Optical adhesive sheet

The optical adhesive sheet with a hard end surface and controlled hardness ratio addresses unintended deformation issues, ensuring flexibility and stability in foldable display panels by using pulsed laser cutting and photoinitiator activation.

JP2024143049APending Publication Date: 2024-10-11NITTO DENKO CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023055526
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Optical adhesive sheets for flexible devices, such as foldable display panels, require high flexibility and stress relaxation properties but suffer from unintended deformation at the end portions due to their softness.

Method used

An optical adhesive sheet with a hard end surface and a specific hardness ratio, achieved through a manufacturing process involving pulsed laser cutting and photoinitiator activation, ensuring a shear storage modulus of 170 kPa or less and a hardness ratio of 1.15 or more at the end surface compared to the inner surface.

Benefits of technology

The solution effectively suppresses unintended deformation of the end portions by creating a locally hard surface, maintaining the adhesive sheet's flexibility while preventing unwanted shape changes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143049000001_ABST
    Figure 2024143049000001_ABST
Patent Text Reader

Abstract

To provide a soft optical adhesive sheet suitable or suppressing unintended deformation of an end part, and a method for producing the sheet.SOLUTION: An adhesive sheet 10 of the present invention is an optical adhesive sheet having 170kPa or less of a shear storage elastic modulus at 25°C, and has a hard end face 11. The hard end face 11 has hardness H1 as surface hardness measured by a nanoindentation method at 25°C. A site in the adhesive sheet 10, which is apart from the hard end face 11 toward inside in a surface direction of the adhesive sheet 10 by 20 μm, has hardness H2 as surface hardness measured by the nanoindentation method at 25°C. A ratio of the hardness H1 to the hardness H2 is 1.15 or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical pressure-sensitive adhesive sheet. [Background technology]

[0002] A display panel has a laminated structure including elements such as a pixel panel, a polarizing film, a touch panel, and a cover film. In the manufacturing process of such a display panel, for example, an optically transparent adhesive sheet (optical adhesive sheet) is used to bond the elements included in the laminated structure.

[0003] Meanwhile, development of repeatedly foldable display panels for, for example, smartphones and tablet terminals is progressing. Specifically, a foldable display panel can be repeatedly deformed between a curved shape and a flat non-bent shape. In such a foldable display panel, each element in the laminated structure is made to be repeatedly foldable, and a thin optical adhesive sheet is used for bonding between such elements. An optical adhesive sheet for flexible devices such as a foldable display panel is described, for example, in Patent Document 1 below. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-111754 A Summary of the Invention [Problem to be solved by the invention]

[0005] Optical adhesive sheets for flexible devices are required to be highly flexible so as to have sufficient conformability to the adherend when the device is bent and excellent stress relaxation. However, the softer the optical adhesive sheet is, the more likely it is that unintended deformation will occur at the end of the optical adhesive sheet. Unintended deformation at the end of the optical adhesive sheet reduces the handleability of the optical adhesive sheet.

[0006] The present invention provides a soft optical adhesive sheet suitable for suppressing unintended deformation at edges, and a method for producing the same. [Means for solving the problem]

[0007] The present invention [1] includes an optical adhesive sheet having a hard end surface, the optical adhesive sheet having a shear storage modulus of 170 kPa or less at 25°C, the hard end surface having a hardness H1 as a surface hardness at 25°C measured by a nanoindentation method, a portion of the optical adhesive sheet 20 μm away from the hard end surface inward in the surface direction of the optical adhesive sheet having a hardness H2 as a surface hardness at 25°C measured by a nanoindentation method, and a ratio of hardness H1 to hardness H2 being 1.15 or more.

[0008] The present invention [2] includes the optical adhesive sheet described in the above [1], in which the ratio is 10 or less.

[0009] The present invention [3] includes the optical adhesive sheet described in [1] or [2] above, which contains a photoinitiator.

[0010] The present invention [4] includes a method for producing an optical adhesive sheet described in any one of [1] to [3] above, comprising a preparation step of preparing an optical adhesive sheet raw material containing a photoinitiator, and a contour processing step of irradiating and scanning the optical adhesive sheet raw material with pulsed laser light, and cutting the optical adhesive sheet raw material by multiphoton absorption of the pulsed laser light in the optical adhesive sheet raw material to form an optical adhesive sheet.

[0011] The present invention [5] includes the method for producing an optical adhesive sheet described in the above [4], wherein the pulsed laser light is picosecond pulsed laser light or femtosecond pulsed laser light.

[0012] The present invention [6] includes the method for producing an optical adhesive sheet according to the above [4] or [5], wherein the pulsed laser light has a wavelength of 500 nm or more and 2500 nm or less. Effect of the Invention

[0013] As described above, the optical adhesive sheet of the present invention has a shear storage modulus of 170 kPa or less at 25° C. and is soft. In addition, as described above, the optical adhesive sheet has a hard end surface, and the ratio (H1 / H2) of the hardness H1 of the hard end surface to the hardness H2 of a portion 20 μm away from the hard end surface toward the inside in the surface direction of the sheet is 1.15 or more. Such an optical adhesive sheet with a locally hard end surface is suitable for suppressing unintended deformation of the end portion.

[0014] The manufacturing method of the optical adhesive sheet of the present invention includes a contour processing step of cutting the optical adhesive sheet raw material by multiphoton absorption of pulsed laser light in the optical adhesive sheet raw material containing a photoinitiator, as described above. At the irradiated portion of the optical adhesive sheet raw material with the pulsed laser light, the polymer chain in the optical adhesive sheet raw material is cut by multiphoton absorption of the pulsed laser light, and a cut end surface is formed. When the cut end surface is formed, the photoinitiator is activated by multiphoton absorption of the pulsed laser light at the cut end surface, and a reaction (crosslinking reaction, etc.) between the resins progresses. This hardens the cut end surface. In addition, cutting by multiphoton absorption of pulsed laser light is a cutting method that can cut the object to be cut while suppressing the temperature rise of the object to be cut. Therefore, the contour processing step is suitable for suppressing the temperature rise of the cut portion and the surrounding area in the optical adhesive sheet raw material. This is suitable for suppressing the length of the hardened area from the cut end surface at the end (the cut end surface and its vicinity) of the optical adhesive sheet formed by the contour processing step. Therefore, this manufacturing method is suitable for manufacturing the above-mentioned optical adhesive sheet of the present invention. [Brief description of the drawings]

