal member and the resin contained in the transfer layer are different materials, so the adhesion between them is likely to be low. In this case, the adhesion between the adherend and the transfer layer can be improved by adhering the adherend and the transfer layer, for example, via an adhesive layer described later. In particular, exterior products (items for outdoor use) are exposed to harsh environments, so it is desirable for the adhesion between the adherend and the transfer layer to be high.
[0085] The metal member is a member containing a simple metal or a metal alloy. Examples of metals used for the metal member include aluminum, iron, steel, and copper. The metal member is preferably an aluminum member. This is because aluminum members are lightweight and have excellent corrosion resistance, and are useful as adherends for exterior products (items for outdoor use). The aluminum member is a member containing aluminum or an aluminum alloy. The aluminum member preferably has an aluminum oxide coating on the surface. This is because the corrosion resistance of the aluminum member is improved. Examples of methods for forming the aluminum oxide coating include anodizing.
[0086] Another example of the adherend is a resin member. Examples of the resin used in the resin member include polycarbonate resin, vinyl chloride resin, acrylic resin, ester resin, styrene resin, olefin resin, acrylonitrile-butadiene-styrene copolymer (ABS resin), phenol resin, cellulose resin, and rubber. Another example of the adherend is a wood member. Examples of the wood member include a wood veneer, wood plywood, particle board, and wood fiber board. Examples of wood used in the wood member include cedar, cypress, pine, and lauan. Another example of the adherend is a ceramic member. The material of the ceramic member may be glass, ceramics, or other ceramics, non-cement ceramic materials such as gypsum, or non-ceramic ceramic materials such as ALC (lightweight aerated concrete).
[0087] The shape of the adherend is not particularly limited, but may be, for example, a plate, a sheet, or a three-dimensional shape. A three-dimensional shape is a three-dimensional shape expressed by the coordinates of the X-axis, the Y-axis, and the Z-axis. The adherend has a plurality of surfaces. The surfaces may be flat or curved.
[0088] 2.Adhesive layer formation process The adhesive layer forming step in the present disclosure is a step of forming an adhesive layer on the surface of the transfer layer opposite to the release film or on the multiple surfaces of the adherend. The method for manufacturing an article in the present disclosure preferably includes an adhesive layer forming step after the preparation step and before the wrapping step described below.
[0089] The adhesive used in the adhesive layer is not particularly limited, and known adhesives can be used. Examples of adhesives include heat-sensitive adhesives and pressure-sensitive adhesives. Examples of resins used in the adhesive include acrylic resins, urethane resins, vinyl chloride resins, vinyl acetate resins, ester resins, amide resins, vinyl chloride-vinyl acetate copolymers, and styrene-acrylic copolymers. In addition, two-liquid curing polyurethane adhesives using an isocyanate compound as a curing agent and polyester adhesives may be used as the adhesive. In addition, the adhesive is preferably a solvent-based adhesive or a polyurethane reactive (PUR) adhesive.
[0090] In the adhesive layer forming step, the adhesive layer coating liquid may be applied to the surface of the transfer sheet opposite to the release film of the transfer layer to form an adhesive layer. In this case, there is an advantage that the adhesive layer coating liquid can be uniformly applied to the transfer sheet. On the other hand, in the adhesive layer forming step, the adhesive layer coating liquid may be applied to multiple surfaces of the adherend to form an adhesive layer. In this case, there is an advantage that the influence of thermal shrinkage of the adhesive is unlikely to occur. The thickness of the adhesive layer is not particularly limited, but may be, for example, 2 μm or more and 100 μm or less, 2 μm or more and 50 μm or less, or 2 μm or more and 35 μm or less. For example, when the transfer sheet has the above-mentioned adhesive layer, the adhesive layer forming step may not be performed.
[0091] 3. Wrapping process The wrapping process in the present disclosure is a process of sequentially laminating the transfer layer of the transfer sheet to the multiple surfaces of the adherend using a roller. "Sequential lamination" refers to laminating a transfer sheet to one surface of the adherend, and then laminating a transfer sheet to a surface adjacent to the surface to which the transfer sheet was laminated. Usually, the operation of laminating a transfer sheet to a surface adjacent to the surface to which the transfer sheet was laminated is repeated. For example, a transfer sheet is laminated to a first surface of the adherend, then a transfer sheet is laminated to a second surface adjacent to the first surface, and then a transfer sheet is laminated to a third surface adjacent to the second surface.
[0092] The multiple surfaces of the adherend are preferably surfaces extending in the longitudinal direction of the adherend. In the lapping process, a single roller may be used to sequentially attach the transfer sheet to the multiple surfaces of the adherend, or multiple rollers may be used to sequentially attach the transfer sheet to the multiple surfaces of the adherend. In the lapping process, it is preferable to fix the position of the roller and transport the adherend and the transfer sheet.
