Ionic type conjugated microporous polymer nano-channel composite membrane as well as preparation method and application thereof

Through the combination of ionic conjugated microporous polymers and macroporous structural membrane materials, the problem of insufficient selectivity of polymer membranes in permeability energy conversion is solved, efficient salinity gradient energy conversion is achieved, and a green and environmentally friendly High performance solution.

CN118756155AActive Publication Date: 2024-10-11NANJING NORMAL UNIVERSITY

Patent Information

Application Number
CN202410765176.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-11
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

Existing polymer membranes have insufficient ion selectivity in permeability energy conversion and complex preparation processes, which limits their applications. In particular, neutral nanopore framework materials lack charge separation capabilities, making it difficult to improve selectivity without sacrificing permeability. .

Method used

Ionic conjugated microporous polymers (i-CMPs) are synthesized through electrochemical polymerization technology, and combined with membrane materials with macroporous structures, such as anodized aluminum membranes, to form an ultrathin composite membrane with charged sub-nanometer pores to achieve selectivity. Ion transport and good penetration properties.

Benefits of technology

It achieves high performance and stable ion selectivity and permeability in salinity gradient energy conversion. The maximum output power density reaches 105W/m2 with almost no attenuation within 10 days, providing a green, environmentally friendly and efficient solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756155A_ABST
    Figure CN118756155A_ABST
Patent Text Reader

Abstract

The invention discloses an ionic type conjugated microporous polymer nano-channel composite membrane and preparation and application thereof, the composite membrane comprises a layer of ionic type conjugated microporous polymer membrane and a layer of membrane material with a macroporous structure, the ionic type conjugated microporous polymer membrane has ultra-thin membrane thickness and regular charged sub-nano channels, the ionic conjugated microporous polymer membrane has good ion permeability and good ion selectivity, and part of pores of the ionic conjugated microporous polymer membrane are correspondingly communicated with part of macropores in the membrane material with the macropore structure. The composite membrane is prepared by taking a membrane material with a macroporous structure as a substrate through electrochemical in-situ polymerization. The salinity gradient energy output power density of the composite membrane can reach 18W / m < 2 > or above. The method is simple and convenient to operate and easy to control, required equipment is simple, large-scale production can be realized, and the method has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an ionic conjugated microporous polymer nanochannel composite membrane and preparation and application thereof, belonging to the field of nanochannel composite membranes. Background Art

[0002] Osmotic energy or salinity gradient energy, also known as "blue energy", is considered a promising renewable energy source due to its abundant reserves and wide distribution, providing an attractive solution to get rid of dependence on fossil fuels and meet the growing energy demand. In the past few decades, membrane-based reverse electrodialysis (RED) has developed into a promising technology to capture this blue energy from natural water. In RED systems, preferential counter-ion diffusion through ion exchange membranes is crucial for osmotic energy conversion, but its performance is often limited by the trade-off between permeability and selectivity. In the past few years, a lot of research has been done on emerging crystalline porous materials such as metal organic frameworks (MOFs), covalent organic frameworks (COFs), MXenes, and graphene oxide (GO) as ion conductive materials. These membranes show excellent ion selectivity due to their highly uniform pore size, but processability remains a major challenge. In recent years, a variety of polymer membranes with dense structures and small channel pore sizes have been developed for selective ion transport. These polymer membranes show high ion selectivity due to size screening and electrostatic interactions. However, the long and discontinuous channels formed by the self-assembly of flexible segments largely hinder the transport of ions. Unfortunately, the osmotic energy conversion performance of the polymer membranes reported so far is still unsatisfactory, mainly because of the insufficient ion permeation selectivity, which increases the Gibbs free energy dissipated by the RED system in the form of Joule heat, and the complex preparation process also greatly limits its application. Therefore, porous membranes with adjustable pore structures and designable channel surfaces are a promising platform for the production of advanced membranes.

