Cured product, dry film, and printed wiring board

A photosensitive resin composition with controlled reflectance values addresses light reflection issues on printed wiring boards, enhancing camera module operation by reducing specular and total reflectance.

JP2024143404APending Publication Date: 2024-10-11TAIYO HOLDINGS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023056063
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing solder resist layers on printed wiring boards reflect light, interfering with camera modules' sensors, leading to operational issues.

Method used

A photosensitive resin composition with specific reflectance values, containing a carboxyl group-containing resin, photopolymerizable monomer, photopolymerization initiator, inorganic filler, and colorant, is used to form a cured product with reduced light reflection, achieved by controlling regular and total reflectance to 2.5% or less and 6.3% or less, respectively.

Benefits of technology

The solution effectively suppresses light reflection, ensuring camera modules operate correctly by minimizing sensor interference.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143404000001
    Figure 2024143404000001
  • Figure 2024143404000002
    Figure 2024143404000002
  • Figure 2024143404000003
    Figure 2024143404000003
Patent Text Reader

Abstract

To provide a cured product of a photosensitive resin composition which can suppress reflection of light, and a dry film using the same, and a printed wiring board.SOLUTION: There is provided a cured product of a photosensitive resin composition, wherein when the surface of the cured product is measured across measurement wavelengths from 360 nm to 730 nm by the SCI system and the SCE system, in the entire range of the measurement wavelengths, a value obtained by subtracting the SCE system from the SCI system (regular reflectance) is 2.5% or less, and a value of the SCI system (total reflectance) is 6.3% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cured product, a dry film, and a printed wiring board. [Background technology]

[0002] 2. Description of the Related Art Electronic devices contain built-in components in which various electronic components are mounted by soldering or the like on a printed wiring board, which is a substrate on which an electronic circuit pattern is printed using copper wire. However, when mounting electronic components on a printed wiring board with exposed copper wires, there is a possibility that the copper wires may break due to external force, or that short circuits may occur due to solder sticking to parts other than the copper wires, etc. Therefore, a solder resist layer is formed on the printed wiring board to protect the circuit pattern and prevent short circuits.

[0003] The solder resist layer is often formed from a cured product of a photosensitive resin composition, and various photosensitive resin compositions have been proposed so far. For example, Patent Document 1 discloses a photosensitive resin composition containing a carboxyl group-containing resin and a photopolymerization initiator.

[0004] In recent years, the number of electronic devices equipped with cameras has increased, and it is becoming more common for camera modules, which are camera components, to be mounted on printed wiring boards. The camera module has a sensor that detects light, and the sensor detects the light that hits the camera module and the camera module operates.

[0005] However, the sensor of the camera module can detect not only the light that hits the camera but also the light reflected from the solder resist layer, so the solder resist layer used to mount the camera module is required to have properties that suppress light reflection. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2016-65942 A Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present invention is to provide a cured product of a photosensitive resin composition capable of suppressing light reflection, and a dry film and a printed wiring board each using the same. [Means for solving the problem]

[0008] That is, the cured product according to the present invention is A cured product of a photosensitive resin composition, When the surface of the cured product is measured by the SCI method and the SCE method at a measurement wavelength of 360 nm to 730 nm, the measured value by the SCI method minus the measured value (specular reflectance) by the SCE method is 2.5% or less over the entire range of measurement wavelengths, and the measured value (total reflectance) by the SCI method is 6.3% or less.

[0009] In another aspect of the present invention, The photosensitive resin composition preferably contains a carboxyl group-containing resin, a photopolymerizable monomer, a photopolymerization initiator, an inorganic filler, and a colorant.

[0010] In another aspect of the present invention, A dry film including a first film and a resin layer made of a photosensitive resin composition, The cured product of the resin layer in the state where it is peeled off from the first film is the above-mentioned cured product.

[0011] A printed wiring board according to another aspect of the present invention is characterized by having the above-mentioned cured product. Effect of the Invention

[0012] According to the present invention, it is possible to provide a cured product of a photosensitive resin composition capable of suppressing light reflection, as well as a dry film and a printed wiring board using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The cured product, dry film, and printed wiring board according to this embodiment will be described below.