[0093] As shown in FIG. 3, in the lapping process, the adherend 20 is wrapped in a wrapping paper in the longitudinal direction D L It is preferable to sequentially laminate the transfer layer X of the transfer sheet 10 to multiple surfaces of the adherend 20 using multiple rollers 60 (60a to 60e) while conveying the adherend 20 along the track. In the wrapping process, the transfer layer X of the transfer sheet 10 is laminated to one surface of the adherend 20 using the rollers 60, and then the transfer layer X of the transfer sheet 10 is laminated to the other surface of the adherend 20 using the rollers 60 successively.
[0094] As shown in Fig. 4(a), the first roller 60a is pressed against the first surface S1 of the adherend 20 via the transfer sheet 10. This causes the transfer sheet 10 (transfer layer X) to be attached to the first surface S1 of the adherend 20. Although not shown in particular, it is preferable that the above-mentioned adhesive layer is formed between the adherend and the transfer sheet (transfer layer). In Fig. 4(a), the axial direction A1 of the first roller 60a is horizontal.
[0095] Next, as shown in Fig. 4(b), the transfer sheet 10 is guided so as to be folded by the first guide rollers 60b, 60b', and then, as shown in Fig. 4(c), the second rollers 60c, 60c' are pressed against the second surfaces S2, S2' of the adherend 20 via the transfer sheet 10, respectively. This causes the transfer sheet 10 (transfer layer X) to be attached to the second surfaces S2, S2' of the adherend 20. In Fig. 4(c), the axial directions A2, A2' of the second rollers 60c, 60c' are vertical.
[0096] Next, as shown in Fig. 4(d), the transfer sheet 10 is guided to be folded by the second guide roller 60d, and then, as shown in Fig. 4(e), the third roller 60e is pressed against the third surface S3 of the adherend 20 via the transfer sheet 10. This causes the transfer sheet 10 (transfer layer X) to be attached to the third surface S3 of the adherend 20. In Fig. 4(e), the axial direction A3 of the third roller 60e is horizontal.
[0097] As shown in FIG. 5, the angle between the axial direction A1 of the first roller and the axial direction A2 of the second roller is defined as θ 12 The axial direction A1 of the first roller to the axial direction A of the first guide roller M The angle to 1M The above angle (central angle) is an angle in the same circumferential direction. 12 and θ 1M θ 12 >θ 1MIt is preferable that the above condition is satisfied. By gradually changing the axial direction of each roller along the longitudinal direction of the adherend 20, it is possible to further suppress the occurrence of cracks in the transfer layer when the transfer layer is transferred to the adherend.
[0098] As shown in FIG. 5, the angle between the axial direction A2 of the second roller and the axial direction A3 of the third roller is defined as θ 23 The axial direction A from the axial direction A2 of the second roller to the axial direction A of the second guide roller N The angle to 2N The above angle (central angle) is an angle in the same circumferential direction. 23 and θ 2N θ 23 >θ 2N It is preferable that the above condition is satisfied. By gradually changing the axial direction of each roller along the longitudinal direction of the adherend 20, it is possible to further suppress the occurrence of cracks in the transfer layer when the transfer layer is transferred to the adherend.
[0099] In the wrapping process, a heated roller may be used. The heating temperature of the roller is, for example, 200°C or less, and may be 180°C or less. If the heating temperature is high, the transfer sheet may be softened more than necessary. On the other hand, the heating temperature of the roller is, for example, 100°C or more, and may be 110°C or more, or may be 120°C or more.
[0100] Fig. 6(a) is a schematic cross-sectional view illustrating a part of an article with a release film in the present disclosure, which corresponds to region α in Fig. 4(e). As shown in Fig. 6(a), an article with a release film 50 having at least a transfer sheet 10 and an adherend 20 is obtained by a wrapping process. The article with a release film 50 shown in Fig. 6(a) has an adhesive layer 30 between the transfer sheet 10 and the adherend 20. The article with a release film 50 shown in Fig. 6(a) has the release film 1, the transfer layer X, the adhesive layer 30 and the adherend 20 arranged in a thickness direction D. T In this order,
[0101] The method for manufacturing an article according to the present disclosure may include a peeling step of peeling the release film from the transfer layer after the wrapping step. As shown in FIG. 6(b), the peeling step provides an article 100 having at least the transfer layer X and the adherend 20. The article 100 shown in FIG. 6(b) also has an adhesive layer 30 between the transfer layer X and the adherend 20. The article 100 shown in FIG. 6(b) also has the transfer layer X, the adhesive layer 30, and the adherend 20 arranged in a thickness direction D. T In this order,
[0102] 3.Goods The article in the present disclosure has an adherend having a plurality of surfaces and a transfer layer disposed so as to follow the plurality of surfaces. An adhesive layer may be disposed between the adherend and the transfer layer. The article in the present disclosure is used, for example, as a building material. The building material is used, for example, in buildings such as houses, offices, stores, hospitals, and clinics. The article may be an exterior product (an article for outdoor use) or an interior product (an article for indoor use). Specific examples of the article include exterior walls, roofs, eaves ceilings, louvers, door pockets, window frames, doors, door frames, handrails, fences, and drying racks.