[0003] Conjugated microporous polymers (CMPs) are emerging porous organic materials with advantages such as high specific surface area, permanent micropores, extended π conjugation, excellent chemical stability and thermal stability. They have broad application prospects as ion exchange membranes for osmotic energy harvesting. However, to the best of our knowledge, CMPs have never been applied to develop ion-selective exchange membranes for osmotic energy harvesting. This is because most CMPs membranes reported so far are neutral nanopore frameworks and do not have the ability to separate charges. Ionic CMPs (i-CMPs) are an interesting type of CMPs because they have the characteristics of CMPs materials; after integrating ion modules into the CMP framework, charged channels can be formed in sub-nanometer spaces, giving them the ability to separate charges. At the same time, this will make ion transport subject to the dual control of size and charge, thereby further improving selectivity without sacrificing permeability. Therefore, i-CMPs are considered to be promising candidates for ion conductors and ion separators, which can break the trade-off between ion conductivity and ion selectivity. However, due to the intrinsic extremely rigid cross-linked structure of CMPs materials, which makes them challenging in terms of processability and control of film formation, only a few i-CMPs films have been reported. Summary of the invention

[0004] Purpose of the invention: The first purpose of the present invention is to provide an ionic conjugated microporous polymer nanochannel composite membrane, which has stable performance and is green and environmentally friendly. The second purpose of the present invention is to provide a method for preparing an ionic conjugated microporous polymer nanochannel composite membrane, which is simple to operate, mild in conditions and easy to implement. The third purpose of the present invention is to provide an application of the ionic conjugated microporous polymer nanochannel composite membrane in salinity gradient energy conversion. The ionic conjugated microporous polymer nanochannel composite membrane can be used for salinity gradient energy conversion, extracting osmotic energy from the salinity gradient, and has the advantages of stable performance, high conversion power, and a wide range of applicable environments.

[0005] Technical solution: The present invention discloses an ionic conjugated microporous polymer nanochannel composite membrane, which comprises a layer of ionic conjugated microporous polymer membrane and a layer of membrane material with a macroporous structure, wherein some pores of the ionic conjugated microporous polymer membrane are correspondingly connected with some macropores in the membrane material with a macroporous structure.

[0006] Furthermore, the ionic conjugated microporous polymer membrane has an ultra-thin membrane thickness and regular charged sub-nanometer pores.

[0007] Furthermore, the ionic conjugated microporous polymer membrane includes 1,3,5-tri(9-carbazolyl)benzene and an ionic carbazole monomer (i-Cbz) and is synthesized by electrochemical polymerization.

[0008] Furthermore, the ionic carbazole monomer is 6-(9H-carbazole-9-yl)-N,N,N-trimethylhexane-1-ammonium bromide (CbzC6-N), 6-(9H-carbazole-9-yl)hexane-1-sodium sulfonate (CbzC6-S) or carbazole (Cbz).

[0009] Furthermore, the membrane material with a macroporous structure is selected from one of anodized aluminum membrane (AAO), titanium dioxide nanotube array membrane (TNT), polycarbonate membrane (PC), cellulose membrane (NC), polytetrafluoroethylene membrane (PTFE) or polyvinylidene fluoride membrane (PVDF), preferably AAO.

[0010] Furthermore, the thickness of the ionic conjugated microporous polymer membrane is 40-100 nm, preferably 40 nm, and the diameter of the pores is 0.7-0.9 nm.

[0011] Furthermore, the diameter of the pores of the membrane material having a macroporous structure is 50 to 80 nm, preferably 60 nm.

[0012] The method for preparing the ionic conjugated microporous polymer nanochannel composite membrane of the present invention comprises the following steps:

[0013] (1) mixing 1,3,5-tri(9-carbazolyl)benzene, an ionic carbazole monomer, and a supporting electrolyte, and adding dichloromethane and acetonitrile to obtain a mixed solution;

[0014] (2) Using a membrane material with a macroporous structure as a working electrode, an electrochemical polymerization reaction is carried out using cyclic voltammetry;

[0015] (3) After the polymerization reaction is completed, the composite membrane material is taken out, washed with a solvent, and vacuum dried to obtain an ionic conjugated microporous polymer nanochannel composite membrane.

[0016] Furthermore, in step (1), the supporting electrolyte is tetrabutylammonium hexafluorophosphate.

[0017] Furthermore, in step (1), the molar ratio of 1,3,5-tri(9-carbazolyl)benzene to the ionic carbazole monomer (i-Cbz) is (1-1.2):(1-1.5), preferably 1:1.

[0018] Furthermore, in step (1), the content of the supporting electrolyte in the mixed solution is 0.1 to 0.2 mol / L.

[0019] Furthermore, in step (1), the volume ratio of dichloromethane to acetonitrile is 3-4:2-1, preferably 3:2.

