Resin composition for powder bed fusion bonding, molded article, and method for producing molded article
A resin composition for 3D printing, combining propylene polymer, thermoplastic elastomer, and filler, addresses the balance of rigidity and impact resistance, facilitating easy powder processing and diverse applications.
Patent Information
- Application Number
- JP2023055828
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing 3D printing methods for resin-based molding, such as powder bed fusion, fail to achieve a balance of rigidity and impact resistance, and the resulting products are difficult to process into powder form for further shaping.
A resin composition comprising a specific propylene polymer, thermoplastic elastomer, and filler, formulated to specific ratios and properties, including melt flow rates, crystallization heat, and particle sizes, to enhance rigidity, impact resistance, and dispersibility.
The composition allows for the production of molded articles with excellent rigidity and impact resistance, enabling easy processing into powder form for further shaping and wide-ranging applications.
Smart Images

Figure 2024143251000001 
Figure 2024143251000002 
Figure 2024143251000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition for powder bed fusion bonding, more specifically, to a resin composition for powder bed fusion bonding, which contains a specific propylene-based polymer (A), a thermoplastic elastomer (B) and a filler (C). The present invention also relates to a molded article using the resin composition for powder bed fusion bonding and a method for producing the same. [Background technology]
[0002] Traditionally, injection molding, film molding, blow molding, sheet molding, thermoforming, etc. have been used as methods for molding resin, but in recent years, 3D printers have been attracting attention as a molding method for more complex shaped three-dimensional objects. There are various methods for 3D printers, such as the Material Extrusion (MEX) method, which melts and deposits resin filaments, the Material Jetting method, which hardens resin discharged from an inkjet head with ultraviolet light, the Vacuum PhotoPolymerization (VP) method, which laminates hardened layers of photocurable resin solutions using a laser, and the Powder Bed Fusion (PBF) method, which sinters a deposited layer of powder material with a laser. However, it is known that the rigidity and impact resistance of the molded object obtained by any of these methods are lower than those obtained by injection molding.
[0003] To solve this problem, Patent Document 1 proposes a powder for three-dimensional modeling that contains a filler containing silicon dioxide as a main component, thereby improving the strength of the three-dimensional modeled object. Moreover, Patent Document 2 proposes a powder that can be 3D printed and has high impact resistance by containing an olefin thermoplastic elastomer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-93515 A [Patent Document 2] International Publication No. 2022 / 023195 Summary of the Invention [Problem to be solved by the invention]
[0005] The problem that the present invention aims to solve is, in view of the current state of the prior art, to provide a resin composition for powder bed fusion bonding, which can give a molded body having an excellent balance of rigidity and impact resistance, and which further has excellent grindability such that it is easily processed into a powder form, and which, after powder processing, has excellent powder spreadability when forming a molded body by the powder bed fusion bonding method. [Means for solving the problem]
[0006] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that a resin composition containing a specific propylene-based polymer (A), a thermoplastic elastomer (B), and a filler (C) in a specific ratio can solve the above problems. Based on these findings, the present invention has been completed.
[0007] That is, the gist of the present invention is as follows.
[0008] [1] A resin composition for powder bed fusion bonding, comprising 100 parts by weight of a propylene-based polymer (A) satisfying the following requirements (Ai) to (A-iii), 10 to 250 parts by weight of a thermoplastic elastomer (B), and 10 to 150 parts by weight of a filler (C). Requirement (Ai): The melt flow rate at 230°C (230°C, 2.16 kg load) is 0.1 to 30 g / 10 min. Requirement (A-ii): The polymer comprises 50 to 95% by weight of a propylene homopolymer portion (a1) and 5 to 50% by weight of a propylene / α-olefin copolymer portion (a2). Requirement (A-iii): The copolymer portion (a2) is a copolymer portion having a propylene unit content of 30 to 80% by weight and an α-olefin unit content of 20 to 70% by weight.
[0009] [2] A resin composition for powder bed fusion bonding according to [1], characterized in that it satisfies the following requirement (I): Requirement (I): In differential scanning calorimetry, the melting peak temperature (Tm) observed in the first heating is 150-170°C, and the total amount of heat of crystallization (ΔH) observed in the first heating is 30-80 J / g. However, in differential scanning calorimetry, the temperature is raised from 23°C to 200°C at a rate of 10°C / min, which is the first heating, then held at 200°C for 5 minutes, and then cooled to 40°C at a rate of 10°C / min, which is the first heating.
[0010] [3] The resin composition for powder bed fusion bonding according to [1] or [2], characterized in that the resin composition for powder bed fusion bonding is contained as a powder satisfying the following requirement (II). Requirement (II): The median diameter D50 of the powder is 5 to 250 μm as measured by laser diffraction.
[0011] [4] The resin composition for powder bed fusion bonding according to any one of [1] to [3], characterized in that the thermoplastic elastomer (B) satisfies the following requirements (Bi) and (B-ii). Requirement (Bi): The melt flow rate at 230°C (230°C, 2.16 kg load) is 0.1 to 20 g / 10 min. Requirement (B-ii): Density is 0.855 to 0.905 g / cm 3 It is.
[0012] [5] The resin composition for powder bed fusion bonding according to any one of [1] to [4], wherein the filler (C) satisfies the following requirement (Ci): Requirement (Ci): The median diameter D50 is 1 to 160 μm as measured by a laser diffraction method in accordance with JIS R1629.
[0013] [6] The resin composition for powder bed fusion bonding according to any one of [1] to [5], further comprising 0.01 to 2.50 parts by weight of a nucleating agent (D) based on 100 parts by weight of the propylene polymer (A).
[0014] [7] The resin composition for powder bed fusion bonding according to any one of [1] to [6], which is a melt-kneaded resin composition of the propylene-based polymer (A), the thermoplastic elastomer (B) and the filler (C).
[0015] [8] A molded article obtained by powder bed fusion bonding using the resin composition for powder bed fusion bonding according to any one of [1] to [7].
[0016] [9] A method for producing a molded product, comprising the step of three-dimensionally molding the molded product by powder bed fusion using a resin composition for powder bed fusion, the resin composition comprising 100 parts by weight of a propylene-based polymer (A) satisfying the following requirements (Ai) to (A-iii), 10 to 250 parts by weight of a thermoplastic elastomer (B) and 10 to 150 parts by weight of a filler (C). Requirement (Ai): The melt flow rate at 230°C (230°C, 2.16 kg load) is 0.1 to 30 g / 10 min. Requirement (A-ii): The polymer comprises 50 to 95% by weight of a propylene homopolymer portion (a1) and 5 to 50% by weight of a propylene / α-olefin copolymer portion (a2). Requirement (A-iii): The copolymer portion (a2) is a copolymer portion having a propylene unit content of 30 to 80% by weight and an α-olefin unit content of 20 to 70% by weight. Effect of the Invention
[0017] According to the resin composition for powder bed fusion of the present invention, a molded article having an excellent balance between rigidity and impact resistance can be produced. Therefore, the resin composition for powder bed fusion of the present invention is not particularly limited in its application and can be appropriately selected according to the purpose, and can be used in a wide range of applications, such as three-dimensional shapes for food containers, cosmetic containers, medical parts, automobile parts, transport trays, furniture, etc. Furthermore, the resin composition for powder bed fusion of the present invention can be easily processed into a powder, and after powder processing, it has excellent powder dispersibility when forming a molded body by powder bed fusion, and can be suitably used for forming a molded body by powder bed fusion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment for carrying out the present invention (hereinafter referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out in various modifications within the scope of its gist.
