Method for manufacturing laminate film having adhesive layer
The roll-to-roll laser processing method addresses inefficiencies in laminated film production by using pulsed laser beams for multiphoton absorption to minimize thermal deformation, ensuring high-quality and efficient manufacturing of laminated films with adhesive layers.
Patent Information
- Application Number
- JP2023055525
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional methods for manufacturing laminated films with adhesive layers are inefficient and prone to thermal deformation due to excessive heat accumulation during laser processing, leading to rough surfaces and impaired processing quality.
A roll-to-roll manufacturing method using pulsed laser beams for multiphoton absorption to cut and shape the adhesive and film layers, with controlled absorbance ratios and laser parameters to minimize thermal deformation and enable continuous processing.
The method efficiently produces laminated films with adhesive layers by suppressing thermal deformation, ensuring high processing quality and continuous production without the need for intermittent feeding, thereby improving manufacturing efficiency.
Smart Images

Figure 2024143048000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a laminated film having a pressure-sensitive adhesive layer. [Background technology]
[0002] A display panel has a laminated structure including elements such as a pixel panel, a polarizing film, a touch panel, and a cover film. In the manufacturing process of such a display panel, for example, an optically transparent adhesive sheet (optical adhesive sheet) is used to bond the elements included in the laminated structure. The optical adhesive sheet is manufactured, for example, in a form in which both sides of the sheet are covered with release liners (in the form of a laminated film having an adhesive layer).
[0003] Meanwhile, development of repeatedly foldable display panels for, for example, smartphones and tablet terminals is progressing. Specifically, a foldable display panel can be repeatedly deformed between a curved shape and a flat non-bent shape. In such a foldable display panel, each element in the laminated structure is made to be repeatedly foldable, and a thin optical adhesive sheet is used for bonding between such elements. An optical adhesive sheet for flexible devices such as a foldable display panel is described, for example, in Patent Document 1 below. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-111754 A Summary of the Invention [Problem to be solved by the invention]
[0005] Conventionally, an optical adhesive sheet for a display panel is produced, for example, as follows.
[0006] First, a work film W' is prepared as shown in Fig. 8A. The work film W' is composed of a laminate sheet 90 as a long original sheet, and a long carrier film C' that supports the laminate sheet 90. The laminate sheet 90 has a release liner 91, an adhesive layer 92, and a release liner 93, in this order in the thickness direction H. The release liner 91 is in releasable contact with one side of the adhesive layer 92. The release liner 93 is in releasable contact with the other side of the adhesive layer 92. The carrier film C' supports the laminate sheet 90 from the release liner 91 side.
[0007] Next, as shown in FIG. 8B, the adhesive layer 92 of the laminated sheet 90 is pressed to form a plurality of sheet-like adhesive sheets 92A (pressing process). In the press process, as shown in FIG. 9, the blade 101 of the blade die 100 is pressed into the laminated sheet 90 from the release liner 93 side until it reaches the release liner 91. This forms an adhesive sheet 92A of a predetermined shape in plan view in the adhesive layer 92. In this process, a peripheral portion 92a is formed around the adhesive sheet 92A in the adhesive layer 92. The release liner 93 is also pressed to form a release liner 93A of the same shape in plan view as the adhesive layer 92, and a peripheral portion 93a is formed around the release liner 93A. Also, a cutting groove 95 is formed in the laminated sheet 90 from the release liner 93 side to the release liner 91.
[0008] FIG. 10 shows an example of a conventional press working process. In the press working process shown in FIG. 10, a workpiece film W' flowing through a production line passes between a pair of nip rollers 201, 201, a press working machine 202, and a pair of nip rollers 203, 203, in this order. The press working machine 202 includes an intermittent feed device, a working stage, and a blade die arranged above the stage (all not shown). Between the pair of nip rollers 201, 201 and the press working machine 202, the workpiece film W' is slackened. Between the press working machine 202 and the pair of nip rollers 203, 203, the workpiece film W' is slackened. Between the nip rollers 201, 201 and the nip rollers 203, 203, the workpiece film W' is intermittently fed by an intermittent feed device of the press working machine 202. As a result, an unworked area of the workpiece film W' is intermittently fed onto the working stage of the press working machine 202. On the processing stage, press processing is performed by a blade die on each unprocessed area of the intermittently supplied workpiece film W'.
[0009] After this pressing process, as shown in Fig. 8C, peripheral portions 92a, 93a (Fig. 8B) are removed from release liner 91 (removal process). Thereafter, as shown in Fig. 8D, long release liner 91 is cut into sheet-shaped release liners 91A by pressing with another pressing machine. This results in sheet-shaped laminate film 90A (release liner 91A / adhesive sheet 92A / release liner 93A) having an adhesive layer.
[0010] In the conventional manufacturing method described above, a press processing step (FIG. 8B) is performed on each unprocessed area of the workpiece film W' that is intermittently fed onto the processing stage of the press processing machine 202. That is, the workpiece film W' is alternately transported and stopped in order to process the outer shape of the adhesive sheet (adhesive layer). To achieve such intermittent feeding, an intermittent feeding device is required, and the device must be controlled. Such a conventional manufacturing method is not preferable from the viewpoint of the manufacturing efficiency of the laminated film having an adhesive layer.
[0011] In the above-mentioned manufacturing method, from the viewpoint of manufacturing efficiency, it is considered to process the outer shapes of the adhesive layer 92 and the release liner 93 on the release liner 91 by laser processing instead of press processing. Also, from the viewpoint of suppressing a rise in temperature in the vicinity of the cut portion of the adhesive layer 92, it is considered to process the outer shapes of the adhesive layer 92 and the release liner 93 by laser processing (ablation processing) using multiphoton absorption of pulsed laser light, rather than laser processing (thermal processing) using melting.
[0012] However, when the adhesive layer 92 and release liner 93 on the release liner 91 are cut by multiphoton absorption of pulsed laser light L' irradiated from the release liner 93 side, in the conventional technology, a rough surface P is likely to be formed on the surface of the release liner 91 (film layer) facing the adhesive layer 92, as shown in Fig. 11. The rough surface P is formed by thermal deformation caused by excessive heat accumulation on the surface of the release liner 91 facing the adhesive layer 92 prior to cutting of the adhesive layer 92. This rough surface P remains on the manufactured laminate film 90A (Fig. 8D) and impairs the processing quality in the laser processing.
[0013] The present invention provides a method for producing a laminated film suitable for efficiently producing a laminated film having a pressure-sensitive adhesive layer while suppressing thermal deformation of the surface of a film layer serving as an undercoat of the pressure-sensitive adhesive layer. [Means for solving the problem]
[0014] The present invention [1] is a roll-to-roll manufacturing method for a laminated film having an adhesive layer, comprising: a preparation step of preparing a long work film having a carrier film, a first film layer, an adhesive layer, and a second film layer in that order in the thickness direction; and a contour processing step of irradiating and scanning the work film with pulsed laser light from the second film layer side, and cutting the second film layer and the adhesive layer on the first film layer by multiphoton absorption of the pulsed laser light in the work film, wherein the absorbance of the pulsed laser light per 100 μm of thickness of the first film layer is 0.13 or less.
[0015] The present invention [2] includes a method for producing a laminated film having a pressure-sensitive adhesive layer as described in [1] above, in which the ratio of the absorbance of the pressure-sensitive adhesive layer for the pulsed laser light per 100 μm thickness to the absorbance of the first film layer is 1.0 or more.
[0016] The present invention [3] includes a method for producing a laminated film having a pressure-sensitive adhesive layer as described in [1] or [2] above, in which the ratio of the absorbance of the pressure-sensitive adhesive layer to the absorbance of the pulsed laser light per 100 μm thickness to the absorbance of the first film layer is 1.5 or less.
