Curable composition and resin composition for optical molding

A curable composition with a core-shell structured rubber polymer particles in a vinyl monomer system addresses the issues of viscosity and water resistance, enhancing toughness and impact resistance in the cured product.

JP2024143007AInactive Publication Date: 2024-10-11KANEKA CORP

Patent Information

Application Number
JP2023055457
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional curable compositions containing N-substituted acrylamides and vinyl monomers like (meth)acrylate monomers face issues with water resistance, brittleness, and increased viscosity due to the inclusion of rubber polymer particles, which impair handleability and toughness.

Method used

A curable composition with a vinyl monomer (A) and rubber polymer particles (B) is developed, where the rubber polymer particles have an elastic core layer covered by an intermediate layer and a shell layer, with specific content ratios and solubility parameters to maintain low viscosity and enhance water resistance.

Benefits of technology

The composition achieves a high content of rubber polymer particles with low viscosity, improving toughness and impact resistance while maintaining good workability and water resistance in the cured product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143007000001
    Figure 2024143007000001
  • Figure 2024143007000002
    Figure 2024143007000002
  • Figure 2024143007000003
    Figure 2024143007000003
Patent Text Reader

Abstract

To provide a curable composition having low viscosity while containing numerous rubber polymer particles in a vinyl monomer.SOLUTION: A curable composition contains a vinyl monomer (A), and rubber polymer particles (B) in which an elastic core layer is coated with an intermediate layer formed using a monomer having two or more radical-polymerizable double bonds, and the intermediate layer is coated with a shell layer, wherein the content of the rubber polymer particles (B) with respect to 100 pts.mass of the vinyl monomer (A) is 30 pts.mass to 100 pts.mass, and in the rubber polymer particles (B), the content of the intermediate layer with respect to 100 mass% of the elastic core layer is 3.0 mass% to 15.0 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable composition and a stereolithography resin composition. [Background technology]

[0002] In recent years, N-substituted acrylamide has come to be widely used as a raw material monomer for inkjet inks, coating materials, materials for forming stereolithographic products, paint resins, semiconductor sealing materials, adhesives, etc. However, many of the general-purpose N-substituted acrylamides contain hydrophilic monomers that are soluble in water, and it has been pointed out that the water resistance may be insufficient depending on the content and the application of the cured product (see Patent Document 1).

[0003] Therefore, in order to improve the water resistance of the cured product, a composition for three-dimensional objects has been proposed that contains a vinyl monomer such as a hydrophobic (meth)acrylate monomer, whose solubility parameter (SP) value is defined as 12 or less (see Patent Document 2).

[0004] However, since vinyl monomers such as (meth)acrylate monomers polymerize while forming a three-dimensional structure during the curing process, they are known to give cured products with excellent hardness. However, if one tries to give the final cured product sufficient hardness, the product tends to be brittle and have reduced toughness.

[0005] In addition, a technology has been proposed in which a mixture of rubber polymer particles and an organic solvent is further mixed with an acrylic monomer and the volatile components are removed to produce a master batch in which the rubber polymer particles are dispersed in the acrylic monomer in the form of primary particles, thereby improving the physical properties of the cured product (see Patent Document 3).

[0006] However, this proposal has the problem that the rubber polymer fine particles swell in the acrylic monomer, causing a significant increase in the viscosity of the curable composition and impairing its handleability. Therefore, in order to keep the viscosity of the curable composition low, the content of the rubber polymer particles must be reduced, and there is a problem that the physical properties of the rubber polymer particles that are desired to be imparted to the cured product cannot be fully obtained in the cured product. Further, such a problem is aggravated by the fact that the solubility parameter (SP) value obtained by the Fedors method is 10.3 (J / cm 3 ) 1 / 2 This was more pronounced in the following vinyl monomers: [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2013-256552 A [Patent Document 2] JP 2019-137812 A [Patent Document 3] JP 2011-213952 A Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention aims to solve the above-mentioned problems in the prior art and to achieve the following object: That is, the present invention aims to provide a curable composition having a low viscosity while containing a large amount of rubber polymer particles in a vinyl monomer. [Means for solving the problem]

[0009] The means for solving the above problems are as follows: That is, the curable composition of the present invention contains a vinyl monomer (A) and rubber polymer particles (B) in which an elastic core layer is coated with an intermediate layer formed by using a monomer having two or more radically polymerizable double bonds, and the intermediate layer is further coated with a shell layer, and the content of the rubber polymer particles (B) relative to 100 parts by mass of the vinyl monomer (A) is 30 parts by mass to 100 parts by mass, and the content of the intermediate layer in the rubber polymer particles (B) relative to 100 parts by mass of the elastic core layer is 3.0 parts by mass to 15.0 parts by mass. Effect of the Invention

[0010] According to the present invention, the above-mentioned conventional problems can be solved and the above-mentioned object can be achieved, and a curable composition having a low viscosity while containing a large amount of rubber polymer particles in a vinyl monomer can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] (Curable composition) The curable composition of the present invention contains a vinyl monomer (A) and rubber polymer particles (B), and further contains other components, if necessary. In the curable composition of the present invention, the content of the rubber polymer particles (B) per 100 parts by mass of the vinyl monomer (A) is 30 parts by mass to 100 parts by mass, and in the rubber polymer particles (B), the content of the intermediate layer per 100 parts by mass of the elastic core layer is 3.0 parts by mass to 15.0 parts by mass.

[0012] The curable composition of the present invention contains rubber polymer particles (B) in addition to the vinyl monomer (A), which allows the properties (e.g., toughness, impact resistance, etc.) derived from the rubber polymer particles (B) to be imparted to the cured product of the present invention obtained by curing the curable composition.

[0013] The curable composition of the present invention has an intermediate layer in the rubber polymer particles (B) contained in the curable composition, and therefore the crosslink density of the elastic core layer covered by the intermediate layer is increased. This has the advantage that the rubber polymer particles (B) are less likely to swell with the vinyl monomer (A), and the viscosity of the curable composition can be kept low. As a result, the cured product of the curable composition can be obtained with good workability. In addition, the content of the rubber polymer particles (B) in the curable composition can be increased while preventing a decrease in workability during curing of the curable composition (i.e., an increase in the viscosity of the curable composition), and therefore the properties of the cured product of the curable composition can be further easily modified. Furthermore, since the rubber polymer particles (B) are less likely to swell with the vinyl monomer (A), and an increase in the viscosity of the curable composition can be kept low, they can be mixed with a resin component having a high viscosity and used. In addition, the rubber polymer particles (B) having the property of being less likely to swell can be mixed with a hydrophobic vinyl monomer to prevent an increase in viscosity, and therefore a cured product having excellent water resistance can be obtained.

[0014] Solubility parameters (SP values) are used to indicate the scale of affinity between substances, and generally, substances with similar values ​​are said to have good affinity with each other. The SP values ​​of components such as diene rubber and polysiloxane rubber used in the elastic core layer of conventional rubber polymer particles are usually 7.0 (J / cm 3 ) 1 / 2 ~9.0(J / cm 3 ) 1 / 2 Conventionally, epoxy resins have also been widely used as the resin component of hardenable compositions, but most commonly used epoxy resins have an SP value of 10.4 (J / cm 3 ) 1 / 2 ~15.0(J / cm 3 ) 1 / 2 This is about the same as the SP value of the component used in the elastic core layer of the rubber polymer particles, so the affinity between them is low and swelling of the rubber polymer particles is unlikely to occur. On the other hand, vinyl monomers that are usually used as materials for forming stereolithography products have an SP value of 7.0 (J / cm 3 ) 1 / 2~10.3(J / cm 3 ) 1 / 2 In many cases, the resin has a low SP value compared to epoxy resins that are generally used, and has a high affinity with the components used in the elastic core layer of the rubber polymer particles, so that it swells easily. The present inventors have conducted extensive research and found that, for a vinyl monomer (A) having such physical properties that it swells easily, an intermediate layer is provided in the rubber polymer particles (B), and the content of the rubber polymer particles (B) relative to 100 parts by mass of the vinyl monomer (A) is 30 parts by mass to 100 parts by mass, and the content of the intermediate layer in the rubber polymer particles (B) relative to 100 parts by mass of the elastic core layer is 3.0 parts by mass to 15.0 parts by mass, so that a curable composition with low viscosity and a cured product with excellent water resistance can be obtained, in which swelling of the rubber polymer particles (B) is suppressed. The SP value in this specification is determined by the method proposed by Fedors et al. Specifically, the above can be determined by referring to POLYMER ENGINEERING AND SCIENCE, FEBRUARY, 1974, Vol. 14, No. 2, ROBERT F. FEDORS. (paragraphs 147 to 154).

[0015] In this specification, the term "curable composition" refers to a composition that is cured by irradiation with active energy rays, heating, a chemical reaction, or the like to form a cured product. Examples of the composition include an active energy ray-curable composition, a thermosetting composition, and a mixed curable composition.

[0016] <Vinyl Monomer (A)> The vinyl monomer (A) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a radically polymerizable vinyl monomer, such as a vinyl monomer having a carbon-carbon unsaturated double bond. Among these, the vinyl monomer (A) is more preferably a (meth)acrylate monomer having a saturated water content of 0% or more and 3% or less at 25° C., from the viewpoint of imparting water resistance to the cured product.

[0017] In this specification, the term "(meth)acrylate" means at least one of acrylate and methacrylate.