[0015] [Figure 1] 1 is a schematic cross-sectional view of one embodiment of an optical adhesive sheet of the present invention. [Diagram 2] 2 shows one embodiment of a method for producing an optical adhesive sheet of the present invention, in which Fig. 2A shows a preparation step, Fig. 2B shows a contour processing step, Fig. 2C shows a removal step, and Fig. 2D shows a cutting step. [Diagram 3] 2B is a schematic plan view of an example of a region in the workpiece film after the contour processing step (FIG. 2B). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] As shown in FIG. 1, an adhesive sheet 10 as an embodiment of the optical adhesive sheet of the present invention has a sheet shape of a predetermined thickness and extends in a direction (plane direction D) perpendicular to the thickness direction H. The adhesive sheet 10 has a first surface 10a and a second surface 10b opposite to the first surface 10a. FIG. 1 exemplarily illustrates a state in which release liners 20, 30 are attached to both surfaces of the adhesive sheet 10. The release liner 20 is in releasable contact with the first surface 10a of the adhesive sheet 10. The release liner 30 is in releasable contact with the second surface 10b. The adhesive sheet 10 and the release liners 20, 30 form an adhesive sheet X with a release liner. Specifically, the adhesive sheet X with a release liner includes a release liner 20, an adhesive sheet 10, and a release liner 30 in this order in the thickness direction H.

[0017] The adhesive sheet 10 is an optically transparent adhesive sheet (optical adhesive sheet) that is disposed at a light passing portion in a flexible device. An example of a flexible device is a flexible display panel. The flexible display panel has a laminated structure including elements such as a pixel panel, a polarizing film, a retardation film, a touch panel, and a cover film. The adhesive sheet 10 is used, for example, in the manufacturing process of the flexible display panel to bond elements included in the laminated structure. The release liners 20 and 30 are each peeled off at a predetermined timing when the adhesive sheet 10 is used.

[0018] The shear storage modulus of the adhesive sheet 10 at 25 ° C. is 170 kPa or less, preferably 150 kPa or less, more preferably 100 kPa or less, even more preferably 80 kPa or less, even more preferably 70 kPa or less, even more preferably 60 kPa or less, and particularly preferably 50 kPa or less, from the viewpoint of realizing the softness required for the optical adhesive sheet for flexible device use in the adhesive sheet 10. The shear storage modulus of the adhesive sheet 10 at 25 ° C. is preferably 10 kPa or more, more preferably 15 kPa or more, even more preferably 20 kPa or more, and particularly preferably 25 kPa or more, from the viewpoint of ensuring the cohesive force of the adhesive sheet 10. Examples of methods for adjusting the shear storage modulus include selecting the type of base polymer in the adhesive sheet 10, adjusting the molecular weight, adjusting the amount of the base polymer, adjusting the glass transition temperature, and adjusting the degree of crosslinking. Examples of methods for adjusting the shear storage modulus include selecting the components other than the base polymer in the adhesive sheet 10 and adjusting the amount of the base polymer. The shear storage modulus of the adhesive layer is determined by dynamic viscoelasticity measurement. The measurement can be performed using a dynamic viscoelasticity measuring device "Advanced Rheometric Expansion System (ARES)" manufactured by Rheometric Scientific. In the measurement, the measurement mode is shear mode, the measurement temperature range is -40°C to 100°C, the temperature rise rate is 5°C / min, and the frequency is 1 Hz. A sample of the adhesive sheet (adhesive sheet 10 in this embodiment) for measuring the shear storage modulus is taken from a region of the adhesive sheet that is 1 mm or more away from the end face of the adhesive sheet inward in the surface direction.

[0019] The adhesive sheet 10 has a hard end surface 11. In a plan view of the adhesive sheet 10, the hard end surface 11 defines at least a part of the outline of the adhesive sheet 10, and preferably defines the entire outline of the adhesive sheet 10 (the entire circumference of the peripheral end surface). The hard end surface 11 has a hardness H1 as a surface hardness at 25°C measured by a nanoindentation method. In addition, a portion (first portion) of the adhesive sheet 10 that is 20 μm away from the hard end surface 11 inward in the surface direction D of the adhesive sheet 10 has a hardness H2 as a surface hardness at 25°C measured by a nanoindentation method. The ratio (H1 / H2) of the hardness H1 to the hardness H2 is 1.15 or more. In FIG. 1, a portion of the adhesive sheet 10 that is a distance d away from the hard end surface 11 inward in the surface direction D is indicated by a thick arrow. Hardness H2 is the surface hardness of the first portion where the distance d is 20 μm.

[0020] Nanoindentation is a technique for measuring various physical properties of a sample on a nanometer scale. In this embodiment, the nanoindentation is performed in accordance with ISO14577. In the nanoindentation, a process of pressing an indenter into a sample set on a stage (load application process) and a process of pulling the indenter out of the sample (unloading process) are performed, and during the series of processes, the load acting between the indenter and the sample and the relative displacement of the indenter with respect to the sample are measured (load-displacement measurement). This makes it possible to obtain a load-displacement curve. From this load-displacement curve, it is possible to obtain various physical properties (hardness, elastic modulus, etc.) based on nanometer-scale measurements for the surface of the measurement sample. For load-displacement measurement by the nanoindentation method, for example, a nanoindenter (product name "Triboindenter", manufactured by Hysitron) can be used. In this measurement, the measurement mode is single indentation measurement, the measurement temperature is 25°C, the indenter used is a Berkovich (triangular pyramid) type diamond indenter (diameter 20 μm), the maximum indentation depth (maximum displacement hmax) of the indenter into the measurement sample during the load application process is 4 μm, the indenter's indentation speed is 1000 nm / sec, and the indenter's withdrawal speed from the measurement sample during the unloading process is 1000 nm / sec. The obtained measurement data is then processed by the dedicated analysis software (Ver. 9.4.0.1) for "TI950 Triboindenter". Specifically, based on the obtained load (F)-displacement (h) curve, the maximum load Fmax (load acting on the indenter at the maximum displacement hmax), the contact projected area Ap (projected area of ​​the contact region between the indenter and the sample at the maximum load), and the surface hardness (=Fmax / Ap) of the measurement sample are calculated. More specifically, the method for measuring surface hardness using the nanoindentation method is as described later in the examples.

