Method of manufacturing cobalt sulfate

Emulsion flow solvent extraction with sodium hydroxide in the production of cobalt sulfate from crude cobalt hydroxide addresses cost and yield challenges, achieving high purity and efficiency by suppressing hydroxide precipitation and downsizing equipment, resulting in reduced costs and improved cobalt recovery.

JP2024142875AActive Publication Date: 2024-10-11PACIFIC METALS
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023055254
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Existing methods for producing cobalt sulfate from crude cobalt hydroxide face challenges in achieving high cobalt yield while reducing costs, particularly due to high equipment and reagent costs associated with solvent extraction using mixer-settlers and the use of ammonia water as a pH adjuster, which requires ammonia recovery and leads to hydroxide precipitation issues.

Method used

The method employs emulsion flow solvent extraction with sodium hydroxide as a pH adjuster, adjusting the volume and flow rate ratios of the organic and aqueous phases, and using mechanical stirring blades to form an emulsion phase, which allows for efficient extraction and reduces equipment size, thereby lowering costs and suppressing hydroxide precipitation.

Benefits of technology

This approach enables the production of high-purity cobalt sulfate with a cobalt yield of 92% or more, and up to 97% when filtrate is reused, while significantly reducing costs by 75% for initial solvent extraction equipment and 7% for pH adjusters, compared to traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142875000001_ABST
    Figure 2024142875000001_ABST
Patent Text Reader

Abstract

To provide a method of manufacturing cobalt sulfate, the method capable of acquiring the cobalt sulfate from rough cobalt hydroxide, whose cost is reduced while maintaining a high yield of cobalt.SOLUTION: According to a method of manufacturing cobalt sulfate from rough cobalt hydroxide containing at least one selected from the group consisting of iron, copper, aluminum, manganese, calcium, zinc, nickel, and magnesium as impurity elements, There is provided the method of manufacturing cobalt sulfate, comprising the steps of: forming an emulsion phase obtained from an aqueous phase and an organic phase, based on a continuous process of adjusting a volume ratio as well as a flow rate between the aqueous phase and the organic phase; and including a solvent extraction process in which an aqueous sodium hydroxide solution is used as a pH adjuster.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing cobalt sulfate from crude cobalt hydroxide, and more specifically, to a method for separating manganese from a sulfuric acid solution containing manganese and cobalt to obtain a high-purity aqueous cobalt sulfate solution having a low manganese concentration, which can be used as a raw material for lithium-ion secondary batteries, etc. [Background technology]

[0002] Cobalt sulfate is an important raw material for the cathode material of lithium-ion batteries. When using cobalt sulfate as a raw material for the cathode material of lithium-ion batteries, it is necessary to separate impurities as much as possible to obtain a high purity in order to ensure the required performance.

[0003] In addition to cobalt, crude cobalt hydroxide contains impurities such as iron, copper, aluminum, manganese, calcium, zinc, nickel, magnesium, etc. In producing cobalt sulfate from crude cobalt hydroxide, it is necessary to reduce costs while maintaining a high cobalt yield.

[0004] For example, Patent Document 1 discloses a method for achieving a high cobalt yield when obtaining cobalt sulfate from crude cobalt hydroxide. Patent Document 1 also discloses that solvent extraction is performed using a mixer settler, and ammonia water is used as a pH adjuster. When ammonia water is used as a pH adjuster, it is necessary to carry out wastewater treatment accompanied by ammonia recovery. The cost of ammonia water and ammonia recovery equipment is high, which hinders cost reduction.

[0005] The present inventors have carried out solvent extraction using a mixer settler to obtain cobalt sulfate from crude cobalt hydroxide, and have attempted to reduce costs by changing the pH adjuster from aqueous ammonia to an aqueous sodium hydroxide solution. However, the present inventors have found that when an aqueous sodium hydroxide solution is used as the pH adjuster in solvent extraction using a mixer settler, hydroxide precipitation occurs, and therefore there is room for improvement in improving the extraction rate of the target element. In addition, the present inventors have found that in some steps of solvent extraction using a mixer settler, a large amount of hydroxide precipitation occurs, and therefore there is room for improvement in improving phase separation by suppressing the precipitation. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2022-104563 A [Patent Document 2] JP 2022-164276 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made based on the above-mentioned background, and an object of the present invention is to provide a method for producing cobalt sulfate, which can produce cobalt sulfate from crude cobalt hydroxide at reduced costs while maintaining a high cobalt yield. [Means for solving the problem]

[0008] It was assumed that the precipitation of hydroxides could be suppressed by lowering the extractant concentration in the organic phase, and the inventors attempted to maintain the extraction rate of the target elements by increasing the flow rate ratio of the organic phase to the aqueous phase to compensate for the reduction in the extractant concentration in the organic phase. However, the expected effects of suppressing hydroxide precipitation and improving phase separation were not obtained. In addition, increasing the ratio of the organic phase to the aqueous phase increases the size of the mixing tank, and there was concern that the equipment costs for solvent extraction would increase. Thus, solvent extraction using a mixer settler had many problems in terms of reducing costs.

[0009] In order to solve the above problems related to solvent extraction, the present inventors applied emulsion flow instead of the conventional mixer settler for the following reasons. Emulsion flow is an innovative solvent extraction technology that is expected to improve productivity by 10 times compared to the conventional mixer settler. For example, Patent Document 2 discloses a solvent extraction and solvent extraction device using emulsion flow. A solvent extraction device using emulsion flow (emulsion flow device) is equipped with a droplet ejection nozzle or mechanical stirring blade, and can perform highly efficient extraction by forming an emulsion mixed phase (emulsion phase) of a heavy liquid phase (in most cases, an aqueous phase) and a light liquid phase (in most cases, an organic phase).

[0010] If emulsion flow is applied to solvent extraction, the above problems can be solved, the pH adjuster can be changed from aqueous ammonia to aqueous sodium hydroxide, and the solvent extraction device can be made smaller, which may result in cost reduction. Therefore, as described below, emulsion flow is used in the solvent extraction process, but the scope of the present invention is not limited to this.