[0017] The present invention [4] includes a method for producing a laminated film having a pressure-sensitive adhesive layer according to any one of the above [1] to [3], wherein the pulsed laser light is picosecond pulsed laser light or femtosecond pulsed laser light.
[0018] The present invention [5] includes a method for producing a laminated film having a pressure-sensitive adhesive layer according to any one of the above [1] to [4], wherein the pulsed laser light has a wavelength of 200 nm or more and 2500 nm or less. Effect of the Invention
[0019] As described above, the manufacturing method includes a contour processing step of cutting the second film layer and the adhesive layer on the first film layer by multiphoton absorption of the pulsed laser light in the work film. In the second film layer and the adhesive layer, the polymer chains are cut by multiphoton absorption of the pulsed laser light to form a cut end surface. Cutting by multiphoton absorption of the pulsed laser light is a cutting method that can cut an object to be cut while suppressing a rise in temperature of the object. Therefore, the contour processing step is suitable for suppressing a rise in temperature at the cut point in the adhesive layer and its vicinity. Suppressing the rise in temperature helps to suppress deformation and deterioration at the contour processing point of the adhesive layer and its vicinity in the manufactured laminated film.
[0020] In addition, the absorbance of the first film layer per 100 μm thickness for the pulsed laser light used in the contour processing step is 0.13 or less, as described above. This configuration is suitable for suppressing excessive heat accumulation on the adhesive layer side surface of the first film layer prior to cutting of the adhesive layer in the contour processing step, and therefore suitable for suppressing thermal deformation on the same surface. This helps to suppress the formation of a rough surface on the film layer serving as the base for the adhesive layer.
[0021] In addition, in the contour processing step of this manufacturing method, as described above, the laminated film having an adhesive layer is contour processed by laser processing. Laser processing is suitable for continuously processing the contour while continuously flowing the work film (it is not necessary to feed the work film intermittently for contour processing). Therefore, this manufacturing method is suitable for efficiently manufacturing a laminated film having an adhesive layer.
[0022] As described above, the present production method is suitable for efficiently producing a laminated film having a pressure-sensitive adhesive layer while suppressing thermal deformation of the surface of the film layer (first film layer) serving as an undercoat for the pressure-sensitive adhesive layer. [Brief description of the drawings]
[0023] [Figure 1]1 shows one embodiment of a method for producing a laminated film having a pressure-sensitive adhesive layer of the present invention, in which Fig. 1A shows a preparation step, Fig. 1B shows a contour processing step, Fig. 1C shows a removal step, and Fig. 1D shows a cutting step. [Diagram 2] 1B is a schematic plan view of an example of a region in the workpiece film after the contour processing process (FIG. 1B). [Diagram 3] 2 is an enlarged cross-sectional view of an end portion of a laminated film produced by the production method shown in FIG. 1. [Figure 4] FIG. [Diagram 5] FIG. 4 is a cross-sectional view showing a contour processing step. [Figure 6] FIG. 2 is a schematic diagram of an internal configuration of a laser processing unit. [Figure 7] FIG. 1 is a perspective view of an example of a galvanometer scanner. [Figure 8] 8A shows an example of a conventional method for producing a laminated film having a pressure-sensitive adhesive layer, in which Fig. 8A shows a preparation step, Fig. 8B shows a press processing step, Fig. 8C shows a removal step, and Fig. 8D shows a cutting step. [Figure 9] This shows the press processing process using a blade die. [Figure 10] 1 shows an example of a conventional press working process. [Figure 11] 1 shows thermal deformation during ablation processing of a conventional laminated sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The laminated film manufacturing method according to one embodiment of the present invention is a method for manufacturing a sheet-shaped laminated film having an adhesive layer by a roll-to-roll method. As shown in Figures 1A to 1D, the manufacturing method includes a preparation step (Figure 1A), a contour processing step (Figure 1B), a removal step (Figure 1C), and a cutting step (Figure 1D).
[0025] In the preparation step, a long work film W is prepared as shown in Fig. 1A. The work film W includes a laminate sheet X and a carrier film C. The laminate sheet X is a long original sheet of a laminate film Y (Fig. 1D) described later. The carrier film C supports the laminate sheet X.
[0026] The laminated sheet X includes a film layer 10 (first film layer), an adhesive layer 20, and a film layer 30 (second film layer) in this order in the thickness direction H. The adhesive layer 20 has a first surface 20a and a second surface 20b opposite to the first surface 20a. The film layer 10 is in contact with the first surface 20a. The film layer 30 is in contact with the second surface 20b. The laminated sheet X extends in a planar direction perpendicular to the thickness direction H.
[0027] The carrier film C is a single-sided adhesive film having an adhesive surface on one side in the thickness direction H. In the workpiece film W, the adhesive surface of the carrier film C is bonded to the film layer 10 side of the laminated sheet X. That is, the workpiece film W specifically includes the carrier film C, the film layer 10, the adhesive layer 20, and the film layer 30 in this order in the thickness direction H.
[0028] In this embodiment, the carrier film C is wider than the laminated sheet X in a width direction D2 (FIG. 2) perpendicular to the flow direction D1 of the workpiece film W. The laminated sheet X is disposed, for example, at the center position in the width direction D2 on the carrier film C. The width (length in the width direction D2) of the laminated sheet X is, for example, 200 mm or more, preferably 280 mm or more, more preferably 400 mm or more, and is, for example, 2000 mm or less, preferably 1800 mm or less, more preferably 1600 mm or less. Such a workpiece film W is run through the production line.
[0029] In this embodiment, the film layer 10 is a release liner. Examples of the material of the release liner include polyester, polyolefin, and polycarbonate. Examples of polyester include polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate. Examples of polyolefin include polyethylene, polypropylene, and cycloolefin polymer (COP). The film layer 10 as a release liner is in contact with the first surface 20a of the adhesive layer 20 in a releasable manner. The surface of such a film layer 10 (the surface on the adhesive layer 20 side) is preferably subjected to a release treatment. Examples of the release treatment include a silicone release treatment and a fluorine release treatment. From the viewpoint of ensuring a protective function against the adhesive layer 20, the thickness of the film layer 10 is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more. From the viewpoint of thinning the laminated film Y (FIG. 1D) to be manufactured, the thickness of the film layer 10 is preferably 150 μm or less, more preferably 120 μm or less, and even more preferably 100 μm or less.
[0030] The adhesive layer 20 is formed from an adhesive composition. The adhesive composition includes a base polymer. The base polymer is an adhesive component that exhibits adhesiveness. Examples of the base polymer include an acrylic polymer, a polyurethane polymer, a polyamide polymer, and a polyvinyl ether polymer. The base polymer may be used alone or in combination of two or more kinds. From the viewpoint of ensuring good transparency and adhesiveness in the adhesive layer 20, an acrylic polymer is preferably used as the base polymer.
[0031] An acrylic polymer is a polymer of a monomer component containing 50% by mass or more of a (meth)acrylic acid ester. "(Meth)acrylic" means acrylic and / or methacrylic. As the (meth)acrylic acid ester, preferably, a (meth)acrylic acid alkyl ester is used, and more preferably, a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 20 carbon atoms is used.
[0032] Examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, pentyl (meth)acrylate, n-hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (i.e., lauryl (meth)acrylate), isotridecyl (meth)acrylate, and tetradecyl (meth)acrylate. The (meth)acrylic acid alkyl esters may be used alone or in combination of two or more. The (meth)acrylic acid alkyl ester is preferably at least one selected from the group consisting of 2-ethylhexyl acrylate (2EHA), lauryl acrylate (LA), and n-butyl acrylate (BA). The proportion of the (meth)acrylic acid alkyl ester in the monomer component is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, from the viewpoint of appropriately expressing basic properties such as adhesiveness in the adhesive layer 20, and is, for example, 99% by mass or less.