[0021] As described above, the adhesive sheet 10 has a shear storage modulus of 170 kPa or less at 25° C. and is soft. As described above, the adhesive sheet 10 has a hard end surface 11, and the ratio (H1 / H2) of the hardness H1 of the hard end surface 11 to the hardness H2 of a portion 20 μm away from the hard end surface 11 inward in the surface direction D of the adhesive sheet 10 is 1.15 or more. Such an adhesive sheet 10 with a locally hard end surface (hard end surface 11) is suitable for suppressing unintended deformation of the end portion.

[0022] From the viewpoint of suppressing unintended deformation of the end portion, the ratio (H1 / H2) is preferably 1.50 or more, more preferably 2.00 or more, even more preferably 2.50 or more, and even more preferably 2.70 or more. From the viewpoint of suppressing cracking of the hard end surface 11, the ratio (H1 / H2) is preferably 10.0 or less, more preferably 7.00 or less, even more preferably 5.00 or less, and even more preferably 3.50 or less.

[0023] In the pressure-sensitive adhesive sheet 10, a portion (second portion) 200 μm away from the hard end surface 11 toward the inside of the surface direction D of the pressure-sensitive adhesive sheet 10 has a hardness H3 as a surface hardness at 25° C. measured by a nanoindentation method. The ratio (H1 / H3) of the hardness H1 to the hardness H3 is preferably 1.15 or more, more preferably 1.50 or more, even more preferably 2.00 or more, even more preferably 2.50 or more, and even more preferably 2.70 or more, from the viewpoint of suppressing unintended deformation of the end portion. The ratio (H1 / H3) is preferably 10.0 or less, more preferably 7.00 or less, even more preferably 5.00 or less, and even more preferably 3.50 or less, from the viewpoint of suppressing cracking of the hard end surface 11.

[0024] From the viewpoint of ensuring the softness of the first portion, the ratio (H2 / H3) of the hardness H2 of the first portion to the hardness H3 of the second portion is preferably 1.05 or less, more preferably 1.01 or less, and even more preferably 1.00 or less. From the viewpoint of ensuring the uniformity of the softness of the adhesive sheet 10, the ratio (H2 / H3) is preferably 0.90 or more, more preferably 0.93 or more, and even more preferably 0.95 or more.

[0025] The adhesive sheet 10 is formed from an adhesive composition. The adhesive composition includes a base polymer. The base polymer is an adhesive component that exhibits adhesiveness. Examples of the base polymer include an acrylic polymer, a polyurethane polymer, a polyamide polymer, and a polyvinyl ether polymer. The base polymer may be used alone or in combination of two or more kinds. From the viewpoint of ensuring good transparency and adhesiveness in the adhesive sheet 10, an acrylic polymer is preferably used as the base polymer.

[0026] An acrylic polymer is a copolymer of monomer components containing 50% by mass or more of (meth)acrylic acid ester. "(Meth)acrylic" means acrylic and / or methacrylic. As the (meth)acrylic acid ester, preferably, a (meth)acrylic acid alkyl ester is used, and more preferably, a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 20 carbon atoms is used.

[0027] Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, pentyl (meth)acrylate, n-hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (i.e., lauryl (meth)acrylate), isotridecyl (meth)acrylate, and tetradecyl (meth)acrylate. The (meth)acrylic acid alkyl ester is preferably at least one selected from the group consisting of 2-ethylhexyl acrylate (2EHA), lauryl acrylate (LA), and n-butyl acrylate. The proportion of the (meth)acrylic acid alkyl ester in the monomer components is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, from the viewpoint of properly expressing basic properties such as adhesiveness in the adhesive sheet 10, and is, for example, 99% by mass or less.

[0028] The monomer component may include a copolymerizable monomer that is copolymerizable with the (meth)acrylic acid alkyl ester. The copolymerizable monomer may include, for example, a monomer having a polar group. The polar group-containing monomer may include, for example, a hydroxy group-containing monomer, a carboxy group-containing monomer, and a monomer having a nitrogen atom-containing ring. The polar group-containing monomer is useful for modifying the acrylic polymer, such as introducing a crosslinking point into the acrylic polymer and ensuring the cohesive force of the acrylic polymer.

[0029] Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. As the hydroxyl group-containing monomer, at least one selected from the group consisting of 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate is preferably used. The ratio of the hydroxyl group-containing monomer in the monomer component is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, from the viewpoint of introducing a crosslinked structure into the acrylic polymer and ensuring the cohesive force in the pressure-sensitive adhesive sheet 10. The ratio is preferably 20% by mass or less, more preferably 15% by mass or less, from the viewpoint of adjusting the polarity of the acrylic polymer (related to the compatibility between various additive components in the pressure-sensitive adhesive sheet 10 and the acrylic polymer).

[0030] Examples of monomers having a nitrogen atom-containing ring include N-vinyl-2-pyrrolidone, acryloylmorpholine (ACMO), N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrrole, N-vinylimidazole, and N-(meth)acryloyl-2-pyrrolidone. As monomers having a nitrogen atom-containing ring, N-vinyl-2-pyrrolidone and / or ACMO are preferably used. The ratio of monomers having a nitrogen atom-containing ring in the monomer components is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, from the viewpoint of ensuring the cohesive force of the pressure-sensitive adhesive sheet 10 and ensuring the adhesive force of the pressure-sensitive adhesive sheet 10 to the adherend. From the viewpoint of adjusting the glass transition temperature of the acrylic polymer and adjusting the polarity of the acrylic polymer (related to the compatibility between the various additive components in the adhesive sheet 10 and the acrylic polymer), the proportion is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less.

[0031] The base polymer preferably has a crosslinked structure. Examples of methods for introducing a crosslinked structure into the base polymer include the following first and second methods. In the first method, a base polymer having a functional group capable of reacting with a crosslinking agent and a crosslinking agent are blended into an adhesive composition, and the base polymer and the crosslinking agent are reacted in an adhesive sheet. In the second method, a polyfunctional monomer as a crosslinking agent is included in the monomer components forming the base polymer, and a base polymer having a branched structure (crosslinked structure) introduced into the polymer chain is formed by polymerization of the monomer components. These methods may be used in combination.

[0032] The crosslinking agent used in the first method includes, for example, a compound that reacts with the functional group (such as a hydroxyl group and a carboxyl group) contained in the base polymer. Such crosslinking agents include, for example, an isocyanate crosslinking agent, a peroxide crosslinking agent, and an epoxy crosslinking agent. The crosslinking agent may be used alone or in combination of two or more kinds.