[0011] The gist of the present invention, which has been made based on the above findings, is as follows. (1) A method for producing cobalt sulfate from crude cobalt hydroxide containing one or more impurity elements selected from the group consisting of iron, copper, aluminum, manganese, calcium, zinc, nickel, and magnesium, comprising the steps of: A method for producing cobalt sulfate, comprising a solvent extraction step of forming an emulsion phase between an aqueous phase and an organic phase based on a continuous treatment in which a volume ratio and a flow rate ratio between the aqueous phase and the organic phase are adjusted, and using an aqueous sodium hydroxide solution as a pH adjuster. (2) The method for producing cobalt sulfate according to (1) above, wherein the emulsion phase is formed using a mechanical stirring blade. (3) The method for producing cobalt sulfate according to (1) or (2) above, wherein the solvent extraction step is carried out in the order of a Mn-removal step, a Ni-removal step, and a Mg-removal step. (4) The method for producing cobalt sulfate according to any one of the above (1) to (3), wherein ammonia water is not used as the pH adjuster. Effect of the Invention

[0012] According to the present invention, it is possible to provide a method for producing cobalt sulfate, which is capable of obtaining cobalt sulfate from crude cobalt hydroxide at reduced costs while maintaining a high cobalt yield. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a process explanatory diagram showing a method for producing cobalt sulfate according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a process explanatory diagram illustrating a method for producing cobalt sulfate according to an embodiment of the present invention, showing details of an impurity removing step. [Diagram 3] FIG. 2 is a process explanatory diagram showing a method for producing cobalt sulfate according to a comparative example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of a method for producing cobalt sulfate according to the present invention will be described with reference to the drawings and tables. In the table, "X to Y" (where X and Y are arbitrary numerical values) means "X or more and Y or less". Also, "<Z1" (where Z1 is an arbitrary numerical value) means that the value is less than Z1, and "≦Z2" (where Z2 is an arbitrary numerical value) means that the value is Z2 or less.

[0015] FIG. 1 is a process explanatory diagram showing a method for producing cobalt sulfate according to an embodiment. As shown in FIG. 1, the method for producing cobalt sulfate according to the present embodiment includes the following leaching step S1, impurity separation step S2, and crystallization step S3.

[0016] Leaching step S1: A step of slurrying crude cobalt hydroxide HRC containing one or more of the group consisting of iron, copper, aluminum, manganese, calcium, zinc, nickel, and magnesium as impurity elements, and further leaching with an acid to obtain a leaching slurry ES. Impurity separation step S2: A step of separating impurities in the leaching slurry ES to obtain a cobalt concentrated liquid CCL. Crystallization step S3: A step of crystallizing the cobalt concentrated liquid CCL to obtain cobalt sulfate RC.

[0017] In the method for producing cobalt sulfate according to the present embodiment, the crude cobalt hydroxide HRC used as a raw material is obtained as a by-product of copper smelting, and is a powder containing iron, copper, aluminum, manganese, calcium, zinc, nickel, magnesium, etc. as impurities in addition to cobalt. An example of the approximate composition of the crude cobalt hydroxide HRC according to the present embodiment is shown in Table 1 below. In Table 1, the content of each metal component other than Co is shown as a relative mass ratio to Co.

[0018]

Table 1

[0019] Hereinafter, the method for producing cobalt sulfate according to this embodiment will be described in detail with reference to Fig. 2. Fig. 2 is a process explanatory diagram showing the method for producing cobalt sulfate according to the embodiment of the present invention, showing details of the impurity removal step. Note that Fig. 2 describes the impurity separation step S2 in detail.

[0020] [Leaching process S1] In the leaching step S1, pure water is added to the crude cobalt hydroxide HRC to form a slurry having a slurry concentration (solid mass relative to the total mass) of about 30%, thereby obtaining a crude cobalt hydroxide slurry. The crude cobalt hydroxide slurry is leached for about 0.5 hours at normal pressure and at a temperature of 95°C or higher by adding a reducing agent and concentrated sulfuric acid, thereby obtaining a leached slurry ES containing cobalt and one or more of the group consisting of iron, copper, aluminum, manganese, calcium, zinc, nickel, and magnesium.

[0021] By setting the leaching temperature at 95°C or higher, the leaching rate of cobalt in the crude cobalt hydroxide slurry can be improved. This shortens the leaching time of cobalt contained in the crude cobalt hydroxide slurry and simultaneously increases the leaching rate of cobalt. The upper limit of the leaching temperature is not particularly limited, but may be the boiling point of the leaching solution.

[0022] The pure water added to the crude cobalt hydroxide HRC should be as pure as possible. Adding low-purity water, such as tap water or industrial water, will cause a decrease in the purity of the final cobalt sulfate RC.

[0023] The amount of concentrated sulfuric acid added can be 0.9 to 1.2 gram equivalents relative to the amount of crude cobalt hydroxide HRC used. By adjusting the amount of concentrated sulfuric acid added within this range, cobalt can be sufficiently leached and the amount of excess sulfuric acid (free sulfuric acid) generated can be suppressed. Therefore, the leaching rate of cobalt from the crude cobalt hydroxide slurry can be maintained while suppressing an increase in the cost of recovering cobalt. As a result, cobalt can be efficiently recovered.

[0024] The cobalt in the crude cobalt hydroxide slurry is mostly divalent cobalt, with a small amount of trivalent cobalt present. Divalent cobalt is easier to leach than trivalent cobalt. By adding a reducing agent to the crude cobalt hydroxide slurry, the trivalent cobalt in the crude cobalt hydroxide slurry is converted to divalent cobalt. As a result, the leaching of cobalt is promoted, and the leaching rate of cobalt can be increased to 99% or more.

[0025] As a reducing agent to be added to the crude cobalt hydroxide slurry, 30 to 35% by weight of hydrogen peroxide solution can be used. The amount of hydrogen peroxide solution added can be about 0.04 to 0.2 gram equivalents relative to the amount of crude cobalt hydroxide HRC used.

[0026] The equipment used for leaching the crude cobalt hydroxide slurry is not particularly limited, and a commonly used vessel equipped with an agitator and provided with an acid-resistant lining will suffice.