[0018] The (meth)acrylate monomer having a saturated water content of 0% or more and 3% or less at 25° C. is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, amyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, tertiary butyl (meth)acrylate, tertiary butyl cyclohexyl (meth)acrylate, isoamyl (meth)acrylate, Examples of the acrylates include isooctyl (meth)acrylate, isodecyl (meth)acrylate, isododecyl (meth)acrylate, tricyclodecyl (meth)acrylate, isostearyl (meth)acrylate, dipropylene glycol di(meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and 1,9-nonanediol di(meth)acrylate. These may be used alone or in combination of two or more.

[0019] The saturated water content of the vinyl monomer (A) can be determined, for example, by a Karl Fischer moisture meter.

[0020] The vinyl monomer (A) may contain an oligomer or prepolymer of the above-mentioned vinyl monomer within a range that does not impair the viscosity of the curable composition or the dispersibility of the rubber polymer particles (B) in the vinyl monomer (A) component.

[0021] The solubility parameter (SP) value of the vinyl monomer (A) determined by the Fedors method is not particularly limited and can be appropriately selected depending on the purpose. 3 ) 1 / 2 More than 11.0(J / cm 3 ) 1 / 2 Less than 7.5 (J / cm 3 ) 1 / 2 More than 10.3(J / cm 3 ) 1 / 2 The SP value of the vinyl monomer (A) is more preferably 7.0 (J / cm 3 ) 1 / 2 If the SP value of the vinyl monomer (A) is less than 11.0 (J / cm), the rubber polymer particles (B) may aggregate, making it difficult to impart the properties derived from the rubber polymer particles (B) to the cured product. 3 ) 1 / 2 If it is larger than this, the hydrophilicity of the cured product increases, and the water resistance of the cured product may decrease.

[0022] The content of the vinyl monomer (A) in the curable composition is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 50% by mass to 80% by mass, more preferably 55% by mass to 75% by mass, based on the total mass of the curable composition. If the content of the vinyl monomer (A) in the curable composition is 80% by mass or more, the content of the rubber polymer particles (B) in the cured product obtained by using the curable composition is reduced, and the intended toughening effect and impact resistance improvement effect may not be sufficiently obtained. In addition, if the content of the vinyl monomer (A) in the curable composition is 50% by mass or less, sufficient dispersibility of the rubber polymer particles (B) may not be obtained.

[0023] <Rubber polymer particles (B)> The rubber polymer particles (B) are rubber polymer particles in which an elastic core layer is coated with an intermediate layer formed by using a monomer having two or more radically polymerizable double bonds, and the intermediate layer is further coated with a shell layer. The rubber polymer particles (B) have an intermediate layer formed by using a monomer having two or more radically polymerizable double bonds, so that the crosslink density of the elastic core layer can be increased and the graft efficiency of the shell layer can be improved. Each layer will be specifically described below.

[0024] <<Elastic core layer>> The elastic core layer is coated with an intermediate layer formed using a monomer having two or more radically polymerizable double bonds, and therefore the elastic core layer is present in the lowermost layer (innermost part) of the rubber polymer particles (B).

[0025] In this specification, "elasticity" means a property whereby when stress is applied, distortion occurs, but when the load is removed, the original dimensions are restored. Due to the elasticity of the elastic core layer, the rubber polymer particles (B) have rubber-like properties. Therefore, the elastic core layer of the rubber polymer particles (B) is preferably made of a rubber-like polymer having rubber properties. This can impart toughness and impact resistance to the cured product of the curable composition.

[0026] The glass transition temperature (Tg) of the elastic core layer of the rubber polymer particle (B) is not particularly limited and may be appropriately selected depending on the purpose, but is preferably less than 0° C., more preferably not more than −20° C., and even more preferably not more than −45° C. When the glass transition temperature (Tg) of the rubber polymer is less than 0° C., the effect of imparting toughness to the cured product of the curable composition is enhanced.

[0027] The glass transition temperature (Tg) of the elastic core layer of the rubber polymer particle (B) is determined by measuring the dynamic viscoelasticity with a dynamic viscoelasticity measuring device (e.g., DVA-200 (manufactured by IT Measurement & Control Co., Ltd.) at a frequency of 1 Hz, a strain of 0.05%, and a heating rate of 4°C / min.

[0028] Examples of the rubber-like polymer constituting the elastic core layer include natural rubber, polysiloxane rubber, diene rubber obtained by polymerizing a conjugated diene monomer as a main monomer (hereinafter sometimes referred to as a "first monomer"), and (meth)acrylic rubber obtained by polymerizing a (meth)acrylate monomer as a first monomer. Also, the polymer may be a polymer obtained by polymerizing these first monomers with vinyl monomers such as aromatic vinyl monomers and vinylcyan monomers (hereinafter sometimes referred to as a "second monomer"). These may be used alone or in combination of two or more. Among these, diene rubber and (meth)acrylic rubber are preferred from the viewpoint of cost.

[0029] -Polysiloxane rubber- The polysiloxane rubber is not particularly limited and can be appropriately selected depending on the purpose. For example, polysiloxane-based polymers composed of alkyl or aryl di-substituted silyloxy units such as dimethylsilyloxy units, diethylsilyloxy units, methylphenylsilyloxy units, diphenylsilyloxy units, and dimethylsilyloxy-diphenylsilyloxy units, and polysiloxane-based polymers composed of alkyl or aryl mono-substituted silyloxy units such as organohydrogensilyloxy units in which a part of the alkyl of the side chain is substituted with a hydrogen atom can be mentioned. These may be used alone or in combination of two or more. Among these, polymers composed of dimethylsilyloxy units, methylphenylsilyloxy units, and dimethylsilyloxy-diphenylsilyloxy units are preferred in that they can impart heat resistance to the cured product of the curable composition, and polymers composed of dimethylsilyloxy units are more preferred because they are easily available and economical.

[0030] -Conjugated diene monomer- The conjugated diene monomer (first monomer) is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include butadienes such as 1,3-butadiene, 2-chloro-1,3-butadiene, and 2-methyl-1,3-butadiene, and isoprene. These may be used alone or in combination of two or more. Among these, 1,3-butadiene is preferred because it is inexpensive, the resulting polymer has good rubber properties, and is easy to polymerize.

[0031] -(Meth)acrylate monomer- The (meth)acrylate monomer (first monomer) is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include alkyl (meth)acrylate, aromatic ring-containing (meth)acrylate, hydroxyalkyl (meth)acrylate, glycidyl (meth)acrylate, alkoxyalkyl (meth)acrylate, allylalkyl (meth)acrylate, polyfunctional (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0032] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate.

[0033] Examples of the aromatic ring-containing (meth)acrylate include phenoxyethyl (meth)acrylate and benzyl (meth)acrylate.

[0034] Examples of the hydroxyalkyl (meth)acrylate include 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate.

[0035] Examples of the glycidyl (meth)acrylate include glycidyl (meth)acrylate and glycidyl alkyl (meth)acrylate.

[0036] Examples of the alkoxyalkyl (meth)acrylate include 2-methoxymethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxymethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, and 4-ethoxybutyl (meth)acrylate.

[0037] Examples of the allyl alkyl (meth)acrylate include allyl (meth)acrylate and allyl alkyl (meth)acrylate.

[0038] Examples of the polyfunctional (meth)acrylate include monoethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate.

[0039] Among these, the (meth)acrylate monomer is preferably the alkyl (meth)acrylate, and more preferably ethyl (meth)acrylate, butyl (meth)acrylate, or 2-ethylhexyl (meth)acrylate.

[0040] -Vinyl monomers- The vinyl monomer (second monomer) copolymerizable with the first monomer is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include vinyl arene, vinyl carboxylic acid, vinyl cyan, vinyl halide, alkene, polyfunctional monomer, etc. These may be used alone or in combination of two or more.

[0041] Examples of the vinyl arene include styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene. Examples of the vinyl carboxylic acid include acrylic acid and methacrylic acid. Examples of the vinyl cyanide include acrylonitrile and methacrylonitrile. Examples of the vinyl halide include vinyl chloride, vinyl bromide, and chloroprene. Examples of the alkene include vinyl acetate; ethylene, propylene, butylene, and isobutylene. Among these, the vinyl monomer is preferably vinyl arene, and more preferably styrene.

[0042] In order for the elastic core layer to have suitable rubber properties, the rubber-like polymer constituting the elastic core layer is preferably a crosslinked rubber polymer having a crosslinked structure. The crosslinked rubber polymer is not dissolved in the vinyl monomer (A). The crosslinked rubber polymer may swell in a solvent that is considered to be a good solvent for the vinyl monomer (A), but is not dissolved therein.

[0043] [Cross-linked structure of elastic core layer] The method for introducing a crosslinked structure into the rubber-like polymer is not particularly limited and may be appropriately selected from commonly used methods. For example, a method may be used in which a crosslinkable monomer such as a polyfunctional monomer described below is added to a polymer component obtained by polymerizing the monomer, followed by polymerization.

[0044] The gel content of the elastic core layer is not particularly limited and can be appropriately selected depending on the purpose. However, since the elastic core layer has rubber properties, it is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0045] In this specification, the term "gel content" refers to the ratio of the toluene-insoluble matter to the total amount of the toluene-soluble matter when 0.5 g of rubber polymer particles (B) having a core-shell structure obtained by solidifying or drying the elastic core layer is immersed in 100 g of toluene, allowed to stand at 23°C for 24 hours, and then the insoluble matter and the soluble matter are separated.

[0046] -Polyfunctional monomer- The polyfunctional monomer is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include allyl alkyl (meth)acrylate, polyfunctional (meth)acrylate, aromatic polycarboxylic acid ester, cyanuric acid derivative, aromatic vinyl polyfunctional monomer, etc. These may be used alone or in combination of two or more.

