Cyclic acid anhydride curing agent, curable resin composition and cured product thereof
A curable resin composition of cyclic acid anhydrides, produced via a Diels-Alder reaction, addresses the handling and productivity issues of existing anhydrides by maintaining a liquid state at room temperature and ensuring heat resistance, suitable for composite materials and diverse applications.
Patent Information
- Application Number
- JP2023055550
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing cyclic acid anhydrides, such as 1-isopropyl-4-methyl-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, are solid at room temperature, requiring energy-intensive heating for dissolution and leading to low productivity and handling difficulties, and mixing with other anhydrides to lower the melting point compromises heat resistance.
A curable resin composition comprising a mixture of cyclic acid anhydrides represented by specific formulas, with a high content of one anhydride maintaining liquid form at 23°C, produced through a Diels-Alder reaction of 1,3-p-mentadiene and maleic anhydride, and optionally blended with biomass-derived anhydrides to enhance stability and handling.
The composition provides a liquid curing agent with improved handling, storage stability, and maintains heat resistance, suitable for carbon fiber reinforced composite materials and various applications.
Smart Images

Figure 2024143066000001 
Figure 2024143066000002 
Figure 2024143066000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a mixture of cyclic acid anhydrides, a curable resin composition, and a cured product thereof, which are suitable for use in electrical and electronic components such as semiconductor encapsulants, printed wiring boards, and build-up laminates, lightweight, high-strength materials such as carbon fiber reinforced plastics and glass fiber reinforced plastics, 3D printing applications, and adhesives. [Background technology]
[0002] Epoxy resins are widely used in various fields due to their excellent mechanical strength, heat resistance, adhesiveness, gas barrier properties, etc. It has been well known that acid anhydrides are effective as curing agents for epoxy resins, and acid anhydrides have been used in applications such as small and large casting, impregnation molding, and powder coatings because they are less toxic and odorous than amine curing agents, and they generate less heat and shrink in volume during curing.
[0003] Hardeners such as epoxy resins and acid anhydrides have often been derived from petroleum as raw materials. In recent years, however, concerns have arisen over the depletion of petroleum resources, and methods of recycling many materials using renewable resources such as plants or by decomposing the hardened materials are being investigated. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 55-118920 [Patent Document 2] Japanese Patent Application Publication No. 01-167326 Summary of the Invention [Problem to be solved by the invention]
[0005] Patent Document 1 describes 1-isopropyl-4-methyl-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride synthesized by addition reaction of 1,3-p-menthadiene with maleic anhydride. The applicant of the present application produced 1-isopropyl-4-methyl-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride by the method described in Patent Document 1, and confirmed that it had a high melting point and was solid at room temperature.
[0006] Since 1-isopropyl-4-methyl-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride is a solid at room temperature, it is necessary to heat and dissolve the container such as a drum in an oven or hot water bath before use. However, it takes a long time to dissolve, which results in low productivity, and the large amount of energy consumed for heating is also an issue. In addition, it returns to a solid after a period of time has passed after heating, making it difficult to handle.
[0007] In Patent Document 2, an attempt is made to lower the melting point by obtaining 1-isopropyl-4-methyl-bicyclo[2.2.2]octane-2,3-dicarboxylic anhydride by subjecting the carbon-carbon double bond of 1-isopropyl-4-methyl-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride to a hydrogen reduction reaction, but the product remains solid at room temperature even if the melting point is lowered, and the problems of productivity, handling, and energy consumption similar to those in Patent Document 1 have not been solved.
[0008] In addition, in Patent Document 2, 1-isopropyl-4-methyl-bicyclo[2.2.2]octane-2,3-dicarboxylic anhydride is mixed with 1-isopropyl-4·5-dimethyl-cyclohexane-2·3-dicarboxylic anhydride in a weight ratio of 80:20 to 20:80 to produce an acid anhydride that is liquid at room temperature. However, mixing with 1-isopropyl-4·5-dimethyl-cyclohexane-2·3-dicarboxylic anhydride reduces heat resistance.
[0009] The present invention has been made in consideration of the above-mentioned problems, and an object of the present invention is to provide a cyclic acid anhydride curing agent that is liquid at 23°C, a curable resin composition, and a cyclic acid anhydride and a method for producing the same. [Means for solving the problem]
[0010] That is, the present invention is as shown in the following [1] to
[10] . In the present invention, "(Numerical value 1) to (Numerical value 2)" indicates that the upper and lower limits are included. [1] A cyclic acid anhydride curing agent (C) containing a cyclic acid anhydride mixture (A) including a cyclic acid anhydride represented by the following formula (Aa), a cyclic acid anhydride represented by the following formula (Ab), and a cyclic acid anhydride represented by the following formula (Ac), and an acid anhydride (B) different from the cyclic acid anhydride mixture (A), The content of the cyclic acid anhydride mixture (A) in the total amount of the cyclic acid anhydride curing agent (C) is 85% by weight or more, A cyclic acid anhydride hardener (C) that is liquid at 23°C.