[0027] [Impurity separation process S2] In the impurity separation step S2, cobalt and impurities in the leaching slurry ES are separated to obtain a cobalt concentrated solution CCL. As shown in Fig. 2, the impurity separation step S2 includes an Fe removal step S21, an Al removal step S22, a Cu removal step S23, a Mn removal step S24, a Ni removal step S25, a Mg removal step S26, and a Co recovery step S27. In this embodiment, the Mn depletion step S24, the Ni depletion step S25, and the Mg depletion step S26 are collectively referred to as a solvent extraction step. It is preferable that the solvent extraction step is performed in this order: the Mn depletion step S24, the Ni depletion step S25, and the Mg depletion step S26.

[0028] The hydroxide precipitation method is adopted in the Fe removal process S21, the Aluminium removal process S22, and the Co recovery process S27. The main objects of separation are iron in the Fe removal process S21, aluminum in the Aluminium removal process S22, and cobalt in the Co recovery process S27. The Cu removal process S23 employs the sulfide precipitation method, with copper being the main target for separation.

[0029] In the Mn depletion step S24, Ni depletion step S25, and Mg depletion step S26 (solvent extraction step), emulsion flow is adopted, but the scope of the present invention is not limited to this. In the Mn depletion step S24, manganese, calcium, and zinc are mainly separated, in the Ni depletion step S25, nickel is mainly separated, and in the Mg depletion step S26, magnesium is mainly separated.

[0030] The Fe depletion step S21, the Al depletion step S22, the Cu depletion step S23, the Mn depletion step S24, the Ni depletion step S25, the Mg depletion step S26, and the Co recovery step S27 included in the impurity separation step S2 will be described in detail below.

[0031] [Fe removal process S21] A neutralizing agent is added to the leaching slurry ES obtained in the leaching step S1 to adjust the pH to a range of 2.0 to 3.0. The temperature of the leaching slurry ES is maintained at 90°C or higher, and the reaction time is 3 to 5 hours. 3+ is preferentially neutralized and precipitates as hydroxide, forming a slurry. The slurry is subjected to solid-liquid separation to obtain neutralized liquid A and neutralized residue A. Neutralized residue A is discarded.

[0032] As a neutralizing agent to be added to the leaching slurry ES, a calcium carbonate slurry of about 25% by weight can be used.

[0033] If the pH of the leaching slurry ES is less than 2.0, iron precipitation is insufficient. If the pH of the leaching slurry ES is more than 3.0, undesired elements such as cobalt are also precipitated, and the amount of neutralizing agent added becomes excessive, resulting in increased costs. Therefore, in the Fe removal step S21, it is preferable to adjust the pH of the leaching slurry ES to a range of 2.0 to 3.0.

[0034] If the temperature of the leaching slurry ES is less than 90° C., the reaction rate is slow and it takes a long time to form hydroxides. Therefore, in the Fe removal step S21, it is preferable to maintain the temperature of the leaching slurry ES at 90° C. or higher.

[0035] The solid-liquid separation device used in the Fe removal step S21 is not particularly limited, and a filtration device such as a filter press can be used. The filtration device may be any device other than a filter press as long as it can separate solids and water.

[0036] [Al removal process S22] A neutralizing agent is added to the neutralization liquid A after the Fe removal step S21 to adjust the pH to a range of 5.0 to 6.0. The temperature of the neutralization liquid A is maintained at 50°C or higher, and the reaction time is 1.5 to 3.5 hours. The aluminum contained in the neutralization liquid A is preferentially neutralized and precipitates as hydroxide, forming a slurry. The slurry is subjected to solid-liquid separation to obtain neutralization liquid B and neutralization residue B.

[0037] Neutralized residue B obtained in the Al removal step S22 contains a small amount of cobalt. By returning neutralized residue B to the leaching slurry ES and dissolving it, a decrease in the cobalt yield can be prevented.

[0038] As the neutralizing agent to be added to the neutralizing solution A, a calcium hydroxide slurry of about 25% by weight can be used.

[0039] If the pH of the neutralizing solution A is less than 5.0, the precipitation of aluminum will be insufficient. If the pH of the leaching slurry is more than 6.0, the co-precipitation of cobalt will be excessive, and the amount of neutralizing agent added will be excessive, resulting in increased costs. Therefore, in the Al removal step S22, it is preferable to adjust the pH of the neutralizing solution A to the range of 5.0 to 6.0.

[0040] If the temperature of neutralization solution A is less than 50° C., the reaction rate is slow and it takes time to form hydroxide. Therefore, in the Al removal step S22, it is preferable to maintain the temperature of neutralization solution A at 50° C. or higher.

[0041] The solid-liquid separation device used in the Al removal step S22 is not particularly limited, but a sedimentation thickening device such as a thickener can be used. The sedimentation thickening device may be any device other than a thickener as long as it can produce a concentrated slurry.

[0042] [Cu removal process S23] A sulfurizing agent is added to the neutralized liquid B after the Al removal step S22, and the reaction is carried out for about 0.5 hours. The oxidation-reduction potential (ORP, based on an Ag / AgCl electrode) is adjusted to be -200 to 100 mV. The copper contained in the neutralized liquid B is sulfurized and precipitated as a sulfide, forming a slurry. The slurry is subjected to solid-liquid separation to obtain a sulfurized liquid and a sulfurized residue.

[0043] The sulfurized residue obtained in the Cu removal step S23 contains a small amount of cobalt. By returning the sulfurized residue to the leaching slurry ES and dissolving it, a decrease in the cobalt yield can be prevented.

[0044] An aqueous solution of sodium hydrogen sulfide at about 10% by weight can be used as the sulfiding agent to be added to the neutralization liquid B. The sodium derived from the sulfiding agent remains in the extract B of the Ni removal step S25 and the extract C of the Magnesium removal step S26, which will be described later, and is finally transferred to the wastewater treatment step.