[0103] C. Items with release film The article with a release film in the present disclosure has an adherend having a plurality of surfaces, a transfer layer arranged so as to conform to the plurality of surfaces, and a release film arranged so as to conform to the transfer layer, wherein the loop stiffness of the release film is 0.18 N / 15 mm or less, the peel strength of the release film and the transfer layer is 0.7 N / 25 mm or less, and when the loop stiffness is X and the peel strength is Y, X and Y satisfy Y≧0.67X+0.17.
[0104] According to the present disclosure, the loop stiffness and the peel strength are each within a specific range, and further, the loop stiffness and the peel strength satisfy a specific relationship, thereby suppressing lifting of the transfer sheet at the corners, suppressing partial peeling of the release film due to springback, and enabling the release film to be satisfactorily peeled off from the transfer layer, resulting in an article with a release film that is compatible with the above. The article with a release film in the present disclosure is the same as that described in "B. Method for manufacturing an article" above, so the description here is omitted.
[0105] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES
[0106] [Example 1] As a release film, a polyethylene terephthalate film (kneaded matte, thickness: 26 μm) that was not subjected to easy-adhesion treatment and had a matting agent kneaded into it was prepared. The composition for forming the first protective layer described below was applied to one side of the release film by gravure coating to form an uncured resin layer. Thereafter, the composition was irradiated with 50 kGy of electron beams at an acceleration voltage of 165 kV to cure the composition, thereby forming a first protective layer having a thickness of 5 μm. Thereafter, corona irradiation was performed on the side of the first protective layer opposite to the release film. <Composition for forming first protective layer (EB1)> ·Ionizing radiation curable resin composition: 100 parts by mass Caprolactam-based urethane acrylate: 30 parts by weight Pentaerythritol triacrylate (hydroxyl group-containing acrylate): 70 parts by mass UV absorber: 2 parts by weight (product name: TINUVIN479, BASF) Light stabilizer with reactive functional groups: 2 parts by weight (product name: Sanol LS-3410, Nippon Nyukazai Co., Ltd.)
[0107] Next, the composition for forming the second protective layer described below was applied by gravure coating onto the corona-irradiated surface of the first protective layer, and dried to form a second protective layer having a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by weight UV absorber: 17 parts by weight (product name: TINUVIN400, BASF) UV absorber: 13 parts by weight (product name: TINUVIN479, BASF) Hindered amine light stabilizer: 8 parts by weight (product name: TINUVIN123, BASF) Anti-blocking agent: 9 parts by weight (silica particles, average particle size 3 μm) Hardener: 25 parts by weight (hexamethylene diisocyanate)
[0108] Next, the ink for forming the design layer described below was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in that order in the thickness direction. <Ink for forming design layer> ·Resin composition: 100 parts by mass Acrylic resin: 80 parts by weight Vinyl chloride-vinyl acetate copolymer: 20 parts by weight Pigments
[0109] [Example 2] As a release film, a mirror-finished polyethylene terephthalate film (thickness: 38 μm) that had not been subjected to an easy-adhesion treatment was prepared. The composition for forming the first protective layer described below was applied to one side of the release film by gravure coating to form an uncured resin layer. Then, the composition was irradiated with 50 kGy of electron beams at an acceleration voltage of 165 kV to cure the composition, thereby forming a first protective layer having a thickness of 5 μm. Then, the surface of the first protective layer opposite to the release film was irradiated with corona radiation. <Composition for forming first protective layer (EB2)> ·Ionizing radiation curable resin composition: 100 parts by mass Caprolactam-based urethane acrylate: 50 parts by weight Pentaerythritol triacrylate (hydroxyl group-containing acrylate): 50 parts by mass UV absorber: 2 parts by weight (product name: TINUVIN479, BASF) Light stabilizer with reactive functional groups: 2 parts by weight (product name: Sanol LS-3410, Nippon Nyukazai Co., Ltd.)