[0033] In the second method, the monomer components (including the multifunctional monomer for introducing a crosslinked structure and other monomers) may be polymerized at once or in multiple stages. In the multistage polymerization method, first, a monofunctional monomer for forming a base polymer is polymerized (preliminary polymerization), thereby preparing a prepolymer composition containing a partial polymer (a mixture of a polymer with a low degree of polymerization and an unreacted monomer). Next, a multifunctional monomer is added as a crosslinking agent to the prepolymer composition, and then the partial polymer and the multifunctional monomer are polymerized (main polymerization). As the multifunctional monomer, for example, a multifunctional (meth)acrylate containing two or more ethylenically unsaturated double bonds in one molecule can be mentioned. As the multifunctional monomer, a multifunctional acrylate is preferable from the viewpoint of being able to introduce a crosslinked structure by active energy ray polymerization (photopolymerization). Examples of the polyfunctional (meth)acrylate include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. As the polyfunctional (meth)acrylate, dipentaerythritol hexaacrylate (DPHA) is preferably used.

[0034] The acrylic polymer can be formed by polymerizing the above-mentioned monomer components. Examples of the polymerization method include solution polymerization, solvent-free photopolymerization (e.g., UV polymerization), bulk polymerization, and emulsion polymerization. Examples of the solvent used in solution polymerization include ethyl acetate and toluene. Examples of the polymerization initiator used include a thermal initiator (thermal polymerization initiator) and a photoinitiator (photopolymerization initiator).

[0035] Photoinitiators include, for example, radical photoinitiators, cationic photoinitiators, and anionic photoinitiators.

[0036] Examples of radical photoinitiators include acylphosphine oxide photoinitiators, benzoin ether photoinitiators, and acetophenone photoinitiators.

[0037] Examples of acylphosphine oxide photoinitiators include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-di-n-butoxyphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide. Examples of benzoin ether photoinitiators include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, and 2,2-dimethoxy-1,2-diphenylethan-1-one. Examples of acetophenone-based photoinitiators include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone.

[0038] The weight average molecular weight of the base polymer is preferably 100,000 or more, more preferably 300,000 or more, and even more preferably 500,000 or more, from the viewpoint of ensuring the cohesive force of the adhesive sheet 10. The weight average molecular weight is preferably 5 million or less, more preferably 3 million or less, and even more preferably 2 million or less. The weight average molecular weight of the base polymer is measured by gel permeation chromatography (GPC) and calculated in terms of polystyrene.

[0039] The glass transition temperature (Tg) of the base polymer can be determined by the following Fox formula (theoretical value). The Fox formula is a relational expression between the glass transition temperature Tg of a polymer and the glass transition temperature Tgi of a homopolymer of a monomer constituting the polymer. In the following Fox formula, Tg represents the glass transition temperature (°C) of a polymer, Wi represents the weight fraction of a monomer i constituting the polymer, and Tgi represents the glass transition temperature (°C) of a homopolymer formed from the monomer i. The glass transition temperature of a homopolymer can be determined by a literature value. For example, the glass transition temperatures of various homopolymers are listed in "Polymer Handbook" (4th edition, John Wiley & Sons, Inc., 1999). On the other hand, the glass transition temperature of a homopolymer of a monomer can also be determined by a method specifically described in JP-A-2007-51271.

[0040] Fox formula 1 / (273+Tg)=Σ[Wi / (273+Tgi)]

[0041] The glass transition temperature (Tg) of the base polymer is preferably 0° C. or lower, more preferably −10° C. or lower, and even more preferably −20° C. or lower, from the viewpoint of ensuring the softness of the pressure-sensitive adhesive sheet 10. The glass transition temperature is, for example, −80° C. or higher.

[0042] The adhesive composition preferably contains a photoinitiator. That is, the adhesive sheet 10 preferably contains a photoinitiator. Examples of the photoinitiator include the following first and second photoinitiators. The first photoinitiator is a photoinitiator (residual photoinitiator) that remains after the polymerization reaction among the photoinitiators blended in the reaction solution as a polymerization initiator for the base polymer. The second photoinitiator is a photoinitiator newly blended in the adhesive composition containing the base polymer. Examples of the photoinitiator include the photoinitiators described above as photopolymerization initiators. The adhesive composition containing a photoinitiator is suitable for forming the hard end surface 11 when the adhesive sheet 10 is manufactured by the manufacturing method described later. The content (residual amount) of the photoinitiator in the adhesive sheet 10 is preferably 0.01 parts by mass or more, more preferably 0.10 parts by mass or more, and also preferably 2.00 parts by mass or less, more preferably 1.00 parts by mass or less, per 100 parts by mass of the base polymer.

[0043] The adhesive composition may contain other components as necessary. Examples of the other components include a solvent, a silane coupling agent, an ultraviolet absorber, a tackifier, a softener, and an antioxidant. Examples of the solvent include a polymerization solvent that is used as necessary during polymerization of the base polymer, and a solvent that is added to the polymerization reaction solution after polymerization. Examples of the solvent include ethyl acetate and toluene.

[0044] The haze of the pressure-sensitive adhesive sheet 10 is preferably 3% or less, more preferably 2% or less, and even more preferably 1% or less. The haze of the pressure-sensitive adhesive sheet 10 can be measured using a haze meter in accordance with JIS K7136 (2000). Examples of haze meters include "NDH2000" manufactured by Nippon Denshoku Industries Co., Ltd. and "HM-150 type" manufactured by Murakami Color Research Laboratory Co., Ltd.

[0045] Examples of materials for the release liner 20 include polyester, polyolefin, polycarbonate, and polyimide. Examples of polyester include polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate. Examples of polyolefin include polyethylene, polypropylene, and cycloolefin polymer (COP). The thickness of the release liner 20 is preferably 5 μm or more, more preferably 10 μm or more, and is preferably 200 μm or less, more preferably 150 μm or less. The release surface 21 of the release liner 20 (the surface on the pressure-sensitive adhesive sheet 10 side) is preferably subjected to a release treatment. Examples of the release treatment include a silicone release treatment and a fluorine release treatment (the same applies to the release treatment described below).

[0046] In this embodiment, the release liner 20 has an extending end 20A. The extending end 20A extends outward from the pressure-sensitive adhesive sheet 10 in the planar direction D. The extending length of the extending end 20A in the planar direction D is, for example, more than 0 mm and, for example, 50 mm or less.