[0045] If the oxidation-reduction potential of neutralizing solution B exceeds 100 mV, the precipitation of copper becomes insufficient. If the oxidation-reduction potential of neutralizing solution B is less than -200 mV, unintended elements such as cobalt are also precipitated, and the amount of sulfurizing agent added becomes excessive, resulting in increased costs. Therefore, in the Cu removal step S23, it is preferable to adjust the oxidation-reduction potential of neutralizing solution B to the range of -200 to 100 mV.

[0046] The solid-liquid separation device used in the Cu removal step S23 is not particularly limited, but a sedimentation thickening device such as a thickener can be used. The sedimentation thickening device may be any device other than a thickener as long as it can produce a concentrated slurry.

[0047] In this way, the hydroxide precipitation methods in the Fe depletion step S21 and the Al depletion step S22 and the sulfide precipitation method in the Cu depletion step S23 mainly separate the iron, aluminum, and copper from the leaching slurry. Impurities such as manganese, calcium, zinc, magnesium, and nickel that may be contained in the sulfide solution after the Cu depletion step are difficult to separate using the hydroxide precipitation method or the sulfide precipitation method, and are separated by carrying out the solvent extraction steps (Mn depletion step S24, Ni depletion step S25, and Mg depletion step S26) described below. Note that sodium hydroxide is used as a pH adjuster in the solvent extraction steps according to this embodiment.

[0048] [Mn removal process S24] (solvent extraction process) In the manganese removal step S24, when the sulfide solution (aqueous phase) is brought into contact with an organic solvent A (organic phase) containing a phosphate ester extractant, a pH adjuster is added to adjust the pH of the aqueous phase to 1.5 to 2.5. Manganese, calcium, and zinc in the aqueous phase are selectively extracted into the organic phase, and an extract A containing concentrated cobalt, magnesium, and nickel is obtained. At this time, not only manganese, calcium, and zinc but also a small amount of cobalt is extracted into the organic phase.

[0049] If the pH of the aqueous phase is less than 1.5 or more than 2.5, the difference between the extraction rates of manganese, calcium, and zinc and that of cobalt becomes small, making separation difficult. Therefore, it is preferable to adjust the pH of the aqueous phase to 1.5 to 2.5.

[0050] As the pH adjuster, a sodium hydroxide solution of about 15% by weight is used. The sodium derived from the pH adjuster remains in the extract B of the Ni removal step S25 and the extract C of the Mg removal step S26 described below, and is finally transferred to the wastewater treatment step.

[0051] As the phosphate extractant, it is preferable to use bis(2-ethylhexyl)phosphate, which has high extractability for manganese, calcium, zinc, etc.

[0052] The manganese removal step S24 is carried out by contacting the above-mentioned extractant with an organic solvent A (organic phase) prepared by diluting the extractant with a hydrocarbon solvent with the sulfurization liquid (aqueous phase) while forming an emulsion phase. When using organic solvent A in which the volume ratio of the extractant to the hydrocarbon solvent is adjusted to 1:1, the volume ratio of organic solvent A to the sulfurization liquid is preferably 2.2 or more. In addition, aromatic, paraffinic, and naphthenic solvents can be used as the hydrocarbon solvent, and among them, naphthenic solvents are preferably used.

[0053] The organic phase after extraction contains cobalt as well as manganese, calcium, and zinc. By contacting the organic phase after extraction with dilute sulfuric acid (aqueous phase) while forming an emulsion phase, manganese, calcium, zinc, and cobalt in the organic phase are stripped into dilute sulfuric acid to obtain stripped liquid A. When using organic solvent A in which the volume ratio of the extractant to the hydrocarbon solvent is adjusted to 1:1, the volume ratio of the organic phase after extraction to the dilute sulfuric acid is preferably 2.2 or more. The organic phase after stripping can be repeatedly used in the Mn removal step S24. Repeated use of the organic phase can contribute to cost reduction. By using emulsion flow for the extraction and back-extraction in the Mn removal step S24, the extractant concentration in the organic phase can be reduced and the flow rate ratio of the organic phase to the aqueous phase can be increased compared to when a mixer-settler is used, so that hydroxide precipitation can be suppressed even when sodium hydroxide is used as a pH adjuster.

[0054] The apparatus used in the Mn removal step S24 may be an emulsion flow apparatus equipped with a mechanical stirring blade, but the scope of the present invention is not limited to this.

[0055] [Ni removal process S25] (solvent extraction process) In the Ni removal step S25, when the extract A (aqueous phase) is contacted with the organic solvent B (organic phase) containing the phosphinic acid ester extractant, a pH adjuster is added to adjust the pH of the aqueous phase to a range of 4.0 to 4.3. This allows the cobalt and magnesium in the aqueous phase to be selectively extracted into the organic phase, and an extract B containing concentrated nickel is obtained. The extract B is then discharged.

[0056] If the pH of the aqueous phase is less than 4.0 or more than 4.3, the difference between the extraction rates of nickel and cobalt becomes small, making separation difficult, so it is preferable to adjust the pH of the aqueous phase to 4.0 to 4.3.

[0057] As the pH adjuster, a sodium hydroxide aqueous solution of about 15% by weight is used. Sodium derived from the pH adjuster remains in the extract B of the Ni removal step S25 and the extract C of the Mg removal step S26, and is finally discharged.

[0058] As the phosphinic acid ester extractant, it is preferable to use di-(2,4,4-trimethylpentyl)-phosphinic acid, which has high extractability for cobalt and the like.

[0059] The Ni removal step S25 is carried out by contacting the above extractant with an organic solvent B (organic phase) prepared by diluting the extractant with a hydrocarbon solvent while forming an emulsion phase of the extractant and the extractant A (aqueous phase). When using organic solvent B in which the volume ratio of the extractant to the hydrocarbon solvent is adjusted to 3:7, the volume ratio of organic solvent B to the extractant A and the washing liquid B is preferably 8.1 or more. As the hydrocarbon solvent, aromatic, paraffinic, naphthenic solvents, etc. can be used, and among them, naphthenic solvents are preferably used.