[0011] [ka]
[0012] [2] The cyclic acid anhydride curing agent (C) according to the above item [1], wherein, when the mixture (A) of cyclic acid anhydrides is analyzed by gas chromatography, the peak area of the cyclic acid anhydride represented by the formula (Ab) is 90.0% or more and 97.5% or less, when the sum of the peak areas of the cyclic acid anhydrides represented by the formulas (Aa) to (Ac) is taken as 100%. [3] The cyclic acid anhydride curing agent (C) according to the above item [1] or [2], wherein, when the sum of the peak areas of the cyclic acid anhydrides represented by the formulas (Aa) to (Ac) is taken as 100% in a gas chromatographic analysis of the cyclic acid anhydride mixture (A), the peak area of the cyclic acid anhydride represented by the formula (Aa) is 1.0% or more and 9.0% or less, and the peak area of the cyclic acid anhydride represented by the formula (Ac) is 1.0% or more and 9.0% or less. [4] The cyclic acid anhydride curing agent (C) according to any one of the above items [1] to [3], wherein the acid anhydride component (B) contains an acid anhydride made from a raw material derived from biomass. [5] The cyclic acid anhydride curing agent (C) according to any one of the preceding items [1] to [4], which is liquid even after being left to stand for one month at room temperature of 23°C. [6] A curable resin composition comprising the cyclic acid anhydride curing agent (C) according to any one of the above items [1] to [5], an epoxy resin, and a curing accelerator. [7] A cured product obtained by curing the curable resin composition described in the above item [6]. [8] A carbon fiber reinforced composite material obtained by curing the curable resin composition according to the above item [6]. [9] A mixture (A) of cyclic acid anhydrides including a cyclic acid anhydride represented by the following formula (Aa), a cyclic acid anhydride represented by the following formula (Ab), and a cyclic acid anhydride represented by the following formula (Ac), The cyclic acid anhydride mixture (A) has a peak area of 90.0% or more and 97.5% or less of the cyclic acid anhydride represented by the following formula (Ab), when the sum of the peak areas of the cyclic acid anhydrides represented by the following formulas (Aa) to (Ac) is taken as 100% when the cyclic acid anhydride mixture (A) is analyzed by gas chromatography.
[0013] [ka]
[0014]
[10] When the mixture (A) of cyclic acid anhydrides is analyzed by gas chromatography, the peak area of the cyclic acid anhydride represented by formula (Aa) is 1.0% or more and 9.0% or less, and the peak area of the cyclic acid anhydride represented by formula (Ac) is 1.0% or more and 9.0% or less, when the sum of the peak areas of the cyclic acid anhydrides represented by formulas (Aa) to (Ac) is taken as 100%. The mixture of cyclic acid anhydrides (A) described in the preceding item [9].
[11] A method for producing the cyclic acid anhydride mixture (A) according to the above item [8] or [9], which is obtained by reacting 1,3-p-menthadiene, maleic anhydride and a solvent at 105°C or higher, and then concentrating the solvent. Effect of the Invention
[0015] According to the present invention, it is possible to provide a cyclic acid anhydride curing agent that is liquid at 23° C., a curable resin composition, and a cyclic acid anhydride and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The cyclic acid anhydride curing agent (C) of the present embodiment comprises a cyclic acid anhydride mixture (A) including a cyclic acid anhydride represented by the following formula (Aa), a cyclic acid anhydride represented by the following formula (Ab), and a cyclic acid anhydride represented by the following formula (Ac), and an acid anhydride (B) different from the cyclic acid anhydride mixture (A). Since the cyclic acid anhydride curing agent (C) is liquid at 23° C., it has good handleability and can be used for carbon fiber reinforced composite materials.
[0017] [ka]
[0018] When the mixture (A) of cyclic acid anhydrides is analyzed by gas chromatography, the sum of the peak areas of the cyclic acid anhydrides represented by the formulas (Aa) to (Ac) is taken as 100%, and the peak area of the cyclic acid anhydride represented by the formula (Aa) is preferably 1.0% or more and 9.0% or less, more preferably 1.5% or more and 5.0% or less, and particularly preferably 1.5% or more and 3.0% or less.
[0019] When the mixture (A) of cyclic acid anhydrides is analyzed by gas chromatography, the peak area of the cyclic acid anhydride represented by formula (Ab) is preferably 90.0% or more and 97.5% or less, more preferably 93.0% or more and 97.3% or less, and particularly preferably 95.0% or more and 97.1% or less, when the sum of the peak areas of the cyclic acid anhydrides represented by formulas (Aa) to (Ac) is taken as 100%.