[0033] The monomer component may include a copolymerizable monomer that is copolymerizable with the (meth)acrylic acid alkyl ester. The copolymerizable monomer may include, for example, a monomer having a polar group. The polar group-containing monomer may include, for example, a hydroxy group-containing monomer, a monomer having a nitrogen atom-containing ring, and a carboxy group-containing monomer. The polar group-containing monomer is useful for modifying the acrylic polymer, such as introducing a crosslinking point into the acrylic polymer and ensuring the cohesive force of the acrylic polymer.
[0034] Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. As the hydroxyl group-containing monomer, at least one selected from the group consisting of 2-hydroxyethyl acrylate (2HEA) and 4-hydroxybutyl acrylate (4HBA) is preferably used. The ratio of the hydroxyl group-containing monomer in the monomer component is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, from the viewpoint of introducing a crosslinked structure into the acrylic polymer and ensuring the cohesive force in the adhesive layer 20. The ratio is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, from the viewpoint of adjusting the polarity of the acrylic polymer. The polarity of the acrylic polymer is related to the compatibility of the acrylic polymer with various additive components in the adhesive layer 20.
[0035] Examples of monomers having a nitrogen atom-containing ring include N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrrole, N-vinylimidazole, N-(meth)acryloyl-2-pyrrolidone, and acryloylmorpholine. As a monomer having a nitrogen atom-containing ring, N-vinyl-2-pyrrolidone (NVP) is preferably used. The ratio of the monomer having a nitrogen atom-containing ring in the monomer component is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, from the viewpoints of ensuring the cohesive force in the pressure-sensitive adhesive layer 20 and ensuring the adhesive force to the adherend in the pressure-sensitive adhesive layer 20. The ratio is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 8% by mass or less, from the viewpoints of adjusting the glass transition temperature of the acrylic polymer and adjusting the polarity of the acrylic polymer.
[0036] The acrylic polymer can be formed by polymerizing the above-mentioned monomer components. Examples of the polymerization method include solution polymerization, solvent-free photopolymerization (e.g., UV polymerization), bulk polymerization, and emulsion polymerization. Examples of the solvent used in solution polymerization include ethyl acetate and toluene. Examples of the polymerization initiator used include a thermal polymerization initiator and a photopolymerization initiator.
[0037] The weight average molecular weight of the base polymer is preferably 100,000 or more, more preferably 300,000 or more, and even more preferably 500,000 or more, from the viewpoint of ensuring the cohesive force in the pressure-sensitive adhesive layer 20. The weight average molecular weight is preferably 5 million or less, more preferably 3 million or less, and even more preferably 2 million or less. The weight average molecular weight of the base polymer is measured by gel permeation chromatography (GPC) and calculated in terms of polystyrene.
[0038] The glass transition temperature (Tg) of the base polymer can be calculated based on the following Fox formula (theoretical value). The Fox formula is expressed as the glass transition temperature (Tg) of a polymer and the glass transition temperature (Tg) of a homopolymer of the monomer that constitutes the polymer. i In the Fox formula below, Tg represents the glass transition temperature (°C) of a polymer, Wi represents the weight fraction of monomer i constituting the polymer, and Tgi represents the glass transition temperature (°C) of a homopolymer formed from monomer i. For the glass transition temperature of a homopolymer, a literature value can be used. For example, the glass transition temperatures of various homopolymers are listed in "Polymer Handbook" (4th edition, John Wiley & Sons, Inc., 1999). On the other hand, the glass transition temperature of a homopolymer of a monomer can also be determined by the method specifically described in JP-A-2007-51271.
[0039] Fox formula 1 / (273+Tg)=Σ[Wi / (273+Tgi)]
[0040] The glass transition temperature (Tg) of the base polymer is preferably 0° C. or lower, more preferably −10° C. or lower, and even more preferably −20° C. or lower, from the viewpoint of ensuring the softness of the pressure-sensitive adhesive layer 20. The glass transition temperature is, for example, −80° C. or higher.
[0041] The base polymer preferably has a crosslinked structure. Examples of methods for introducing a crosslinked structure into the base polymer include the following first and second methods. In the first method, a base polymer having a functional group capable of reacting with a crosslinking agent and a crosslinking agent are blended into an adhesive composition, and the base polymer and the crosslinking agent are reacted in an adhesive sheet. In the second method, a polyfunctional compound is included as a crosslinking agent in the monomer components forming the base polymer, and a base polymer having a branched structure (crosslinked structure) introduced into the polymer chain is formed by polymerization of the monomer components. These methods may be used in combination.
[0042] The crosslinking agent used in the first method includes, for example, a compound that reacts with the functional group (such as a hydroxyl group and a carboxyl group) contained in the base polymer. Such crosslinking agents include, for example, an isocyanate crosslinking agent, a peroxide crosslinking agent, and an epoxy crosslinking agent. The crosslinking agent may be used alone or in combination of two or more kinds.
[0043] In the second method, the monomer components (including monofunctional monomers and polyfunctional compounds such as polyfunctional monomers for introducing a crosslinked structure) may be polymerized at once or in multiple stages. In the multi-stage polymerization method, first, a monofunctional monomer for forming a base polymer is polymerized (preliminary polymerization), thereby preparing a prepolymer composition containing a partial polymer (a mixture of a polymer with a low degree of polymerization and an unreacted monomer). Next, a polyfunctional compound is added as a crosslinking agent to the prepolymer composition, and then the partial polymer and the polyfunctional compound are polymerized (main polymerization). Examples of the polyfunctional compound include polyfunctional monomers and polyfunctional oligomers containing two or more ethylenically unsaturated double bonds in one molecule. Examples of the polyfunctional monomer include polyfunctional (meth)acrylates. Examples of the polyfunctional (meth)acrylates include dipentaerythritol hexaacrylate (DPHA), 1,6-hexanediol di(meth)acrylate, and trimethylolpropane tri(meth)acrylate. Examples of polyfunctional oligomers include urethane (meth)acrylate oligomers and polyester (meth)acrylate oligomers.
[0044] The pressure-sensitive adhesive composition may contain other components as necessary, such as a solvent, a silane coupling agent, an ultraviolet absorber, a tackifier, a softener, and an antioxidant.
[0045] The haze of the adhesive layer 20 is preferably 3% or less, more preferably 2% or less, and even more preferably 1% or less. The haze of the adhesive layer 20 can be measured using a haze meter in accordance with JIS K7136 (2000). Examples of haze meters include "NDH2000" manufactured by Nippon Denshoku Industries Co., Ltd. and "HM-150 type" manufactured by Murakami Color Research Laboratory Co., Ltd.
[0046] The shear storage modulus of the adhesive layer 20 at 25 ° C. is preferably 10 kPa or more, more preferably 15 kPa or more, even more preferably 20 kPa or more, and particularly preferably 25 kPa or more, from the viewpoint of ensuring the cohesive force of the adhesive layer 20. The shear storage modulus of the adhesive layer 20 at 25 ° C. is preferably 100 kPa or less, more preferably 80 kPa or less, even more preferably 70 kPa or less, even more preferably 60 kPa or less, and particularly preferably 50 kPa or less, from the viewpoint of realizing the softness required for the optical adhesive sheet for flexible device use in the adhesive layer 20. Examples of methods for adjusting the shear storage modulus include selection of the type of base polymer in the adhesive layer 20, adjustment of the molecular weight, adjustment of the blending amount, adjustment of the glass transition temperature, and adjustment of the degree of crosslinking. Examples of methods for adjusting the shear storage modulus include selection of components other than the base polymer in the adhesive layer 20 and adjustment of the blending amount. The shear storage modulus of the adhesive layer is determined by dynamic viscoelasticity measurement. The measurement can be performed using a dynamic viscoelasticity measuring device "Advanced Rheometric Expansion System (ARES)" manufactured by Rheometric Scientific. In the measurement, the measurement mode is shear mode, the measurement temperature range is -40°C to 100°C, the heating rate is 5°C / min, and the frequency is 1Hz. The method for measuring the shear storage modulus is specifically described below in the examples.