[0060] The organic phase after extraction is washed by contacting the organic phase after extraction with an emulsion phase of dilute sulfuric acid (aqueous phase) while forming the emulsion phase, to obtain a post-wash liquid B. When using an organic solvent B in which the volume ratio of the extractant to the hydrocarbon solvent is adjusted to 3:7, the volume ratio of dilute sulfuric acid to the organic phase after extraction is not particularly limited, but is preferably 8.1 or more. The post-wash liquid B contains a small amount of cobalt, and the cobalt yield can be improved by recovering the post-wash liquid B. In addition, by reducing the amount of dilute sulfuric acid used for washing, the amount of cobalt distributed to the post-wash liquid B can be reduced and recovered at a high concentration.

[0061] By contacting the washed organic phase with dilute sulfuric acid (aqueous phase) while forming an emulsion phase, the cobalt and nickel in the organic phase are stripped into dilute sulfuric acid to obtain stripped liquid B. When using organic solvent B in which the volume ratio of the extractant to the hydrocarbon solvent is adjusted to 3:7, the volume ratio of the organic phase after extraction to the dilute sulfuric acid is preferably 8.1 or more. The organic phase after stripping can be repeatedly used in the Ni removal step S25. Repeated use of the organic phase can contribute to cost reduction. By using emulsion flow for the extraction, washing, and back-extraction in the Ni removal process S25, the extractant concentration in the organic phase can be reduced and the flow rate ratio of the organic phase to the aqueous phase can be increased compared to when a mixer-settler is used. This makes it possible to suppress hydroxide precipitation even when sodium hydroxide is used as a pH adjuster.

[0062] The device used in the Ni removal step S25 may be an emulsion flow device equipped with a mechanical stirring blade, but the scope of the present invention is not limited to this.

[0063] [Mg removal process S26] (solvent extraction process) In the magnesium removal step S26, when the stripped liquid B (aqueous phase) is contacted with an organic solvent C (organic phase) containing a carboxylic acid ester extractant, a pH adjuster is added to adjust the pH of the aqueous phase to a range of 5.5 to 7.5. Cobalt in the aqueous phase is selectively extracted into the organic phase to obtain an extract C in which magnesium is concentrated. The extract C is then discharged.

[0064] If the pH of the aqueous phase is less than 5.5 or more than 7.5, the difference between the extraction rates of magnesium and cobalt becomes small, making separation difficult, so it is preferable to adjust the pH of the aqueous phase to 5.5 to 7.5.

[0065] As the pH adjuster, an aqueous solution of sodium hydroxide at about 15% by weight is used. As the carboxylic acid ester extractant, it is preferable to use 9,9-dimethyldecanoic acid, which has high extractability for cobalt and nickel.

[0066] The magnesium removal step S26 is carried out by contacting the above extractant with an organic solvent C (organic phase) prepared by diluting the extractant with a hydrocarbon solvent with the back extraction liquid B (aqueous phase) while forming an emulsion phase. When using an organic solvent C in which the volume ratio of the extractant to the hydrocarbon solvent is adjusted to 4:6, the volume ratio of the organic solvent C to the back extraction liquid B is preferably 3.6 or more. As the hydrocarbon solvent, aromatic, paraffinic, naphthenic solvents, etc. can be used, and among them, naphthenic solvents are preferably used.

[0067] Most of the cobalt in the reverse extraction liquid B is extracted into the organic phase. The organic phase after extraction is washed by contacting the organic phase after extraction with an emulsion phase of dilute sulfuric acid (aqueous phase) while forming the emulsion phase, to obtain a washed liquid C. When using an organic solvent C in which the volume ratio of the extractant to the hydrocarbon solvent is adjusted to 4:6, the volume ratio of dilute sulfuric acid to the organic phase after extraction is not particularly limited, but is preferably 3.6 or more. The washed liquid C contains a small amount of cobalt, and the cobalt yield can be improved by recovering the washed liquid C. In addition, by reducing the amount of dilute sulfuric acid used for washing, the amount of cobalt distributed to the washing liquid C can be reduced and recovered at a high concentration.

[0068] By contacting the washed organic phase with dilute sulfuric acid (aqueous phase) while forming an emulsion phase, the cobalt in the organic phase is stripped into dilute sulfuric acid to obtain stripped liquid B1. When using organic solvent C in which the volume ratio of the extractant to the hydrocarbon solvent is adjusted to 4:6, the volume ratio of the organic phase after extraction to the dilute sulfuric acid is preferably 3.6 or more. The organic phase after stripping can be repeatedly used in the Mg removal step S26. Repeated use of the organic phase can contribute to cost reduction. By using emulsion flow for the extraction, washing, and back-extraction in the magnesium removal step S26, the extractant concentration in the organic phase can be reduced and the flow rate ratio of the organic phase to the aqueous phase can be increased compared to when a mixer-settler is used, so that hydroxide precipitation can be suppressed even when sodium hydroxide is used as a pH adjuster.

[0069] The apparatus used in the magnesium removal step S26 may be an emulsion flow apparatus equipped with a mechanical stirring blade, but the scope of the present invention is not limited to this.

[0070] [Co recovery process S27] The stripped liquid A obtained from the Mn removal step S24 contains manganese, calcium, zinc, and cobalt. A neutralizing agent is added to stripped liquid A to adjust the pH to a range of 8.2 to 8.8. The temperature of stripped liquid A is maintained at 50°C or higher, and the reaction time is 1 to 3 hours. Cobalt contained in stripped liquid A is preferentially neutralized and precipitates as a hydroxide, forming a slurry. The slurry is subjected to solid-liquid separation to obtain neutralized liquid C and neutralized residue C. The neutralized liquid C is discharged.

[0071] Neutralization residue C contains cobalt. By returning neutralization residue C to the leaching slurry and dissolving it, it is possible to prevent a decrease in the cobalt yield.

[0072] As a neutralizing agent, a sodium hydroxide solution of about 25% by weight can be used. The sodium derived from the pH adjuster remains in the extract B of the Ni removal step S25 and the extract C of the Magnesium removal step S26, and is finally transferred to the wastewater treatment step.

