Method for manufacturing stainless steel strip

A multi-step cold rolling and pickling process with controlled rolling rates and surface roughness addresses the issue of scab marks and inclusions in thin stainless steel strips, enhancing surface quality.

JP2024142901APending Publication Date: 2024-10-11PROTERIAL LTD

Patent Information

Application Number
JP2023055294
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods fail to effectively reduce the occurrence of scab marks and inclusions in thin stainless steel strips, which are prone to surface defects like scratches and acid pits, especially during the manufacturing process.

Method used

A multi-step cold rolling and pickling process is employed, including first and second cold rolling steps with specific reduction rates, followed by pickling and recrystallization annealing, using rolling rolls with controlled surface roughness to remove inclusions and surface defects.

Benefits of technology

The method significantly reduces the occurrence of scab marks and improves surface quality by effectively removing inclusions and surface defects in thin stainless steel strips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142901000001_ABST
    Figure 2024142901000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a stainless steel strip which can reduce the generation of a scab even in a thin stainless steel strip containing inclusions.SOLUTION: This method for manufacturing a stainless steel strip includes a first cold rolling process for executing cold rolling of a rolling reduction 50 - 80% by preparing a cold-rolling strip material of a thickness 1 mm or less, an acid cleaning process for performing acid cleaning on a cold rolling face of the intermediate cold rolling material to obtain an acid cleaning treatment material, and a second cold rolling process for performing cold rolling of a rolling reduction 50 - 90% on the acid cleaning treatment material to obtain a stainless steel strip of a thickness 0.1 mm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a stainless steel strip. [Background technology]

[0002] Stainless steel strips containing 10.5% or more Cr by mass have good mechanical properties and corrosion resistance, and are therefore used in a variety of fields, including switch materials, corrosion-resistant springs, inkjet heads, and suspension springs for HDDs. In order to improve the surface gloss, corrosion resistance, and adhesion of this stainless steel, it is required to remove surface defects as much as possible to achieve high-quality surface properties.

[0003] One of the surface defects formed during the production of stainless steel strips is known to be a defect called a scab, which extends along the rolling direction of the steel strip. As described above, the scab is a factor that deteriorates the surface properties, and therefore various studies have been conducted in the past to remove the scab. For example, Patent Document 1 describes that in order to remove scabs efficiently and at low cost, surface defects such as scabs and grain boundary grooves present on the surface of a stainless steel sheet that has been descaled after hot rolling are removed by pickling with a mixed acid aqueous solution.

[0004] Patent Document 2 describes a method for producing an austenitic stainless steel sheet with excellent surface properties, characterized in that when a steel material for an austenitic stainless steel sheet is extracted from a heating furnace, hot rolled, then cold rolled, and then finish annealed to produce an austenitic stainless steel sheet, the temperature at which the steel material is extracted from the heating furnace is adjusted in accordance with the Sn content of the steel material, in order to reduce scab defects formed by hot cracking. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2000-144461 A [Patent Document 2] JP 2003-147439 A Summary of the Invention [Problem to be solved by the invention]

[0006] Besides the above-mentioned hot cracks, the cause of scabs may also be inclusions (precipitates) present on the surface of the steel strip. In particular, when stainless steel is produced into slabs by continuous casting, scabs caused by such inclusions tend to occur easily. The technology described in Patent Document 1 is an invention useful for removing scabs, but it is intended for thick plate materials with a plate thickness of about 1.8 mm after cold rolling. The thinner the plate material, the more likely it is that even a small defect will cause a decrease in strength. Patent Document 2 is an invention that suppresses scabs caused by hot cracks by adjusting the heating temperature according to the Sn content, but does not disclose a method for suppressing scabs caused by inclusions. As a method for reducing scabs caused by inclusions, it is possible to add a deoxidizing agent in the melting process or adjust the melting method to reduce the inclusions themselves, but there is a concern that this will increase manufacturing costs. Therefore, an object of the present invention is to provide a method for producing a stainless steel strip that can reduce the occurrence of scab defects even in a thin stainless steel strip containing inclusions. [Means for solving the problem]