[0020] When the mixture (A) of cyclic acid anhydrides is analyzed by gas chromatography, the sum of the peak areas of the cyclic acid anhydrides represented by the formulas (Aa) to (Ac) is taken as 100%, and the peak area of the cyclic acid anhydride represented by the formula (Ac) is preferably 1.0% or more and 9.0% or less, more preferably 1.2% or more and 5.0% or less, and even more preferably 1.2% or more and 3.0% or less.
[0021] The gas chromatography analysis was carried out under the following conditions. Gas chromatography (GC) measurements Equipment: 8890GC System (Agilent Technologies) Column: HP-5MS (Agilent Technologies) Column flow rate: 1.2 ml / min Oven: 100℃ (2min) - 5℃ / min - 300℃ (3min) Injection port: 300℃, injection volume 1.0 μl Detector: FID (300 °C)
[0022] The mixture (A) of cyclic acid anhydrides of this embodiment can be easily obtained by addition reaction of 1,3-p-menthadiene and maleic anhydride. The addition reaction conditions are the same as those of the usual Diels-Alder reaction. In other words, the reaction ratio is preferably about equimolar or slightly excess of maleic anhydride to 1,3-p-menthadiene.
[0023] The reaction may be carried out in a suitable solvent, such as aromatic hydrocarbons and alicyclic hydrocarbons (eg, n-heptane, benzene, toluene, xylene, cyclohexane, etc.).
[0024] The reaction temperature is preferably 100 to 200° C., and more preferably 105 to 185° C. By carrying out the reaction within the above temperature range, the component ratio of the cyclic acid anhydrides represented by the formulas (Aa) to (Ac) falls within a specific range, and the cyclic acid anhydride curing agent of the present embodiment is easily turned into a liquid.
[0025] The acid anhydride (B) (hereinafter also simply referred to as "acid anhydride (B)") used in the cyclic acid anhydride curing agent of this embodiment, which is different from the mixture (A) of cyclic acid anhydrides, is not particularly limited as long as it can be handled as a liquid at 23 ° C. by blending it with the mixture (A) of cyclic acid anhydrides, but examples thereof include phthalic anhydride, maleic anhydride, trimellitic anhydride, pyromellitic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methylnadic anhydride, nadic anhydride, glutaric anhydride, dimethylglutaric anhydride, diethylglutaric anhydride, succinic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, etc. Among these, at least one selected from the group consisting of phthalic anhydride, trimellitic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, glutaric anhydride, dimethylglutaric anhydride and diethylglutaric anhydride is preferred.
[0026] From the viewpoint of reducing the environmental load, it is preferable to use an acid anhydride (B) made from a biomass-derived raw material. For example, a carboxylic acid anhydride obtained by subjecting a biomass-derived conjugated diene raw material and an unsaturated acid carboxylic acid anhydride to a Diels-Alder reaction and a subsequent hydrogen reduction reaction may be used. It is preferable that both the conjugated diene raw material and the unsaturated acid carboxylic acid anhydride used in the Diels-Alder reaction and the subsequent hydrogen reduction reaction are biomass-derived raw materials, but only one of them may be a biomass-derived raw material.
[0027] The biomass-derived conjugated diene raw material is not particularly limited, but chain terpenes (myrcene, ocimene, alloocimene, farnesene) and monocyclic terpenes (α-terpinene, α-, β-phellandrene, isopinolene) are preferred.
[0028] The biomass-derived unsaturated carboxylic acid anhydride is not particularly limited, but itaconic anhydride and citraconic anhydride are preferred.
[0029] In the total amount of the cyclic acid anhydride curing agent (C) of this embodiment, the content of the cyclic acid anhydride mixture (A) is preferably 85% by weight or more, more preferably 90% by weight or more, and the upper limit of the content of the cyclic acid anhydride mixture (A) is preferably 98% by weight or less, more preferably 95% by weight or less.
[0030] The mixture of cyclic acid anhydrides (A) and the acid anhydride (B) may be melt-mixed after being separately produced, or may be produced by reacting and distilling the two raw materials in a predetermined ratio.
[0031] The cyclic acid anhydride curing agent (C) of the present embodiment is liquid at 23° C., but it is more preferable that it maintains its liquid state even after long-term storage at 23° C., i.e., that it has excellent storage stability. Specifically, it is preferable that it remains liquid without crystal precipitation even after being left to stand at room temperature of 23° C. for one month.
[0032] The curable resin composition of the present embodiment includes the cyclic acid anhydride curing agent (C), an epoxy resin, and a curing accelerator. The epoxy resin is not particularly limited and can be appropriately selected from commonly used epoxy resins. Among them, an epoxy resin having two or more epoxy groups in one molecule is preferable. Examples of epoxy resins having two or more epoxy groups in one molecule include various polyfunctional epoxy resins such as naphthalene type, phenol novolac type, cresol novolac type, phenol aralkyl type, biphenyl type, hydroxybenzaldehyde type, dicyclopentadiene type, glycidyl ester type, glycidyl amine type, hydantoin type, and isocyanurate type. These epoxy resins may be used alone or in combination of two or more types.