[0019] [Resin composition for powder bed fusion bonding] The resin composition for powder bed fusion bonding of the present invention (hereinafter, may be referred to as "the resin composition of the present invention") is characterized by containing 10 to 250 parts by weight of a thermoplastic elastomer (B) and 10 to 150 parts by weight of a filler (C) based on 100 parts by weight of a propylene-based polymer (A) satisfying the following requirements (Ai) to (A-iii): Requirement (Ai): The melt flow rate at 230°C (230°C, 2.16 kg load) is 0.1 to 30 g / 10 min. Requirement (A-ii): The polymer comprises 50 to 95% by weight of a propylene homopolymer portion (a1) and 5 to 50% by weight of a propylene / α-olefin copolymer portion (a2). Requirement (A-iii): The copolymer portion (a2) is a copolymer portion having a propylene unit content of 30 to 80% by weight and an α-olefin unit content of 20 to 70% by weight.
[0020] <Physical properties of resin composition> The resin composition of the present invention preferably satisfies the following requirement (I). Requirement (I): In differential scanning calorimetry, the melting peak temperature (Tm) observed in the first heating is 150-170°C, and the total amount of heat of crystallization (ΔH) observed in the first heating is 30-80 J / g. However, in differential scanning calorimetry, the temperature is raised from 23°C to 200°C at a rate of 10°C / min, which is the first heating, then held at 200°C for 5 minutes, and then cooled to 40°C at a rate of 10°C / min, which is the first heating.
[0021] The melting peak temperature (Tm) is preferably from 150 to 170°C, more preferably from 152 to 168°C, and further preferably from 155 to 165°C. If the melting peak temperature (Tm) is less than 150° C., the resin composition may not have sufficient rigidity, and if the melting peak temperature (Tm) is more than 170° C., the molded article produced using the resin composition may not have sufficient impact resistance. The total amount of heat of crystallization (ΔH) is preferably 30 to 80 J / g, more preferably 40 to 75 J / g, and further preferably 50 to 70 J / g. If the total amount of heat of crystallization (ΔH) is less than 30 J / g, the rigidity of the molded body produced by powder bed fusion using the resin composition may not be sufficient. Also, if the total amount of heat of crystallization (ΔH) is more than 80 J / g, the molded body may be warped or otherwise deformed during the process of producing a three-dimensional molded body by powder bed fusion using the resin composition.
[0022] Furthermore, the melt flow rate (hereinafter sometimes abbreviated as MFR) (230°C, 2.16 kg load) of the resin composition of the present invention is preferably 0.1 to 30 g / 10 min, more preferably 1 to 15 g / 10 min, and even more preferably 3 to 8 g / 10 min, from the viewpoint of moldability such as strength, density, and dimensional accuracy of a molded article produced using the resin composition. If the MFR is less than 0.1 g / 10 min, the load on the kneading device may be high during melt kneading in the production of the resin composition, and if the MFR is more than 30 g / 10 min, the shape may be distorted when a molded product is produced by powder bed fusion bonding. Here, the MFR of the resin composition is a value measured in accordance with JIS K7210:1999 "Testing method for melt mass-flow rate (MFR) and melt volume-flow rate (MVR) of plastics - thermoplastics", Method A, Condition M (230°C, 2.16 kg load).
[0023] <Shape of resin composition> The resin composition of the present invention is preferably a powder that satisfies the following requirement (II). Requirement (II): The median diameter D50 of the powder is 5 to 250 μm as measured by laser diffraction. The powder median diameter D50, as measured by laser diffraction, is preferably from 5 to 250 μm, more preferably from 30 to 250 μm, further preferably from 40 to 150 μm, and particularly preferably from 50 to 100 μm. If the median diameter D50 is less than 5 μm, the production time of the powder may be long, and the productivity of the powder of the resin composition of the present invention may decrease. Also, if the median diameter D50 is more than 250 μm, when molding a molded body by powder bed fusion, it may be difficult to produce a molded body with a fine structure and / or to handle the powder during molding, such as dispersibility.
[0024] The above D50 is the particle size at 50% of the powder frequency distribution among the particle size distribution detected by a particle size measuring device using a laser diffraction / scattering technique as described later. The specific measurement method is as described in the Examples section below.
[0025] <Powder manufacturing method> The powdering means for producing the powder of the resin composition of the present invention include melt granulation, in which the resin composition of the present invention melted near the melting point is made into a fibrous form and then cut, and pulverization, in which the resin composition of the present invention is cut or destroyed by applying impact or shear. In order to improve the coatability of the powder in the powder bed fusion method, it is preferable that the powder does not contain fine powder of about 10 μm and has a certain particle size and particle size distribution, so that a suitable powdering means is selected so as to obtain a powder of such a suitable shape.
[0026] As the pulverizing means, for example, a stamp mill, a ring mill, a stone mill, a mortar, a roller mill, a jet mill, a high-speed rotary mill, a hammer mill, a pin mill, a container-driven mill, a disk mill, a media stirring mill, or the like can be used.
[0027] In addition, in order to prevent the stretching of the resin material due to shear heat during grinding, there is a method in which the resin temperature during grinding is lowered by cooling the grinding system using liquid nitrogen or the like, and powder is produced by brittle fracture rather than ductile fracture. This is called low-temperature grinding or freeze grinding. Among them, it is preferable to use a high-speed rotating mill for grinding, which can obtain powder with a particle size distribution and shape suitable for powder additive manufacturing, because this improves the flowability and powder application properties during molding. In addition, it is preferable to use liquid nitrogen to produce powder by brittle fracture of the resin material, in order to suppress changes in the physical properties and color of the resin material due to grinding.
[0028] In addition, from the viewpoint of removing the elongated powder from the pulverized powder to increase the circularity and from the viewpoint of removing the fine powder to prevent the powder from flying up during handling, it is preferable to carry out a classification process after pulverization. In this case, classification methods include air classification, sieve classification, etc. In addition, inorganic particles or reinforcing materials as flow aids described below may be added and mixed into the powder of the resin composition of the present invention obtained as necessary.
[0029] <Propylene-based polymer (A)> The propylene polymer (A) used in the present invention satisfies the following requirements (Ai) to (A-iii). Requirement (Ai): The melt flow rate at 230°C (230°C, 2.16 kg load) is 0.1 to 30 g / 10 min. Requirement (A-ii): The polymer comprises 50 to 95% by weight of a propylene homopolymer portion (a1) and 5 to 50% by weight of a propylene / α-olefin copolymer portion (a2). Requirement (A-iii): The copolymer portion (a2) is a copolymer portion having a propylene unit content of 30 to 80% by weight and an α-olefin unit content of 20 to 70% by weight. Each requirement will be explained in detail below. The contents of the propylene homopolymer portion (a1) and the propylene-α-olefin copolymer portion (a2) in the propylene polymer (A), and the propylene unit content and the α-olefin unit content in the propylene-α-olefin copolymer portion (a2) are measured by the method described later in the Examples section.
[0030] Requirements (Ai): The melt flow rate (hereinafter sometimes abbreviated as MFR) (230°C, 2.16 kg load) of the propylene-based polymer (A) used in the present invention is a value measured in accordance with JIS K7210:1999 "Testing method for melt mass-flow rate (MFR) and melt volume-flow rate (MVR) of plastics-thermoplastics", method A, condition M (230°C, 2.16 kg load).
[0031] MFR is the most fundamental factor in the molding and processing of polypropylene, and therefore, the MFR of the propylene polymer (A) used in the present invention is in the range of 0.1 to 30 g / 10 min, preferably 0.5 to 25 g / 10 min, and more preferably 1.0 to 20 g / 10 min. If the MFR is less than 0.1 g / 10 min, the load on the kneading device may be increased when melt-kneading the propylene polymer (A), the thermoplastic elastomer (B), and the filler (C).If the MFR is more than 30 g / 10 min, the shape may be distorted when a molded product is formed by the powder bed fusion bonding method.