[0073] If the pH of the back extraction solution A is less than 8.2, the precipitation of cobalt becomes insufficient. If the pH of the back extraction solution A is more than 8.8, the coprecipitation of manganese becomes excessive, and the amount of neutralizing agent added becomes excessive, resulting in an increase in costs. Therefore, in the Co recovery step S27, it is preferable to adjust the pH of the back extraction solution A to the range of 8.2 to 8.8.

[0074] If the temperature of the back-extracted liquid A is less than 50° C., the reaction rate is slow and it takes time to form hydroxides. Therefore, in the Co recovery step S27, it is preferable to maintain the temperature of the back-extracted liquid A at 50° C. or higher.

[0075] The solid-liquid separation device used in the Co recovery step S27 is not particularly limited, but a sedimentation thickening device such as a thickener can be used. The sedimentation thickening device may be any device other than a thickener as long as it can produce a concentrated slurry.

[0076] [Crystallization process S3] In the crystallization step S3, cobalt sulfate RC is obtained from the cobalt concentrated liquid CCL. The apparatus used in the crystallization step S3 is not particularly limited, but a cooling crystallizer can be used. An example of the general components of the cobalt sulfate RC obtained after the crystallization step S3 is the composition and components shown in Table 2 below. In Table 2, the content of each component is shown in mass%.

[0077] [Table 2]

[0078] By using the above process to produce cobalt sulfate RC from crude cobalt hydroxide HRC, the cobalt yield can be increased to 92% or more. If the filtrate from the cooling crystallizer is reused, the cobalt yield can be increased to 97% or more. EXAMPLES

[0079] The present invention will be described in detail below with reference to examples. However, the conditions in the examples are merely examples of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to these examples. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.

[0080] (Example) [Leaching process] Crude cobalt hydroxide and pure water were added to a beaker so that the slurry concentration was 30%, and the mixture was stirred to obtain a crude cobalt hydroxide slurry. The components of the crude cobalt hydroxide are shown in Table 3 below. In Table 3, the contents of each metal component other than Co are shown as relative mass ratios to Co.

[0081] [Table 3]

[0082] Hydrogen peroxide (concentration 34.5% by mass) and concentrated sulfuric acid were added to crude cobalt hydroxide slurry with a slurry concentration of 30% under normal pressure. Leaching was performed under conditions of a reaction temperature of 98°C and a reaction time of 0.5 hours to obtain a leached slurry containing cobalt, iron, copper, aluminum, manganese, calcium, zinc, nickel, and magnesium. The leaching rate of cobalt was 99.9%. The amount of concentrated sulfuric acid added was 1.1 gram equivalents relative to the amount of crude cobalt hydroxide used. The amount of hydrogen peroxide added was 0.15 gram equivalents relative to the amount of crude cobalt hydroxide used.

[0083] [Fe removal process] Calcium carbonate slurry (concentration 25% by weight) was added to the leaching slurry, and the pH was adjusted to 3.0. A slurry was formed by neutralizing the mixture at a reaction temperature of 95°C for a reaction time of 4 hours. The slurry was subjected to solid-liquid separation using a suction filtration device to obtain neutralized liquid A and neutralized residue A. All of the iron in the leaching slurry was separated into neutralized residue A. Neutralized residue A was discarded. A commonly used suction filtration device consisting of filter paper, a Büchner funnel, a filtration bottle, a vacuum pump, etc. was used.

[0084] [Al removal process] A calcium hydroxide slurry (concentration 25% by weight) was added to neutralization solution A to adjust the pH to 5.0. Neutralization was performed at a reaction temperature of 50°C for a reaction time of 2.5 hours to form a slurry. The slurry was subjected to solid-liquid separation in a thickener to obtain neutralization solution B and neutralization residue B. All of the aluminum in neutralization solution A was separated into neutralization residue B. Neutralization residue B was returned to the leaching slurry and dissolved.

[0085] [Cu removal process] An aqueous solution of sodium hydrogen sulfide (concentration 10% by weight) was added to neutralization solution B. Sulfurization was carried out under conditions of an oxidation-reduction potential of 100 mV and a reaction time of 0.5 hours, resulting in the formation of a slurry. The slurry was subjected to solid-liquid separation in a thickener to obtain a sulfurization solution and a sulfurization residue. All of the copper in neutralization solution B was separated into the sulfurization residue. The sulfurization residue was returned to the leaching slurry and dissolved therein.

[0086] The components of the sulfurizing solution were as shown in Table 4 below. In Table 4, the content of each metal component other than Co is shown as a relative mass ratio to Co.

[0087] [Table 4]

[0088] [Mn removal process] (solvent extraction process) Organic solvent A (organic phase) was prepared by mixing the extractant "bis(2-ethylhexyl) phosphate: D2EHPA" with the diluent "Exxol D80 (manufactured by ExxonMobil)" in a volume ratio of 1:1. A sodium hydroxide solution (concentration 15% by weight) was added to the sulfide solution (aqueous phase) to adjust the pH to 2.2. Using an emulsion flow device equipped with a mechanical stirring blade, 11 stages of extraction were performed in which the organic phase and the pH-adjusted aqueous phase were contacted in a volume ratio of 2.2:1, and 4 stages of back extraction were performed in which the organic phase after extraction was contacted with dilute sulfuric acid (concentration 150g / L) in a volume ratio of 2.2:1, to obtain extract A and back extraction solution A. At this time, more than 99.9% of the manganese in the sulfide solution was distributed to back extraction solution A. The entire amount of calcium and zinc in the sulfide solution was distributed to back extraction solution A. In addition, back extraction solution A contained 5g / L of cobalt.