[0033] The epoxy equivalent of the epoxy resin is not particularly limited, but from the viewpoint of the heat resistance and water absorbency of the cured product, it is preferably 100 to 350 (g / eq), and more preferably 150 to 300 (g / eq).
[0034] From the viewpoints of heat resistance, electrical properties and water absorbency, the epoxy resin is preferably at least one type of multifunctional epoxy resin selected from the group consisting of dicyclopentadiene type, o-cresol novolac type, naphthalene type, biphenyl type, phenol aralkyl type and trisphenolmethane type, and has an epoxy equivalent of 100 to 350 (g / eq), and more preferably at least one type of multifunctional epoxy resin selected from the group consisting of dicyclopentadiene type, o-cresol novolac type, naphthalene type and trisphenolmethane type, and has an epoxy equivalent of 150 to 300 (g / eq).
[0035] The content of the epoxy resin in the curable resin composition is not particularly limited. From the viewpoints of moldability and heat resistance, the content is preferably 10% by weight to 80% by weight, and more preferably 40% by weight to 50% by weight, based on the total weight of the curable resin composition.
[0036] In the curable resin composition of the present embodiment, the amount of the cyclic acid anhydride curing agent (C) used is preferably 0.7 to 1.2 equivalents relative to 1 equivalent of the epoxy group of the epoxy resin. If the amount is less than 0.7 equivalents relative to 1 equivalent of the epoxy group or exceeds 1.2 equivalents, curing may be incomplete and good cured properties may not be obtained.
[0037] In addition to the cyclic acid anhydride curing agent (C), the curable resin composition may further contain other curing agents as necessary. The other curing agents can be appropriately selected from the curing agents usually used in curable resin compositions. Examples of the other curing agents include phenolic resins.
[0038] The curable resin composition of the present embodiment can also adjust the gelation time by using a curing accelerator. Examples of curing accelerators that can be used include imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole, tertiary amines such as 2-(dimethylaminomethyl)phenol and 1,8-diaza-bicyclo[5,4,0]undecene-7, phosphines such as triphenylphosphine, and metal compounds such as tin octylate. The curing accelerator is used in an amount of 0.01 to 5.0 parts by weight per 100 parts by weight of the epoxy resin, as necessary.
[0039] The curable resin composition of the present embodiment may further contain various additives as exemplified below, as necessary. However, the curable resin composition of the present embodiment is not limited to the additives below, and may contain various additives well known in the art, as necessary.
[0040] The curable resin composition of the present embodiment may further contain a flame retardant as necessary for the purpose of imparting flame retardancy. The flame retardant is not particularly limited, and examples thereof include phosphorus compounds such as red phosphorus, phosphoric acid esters, and triphenylphosphine oxide coated with a thermosetting resin such as a phenolic resin; nitrogen-containing compounds such as melamine, melamine derivatives, melamine-modified phenolic resins, compounds having a triazine ring, cyanuric acid derivatives, and isocyanuric acid derivatives; phosphorus and nitrogen-containing compounds such as cyclophosphazene; metal complex compounds such as dicyclopentadienyl iron; zinc compounds such as zinc oxide, zinc stannate, zinc borate, and zinc molybdate; metal oxides such as iron oxide and molybdenum oxide; metal hydroxides such as aluminum hydroxide and magnesium hydroxide; and composite metal hydroxides represented by the following composition formula (A). Examples of the flame retardant include known organic or inorganic compounds and metal hydroxides containing halogen atoms, antimony atoms, nitrogen atoms, or phosphorus atoms.
[0041] The curable resin composition of the present embodiment may further contain an inorganic filler as necessary. Specific examples of the inorganic filler include fine powders of fused silica, crystalline silica, glass, alumina, calcium carbonate, zirconium silicate, calcium silicate, silicon nitride, aluminum nitride, boron nitride, beryllia, zirconia, zircon, fosterite, steatite, spinel, mullite, titania, talc, clay, mica, etc., or beads obtained by sphering these.
[0042] Inorganic fillers having a flame retardant effect may be used, such as aluminum hydroxide, magnesium hydroxide, composite metal hydroxides such as a composite hydroxide of magnesium and zinc, and zinc borate.
[0043] When the curable resin composition contains an inorganic filler, its content is not particularly limited as long as the effect of this embodiment can be obtained. The content of the inorganic filler is preferably 50% by weight or more in the total weight of the curable resin composition, more preferably 60% by weight to 95% by weight from the viewpoint of flame retardancy, and even more preferably 70% by weight to 90% by weight. By containing an inorganic filler, the thermal expansion coefficient, thermal conductivity, elastic modulus, etc. of the cured product can be improved to desired properties. When the content of the inorganic filler is 50% by weight or more, the effect of improving these properties can be obtained more effectively. Also, when it is 95% by weight or less, the viscosity increase of the curable resin composition is more suppressed, sufficient fluidity is easily obtained, and moldability is further improved.