[0020] Furthermore, in step (1), the volume molar ratio of dichloromethane to 1,3,5-tri(9-carbazolyl)benzene is 24:03-0.05 mL / mmol, preferably 24:0.04 mL / mmol.

[0021] Furthermore, in step (2), the window potential of the cyclic voltammetry is -0.6 to +1.23 V, the scan rate is 50 to 100 mV / s, the polymerization time is 0.5 to 6 h, and the reaction temperature is maintained at 20 to 25° C., preferably: the temperature is 20° C. and the polymerization time is 1 h.

[0022] Furthermore, in step (3), the solvent is a mixed solution of dichloromethane and acetonitrile, and the volume ratio of dichloromethane to acetonitrile is 3-4:2-1, preferably 3:2.

[0023] Furthermore, in step (3), the washing method is to immerse the composite membrane in the solvent for 10 to 12 hours, preferably for 10 hours.

[0024] Furthermore, in step (3), vacuum drying is performed at 60-100° C. for 6-8 h, preferably at 80° C. for 8 h.

[0025] The invention discloses an application of the ionic conjugated microporous polymer nanochannel composite membrane in a salinity gradient energy conversion process.

[0026] Furthermore, during the application process, a salinity difference is formed between the concentrated salt solution and the dilute salt solution, and the salt difference energy is converted into electrical energy.

[0027] Furthermore, the molar ratio of the concentrated salt solution to the dilute salt solution is (0.1-5):(0.0001-0.1).

[0028] Furthermore, the concentrated salt solution and the dilute salt solution are both sodium chloride solution, potassium chloride solution, magnesium chloride solution, lithium bromide solution or calcium chloride solution.

[0029] Furthermore, the molar concentration of the concentrated salt solution is 0.1-5 mol / L.

[0030] Furthermore, the molar concentration of the dilute salt solution is 0.0001-0.1 mol / L.

[0031] Furthermore, the concentrated salt solution and the dilute salt solution have the same salt type.

[0032] The present invention uses 1,3,5-tri(9-carbazolyl)benzene and ionic carbazole monomers as raw materials and prepares an ionic conjugated microporous polymer nanochannel composite membrane through electrochemical polymerization technology. The ionic conjugated microporous polymer membrane prepared by the present invention has an ultra-thin membrane thickness and charged sub-nanometer membrane pores; it can simultaneously achieve selective ion transmission and have good ion permeability.

[0033] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:

[0034] (1) The ionic conjugated microporous polymer nanochannel composite membrane of the present invention includes an ionic conjugated microporous polymer membrane with regular charged sub-nanopores. The ionic conjugated microporous polymer nanochannel composite membrane has stable performance, is green and environmentally friendly, and has a simple preparation method, mild conditions and is easy to implement. It overcomes the shortcomings of the prior art that ion selectivity and ion permeability cannot be taken into account at the same time, the process is complicated, and the controllability is poor.

[0035] (2) The application of the ionic conjugated microporous polymer nanochannel composite membrane of the present invention in salinity gradient osmotic energy conversion has obvious advantages:

[0036] First, the ionic conjugated microporous polymer membrane used as the ion selective layer has abundant charged sub-nanopores in the membrane, which endows the ion selective layer with excellent ion selectivity; the introduction of more electronegative functional groups can further increase the surface charge density and further improve the ion selectivity of the membrane. The ultra-thin membrane thickness and regular pores and structures significantly reduce the resistance of ion transport across the membrane, effectively improving the permeability of ions through the selective layer.

[0037] Secondly, the inherent surface charge distribution asymmetry and structural asymmetry of the ionic conjugated microporous polymer nanochannel composite membrane make the charge density of the ionic conjugated microporous polymer membrane layer higher than that of the membrane material with a macroporous structure, and the pore size is smaller than that of the membrane material with a macroporous structure. This makes the asymmetric ionic conjugated microporous polymer nanochannel composite membrane have good ion current rectification characteristics, greatly improving the ion selectivity of the osmotic energy conversion system.