[0047] The thickness of the pressure-sensitive adhesive layer 20 is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more, from the viewpoint of ensuring the adhesive strength of the pressure-sensitive adhesive layer 20. The thickness of the pressure-sensitive adhesive layer 20 is preferably 250 μm or less, more preferably 230 μm or less, and even more preferably 200 μm or less, from the viewpoint of making the laminated film Y thinner.
[0048] The film layer 30 is, for example, a release liner, a surface protection film, a functional optical film, or a substrate film (support film).
[0049] Examples of the material of the release liner include polyester, polyolefin, and polycarbonate. Specifically, the materials of the release liner described above with respect to the film layer 10 are included. The film layer 30 as the release liner is in peelable contact with the second surface 20b of the adhesive layer 20. The surface of such a film layer 30 (the surface on the adhesive layer 20 side) is preferably subjected to a release treatment. Examples of the release treatment include a silicone release treatment and a fluorine release treatment. From the viewpoint of ensuring the protective function for the adhesive layer 20, the thickness of the film layer 30 as the release liner is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more. From the viewpoint of making the laminated film Y thinner, the thickness of the film layer 30 as the release liner is preferably 150 μm or less, more preferably 120 μm or less, and even more preferably 100 μm or less.
[0050] When the film layer 30 is a surface protection film, the second surface 20b of the pressure-sensitive adhesive layer 20 is bonded to such a film layer 30. The film layer 30 as a surface protection film and the pressure-sensitive adhesive layer 20 form a surface protection film with a pressure-sensitive adhesive layer.
[0051] Examples of the material of the surface protection film include polyimide (PI), polyester, polyolefin, and polycarbonate. Examples of polyester include polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate. Examples of polyolefin include polyethylene, polypropylene, and cycloolefin polymer (COP). From the viewpoint of ensuring the protective function as a surface protection film, the thickness of the film layer 30 as a surface protection film is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more. From the viewpoint of making the surface protection film with the adhesive layer thinner, the thickness of the film layer 30 as a surface protection film is preferably 100 μm or less, more preferably 70 μm or less, and even more preferably 50 μm or less.
[0052] Examples of the functional optical film include a polarizing film and a retardation film. The functional optical film may be other optical films such as a panel reinforcement material. When the film layer 30 is a functional optical film, the second surface 20b of the adhesive layer 20 is bonded to the film layer 30. The film layer 30 as a functional optical film and the adhesive layer 20 form a functional optical film with an adhesive layer.
[0053] The polarizing film may be, for example, a hydrophilic polymer film that has been dyed with a dichroic substance and then stretched. The dichroic substance may be, for example, iodine and a dichroic dye. The hydrophilic polymer film may be, for example, a polyvinyl alcohol (PVA) film, a partially formalized PVA film, and a partially saponified film of an ethylene-vinyl acetate copolymer. The polarizing film may also be a polyene-oriented film. The material of the polyene-oriented film may be, for example, a dehydrated product of PVA and a dehydrochlorinated product of polyvinyl chloride. The polarizing film may have a protective film bonded to one side and / or the other side in the thickness direction via an adhesive. The thickness of the polarizing film is preferably 10 μm or more, more preferably 20 μm or more, from the viewpoint of ensuring the function, strength, and durability of the polarizing film. The thickness of the polarizing film is preferably 500 μm or less, more preferably 300 μm or less, from the viewpoint of making the laminated film Y thinner.
[0054] Examples of the retardation film include λ / 2 wavelength film, λ / 4 wavelength film, and viewing angle compensation film. Examples of the material of the retardation film include polymer films that are birefringent by stretching. Examples of the polymer films include cellulose films and polyester films. Examples of the cellulose films include triacetyl cellulose films. Examples of the polyester films include polyethylene terephthalate films, polyethylene naphthalate films, and polybutylene terephthalate films. Examples of the retardation film include films that include a substrate such as a cellulose film and an orientation layer on the substrate. The orientation layer is formed from a liquid crystal compound such as a liquid crystal polymer. The thickness of the retardation film is preferably 1 μm or more, more preferably 2 μm or more, from the viewpoint of ensuring the function and strength of the retardation film. The thickness of the retardation film is preferably 100 μm or less, more preferably 80 μm or less, from the viewpoint of making the laminated film Y thinner.
[0055] Examples of materials for the base film include the materials mentioned above as materials for the release liner. When the film layer 30 is a base film, the second surface 20b of the adhesive layer 20 is bonded to such a film layer 30. The film layer 30 as a base film and the adhesive layer 20 form a single-sided adhesive sheet. From the viewpoint of ensuring the strength as a base, the thickness of the base film is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more. From the viewpoint of making the laminated film Y thinner, the thickness of the base film is preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 100 μm or less.
[0056] The laminated sheet X can be manufactured, for example, as follows. First, the above-mentioned adhesive composition is applied onto the film layer 30 to form a coating film. Next, the film layer 10 is laminated onto the coating film on the film layer 30. Next, the coating film between the film layers 10 and 30 is dried, and the coating film is irradiated with light as necessary. In this way, the adhesive layer 20 is formed between the film layers 10 and 30. Examples of methods for applying the adhesive composition include roll coating, kiss roll coating, gravure coating, and die coating. The drying temperature for the coating film is, for example, 50° C. to 200° C. The drying time is, for example, 5 seconds to 20 minutes.
[0057] In the laminated sheet X, the absorbance A1 per 100 μm thickness of the film layer 10 for the pulsed laser light L of a predetermined wavelength (constant wavelength) used in the next contour processing step (FIG. 1B) is 0.13 or less, preferably 0.12 or less, more preferably 0.11 or less, and even more preferably 0.10 or less. The absorbance A1 is, for example, 0.00 or more, 0.01 or more, or 0.02 or more. The absorbance A2 per 100 μm thickness of the pressure-sensitive adhesive layer 20 for the pulsed laser light L of a predetermined wavelength used in the contour processing step is preferably 0.13 or less, more preferably 0.12 or less, and even more preferably 0.11 or less. The absorbance A2 is, for example, 0.00 or more, 0.01 or more, or 0.02 or more. The ratio (A2 / A1) of the absorbance A2 to the absorbance A1 is preferably 1.0 or more, more preferably 1.1 or more, and even more preferably 1.2 or more, and is preferably 1.5 or less, more preferably 1.4 or less, and even more preferably 1.2 or less. The absorbance A3 per 100 μm of the film layer 30 for the pulsed laser light L of a predetermined wavelength used in the contour processing step is preferably 0.13 or less, more preferably 0.11 or less, and even more preferably 0.10 or less. The absorbance A3 is, for example, 0.00 or more, 0.01 or more, or 0.02 or more. The weighted average value (average absorbance A') of the absorbances A1 to A3 of each layer is preferably 0.00 or more, more preferably 0.001 or more, and is preferably 0.13 or less, and even more preferably 0.11 or less. When the thickness of the film layer 10 is T1, the thickness of the pressure-sensitive adhesive layer 20 is T2, and the thickness of the film layer 30 is T3, the average absorbance A' is calculated by the following formula.