[0044] The curable resin composition of the present embodiment may further contain an antioxidant as necessary. This can prevent oxidation of the cured product of the curable resin composition, and can suppress weight loss of the cured product even when left in a high-temperature environment. Electrical properties are further improved.
[0045] Examples of the antioxidant include phenol-based antioxidants, phosphite-based antioxidants, sulfur-based antioxidants, hindered amine-based antioxidants, etc. These antioxidants may be used alone or in combination of two or more.
[0046] When the curable resin composition contains an antioxidant, the content is not particularly limited as long as the weight loss suppression effect is achieved. From the viewpoint of the heat resistance (high Tg) of the curable resin composition, the content of the antioxidant is preferably 0.5 parts by weight to 20 parts by weight, more preferably 1 part by weight to 10 parts by weight, based on 100 parts by weight of the total amount of the epoxy resin. By making the content of the antioxidant 0.5 parts by weight or more, the effect of suppressing the weight loss of the cured product can be sufficiently obtained, and by making the content of the antioxidant 20 parts by weight or less, the heat resistance (high Tg) of the cured product is suppressed from decreasing.
[0047] The curable resin composition of the present embodiment may further contain a coupling agent as necessary. This improves the adhesion between the resin component and the inorganic filler, and improves the electrical properties. The coupling agent may be appropriately selected from compounds that are commonly used. Examples of the coupling agent include known coupling agents such as various silane-based compounds such as epoxysilane, mercaptosilane, aminosilane, alkylsilane, ureidosilane, vinylsilane, styrylsilane, methacrylsilane, acrylicsilane, and sulfidosilane, titanium-based compounds, aluminum chelate compounds, and aluminum / zirconium-based compounds. Among these, silane-based compounds are preferred. These coupling agents may be used alone or in combination of two or more.
[0048] When the curable resin composition contains a coupling agent, the content is preferably 0.05 to 5.0 parts by weight, and more preferably 0.1 to 4.5 parts by weight, based on 100 parts by weight of the total amount of the inorganic filler. By making the content 0.05 parts by weight or more, the adhesion to the frame, etc. can be further improved.
[0049] The method for preparing the curable resin composition of the present embodiment is not particularly limited, but each component may be mixed uniformly or may be prepolymerized. For example, a mixture containing the compound of the present embodiment is heated in the presence or absence of a curing accelerator or a polymerization initiator, and in the presence or absence of a solvent to form a prepolymer. Similarly, an amine compound, a compound having an ethylenically unsaturated bond, a maleimide compound, a cyanate ester compound, polybutadiene and its modified products, polystyrene and its modified products, inorganic fillers, and other additives may be added to form a prepolymer. The mixing or prepolymerization of each component is carried out using, for example, an extruder, a kneader, a roll, or the like in the absence of a solvent, and a reaction kettle with a stirrer in the presence of a solvent.
[0050] The curable resin composition of the present embodiment is obtained by uniformly mixing the above-mentioned components. The method for producing the curable resin composition of the present embodiment is not particularly limited, but for example, the composition can be obtained by thoroughly mixing the epoxy resin with a curing agent, a curing accelerator, an inorganic filler, a mold release agent, a silane coupling agent, an additive, etc., using an extruder, a kneader, a roll, a planetary mixer, etc., until the mixture is uniform.
[0051] The obtained curable resin composition can be formed into various forms such as a resin sheet, a prepreg, etc. The prepreg form can be obtained, for example, by heating and melting the curable resin composition and / or the resin sheet of the present embodiment to reduce the viscosity and impregnating the composition into a fiber substrate.
[0052] The curable resin composition of the present embodiment may be dissolved in a solvent such as toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, dimethylformamide, dimethylacetamide, or N-methylpyrrolidone as necessary to form a varnish-like composition (hereinafter, simply referred to as varnish), which may be impregnated into a substrate such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, alumina fiber, or paper, and dried by heating to produce a prepreg. The solvent used in this case is in an amount that occupies 10 to 70% by weight, preferably 15 to 70% by weight, of the mixture of the curable resin composition of the present embodiment and the solvent.
[0053] The prepreg is cut into a desired shape, laminated, and then the epoxy resin composition is heated and cured while applying pressure to the laminate by press molding, autoclave molding, sheet winding molding, etc., to obtain a carbon fiber reinforced plastic (CFRP). Copper foil or an organic film can also be laminated when laminating the prepreg.