[0047] Examples of the allyl alkyl (meth)acrylate include allyl (meth)acrylate and allyl alkyl (meth)acrylate. Examples of the polyfunctional (meth)acrylate include butanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate. Examples of the aromatic polycarboxylic acid ester include diallyl phthalate. Examples of the cyanuric acid derivative include triallyl cyanurate and triallyl isocyanurate. Examples of the aromatic vinyl polyfunctional monomer include divinylbenzene. Among these, the polyfunctional monomer is preferably allyl (meth)acrylate, triallyl isocyanurate, butanediol di(meth)acrylate, or divinylbenzene. In this specification, the polyfunctional monomer for introducing a crosslinked structure into the rubber-like polymer does not include butadiene, isoprene, and the like as the conjugated diene monomer (first monomer).

[0048] The shape of the elastic core layer is not particularly limited and may be appropriately selected depending on the purpose, but is preferably spherical.

[0049] When the elastic core layer has a spherical shape, the volume average particle size (Mv) of the elastic core layer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.03 μm to 0.60 μm, more preferably 0.05 μm to 0.50 μm, and even more preferably 0.10 μm to 0.30 μm. It is often difficult to stably obtain an elastic core layer having a volume average particle size of less than 0.03 μm. In addition, when the volume average particle size of the elastic core layer is 0.60 μm or less, the heat resistance and impact resistance of the cured product of the curable composition are good.

[0050] The volume average particle size of the elastic core layer can be measured using a particle size distribution measuring device (e.g., Microtrac UPA 150, manufactured by Nikkiso Co., Ltd.). Since the elastic core layer is preferably insoluble in the vinyl monomer (A), the particle size of the elastic core layer in the rubber polymer particles (B) can also be confirmed by observing the curable composition using a transmission electron microscope (TEM).

[0051] The elastic core layer may have a single layer structure or a multi-layer structure. When the elastic core layer has a multi-layer structure, the polymer composition of each layer in the elastic core layer may be the same or different.

[0052] The content of the elastic core layer in the rubber polymer particles (B) is not particularly limited and can be appropriately selected depending on the purpose, but from the viewpoint of improving the properties (e.g., toughness, etc.) of the cured product of the curable composition, it is preferably 40 parts by mass or more, more preferably 60 parts by mass or more, based on 100 parts by mass of the total content of the core layer content and the shell layer content. In addition, the upper limit of the content of the elastic core layer in the rubber polymer particles (B) is not particularly limited, but from the viewpoint of improving the dispersion state of the rubber polymer particles (B) in the curable composition, it is preferably 95 parts by mass or less, more preferably 88 parts by mass or less, based on 100 parts by mass of the total content of the core layer content and the shell layer content.

[0053] <<Middle layer>> The intermediate layer is a layer that exists between the elastic core layer and the shell layer, and is formed using a monomer having two or more radically polymerizable double bonds (hereinafter, sometimes referred to as "monomer for forming the intermediate layer").

[0054] The intermediate layer-forming monomer is preferably a monomer having two or more radically polymerizable double bonds in the same molecule.

[0055] By covering the elastic core layer with the intermediate layer formed by using a monomer having two or more radically polymerizable double bonds, the intermediate layer forming monomer is graft polymerized to the polymer forming the elastic core layer via one radically polymerizable double bond of the intermediate layer forming monomer, and the intermediate layer and the shell layer are substantially chemically bonded together, and the surface of the elastic core layer is crosslinked via the other radically polymerizable double bond of the intermediate layer forming monomer. In addition, since many radically polymerizable double bonds are arranged in the elastic core layer, the graft efficiency of the shell layer is increased. As a result, the shell layer and the elastic core layer can be bonded more firmly via the intermediate layer.

[0056] Therefore, since the rubber polymer particles (B) have the intermediate layer, the crosslink density of the elastic core layer is increased, so that the rubber polymer particles (B) are less likely to swell even when mixed with the vinyl monomer (A), and as a result, an increase in the viscosity of the curable composition can be prevented.

[0057] The intermediate layer forming monomer is not particularly limited as long as it is a monomer having two or more radically polymerizable double bonds, and can be appropriately selected depending on the purpose, and examples thereof include (meth)acrylate-based polyfunctional monomers, dienes, aromatic vinyl-based polyfunctional monomers, aromatic polycarboxylic acid esters, tertiary amines, isocyanuric acid derivatives, cyanuric acid derivatives, biphenyl derivatives, etc. These may be used alone or in combination of two or more.

[0058] Examples of the (meth)acrylate-based polyfunctional monomer include allyl (meth)acrylate, ethylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, and butanediol di(meth)acrylate. Examples of the diene include butadiene and isoprene. Examples of the aromatic vinyl-based polyfunctional monomer include divinylbenzene, diisopropenylbenzene, divinylnaphthalene, and divinylanthracene. Examples of the aromatic polycarboxylic acid ester include triallylbenzene tricarboxylate and diallyl phthalate. Examples of the tertiary amine include triallylamine. Examples of the isocyanuric acid derivative include diallyl isocyanurate, diallyl-n-propyl isocyanurate, triallyl isocyanurate, trimethallyl isocyanurate, and tris((meth)acryloxyethyl)isocyanurate. Examples of the cyanuric acid derivative include triallyl cyanurate. Examples of the biphenyl derivatives include tri(meth)acryloylhexahydrotriazine; 2,2'-divinylbiphenyl, 2,4'-divinylbiphenyl, 3,3'-divinylbiphenyl, 4,4'-divinylbiphenyl, 2,4'-di(2-propenyl)biphenyl, 4,4'-di(2-propenyl)biphenyl, 2,2'-divinyl-4-ethyl-4'-propylbiphenyl, and 3,5,4'-trivinylbiphenyl.Among these, the (meth)acrylate-based polyfunctional monomer is preferably at least one polyfunctional monomer selected from (meth)acrylate-based polyfunctional monomers, isocyanuric acid derivatives, aromatic vinyl-based polyfunctional monomers, and aromatic polycarboxylic acid esters, from the viewpoint of increasing the crosslink density of the elastic core layer and increasing the graft efficiency of the shell layer, and more preferably allyl (meth)acrylate, ethylene glycol dimethacrylate, triallyl isocyanurate, butanediol di(meth)acrylate, and divinylbenzene. From the viewpoint of suppressing swelling of the rubber polymer particles (B) relative to the vinyl monomer (A), it is even more preferable that the monomer has at least one (meth)acryloyl group, and allyl (meth)acrylate and ethylene glycol dimethacrylate are even more preferable.

[0059] When the intermediate layer forming monomer is at least one polyfunctional monomer selected from (meth)acrylate-based polyfunctional monomers, isocyanuric acid derivatives, aromatic vinyl-based polyfunctional monomers, and aromatic polycarboxylic acid esters, the content of at least one polyfunctional monomer selected from (meth)acrylate-based polyfunctional monomers, isocyanuric acid derivatives, aromatic vinyl-based polyfunctional monomers, and aromatic polycarboxylic acid esters relative to the total mass of the intermediate layer forming monomers is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 30% by mass to 100% by mass, more preferably 50% by mass to 100% by mass. If the content of at least one polyfunctional monomer selected from (meth)acrylate-based polyfunctional monomers, isocyanuric acid derivatives, aromatic vinyl-based polyfunctional monomers, and aromatic polycarboxylic acid esters is less than 30% by mass, the swelling of the rubber polymer particles (B) cannot be sufficiently suppressed when mixed with the vinyl monomer (A), and the viscosity of the curable composition may increase.

[0060] The ratio [n / m] of the number of functional groups (n) per molecule of the monomer having two or more radical polymerizable double bonds to the molecular weight (m) of the monomer having two or more radical polymerizable double bonds is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01 to 0.1, and more preferably 0.015 to 0.09. When the ratio [n / m] is 0.01 or more, the network structure formed by polymerization can be made dense, and the effect of suppressing the swelling of the rubber polymer particles (B) with respect to the vinyl monomer (A) is improved. In addition, when the ratio [n / m] is more than 0.1, the crosslink density of the elastic core layer becomes excessively high, so that the ability of the rubber polymer particles (B) as an elastic body is reduced, and the toughening and impact resistance improving effects derived from the rubber polymer particles (B) may not be sufficiently exhibited. In addition, when simply described as "molecular weight" in this specification, it refers to a value calculated based on atomic weight.

[0061] In the rubber polymer particles (B), the content of the intermediate layer relative to 100 parts by mass of the elastic core layer is 3.0 parts by mass to 15.0 parts by mass, preferably 3.5 parts by mass to 13 parts by mass, and more preferably 4.0 parts by mass to 8.0 parts by mass. In the rubber polymer particles (B), if the content of the intermediate layer relative to 100 parts by mass of the elastic core layer is less than 3.0 parts by mass, the radical polymerizable double bonds are not sufficiently arranged on the surface of the elastic core layer, the swelling of the rubber polymer particles (B) relative to the vinyl monomer (A) cannot be suppressed, and the viscosity of the curable composition increases. In addition, in the rubber polymer particles (B), if the content of the intermediate layer relative to 100 parts by mass of the elastic core layer exceeds 15.0 parts by mass, the crosslink density of the elastic core layer increases, so that the ability of the rubber polymer particles (B) as an elastic body decreases, and the toughening and impact resistance improving effects derived from the rubber polymer particles (B) cannot be sufficiently imparted to the cured product of the curable composition. In this specification, the total mass of the intermediate layer-forming monomers constituting the intermediate layer is regarded as the mass (content) of the intermediate layer.

[0062] <<Shell layer>> The shell layer is made of a shell polymer that plays a role in improving the compatibility between the rubber polymer particles (B) and the vinyl monomer (A) and enabling the rubber polymer particles (B) to be suitably dispersed in the curable composition or its cured product.