[0038] Again, the ionic conjugated microporous polymer nanochannel composite membrane of the present invention successfully converts salinity gradient energy into electrical energy in the salinity gradient osmotic energy conversion. Under the conditions of simulating the salinity gradient of seawater (0.5 mol / L NaCl) and river water (0.01 mol / L NaCl), the maximum output power density reached 18.91 W / m 2 , this is the commercial standard 5W / m 2 Above that, further increasing the salinity gradient (5mol / L NaCl / 0.01mol / L NaCl), the maximum output power density can be increased to 105W / m 2 .

[0039] Finally, the ionic conjugated microporous polymer nanochannel composite membrane of the present invention showed good stability in the application of salinity gradient osmotic energy conversion. After 10 days of performance stability testing, the maximum output power density had almost no attenuation, laying a solid foundation for subsequent practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 Schematic diagram of the preparation process of the ionic conjugated microporous polymer nanochannel composite membrane prepared in Example 1;

[0041] Figure 2 This is a scanning electron microscope image of the AAO film prepared in Example 1;

[0042] Figure 3 is a scanning electron microscope image of the Au-AAO film prepared in Example 1;

[0043] Figure 4 This is a scanning electron microscope image of the ionic conjugated microporous polymer nanochannel composite membrane prepared in Example 1;

[0044] Figure 5 This is a schematic diagram of the salinity gradient osmotic energy conversion device in Example 4;

[0045] Figure 6 The current density and external resistance relationship diagram and the power density and external resistance relationship diagram obtained in the salinity gradient osmotic energy conversion of the ionic conjugated microporous polymer nanochannel composite membranes of different thicknesses in Example 1 and Example 3;

[0046] Figure 7 The current density-external resistance relationship diagram and the power density-external resistance relationship diagram obtained in the salinity gradient osmotic energy conversion of the i-CMPs / AAO composite membrane in Example 1-2 and the CMPs / AAO composite membrane and the AAO membrane in Comparative Example 1;

[0047] Figure 8 It is a comparison chart of the energy conversion performance of salinity gradient osmosis of membrane materials reported in relevant literature in Example 2 and Comparative Example 2;

[0048] Fig. 9 This is a test graph of the salinity gradient osmotic energy conversion of the ionic conjugated microporous polymer nanochannel composite membrane in Example 5 within 10 days. DETAILED DESCRIPTION

[0049] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0050] Example 1 Preparation of ionic conjugated microporous polymer nanochannel composite membrane

[0051] (1) Preparation of anodized aluminum (AAO) membrane: First, the aluminum foil was ultrasonically cleaned with acetone and 1 mol / L NaOH solution for 10 minutes, and the residual liquid on the surface of the aluminum foil was rinsed with deionized water after the ultrasonic treatment. The first anodization was carried out with 0.4 mol / L oxalic acid as the electrolyte at 50 V and 25°C for 40 minutes. In order to eliminate the irregular oxide layer formed, the oxide layer formed on the surface of the aluminum foil after the first anodization was cleaned with a mixed acid solution consisting of 6 wt% H3PO4 and 2 wt% H2CrO4 at 60°C for 30 minutes. Subsequently, the second anodization was carried out for 6 hours, and the other conditions were the same as the first anodization. The aluminum substrate was removed with a saturated CuCl2 solution. The AAO membrane was treated with a 5 wt% H3PO4 solution at 30°C for 40 minutes to remove the barrier layer on the top of the anodized aluminum membrane. The AAO membrane was soaked in deionized water overnight and dried. The pore size of the nanochannels in the anodic aluminum oxide membrane can be controlled by adjusting the voltage during anodization. Scanning electron microscopy analysis of the AAO membrane shows that the pore size of the AAO membrane is 60 nm, the thickness is 40 μm, and the pores are evenly distributed. Figure 2 shown. Figure 2 The following are scanning electron microscope images of the AAO membrane prepared in Example 1, wherein A is the SEM image of the AAO top barrier layer, B is the SEM image of the top cross section, C is the SEM image of the AAO bottom, and D is the SEM image of the bottom cross section. Figure 2 It can be seen that the prepared AAO has a regular and orderly morphology and structure.

[0052] (2) Preparation of Au-AAO: A thin Au-AAO film with gold conductive function was plated on one side of the prepared AAO film using magnetron sputtering technology. Scanning electron microscopy analysis of Au-AAO was performed, such as Figure 3 shown. Figure 3 The following are scanning electron microscope images of the Au-AAO film prepared in Example 1, wherein A is the SEM image of the top of Au-AAO and B is the SEM image of the top cross section. Figure 3 It can be seen that the sputtered Au layer has no effect on the surface morphology of AAO.