[0054] In addition to the above-mentioned methods, CFRP can also be obtained by molding using known methods. For example, a resin transfer molding technique (RTM method) can be used in which a carbon fiber substrate (usually a carbon fiber fabric) is cut, laminated, and shaped to prepare a preform (a preform before being impregnated with resin), the preform is placed in a mold, the mold is closed, resin is injected to impregnate the preform, and the resin is hardened, and then the mold is opened to remove the molded product. In addition, a type of RTM method, such as the VaRTM method, the SCRIMP (Seeman's Composite Resin Infusion Molding Process) method, and the CAPRI (Controlled Atmospheric Pressure Resin Infusion) method, which is described in JP-T 2005-527410, can be used, which more appropriately controls the resin injection process, especially the VaRTM method, by evacuating a resin supply tank to a pressure lower than atmospheric pressure, using cyclic compression, and controlling the net molding pressure. In addition, other methods that can be used include the film stacking method, in which the fiber substrate is sandwiched between resin sheets (films), the method of attaching powdered resin to the reinforcing fiber substrate to improve impregnation, the molding method (Powder Impregnated Yarn) that uses a fluidized bed or fluid slurry method in the process of mixing the resin into the fiber substrate, and the method of blending resin fibers into the fiber substrate.
[0055] Examples of carbon fibers include acrylic, pitch, and rayon carbon fibers, and among them, acrylic carbon fibers having high tensile strength are preferably used. As the form of carbon fibers, twisted yarn, untwisted yarn, non-twisted yarn, etc. can be used, but untwisted yarn or non-twisted yarn is preferably used because it has a good balance between the formability and strength properties of the fiber-reinforced composite material.
[0056] The cured product of the curable resin composition of the present embodiment can be used for various applications other than the above-mentioned applications such as CFRP. Examples of the applications include adhesives, paints, coating agents, molding materials (including sheets, films, CFRP, etc.), encapsulants for semiconductor elements, encapsulants for liquid crystal display elements, encapsulants for organic EL elements, printed wiring boards (BGA substrates, build-up substrates, etc.), and electric / electronic parts, 3D printing, as well as additives for other resins, etc.
[0057] The adhesives include adhesives for civil engineering, construction, automobiles, general office use, medical use, and adhesives for electronic materials. Among these, adhesives for electronic materials include interlayer adhesives for multilayer boards such as build-up boards, die bonding agents, semiconductor adhesives such as underfills, underfills for reinforcing BGAs, and mounting adhesives such as anisotropic conductive films (ACFs) and anisotropic conductive pastes (ACPs), and are applicable to various uses.
[0058] When the curable resin composition of this embodiment is applied to a semiconductor element encapsulant, the curable resin composition of this embodiment is placed on a lead frame equipped with a semiconductor element, a semiconductor package substrate, and molded by a melt casting method, a transfer molding method, an injection molding method, a compression molding method, or the like, and further heated at 80 to 200° C. for 2 to 10 hours to obtain a cured product. Examples of semiconductor devices manufactured using this encapsulant include potting, dipping, and transfer mold encapsulation for capacitors, transistors, diodes, light-emitting diodes, ICs, and LSIs, potting encapsulation for COB, COF, TAB, and the like of ICs and LSIs, underfill for flip chips, and encapsulation (including reinforcing underfill) when mounting IC packages such as QFP, BGA, and CSP.
[0059] When the curable resin composition of the present embodiment is applied to a printed wiring board application, a prepreg can be obtained by heating and melting the composition to reduce the viscosity and impregnating the composition into reinforcing fibers such as glass fibers and polyamide fibers. Specific examples of the composition include glass fibers such as E glass cloth, D glass cloth, S glass cloth, Q glass cloth, spherical glass cloth, NE glass cloth, and T glass cloth, and / or organic fibers, but are not particularly limited thereto. The shape of the substrate is not particularly limited, but examples include woven fabric, nonwoven fabric, roving, chopped strand mat, and the like. In addition, as the weaving method of the woven fabric, plain weave, sash weave, twill weave, and the like are known, and these known weaves can be appropriately selected and used according to the intended application and performance. In addition, woven fabrics that have been subjected to fiber opening treatment or glass woven fabrics that have been surface-treated with a silane coupling agent or the like are preferably used. The thickness of the substrate is not particularly limited, but is preferably about 0.01 to 0.4 mm. Moreover, the varnish can be impregnated into reinforcing fibers and dried by heating to obtain a prepreg, which can be used to prepare a copper clad laminate (CCL). The obtained prepreg and CCL can be hot-press molded to prepare a laminate using the curable resin composition of the present embodiment. The laminate is not particularly limited as long as it has one or more prepregs, and may have any other layers. Moreover, a sheet-shaped adhesive can be obtained by applying the varnish onto a release film, removing the solvent under heating, and performing B-stage formation. This sheet-shaped adhesive can be used as an interlayer insulating layer in a multilayer board or an adhesive sheet when mounting a semiconductor. The curable resin composition of the present embodiment can also be suitably used for special board materials such as package boards (substrates) and HDI (high density interconnect). EXAMPLES
[0060] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples in any way.