[0110] Next, the composition for forming the second protective layer described below was applied by gravure coating onto the corona-irradiated surface of the first protective layer, and dried to form a second protective layer having a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by weight UV absorber: 17 parts by weight (product name: TINUVIN400, BASF) UV absorber: 13 parts by weight (product name: TINUVIN479, BASF) Hindered amine light stabilizer: 8 parts by weight (product name: TINUVIN123, BASF) Anti-blocking agent: 9 parts by weight (silica particles, average particle size 3 μm) Hardener: 25 parts by weight (hexamethylene diisocyanate)
[0111] Next, the ink for forming the design layer described below was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in that order in the thickness direction. <Ink for forming design layer> ·Resin composition: 100 parts by mass Acrylic resin: 80 parts by weight Vinyl chloride-vinyl acetate copolymer: 20 parts by weight Pigments
[0112] [Example 3] A polyethylene terephthalate film (matte coat, thickness: 50 μm) having a matte layer containing a matting agent was prepared as a release film. The composition for forming the first protective layer described below was applied by gravure coating to the surface of the release film on the matte layer side to form an uncured resin layer. Then, the composition was irradiated with 50 kGy of electron beams at an acceleration voltage of 165 kV to cure the composition, thereby forming a first protective layer having a thickness of 5 μm. Then, the surface of the first protective layer opposite to the release film was irradiated with corona radiation. <Composition for forming first protective layer (EB1)> ·Ionizing radiation curable resin composition: 100 parts by mass Caprolactam-based urethane acrylate: 30 parts by weight Pentaerythritol triacrylate (hydroxyl group-containing acrylate): 70 parts by mass UV absorber: 2 parts by weight (product name: TINUVIN479, BASF) Light stabilizer with reactive functional groups: 2 parts by weight (product name: Sanol LS-3410, Nippon Nyukazai Co., Ltd.)
[0113] Next, the composition for forming the second protective layer described below was applied by gravure coating onto the corona-irradiated surface of the first protective layer, and dried to form a second protective layer having a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by weight UV absorber: 17 parts by weight (product name: TINUVIN400, BASF) UV absorber: 13 parts by weight (product name: TINUVIN479, BASF) Hindered amine light stabilizer: 8 parts by weight (product name: TINUVIN123, BASF) Anti-blocking agent: 9 parts by weight (silica particles, average particle size 3 μm) Hardener: 25 parts by weight (hexamethylene diisocyanate)
[0114] Next, the ink for forming the design layer described below was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in that order in the thickness direction. <Ink for forming design layer> ·Resin composition: 100 parts by mass Acrylic resin: 80 parts by weight Vinyl chloride-vinyl acetate copolymer: 20 parts by weight Pigments
[0115] [Example 4] As a release film, a polyethylene terephthalate film (kneaded matte, thickness: 50 μm) that was not subjected to easy-adhesion treatment and had a matting agent kneaded into it was prepared. The composition for forming the first protective layer described below was applied to one side of the release film by gravure coating to form an uncured resin layer. Then, the composition was irradiated with 50 kGy of electron beams at an acceleration voltage of 165 kV to cure the composition, thereby forming a first protective layer having a thickness of 5 μm. Then, corona irradiation was performed on the side of the first protective layer opposite to the release film. <Composition for forming first protective layer (EB3)> Ionizing radiation curable resin composition (caprolactone-based urethane acrylate): 100 parts by mass UV absorber: 2 parts by weight (product name: TINUVIN479, BASF) Light stabilizer with reactive functional groups: 2 parts by weight (product name: Sanol LS-3410, Nippon Nyukazai Co., Ltd.)
[0116] Next, the composition for forming the second protective layer described below was applied by gravure coating onto the corona-irradiated surface of the first protective layer, and dried to form a second protective layer having a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by weight UV absorber: 17 parts by weight (product name: TINUVIN400, BASF) UV absorber: 13 parts by weight (product name: TINUVIN479, BASF) Hindered amine light stabilizer: 8 parts by weight (product name: TINUVIN123, BASF) Anti-blocking agent: 9 parts by weight (silica particles, average particle size 3 μm) Hardener: 25 parts by weight (hexamethylene diisocyanate)
[0117] Next, the ink for forming the design layer described below was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in that order in the thickness direction. <Ink for forming design layer> ·Resin composition: 100 parts by mass Acrylic resin: 80 parts by weight Vinyl chloride-vinyl acetate copolymer: 20 parts by weight Pigments
[0118] [Example 5] A transfer paper (matte PP, thickness: 75 μm) having a matte polypropylene (PP) layer was prepared as a release film. The composition for forming the first protective layer described below was applied by gravure coating to the surface of the release film facing the PP layer to form an uncured resin layer. Then, the composition was irradiated with 50 kGy of electron beams at an acceleration voltage of 165 kV to cure the composition, thereby forming a first protective layer having a thickness of 5 μm. Then, the surface of the first protective layer opposite to the release film was irradiated with corona radiation. <Composition for forming first protective layer (EB3)> Ionizing radiation curable resin composition (caprolactone-based urethane acrylate): 100 parts by mass UV absorber: 2 parts by weight (product name: TINUVIN479, BASF) Light stabilizer with reactive functional groups: 2 parts by weight (product name: Sanol LS-3410, Nippon Nyukazai Co., Ltd.)