[0063] The monomer used to form the shell layer (hereinafter, sometimes referred to as "shell layer forming monomer") is polymerized, preferably graft polymerized, with the polymer forming the intermediate layer, so that the shell layer and the intermediate layer are substantially chemically bonded to each other to cover the intermediate layer. Therefore, the shell layer is present on the outermost surface of the rubber polymer particle (B).

[0064] That is, preferably, the shell polymer is formed by graft polymerizing a monomer that is a component of the shell polymer in the presence of the elastic core layer coated with the intermediate layer, and in this manner, the shell polymer is graft polymerized onto the elastic core layer coated with the intermediate layer.

[0065] The elastic core layer covered with the intermediate layer may be covered entirely or partially with the shell layer. The coverage of the elastic core layer covered with the intermediate layer by the shell layer can be confirmed by the following graft ratio.

[0066] The graft ratio of the shell layer in the rubber polymer particles (B) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more. If the graft ratio of the shell layer is 70% or more, the viscosity of the curable composition is likely to decrease.

[0067] In this specification, the graft ratio of the shell layer in the rubber polymer particles (B) is calculated as follows. The aqueous latex containing the rubber polymer particles (B) is coagulated and dehydrated, and finally dried to obtain a powder of the rubber polymer particles (B). Next, 2 g of the powder of the rubber polymer particles (B) is immersed in 100 g of methyl ethyl ketone (MEK) at 23° C. for 24 hours, after which the MEK soluble matter is separated from the MEK insoluble matter, and the methanol insoluble matter is further separated from the MEK soluble matter. The ratio of the MEK insoluble matter to the total amount of the MEK insoluble matter and the methanol insoluble matter is then calculated.

[0068] The monomer for forming the shell layer is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable that the shell polymer formed by polymerizing the monomer for forming the shell layer is compatible with the vinyl monomer (A).

[0069] Examples of such a monomer for forming the shell layer include (meth)acrylate, alkoxyalkyl (meth)acrylate, glycidyl (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0070] Examples of the (meth)acrylate include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, myristyl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, behenyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate, and 2-aminoethyl (meth)acrylate. Examples of the alkoxyalkyl (meth)acrylate include 2-methoxyethyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, and 2-phenoxyethyl (meth)acrylate. Examples of the glycidyl (meth)acrylate include glycidyl (meth)acrylate and glycidyl alkyl (meth)acrylate. Among these, methyl (meth)acrylate, butyl (meth)acrylate, and 2-ethoxyethyl (meth)acrylate are preferred from the viewpoint of compatibility with the shell polymer for the vinyl monomer (A) since the primary particles are dispersed in the vinyl monomer (A).

[0071] In addition, the shell layer forming monomer may be used in combination with other monomers other than the above monomers. Examples of the other monomers include hydroxyalkyl (meth)acrylate, alkyl (meth)acrylate, styrene, α-methylstyrene, (meth)acrylonitrile, polyfunctional vinyl monomers, vinyl monomers, etc. These may be used alone or in combination of two or more.

[0072] Examples of the hydroxyalkyl (meth)acrylate include 2-hydroxypropyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate. The alkyl (meth)acrylate is not particularly limited and can be appropriately selected depending on the purpose, but is preferably an alkyl (meth)acrylate having an alkyl group having 2 to 10 carbon atoms, such as ethyl (meth)acrylate, butyl (meth)acrylate, tertiary butyl (meth)acrylate, and cyclohexyl (meth)acrylate. Examples of the polyfunctional vinyl monomer include allyl (meth)acrylate, 1,3-butanediol di(meth)acrylate, diallyl phthalate, (poly)ethylene glycol di(meth)acrylate, trimethylolpropane (tri)acrylate, triallyl isocyanurate, and tris(2-hydroxyethyl)isocyanurate triacrylate. Examples of the vinyl monomer include (meth)acrylamide-based monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, and N-isopropyl(meth)acrylamide; examples of the allyl ester-based monomers include allyl ester-based monomers such as diallyl phthalate; and N-vinyl amide-based monomers such as N-vinylpyrrolidone and N-vinylcaprolactam.

[0073] The content of the shell layer in the rubber polymer particles (B) is not particularly limited and can be appropriately selected according to the purpose, but is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, relative to 100 parts by mass of the total content of the core layer content and the shell layer content. The upper limit of the content of the shell layer in the rubber polymer particles (B) is also not particularly limited, but is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, relative to 100 parts by mass of the total content of the core layer content and the shell layer content. When the content of the shell layer is 10 parts by mass or more, relative to 100 parts by mass of the total content of the core layer content and the shell layer content, the rubber polymer particles (B) are less likely to aggregate and have good handleability, and when it is 40 parts by mass or less, the content of the elastic core layer in the rubber polymer particles (B) does not decrease too much, and the toughness improvement effect of the cured product of the curable composition is suitably obtained.

[0074] The rubber polymer particles (B) are preferably dispersed as primary particles in the vinyl monomer (A) in order to improve the toughness of the cured product of the curable composition.

[0075] The volume average particle size (Mv) of the rubber polymer particles (B) in the vinyl monomer (A) is not particularly limited and can be appropriately selected depending on the purpose. In consideration of industrial productivity, however, it is preferably 0.03 μm to 1.0 μm, more preferably 0.05 μm to 0.5 μm, and even more preferably 0.1 μm to 0.40 μm.

[0076] The volume average particle size (Mv) of the rubber polymer particles (B) in the vinyl monomer (A) can be measured using a particle size distribution measuring device (for example, Microtrac UPA 150, manufactured by Nikkiso Co., Ltd.).

[0077] The content of the rubber polymer particles (B) relative to 100 parts by mass of the vinyl monomer (A) is 30 parts by mass to 100 parts by mass, and preferably 50 parts by mass to 70 parts by mass. If the content of the rubber polymer particles (B) relative to 100 parts by mass of the vinyl monomer (A) is less than 30 parts by mass, the cured product of the curable composition does not have sufficient impact resistance and toughness, and if it exceeds 100 parts by mass, the rubber polymer particles (B) do not have sufficient dispersibility.

[0078] <<Production method of rubber polymer particles (B)>> The method for producing the rubber polymer particles (B) is not particularly limited and may be appropriately selected depending on the purpose, but one embodiment of the method for producing the rubber polymer particles (B) is described below. One embodiment of the method for producing the rubber polymer particles (B) includes an elastic core layer forming step, an intermediate layer forming step, and a shell layer forming step, and further includes other steps as necessary.

[0079] -Core layer formation process- When the polymer forming the elastic core layer constituting the rubber polymer particle (B) is formed by polymerizing at least one monomer (first monomer) selected from diene monomers (conjugated diene monomers) and (meth)acrylate monomers, the elastic core layer can be formed by, for example, emulsion polymerization, suspension polymerization, microsuspension polymerization, etc. As a specific example, the method described in International Publication No. 2005 / 028546 can be used.

[0080] When the polymer forming the elastic core layer contains a polysiloxane-based polymer, the elastic core layer can be formed by, for example, emulsion polymerization, suspension polymerization, microsuspension polymerization, etc. As a specific example, the method described in International Publication No. 2006 / 070664 can be used.

[0081] - Intermediate layer formation process - The intermediate layer can be formed by polymerizing the intermediate layer forming monomer by known radical polymerization in the presence of the elastic core layer (particles). When the rubber elastic body constituting the elastic core layer is obtained as an emulsion, it is preferable to polymerize the intermediate layer forming monomer by emulsion polymerization.

[0082] The emulsifier (dispersant) that can be used in the emulsion polymerization is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include alkyl or aryl sulfonic acids such as dioctyl sulfosuccinic acid and dodecylbenzene sulfonic acid; alkyl or aryl ether sulfonic acids, alkyl or aryl sulfuric acids such as dodecyl sulfuric acid; alkyl or aryl ether sulfuric acids, alkyl or aryl substituted phosphoric acids, alkyl or aryl ether substituted phosphoric acids, N-alkyl or aryl sarcosinic acids such as dodecyl sarcosinic acid; alkyl or aryl carboxylic acids such as oleic acid and stearic acid; various acids such as alkyl or aryl ether carboxylic acids; anionic emulsifiers (dispersants) such as alkali metal salts or ammonium salts of these acids; nonionic emulsifiers (dispersants) such as alkyl or aryl substituted polyethylene glycol; dispersants such as polyvinyl alcohol, alkyl substituted cellulose, polyvinylpyrrolidone, and polyacrylic acid derivatives. These may be used alone or in combination of two or more.

[0083] As long as the dispersion stability of the aqueous latex of the rubber polymer particles (B) is not adversely affected, it is preferable to use a small amount of the emulsifier (dispersant). In addition, the higher the water solubility of the emulsifier (dispersant), the more preferable it is. High water solubility makes it easier to wash off the emulsifier (dispersant) with water, and can easily prevent adverse effects on the final cured product.

[0084] When the emulsion polymerization method is employed, known initiators such as 2,2'-azobisisobutyronitrile, hydrogen peroxide, potassium persulfate, and ammonium persulfate can be used as thermal decomposition initiators.

[0085] Also usable is a redox type initiator in which a peroxide such as an organic peroxide, such as t-butyl peroxyisopropyl carbonate, paramenthane hydroperoxide, cumene hydroperoxide, dicumyl peroxide, t-butyl hydroperoxide, di-t-butyl peroxide, or t-hexyl peroxide; or an inorganic peroxide, such as hydrogen peroxide, potassium persulfate, or ammonium persulfate, is used in combination with a reducing agent, such as sodium formaldehyde sulfoxylate or glucose, if necessary, and a transition metal salt, such as iron (II) sulfate, if necessary, and further a chelating agent, such as disodium ethylenediaminetetraacetate, if necessary, and further a phosphorus-containing compound, such as sodium pyrophosphate, if necessary, is used in combination.