[0047] Examples of materials for release liner 30 include the materials mentioned above for release liner 20. The thickness of release liner 30 is preferably 5 μm or more, more preferably 10 μm or more, and is preferably 200 μm or less, more preferably 150 μm or less. Release surface 31 of release liner 30 (surface on the pressure-sensitive adhesive sheet 10 side) is preferably release-treated.

[0048] 2A to 2D show a method for producing an adhesive sheet 10 as one embodiment of the method for producing an optical adhesive sheet of the present invention. This production method includes a preparation step (FIG. 2A), a contour processing step (FIG. 2B), a removal step (FIG. 2C), and a cutting step (FIG. 2D). In this embodiment, this production method is a roll-to-roll method for producing an adhesive sheet X (FIG. 1) with a release liner.

[0049] 2A, a long work film W is prepared. The work film W includes a laminated sheet Y and a carrier film 104. The laminated sheet Y is a long original sheet of the adhesive sheet X with a release liner. The carrier film 104 supports the laminated sheet Y.

[0050] The laminate sheet Y comprises a long release liner 102, an adhesive layer 101, and a long release liner 103 in this order in the thickness direction H. The adhesive layer 101 is the raw material of the adhesive sheet 10, and is a long optical adhesive sheet raw material. That is, in this process, an optical adhesive sheet raw material is prepared. The release liner 102 is releasably in contact with one side of the adhesive layer 101 in the thickness direction H. The release liner 103 is releasably in contact with the other side of the adhesive layer 101 in the thickness direction H. The laminate sheet Y extends in a plane direction perpendicular to the thickness direction H. The laminate sheet Y can be produced, for example, as follows.

[0051] First, the above-mentioned pressure-sensitive adhesive composition is applied onto the release liner 102 to form a coating film. The pressure-sensitive adhesive composition used in this manufacturing method contains a photoinitiator. The content of the photoinitiator in the pressure-sensitive adhesive composition is preferably 0.01 parts by mass or more, more preferably 0.10 parts by mass or more, and preferably 2.00 parts by mass or less, more preferably 1.00 parts by mass or less, per 100 parts by mass of the base polymer. Examples of methods for applying the pressure-sensitive adhesive composition include roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating.

[0052] Next, release liner 103 is laminated onto the coating film on release liner 102. Next, the coating film is dried as necessary, and is irradiated with ultraviolet light as necessary. This forms adhesive layer 101 (optical adhesive sheet raw material) containing a photoinitiator. The drying temperature for the coating film is, for example, 50°C to 200°C. The drying time is, for example, 5 seconds to 20 minutes. Examples of light sources for ultraviolet light irradiation include ultraviolet LED lights, black lights, high-pressure mercury lamps, and metal halide lamps. The irradiation intensity of ultraviolet light irradiation is, for example, 2 to 200 mW / cm. 2 When ultraviolet light is irradiated in this step, ultraviolet light is irradiated so that at least a part of the photoinitiator in the pressure-sensitive adhesive composition remains. The content of the photoinitiator in the pressure-sensitive adhesive layer 101 formed as described above is preferably 0.01 parts by mass or more, more preferably 0.10 parts by mass or more, and preferably 2.00 parts by mass or less, more preferably 1.00 parts by mass or less, per 100 parts by mass of the base polymer.

[0053] The carrier film 104 is a single-sided adhesive film having an adhesive surface on one side in the thickness direction H. In the workpiece film W, the adhesive surface of the carrier film 104 is bonded to the release liner 102 side of the laminated sheet Y. That is, the workpiece film W specifically includes the carrier film 104, the release liner 102, the adhesive layer 101, and the release liner 103 in this order in the thickness direction H.

[0054] In this embodiment, the carrier film 104 is wider than the laminated sheet Y in a width direction D2 (FIG. 3) perpendicular to the flow direction D1 of the workpiece film W. The laminated sheet Y is disposed, for example, at the center position of the width direction D2 on the carrier film 104. The width (length in the width direction D2) of the laminated sheet Y is, for example, 200 mm or more, preferably 280 mm or more, more preferably 400 mm or more, and is, for example, 2000 mm or less, preferably 1800 mm or less, more preferably 1600 mm or less. Such a workpiece film W is run through the production line.

[0055] Next, in the contour processing step, as shown in FIG. 2B, the adhesive layer 101 on the release liner 102 is laser processed to form an adhesive sheet 10 having a predetermined shape in plan view. Specifically, the adhesive layer 101 (optical adhesive sheet raw material) is irradiated and scanned with a pulsed laser light L from the release liner 103 side, and the adhesive layer 101 and the release liner 103 are cut by multiphoton absorption of the pulsed laser light L in the adhesive layer 101 and the release liner 103 on the release liner 102. This forms a cut groove G having a depth in the thickness direction H. The cut groove G is formed so as to follow a predetermined processing planned line (design cutting line) in the work film W. In this step, the adhesive layer 101 is formed into individual adhesive sheets 10, and a peripheral portion 101a (first peripheral portion) is formed around the adhesive sheet 10. Furthermore, in the release liner 103, individualized release liners 30 are formed, and a peripheral portion 103a (second peripheral portion) is formed around the release liner 30. Fig. 3 is a plan view that shows a schematic example of an area of ​​the workpiece film W after the contour processing step. In Fig. 3, the cut grooves G are shown with hatching. The partial cross-sectional view shown in Fig. 2B corresponds to the partial cross-sectional view taken along line II in the workpiece film W shown in Fig. 3.

[0056] The pulsed laser light L is preferably a picosecond pulsed laser light or a femtosecond pulsed laser light from the viewpoint of appropriately causing multiphoton absorption in the pressure-sensitive adhesive layer 101, and more preferably a femtosecond pulsed laser light from the viewpoint of suppressing thermal denaturation of the laser-processed portion. The pulse width of the pulsed laser light L is preferably 100 fs (femtoseconds) or more and preferably 60 ps (picoseconds) or less from the viewpoint of appropriately causing multiphoton absorption in the pressure-sensitive adhesive layer 101.

[0057] The wavelength of the pulsed laser light L is preferably 500 nm or more, more preferably 800 nm or more, and even more preferably 1000 nm or more, and is preferably 2500 nm or less, more preferably 1800 nm or less, and even more preferably 1200 nm or less. Such a configuration is preferable for appropriately causing multiphoton absorption in the pressure-sensitive adhesive layer 101, and is also preferable for ensuring the cleanliness (quality) of the cut end surface.