[0032] Requirement (A-ii): The propylene polymer (A) used in the present invention comprises 50 to 95% by weight, preferably 70 to 92% by weight, more preferably 80 to 90% by weight of a propylene homopolymer portion (a1) and 5 to 50% by weight, preferably 8 to 30% by weight, more preferably 10 to 20% by weight of a propylene-α-olefin copolymer portion (a2). If the propylene homopolymer portion (a1) is less than 50% by weight, the grindability of the resin composition may be deteriorated, whereas if the propylene homopolymer portion (a1) is more than 95% by weight, the molded article produced from the resin composition of the present invention may not have sufficient impact resistance. In addition, when the propylene-α-olefin copolymer portion (a2) is less than 5% by weight, the molded product formed from the resin composition of the present invention is There is a risk that sufficient impact resistance cannot be obtained, and when the propylene-α-olefin copolymer portion (a2) is more than 50% by weight, the grindability of the resin composition is deteriorated.
[0033] Requirement (A-iii): The propylene-α-olefin copolymer portion (a2) of the propylene polymer (A) used in the present invention is a copolymer portion having a propylene unit content of 30 to 80% by weight, preferably 40 to 75% by weight, more preferably 50 to 70% by weight, and an α-olefin unit content of 20 to 70% by weight, preferably 25 to 60% by weight, more preferably 30 to 50% by weight. The term "unit" as used herein refers to a structural unit formed in the propylene polymer (A) derived from a raw material compound of the propylene polymer (A). If the propylene unit content and the α-olefin unit content are outside the above ranges, there is a risk that a molded article made from the resin composition of the present invention will not have sufficient impact resistance, which is undesirable.
[0034] Examples of the α-olefin of the propylene-α-olefin copolymer portion (a2) of the propylene-based polymer (A) used in the present invention include ethylene, 1-butene, 2-methyl-1-propene, 1-pentene, 2-methyl-1-butene, 3-methyl-1-butene, 1-hexene, 2-ethyl-1-butene, 2,3-dimethyl-1-butene, 2-methyl-1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 3,3-dimethyl-1-butene, 1-heptene, methyl-1-hexene, dimethyl-1-pentene, ethyl-1-pentene, trimethyl-1-butene, and 1-octene. These may be copolymerized with propylene using one kind, or may be copolymerized with propylene using two or more kinds in combination. Among them, from the viewpoint of improving the impact strength of the obtained molded article, ethylene or 1-butene, which have a large effect, are preferable, and ethylene is most preferable.
[0035] The propylene-based polymer (A) used in the present invention is not particularly limited as long as it satisfies the above-mentioned requirements (Ai) to (A-iii), and examples thereof include propylene-based block copolymers consisting of 50 to 95% by weight of a propylene homopolymer block and 5 to 50% by weight of a propylene-α-olefin copolymer block.
[0036] The propylene polymer (A) may be used in a mixture of two or more kinds so as to satisfy the above-mentioned requirements (Ai) to (A-iii), and further, if necessary, a propylene homopolymer may be mixed within a range that does not significantly impair the effects of the present invention.
[0037] <Method for producing propylene polymer (A)> The method for producing the propylene polymer (A) used in the resin composition of the present invention will be described below.
[0038] The propylene polymer (A) used in the present invention is preferably produced by polymerization using a highly stereoregular catalyst. The propylene polymer (A) is a reaction mixture of a propylene homopolymer portion (a1) and a propylene-α-olefin copolymer portion (a2). This is obtained by a production process of polymerization of the propylene homopolymer portion (a1), which is a crystalline propylene polymer portion (first step), followed by polymerization of the propylene-α-olefin copolymer portion (a2) (second step).
[0039] The catalyst used in the polymerization is not particularly limited as long as it is a highly stereoregular catalyst, and known catalysts can be used. For example, so-called Ziegler-Natta catalysts that combine titanium compounds and organoaluminum (for example, as described in Polypropylene Handbook (first edition, first printing published May 15, 1998)) or metallocene catalysts (for example, see JP-A-5-295022) can be used.
[0040] Ziegler-Natta catalysts include those obtained by treating titanium trichloride or titanium trichloride compositions obtained by reduction with organoaluminum or the like as a titanium compound with an electron donor compound for further activation (see, for example, JP-A-47-34478, JP-A-58-23806, and JP-A-63-146906), and so-called supported catalysts obtained by supporting titanium tetrachloride on a carrier such as magnesium chloride (see, for example, JP-A-58-157808, JP-A-58-83006, JP-A-58-5310, and JP-A-61-218606).
[0041] Examples of the organoaluminum compound used as a promoter include trialkylaluminum such as trimethylaluminum, triethylaluminum, and triisobutylaluminum, alkylaluminum halides such as diethylaluminum chloride and diisobutylaluminum chloride, alkylaluminum hydrides such as diethylaluminum hydride, alkylaluminum alkoxides such as diethylaluminum ethoxide, alumoxanes such as methylalumoxane and tetrabutylalumoxane, complex organoaluminum compounds such as dibutyl methylboronate and lithiumaluminum tetraethyl, etc. Two or more of these can also be used in combination.
[0042] The above-mentioned catalysts can be used with various polymerization additives for the purpose of improving stereoregularity, controlling particle properties, controlling soluble components, controlling molecular weight distribution, etc. Examples of the polymerization additives include electron donor compounds such as organosilicon compounds such as diphenyldimethoxysilane and tert-butylmethyldimethoxysilane, esters such as ethyl acetate, butyl benzoate, methyl p-toluate, and dibutyl phthalate, ketones such as acetone and methyl isobutyl ketone, ethers such as diethyl ether, organic acids such as benzoic acid and propionic acid, and alcohols such as ethanol and butanol.
[0043] The polymerization method may be a slurry polymerization using an inert hydrocarbon such as hexane, heptane, octane, benzene, or toluene as a polymerization solvent, a bulk polymerization using propylene itself as a polymerization solvent, or a gas phase polymerization in which the raw material propylene is polymerized in a gas phase state. It is also possible to combine these polymerization methods. For example, the propylene homopolymer part (a1) may be produced by bulk polymerization, and the propylene-α-olefin copolymer part (a2) may be produced by gas phase polymerization, or the propylene homopolymer part (a1) may be produced by bulk polymerization, followed by gas phase polymerization, and the propylene-α-olefin copolymer part (a2) may be produced by gas phase polymerization.
[0044] The polymerization may be carried out in a batch, continuous or semi-batch manner, and if desired, a multi-stage, such as two-stage or three-stage, continuous polymerization method may be used. Furthermore, the polymerization reactor may be of any shape or structure, and examples thereof include a reactor equipped with a stirrer that is generally used in slurry polymerization or bulk polymerization, a tubular reactor, a fluidized bed reactor that is generally used in gas phase polymerization, and a horizontal reactor equipped with a stirring blade.
[0045] In the gas phase polymerization, the polymerization step of the propylene homopolymer part (a1) is carried out by supplying propylene and hydrogen as a chain transfer agent in the presence of the catalyst under the conditions of a temperature of 0 to 100°C, preferably 30 to 90°C, particularly preferably 40 to 80°C, a propylene partial pressure of 0.6 to 4.2 MPa, preferably 1.0 to 3.5 MPa, particularly preferably 1.5 to 3.0 MPa, and a residence time of 0.5 to 10 hours. The propylene homopolymer part (a1) may be copolymerized with an α-olefin other than propylene, for example, ethylene at a ratio of less than 0.5 wt%, within a range that does not impair the effects of the present invention.
[0046] The MFR (230° C., 2.16 kg load) of the propylene homopolymer portion (a1) of the propylene polymer (A) used in the present invention is usually in the range of 1 to 350 g / 10 min. In order to make the propylene homopolymer portion (a1) of the propylene polymer (A) in such a range, depending on the type of catalyst, hydrogen of the chain transfer agent is preferably added at a molar ratio of hydrogen / propylene of 1×10 -2 By using it in the range of 0.75 or less, it is possible to adjust the MFR to a desired value.