[0058] A'=(A1×T1+A2×T2+A3×T3) / (T1+T2+T3)
[0059] In the outer shape processing step, as shown in FIG. 1B, a half-cut groove G is formed by laser processing the workpiece film W. Specifically, a pulsed laser light L is irradiated and scanned on the workpiece film W from the film layer 30 side by a laser processing device, and the film layer 30 and the adhesive layer 20 are cut on the film layer 10 by multiphoton absorption of the pulsed laser light L in the workpiece film W. More specifically, the film layer 30 and the adhesive layer 20 are cut by ablation processing (non-thermal processing) by multiphoton absorption of the pulsed laser light. The half-cut groove G is formed so as to follow a predetermined processing planned line (designed cutting line) in the workpiece film W. In this step, in the adhesive layer 20, an individualized adhesive layer 21 and a peripheral portion 22 around the adhesive layer 21 are formed. In addition, in the film layer 30, a film 31 on the adhesive layer 21 and a peripheral portion 32 around the film 31 are formed. In the film layer 10, a groove Ga (FIG. 3) is formed as a part of the half-cut groove G. In this step, the irradiation intensity of the laser light L is adjusted so that the groove Ga is formed without fully cutting the film layer 10. The groove Ga is formed along the end surface 21a of the adhesive layer 21. FIG. 2 is a plan view that shows a schematic example of an area of the workpiece film W after the contour processing step. In FIG. 2, the half-cut groove G is shown with hatching. The partial cross-sectional view shown in FIG. 1B corresponds to the partial cross-sectional view taken along line II in the workpiece film W shown in FIG. 2.
[0060] The pulsed laser light L is preferably a picosecond pulsed laser light or a femtosecond pulsed laser light from the viewpoint of appropriately causing multiphoton absorption in the film layer 30 and the adhesive layer 20, and more preferably a femtosecond pulsed laser light from the viewpoint of suppressing thermal denaturation of the laser processed portion. The pulse width of the pulsed laser light L is preferably 100×10 -15 s (100 femtoseconds) or more, and more preferably 150×10 -15 s or more, more preferably 200×10 -15 s or more, and preferably 60×10 -12s (60 picoseconds) or less, and more preferably 20×10 -12 s or less, more preferably 10×10 -12 s or less.
[0061] The wavelength of the pulsed laser light L is preferably 200 nm or more, more preferably 500 nm or more, even more preferably 800 nm or more, and even more preferably 1000 nm or more, from the viewpoint of suppressing the above-mentioned thermal deformation in the film layer 10 (rough surface P in Figure 11) while appropriately causing multiphoton absorption in the film layer 30 and the adhesive layer 20, and is preferably 2500 nm or less, more preferably 1800 nm or less, and even more preferably 1200 nm or less.
[0062] The pulse energy of the pulsed laser light L is preferably 10 μJ or more, more preferably 20 μJ or more, and even more preferably 30 μJ or more, from the viewpoint of appropriately causing multiphoton absorption in the film layer 30 and the pressure-sensitive adhesive layer 20. The pulse energy of the pulsed laser light L is preferably 300 μJ or less, more preferably 150 μJ or less, even more preferably 100 μJ or less, and even more preferably 60 μJ or less, from the viewpoint of suppressing thermal deformation in the film layer 10 in the outer shape processing step.
[0063] The pulse repetition frequency of the pulsed laser light L is preferably 100 kHz or more, more preferably 200 kHz or more, from the viewpoint of properly inducing multiphoton absorption in the film layer 30 and the adhesive layer 20, and is preferably 5000 kHz or less, more preferably 4000 kHz or less, and even more preferably 3000 kHz or less.
[0064] From the viewpoint of achieving both manufacturing efficiency and quality of the laser-processed area, the irradiation spot diameter of the pulsed laser light L is preferably 20 μm or more, more preferably 25 μm or more, and is preferably 90 μm or less, more preferably 80 μm or less.
[0065] From the viewpoint of appropriately causing multiphoton absorption in the film layer 30 and the pressure-sensitive adhesive layer 20, the peak power Pw of the pulsed laser light L is preferably 1×107 W or more, preferably 5×10 7 W or more, more preferably 10×10 7 The peak power Pw of the pulsed laser light L is, for example, 100×10 7 W or less, 500×10 7 W or less, or 800 x 10 7 It is less than W.
[0066] From the average absorbance A' of the film layers 10, 30 and the pressure-sensitive adhesive layer 20, the wavelength λ of the pulsed laser light, and the peak power Pw, the parameter Z represented by the following formula is preferably 3.0×10 11 W 2 / nm or more, more preferably 4.5×10 11 W 2 / nm or more, more preferably 8.0×10 11 W 2 / nm or more, more preferably 1.0×10 12 W 2 / nm or more, and preferably 5.0×10 13 W 2 / nm or less, more preferably 1.0×10 13 W 2 / nm or less, more preferably 7.0×10 12 W 2 / nm or less, more preferably 5.0×10 12 W 2 / nm or less. The processing speed is the scanning speed of the irradiation spot of the laser light L on the workpiece film W. The efficiency of thermal processing by normal light absorption on the workpiece film W tends to be higher as the average absorbance A' of the workpiece film W is larger. The efficiency of non-thermal processing by multiphoton absorption on the workpiece film W tends to be higher as the peak power Pw of the laser light L irradiated to the workpiece film W is larger. In addition, the efficiency of non-thermal processing by multiphoton absorption on the workpiece film W tends to be lower as the wavelength λ of the laser light L irradiated to the workpiece film W is longer. The larger the value of parameter Z, which is expressed by the following formula from the average absorbance A', peak power Pw, and wavelength λ, the higher the processing efficiency of the workpiece film W in the external processing process (Figure 1B).
[0067] Z = (A' × Pw 2 ) / λ
[0068] From the viewpoint of ensuring manufacturing efficiency, the processing speed in the external shape processing step is preferably 20 mm / sec or more, more preferably 40 mm / sec or more, and even more preferably 50 mm / sec or more. From the viewpoint of ensuring good processing quality, the processing speed in the external shape processing step is preferably 6000 mm / sec or less, more preferably 4000 mm / sec or less, and even more preferably 3000 mm / sec or less.
[0069] Examples of lasers for laser processing include gas lasers, solid lasers, and semiconductor lasers. Examples of gas lasers include F2 lasers (wavelength 157 nm). Examples of solid lasers include titanium sapphire lasers (wavelength 800 nm), Yb:YAG lasers (wavelength 1030 nm), the second harmonic of Yb:YAG lasers (wavelength 515 nm), Nd:YAG lasers (wavelength 1064 nm), the second harmonic of Nd:YAG lasers (wavelength 532 nm), the third harmonic of Nd:YAG lasers (wavelength 355 nm), and the fourth harmonic of Nd:YAG lasers (wavelength 266 nm). The pulsed laser light L in the external processing step (Figure 1B) is preferably selected from the group consisting of a Yb:YAG laser (wavelength 1030 nm), a second harmonic of a Yb:YAG laser (wavelength 515 nm), a Nd:YAG laser (wavelength 1064 nm), and a second harmonic of a Nd:YAG laser (wavelength 532 nm) from the viewpoints of suppressing variations in absorbance of each layer in the work film W and of using a high-output oscillator to increase the cutting speed and ensure productivity.
[0070] In this embodiment, a laser processing apparatus 100 shown in FIGS. 4 and 5 is used as the laser processing apparatus for carrying out the outer shape processing step (FIG. 1B).
[0071] In this embodiment, the laser processing apparatus 100 includes a processing stage 110, a laser processing unit 120, and a control unit (not shown).
[0072] The processing stage 110 is a stage that supports the workpiece film W that flows through the production line. As shown in FIG. 5, the processing stage 110 has a support table 111 and a suction path 112. The support table 111 forms a support surface for the workpiece film W in the processing stage 110. The support table 111 has a plurality of suction holes 111a that penetrate the support table 111 in the thickness direction H. The suction path 112 is a space formed in the processing stage 110. The suction path 112 is located below the support table 111. Each suction hole 111a of the support table 111 communicates with the suction path 112. The suction path 112 is connected to a suction path of a vacuum pump (not shown). The suction path 112 is depressurized by the operation of the vacuum pump. The vacuum pump can select an operating state or a non-operating state according to the control by the control unit. When the workpiece film W is on the support table 111 , the suction path 112 is depressurized, so that the workpiece film W is sucked toward the support table 111 of the processing stage 110 .