[0058] The pulse energy of the pulsed laser light L is preferably 30 μJ or more, more preferably 40 μJ or more, and is preferably 300 μJ or less, more preferably 280 μJ or less. Such a configuration is preferable for suppressing a temperature rise at the laser-processed portion of the adhesive layer 101 to suppress thermal denaturation, and is also preferable for causing multiphoton absorption in the adhesive layer 101 appropriately.

[0059] The pulse repetition frequency of the pulsed laser light L is preferably 100 kHz or more, more preferably 200 kHz or more, from the viewpoint of appropriately causing multiphoton absorption in the adhesive layer 101 and from the viewpoint of production efficiency, and is preferably 10 MHz or less, more preferably 5 MHz or less.

[0060] From the viewpoint of achieving both the quality of the laser-processed area and manufacturing efficiency, the irradiation spot diameter of the pulsed laser light L is preferably 20 μm or more, more preferably 25 μm or more, and is preferably 90 μm or less, more preferably 80 μm or less.

[0061] Examples of the pulsed laser light L for laser processing by multiphoton absorption include gas lasers, solid lasers, and semiconductor lasers. Examples of gas lasers include excimer lasers and CO2 lasers. Examples of excimer lasers include F2 excimer lasers, ArF excimer lasers, KrF excimer lasers, and XeCl excimer lasers (numbers in parentheses indicate the laser wavelengths. The same applies below for lasers). Examples of solid lasers include Yb:YAG lasers (wavelength 1030 nm), second harmonic of Yb:YAG lasers (wavelength 515 nm), Nd:YAG lasers (1064 nm), second harmonic of Nd:YAG lasers (532 nm), third harmonic of Nd:YAG lasers (355 nm), and fourth harmonic of Nd:YAG lasers (266 nm). The pulsed laser light L is preferably selected from the group consisting of an Yb:YAG laser (wavelength 1030 nm), a second harmonic of an Yb:YAG laser (wavelength 515 nm), an Nd:YAG laser (1064 nm), and a second harmonic of an Nd:YAG laser (532 nm).

[0062] In this manufacturing method, next, as shown in FIG. 2C, the peripheral portions 101a and 103a are removed from the release liner 102 (removal step).

[0063] 2D, the long release liner 102 is cut into sheet-like release liners 20 (cutting step). Examples of cutting methods include cutting by irradiation with laser light and cutting by punching.

[0064] In this manner, the pressure-sensitive adhesive sheet 10 (optical pressure-sensitive adhesive sheet) with release liners 20, 30 can be manufactured.

[0065] As described above, the present manufacturing method includes a contour processing step of cutting the adhesive layer 101 (optical adhesive sheet raw material) containing a photoinitiator by multiphoton absorption of the pulsed laser light L. At the irradiated portion of the adhesive layer 101 with the pulsed laser light L, the polymer chain in the adhesive layer 101 is cut by multiphoton absorption of the pulsed laser light L to form a cut end surface. When the cut end surface is formed, the photoinitiator is activated by multiphoton absorption of the pulsed laser light L at the cut end surface, and a reaction (crosslinking reaction, etc.) between the resins progresses. As a result, the cut end surface is hardened, and a hard end surface 11 (FIG. 2B) of the adhesive sheet 10 is formed. In addition, cutting by multiphoton absorption of the pulsed laser light L is a cutting method that can cut the object to be cut while suppressing a rise in temperature of the object to be cut. Therefore, the contour processing step is suitable for suppressing a rise in temperature at the cut portion in the adhesive layer 101 and the surrounding area. This is suitable for restricting the length of the hardened region from the hard end surface 11 at and near the hard end surface 11 (cut end surface) of the adhesive sheet 10 formed by the contour processing step. Specifically, the hard end surface 11 can be formed without hardening a first portion of the adhesive sheet 10 that is 20 μm away from the hard end surface 11 inward in the surface direction D of the adhesive sheet 10. According to the present manufacturing method as described above, the above-mentioned adhesive sheet 10 can be appropriately manufactured. EXAMPLES

[0066] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the examples. In addition, the specific numerical values ​​of the blending amounts (contents), physical property values, parameters, etc. described below can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than") of the blending amounts (contents), physical property values, parameters, etc. corresponding to those described in the above-mentioned "Form for carrying out the invention".

[0067] Example 1 Preparation of Pressure-Sensitive Adhesive Composition C1 First, a mixture containing 71 parts by mass of butyl acrylate (BA), 13 parts by mass of N-vinyl-2-pyrrolidone (NVP), 13 parts by mass of 4-hydroxybutyl acrylate (4HBA), 3 parts by mass of acryloylmorpholine (ACMO), 0.031 parts by mass of a first photopolymerization initiator (product name "Irgacure 184", 1-hydroxy-cyclohexyl-phenyl-ketone, manufactured by BASF), and 0.031 parts by mass of a second photopolymerization initiator (product name "Irgacure 651", 2,2-dimethoxy-1,2-diphenylethane-1-one, manufactured by BASF) was irradiated with ultraviolet light (polymerization reaction) to obtain a prepolymer composition (polymerization rate of about 10%) (the prepolymer composition contains monomer components that have not undergone the polymerization reaction). Next, 100 parts by mass of the prepolymer composition, 0.6 parts by mass of a urethane acrylate oligomer (product name "UN-350", manufactured by Negami Chemical Industries Co., Ltd.) as a photopolymerizable multifunctional compound, 0.4 parts by mass of a photopolymerization initiator (product name "Irgacure 819", bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, manufactured by BASF), and 0.3 parts by mass of a silane coupling agent (product name "KBM-403", 3-glycidoxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed to obtain adhesive composition C1.

[0068] <Preparation of Laminated Sheet> First, the adhesive composition C1 was applied onto the release-treated surface of the release liner R1 as the first release liner to form a coating film. The release liner R1 is a polyethylene terephthalate (PET) film (product name "Diafoil MRF75", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) with one side treated for release with silicone. Next, the release-treated surface of the release liner R2 as the second release liner was bonded to the coating film on the release liner R1. The release liner R2 is a PET film (product name "Diafoil MRE75", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) with one side treated for release with silicone. Next, the coating film was irradiated with ultraviolet light through the release liner R2 to cure the coating film with ultraviolet light, forming a first adhesive layer with a thickness of 100 μm. For ultraviolet irradiation, a black light (manufactured by Toshiba) was used as the light source, and the irradiation intensity was 6.5 mW / cm. 2The cumulative irradiation dose was 1500 mJ / cm 2 In the ultraviolet irradiation step, a photopolymerization reaction proceeds in the coating film in a system containing the above-mentioned residual monomer and a photopolymerizable multifunctional compound (urethane acrylate oligomer), forming a photopolymerized polymer having a photocrosslinking structure. This results in a laminated sheet (release liner R1 / first adhesive layer / second release liner R2) being obtained as the base sheet for the optical adhesive sheet with release liner.