[0119] Next, the composition for forming the second protective layer described below was applied by gravure coating onto the corona-irradiated surface of the first protective layer, and dried to form a second protective layer having a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by weight UV absorber: 17 parts by weight (product name: TINUVIN400, BASF) UV absorber: 13 parts by weight (product name: TINUVIN479, BASF) Hindered amine light stabilizer: 8 parts by weight (product name: TINUVIN123, BASF) Anti-blocking agent: 9 parts by weight (silica particles, average particle size 3 μm) Hardener: 25 parts by weight (hexamethylene diisocyanate)
[0120] Next, the ink for forming the design layer described below was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in that order in the thickness direction. <Ink for forming design layer> ·Resin composition: 100 parts by mass Acrylic resin: 80 parts by weight Vinyl chloride-vinyl acetate copolymer: 20 parts by weight Pigments
[0121] [Comparative Example 1] As a release film, a polyethylene terephthalate film (kneaded matte, thickness: 50 μm) that was not subjected to easy-adhesion treatment and had a matting agent kneaded into it was prepared. The composition for forming the first protective layer described below was applied to one side of the release film by gravure coating to form an uncured resin layer. Then, the composition was irradiated with 50 kGy of electron beams at an acceleration voltage of 165 kV to cure the composition, thereby forming a first protective layer having a thickness of 5 μm. Then, corona irradiation was performed on the side of the first protective layer opposite to the release film. <Composition for forming first protective layer (EB1)> ·Ionizing radiation curable resin composition: 100 parts by mass Caprolactam-based urethane acrylate: 30 parts by weight Pentaerythritol triacrylate (hydroxyl group-containing acrylate): 70 parts by mass UV absorber: 2 parts by weight (product name: TINUVIN479, BASF) Light stabilizer with reactive functional groups: 2 parts by weight (product name: Sanol LS-3410, Nippon Nyukazai Co., Ltd.)
[0122] Next, the composition for forming the second protective layer described below was applied by gravure coating onto the corona-irradiated surface of the first protective layer, and dried to form a second protective layer having a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by weight UV absorber: 17 parts by weight (product name: TINUVIN400, BASF) UV absorber: 13 parts by weight (product name: TINUVIN479, BASF) Hindered amine light stabilizer: 8 parts by weight (product name: TINUVIN123, BASF) Anti-blocking agent: 9 parts by weight (silica particles, average particle size 3 μm) Hardener: 25 parts by weight (hexamethylene diisocyanate)
[0123] Next, the ink for forming the design layer described below was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in that order in the thickness direction. <Ink for forming design layer> ·Resin composition: 100 parts by mass Acrylic resin: 80 parts by weight Vinyl chloride-vinyl acetate copolymer: 20 parts by weight Pigments
[0124] [Comparative Example 2] As a release film, a mirror-finished polyethylene terephthalate film (thickness: 50 μm) that had not been subjected to an easy-adhesion treatment was prepared. The composition for forming the first protective layer described below was applied to one side of the release film by gravure coating to form an uncured resin layer. Then, the composition was irradiated with 50 kGy of electron beams at an acceleration voltage of 165 kV to cure the composition, thereby forming a first protective layer having a thickness of 5 μm. Then, the surface of the first protective layer opposite to the release film was irradiated with corona radiation. <Composition for forming first protective layer (EB1)> ·Ionizing radiation curable resin composition: 100 parts by mass Caprolactam-based urethane acrylate: 30 parts by weight Pentaerythritol triacrylate (hydroxyl group-containing acrylate): 70 parts by mass UV absorber: 2 parts by weight (product name: TINUVIN479, BASF) Light stabilizer with reactive functional groups: 2 parts by weight (product name: Sanol LS-3410, Nippon Nyukazai Co., Ltd.)