[0073] As shown in FIG. 4, a pair of nip rollers N1, N1 are arranged on the upstream side of the manufacturing line of the processing stage 110. The workpiece film W is pinched between the pair of nip rollers N1, N1, and each nip roller N1 is rotated at a constant speed to pull and send the workpiece film W toward the processing stage 110. Meanwhile, a pair of nip rollers N2, N2 are arranged on the downstream side of the manufacturing line of the processing stage 110. The workpiece film W is pinched between the pair of nip rollers N2, N2, and each nip roller N2 is rotated at a constant speed to pull and send the workpiece film W toward the downstream side of the nip rollers N2, N2. The nip rollers N1, N1 and the nip rollers N2, N2 cause the workpiece film W to flow on the support stage 111 of the processing stage 110 in the length direction of the film (flow direction D1). In this state, the suction path 112 (FIG. 5) of the processing stage 110 is depressurized, so that the workpiece film W slides on the processing stage 110 while being sucked into the processing stage 110. This is preferable for precisely focusing the pulsed laser light L on the workpiece film W that is continuously flowing on the production line in the contour processing step, and is therefore preferable for efficient and highly accurate laser processing of the workpiece film W.
[0074] 6, the laser processing unit 120 includes a housing 121, a laser light source 122, a beam expander 123, a movable lens 124, a condenser lens 125, and a galvano scanner S. The laser light source 122, the beam expander 123, the movable lens 124, the condenser lens 125, and the galvano scanner S are housed in the housing 121. The housing 121 has a laser light emission port (not shown).
[0075] The laser light source 122 oscillates a pulsed laser light L. The beam expander 123 is an optical component that adjusts the beam size of the pulsed laser light L. Other optical components may be disposed between the beam expander 123 and the movable lens 124. Examples of the other optical components include a collimator lens and a homogenizer.
[0076] The movable lens 124 is a lens that is displaceable in the optical axis direction of the pulsed laser light L. As the movable lens 124 is displaced in the optical axis direction, the position of the focal point of the pulsed laser light L focused by the focusing lens 125 (the position of the focal point on the work film W) changes. The position of the movable lens 124 in the optical axis direction can be adjusted according to the control by the control unit (position control of the movable lens 124).
[0077] The pulsed laser light L that has passed through the condenser lens 125 is reflected by the galvanometer scanner S. As shown in Fig. 6 and Fig. 7, the galvanometer scanner S includes a galvanometer mirror 126 (first galvanometer mirror), a galvanometer motor 127 (first galvanometer motor), a galvanometer mirror 128 (second galvanometer mirror), and a galvanometer motor 129 (second galvanometer motor).
[0078] The galvanometer mirror 126 has a mirror surface 126a capable of reflecting the pulsed laser light L. The galvanometer motor 127 has a motor shaft 127a connected to the galvanometer mirror 126. The motor shaft 127a extends in a first direction. The first direction is preferably a direction perpendicular to each of the flow direction D1 and the width direction D2 of the workpiece film W. The galvanometer motor 127 can swing the direction in which the mirror surface 126a of the galvanometer mirror 126 faces (first mirror surface direction) around a rotation axis extending along the motor shaft 127a. The galvanometer motor 127 can control the first mirror surface direction of the galvanometer mirror 126 according to the control by the control unit.
[0079] The galvanometer mirror 128 has a mirror surface 128a capable of reflecting the pulsed laser light L. The galvanometer motor 129 has a motor shaft 129a connected to the galvanometer mirror 128. The motor shaft 129a extends in a second direction. The second direction intersects with the first direction. The second direction is preferably perpendicular to the first direction. The second direction is preferably the width direction D2. The galvanometer motor 129 can swing the direction in which the mirror surface 128a of the galvanometer mirror 128 faces (second mirror surface direction) around a rotation axis extending along the motor shaft 129a. The galvanometer motor 129 can control the second mirror surface direction of the galvanometer mirror 128 according to the control by the control unit.
[0080] In the galvanometer scanner S, the pulsed laser light L is successively reflected by a mirror surface 126a of the galvanometer mirror 126 and a mirror surface 128a of the galvanometer mirror 128. After passing through a laser light exit port of the housing 121, the pulsed laser light L is irradiated onto the workpiece film W on the processing stage 110.
[0081] In the laser processing unit 120, the pulsed laser light L is scanned on the workpiece film W by controlling the first and second mirror surface directions of the galvanometer motors 127 and 129. Specifically, the pulsed laser light L is scanned in the flow direction D1 and the width direction D2 by controlling the first and second mirror surface directions of the galvanometer motors 127 and 129 so that the irradiation spot on the workpiece film W of the pulsed laser light L from the laser processing unit 120 follows the line to be processed on the workpiece film W. In the laser processing unit 120, the pulsed laser light L is scanned within a predetermined range (scanning area) centered substantially directly below the galvanometer scanner S. In addition, the position of the movable lens 124 is controlled according to the first and second mirror surface directions so that the size of the irradiation spot of the scanned pulsed laser light L is the same regardless of the change in the incident angle with respect to the workpiece film W (the angle formed by the normal direction to the surface of the film and the optical axis direction of the pulsed laser light L). In addition, when scanning with the pulsed laser light L, the control unit controls the galvanometer scanner S (galvanometer motors 127, 129) so that the position of the irradiation spot, which is determined by the combined speed (vector) of the transport speed (vector) of the work film W and the scanning speed (vector) of the pulsed laser light L, follows the planned processing line on the work film W.
[0082] The laser processing unit 120 may be provided with a telecentric type fθ lens at a position where the pulsed laser light L passes after the galvano scanner S. The fθ lens is useful for making the spot diameter S of the pulsed laser light L the same regardless of the change in the incident angle of the pulsed laser light L to the work film W. When the laser processing unit 120 is provided with such an fθ lens, it is not necessarily provided with the movable lens 124. When a telecentric type fθ lens having a diameter larger than the width (length in the width direction D2) of the scanning area assigned to the laser processing unit 120 can be used, it is preferable to use such an fθ lens. In addition, in the laser processing unit 120, the telecentric type fθ lens and the above-mentioned movable lens 124 may be used in combination.
[0083] In this manufacturing method, next, as shown in FIG. 1C, the peripheral portions 22 and 32 (FIG. 1B) are removed from the film layer 10 (removal step).
[0084] 1D, the long film layer 10 is cut into sheet-like films 11 (cutting step). This forms individual films 11 in the film layer 10. Examples of cutting methods include cutting by irradiation with laser light and cutting by punching.
[0085] In this manner, the laminated film Y (a laminated film having a pressure-sensitive adhesive layer) can be produced.
[0086] As shown in FIG. 3, the laminated film Y includes a film 11, a pressure-sensitive adhesive layer 21, and a film 31 in this order in the thickness direction H. The pressure-sensitive adhesive layer 21 has an end face 21a formed in the above-mentioned contour processing step. The film 31 has an end face 31a formed in the contour processing step. The end face 31a is flush with the end face 21a. The film 11 has a groove Ga formed along the end face 21a. The end faces 21a, 31a form an inclined surface that is inclined to expand outward toward the carrier film C in the thickness direction H, for example. The angle α formed between the end face 21a and the surface of the pressure-sensitive adhesive layer 21 on the film layer 10 side (the inclination angle of the end face 21a) is, for example, 60° to 88°. The angle β formed between the end face 31a and the surface of the film layer 31 on the pressure-sensitive adhesive layer 20 side (the inclination angle of the end face 31a) is, for example, 60° to 88°.