[0053] (3) Preparation of a mixed reaction liquid: 23 mg of 1,3,5-tri(9-carbazolyl)benzene and an equal molar amount of ionic carbazole monomer CbzC6-S: 12.45 mg, and 1.55 g of tetrabutylammonium hexafluorophosphate were dissolved in 40 mL of a mixed solution of dichloromethane and acetonitrile (volume ratio 3:2) to obtain a mixed reaction liquid.

[0054] (4) Preparation of ionic conjugated microporous polymer nanochannel composite membrane: 40 mL of the mixed reaction solution was placed in an electrolytic cell device, in which an Au-AAO membrane with a lead wire was fixed, and electrochemical polymerization was carried out by cyclic voltammetry, with a window potential of -0.6 to +1.23 V, a scan rate of 50 mV / s, and a polymerization time of 1 h. The ionic conjugated microporous polymer membrane structure was deposited on an area of ​​1.14 cm 2 On the conductive gold surface of the Au-AAO membrane material with a macroporous structure, an ionic conjugated microporous polymer nanochannel (S-CMP / AAO) composite membrane with an AAO nanochannel pore size of 60 nm was obtained. The preparation process is as follows Figure 1 The ionic conjugated microporous polymer nanochannel composite membrane layer prepared in this embodiment was analyzed by scanning electron microscope, and the thickness of the ionic conjugated microporous polymer membrane layer was found to be 40±0.5nm. Figure 4 shown. Figure 4 The scanning electron microscope images of the ionic conjugated microporous polymer nanochannel composite membrane prepared in Example 1, wherein (A) is the top image of the i-CMPs / AAO composite membrane, (B) is the cross-sectional image of the i-CMPs / AAO composite membrane, (C) is the bottom image of the i-CMPs / AAO composite membrane, and (D) is the top magnified image of the cross-sectional top of the i-CMPs / AAO composite membrane. Figure 4 It can be seen that the ionic conjugated microporous polymer membrane is tightly covered on the top of the AAO nanochannel, indicating the successful preparation of the ionic conjugated microporous polymer nanochannel composite membrane. The pore size of the ionic conjugated microporous polymer membrane layer was measured to be 0.78nm by 77K nitrogen adsorption experiment.

[0055] Example 2

[0056] The preparation process is the same as in Example 1, except that CbzC6-N: 15.6 mg or Cbz: 6.69 mg is used instead of CbzC6-S: 12.45 mg, and two groups of ionic conjugated microporous polymer nanochannel (i-CMPs / AAO) composite membranes are obtained, which are respectively recorded as N-CMP / AAO and H-CMP / AAO. Scanning electron microscopy analysis shows that the thickness of the two groups of ionic conjugated microporous polymer membrane layers is 40±0.5 nm, and the pore sizes of the ionic conjugated microporous polymer membrane layers measured by 77K nitrogen adsorption experiments are 0.73 nm and 0.85 nm, respectively. Successful preparation of ionic conjugated microporous polymer nanochannel composite membranes.

[0057] Example 3 Experimental process for preparing ionic conjugated microporous polymer nanochannel composite membranes with different thicknesses

[0058] The preparation process is the same as that of Example 1, except that by changing the electrochemical polymerization time in step (4) of Example 1 to 1.5 h, 2 h, 2.5 h, and 3 h, four groups of clay-based nanofiber nanochannel composite membranes with an anodic aluminum oxide nanochannel pore size of 60 nm can be obtained. Scanning electron microscopy analysis shows that the thicknesses of the four groups of ionic conjugated microporous polymer membrane layers are 50 ± 0.5 nm, 60 ± 0.5 nm, 80 ± 0.5 nm, and 100 ± 0.5 nm, respectively. This indicates that the electrochemical polymerization time can regularly affect the thickness of the ionic conjugated microporous polymer membrane layer.