[0007] The present invention has been made in view of the above-mentioned problems. That is, the present invention is a method for producing a stainless steel strip, comprising a first cold rolling step of preparing a cold rolling strip having a thickness of 1 mm or less and cold rolling it at a rolling reduction of 50 to 80%, a pickling step of pickling the cold rolled surface of the intermediate cold rolled strip to obtain a pickled material, and a second cold rolling step of cold rolling the pickled material at a rolling reduction of 50 to 90% to obtain an iron-based alloy strip having a thickness of 0.1 mm or less. Preferably, in the pickling step, the intermediate cold rolled material is pickled so that the loss amount is 3 to 7 μm. Preferably, the second cold rolling process includes an intermediate cold rolling process in which an intermediate cold rolled material is obtained by rolling at a reduction ratio of 50% or more, a recrystallization annealing process in which the intermediate cold rolled material is recrystallized annealed to obtain an annealed material, and a finish cold rolling process in which the annealed material is rolled at a reduction ratio of less than 50%, and when the total number of passes in the intermediate cold rolling process is n, the roughness of the rolling rolls used in rolling from the start of the intermediate cold rolling to at least 0.6n passes is 0.1 μm or more in arithmetic mean roughness Ra. Effect of the Invention

[0008] According to the present invention, a stainless steel strip capable of reducing the occurrence of scab defects can be obtained. [Brief description of the drawings]

[0009] [Figure 1] 1 is an enlarged photograph of a surface of a sample of a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. However, the present invention is not limited to the embodiments described here, and appropriate combinations and improvements are possible within the scope of the technical idea of ​​the invention. The present invention is directed to a stainless steel strip. The stainless steel strip can be stainless steel such as ferritic stainless steel, austenitic stainless steel, martensitic stainless steel, austenitic-ferritic stainless steel, and precipitation hardening stainless steel as specified in JIS-G-4305, but it is preferable to target ferritic stainless steel and austenitic stainless steel, which are often manufactured by continuous casting and tend to form carbides aligned in the rolling direction during the process. More preferably, it is directed to austenitic stainless steel.

[0011] In the manufacturing method of this embodiment, first, a stainless steel material for cold rolling is prepared. This material for cold rolling can be produced by subjecting a hot-rolled steel strip after hot rolling to recrystallization annealing and pickling for descaling, and then cold rolling one or more times to adjust the plate thickness. The cold rolling material is preferably 1 mm or less in thickness in order to easily obtain the stainless steel strip having a thickness of 0.1 mm or less that is the subject of the present invention. On the other hand, in order to stably obtain the effect of suppressing scab defects in the pickling process described below, the lower limit of the sheet thickness of the cold rolling material is preferably 0.3 mm or more.

[0012] Next, the cold rolling (first cold rolling process) is performed on the prepared cold rolling material with a rolling reduction of 50 to 80%. By performing this first cold rolling process before the pickling process described later, it is possible to efficiently remove inclusions that cause scab scratches in the pickling process. In particular, in thin plate materials, even if inclusions on the plate surface are removed at the preparation stage, when the plate thickness is reduced by performing the rolling process, inclusions present inside the plate are exposed on the plate surface, causing scab scratches. Therefore, it is important to perform pickling in a state as close as possible to the plate thickness of the final product, as in the first cold rolling process of this embodiment. The lower limit of the rolling reduction is preferably 55%. The lower limit of the rolling reduction is more preferably 70%.