[0069] <External shape processing process> Next, the first adhesive layer of the laminate sheet was processed. Specifically, the first adhesive layer on the release liner R1 and the release liner R2 were cut in the thickness direction (laser processing) by irradiating the laminate sheet with pulsed laser light from the release liner R2 side along the first planned cutting line of the laminate sheet. In this laser processing, the first adhesive layer (optical adhesive sheet raw material) and the release liner R2 were cut on the release liner R1 by multiphoton absorption of the pulsed laser light in the laminate sheet. In the laser light irradiation, a specified laser processing device was used, and a Yb:YAG laser was used as the laser light source (laser medium), the wavelength of the laser light was 1030 nm, the pulse energy was 50 μJ, the pulse repetition frequency was 200 kHz, the pulse width was 300 fs (femtoseconds), the irradiation spot diameter was 33 μm, and the scanning speed was 60 mm / s. In this process, an optical adhesive sheet having a predetermined shape in plan view and a first peripheral portion around it were produced in the large-sized optical adhesive sheet, and a second peripheral portion was produced on the first peripheral portion in the release liner R2.

[0070] <Removal and cutting of surrounding areas> After the external shape processing process, the first and second peripheral parts were removed from the release liner R1. The release liner R1 was then cut. Specifically, a CO2 laser was irradiated in the thickness direction of the release liner R1 along the second planned cutting line of the release liner R1, thereby cutting the release liner R1 into a specified shape in plan view. The second planned cutting line is 3 mm away from the first planned cutting line in the plan direction. In addition, a laser processing device (product name "LC500", Takei Electric Industry Co., Ltd.) was used for the laser irradiation in this process, and the pulse width of the irradiated laser was set to 3.3 μs, the pulse repetition frequency was set to 15 kHz, and the laser output was set to 40 W.

[0071] In this manner, the optical adhesive sheet of Example 1 was produced as an adhesive sheet with double-sided release liners (first release liner / optical adhesive sheet (formed from adhesive composition C1, thickness 100 μm) / second release liner).

[0072] Example 2 An optical adhesive sheet of Example 2 was produced in the same manner as the optical adhesive sheet of Example 1, except for the following: In the step of producing a laminated sheet, adhesive composition C2 was used instead of adhesive composition C1, and the irradiation intensity of the ultraviolet light irradiated to the coating film between the release liners was 5 mW / cm 2 A second pressure-sensitive adhesive layer having a thickness of 100 μm was then formed between release liners R1 and R2.

[0073] In preparing the adhesive composition C2, first, a mixture containing 45 parts by mass of 2-ethylhexyl acrylate (2EHA), 42 parts by mass of lauryl acrylate (LA), 2 parts by mass of n-butyl acrylate (BA), 4 parts by mass of 4-hydroxybutyl acrylate (4HBA), 7 parts by mass of N-vinyl-2-pyrrolidone (NVP), and 0.015 parts by mass of a photopolymerization initiator (Irgacure 184) was irradiated with ultraviolet light (polymerization reaction) to obtain a prepolymer composition (polymerization rate of about 10%). Next, 100 parts by mass of the prepolymer composition, 0.08 parts by mass of dipentaerythritol hexaacrylate (DPHA) as a multifunctional acrylate monomer, and 0.3 parts by mass of a silane coupling agent (KBM-403) were mixed. In this manner, the adhesive composition C2 was obtained.

[0074] Comparative Example 1 Preparation of Pressure-Sensitive Adhesive Composition C3 First, in a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube, a mixture containing 70 parts by mass of 2-ethylhexyl acrylate (2EHA), 20 parts by mass of n-butyl acrylate (BA), 8 parts by mass of lauryl acrylate (LA), 1 part by mass of 4-hydroxybutyl acrylate (4HBA), 0.6 parts by mass of N-vinyl-2-pyrrolidone (NVP), 0.1 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator, and ethyl acetate as a solvent (solid concentration 47% by mass) was stirred under a nitrogen atmosphere at 56°C for 6 hours (polymerization reaction). As a result, a polymer solution containing an acrylic-based polymer was obtained. The weight average molecular weight of the acrylic-based polymer in this polymer solution was about 2 million. Next, 0.26 parts by mass of a first crosslinking agent (trade name "Niper BMT-40SV", dibenzoyl peroxide, manufactured by Nippon Oil & Fats Co., Ltd.), 0.02 parts by mass of a second crosslinking agent (trade name "Coronate L", trimethylolpropane / tolylene diisocyanate trimer adduct, manufactured by Tosoh Co., Ltd.), and 0.3 parts by mass of a silane coupling agent (KBM-403) were added to the polymer solution and mixed per 100 parts by mass of the solid content of the polymer solution to prepare adhesive composition C3. Adhesive composition C3 does not contain a photoinitiator.

[0075] <Preparation of Laminated Sheet> First, the adhesive composition C3 was applied onto the release-treated surface of the release liner R1 as the first release liner to form a coating film. Next, the release-treated surface of the release liner R2 as the second release liner was attached to the coating film on the release liner R1. The release liner R2 is a PET film (product name "Diafoil MRE75", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) with one side treated for silicone release. Next, the coating film between the release liners R1 and R2 was dried by heating at 100 ° C for 1 minute and then at 150 ° C for 3 minutes to form a third adhesive layer with a thickness of 100 μm. This resulted in a laminated sheet (release liner R1 / third adhesive layer / second release liner R2) being obtained as a raw material sheet for an optical adhesive sheet with a release liner.

[0076] <Shear storage modulus> For each of the optical pressure-sensitive adhesive sheets of Examples 1 and 2 and Comparative Example 1, the dynamic viscoelasticity was measured.

[0077] First, a sample sheet with a thickness of about 1.5 mm was prepared by laminating a plurality of adhesive sheet pieces cut from the optical adhesive sheet. Each adhesive sheet piece was taken from an area of ​​the optical adhesive sheet that was 300 μm or more away from the end face of the sheet inward in the surface direction. Next, this sheet was punched out to obtain a cylindrical pellet (diameter 7.9 mm) as a measurement sample.