[0059] Example 4 Application of salinity gradient osmotic energy conversion of ionic conjugated microporous polymer nanochannel composite membrane

[0060] 1. Salinity gradient osmotic energy conversion device such as Figure 5 As shown, the salinity gradient osmotic energy conversion device is a homemade H-two-chamber electrochemical electrolytic cell, and the ionic conjugated microporous polymer nanochannel composite membrane is sandwiched between the two cells, and the entire device is fixed by screws. The large pore end of the ionic conjugated microporous polymer nanochannel composite membrane, that is, the side of the anodized aluminum, is filled with a concentrated salt solution (0.5M NaCl electrolyte solution), and the small pore end of the ionic conjugated microporous polymer nanochannel composite membrane, that is, the side of the ionic conjugated microporous polymer membrane, is filled with a dilute salt solution (0.01M NaCl electrolyte solution). The two salt solutions are connected to the circuit through an external electrochemical workstation and a load resistor, and the measurement of the relationship curve between current density, power density and external resistance is achieved by adjusting the change of the external resistance value.

[0061] 2. Salinity gradient osmotic energy conversion of ionic conjugated microporous polymer nanochannel composite membranes with different thicknesses

[0062] The salinity gradient osmotic energy conversion device in step 1 was used, and the composite membranes in the salinity gradient osmotic energy conversion device were replaced by the ionic conjugated microporous polymer nanochannel composite membranes prepared in Example 1 and Example 3, respectively. Other conditions remained unchanged, and the effect of the thickness of the ionic conjugated microporous polymer membrane on the salinity gradient osmotic energy conversion performance was tested. The results are as follows: Figure 6 shown.

[0063] Figure 6 The current density and external resistance relationship diagrams and the power density and external resistance relationship diagrams obtained in the salinity gradient osmotic energy conversion of ionic conjugated microporous polymer nanochannel composite membranes of different thicknesses in Example 1 and Example 3, wherein A is the current density and external resistance relationship diagram, and B is the power density and external resistance relationship diagram. Figure 6It can be found that when the thickness of the ionic conjugated microporous polymer membrane is 40±0.5nm, 50±0.5nm, 60±0.5nm, 80±0.5nm and 100±0.5nm, the corresponding external circuit power density is 18.91W / m 2 、13.67W / m 2 、10.7W / m 2 、8.59W / m 2 and 7.05W / m 2 When the thickness of the ionic conjugated microporous polymer membrane is within 40~100±0.5nm, it meets the commercial standard of 5W / m 2 , and when the thickness of the ionic conjugated microporous polymer membrane is 40±0.5nm, its salinity gradient osmotic energy conversion output power is the highest.

[0064] Comparative Example 1

[0065] Preparation of CMPs / AAO membrane: The preparation process is the same as that in Example 1, except that 40 mL of the mixed reaction solution in Example 1 is replaced with 40 mL of 1 mmol / L pure 1,3,5-tri(9-carbazolyl)benzene solution, and the CMPs / AAO membrane is formed on Au-AAO by electrochemical polymerization.

[0066] The output power density of salinity gradient osmotic energy conversion of pure AAO membrane and CMPs / AAO membrane. The ionic conjugated microporous polymer nanochannel composite membrane in Example 4 was replaced with the pure AAO membrane prepared in Example 1 and the CMPs / AAO membrane prepared in this comparative example, respectively. Other conditions remained unchanged, and the salinity gradient osmotic energy conversion was tested. The results are shown in Figure 7 shown.

[0067] Figure 7 The current density-to-resistance relationship diagram and the power density-to-resistance relationship diagram obtained in the salinity gradient osmotic energy conversion of the i-CMPs / AAO composite membrane in Example 1-2 and the CMPs / AAO composite membrane and AAO membrane in Comparative Example 1 are shown in Figure 1-2; A is the current density-to-resistance relationship diagram; B is the power density-to-resistance relationship diagram. Figure 7 The experimental results show that the corresponding external circuit power density of pure AAO membrane and CMPs / AAO membrane under 0.01M:0.5M NaCl gradient is 0.58W / m 2 and 1.41W / m 2, which is far lower than the external circuit power density of the i-CMPs / AAO membrane with a thickness of 40±0.5nm of the present invention. Since the pure AAO membrane does not have the functional layer of ionic conjugated microporous polymer membrane to improve the ion selective transmission performance, the salinity gradient osmotic energy conversion performance of the pure AAO membrane is far inferior to that of the ionic conjugated microporous polymer nanochannel composite membrane.