[0086] When the redox type initiator system is used, the polymerization can be carried out even at a low temperature where the peroxide does not substantially decompose thermally, and the polymerization temperature can be set in a wide range, which is preferable. Among these, it is preferable to use an organic peroxide such as cumene hydroperoxide, dicumyl peroxide, or t-butyl hydroperoxide as a redox type initiator. The amount of the initiator used, and the amount of the reducing agent, transition metal salt, chelating agent, etc. used when using a redox type initiator can be used within a known range. In addition, when polymerizing the monomer having two or more radically polymerizable double bonds, a known chain transfer agent can be used within a known range of use. In addition, a known surfactant can be used within a known range of use.

[0087] The polymerization conditions such as polymerization temperature, pressure, and deoxidation can be within the known range. The polymerization of the intermediate layer monomer can be carried out in one stage or in two or more stages. For example, the intermediate layer monomer can be added to the emulsion of the rubber elastomer constituting the elastic core layer at once or continuously, or the intermediate layer monomer can be added to the emulsion of the rubber elastomer constituting the elastic core layer in a reactor in which the intermediate layer monomer has been charged beforehand, and then the polymerization can be carried out.

[0088] -Method of forming the shell layer- The shell layer can be formed by polymerizing the monomer for forming the shell layer by known radical polymerization in the presence of the elastic core layer (particle) covered with the intermediate layer. When the elastic core layer (particle) covered with the intermediate layer is obtained as an emulsion, it is preferable to polymerize the monomer for forming the shell layer by emulsion polymerization. As a specific example, it can be produced according to the method described in WO2005 / 028546.

[0089] <Other ingredients> The other components in the curable composition are not particularly limited as long as they do not impair the effects of the present invention, and can be appropriately selected depending on the purpose, and examples thereof include polymerization inhibitors, polymerization initiators, photosensitizers, cocatalysts, curing accelerators (promoters), chain transfer agents, reducing agents, plasticizers, fillers, dyes, pigments, stabilizers, UV absorbers, diluents (reactive / non-reactive), organic solvents, etc. These may be used alone or in combination of two or more.

[0090] <<Polymerization inhibitor (C)>> The curable composition may contain a polymerization inhibitor (C) in order to prevent undesirable spontaneous polymerization or deterioration of quality of the vinyl monomer (A).

[0091] The polymerization inhibitor (C) is not particularly limited, and can be used those generally added to commercially available radical polymerizable monomers as polymerization inhibitors.Both aerobic and anaerobic inhibitors can be used, and examples thereof include phenolic compounds, aromatic amine compounds, nitroxy compounds, nitroso compounds, quinone compounds, etc. Specifically, hydroquinone, MEHQ (hydroquinone monomethyl ether), catechol, t-butylcatechol, di-t-butylphenol, benzoquinone, phenothiazine, TEMPO (2,2,6,6-tetramethylpiperidine-1-oxyl), OH-TEMPO (4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl), vitamin C, vitamin E, phenylenediamine, Naugard (manufactured by Chemtura), Sumilizer (manufactured by Sumitomo Chemical Co., Ltd.), p-nitrosophenol, quinones (e.g., benzoquinone, naphthoquinone, etc.), phenols (e.g., hydroquinone, hydroquinone monomethyl ether, t-butylhydroquinone, t-butylcatechol, etc.), etc. These may be used alone or in combination of two or more.

[0092] The content of the polymerization inhibitor (C) in the curable composition is not particularly limited and can be appropriately selected depending on the type of the polymerization inhibitor (C) used, but is preferably 50 ppm to 5,000 ppm. If the content of the polymerization inhibitor (C) is 50 ppm or more, undesirable spontaneous polymerization and quality deterioration of the vinyl monomer (A) can be suitably prevented, and if it is 5,000 ppm or less, the effect can be sufficiently obtained.

[0093] <<Polymerization initiator>> The polymerization initiator is not particularly limited, and examples thereof include radical polymerization initiators, photopolymerization initiators, etc. These may be used alone or in combination of two or more kinds.

[0094] -Radical polymerization initiator- As the radical polymerization initiator, an organic peroxide or a compound capable of generating free radicals by light, electron beam, or heat can be used. For example, organic peroxides such as benzoyl peroxide, t-butyl peroxybenzoate, and dicumyl peroxide can be used. These can be used alone or in combination of two or more. Among these, hydroperoxides such as cumene hydroperoxide and t-butyl hydroperoxide are preferred.

[0095] -Photopolymerization initiator- The photopolymerization initiator is not particularly limited and can be appropriately selected from those which radically polymerize the vinyl monomer (A) when irradiated with ultraviolet light, electron beams, or visible light. Examples of the photopolymerization initiator include benzophenones such as benzophenone and 4,4-bis(N,N'-dimethylamino)benzophenone; benzoins such as benzoin and benzoin alkyl ether (alkyl = methyl, ethyl, isopropyl); acetophenones such as 2,2-dimethoxyacetophenone and 1,1-dichloroacetophenone; benzil ketals such as benzil dimethyl ketal (e.g., Irgacure 651, manufactured by Ciba Specialty Chemicals); anthraquinones such as 2-methylanthraquinone, 1-chloroanthraquinone, and 2-amyl anthraquinone; phenyldi(2,4,6-trimethylbenzoyl)phenyl Examples of usable compounds include bisacylphosphine oxides such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (e.g., Irgacure 819, manufactured by Ciba Specialty Chemicals); benzoylphosphine oxides such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide; triphenylphosphine; α-hydroxyphenyl ketones such as 1-hydroxycyclohexyl phenyl ketone (e.g., Irgacure 184, manufactured by Ciba Specialty Chemicals), 2-hydroxyisopropyl phenyl ketone, and 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone; thioxanthones such as thioxanthone and 2-chlorothioxanthone; camphorquinone; and the like. In addition, acridine derivatives, phenazine derivatives, and quinoxaline derivatives can also be used.

[0096] Such a photopolymerization initiator is not necessarily required when the curable composition is cured with an electron beam, but is necessary when the composition is cured with ultraviolet light or visible light.

[0097] The content of the polymerization initiator in the curable composition is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1 parts by mass to 12 parts by mass with respect to 100 parts by mass of the vinyl monomer (A).

[0098] <<Photosensitizer>> The photosensitizer is a compound that is not activated by irradiation with ultraviolet light or the like by itself, but has a function of facilitating radical polymerization when used together with a photoinitiator, compared to the case where the photoinitiator is used alone. The photosensitizer may be contained in the photopolymerization initiator.

[0099] Examples of the photosensitizer include amines such as n-butylamine, triethylamine, N-methyldiethanolamine, piperidine, N,N-dimethylaniline, triethylenetetramine, and diethylaminoethyl (meth)acrylate; urea compounds such as O-tolylthiourea; sulfur compounds such as s-benzyl-isothiuronium-p-toluenesulfinate; nitriles such as N,N-dimethyl-p-aminobenzonitrile; and phosphorus compounds such as sodium diethylthiophosphate.

[0100] The content of the photosensitizer in the curable composition is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0 parts by mass to 6 parts by mass.

[0101] <<Co-catalyst>> The co-catalyst is preferably used together with the radical polymerization initiator. The co-catalyst is an additive that acts on the radical polymerization initiator to generate radicals and harden the adhesive of the present invention in a predetermined time, and examples thereof include N,N-dimethylaniline, N,N-diethylaniline, N,N-dimethyltoluidine, N,N-diethyltoluidine, triethylamine, triethanolamine, and further, reaction products of aldehydes and amines such as butylaldehyde-aniline and butylaldehyde-butylamine. These may be used alone or in combination of two or more.

[0102] The reaction product of butyraldehyde-aniline is industrially produced and available. Preferred examples thereof include Noccela 8 (registered trademark) (manufactured by Ouchi Shinko Chemical), VANAX808 (registered trademark) (manufactured by RT Vanderbilt), and Reilly PDHP (registered trademark) (manufactured by Vertellus Specialty Chemicals).

[0103] The content of the co-catalyst in the curable composition is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01 parts by mass to 10 parts by mass with respect to 100 parts by mass of the vinyl monomer (A).

[0104] <<Cure accelerator (promoter)>> The curing accelerator (promoter) is preferably used together with the radical polymerization initiator. The curing accelerator is an additive that acts as a catalyst for the decomposition reaction of the radical polymerization initiator, and examples thereof include metal salts such as cobalt naphthenate, iron naphthenate, copper octanoate, iron hexanoate, and copper acetylacetone, as well as metal salts such as iron, copper, tin, and lead. These may be used alone or in combination of two or more.

[0105] The content of the curing accelerator (promoter) in the curable composition is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.00001 parts by mass to 1 part by mass with respect to 100 parts by mass of the vinyl monomer (A).

[0106] <Method of producing curable composition> The method for producing the curable composition is not particularly limited and can be appropriately selected depending on the purpose. In one embodiment, the curable composition can be produced by the following first, second, and third steps.

[0107] <<First step>> The first step is a step of mixing an aqueous latex containing the rubber polymer particles (B) (more specifically, a reaction mixture obtained after producing the rubber polymer particles (B) by emulsion polymerization) with an organic solvent having a solubility in water at 20°C of 5% by mass or more and 40% by mass or less, and then further mixing the mixture with excess water to aggregate the rubber polymer particles (B).