[0047] Following the production of the propylene homopolymer part (a1), i.e., in the presence of the propylene homopolymer part (a1) produced in the first polymerization step, in the second polymerization step, propylene, α-olefin and hydrogen are supplied and copolymerized with propylene and α-olefin in the presence of the catalyst (the catalyst used in the production of the propylene homopolymer part (a1)) under conditions of 0 to 100°C, preferably 30 to 90°C, particularly preferably 40 to 80°C, partial pressures of propylene and α-olefin of 0.1 to 2.0 MPa, preferably 0.1 to 1.5 MPa, and a residence time of 0.5 to 10 hours, to produce a propylene-α-olefin copolymer part (a2), and obtain a propylene-based polymer (A) as a final product. In the propylene-α-olefin copolymer portion (a2), propylene may be copolymerized with two or more kinds of α-olefins within the range that does not impair the effects of the present invention.
[0048] In order to set the MFR of the propylene polymer (A) used in the present invention in the range of 0.1 to 30 g / 10 min, as described above, since the MFR of the propylene homopolymer portion (a1) is usually in the range of 1 to 350 g / 10 min, the MFR (230° C., 2.16 kg load) of the propylene-α-olefin copolymer portion (a2) must be within the range of 1×10 -3 It is preferable to set it to 100g / 10 minutes or less. The MFR of the propylene-α-olefin copolymer part (a2) is 1×10 -3 To control the reaction rate to 100g / 10min, the hydrogen / (propylene + α-olefin) molar ratio should be set to 1×10 -4 By performing the process within the range of 0.2 to 1.0, it is possible to adjust the MFR to a desired value. In order to maintain the α-olefin unit content in the propylene-α-olefin copolymer portion (a2) within a specific range, the α-olefin concentration relative to the propylene concentration in the latter step may be adjusted.
[0049] Furthermore, in order to prevent gelation or stickiness, it is desirable to add alcohols such as ethanol during or before the reaction of the propylene-α-olefin copolymer part (a2). Specifically, the reaction can be carried out under conditions of an alcohol / organoaluminum compound molar ratio of 0.5 to 3.0. The proportion of the propylene-α-olefin copolymer part (a2) in the propylene-based polymer (A) can also be controlled by the amount of the alcohol added.
[0050] The melting peak temperature (Tm2nd) observed in the second heating (second heating) of the differential scanning calorimetry of the propylene-based polymer (A) used in the present invention is preferably 150 to 170°C, more preferably 152 to 168°C, and even more preferably 155 to 165°C. If the melting peak temperature (Tm2nd) is less than 150°C, the rigidity of the resin composition of the present invention may not be sufficient. If the melting peak temperature (Tm2nd) is higher than 170°C, the impact resistance of the molded article formed using the resin composition of the present invention may not be sufficient.
[0051] Furthermore, the total amount of heat of crystallization (ΔH) observed in the first temperature drop (first temperature drop) of differential scanning calorimetry of the propylene-based polymer (A) used in the present invention is preferably 40 to 110 J / g, more preferably 60 to 105 J / g, and even more preferably 80 to 103 J / g. If the total amount of heat of crystallization (ΔH) is less than 40 J / g, there is a risk that the rigidity of the molded body obtained by the powder bed fusion method using the resin composition of the present invention is insufficient. If the total amount of heat of crystallization (ΔH) is more than 110 J / g, there is a risk that the molded body will be deformed, such as warped, in the process of forming a three-dimensional molded body by the powder bed fusion method using the resin composition of the present invention.
[0052] In addition, since various companies have put various kinds of commercial products of such propylene-based polymers (A) on the market, it is also possible to measure the physical properties of these commercial products and use those that satisfy the above conditions (Ai) to (A-iii).
[0053] <Thermoplastic elastomer (B)> The resin composition of the present invention contains, in addition to the propylene polymer (A), a thermoplastic elastomer (B), preferably a thermoplastic elastomer (B) satisfying the following requirements (Bi) and (B-ii): Requirement (Bi): The melt flow rate at 230°C (230°C, 2.16 kg load) is 0.1 to 20 g / 10 min. Requirement (B-ii): Density is 0.855 to 0.905 g / cm 3 It is.
[0054] Requirements(Bi): The thermoplastic elastomer (B) used in the present invention preferably has an MFR of 0.1 to 20 g / 10 min, more preferably 0.3 to 15 g / 10 min, and even more preferably 0.5 to 10 g / 10 min, from the viewpoints of improving the impact resistance of the resin composition of the present invention and of pulverizability and dispersibility of the powder. If the MFR is less than 0.1 g / 10 min, the crushability may decrease, and the productivity of the powder of the resin composition may decrease. If the MFR is more than 20 g / 10 min, the impact resistance of the molded body formed using the resin composition may not be sufficient, or the powders may aggregate when forming a molded body by powder bed fusion bonding, resulting in decreased dispersibility.
[0055] Requirement (B-ii): The thermoplastic elastomer (B) used in the present invention has a density of 0.855 to 0.905 g / cm from the viewpoints of improving the impact resistance and crushability of the molded article obtained by using the resin composition of the present invention. 3 and more preferably 0.870 to 0.900 g / cm 3 , and more preferably 0.880 to 0.895 g / cm 3 minutes. Density 0.855g / cm 3 If the density is less than 0.905 g / cm, the crushability is reduced, the productivity of the powder of the resin composition is reduced, or the powder may aggregate when forming a molded body by the powder bed fusion method, resulting in reduced dispersibility. 3If it is larger, there is a concern that a molded article produced using the resin composition may not have sufficient impact resistance. Here, the density of the thermoplastic elastomer (B) is a value measured at 23° C. in accordance with JIS K7112.
[0056] The thermoplastic elastomer (B) may be, for example, at least one selected from the group consisting of olefin-based elastomers and styrene-based elastomers.
[0057] Examples of olefin-based elastomers include ethylene-α-olefin copolymer elastomers such as ethylene-propylene copolymer elastomer (EPR), ethylene-butene copolymer elastomer (EBR), ethylene-hexene copolymer elastomer (EHR), and ethylene-octene copolymer elastomer (EOR); and ethylene-α-olefin-diene terpolymer elastomers such as ethylene-propylene-ethylidenenorbornene copolymer, ethylene-propylene-butadiene copolymer, and ethylene-propylene-isoprene copolymer. Specific examples of olefin-based elastomers include those commercially available under the trade name DYNARON (registered trademark) from JSR Corporation, under the trade name TAFMER (registered trademark) from Mitsui Chemicals, Inc., under the trade names ENGAGE (registered trademark), AFFINITY (registered trademark), and VERSIFY (registered trademark) from The Dow Chemical Company, Ltd., under the trade name Kernel from Japan Polyethylene Corporation, and under the trade name Vistamaxx (registered trademark) from ExxonMobil Chemical Corporation.
[0058] Examples of styrene-based elastomers include styrene-butadiene-styrene triblock copolymer elastomer (SBS), styrene-isoprene-styrene triblock copolymer elastomer (SIS), styrene-ethylene-butylene copolymer elastomer (SEB), styrene-ethylene-propylene copolymer elastomer (SEP), styrene-ethylene-butylene-styrene copolymer elastomer (SEBS), styrene-ethylene-butylene-ethylene copolymer elastomer (SEBC), hydrogenated styrene-butadiene elastomer (HSBR), styrene Examples of elastomers include styrene-based elastomers such as ethylene-propylene-styrene copolymer elastomer (SEPS), styrene-ethylene-ethylene-propylene-styrene copolymer elastomer (SEEPS), styrene-butadiene-butylene-styrene copolymer elastomer (SBBS), partially hydrogenated styrene-isoprene-styrene copolymer elastomer, and partially hydrogenated styrene-isoprene-butadiene-styrene copolymer elastomer, as well as hydrogenated polymer-based elastomers such as ethylene-ethylene-butylene-ethylene copolymer elastomer (CEBC). Specific examples of styrene-based elastomers include those commercially available under the trade names Dynaron (registered trademark) and JSR SIS (registered trademark) from JSR Corporation, under the trade names Hybler (registered trademark) and Septon (registered trademark) from Kuraray Co., Ltd., under the trade name Tuftec (registered trademark) from Asahi Kasei Corporation, under the trade name Sibstar (registered trademark) from Kaneka Corporation, and under the trade names Kraton (registered trademark) and Kraton D (registered trademark) from Shell Corporation.