[0125] Next, the composition for forming the second protective layer described below was applied by gravure coating onto the corona-irradiated surface of the first protective layer, and dried to form a second protective layer having a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by weight UV absorber: 17 parts by weight (product name: TINUVIN400, BASF) UV absorber: 13 parts by weight (product name: TINUVIN479, BASF) Hindered amine light stabilizer: 8 parts by weight (product name: TINUVIN123, BASF) Anti-blocking agent: 9 parts by weight (silica particles, average particle size 3 μm) Hardener: 25 parts by weight (hexamethylene diisocyanate)
[0126] Next, the ink for forming the design layer described below was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in that order in the thickness direction. <Ink for forming design layer> ·Resin composition: 100 parts by mass Acrylic resin: 80 parts by weight Vinyl chloride-vinyl acetate copolymer: 20 parts by weight Pigments
[0127] [Comparative Example 3] As a release film, a mirror-finished polyethylene terephthalate film (thickness: 75 μm) that had not been subjected to easy-adhesion treatment was prepared. The composition for forming the first protective layer described below was applied to one side of the release film by gravure coating to form an uncured resin layer. Then, the composition was irradiated with 50 kGy of electron beams at an acceleration voltage of 165 kV to cure the composition, thereby forming a first protective layer having a thickness of 5 μm. Then, the surface of the first protective layer opposite to the release film was irradiated with corona radiation. <Composition for forming first protective layer (EB3)> Ionizing radiation curable resin composition (caprolactone-based urethane acrylate): 100 parts by mass UV absorber: 2 parts by weight (product name: TINUVIN479, BASF) Light stabilizer with reactive functional groups: 2 parts by weight (product name: Sanol LS-3410, Nippon Nyukazai Co., Ltd.)
[0128] Next, the composition for forming the second protective layer described below was applied by gravure coating onto the corona-irradiated surface of the first protective layer, and dried to form a second protective layer having a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by weight UV absorber: 17 parts by weight (product name: TINUVIN400, BASF) UV absorber: 13 parts by weight (product name: TINUVIN479, BASF) Hindered amine light stabilizer: 8 parts by weight (product name: TINUVIN123, BASF) Anti-blocking agent: 9 parts by weight (silica particles, average particle size 3 μm) Hardener: 25 parts by weight (hexamethylene diisocyanate)
[0129] Next, the ink for forming the design layer described below was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in that order in the thickness direction. <Ink for forming design layer> ·Resin composition: 100 parts by mass Acrylic resin: 80 parts by weight Vinyl chloride-vinyl acetate copolymer: 20 parts by weight Pigments
[0130] [Comparative Example 4] A polyethylene terephthalate film (matte coat, thickness: 38 μm) having a matte layer containing a matting agent was prepared as a release film. The composition for forming the first protective layer described below was applied to one side of the release film by gravure coating to form an uncured resin layer. Then, the composition was irradiated with 50 kGy of electron beams at an acceleration voltage of 165 kV to cure the composition, thereby forming a first protective layer having a thickness of 5 μm. Then, the surface of the first protective layer opposite to the release film was irradiated with corona radiation. <Composition for forming first protective layer (EB1)> ·Ionizing radiation curable resin composition: 100 parts by mass Caprolactam-based urethane acrylate: 30 parts by weight Pentaerythritol triacrylate (hydroxyl group-containing acrylate): 70 parts by mass UV absorber: 2 parts by weight (product name: TINUVIN479, BASF) Light stabilizer with reactive functional groups: 2 parts by weight (product name: Sanol LS-3410, Nippon Nyukazai Co., Ltd.)
[0131] Next, the composition for forming the second protective layer described below was applied by gravure coating onto the corona-irradiated surface of the first protective layer, and dried to form a second protective layer having a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by weight UV absorber: 17 parts by weight (product name: TINUVIN400, BASF) UV absorber: 13 parts by weight (product name: TINUVIN479, BASF) Hindered amine light stabilizer: 8 parts by weight (product name: TINUVIN123, BASF) Anti-blocking agent: 9 parts by weight (silica particles, average particle size 3 μm) Hardener: 25 parts by weight (hexamethylene diisocyanate)
[0132] Next, the ink for forming the design layer described below was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in that order in the thickness direction. <Ink for forming design layer> ·Resin composition: 100 parts by mass Acrylic resin: 80 parts by weight Vinyl chloride-vinyl acetate copolymer: 20 parts by weight Pigments
[0133] [evaluation] (Loop stiffness measurement) The loop stiffness of the release film in the transfer sheet obtained in each example and each comparative example was measured. First, the transfer layer was peeled off from the transfer sheet to leave only the release film. Next, the release film was cut into a strip of 15 mm width and 150 mm length to prepare a sample. Next, the sample was fixed to a "loop stiffness tester (model: DR)" manufactured by Toyo Seiki so that the loop length was 60 mm, and a pressure tool was pressed against it from the vertical direction to measure the stress during compression, and the maximum value of the stress was obtained as the loop stiffness (RS).