[0108] By using the organic solvent having a solubility in water at 20°C of 5% by mass or more and 40% by mass or less, when water is further added after the above mixing operation, phase separation occurs, and the rubber polymer particles (B) can be aggregated at the interface in a gentle state that allows redispersion. When the solubility of the organic solvent is 5% by mass or more, the organic solvent is easily mixed with the aqueous latex containing the rubber polymer particles (B). Furthermore, when the solubility of the organic solvent is 40% by mass or less, the rubber polymer particles (B) can be easily separated and recovered from the liquid phase (mainly the aqueous phase) in the second step.

[0109] Examples of the organic solvent having a solubility in water at 20° C. of 5% by mass or more and 40% by mass or less include ketones such as methyl ethyl ketone, esters such as methyl formate, methyl acetate, ethyl acetate, ethers such as diethyl ether, ethylene glycol diethyl ether, tetrahydropyran, acetals such as methylal, alcohols such as isobutyl alcohol, sec-butyl alcohol, etc. These may be used alone or in combination of two or more.

[0110] The organic solvent used in the first step may be a mixed organic solvent, for example, a mixed organic solvent obtained by appropriately combining two or more of a low water-soluble organic solvent such as ketones such as methyl propyl ketone, diethyl ketone, methyl isobutyl ketone, ethyl butyl ketone, etc.; esters such as diethyl carbonate, butyl formate, propyl acetate, butyl acetate, etc.; ethers such as diisopropyl ether, dibutyl ether, etc.; aliphatic hydrocarbons such as pentane, hexane, heptane, octane, etc.; aromatic hydrocarbons such as benzene, toluene, xylene, etc.; halogenated hydrocarbons such as methylene chloride, chloroform, etc., and a ketone such as acetone, cyclohexanone, etc.; esters such as γ-valerolactone, ethylene glycol monomethyl ether acetate, etc.; ethers such as dioxane, ethylene glycol monomethyl ether, etc.; alcohols such as ethanol, isopropyl alcohol, t-butyl alcohol, etc.; and a highly water-soluble organic solvent such as tetrahydrofuran, etc.

[0111] Moreover, the organic solvent used in the first step preferably has a specific gravity lower than that of water, from the viewpoint of facilitating removal of the liquid phase (mainly the aqueous phase) in the second step described below. The amount of the organic solvent mixed with the aqueous latex is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 50 parts by mass to 250 parts by mass, more preferably 60 parts by mass to 150 parts by mass, relative to 100 parts by mass of the aqueous latex. If the amount of the organic solvent mixed is 50 parts by mass or more, aggregates of the rubber polymer particles (B) contained in the aqueous latex are easily generated. If the amount of the organic solvent mixed is 250 parts by mass or less, the amount of water required to subsequently aggregate the rubber polymer particles (B) increases, which can prevent a decrease in production efficiency.

[0112] The mixing operation of the aqueous latex and the organic solvent can be performed using known devices. For example, a general device such as a stirring tank with a stirring blade, a static mixer (static mixer), a line mixer (a type in which a stirring device is incorporated into a part of a piping), etc. may be used.

[0113] The first step includes an operation of mixing the aqueous latex with an organic solvent, followed by an operation of adding excess water and mixing. This causes phase separation, allowing the rubber polymer particles (B) to aggregate in a gentle state. In addition, most of the water-soluble emulsifier or dispersant, water-soluble polymerization initiator, or electrolytes such as reducing agents used in preparing the aqueous latex can be dissolved into the aqueous phase.

[0114] The amount of water to be mixed is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 40 parts by mass to 330 parts by mass, more preferably 60 parts by mass to 250 parts by mass, relative to 100 parts by mass of the organic solvent used when mixing with the aqueous latex. When the amount of water to be mixed is 40 parts by mass or more, it is easy to aggregate the rubber polymer particles (B). When the amount of water to be mixed is 300 parts by mass or less, the organic solvent concentration in the aggregated rubber polymer particles (B) is not reduced, and the time required to redisperse the aggregated rubber polymer particles (B) in the second step is shortened, thereby improving the dispersibility of the rubber polymer particles (B).

[0115] The mixing of the water is desirably carried out under stirring or under flow conditions that can impart the same fluidity as stirring, in order to prevent the rubber polymer particles (B) from partially becoming unagglomerated. Specifically, a batch operation or continuous operation in a stirring tank equipped with a stirrer can be mentioned. The method of adding water can be a method of adding water continuously or a method of adding water all at once.

[0116] <<Second step>> The second step is a step of separating and recovering the aggregated rubber polymer particles (B) obtained in the first step from the liquid phase, and then mixing the collected particles with an organic solvent again to obtain an organic solvent solution of the rubber polymer particles (B). The second step makes it possible to separate and remove water-soluble impurities such as an emulsifier from the rubber polymer particles (B).

[0117] As a method for separating and recovering the agglomerated rubber polymer particles (B) from the liquid phase, for example, since the agglomerated rubber polymer particles (B) generally have a tendency to float in the liquid phase, when a stirring tank is used in the first step, the liquid phase (mainly the aqueous phase) may be discharged from the bottom of the stirring tank, or the particles may be filtered using filter paper, filter cloth or a metal screen having relatively coarse openings.

[0118] The amount of the organic solvent contained in the aggregate of the rubber polymer particles (B) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 30% by mass to 75% by mass, more preferably 35% by mass to 70% by mass, based on the total mass of the rubber polymer particles (B). If the content of the organic solvent is 30% by mass or more, inconveniences such as a prolonged time required for the stage of re-dispersing the aggregate of the rubber polymer particles (B) in the organic solvent in the subsequent step and an increased tendency for the aggregate to remain can be prevented. If the content of the organic solvent is 75% by mass or less, a large amount of water does not dissolve and remain in the organic solvent, and the rubber polymer particles (B) are less likely to aggregate in the third step.

[0119] In this specification, the amount of the organic solvent contained in the aggregate of the rubber polymer particles (B) is a value obtained by precisely weighing the aggregate of the rubber polymer particles (B), drying it at 120°C for 15 minutes, and measuring the loss on drying.

[0120] The second step includes an operation of mixing the aggregates of the rubber polymer particles (B) with an organic solvent. Since the rubber polymer particles (B) are loosely aggregated, the rubber polymer particles (B) can be easily redispersed in the organic solvent in the form of primary particles by mixing with the organic solvent.

[0121] Examples of the organic solvent used in the second step include the organic solvents exemplified in the first step. By using such an organic solvent, when the organic solvent is distilled off in the third step described below, it is possible to remove the water contained in the rubber polymer particles (B) by azeotroping with water. The organic solvent used in the second step may be different from the organic solvent used in the first step, but from the viewpoint of ensuring the redispersion of the aggregates in the second step, it is preferable that the organic solvent used in the second step is the same as the organic solvent used in the first step.

[0122] The amount of the organic solvent used in the second step is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 40 parts by mass to 1,400 parts by mass, more preferably 200 parts by mass to 1,000 parts by mass, relative to 100 parts by mass of the aggregates of the rubber polymer particles (B). When the amount of the organic solvent is 40 parts by mass or more, the rubber polymer particles (B) are easily dispersed uniformly in the organic solvent, and problems such as the aggregated rubber polymer particles (B) remaining as lumps or the viscosity increasing and making it difficult to handle can be prevented. In addition, when the amount of the organic solvent is 1,400 parts by mass or less, it is possible to prevent the need for a large amount of energy and a large-scale device when evaporating and distilling off the organic solvent in the third step described below, which is uneconomical.

[0123] Between the first step and the second step, it is preferable to separate and recover the aggregated rubber polymer particles (B) from the liquid phase, mix them again with an organic solvent having a solubility in water of 5% by mass to 40% by mass at 20° C., and then mix them with excess water to aggregate the rubber polymer particles (B) at least once. This makes it possible to further reduce the amount of water-soluble impurities such as emulsifiers remaining in the rubber polymer particle (B) dope.

[0124] <<Third step>> The third step is a step of distilling off the organic solvent after further mixing with a vinyl monomer (A) after the second step. The third step makes it possible to obtain a curable composition in which the rubber polymer particles (B) are uniformly dispersed and in which the amount of remaining impurities such as emulsifiers is small. In addition, the water remaining in the rubber polymer particles (B) can be distilled off by azeotropy.

[0125] The amount of the vinyl monomer (A) to be mixed in the third step is not particularly limited, and may be appropriately adjusted depending on the final desired concentration of the rubber polymer particles (B) in the curable composition.

[0126] As a method for replacing the organic solvent with a liquid vinyl monomer (A), a known method can be applied. For example, a method of charging a mixture of an organic solvent solution and a vinyl monomer (A) in a tank and distilling under reduced pressure by heating, a method of countercurrently contacting the mixture with a dry gas in a tank, a continuous method using a thin-film evaporator, a method using an extruder or a continuous stirring tank equipped with a volatilization mechanism, etc. can be mentioned. Conditions such as temperature and required time when distilling off the organic solvent can be appropriately selected within a range that does not impair the quality of the obtained curable composition. In addition, the amount of volatile matter remaining in the curable composition can be appropriately selected within a range that does not cause problems depending on the purpose of use of the curable composition.

[0127] [Application] The application of the curable composition is not particularly limited, and the composition can be suitably used, for example, as a thermosetting composition or a masterbatch thereof, or as a thermoplastic resin raw material, in the form of an adhesive, a dental resin, a resin syrup, a coating material, an overprint varnish, a solder mask, a material cured by ultraviolet light / electron beam, a photo-molding material, a casting material, a plastisol, a resin concrete or a resin mortar, a cast material, an insulating resin, an anaerobic curing resin, a screw fastener, a bonding paste, a sealant, a gasket, a packing, a material for forming a three-dimensional object (for example, an ink used in a printer for producing a three-dimensional object (additive structure)), or the like.