[0059] These thermoplastic elastomers (B) may be used alone or in combination of two or more. Since various products of these thermoplastic elastomers (B) are commercially available from many companies, a desired product can be purchased and used.
[0060] <Thermoplastic elastomer (B) blend ratio> The resin composition of the present invention contains 10 to 250 parts by weight of the thermoplastic elastomer (B) based on 100 parts by weight of the propylene polymer (A). The content of the thermoplastic elastomer (B) is preferably 12 to 100 parts by weight, more preferably 15 to 50 parts by weight. If the amount of the thermoplastic elastomer (B) is less than 10 parts by weight, the impact resistance of the molded article produced using the resin composition may not be sufficient. If the amount of the thermoplastic elastomer (B) is more than 250 parts by weight, the crushability may decrease, the productivity of the powder of the resin composition may decrease, or the powder may aggregate when the molded article is produced by the powder bed fusion method, resulting in a decrease in the dispersibility.
[0061] <Filler (C)> The resin composition of the present invention contains, in addition to the above-mentioned propylene polymer (A) and thermoplastic elastomer (B), a filler (C), preferably a filler (C) satisfying the following requirement (Ci). Requirement (Ci): The median diameter D50 is 1 to 160 μm as measured by a laser diffraction method in accordance with JIS R1629.
[0062] Requirements(Ci): From the viewpoints of the balance between rigidity and impact resistance of the resin composition of the present invention and crushability, the filler (C) used in the present invention preferably has a median diameter D50 measured by a laser diffraction method in accordance with JIS R1629 of 1 to 160 μm, more preferably 2 to 50 μm, and even more preferably 3 to 10 μm. If the median diameter D50 is less than 1 μm, the molded article produced using the resin composition may not have sufficient rigidity, and if the median diameter D50 is more than 160 μm, the molded article produced using the resin composition may not have sufficient impact resistance, or may be difficult to crush to a size of 160 μm or less.
[0063] The median diameter D50 is a value measured by a laser diffraction method in accordance with JIS R1629, and is determined from the particle size value at a cumulative amount of 50% by weight read from a particle size cumulative distribution curve measured using a laser particle size distribution analyzer in accordance with JIS R1629. Examples of the laser particle size distribution analyzer that can be used include "LA960" manufactured by Horiba Ltd. and "SALD-2000J" manufactured by Shimadzu Corporation.
[0064] Examples of the filler (C) include oxides such as silica, diatomaceous earth, barium ferrite, beryllium oxide, pumice, and pumice balloon; hydroxides such as aluminum hydroxide, magnesium hydroxide, and basic magnesium carbonate; carbonates such as calcium carbonate, magnesium carbonate, dolomite, and dawsonite; sulfates or sulfites such as calcium sulfate, barium sulfate, ammonium sulfate, and calcium sulfite; talc, clay, mica, glass fiber, carbon fiber, glass balloon, glass beads, calcium silicate, wollastonite, montmorillonite, and bentonite; molybdenum sulfide, boron fiber, zinc borate, barium metaborate, calcium borate, sodium borate, basic magnesium sulfate fiber, potassium titanate fiber, aluminum borate fiber, calcium silicate fiber, and calcium carbonate fiber. These may be used alone or in combination of two or more types, but it is preferable to use talc, which can further improve the rigidity of the molded article produced using the resin composition, as well as from the standpoint of economy. Various types of these fillers (C) are commercially available from many companies, and a desired product can be purchased and used from among them.
[0065] <Filler (C) Mixture Ratio> The resin composition of the present invention contains 10 to 150 parts by weight of the filler (C) based on 100 parts by weight of the propylene polymer (A). The content of the filler (C) is more preferably 12 to 100 parts by weight, and further preferably 15 to 50 parts by weight. If the amount of the filler (C) is less than 10 parts by weight, the rigidity of the resin composition may not be sufficient, whereas if the amount of the filler (C) is more than 150 parts by weight, the crushability may decrease, and the impact resistance of the molded article formed using the resin composition may not be sufficient.
[0066] <Nucleating agent (D)> The resin composition of the present invention may further contain 0.01 to 2.50 parts by weight of a nucleating agent (D) based on 100 parts by weight of the propylene polymer (A).
[0067] As the nucleating agent (D), various general known nucleating agents can be used, such as sterically hindered amide compounds, organic dicarboxylic acid metal salts, organic monocarboxylic acid metal salts, sorbitol or its derivatives, nonitol or its derivatives, diterpene acid metal salts, polymer nucleating agents, etc. Specific examples include those commercially available under the trade names Adeka STAB NA-11 and Adeka STAB NA-21 from ADEKA CORPORATION, Millidian & Company under the trade name Millad NX8000J, and Japan Chemtech Corporation under the trade name AL-PTBBA. These may be used alone or in combination of two or more.
[0068] In particular, it is preferable to contain an organophosphate metal salt compound represented by the following formula (1) as the nucleating agent (D) in order to improve the rigidity of a molded article produced using the resin composition of the present invention.
[0069] [ka]
[0070] (In formula (1), R 1 is a direct bond, a sulfur atom, an alkylene group having 1 to 9 carbon atoms, or an alkylidene group having 2 to 9 carbon atoms; R 2 and R 3are each independently a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or an alkylaryl group having 7 to 9 carbon atoms, M is Li, Na, K, Mg, Ca, Zn, or Al, and n is the valence of M.
[0071] Specific examples of the organophosphate metal salt compound represented by formula (1) include sodium-2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate, sodium-2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate, sodium-2,2'-methylene-bis(4-cumyl-6-t-butylphenyl)phosphate, lithium-2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate, lithium-2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate, lithium-2,2'-methylene-bis(4-cumyl-6-t-butylphenyl)phosphate, sodium-2,2'-ethylidene-bis(4-i-propyl Lithium-2,2'-methylene-bis(4-methyl-6-t-butylphenyl)phosphate, Lithium-2,2'-methylene-bis(4-ethyl-6-t-butylphenyl)phosphate, Sodium-2,2'-butylidene-bis(4,6-dimethylphenyl)phosphate, Sodium-2,2'-butylidene-bis(4,6-di-t-butylphenyl)phosphate, Sodium-2,2'-t-octylmethylene-bis(4,6-dimethylphenyl)phosphate, Sodium -2,2'-t-octylmethylene-bis(4,6-di-t-butylphenyl)phosphate, sodium-2,2'-methylene-bis(4-methyl-6-t-butylphenyl)phosphate, sodium-2,2'-methylene-bis(4-ethyl-6-t-butylphenyl)phosphate, sodium (4,4'-dimethyl-6,6'-di-t-butyl-2,2'-biphenyl)phosphate, sodium-2,2'-ethylidene-bis(4-s-butyl-6-t-butylphenyl)phosphate, sodium-2,2'-methylene-bis (4,6-di-methylphenyl) phosphate, sodium-2,2'-methylene-bis(4,6-di-ethylphenyl) phosphate, potassium-2,2'-ethylidene-bis(4,6-di-t-butylphenyl) phosphate, calcium-bis[2,2'-methylene-bis(4,6-di-t-butylphenyl) phosphate], magnesium-bis[2,2'-methylene-bis(4,6-di-t-butylphenyl) phosphate], zinc-bis[2,2'-methylene-bis(4,6-di-t-butylphenyl) phosphate], a Aluminum tris[2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate], calcium bis[2,2'-methylene-bis-(4-methyl-6-t-butylphenyl)phosphate], calcium bis[2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate], calcium bis[2,2'-thiobis(4-methyl-6-t-butylphenyl)phosphate], calcium bis[2,2'-thiobis(4-ethyl-6-t-butylphenyl)phosphate], calcium bis[2,2'-thiobis(4,6-di-t-butylphenyl)phosphate], magnesium bis[2,2'-thiobis(4,6-di-t-butylphenyl)phosphate], magnesium bis[2,2'-thiobis(4-t-octylphenyl)phosphate], calcium bis[(4,4'-dimethyl-6,6'-di-t-butyl-2,2'-biphenyl)phosphate], magnesium bis[2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate], aluminum tris[2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate] and mixtures of two or more of these. Of these, sodium 2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate is particularly preferred.