[0061] Various analytical methods were carried out under the following conditions. ·GC / MS measurement (EI, CI) Equipment: GC-2020Plus / GCMS-QP2020 (Shimadzu Corporation) Column: HP-5MS (Agilent Technologies) Column flow rate: 1.2 ml / min Oven: 50℃ (2min)-10℃ / min-300℃ (18min) Mass range: m / z 35~800 Ion source: 230℃ Inlet: 320 ℃, injection volume 1.0 μl
[0062] ·GC measurement Equipment: 8890GC System (Agilent Technologies) Column: HP-5MS (Agilent Technologies) Column flow rate: 1.2 ml / min Oven: 100℃ (2 min) - 5℃ / min - 300℃ (3 min) Injection port: 300℃, injection volume 1.0 μl Detector: FID (300 °C)
[0063] [Synthesis Example 1] 25.8 parts of α-terpinene (1,3-p-menthadiene, manufactured by Guangxi Jie Xin Fragrance Co., Ltd.) was placed in a four-neck flask and heated to 185°C while stirring. 16.7 parts of maleic anhydride (manufactured by Junsei Chemical Co., Ltd.) was added to this solution in four portions over one hour. After the addition was completed, the mixture was stirred at 185°C for three hours. After the reaction was completed, the mixture was concentrated under reduced pressure at 185°C to obtain 37 parts of a mixture of cyclic acid anhydrides (A-1).
[0064] [Synthesis Example 2] The same procedure as in Synthesis Example 1 was carried out except that the reaction temperature was changed to 150° C., and 35 parts of a cyclic acid anhydride mixture (A-2) was obtained.
[0065] [Synthesis Example 3] The same procedure as in Synthesis Example 1 was carried out except that the reaction temperature was changed to 125° C., and 35 parts of a cyclic acid anhydride mixture (A-3) was obtained.
[0066] [Synthesis Example 4] The same procedure as in Synthesis Example 1 was carried out except that the reaction temperature was changed to 105° C., and 35 parts of a cyclic acid anhydride mixture (A-4) was obtained.
[0067] [Synthesis Example 5] The same procedure as in Synthesis Example 1 was carried out except that the reaction temperature was changed to 85° C., and 35 parts of a cyclic acid anhydride mixture (A-5) was obtained.
[0068] [Synthesis Example 6] The same procedure as in Synthesis Example 1 was carried out except that the reaction temperature was changed to 65°C, and 35 parts of a cyclic acid anhydride mixture (A-6) was obtained.
[0069] [Synthesis Example 7] A four-neck flask was charged with 49.1 parts of toluene and 25.8 parts of α-terpinene, which were then heated to 45°C and stirred. 16.7 parts of maleic anhydride were added to this solution in four portions over one hour. After the addition was complete, the mixture was stirred at 45°C for three hours. After the reaction was complete, the mixture was concentrated under reduced pressure at 185°C to obtain 37 parts of a mixture of cyclic acid anhydrides (A-7).
[0070] [Synthesis Example 8] 100 parts of alloocimene was placed in a four-neck flask and heated to 135°C while stirring. 72.6 parts of maleic anhydride was added to this solution in 4 portions over 1 hour. After the addition was completed, the mixture was stirred at 45°C for 3 hours. After the reaction was completed, the mixture was concentrated under reduced pressure at 185°C to obtain 225 parts of a mixture of cyclic acid anhydrides (B-3).
[0071] [Synthesis Example 9] 127 parts of myrcene was placed in a four-neck flask and heated to 125°C while stirring. 68 parts of maleic anhydride was added to this solution in 4 portions over 1 hour. After the addition was completed, the mixture was stirred at 125°C for 3 hours. After the reaction was completed, the mixture was concentrated under reduced pressure at 185°C to obtain 259 parts of a mixture of cyclic acid anhydrides (B-4).
[0072] The structures of the mixtures of cyclic acid anhydrides obtained in Synthesis Examples 1 to 9 were identified by GC / MS measurement. The area percentage results obtained by GC measurement are shown in Table 1. The structures of the mixtures of cyclic acid anhydrides obtained in Synthesis Examples 1 to 9 were identified by GC / MS measurement, and the area percentages when the sum of the peak areas of the cyclic acid anhydrides represented by formulae (Aa) to (Ac) measured by GC was taken as 100% are shown in Table 1.
[0073] [Table 1]
[0074] The melting point and crystallization rate were measured under the following conditions. <Melting point measurement conditions> Differential scanning calorimeter: Linseis CHIP DSC Gas flow rate: N 2 Gas 50ml / min Heating rate: 20℃ / min Measurement temperature range: 30℃-270℃
[0075] <Crystallization confirmation> The mixtures of cyclic acid anhydrides obtained in Synthesis Examples 1 to 9 were mixed in the compositions shown in Table 2, and left to stand at room temperature (23° C.) for one month, and visually confirmed whether crystals were precipitated. Compositions that were partially crystallized were described as solid.