[0128] (Resin composition for stereolithography) The stereolithography resin composition of the present invention contains the curable composition of the present invention, and further contains other components, if necessary.

[0129] <Curable composition> The content of the curable composition in the optical molding composition is not particularly limited and can be appropriately selected depending on the purpose. The optical molding composition may be the curable composition itself (i.e., the content of the curable composition is 100% by mass).

[0130] <Other ingredients> The other components in the stereolithography resin composition are not particularly limited, and examples thereof include those described in the section <Other components> of the (Curable composition) above. The content of the other components in the stereolithography composition is not particularly limited as long as it does not impair the effects of the present invention, and can be appropriately selected depending on the purpose.

[0131] (hardened products and photo-fabricated products) The cured product of the present invention is obtained by curing the curable composition of the present invention. The stereolithographic object of the present invention is produced by curing the stereolithographic resin composition of the present invention. By curing the curable composition or the stereolithography resin composition, the rubber polymer particles (B) are unlikely to swell, and the viscosity of the curable composition or the stereolithography resin composition is low, so that a cured product or a stereolithography product can be obtained with good workability. Also, a cured product or a stereolithography product in which the rubber polymer particles (B) are uniformly dispersed can be easily obtained.

[0132] The method for curing the curable composition or the resin composition for photopolymerization may be appropriately selected depending on the form of the curable composition or the resin composition for photopolymerization. For example, the curing may be performed by a known curing method such as the action of a curing agent or a catalyst, or the action of heat, light (such as ultraviolet light), or radiation (such as an electron beam), or a combination of these.

[0133] In addition, for example, a cured product can be obtained from the curable composition or the stereolithography resin composition by a conventionally known molding method such as transfer molding, injection molding, compression molding, casting, coating and baking, or stereolithography. EXAMPLES

[0134] The present invention will be specifically described below with reference to Production Examples, Examples, and Comparative Examples, but the present invention is not limited to these Production Examples and Examples. In the Production Examples, Examples, and Comparative Examples, "%" means "% by mass" and "parts" means "parts by mass" unless otherwise specified.

[0135] (Production Example 1-1: Production of polybutadiene rubber latex (R-1)) In a 100L pressure-resistant polymerization reactor, 200 parts of deionized water, 0.03 parts of tripotassium phosphate, 0.25 parts of potassium dihydrogen phosphate, 0.002 parts of disodium ethylenediaminetetraacetate (EDTA), 0.001 parts of ferrous sulfate heptahydrate (hereinafter sometimes abbreviated as "Fe"), and 1.5 parts of sodium dodecylbenzenesulfonate (SDS) were added, and the mixture was thoroughly purged with nitrogen while stirring to remove oxygen. Then, 100 parts of butadiene (BD) were added to the system, and the temperature was raised to 45°C. 0.015 parts of paramenthane hydroperoxide (PHP) and then 0.04 parts of sodium formaldehyde sulfoxylate (SFS) were added to initiate polymerization. Four hours after the start of polymerization, 0.01 parts of PHP, 0.0015 parts of EDTA, and 0.001 parts of Fe were added. After 10 hours of polymerization, the remaining monomer was removed by volatilization under reduced pressure to terminate the polymerization, and a latex (R-1) containing polybutadiene rubber particles was obtained. The volume average particle diameter of the polybutadiene rubber particles contained in the obtained latex was 0.19 μm.

[0136] (Production Example 2-1: Production of Rubber Polymer Particles (B-1)) In an 8L glass container, 210 parts of deionized water and 73 parts of the polybutadiene rubber latex (R-1) obtained in Production Example 1-1 were charged in terms of solid content, and the mixture was stirred at 60°C for 30 minutes while nitrogen substitution was performed. After adding 0.004 parts of EDTA, 0.001 parts of Fe, and 0.03 parts of SFS, 5 parts of allyl methacrylate (ALMA) were added all at once. Then, 0.021 parts of cumene hydroperoxide (CHP) were added to start polymerization. After continuing stirring for 1 hour, a mixture of 0.17 parts of SFS, 16.2 parts of methyl acrylate (MA), and 10.8 parts of butyl acrylate (BA) was continuously added over 2 hours to perform graft polymerization. After the addition was completed, the mixture was stirred for another 2 hours to complete the reaction, and rubber polymer particles (B-1) having a core layer, an intermediate layer, and a shell layer were obtained.

[0137] (Production Examples 2-2 and 2-3: Production of Rubber Polymer Particles (B-2) and (B-3)) Rubber polymer particles (B-2) and (B-3) having a core layer, an intermediate layer, and a shell layer were obtained in the same manner as in Production Example 2-1, except that the amounts of each component in Production Example 2-1 were changed to the amounts shown in Table 1 below.

[0138] (Production Example 2-4: Production of Rubber Polymer Particles (B-4)) In an 8L glass container, 210 parts of deionized water and 70 parts of the polybutadiene rubber latex (R-1) obtained in Production Example 1-1 were charged in terms of solid content, and the mixture was stirred at 60°C for 30 minutes while nitrogen substitution was performed. 0.004 parts of EDTA, 0.001 parts of Fe, and 0.03 parts of SFS were added, and then 3.3 parts of ALMA were added all at once. Then, 0.021 parts of cumene hydroperoxide (CHP) was added to start polymerization. After continuing stirring for 1 hour, a mixture of 0.17 parts of SFS, 15 parts of butyl acrylate (BA), 6 parts of methyl methacrylate (MMA), and 9 parts of 2-methoxyethyl acrylate (2-MEA) was continuously added over 2 hours to perform graft polymerization. After the addition was completed, the mixture was stirred for another 2 hours to complete the reaction, and rubber polymer particles (B-4) having a core layer, an intermediate layer, and a shell layer were obtained.

[0139] (Production Example 2-5: Production of Rubber Polymer Particles (B-5)) Rubber polymer particles (B-5) having a core layer, an intermediate layer, and a shell layer were obtained in the same manner as in Production Example 2-4, except that ALMA in Production Example 2-4 was changed to ethylene glycol dimethacrylate (EGDM).

[0140] (Production Example 2-6: Production of Rubber Polymer Particles (B-6)) Rubber polymer particles (B-6) having a core layer, an intermediate layer, and a shell layer were obtained in the same manner as in Production Example 2-4, except that ALMA in Production Example 2-4 was changed to triallyl isocyanurate (TAIC).

[0141] (Production Example 2-7: Production of Rubber Polymer Particles (B-7)) Rubber polymer particles (B-7) having a core layer, an intermediate layer, and a shell layer were obtained in the same manner as in Production Example 2-4, except that ALMA in Production Example 2-4 was changed to 1,3-butadienediol dimethacrylate (BDMA).

[0142] (Production Example 2-8: Production of Rubber Polymer Particles (B-8)) Rubber polymer particles (B-8) having a core layer, an intermediate layer, and a shell layer were obtained in the same manner as in Production Example 2-4, except that ALMA in Production Example 2-4 was changed to divinylbenzene (DVB).

[0143] (Production Example 2-9: Production of Rubber Polymer Particles (B-9)) In Production Example 2-1, rubber polymer particles (B-9) having a core layer, an intermediate layer, and a shell layer were obtained in the same manner as in Production Example 2-1, except that 0.004 parts of EDTA, 0.001 parts of Fe, 0.03 parts of SFS, and 5 parts of ALMA were not added before the start of polymerization.

[0144] (Production Example 2-10: Production of Rubber Polymer Particles (B-10)) In Production Example 2-4, rubber polymer particles (B-10) having a core layer, an intermediate layer, and a shell layer were obtained in the same manner as in Production Example 2-4, except that the amount of ALMA was changed from 3.3 parts to 1.8 parts.

[0145] (Production Example 2-11: Production of Rubber Polymer Particles (B-11)) Rubber polymer particles (B-11) having a core layer, an intermediate layer, and a shell layer were obtained in the same manner as in Production Example 2-10, except that ALMA in Production Example 2-10 was changed to TAIC.

[0146] (Production Example 2-12: Production of Rubber Polymer Particles (B-12)) Rubber polymer particles (B-12) having a core layer, an intermediate layer, and a shell layer were obtained in the same manner as in Production Example 2-10, except that ALMA in Production Example 2-10 was changed to BDMA.

[0147] (Production Example 2-13: Production of Rubber Polymer Particles (B-13)) Rubber polymer particles (B-13) having a core layer, an intermediate layer, and a shell layer were obtained in the same manner as in Production Example 2-10, except that ALMA in Production Example 2-10 was changed to DVB.

[0148] (Example 1: Preparation of curable composition (D-1)) 126 g of methyl ethyl ketone (MEK) was introduced into a 1 L mixing tank at 25°C, and 126 g of the rubber polymer particles (B-1) obtained in Production Example 2-1 was added while stirring. After uniform mixing, 200 g of water was added at a feed rate of 80 g / min. After the end of the feed, the stirring was stopped immediately, and a slurry liquid consisting of floating aggregates and an aqueous phase containing a part of an organic solvent was obtained. Next, 350 g of the aqueous phase was discharged from the outlet at the bottom of the tank, leaving the aggregates containing a part of the aqueous phase. 90 g of MEK was added to the obtained aggregates and mixed uniformly, and a dispersion in which the rubber polymer particles (B-1) were uniformly dispersed was obtained. 40 parts of the rubber polymer particles (B-1) were mixed with 60 parts (solids equivalent) of isobornyl acrylate (IBOA) and 0.24 parts of 2,6-di-tert-butyl-p-cresol (BHT) as a polymerization inhibitor, and the MEK was distilled off under reduced pressure to obtain a curable composition (D-1) containing the rubber polymer particles (B-1).