[0078] The measurement sample was then fixed to a parallel plate jig with a diameter of 7.9 mm and subjected to dynamic viscoelasticity measurement using a dynamic viscoelasticity measuring device (name: Advanced Rheometric Expansion System (ARES), manufactured by Rheometric Scientific). In this measurement, the measurement mode was shear mode, the measurement temperature range was -40°C to 100°C, the heating rate was 5°C / min, and the frequency was 1 Hz. From the measurement results, the shear storage modulus at 25°C was read. The values ​​are shown in Table 1.

[0079] <Hardness measurement using nanoindentation method> For the end face (end face 11 in FIG. 1) of each of the optical adhesive sheets of Examples 1 and 2 and Comparative Example 1, a load-displacement measurement was performed by a nanoindentation method (first measurement).

[0080] Specifically, a nanoindenter (product name "Triboindenter", manufactured by Hysitron) was used to perform load-displacement measurements conforming to ISO14577, and load-displacement curves were obtained. In this measurement, the measurement mode was single indentation measurement, the measurement temperature was 25°C, the indenter used was a Berkovich (triangular pyramid)-type diamond indenter (diameter 20 μm), the maximum indentation depth (maximum displacement hmax) of the indenter into the measurement sample during the load application process was 4 μm, the indenter indentation speed was 1000 nm / sec, and the indenter withdrawal speed from the measurement sample during the unloading process was 1000 nm / sec. The obtained measurement data was then processed using the dedicated analysis software (Ver. 9.4.0.1) for the "TI950 Triboindenter." Specifically, based on the obtained load (F)-displacement (h) curve, the maximum load Fmax (load acting on the indenter at the maximum displacement hmax) and the contact projected area Ap (projected area of ​​the contact region between the indenter and the sample at the maximum load) were obtained. Then, the surface hardness (=Fmax / Ap) of the end face of the optical adhesive sheet was calculated from the maximum load Fmax and the contact projected area Ap. The calculated surface hardness is shown in Table 1 as hardness H1 (kPa).

[0081] Meanwhile, for each of the optical adhesive sheets of Examples 1 and 2 and Comparative Example 1, a load-displacement measurement was carried out by a nanoindentation method (second measurement).

[0082] First, the first release liner was peeled off from the optical adhesive sheet with double-sided release liner. Next, a load-displacement measurement was performed on the exposed surface of the optical adhesive sheet exposed by the peeling using a nanoindenter (product name "Triboindenter", manufactured by Hysitron) to obtain a load-displacement curve. The measurement site in the second measurement was a site 20 μm away from the end face of the optical adhesive sheet toward the inside in the surface direction of the sheet. The measurement conditions in the second measurement were the same as those in the first measurement. The obtained measurement data was then processed using a dedicated analysis software (Ver. 9.4.0.1) for "TI950 Triboindenter", and the surface hardness (=Fmax / Ap) of the site 20 μm away from the end face of the optical adhesive sheet was calculated. The calculated surface hardness is shown in Table 1 as hardness H2 (kPa). The ratio (H1 / H2) of the above hardness H1 to the hardness H2 is also shown in Table 1.

[0083] In addition, for each of the optical adhesive sheets of Examples 1 and 2 and Comparative Example 1, a load-displacement measurement was performed by the nanoindentation method in the same manner as in the second measurement except for the measurement site (third measurement). The measurement site in the third measurement was a site 200 μm away from the end face of the optical adhesive sheet toward the inside in the surface direction of the sheet. The obtained measurement data was processed by a dedicated analysis software (Ver. 9.4.0.1) for "TI950 Triboindenter", and the surface hardness (=Fmax / Ap) of the site 200 μm away from the end face of the optical adhesive sheet was calculated. The calculated surface hardness is shown in Table 1 as hardness H3 (kPa). The ratio (H1 / H3) of the above hardness H1 to the hardness H3 is also shown in Table 1.

[0084] The optical adhesive sheets of Examples 1 and 2 and Comparative Example 1 all have a shear storage modulus of 170 kPa or less at 25°C and are soft. The optical adhesive sheet of Comparative Example 1 has a ratio (H1 / H2) and a ratio (H1 / H3) below 1.15 and below 1.00. In such optical adhesive sheets, the end faces are soft as well as the internal region. In contrast, the optical adhesive sheets of Examples 1 and 2 have a ratio (H1 / H2) and a ratio (H1 / H3) of 1.15 or more and have hard end faces. Such optical adhesive sheets with locally hard end faces are suitable for suppressing unintended deformation of the end faces.

[0085] [Table 1] [Explanation of symbols]

[0086] X Adhesive sheet with release liner 10 Adhesive sheet (optical adhesive sheet) 11 Hard end face 20,30 Release liner H Thickness direction Y-Layer Sheet C. Carrier film 101 Adhesive layer (optical adhesive sheet raw material)

Claims

1. An optical adhesive sheet having a hard end surface, The optical adhesive sheet has a shear storage modulus of 170 kPa or less at 25 ° C., The hard end surface has a surface hardness H1 at 25° C. measured by a nanoindentation method, In the optical adhesive sheet, a portion 20 μm away from the hard end surface toward the inside in the surface direction of the optical adhesive sheet has a hardness H2 as a surface hardness at 25 ° C. measured by a nanoindentation method; An optical adhesive sheet having a ratio of hardness H1 to hardness H2 of 1.15 or more.

2. The optical adhesive sheet according to claim 1 , wherein the ratio is 10 or less.

3. The optical adhesive sheet according to claim 1 or 2, comprising a photoinitiator.

4. A method for producing the optical adhesive sheet according to claim 1, A preparation step of preparing an optical adhesive sheet raw material containing a photoinitiator; A method for producing an optical adhesive sheet, comprising: irradiating and scanning the optical adhesive sheet raw material with pulsed laser light; and cutting the optical adhesive sheet raw material by multiphoton absorption of the pulsed laser light in the optical adhesive sheet raw material to form the optical adhesive sheet.

5. The method for producing an optical adhesive sheet according to claim 4, wherein the pulsed laser light is picosecond pulsed laser light or femtosecond pulsed laser light.

6. The method for producing an optical adhesive sheet according to claim 4 or 5, wherein the pulsed laser light has a wavelength of 500 nm or more and 2500 nm or less.