[0134] (Peel strength measurement) The peel strength of the transfer sheet obtained in each Example and Comparative Example was measured. First, the transfer sheet was cut to a width of 25 mm, and a double-sided tape was attached to the entire surface of the release film opposite to the transfer layer, and the release film was fixed to a metal plate with a width of 25 mm. Next, a 25 mm wide cellophane tape (registered trademark) made by Nichiban was attached to the entire surface of the transfer layer opposite to the release film. Next, the peel strength was measured using "Tensilon RTG1250" made by A&D Co., Ltd. under the conditions of a peel speed of 200 mm / min and a peel angle of 90°. After exceeding the upper yield point, the integral average value of the peel strength from the point where the lower yield point load was reached to 20 mm was taken, and the peel strength (N / 25 mm) was calculated. The results are shown in Table 1.
[0135] (corner lift, spring back, release film peelability) The transfer sheets obtained in each Example and Comparative Example were evaluated for corner lifting (lifting of the transfer sheet at the corner), springback (partial peeling of the release film due to springback), and release film releasability (release film releasability after the transfer sheet is attached to the adherend). First, an aluminum substrate (adherend) having a cross section of 40 mm x 40 mm and a length of 2 m was prepared. Next, an adhesive was applied to the transfer layer of the transfer sheet (YR117-1, thickness 50 μm, manufactured by Showa Denko Material), and the transfer sheet was attached to the aluminum substrate using a wrapping machine. Next, the corner lifting, springback, and release film releasability were evaluated according to the following criteria. <Corner floating> A: The transfer sheet fitted perfectly to the corners. B: The transfer sheet was slightly raised from the corners, but this was not a problem for use. C: The transfer sheet has come loose from the corner. <Springback> A: The release film did not float off the transfer layer and fitted well. B: The release film was slightly raised from the edge of the transfer sheet, but was at a level that did not cause any problems in use. C: A large portion of the release film peeled off from the edge of the transfer sheet. <Release film releasability> A: The release film was easily peeled off. B: Some force was required for peeling, but the release film was peeled off without remaining on the transfer layer. C: The release film could not be peeled off from the transfer layer and was damaged.
[0136] [Table 1]
[0137] [Table 2]
[0138] As shown in Tables 1 and 2, in Examples 1 to 5, the corner lift, spring back, and release film releasability were all good. In contrast, in Comparative Examples 1 to 4, any of the corner lift, spring back, and release film releasability was insufficient. FIG. 7 shows the relationship between loop stiffness and peel strength in Examples 1 to 5 and Comparative Examples 1 to 3. Note that Comparative Example 4 is not shown in FIG. 7 because its peel strength was too high.
[0139] As shown in FIG. 7, it was confirmed that springback can be suppressed well when Y≧0.67X+0.17 is satisfied, where X is loop stiffness and Y is peel strength. Comparative Example 3 can suppress springback well, and the straight line connecting Comparative Example 3 and Example 1 is Y=0.67X+0.19 (Straight Line 1). On the other hand, the straight line with a slope of 0.67 and passing through Comparative Example 1 is Y=0.67X+0.14 (Straight Line 2). It is presumed that springback can be suppressed well if Y≧0.67X+0.17 is within the range with Y=0.67X+0.17 located midway between Straight Lines 1 and 2 as the boundary. In addition, the straight line connecting Example 1 and Example 5 was Y=2.25X+0.12. In addition, the straight line connecting Example 1 and Example 4 was Y=2.99X+0.03. Furthermore, as shown in FIG. 7, it was suggested that when the loop stiffness X exceeds 0.18 N / 15 mm, corner lifting is likely to occur, and when the peel strength Y exceeds 0.7 N / 25 mm, the peelability decreases.
[0140] Thus, in the present disclosure, for example, the following inventions are provided:
[0141] [1] A transfer sheet, The transfer sheet has a release film and a transfer layer disposed on one surface of the release film, The loop stiffness of the release film is 0.18N / 15mm or less, The peel strength of the release film and the transfer layer is 0.7 N / 25 mm or less; A transfer sheet, in which, when the loop stiffness is X and the peel strength is Y, the above X and Y satisfy Y≧0.67X+0.17.
[0142] [2] The transfer sheet described in [1] is used for wrapping processing.
[0143] [3] The transfer sheet according to [1] or [2], wherein the transfer layer has a first protective layer and a second protective layer in this order in the thickness direction from the release film side.
[0144] [4] The transfer sheet according to [3], wherein the first protective layer contains a cured product of an ionizing radiation curable resin composition.
[0145] [5] The transfer sheet according to [3] or [4], wherein the second protective layer contains a cured product of a thermosetting resin composition.