[0068] Comparative Example 2

[0069] The existing publicly reported:

[0070] Two-dimensional layered transition metal carbide (MXenes) films (see L. Ding, M. Zheng, D. Xiao, et al. Bioinspired Ti3C2T x MXene-Based Ionic Diode Membrane for High-EfficientOsmotic Energy Conversion. Angew. Chem. Int. Ed. 2022, 61, e202206152.);

[0071] Metal organic framework (MOFs) membrane (see C. Chen, L. Meng, L. Cao, et al. Phase Engineering of Zirconium MOFs Enables Efficient Osmotic Energy Conversion: Structural Evolution Unveiled by Direct Imaging. J. Am. Chem. Soc. 2024 146 (17), 11855-11865.);

[0072] Covalent organic framework alumina (COFs / AAO) composite membrane (see M. Chen, K. Yang, J. Wang, et al. InSitu Growth of Imine-Bridged Anion-Selective COF / AAO Membrane for Ion Current Rectification and Nanofluidic Osmotic Energy Conversion. Adv. Funct. Mater., 33: 2302427.);

[0073] Polymer (SPEEKs) membrane (see Y.Sun, T.Dong, C.Lu, et al. Tailoring A Poly (ethersulfone) Bipolar Membrane: Osmotic-Energy Generator with High Power Density. Angew. Chem. Int. Ed. 2020, 59, 17423.)

[0074] The salinity gradient osmotic energy conversion output power density of the above membrane material is compared with the salinity gradient osmotic energy collection performance of the ionic conjugated microporous polymer nanochannel composite membrane (S-CMP / AAO) in Example 1. The results are as follows Figure 8 Shown

[0075] Figure 8 This is a comparison chart of the maximum output power density obtained by the ionic conjugated microporous polymer nanochannel composite membrane in Example 1 and the existing membrane material in Comparative Example 2 in salinity gradient osmotic energy conversion. Figure 8 The comparison results show that the corresponding external circuit power density of MXenes membrane, MOF membrane, COF membrane and Polymers membrane under the salinity gradient of 0.01M:0.5M is 8.6W / m 2 、10.08W / m 2 , 2.55W / m 2 and 6.2W / m 2 , which is lower than the external circuit power density of 18.91 W / m of the ionic conjugated microporous polymer membrane (S-CMP / AAO) with a thickness of 40±0.5 nm of the present invention. 2 The salinity gradient osmotic energy conversion performance of some existing advanced membrane materials is inferior to that of the ionic conjugated microporous polymer nanochannel composite membrane of the present invention.

[0076] Example 5 Stability test of salinity gradient osmotic energy conversion of ionic conjugated microporous polymer nanochannel composite membrane

[0077] The ionic conjugated microporous polymer nanochannel composite membranes with a thickness of 40±0.5 nm in Examples 1 and 2 were placed for 2 days, 4 days, 6 days, 8 days, and 10 days to perform salinity gradient osmotic energy conversion tests. The process after the test was the same as in Example 4, and other conditions remained unchanged. The results are shown in Fig. 9 shown.

[0078] Fig. 9 This is a 10-day salinity gradient osmotic energy conversion test of the ionic conjugated microporous polymer nanochannel composite membrane in Example 1 and Example 2. Fig. 9The experimental results show that the ionic conjugated microporous polymer nanochannel composite membranes prepared in Examples 1 and 2 show good stability in the application of salinity gradient osmotic energy conversion. After 10 consecutive days of testing, the reduction in output power density was less than 5%, laying a reliable foundation for subsequent practical applications.

Claims

1. An ionic conjugated microporous polymer nanochannel composite membrane, characterized in that: The ionic conjugated microporous polymer nanochannel composite membrane comprises a layer of ionic conjugated microporous polymer membrane and a layer of membrane material with a macroporous structure. Part of the pores of the ionic conjugated microporous polymer membrane are correspondingly connected with part of the macropores in the membrane material with a macroporous structure.

2. The ionic conjugated microporous polymer nanochannel composite membrane according to claim 1, characterized in that: The ionic conjugated microporous polymer membrane has an ultra-thin membrane thickness and regular charged sub-nanopores. The ionic conjugated microporous polymer membrane is synthesized by electrochemical polymerization of 1,3,5-tri(9-carbazolyl)benzene and ionic carbazole monomers.

3. The ionic conjugated microporous polymer nanochannel composite membrane according to claim 1, characterized in that: The ionic carbazole monomer is 6-(9H-carbazole-9-yl)-N,N,N-trimethylhexane-1-ammonium bromide, 6-(9H-carbazole-9-yl)hexane-1-sodium sulfonate or carbazole.