[0072] The content of the nucleating agent (D) contained in the resin composition of the present invention is preferably in the range of 0.01 to 2.50 parts by weight, more preferably 0.05 to 1.50 parts by weight, and even more preferably 0.1 to 1.00 parts by weight, based on 100 parts by weight of the propylene polymer (A). If the content of the nucleating agent (D) is less than 0.01 parts by weight, the rigidity of the molded body formed using the resin composition may not be sufficient. Also, if the content of the nucleating agent (D) is more than 2.50 parts by weight, the rigidity improvement effect may be impaired, and there may be a disadvantage in terms of cost-effectiveness (cost performance).
[0073] <Optional addition ingredients> In addition to the propylene polymer (A), thermoplastic elastomer (B), filler (C) and granulating agent (D), the resin composition of the present invention may further contain optional additives, if necessary, within a range that does not significantly impair the effects of the present invention, for the purpose of, for example, further improving the effects of the present invention or imparting other effects. Examples of the optional additives include inorganic particles such as silica, alumina and kaolin as flow aids, organic particles such as acrylic resin particles and melamine resin particles, titanium oxide, carbon black and dyes as laser absorbents for improving formability, nylon powder and the like, which are added for the purpose of improving and adjusting the formability and stability of a molded product molded by powder bed fusion bonding and various physical properties of the molded product. As the flow aid, silica and alumina are particularly preferred because they are hard and can contribute to improving strength and flowability.Furthermore, depending on its particle size, the filler (C) can also function as a flow aid or a reinforcing material by mixing additives and the like with the powder of the resin composition produced by the above-mentioned method, that is, by adding the powder to the resin composition of the present invention as a powder mixture, without melt-kneading the resin composition and additives and the like, and adding the powder to the resin composition of the present invention as an external additive.
[0074] These optional components may be added separately from the powder obtained by melt-kneading and pulverizing the resin composition of the present invention containing the propylene polymer (A), the plastic elastomer (B) and the filler (C). In particular, silica, alumina, etc., which are added as flow aids, can be added externally in an amount of 0.01 to 2 parts by weight per 100 parts by weight of the powder of the resin composition of the present invention to increase the flowability of the powder and improve the spreadability during molding.
[0075] The resin composition of the present invention may further contain optional additives such as colorants such as pigments, light stabilizers such as hindered amines, ultraviolet absorbers such as benzotriazoles, antioxidants such as phenols and phosphorus-based antioxidants, nonionic antistatic agents, β-crystal nucleating agents such as amide compounds, neutralizing agents such as inorganic compounds, antibacterial and antifungal agents such as thiazoles, flame retardants such as halogen compounds, plasticizers, dispersants such as organic metal salts, lubricants such as fatty acid amides, metal deactivators such as nitrogen compounds, nonionic surfactants, weather resistance stabilizers, heat resistance stabilizers, melt viscosity improvers, crosslinking agents, antioxidants, antifogging agents, antiblocking agents, slip agents, reinforcing materials, weight-reducing materials, conductive materials, magnetic materials, and thermoplastic resins such as polyolefin resins, polyamide resins, and polyester resins other than the propylene polymer (A). These optional added components may be used in combination of two or more kinds. They may be added to the resin composition of the present invention separately from the propylene-based polymer (A) and the thermoplastic elastomer (B), or may be added to the propylene-based polymer (A) and the thermoplastic elastomer (B), etc., and two or more kinds of each component may also be used in combination.
[0076] Colorants such as inorganic or organic pigments are effective in imparting or improving the colored appearance, appearance, texture, commercial value, weather resistance, durability, etc. of the resin composition of the present invention and the molded article obtained by powder bed fusion bonding using the resin composition of the present invention. Specific examples of inorganic pigments include carbon black such as furnace carbon and ketjen carbon, titanium oxide, iron oxide (e.g., red iron oxide), chromic acid (e.g., yellow lead), molybdic acid, selenide sulfide, and ferrocyanide. Examples of organic pigments include azo pigments such as sparingly soluble azo lake, soluble azo lake, insoluble azo chelate, condensed azo chelate, and other azo chelates, phthalocyanine pigments such as phthalocyanine blue and phthalocyanine green, threne pigments such as anthraquinone, perinone, perylene, and thioindigo, dye lake, quinacridone, dioxazine, and isoindolinone. In order to achieve a metallic or pearlescent look, aluminum flakes and pearl pigments can be added. Dyes can also be added.
[0077] Light stabilizers and ultraviolet absorbers, such as hindered amine compounds, benzotriazoles, benzophenones, and salicylates, are effective in imparting or improving weather resistance, durability, and the like to the resin composition of the present invention and to a molded article obtained by powder bed fusion bonding using the resin composition of the present invention, and are effective in further improving weather discoloration resistance.
[0078] Specific examples of these include the following: Examples of the hindered amine compound include a condensation product of dimethyl succinate and 1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine; poly[[6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidyl)imino]hexamethylene[(2,2,6,6-tetramethyl-4-piperidyl)imino] tetrakis(2,2,6,6-tetramethyl-4-piperidyl) 1,2,3,4-butanetetracarboxylate; tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl) 1,2,3,4-butanetetracarboxylate; bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate; bis-2,2,6,6-tetramethyl-4-piperidylsebacate, and the like. Benzotriazoles include 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole; 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole, and the like. Benzophenones include 2-hydroxy-4-methoxybenzophenone and 2-hydroxy-4-n-octoxybenzophenone. Examples of the salicylates include 4-t-butylphenyl salicylate; 2,4-di-t-butylphenyl 3',5'-di-t-butyl-4'-hydroxybenzoate, and the like. Here, the method of using the light stabilizer and the ultraviolet absorber in combination is preferable because it has a large effect of improving weather resistance, durability, weather discoloration resistance, and the like.
[0079] Antioxidants such as phenol-based, phosphorus-based and sulfur-based antioxidants are effective in imparting or improving the heat resistance, processing stability, heat aging resistance, etc. of molded articles obtained by powder bed fusion bonding using the resin composition of the present invention. In addition, antistatic agents such as nonionic and cationic antistatic agents are effective in imparting or improving antistatic properties to molded articles obtained by powder bed fusion bonding using the resin composition of the present invention.
[0080] The β-crystal nucleating agent is not particularly limited as long as it is a crystallization nucleating agent that selectively forms β-crystals when added to a polypropylene resin. Various pigment-based compounds (such as quinacridone) and amide-based compounds can be preferably used, and amide-based compounds are particularly preferred for achieving high β-crystal formation ability.