[0013] In this embodiment, the plate material (first cold rolled material) after the first cold rolling is pickled (pickling process). By introducing the pickling process, it is possible to remove the inclusions on the plate material surface that cause scabs by dissolving them or to render them harmless by miniaturizing them. Furthermore, in this pickling process, it is preferable to dissolve the intermediate cold rolled material after pickling so that the loss (dissolution amount) is 3 to 7 μm. By making the loss amount of the cold rolled material by pickling 3 μm or more, the inclusions present in the surface layer of the first cold rolled material can be stably removed. Furthermore, by making the loss amount of the cold rolled material by pickling 7 μm or less, the occurrence of deep acid pits can be suppressed, and the acid pits can be adjusted so that they can be removed in the second cold rolling process described later, and the surface properties can be further improved. Note that, as for the pickling device, a device generally used for pickling steel strips may be used, and for example, a type in which the steel strip is passed through a pickling tank filled with pickling liquid to wash it, or a type in which the pickling liquid is sprayed onto the steel strip surface by a nozzle can be used. Although this pickling process can be performed multiple times, it is preferable to perform it only once in order to suppress the occurrence of acid pits. Here, the amount of wear of the first cold rolled material can be confirmed by measuring the thickness of the plate before pickling and the thickness of the plate after pickling with a hand micrometer. Other pickling conditions such as the plate threading speed and the immersion time can be appropriately adjusted according to the type of stainless steel so as to obtain the above-mentioned amount of wear. In the pickling process of the present invention, pickling is performed on the "rolled surface" of the first cold rolled material. This means that pickling is not performed on the ground surface after mechanical grinding, that is, in the present invention, a mechanical grinding process is not performed between the first cold rolling process and the pickling process. The reason why mechanical grinding is not performed is that the thickness of the steel strip to be targeted in the present invention is thin, and therefore, due to the influence of mechanical grinding, shape defects such as width warping tend to occur in the subsequent rolling. In addition, in order to increase the rolling reduction in the second cold rolling process described later, recrystallization annealing may be performed on the steel strip before or after pickling.

[0014] In this embodiment, the steel strip that has been subjected to the pickling process is subjected to cold rolling at a reduction rate of 50 to 90% (second cold rolling process). By performing the above-mentioned pickling process, inclusions remaining on the surface layer of the steel strip can be removed, but scratches and acid pits formed by the inclusions falling off remain. In particular, steel strips containing carbon, such as stainless steel used in this embodiment, tend to have carbides falling off due to the difference in dissolution between carbides and the parent phase, and acid pits are likely to occur. In this embodiment, by performing the second cold rolling at a reduction rate of 50% or more, it is possible to remove the above-mentioned surface defects such as scratches and acid pits by plastic deformation due to strong reduction. If the reduction rate is less than 90%, the removal of scratches by plastic deformation only works on the very surface layer of the steel strip, so there is a problem that the surface defects cannot be completely removed and remain. The preferable lower limit of the reduction rate is 55%, and the preferable upper limit of the reduction rate is 85%. The reduction ratio of the finish cold rolling indicates the total reduction ratio. Therefore, the specified reduction ratio may be achieved in one pass, or may be achieved by performing multiple passes of rolling. In particular, in the case of a thin plate such as that of the present invention, the effect of work hardening is significant, so it is preferable to perform 10 passes or more of rolling, and one or more recrystallization annealing may be performed during rolling.

[0015] In the second cold rolling process of this embodiment, it is preferable to include an intermediate cold rolling process in which an intermediate cold rolled material is obtained by rolling at a reduction rate of 50% or more, a recrystallization annealing process in which the intermediate cold rolled material is recrystallized and annealed to obtain an annealed material, and a finish cold rolling process in which the annealed material is rolled at a reduction rate of less than 50%. In addition, when the total number of passes in the intermediate cold rolling process is n, it is preferable that the roughness of the rolling roll used in rolling from the start of the intermediate cold rolling to at least 0.6n passes (surface roughness measured in a direction perpendicular to the circumferential direction of the roll) is 0.1 μm or more in arithmetic mean roughness Ra. This can further improve the ability to remove surface defects, and in particular, it is effective in improving surface properties because rolling pits are easily removed by rolling processing. More preferably, the roughness of the rolling roll used in rolling up to 0.6n passes is 0.2 μm or more in Ra. In this embodiment, rolling rolls with Ra 0.1 μm or more may be used in all passes of intermediate cold rolling, or at least one pass of rolling using rolling rolls with an arithmetic mean roughness Ra of less than 0.1 μm may be combined. Note that the number of passes "0.6n" mentioned above is rounded off to the nearest integer. For example, when n is 6 passes, 0.6n = 3.6, so rolling rolls with an arithmetic mean roughness Ra of 0.1 μm or more may be used from the start of intermediate cold rolling to the fourth pass.