4. The ionic conjugated microporous polymer nanochannel composite membrane according to claim 1, characterized in that: The membrane material with a macroporous structure is selected from one of an anodic aluminum oxide membrane, a titanium dioxide nanotube array membrane, a polycarbonate membrane, a cellulose membrane, a polytetrafluoroethylene membrane or a polyvinylidene fluoride membrane.

5. The ionic conjugated microporous polymer nanochannel composite membrane according to claim 1, characterized in that: The thickness of the ionic conjugated microporous polymer membrane is 40-100 nm, the diameter of the pores is 0.7-0.9 nm, and the diameter of the pores of the membrane material with a macroporous structure is 50-80 nm.

6. The method for preparing the ionic conjugated microporous polymer nanochannel composite membrane according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) 1,3,5-tri(9-carbazolyl)benzene, an ionic carbazole monomer and a supporting electrolyte are mixed, and dichloromethane and acetonitrile are added to obtain a mixed solution; (2) Using a membrane material with a macroporous structure as the working electrode, the electrochemical polymerization reaction was carried out using cyclic voltammetry; (3) After the polymerization reaction is completed, the composite membrane material is taken out, washed with a solvent, and vacuum dried to obtain an ionic conjugated microporous polymer nanochannel composite membrane.

7. The method for preparing the ionic conjugated microporous polymer nanochannel composite membrane according to claim 6, characterized in that: In step (1), the supporting electrolyte is tetrabutylammonium hexafluorophosphate, the molar ratio of 1,3,5-tri(9-carbazolyl)benzene to the ionic carbazole monomer is 1-1.2:1-1.5, the content of the supporting electrolyte in the mixed solution is 0.1-0.2 mol / L, the volume ratio of dichloromethane to acetonitrile is 3-4:2-1, and the volume molar ratio of dichloromethane to 1,3,5-tri(9-carbazolyl)benzene is 24:0.03-0.05 mL / mmol.

8. The method for preparing the ionic conjugated microporous polymer nanochannel composite membrane according to claim 6, characterized in that: In step (2), the window potential of the cyclic voltammetry is -0.6 ~ +1.23 V, the scan rate is 50~100 mV / s, the time is 0.5~6 h, and the reaction temperature is maintained at 20~25 °C; in step (3), the solvent is a mixed solution of dichloromethane and acetonitrile, the washing method is to immerse the composite membrane in the solvent for 10~12 h; the vacuum drying is to dry at 60~100 °C for 6~8 h.

9. Use of the ionic conjugated microporous polymer nanochannel composite membrane according to any one of claims 1 to 5 in a salinity gradient energy conversion process.

10. The use according to claim 9, characterized in that: During the application process, a salinity difference is formed between the concentrated salt solution and the dilute salt solution, and the salt difference energy is converted into electrical energy, wherein the molar ratio of the concentrated salt solution to the dilute salt solution is 0.1~5:0.0001~0.1, and the concentrated salt solution and the dilute salt solution are both sodium chloride solution, potassium chloride solution, magnesium chloride solution, lithium bromide solution or calcium chloride solution, and the types of salt in the concentrated salt solution and the dilute salt solution are consistent.

Citation Information

Patent Citations

  • Mesoporous carbon-silicon / anodic aluminum oxide composite film, super-assembly preparation method and application thereof

    CN111729512A

  • Plasma electronic sponge nano-channel composite membrane as well as preparation method and application thereof

    CN117018870A

  • Method of preparing nano-composite membrane for high-temperature polymer electrolyte membrane fuel cell (htpemfc)

    IN201711038293A

  • Ultrathin-film composite membrane

    US5198112A

Cited By

  • Multistage asymmetric covalent organic framework film and preparation method and application thereof

    CN119869241A

  • Conjugated microporous polymer composite organic solvent nanofiltration membrane as well as preparation method and application thereof

    CN120984119A

  • In-situ polymerization functional polymer composite film as well as preparation method and application thereof

    CN122381522A

  • In-situ polymerized functional polymer composite film, and preparation method and application thereof

    CN122381522B

  • Ion channel and ion pump synergetic energy conversion system and method for enhancing permeation power generation performance through light

    CN122643894A