[0081] The content of the above-mentioned optional additive components in the resin composition of the present invention is not particularly specified, but from the viewpoint of the stability of the resin composition and the molded product when the molded product is formed by the powder bed fusion method, it is preferably 0.01 parts by weight or more, more preferably 0.05 parts by weight or more, even more preferably 0.08 parts by weight or more, and particularly preferably 0.1 parts by weight or more, based on 100 parts by weight of the total resin composition of the present invention. Also, from the viewpoint of suppressing the decrease in interlayer adhesion of the molded product, the upper limit of the content of the optional additive components is preferably 30 parts by weight or less, more preferably 28 parts by weight or less, and even more preferably 25 parts by weight or less.
[0082] <Method of producing resin composition> The resin composition of the present invention can be produced by mixing and / or melt-kneading the specific propylene-based polymer (A), the thermoplastic elastomer (B), and the filler (C), as well as the nucleating agent (D) and any optional additional components, which are used as necessary, in the above-mentioned blending ratio by a conventionally known method.
[0083] The mixing can be usually carried out using a mixing device such as a tumbler, a V blender, a ribbon blender, a Henschel mixer, etc. The melt kneading can be usually carried out using a kneading device such as a single screw extruder, a twin screw extruder, a Banbury mixer, a roll mixer, a Brabender plastograph, a kneader, a gelation mixer, etc. The resin composition of the present invention can be produced by melt kneading and powdering, preferably by the above-mentioned method.
[0084] When the resin composition of the present invention is used in the form of a powder, the above-mentioned additives, particularly the flow aid, may be mixed with the powder of the resin composition produced by the above-mentioned method, without melt-kneading the resin composition and the additives, i.e., added externally to the resin composition of the present invention, and then blended as a powder mixture.
[0085] <Molded body> The molded article of the present invention is made of the above-mentioned resin composition. As a method for producing the molded article, molding is preferably performed using a three-dimensional printer. The detailed production method is described below.
[0086] <Method of manufacturing molded body> In the method for producing a molded article made from the resin composition of the present invention, the resin composition of the present invention is used and molded by a three-dimensional printer to obtain a resin molded article. As mentioned above, molding methods using a 3D printer include the material extrusion (MEX) method, the material jetting method in which resin ejected from an inkjet head is cured with ultraviolet light, the vat photopolymerization (VP) method in which a cured layer of a photocurable resin solution is laminated using a laser, and the powder bed fusion (PBF) method in which a deposited layer of powder material is sintered with a laser. However, the powder bed fusion method in which a powdered thermoplastic resin is melted to produce a molded body is applied to the resin composition of the present invention.
[0087] In the production of molded articles by the powder bed fusion method, particles of a resin composition spread on a stage are irradiated with a laser or an electron beam to sinter or fuse the particles to form a layer in the height direction, and then particles of the resin composition are spread in contact with the layer formed above and irradiated with a laser or an electron beam to form the next layer. By successively stacking in this manner, a molded article of a desired shape can be obtained. EXAMPLES
[0088] The present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples. The evaluation methods, analytical methods and materials used in the examples are as follows.
[0089] 1. Evaluation and analysis methods (1) MFR (unit: g / 10 min) The MFR (230°C, 2.16 kg load) of the propylene-based polymer (A), the thermoplastic elastomer (B) and the resin composition was measured in accordance with JIS K 7210. The resin composition used for the measurement was pellets obtained by melt kneading, which will be described later.
[0090] (2) The content (wt%) of the propylene homopolymer portion (a1), the propylene-α-olefin copolymer portion (a2) in the propylene polymer (A), and the α-olefin in the propylene-α-olefin copolymer portion (a2) This was determined by a combination of the cross-fractionation method and FT-IR method described in JP 2017-031359 A.
[0091] (3) Flexural modulus (unit: MPa) Using injection-molded test pieces with a thickness of 4.0 mm, width of 10.0 mm, and length of 80 mm, measurements were taken in accordance with JIS K7171 at an atmospheric temperature of 23°C (units are MPa). The test pieces were molded by feeding the pellets obtained by melt kneading, which will be described later, into a Toshiba injection molding machine IS80G under the conditions of a molding temperature of 200°C, a mold temperature of 40°C, an injection speed of 200 mm / sec, and a total cycle time of 60 sec.
[0092] (4) Charpy impact value (kJ / m 2 ) A Charpy impact test was carried out at a measurement atmosphere temperature of 23°C in accordance with ISO179 (notched) using injection-molded test pieces with a thickness of 4.0 mm, width of 10.0 mm, and length of 80 mm and a notch (notch radius of 0.25 mm). The test pieces were molded in the same manner as in the molding of the test pieces for the flexural modulus.
[0093] (5) Melting peak temperature (Tm), total heat of crystallization (ΔH) The powder obtained by the powderization described below was measured by differential scanning calorimetry (DSC, TA Instruments, Q2000) to measure the temperature of the endothermic peak top observed during the first heating from 23°C to 200°C at a rate of 10°C / min, which was determined as the melting peak temperature (Tm), and the total amount of heat of the exothermic peak observed during the subsequent heating at 200°C for 5 minutes and then cooling to 40°C at a rate of 10°C / min was determined as the total heat of crystallization (ΔH). The melting peak temperature (melting point) (Tm2nd) of the propylene polymer (A) was measured using a differential scanning calorimeter (DSC, TA Instruments, Q2000) by first heating the sample to 200°C, leaving the sample for 5 minutes, then lowering the temperature to 40°C at a temperature drop rate of 10°C / min, and then measuring again at a temperature increase rate of 10°C / min. The endothermic peak top temperature was determined as the melting peak temperature (Tm2nd) observed during the second heating. The total heat of crystallization (ΔH) was calculated from the area of the exothermic peak observed when the temperature was decreased from 200° C. to 40° C. in accordance with JIS K7122 (1987).
[0094] (6) Powder particle size The particle size of the powder obtained by powderization, which will be described later, was measured by a laser diffraction method. Using a spray particle size distribution measuring device Aerotrac3500A manufactured by MicrotracBEL, a laser beam was irradiated onto the dispersed measurement sample, the diffracted and scattered light was detected, and the analysis was performed based on the Fraunhofer diffraction theory to calculate the volume-based particle size distribution. The total volume of the fine particles obtained by the analysis was taken as 100% to obtain a cumulative curve, and the particle size at the point where the cumulative curve reached 50% (median diameter: D50) was taken as the average particle size of the powder.
[0095] (7) Dispersibility The powder obtained by the powderization described below was taken as 100 parts by weight, and 0.3 parts by weight of silica particles (AEROSIL RX200, manufactured by Nippon Aerosil Co., Ltd., average primary particle size 12 nm) were added as a flow aid to prepare a sample for evaluating spreadability. 0.3 g of the powder sample was placed in a recess of a table having a size of 25 mm x 30 mm and a depth of 0.2 mm, and then a roller was rolled on the table at a speed of about 64 mm / sec to smooth the powder in the recess. From the area of the powder filled in the measurement site of the recess, the area occupied by the powder relative to the area of the recess was calculated as the dispersion rate of the powder. The temperature of the table was set at a temperature 15°C lower than the melting point of the powder measured above. The appearance at the time of spraying was evaluated according to the following criteria. ○: In the spreadability evaluation, the powder was spread evenly. ×: In the spreadability evaluation, the powder was not spread uniformly, or aggregation of powder particles was observed.