[0016] In the present embodiment, the finish cold rolling after the recrystallization annealing is preferably performed with a roll having a surface roughness of less than 0.1 μm in terms of arithmetic mean roughness Ra of the roll used in the final pass. This allows the surface properties of the steel strip after rolling to be of higher quality. In this embodiment, a roll having a surface roughness of less than Ra 0.1 μm may be used in all passes of the finish cold rolling, and at least one pass of rolling with a roll having a roughness of 0.1 μm or more in terms of arithmetic mean roughness Ra may be combined. When the above-mentioned roll having a roughness of 0.1 μm or more in terms of arithmetic mean roughness Ra is used in the finish cold rolling, it is preferable to apply it from the first pass of the finish cold rolling. This makes it easier to obtain the effect of suppressing the roughness of the smooth roll surface due to the scale generated on the steel strip by the recrystallization annealing and improving the roll life. EXAMPLES

[0017] The present invention is further illustrated in the following examples. First, a strip-shaped intermediate cold rolling material (thickness 0.5 mm) having the composition of SUS304 specified in JIS-G-4305 was prepared. Then, the manufacturing method shown in Table 1 was carried out to obtain steel strips of the present invention and comparative examples having a thickness of 0.04 mm. The intermediate cold rolling roll roughness Ra of the present invention is the roughness of the rolling roll used in rolling from the start of intermediate cold rolling to the 0.6n pass. In the finish cold rolling of sample No. 1, "start" refers to the start pass of the finish cold rolling, and "final" refers to the final pass of the finish cold rolling. A sample was taken from this steel strip, and the presence or absence of scabs was visually observed within an area of ​​350 mm x 500 mm. As a result, it was confirmed that the occurrence of scabs was suppressed in the example of the present invention compared to the comparative example. As an example, an example of scabs confirmed in sample No. 11 is shown in Figure 1. From the above, it is believed that the steel strip of the present invention is suitable for applications requiring high-quality surface properties.

[0018] [Table 1]

Claims

1. A first cold rolling process in which a cold rolling strip having a thickness of 1 mm or less is prepared and cold rolling is performed at a rolling reduction rate of 50 to 80%; a pickling process for pickling a cold-rolled surface of the intermediate cold-rolled material to obtain a pickled material; and a second cold rolling step in which the pickled material is cold rolled at a rolling reduction of 50 to 90% to obtain a stainless steel strip with a thickness of 0.1 mm or less.

2. The method for producing a stainless steel strip according to claim 1, wherein the pickling step is performed so that the amount of loss of the intermediate cold rolled material is 3 to 7 μm.

3. The second cold rolling step is an intermediate cold rolling step of rolling at a rolling reduction rate of 50% or more to obtain an intermediate cold rolled material; a recrystallization annealing step of recrystallizing the intermediate cold-rolled material to obtain an annealed material; A finish cold rolling process of rolling the annealed material at a rolling reduction of less than 50%, When the total number of passes in the intermediate cold rolling step is n, the roughness of the rolling roll used in rolling from the start of the intermediate cold rolling to at least 0.6n passes is 0.1 μm or more in terms of arithmetic average roughness Ra; 3. The method for producing a stainless steel strip according to claim 1, wherein the roughness of the rolling rolls used in the final pass of the finish cold rolling step is less than 0.1 μm in terms of arithmetic mean roughness Ra.

Citation Information

Patent Citations

  • Surface treatment of stainless steel

    JP2000144461A

  • Ferritic stainless steel sheet superior in cleanability and manufacturing method therefor

    JP2011214079A

  • Ferritic stainless steel foil for laminate case of lithium ion secondary battery and method for manufacturing the same

    JP2012092360A

  • Austenitic stainless steel sheet, cover member, and method for producing the austenitic stainless steel sheet

    JP2016196682A

  • Installation for making cold rolled stainless steel bands

    US6478899B1

Cited By

  • Narrow and thick stainless steel cold plate and preparation method thereof

    CN120961594A