[0087] The film 11 has an extended end 11A. The extended end 11A extends outward from the end face 21a of the adhesive layer 21 in a plane direction D (FIG. 3) perpendicular to the thickness direction H. That is, the film 11 has an outer end 11e further outward than the outer end 21e of the adhesive layer 21 in the plane direction D. From the viewpoint of suppressing end blocking when a plurality of laminated films Y are stacked in the thickness direction H, the extended length d1 of the extended end 11A from the outer end 21e in the plane direction D (direction perpendicular to the end face 21a in a plan view) is preferably 70 μm or more, more preferably 90 μm or more, and even more preferably 100 μm or more. From the viewpoint of efficient production of the laminated film Y, the extended length d1 is preferably 200 μm or less, more preferably 170 μm or less, and even more preferably 150 μm or less. The extension length d1 is the length in the planar direction D from the outer end 21e of the pressure-sensitive adhesive layer 21 to the outer end 11e of the film 11, and is the maximum length of the extension end portion 11A.
[0088] The distance between the inner end 31e of the end face 31a of the film 31 and the outer end Ge of the groove Ga in the surface direction D (the direction perpendicular to the end face 21a in a plan view) is defined as the edge width d2. The edge width d2 is preferably 100 μm or less, more preferably 80 μm or less. The edge width d2 is, for example, 10 μm or more or 20 μm or more. The region of the edge width d2 is a part of the edge region that can be used as an alignment mark (edge alignment mark) for detecting the end of the laminated film Y to be manufactured. When the edge width d2 is 100 μm or less (preferably 80 μm or less), erroneous detection of the edge alignment mark by the detection camera can be suppressed (if the edge alignment mark is too large, erroneous detection occurs).
[0089] In the contour processing step (FIG. 1B) of this manufacturing method, as described above, the film layer 30 and the adhesive layer 20 are cut on the film layer 10 by the multiphoton absorption of the pulsed laser light L in the workpiece film W. In the adhesive layer 20 and the film layer 30, the polymer chains are cut by the multiphoton absorption of the pulsed laser light L, and cut end faces (end faces 21a, 31a) are formed. Cutting by multiphoton absorption of the pulsed laser light L is a cutting method that can cut an object to be cut while suppressing a rise in temperature of the object. Therefore, the contour processing step is suitable for suppressing a rise in temperature at the cut location in the adhesive layer 20 and its vicinity. Suppressing the rise in temperature helps to suppress deformation and deterioration at the contour processing location of the adhesive layer 20 and its vicinity in the manufactured laminated film Y.
[0090] In addition, the absorbance A1 of the film layer 10 per 100 μm thickness for the pulsed laser light L used in the contour processing step is 0.13 or less, preferably 0.12 or less, more preferably 0.11 or less, and even more preferably 0.10 or less, as described above. Such a configuration is suitable for suppressing excessive heat accumulation on the surface of the film layer 10 on the side of the adhesive layer 20 prior to cutting the adhesive layer 20 in the contour processing step, and therefore suitable for suppressing thermal deformation on the same surface. This helps to ensure the processing quality of the laminated film Y. Specifically, it helps to ensure the above-mentioned alignment mark by suppressing roughening of the area directly below the end surface 21a of the adhesive layer 21 in the film 11 of the laminated film Y.
[0091] In addition, in the contour processing step, as described above, the laminated film Y (laminate film having an adhesive layer) is contour processed by laser processing. Laser processing is suitable for continuously processing the contour while continuously flowing the work film W (it is not necessary to feed the work film W intermittently for contour processing). Therefore, this manufacturing method is suitable for efficiently manufacturing the laminated film Y.
[0092] As described above, the present production method is suitable for efficiently producing a laminated film Y having a pressure-sensitive adhesive layer 20 while suppressing thermal deformation of the surface of the film layer 10 serving as a base for the pressure-sensitive adhesive layer 20. EXAMPLES
[0093] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the examples. In addition, the specific numerical values of the blending amounts (contents), physical property values, parameters, etc. described below can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than") of the blending amounts (contents), physical property values, parameters, etc. corresponding to those described in the above-mentioned "Form for carrying out the invention".
[0094] Example 1 A laminated film having a pressure-sensitive adhesive layer was produced as follows.
[0095] Preparation of Pressure-Sensitive Adhesive Composition First, a mixture containing 45 parts by mass of 2-ethylhexyl acrylate (2EHA), 42 parts by mass of lauryl acrylate (LA), 2 parts by mass of n-butyl acrylate (BA), 4 parts by mass of 4-hydroxybutyl acrylate (4HBA), 7 parts by mass of N-vinyl-2-pyrrolidone (NVP), and 0.015 parts by mass of a photopolymerization initiator (product name: Irgacure 184, 1-hydroxycyclohexylphenyl ketone, manufactured by BASF) was irradiated with ultraviolet light (polymerization reaction) to obtain a prepolymer composition (polymerization rate: approximately 10%) (the prepolymer composition contains monomer components that have not undergone the polymerization reaction). Next, 100 parts by mass of the prepolymer composition, 0.08 parts by mass of dipentaerythritol hexaacrylate (DPHA) as a polyfunctional acrylate monomer, and 0.3 parts by mass of a silane coupling agent (product name "KBM-403", 3-glycidoxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed together. In this manner, a pressure-sensitive adhesive composition was obtained.
[0096] <Preparation of Laminated Sheet> First, a pressure-sensitive adhesive composition was applied onto the release-treated surface of release liner R1 as the first release liner to form a coating film. Release liner R1 is a polyethylene terephthalate (PET) film (product name "Diafoil MRF75", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) with one side treated for release with silicone, and has a predetermined ultraviolet absorbing ability. Next, the release-treated surface of release liner R2 as the second release liner was bonded to the coating film on release liner R1. Release liner R2 is a PET film (product name "Diafoil MRE75", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) with one side treated for release with silicone, and has a predetermined ultraviolet absorbing ability. Next, ultraviolet light was irradiated onto the coating film through release liner R2 to cure the coating film with ultraviolet light, and a pressure-sensitive adhesive layer with a thickness of 75 μm was formed. For ultraviolet irradiation, a black light (manufactured by Toshiba) was used as the light source, and the irradiation intensity was 5 mW / cm. 2 The cumulative irradiation dose was 1500 mJ / cm 2 This resulted in a laminate sheet (release liner R1 / adhesive layer / second release liner R2) being obtained as a base sheet for the optical adhesive sheet with a release liner.
[0097] <External shape processing process> Next, the adhesive layer of the laminate sheet was contoured. Specifically, the adhesive layer on the release liner R1 and the release liner R2 were cut (laser processing) by irradiating the laminate sheet with a pulsed laser beam in the thickness direction from the release liner R2 side along the first planned cutting line of the laminate sheet. In this laser processing, the adhesive layer and the release liner R2 were cut on the release liner R1 by multiphoton absorption of the pulsed laser beam in the laminate sheet. Specifically, in the laser processing, a specified laser processing device was used, an Yb:YAG laser was used as the laser light source (laser medium), the wavelength (λ) of the laser beam was 1030 nm, the pulse width was 2540 fs (femtoseconds), and the peak power (Pw) was 2.0×10 8The laser beam L was applied to the workpiece film W at a predetermined planar shape, and the laser beam energy was 50 μJ, the pulse repetition frequency was 200 kHz, the irradiation spot diameter was 32 μm, and the processing speed was 61 mm / s. The processing speed is the scanning speed of the irradiation spot of the laser beam L on the workpiece film W. In this process, an optical adhesive sheet having a predetermined planar shape and a first peripheral portion around it were generated in the adhesive layer, and a second peripheral portion was generated on the first peripheral portion in the release liner R2.
[0098] <Removal and cutting of surrounding areas> After the outer shape processing step, the first and second peripheral parts were removed from the release liner R1. The release liner R1 was then cut. Specifically, a CO2 laser was irradiated in the thickness direction of the release liner R1 along the second planned cutting line of the release liner R1, thereby cutting the release liner R1 into a predetermined shape in plan view. The second planned cutting line is 3 mm away from the first planned cutting line in the plan direction. In addition, a laser processing device (product name "LC500", Takei Electric Industry Co., Ltd.) was used for the laser irradiation in this step, and the pulse width of the irradiated laser was set to 3.3 μs, the pulse repetition frequency was set to 15 kHz, and the laser output was set to 40 W.