[0096] 2.Materials used 2-1. Propylene polymer (A) The following propylene-based polymers, Components A1 and A2, were prepared. The properties of these resins are summarized in Table 1. (All of the following are pellets to which an antioxidant and a neutralizing agent have been added.) Component A1: A grade of "Novatec PP" manufactured by Japan Polypropylene Corporation and having the following composition was used. The material is a propylene-α-olefin block copolymer polymerized with a Ziegler-Natta catalyst, where the α-olefin is ethylene. The MFR (230°C, 2.16 kg load) of the entire copolymer is 8.5 g / 10 min, the content of the propylene-α-olefin copolymer part (a2) is 16 wt%, the α-olefin content of the propylene-α-olefin copolymer part (a2) is 49 wt%, the melting peak temperature (Tm2nd) observed during the second heating is 163°C, and the heat of crystallization (ΔH) observed during the first cooling is 94 J / g. Component A2: A grade of "Novatec PP" manufactured by Japan Polypropylene Corporation and having the following composition was used. The material is a propylene-α-olefin random copolymer polymerized with a Ziegler-Natta catalyst, where the α-olefin is ethylene. The MFR (230°C, 2.16 kg load) of the entire copolymer is 8.0 g / 10 min, the content of the propylene-α-olefin copolymer part (a2) is 0 wt%, the melting peak temperature (Tm2nd) observed during the second heating is 141°C, and the heat of crystallization (ΔH) observed during the first cooling is 74 J / g.
[0097] [Table 1]
[0098] 2-2. Thermoplastic elastomer (B) The following commercially available thermoplastic elastomer (B), component B1, was prepared: Ingredient B1: Manufactured by Mitsui Chemicals, Inc., product name "Tafmer A4090S". The MFR of component B1 (230°C, 2.16 kg load) is 6.7 g / 10 min, and the density is 0.893 g / cm 3 It is.
[0099] 2-3. Filler (C) Ingredient C1: Manufactured by Nippon Talc Co., Ltd., product name "PC25RC". The median diameter D50 of the component C1, measured by the method described above, was 5.8 μm.
[0100] 3. Examples 1 to 2 and Comparative Examples 1 to 3 3-1.Mixing and melt kneading The propylene-based polymer (A), thermoplastic elastomer (B) and filler (C) shown in Table 2 were blended in the ratios shown in Table 2. 0.5 parts by weight of a phenol-based antioxidant (BASF: IRGANOX1010) and 0.5 parts by weight of a phosphorus-based antioxidant (BASF: Irgafos168) were added per 100 parts by weight of the total composition including the propylene-based polymer (A), thermoplastic elastomer (B) and filler (C) and mixed using a super mixer. The mixture was then melt-kneaded using a twin-screw extruder (TEX30, manufactured by Japan Steel Works) at an extrusion temperature of 230°C and a discharge rate of 20 kg / h to obtain pellets of the resin composition.
[0101] 3-2. Powder production The pellets of the resin composition obtained by the above melt kneading were pulverized by freeze-pulverization using liquid nitrogen and high-speed rotary pulverization.
[0102] 3-3.Evaluation The resulting resin composition and its powder were subjected to performance evaluation according to the methods described above. The results are shown in Table 2.
[0103] [Table 2]
[0104] From the results shown in Table 2, in Examples 1 and 2, which satisfy the invention specific requirements of the resin composition of the present invention, the flexural modulus is 1500 MPa or more, the rigidity is high, and the Charpy impact value is 20 kJ / m 2 The above properties also provide good impact resistance, and the total heat of crystallization of the powder is small at 80 J / g or less, providing a well-balanced and excellent spread rate and appearance. On the other hand, from the results shown in Table 2, Comparative Examples 1 to 3, which do not satisfy the specific features of the present invention, are inferior because of a poor balance of these performances. For example, Comparative Examples 1 and 2, which do not contain the thermoplastic elastomer (B), have a Charpy impact value of 10 kJ / m 2The melting peak temperature (Tm) of Comparative Example 3 is less than 150° C., so the resin composition is unlikely to have sufficient rigidity, and the Charpy impact value is less than 10 kJ / m. 2 It is inferior in terms of dispersibility evaluation. [Industrial Applicability]
[0105] The resin composition for powder bed fusion of the present invention makes it possible to produce molded articles having an excellent balance between rigidity and impact resistance. Therefore, there are no particular limitations on the uses of the composition and the applications can be appropriately selected depending on the purpose. For example, the composition can be used in a wide range of applications, such as three-dimensional shapes for food containers, cosmetic containers, medical parts, automobile parts, transport trays, and furniture.
Claims
1. A resin composition for powder bed fusion bonding, comprising 100 parts by weight of a propylene-based polymer (A) satisfying the following requirements (A-i) to (A-iii), 10 to 250 parts by weight of a thermoplastic elastomer (B), and 10 to 150 parts by weight of a filler (C). Requirement (Ai): The melt flow rate at 230° C. (230° C., 2.16 kg load) is 0.1 to 30 g / 10 min. Requirement (A-ii): The copolymer comprises 50 to 95% by weight of a propylene homopolymer portion (a1) and 5 to 50% by weight of a propylene / α-olefin copolymer portion (a2). Requirement (A-iii): The copolymer portion (a2) is a copolymer portion having a propylene unit content of 30 to 80% by weight and an α-olefin unit content of 20 to 70% by weight.
2. 2. The resin composition for powder bed fusion bonding according to claim 1, which satisfies the following requirement (I): Requirement (I): In differential scanning calorimetry, the melting peak temperature (Tm) observed in the first heating is 150 to 170°C, and the total amount of heat of crystallization (ΔH) observed in the first heating is 30 to 80 J / g. However, in the differential scanning calorimetry, the temperature is raised from 23°C to 200°C at a rate of 10°C / min, which is the first heating, then held at 200°C for 5 minutes, and then cooled to 40°C at a rate of 10°C / min, which is the first heating.
3. 2. The resin composition for powder bed fusion bonding according to claim 1, wherein the resin composition for powder bed fusion bonding is contained in a form of a powder that satisfies the following requirement (II): Requirement (II): The median diameter D50 of the powder is 5 to 250 μm as measured by laser diffraction.
4. 2. The resin composition for powder bed fusion bonding according to claim 1, wherein the thermoplastic elastomer (B) satisfies the following requirements (Bi) and (B-ii): Requirement (Bi): The melt flow rate at 230° C. (230° C., 2.16 kg load) is 0.1 to 20 g / 10 min. Requirement (B-ii): Density is 0.855 to 0.905 g / cm 3 It is.
5. 2. The resin composition for powder bed fusion bonding according to claim 1, wherein the filler (C) satisfies the following requirement (C-i): Requirement (Ci): The median diameter D50 is 1 to 160 μm as measured by a laser diffraction method in accordance with JIS R1629.
6. 2. The resin composition for powder bed fusion bonding according to claim 1, further comprising 0.01 to 2.50 parts by weight of a nucleating agent (D) based on 100 parts by weight of the propylene polymer (A).
7. 2. The resin composition for powder bed fusion bonding according to claim 1, which is a melt-kneaded resin composition comprising the propylene-based polymer (A), the thermoplastic elastomer (B) and the filler (C).
8. A molded article obtained by powder bed fusion using the resin composition for powder bed fusion according to any one of claims 1 to 7.
9. A method for producing a molded article, comprising the step of three-dimensionally molding a molded article by powder bed fusion using a resin composition for powder bed fusion, the resin composition comprising 100 parts by weight of a propylene-based polymer (A) satisfying the following requirements (A-i) to (A-iii), 10 to 250 parts by weight of a thermoplastic elastomer (B) and 10 to 150 parts by weight of a filler (C). Requirement (Ai): The melt flow rate at 230° C. (230° C., 2.16 kg load) is 0.1 to 30 g / 10 min. Requirement (A-ii): The copolymer comprises 50 to 95% by weight of a propylene homopolymer portion (a1) and 5 to 50% by weight of a propylene / α-olefin copolymer portion (a2). Requirement (A-iii): The copolymer portion (a2) is a copolymer portion having a propylene unit content of 30 to 80% by weight and an α-olefin unit content of 20 to 70% by weight.
Citation Information
Patent Citations
Powder for stereo-lithography, molding device, molding method and powder
JP2020093515A
Powder composition for additive process and printed articles thereof
WO2022023195A1