[0076] [Table 2]
[0077] B-1: KAHAHARD MCD (manufactured by Nippon Kayaku Co., Ltd., methylnadic anhydride) B-2: Rikacid MH (Methylhexahydrophthalic anhydride, manufactured by New Japan Chemical Co., Ltd.)
[0078] As shown in Tables 1 and 2, the cyclic acid anhydride curing agent of the present invention has a low melting point and can be used in liquid form even when the cyclic acid anhydride mixture is used in a high blend ratio of 85% by weight. Therefore, the curable resin composition containing the cyclic acid anhydride curing agent of the present invention can be suitably used for carbon fiber reinforced composite materials.
Claims
1. A cyclic acid anhydride curing agent (C) containing a cyclic acid anhydride mixture (A) including a cyclic acid anhydride represented by the following formula (A-a), a cyclic acid anhydride represented by the following formula (A-b), and a cyclic acid anhydride represented by the following formula (A-c), and an acid anhydride (B) different from the cyclic acid anhydride mixture (A), The content of the cyclic acid anhydride mixture (A) in the total amount of the cyclic acid anhydride curing agent (C) is 85% by weight or more, A cyclic acid anhydride curing agent (C) that is liquid at 23°C. 【Chemistry 1】
2. 2. The cyclic acid anhydride curing agent (C) according to claim 1, wherein, when the mixture (A) of cyclic acid anhydrides is analyzed by gas chromatography, the peak area of the cyclic acid anhydride represented by the formula (A-b) is 90.0% or more and 97.5% or less, when the sum of the peak areas of the cyclic acid anhydrides represented by the formulas (A-a) to (A-c) is taken as 100%.
3. 3. The cyclic acid anhydride curing agent (C) according to claim 2, wherein, when the sum of the peak areas of the cyclic acid anhydrides represented by the formulas (A-a) to (A-c) in a gas chromatographic analysis of the cyclic acid anhydride mixture (A) is taken as 100%, the peak area of the cyclic acid anhydride represented by the formula (A-a) is 1.0% or more and 9.0% or less, and the peak area of the cyclic acid anhydride represented by the formula (A-c) is 1.0% or more and 9.0% or less.
4. The cyclic acid anhydride curing agent (C) according to claim 1, wherein the acid anhydride component (B) contains an acid anhydride made from a raw material derived from biomass.
5. The cyclic acid anhydride curing agent (C) according to claim 1, which is liquid even after being left to stand at room temperature of 23°C for one month.
6. A curable resin composition comprising the cyclic acid anhydride curing agent (C) according to any one of claims 1 to 5, an epoxy resin, and a curing accelerator.
7. A cured product obtained by curing the curable resin composition according to claim 6.
8. A carbon fiber reinforced composite material obtained by curing the curable resin composition according to claim 6.
9. A mixture (A) of cyclic acid anhydrides including a cyclic acid anhydride represented by the following formula (A-a), a cyclic acid anhydride represented by the following formula (A-b), and a cyclic acid anhydride represented by the following formula (A-c), The cyclic acid anhydride mixture (A) has a peak area of 90.0% or more and 97.5% or less of a cyclic acid anhydride represented by the following formula (A-b), when the sum of the peak areas of the cyclic acid anhydrides represented by the following formulas (A-a) to (A-c) is taken as 100% when the cyclic acid anhydride mixture (A) is analyzed by gas chromatography. 【Chemistry 2】
10. The cyclic acid anhydride mixture (A) according to claim 9, wherein, when the sum of the peak areas of the cyclic acid anhydrides represented by the formulas (A-a) to (A-c) is taken as 100% in a gas chromatographic analysis of the cyclic acid anhydride mixture (A), the peak area of the cyclic acid anhydride represented by the formula (A-a) is 1.0% or more and 9.0% or less, and the peak area of the cyclic acid anhydride represented by the formula (A-c) is 1.0% or more and 9.0% or less.
11. The method for producing the cyclic acid anhydride mixture (A) according to claim 9 or 10, which is obtained by reacting 1,3-p-menthadiene, maleic anhydride and a solvent at 105°C or higher, and then concentrating the solvent.
Citation Information
Patent Citations
Curable epoxy resin composition
JP1980118920A
Epoxy resin composition
JP1989167326A
Flux for soldering
JP1996090284A
Epoxy resin composition and epoxy resin composition for sealing light-emitting element
JP2004339319A
Volatile binder composition
JP2007217603A
Cited By
Mixture of cyclic acid anhydrides, curable resin composition and cured product thereof
JP2024143065A