[0099] In this manner, the pressure-sensitive adhesive sheet with release liner of Example 1 (first release liner / optical adhesive sheet / second release liner) was produced as a laminate film having a pressure-sensitive adhesive layer.
[0100] Example 2 The pressure-sensitive adhesive sheet with release liner of Example 2 was produced in the same manner as the pressure-sensitive adhesive sheet with release liner of Example 1, except for the following: In the contour processing step, the wavelength of the laser light was 515 nm (second harmonic of Yb:YAG laser), and the peak power was 1.0×10 8 We decided on W.
[0101] Example 3 The PSA sheet with release liner of Example 3 was produced in the same manner as the PSA sheet with release liner of Example 1, except for the following: In the contour processing step, the peak power was set to 7.0×107 The scanning speed was set to 25 mm / s, the pulse energy was set to 18.5 μJ, the pulse repetition frequency was set to 540 kHz, and the scanning speed was set to 25 mm / s.
[0102] Comparative Example 1 The release-lined adhesive sheet of Comparative Example 1 was produced in the same manner as the release-lined adhesive sheet of Example 1, except for the following, but the adhesive layer could not be cut in the contour processing step (the adhesive layer side of release liner R1 was half-cut). In the contour processing step, an Nd:YAG laser was used as the laser light source (laser medium), the wavelength of the laser light was 355 (third harmonic of the Nd:YAG laser) nm, the pulse width was 100 ns (nanoseconds), and the peak power was 1.0×10 11 The laser power was set to 1 W, the pulse energy was set to 133 μJ, the pulse repetition frequency was set to 30 kHz, and the irradiation spot diameter was set to 15 μm.
[0103] In the contour processing step in Comparative Example 1, the material forming the adhesive layer has low UV absorption, so the adhesive layer does not undergo thermal processing (cutting) due to light absorption (this is also true for other Examples and Comparative Examples). In addition, in the contour processing step in Comparative Example 1, the pulse width of the laser light is long at 100 ns, so multiphoton absorption of the laser light does not occur in the adhesive layer. Therefore, although the laser light does not pass through the adhesive layer and cut the adhesive layer, the adhesive layer side of the release liner R1 is significantly thermally processed.
[0104] Comparative Example 2 An adhesive sheet with a release liner of Comparative Example 2 was produced in the same manner as the adhesive sheet with a release liner of Example 1, except for the following: In the contour processing step, an Nd:YAG laser was used as the laser light source (laser medium), the wavelength of the laser light was 355 nm (third harmonic of the Nd:YAG laser), the pulse width was 15 ps (picoseconds), and the peak power was 4.0 × 10 6 The irradiation spot diameter was 13 μm, and the scanning speed was 50 mm / s.
[0105] <Shear storage modulus> For the optical pressure-sensitive adhesive sheets of Examples 1 to 3 and Comparative Examples 1 and 2, the dynamic viscoelasticity was measured.
[0106] First, a sample sheet with a thickness of about 1.5 mm was prepared by laminating a plurality of adhesive sheet pieces cut from the optical adhesive sheet. Each adhesive sheet piece was taken from an area of the optical adhesive sheet that was 300 μm or more away from the end face of the sheet inward in the surface direction. Next, this sheet was punched out to obtain a cylindrical pellet (diameter 7.9 mm) as a measurement sample.
[0107] The measurement sample was then fixed to a parallel plate jig with a diameter of 7.9 mm and subjected to dynamic viscoelasticity measurement using a dynamic viscoelasticity measuring device (name: Advanced Rheometric Expansion System (ARES), manufactured by Rheometric Scientific). In this measurement, the measurement mode was shear mode, the measurement temperature range was -40°C to 100°C, the heating rate was 5°C / min, and the frequency was 1 Hz. From the measurement results, the shear storage modulus at 25°C was read. The values are shown in Table 1.
[0108] <Absorbance> The absorbance of each layer (release liner R1 / adhesive layer / release liner R2) of the laminated sheet of Examples 1 to 3 and Comparative Examples 1 and 2 was measured for the pulsed laser light used in the contour processing process. For the measurement, an Agilent Cary 7000 multi-angle variable automatic measurement spectrophotometer manufactured by Agilent Technologies was used. The absorbance A1 per 100 μm thickness of the release liner R1, the absorbance A2 per 100 μm thickness of the adhesive layer, and the absorbance A3 per 100 μm thickness of the release liner R2 are shown in Table 1 as the measurement results (the measurement results are 4 / 3 times the actual absorbance value per 75 μm thickness). The ratio of absorbance A2 to absorbance A1 (A2 / A1) is also shown in Table 1. In addition, the weighted average value of absorbance A1, A2, and A3 was calculated as the average absorbance A'. Then, a parameter Z represented by the following formula was calculated from the average absorbance A', the above-mentioned wavelength λ of the pulsed laser light in the external shape processing step, and the peak power Pw. The value is also shown in Table 1.
[0109] Z = (A' × Pw 2 ) / λ
[0110] <Processing quality> The shape of the adhesive layer in each laminate film of Examples 1 to 3 and Comparative Examples 1 and 2 was analyzed using a shape analysis laser microscope (product name "VK-X1000", manufactured by KEYENCE). Specifically, the microscope was used to check whether the area along the edge of the adhesive layer and its vicinity on the adhesive layer side surface of the release liner R1 was roughened. The quality of the laser processing was evaluated as "good" when the area along the edge of the adhesive layer and its vicinity on the adhesive layer side surface of the release liner R1 was not roughened, and as "poor" when it was roughened. The evaluation results are shown in Table 1.
[0111] [Table 1] [Explanation of symbols]
[0112] W Work Film X-Laminated Sheet Y laminated film C Carrier Film H Thickness direction D plane direction D1 Flow direction D2 width direction 10 Film layer (first film layer) 11 Film 11A Extension end 20, 21 Adhesive layer 30 Film layer (2nd film layer) 31 Film L Pulsed laser light 100 Laser processing equipment 110 Processing stage 111 Support Table 111a Suction hole 112 Suction channel 120 Laser Processing Unit S Galvanometer Scanner
Claims
1. A roll-to-roll method for producing a laminated film having a pressure-sensitive adhesive layer, comprising: A preparation process of preparing a long work film having a carrier film, a first film layer, an adhesive layer, and a second film layer in this order in a thickness direction; and a contour processing step of irradiating and scanning the workpiece film from the second film layer side with a pulsed laser light, and cutting the second film layer and the adhesive layer on the first film layer by multiphoton absorption of the pulsed laser light in the workpiece film. A method for producing a laminated film having a pressure-sensitive adhesive layer, wherein the first film layer has an absorbance of 0.13 or less for the pulsed laser beam per 100 μm of thickness.
2. 2. The method for producing a laminated film having a pressure-sensitive adhesive layer according to claim 1, wherein a ratio of the absorbance of the pressure-sensitive adhesive layer for the pulsed laser light per 100 μm thickness to the absorbance of the first film layer is 1.0 or more.
3. 2. The method for producing a laminated film having a pressure-sensitive adhesive layer according to claim 1, wherein a ratio of the absorbance of the pressure-sensitive adhesive layer for the pulsed laser light per 100 μm thickness to the absorbance of the first film layer is 1.5 or less.
4. The method for producing a laminated film having a pressure-sensitive adhesive layer according to claim 1 , wherein the pulsed laser light is picosecond pulsed laser light or femtosecond pulsed laser light.
5. The method for producing a laminated film having a pressure-sensitive adhesive layer according to claim 1 , wherein the pulsed laser light has a wavelength of 200 nm or more and 2500 nm or less.
Citation Information
Patent Citations
Adhesive sheet
JP2018111754A
Cited By
Method for manufacturing an adhesive sheet
CN123149591A