[0089] [Ni removal process] (solvent extraction process) Organic solvent B (organic phase) was prepared by mixing the extractant "Di-(2,4,4-trimethylpentyl)-phosphinic acid: CYANEX272 (Cytec Industries Inc.)" with the diluent "Exxol D80 (ExxonMobil)" in a volume ratio of 3:7. Sodium hydroxide solution (concentration 15% by weight) was added to the extract A (aqueous phase) to adjust the pH to 4.0. Using an emulsion flow device equipped with a mechanical stirring blade, seven stages of extraction were performed in which the organic phase and the pH-adjusted aqueous phase were contacted in a volume ratio of 8.1:1, two stages of washing were performed in which the organic phase after extraction was contacted with dilute sulfuric acid (concentration 100 g / L) in a volume ratio of 8.1:1, and three stages of back extraction were performed in which the organic phase after washing was contacted with dilute sulfuric acid (concentration 100 g / L) in a volume ratio of 8.1:1, to obtain extract B, post-wash liquid B, and back-extraction liquid B. At this time, 99% or more of the cobalt and 99.9% or more of the nickel in the extract A were distributed to the back-extraction liquid B. 99% of the sodium derived from the sulfiding agent used in the Cu removal process, the sodium derived from the pH adjuster in the Mn removal and Ni removal processes, and the sodium derived from the neutralizing agent used in the Co recovery process were distributed to the extract B.

[0090] [Mg removal process] (solvent extraction process) Organic solvent C (organic phase) was prepared by mixing the extractant "9,9-dimethyldecanoic acid: Versatic acid-10 (Hexion Management (Shanghai) Co., Ltd.)" with the diluent "Exxol D80 (ExxonMobil)" in a volume ratio of 4:6. Sodium hydroxide solution (concentration 15% by weight) was added to the back extraction liquid B (aqueous phase) to adjust the pH to 5.95. Using an emulsion flow device equipped with a mechanical stirring blade, seven stages of extraction were performed in which the organic phase and the pH-adjusted aqueous phase were contacted in a volume ratio of 3.6:1, five stages of washing were performed in which the organic phase after extraction was contacted with dilute sulfuric acid (concentration 100g / L) in a volume ratio of 3.6:1, and three stages of back extraction were performed in which the organic phase after washing was contacted with dilute sulfuric acid (concentration 300g / L) in a volume ratio of 3.6:1, to obtain extract liquid C and a cobalt concentrate. At this time, 99.9% or more of the cobalt in the back extraction solution B was distributed to the cobalt concentrated solution. The sodium derived from the pH adjuster used in the magnesium removal process and 99.9% of the sodium in the back extraction solution B were distributed to the extraction solution C. The extraction solution C was transferred to the wastewater treatment process.

[0091] [Co recovery process] Aqueous sodium hydroxide solution (concentration 25% by weight) was added to the back extraction liquid A to neutralize the free sulfuric acid, and then calcium hydroxide slurry (concentration 25% by weight) was added to adjust the pH to 8.6. A slurry was formed by neutralizing the solution at a reaction temperature of 50°C for a reaction time of 2 hours. The slurry was subjected to solid-liquid separation using a suction filtration device to obtain neutralized solution C and neutralized residue C. All of the cobalt in the back extraction liquid A was separated into neutralized residue C. Neutralized solution C was discharged. A commonly used suction filtration device consisting of filter paper, a Büchner funnel, a filtration bottle, a vacuum pump, etc. was used. Neutralized residue C was returned to the leaching slurry and dissolved.

[0092] [Crystallization process] The cobalt concentrated solution was crystallized in a cooling crystallizer to obtain cobalt sulfate. The components of the cobalt sulfate obtained by the manufacturing method of the example are shown in Table 5 below. In Table 5, the content of each component is shown in mass%.

[0093] [Table 5]

[0094] The cobalt yield (the ratio of the mass of cobalt in the cobalt sulfate produced per unit time to the mass of cobalt in the crude cobalt hydroxide used per unit time) of the above manufacturing method was 92.2%. Furthermore, by reusing the filtrate generated from the cooling crystallizer, the cobalt yield was increased to 97.2%.

[0095] (Comparative Example) As shown in Fig. 3, the Comparative Example includes a leaching step, an Fe removal step, an Al removal step, a Cu removal step, a Mn removal step, a Mg removal step, a Ni removal step, a Co recovery step, and a crystallization step in obtaining cobalt sulfate from crude cobalt hydroxide. The leaching step, the Fe removal step, the Al removal step, the Cu removal step, the Co recovery step, and the crystallization step in the Comparative Example are similar to those in the Example. The Mn removal step, the Mg removal step, and the Ni removal step in the Comparative Example are different from those in the Example in that the solvent extraction step is performed in this order and that ammonia water is used as a pH adjuster.

[0096] The composition of the cobalt sulfate obtained by the manufacturing method of the Comparative Example was equivalent to that of the cobalt sulfate obtained by the manufacturing method of the Example. Also, the cobalt yield by the manufacturing method of the Comparative Example was equivalent to that of the Example. The Mn removal step, the Mg removal step, and the Ni removal step in the comparative example will be described below.

[0097] [Mn removal process] The organic solvent (organic phase) was prepared by mixing the extractant "bis(2-ethylhexyl) phosphate: D2EHPA" with the diluent "Exxol D80 (manufactured by ExxonMobil)" in a volume ratio of 4:1. Ammonia water (concentration 30 wt%) was added to the sulfide solution (aqueous phase) to adjust the pH to 2.2. Using a mixer settler, 12 stages of extraction were performed in which the organic phase and the pH-adjusted aqueous phase were contacted in a volume ratio of 1 to 1.1:1, two stages of first stripping were performed in which the organic phase after extraction was contacted with the stripping solution obtained after the second stripping step of the demagnesium process described below in a volume ratio of 10 to 11:1, and one stage of second stripping was performed in which the organic phase after the first stripping was contacted with dilute sulfuric acid (concentration 150 g / L) in a volume ratio of 10 to 11:1. The stripping solution obtained after the first stripping was used in the Co recovery step. The stripping solution obtained after the second stripping was returned to the leaching step.