[0149] (Examples 2 to 12 and Comparative Examples 1 to 6) In Example 1, the type and amount of the vinyl monomer (A) and the type and amount of the rubber polymer particles (B) were changed to the types and amounts shown in Tables 3 to 5 below, respectively. The curable compositions (D-2) to (D-18) of Examples 2 to 12 and Comparative Examples 1 to 6 were obtained in the same manner as in Example 1.

[0150] The information on each component used in the Production Examples, Examples, and Comparative Examples is as follows: - Monomer for forming intermediate layer - Allyl methacrylate (ALMA): Acryester (registered trademark) A (manufactured by Mitsubishi Chemical Corporation) Ethylene glycol dimethacrylate (EGDM): Light Ester EG (Kyoeisha Chemical Co., Ltd.) Triallyl isocyanurate (TAIC): TAIC (manufactured by Shinryo Corporation) 1,3-Butadiene diol dimethacrylate (BDMA): Acryester (registered trademark) B (manufactured by Mitsubishi Chemical Corporation) Divinylbenzene (DVB): Manufactured by Nippon Steel Chemical & Material Co., Ltd.

[0151] - Monomer for forming the shell layer - Methyl acrylate (MA): Nippon Shokubai Co., Ltd. -Butyl acrylate (BA): manufactured by Nippon Shokubai Co., Ltd. Methyl methacrylate (MMA): Acryester (registered trademark) M (manufactured by Mitsubishi Chemical Corporation) 2-Methoxyethyl acrylate (2-MEA): Nippon Shokubai Co., Ltd.

[0152] -Vinyl monomer (A)- Isobornyl acrylate (IBOA): Light Acrylate IB-XA (Kyoeisha Chemical Co., Ltd.) Cyclohexyl methacrylate (CHMA): Light Ester CH (Kyoeisha Chemical Co., Ltd.) Isobornyl methacrylate (IBOMA): Light Ester IB-X (Kyoeisha Chemical Co., Ltd.) · Phenoxyethyl acrylate (PEA): Light Acrylate PO-A (manufactured by Kyoeisha Chemical Co., Ltd.)

[0153] <Measurement of SP value> The SP values of the vinyl monomer (A) used in the production of the curable compositions of Examples 1 to 12 and Comparative Examples 1 to 6 were determined by the method proposed by Fedors et al. Specifically, it was determined with reference to POLYMER ENGINEERING AND SCIENCE, FEBRUARY, 1974, Vol.14, No.2, ROBERT F. FEDORS. (Items 147 to 154). The results are shown in Tables 3 to 5 below.

[0154] <Measurement of saturated water content> The saturated water content of the vinyl monomer (A) used in the production of the curable compositions of Examples 1 to 12 and Comparative Examples 1 to 6 was obtained by adding pure water to the vinyl monomer (A) by 0.20% each, and at 25°C, using a Karl Fischer moisture meter CA-100 (manufactured by Nitto Seiko Analytic Co., Ltd.) to determine the moisture content, and taking the moisture content when the moisture content no longer changed after adding pure water as the saturated water content. The results are shown in Tables 3 to 5 below.

[0155] <Measurement of viscosity> The viscosities of the curable compositions of Examples 1 to 12 and Comparative Examples 1 to 6 were measured using a digital viscometer (DV-II+Pro programmable viscometer, manufactured by Brookfield). Depending on the viscosity range, the cone spindle was properly used in type CPE-41 or type CPE-52, and the viscosity at a measurement temperature of 25°C and a shear rate of 10 (1 / s) was measured. The results are shown in Tables 3 to 5 below.

[0156]

Table 1

[0157]

Table 2

[0158] [Table 3]

[0159] [Table 4]

[0160] [Table 5]

[0161] In Comparative Examples 1 and 2, the rubber polymer particles did not have an intermediate layer, and therefore the viscosity of the curable composition was very high. In Comparative Examples 3 to 6, the rubber polymer particles had an intermediate layer, but the content of the intermediate layer per 100 parts by mass of the elastic core layer of the rubber polymer particles was less than 3.0 parts by mass, and therefore the viscosity of the curable composition was very high. In contrast, the curable compositions of Examples 1 to 12 all had low viscosities.

[0162] Examples of aspects of the present invention include the following. <1> A vinyl monomer (A); rubber polymer particles (B) in which an elastic core layer is coated with an intermediate layer formed using a monomer having two or more radically polymerizable double bonds, and the intermediate layer is further coated with a shell layer; Contains The content of the rubber polymer particles (B) relative to 100 parts by mass of the vinyl monomer (A) is 30 parts by mass to 100 parts by mass, and The curable composition is characterized in that the content of the intermediate layer per 100 parts by mass of the elastic core layer in the rubber polymer particles (B) is 3.0 parts by mass to 15.0 parts by mass. <2> The solubility parameter (SP) of the vinyl monomer (A) determined by the Fedors method was 7.0 (J / cm 3 ) 1 / 2 More than 11.0(J / cm 3 ) 1 / 2 The above-mentioned <1> The curable composition according to claim 1, <3> The solubility parameter (SP) of the vinyl monomer (A) determined by the Fedors method was 7.5 (J / cm 3 ) 1 / 2 More than 10.3(J / cm 3 ) 1 / 2 The above-mentioned <1> or <2> The curable composition according to claim 1, <4> The saturated water content of the vinyl monomer (A) is 0% or more and 3% or less at 25° C. <1> from <3> The curable composition according to any one of claims 1 to 5, <5> The monomer having two or more radically polymerizable double bonds contains 30% by mass to 100% by mass of at least one polyfunctional monomer selected from a (meth)acrylate-based polyfunctional monomer, an isocyanuric acid derivative, an aromatic vinyl-based polyfunctional monomer, and an aromatic polycarboxylic acid ester. <1> from <4> The curable composition according to any one of claims 1 to 5, <6> The monomer having two or more radically polymerizable double bonds has at least one (meth)acryloyl group. <1> from <5> The curable composition according to any one of claims 1 to 5, <7> the ratio [n / m] of the number of functional groups (n) per molecule of the monomer having two or more radically polymerizable double bonds to the molecular weight (m) of the monomer having two or more radically polymerizable double bonds is 0.01 or more; <1> from <6> The curable composition according to any one of claims 1 to 5, <8> The rubber polymer particles (B) are dispersed as primary particles in the vinyl monomer (A). <1> from <7> The curable composition according to any one of claims 1 to 5, <9> The polymerization inhibitor (C) is further contained in an amount of 50 ppm to 5,000 ppm. <1> from <8> The curable composition according to any one of claims 1 to 5, <10> The above <1> from <9> 1. A stereolithography resin composition comprising the curable composition according to claim 1. <11> The above-mentioned is used for forming a three-dimensional object. <10> 1. The stereolithography resin composition according to claim 1,

Claims

1. A vinyl monomer (A), a rubber polymer particle (B) having an elastic core layer coated with an intermediate layer formed from a monomer having two or more radically polymerizable double bonds, and the intermediate layer further coated with a shell layer; Contains The content of the rubber polymer particles (B) relative to 100 parts by mass of the vinyl monomer (A) is 30 parts by mass to 100 parts by mass, and A curable composition, characterized in that in the rubber polymer particles (B), the content of the intermediate layer per 100 parts by mass of the elastic core layer is 3.0 parts by mass to 15.0 parts by mass.

2. The solubility parameter (SP) of the vinyl monomer (A) determined by the Fedors method is 7.0 (J / cm 3 ) 1/2 11.0 (J / cm 3 ) 1/2 2. The curable composition of claim 1, wherein:

3. The solubility parameter (SP) of the vinyl monomer (A) determined by the Fedors method is 7.5 (J / cm 3 ) 1/2 10.3 (J / cm 3 ) 1/2 2. The curable composition of claim 1, wherein:

4. The curable composition according to claim 1, wherein the saturated water content of the vinyl monomer (A) is 0% or more and 3% or less at 25°C.

5. The curable composition according to claim 1, wherein the monomer having two or more radically polymerizable double bonds contains 30% by mass to 100% by mass of at least one polyfunctional monomer selected from a (meth)acrylate-based polyfunctional monomer, an isocyanuric acid derivative, an aromatic vinyl-based polyfunctional monomer, and an aromatic polycarboxylic acid ester.

6. The curable composition according to claim 1 , wherein the monomer having two or more radically polymerizable double bonds has at least one (meth)acryloyl group.

7. 2. The curable composition according to claim 1, wherein a ratio [n / m] of the number of functional groups (n) per molecule of the monomer having two or more radically polymerizable double bonds to the molecular weight (m) of the monomer having two or more radically polymerizable double bonds is 0.01 or more.

8. 2. The curable composition according to claim 1, wherein the rubber polymer particles (B) are dispersed as primary particles in the vinyl monomer (A).

9. The curable composition according to claim 1, further comprising 50 ppm to 5,000 ppm of a polymerization inhibitor (C).

10. A stereolithography resin composition comprising the curable composition according to claim 1.

11. The stereolithography resin composition according to claim 10, which is used for forming a three-dimensional stereolithography.

Citation Information

Patent Citations

  • Curable composition and cured product thereof

    JP2011213952A

  • Photopolymerizable adhesive, adhesive sheet, and laminate for touch panel

    JP2013256552A

  • Composition for solid molded article, manufacturing device of solid molded article, and manufacturing method of solid molded article

    JP2019137812A

Cited By

  • Photocuring elastomer slurry and preparation method and application thereof

    CN119978255A