[0146] [6] The transfer sheet according to any one of [3] to [5], wherein the first protective layer contains at least one of an ultraviolet absorber and a light stabilizer.
[0147] [7] The transfer sheet according to any one of [3] to [6], wherein the second protective layer contains at least one of an ultraviolet absorber and a light stabilizer.
[0148] [8] A transfer sheet described in any of [3] to [7], wherein the transfer layer has a design layer on the side of the second protective layer opposite the first protective layer.
[0149] [9] The transfer sheet is a transfer sheet described in any one of [1] to [8], which is used in the manufacture of exterior products.
[0150]
[10] A preparation step of preparing an adherend having a plurality of surfaces and a transfer sheet according to any one of [1] to [9]; a lapping process step of sequentially laminating the transfer layer of the transfer sheet to the multiple surfaces of the adherend using a roller; The method for manufacturing an article comprising the steps of:
[0151]
[11] The method for manufacturing the article described in
[10] includes, after the preparation step and before the wrapping step, an adhesive layer formation step of forming an adhesive layer on the surface of the transfer layer opposite the release film, or on the multiple surfaces of the adherend.
[0152]
[12] The adhesive tape has an adherend having a plurality of surfaces, a transfer layer disposed so as to conform to the plurality of surfaces, and a release film disposed so as to conform to the transfer layer, The loop stiffness of the release film is 0.18N / 15mm or less, The peel strength of the release film and the transfer layer is 0.7 N / 25 mm or less; An article with a release film, wherein, when the loop stiffness is X and the peel strength is Y, the above X and Y satisfy Y≧0.67X+0.17.
[0153]
[13] The article with a release film according to
[12] , wherein the article with a release film has an adhesive layer between the transfer layer and the adherend. [Explanation of symbols]
[0154] 1 ... Release film 2 … 1st protective layer 3…Second protective layer 4 … Design layer 10 ... Transfer sheet 20 … Adherent 50 ... Items with release film 100 … Goods
Claims
1. A transfer sheet, The transfer sheet has a release film and a transfer layer disposed on one surface of the release film, The loop stiffness of the release film is 0.18 N / 15 mm or less, The peel strength between the release film and the transfer layer is 0.7 N / 25 mm or less; A transfer sheet, in which, when the loop stiffness is X and the peel strength is Y, the X and Y satisfy Y≧0.67X+0.
17.
2. The transfer sheet according to claim 1 , which is used in a wrapping process.
3. The transfer sheet according to claim 1 , wherein the transfer layer has a first protective layer and a second protective layer in this order in the thickness direction from the release film side.
4. The transfer sheet according to claim 3 , wherein the first protective layer comprises a cured product of an ionizing radiation curable resin composition.
5. The transfer sheet according to claim 3 , wherein the second protective layer comprises a cured product of a thermosetting resin composition.
6. The transfer sheet according to claim 3 , wherein the first protective layer contains at least one of an ultraviolet absorbing agent and a light stabilizer.
7. The transfer sheet according to claim 3 , wherein the second protective layer contains at least one of an ultraviolet absorbing agent and a light stabilizer.
8. The transfer sheet according to claim 3 , wherein the transfer layer has a design layer on a surface of the second protective layer opposite to the first protective layer.
9. The transfer sheet of claim 1 , wherein the transfer sheet is used in the manufacture of exterior products.
10. A preparation step of preparing an adherend having a plurality of surfaces and a transfer sheet according to any one of claims 1 to 9; a lapping process step of sequentially laminating the transfer layer of the transfer sheet to the multiple surfaces of the adherend using a roller; The method for manufacturing an article comprising the steps of:
11. The method for manufacturing an article according to claim 10, further comprising, after the preparation step and before the wrapping step, an adhesive layer formation step of forming an adhesive layer on the surface of the transfer layer opposite the release film or on the multiple surfaces of the adherend.
12. The method comprises: an adherend having a plurality of surfaces; a transfer layer disposed so as to conform to the plurality of surfaces; and a release film disposed so as to conform to the transfer layer; The loop stiffness of the release film is 0.18 N / 15 mm or less, The peel strength between the release film and the transfer layer is 0.7 N / 25 mm or less; An article with a release film, wherein, when the loop stiffness is X and the peel strength is Y, the X and Y satisfy Y≧0.67X+0.
17.
13. The article with a release film according to claim 12, further comprising an adhesive layer between the transfer layer and the adherend.
Citation Information
Patent Citations
Decorative sheet
JP2012040815A
Three-dimensional molding film and resin molding
JP2019064027A
Transfer sheet
JP2019081335A
Laminate and resin film
JP2019181949A
Transfer sheet, decorative molding and method for manufacturing decorative molding
JP2022155130A