[0098] [Mg removal process] The organic solvent (organic phase) was prepared by mixing the extractant "9,9-dimethyldecanoic acid: Versatic acid-10 (Hexion Management (Shanghai) Co., Ltd.)" with the diluent "Exxol D80 (ExxonMobil)" in a volume ratio of 1:1. Ammonia water (concentration 30% by weight) was added to the extract (aqueous phase) obtained in the Mn removal process, and the pH was adjusted to 6.25. Using a mixer settler, five stages of extraction were performed in which the organic phase and the pH-adjusted aqueous phase were contacted at a volume ratio of 1.4:1, two stages of first washing in which the organic phase after extraction was contacted with dilute sulfuric acid (concentration 150g / L) at a volume ratio of 9:1, two stages of second washing, two stages of first stripping in which the organic phase after the second washing was contacted with the stripping solution obtained after the second stripping in the Ni removal process described below at a volume ratio of 2:1, and one stage of second stripping in which the organic phase after the first stripping was contacted with dilute sulfuric acid (concentration 150g / L) at a volume ratio of 2:1. The extract obtained after the extraction was subjected to wastewater treatment accompanied by ammonia recovery. The stripping solution obtained after the second stripping was used for the first stripping in the Mn removal process described above.

[0099] [Ni removal process] The organic solvent (organic phase) was prepared by mixing the extractant "Di-(2,4,4-trimethylpentyl)-phosphinic acid: CYANEX272 (Cytec Industries Inc.)" with the diluent "Exxol D80 (ExxonMobil)" in a volume ratio of 1:1. Ammonia water (concentration 30% by weight) was added to the stripped liquid (aqueous phase) obtained in the first stripping step of the magnesium removal process to adjust the pH to 4.6. Using a mixer settler, six stages of extraction were performed in which the organic phase and the pH-adjusted aqueous phase were contacted in a volume ratio of 2.4:1, two stages of first stripping were performed in which the organic phase after the extraction was contacted with dilute sulfuric acid (concentration 150 g / L) in a volume ratio of 3.4:1, and one stage of second stripping was performed in which the organic phase after the first stripping was contacted with dilute sulfuric acid (concentration 150 g / L) in a volume ratio of 2.4:1. The extract obtained after the extraction was subjected to wastewater treatment with ammonia recovery. The strip solution obtained after the second stripping was used in the first stripping step of the magnesium removal process. The cobalt-enriched solution obtained after the first stripping step was used in the crystallization process.

[0100] The differences in the solvent extraction steps between the Examples and Comparative Examples and their impact on costs are explained using Table 6 below. Note that the Roman numerals in parentheses in the Comparative Examples in Table 6 indicate the ordinal numbers of each step. For example, (i) in Washing indicates the first wash.

[0101] [Table 6]

[0102] The order of the solvent extraction steps in the examples is Mn depletion step, Ni depletion step, Mg depletion step, whereas the solvent extraction steps in the comparative examples are Mn depletion step, Mg depletion step, Ni depletion step. The reason for changing the order of the Ni depletion step and the Mg depletion step is that if the Mg depletion step, which is a non-chelating extraction system, is made the final step in the examples, the ammonium ions derived from the ammonia water used in the Mg depletion step will be mixed into the product without being separated. In the solvent extraction of the examples, ammonia water is not used as a pH adjuster, so it is possible to make the Mg depletion step the final step. In addition, since it is easy to separate and remove sodium in the aqueous phase in the Mg depletion step, making the Mg depletion step the final step is also rational from the viewpoint of sodium removal.

[0103] In the solvent extraction of the examples, emulsion flow was used, making it possible to send the solution at a high O / A ratio without compromising phase separation. As a result, we succeeded in changing the pH adjuster to a sodium hydroxide aqueous solution and miniaturizing the solvent extraction device. By miniaturizing the solvent extraction device, we succeeded in reducing the initial cost of the organic solvent (liquid filling amount) required in the examples by 75% compared to the comparative example.

[0104] Furthermore, because the solvent extraction in the examples used emulsion flow, it was possible to use an aqueous sodium hydroxide solution as a pH adjuster. When using an aqueous sodium hydroxide solution as a pH adjuster, the extractant concentration in the organic phase was lowered and the flow rate ratio of the organic phase to the aqueous phase was increased in order to suppress hydroxide precipitation while maintaining reaction efficiency. By changing the pH adjuster, we succeeded in reducing the cost of the pH adjuster by 7% compared to the comparative example. In addition, ammonia recovery equipment was no longer necessary, which greatly contributed to cost reduction. [Explanation of symbols]

[0105] HRC... crude cobalt hydroxide, ES... leaching slurry, CCL... cobalt concentrate, RC... cobalt sulfate, S1... leaching process, S2... impurity separation process, S3... crystallization process, S21... Fe removal process, S22... Al removal process, S23... Cu removal process, S24... Mn removal process, S25... Ni removal process, S26... Magnesium removal process, S27... Co recovery process.

Claims

1. 1. A method for producing cobalt sulfate from crude cobalt hydroxide containing one or more impurity elements selected from the group consisting of iron, copper, aluminum, manganese, calcium, zinc, nickel and magnesium, comprising the steps of:

1. A method for producing cobalt sulfate, comprising: forming an emulsion phase between an aqueous phase and an organic phase based on a continuous process in which a volume ratio and a flow rate ratio between the aqueous phase and the organic phase are adjusted; and using an aqueous sodium hydroxide solution as a pH adjuster.

2. 2. The method for producing cobalt sulfate according to claim 1, wherein the emulsion phase is formed using a mechanical stirring blade.

3. 2. The method for producing cobalt sulfate according to claim 1, wherein the solvent extraction step is carried out in the order of a Mn removal step, a Ni removal step, and a Mg removal step.

4. 3. The method for producing cobalt sulfate according to claim 2, wherein the solvent extraction step is carried out in the order of a Mn removal step, a Ni removal step, and a Mg removal step.

5. The method for producing cobalt sulfate according to any one of claims 1 to 3, characterized in that no ammonia water is used as the pH adjuster.

6. 5. The method for producing cobalt sulfate according to claim 4, wherein no ammonia water is used as the pH adjuster.

Citation Information

Patent Citations

  • Method for producing high-purity cobalt sulfate solution and method for producing cobalt sulfate

    JP2021063281A

  • Production method of cobalt sulfate

    JP2022104563A

  • Method for producing cobalt sulfate

    JP2022191115A

  • Liquid-liquid system multistage device, and method for manufacturing specific substance using the same

    JP2022164276A