[0014] (cured product) The cured product of the present embodiment has a surface that is measured using the SCI (Specular Component Include: including specular reflected light) method and the SCE (Specular Component Exclude: excluding specular reflected light) method, and the measured values ​​satisfy the following conditions (1) and (2). (1) The measured value by the SCI method - the measured value by the SCE method (regular reflectance) is 2.5% or less (2) The measured value (total reflectance) by the SCI method is 6.3% or less

[0015] The measurement by the SCI method according to this embodiment is performed by an apparatus capable of measuring reflected light. Specifically, the surface of the cured product is irradiated with light of a predetermined wavelength range, and the reflected light, including specular reflected light, from the surface of the cured product is measured. According to this embodiment, the predetermined range of wavelengths is 360 nm to 730 nm. The measurement by the SCI method according to this embodiment is performed in increments of 10 nm. The measurement value by the SCI method according to this embodiment is the maximum value among the values ​​obtained by measurement in the above measurement range.

[0016] The measurement by the SCE method according to the present embodiment is performed using an apparatus capable of measuring reflected light. Specifically, light of a predetermined wavelength range is irradiated onto the surface of the cured product, and the reflected light excluding the specularly reflected light from the surface of the cured product is measured. According to this embodiment, the predetermined range of wavelengths is 360 nm to 730 nm. The measurement by the SCE method according to this embodiment is performed in increments of 10 nm. The measurement value by the SCE method according to this embodiment is the maximum value among the values ​​obtained by measurement in the above measurement range.

[0017] The measured value of the cured product by the SCI method minus the measured value by the SCE method (regular reflectance) is 2.5% or less, preferably 2% or less. The measured value of the cured product by the SCI method (total reflectance) is 6.3% or less, preferably 6% or less. When the values ​​measured by the SCI method and the SCE method satisfy the above (1) and (2), the cured product is able to suppress light reflection from the surface by absorbing the light that hits the surface.

[0018] The method for measuring the cured product by the SCI method and the SCE method is not particularly limited and can be appropriately selected depending on the purpose as long as it is a common method. For example, a color difference meter can be used.

[0019] <Method of manufacturing the cured product> The method for producing the cured product is not particularly limited and can be appropriately selected depending on the purpose. For example, the cured product can be formed by the method described below.

[0020] The method of forming a resin layer made of a photosensitive resin composition on a substrate is not particularly limited and can be appropriately selected according to the purpose. For example, the photosensitive resin composition is adjusted to an appropriate viscosity using an organic solvent, and then coated on a substrate. The substrate is then heated at a temperature of 60°C to 100°C for 15 to 90 minutes to evaporate and dry (temporarily dry) the organic solvent contained in the photosensitive resin composition, thereby forming a tack-free resin layer. Examples of the coating method include a dip coating method, a flow coating method, a roll coating method, a bar coater method, a screen printing method, and a curtain coating method. The volatilization drying performed after coating the photosensitive resin composition can be performed using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, etc. (a method of contacting the hot air in the dryer with a countercurrent flow using a heat source of an air heating method using steam, and a method of blowing the hot air from a nozzle onto a support). In addition, in the case of a dry film described later, a resin layer is formed on a substrate by laminating the substrate with a laminator or the like so that the resin layer contacts the substrate, and then the first film is peeled off.

[0021] Substrates include printed wiring boards and flexible printed wiring boards with circuits already formed using copper etc., as well as materials such as paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, copper-clad laminates for high frequency circuits using materials such as fluororesin-polyethylene-polyphenylene ether, polyphenylene oxide-cyanate etc., including copper-clad laminates of all grades (FR-4 etc.), as well as metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer plates etc.

[0022] In the case of a dry film form, the lamination onto the substrate is preferably performed under pressure and heat using a vacuum laminator or the like. By using such a vacuum laminator, when a circuit-formed substrate is used, even if the surface of the circuit substrate is uneven, the dry film adheres to the circuit substrate, so that no air bubbles are mixed in, and the filling of the recesses on the substrate surface is improved. The pressure condition is preferably about 0.1 to 2.0 MPa, and the heating condition is preferably 40 to 120°C.

[0023] When the photosensitive resin composition of the present invention contains an organic solvent, it is preferable to apply the photosensitive resin composition to the surface of a substrate and then perform volatilization drying. The volatilization drying can be performed using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, etc. (a method of countercurrent contact of hot air in a dryer using a heat source of an air heating method using steam, or a method of spraying the hot air from a nozzle onto the substrate).

[0024] After forming a resin layer on a substrate, the resin layer is selectively exposed to active energy rays through a photomask having a predetermined pattern formed thereon, and the unexposed portion is developed with a dilute alkaline aqueous solution (e.g., 0.3 to 3 mass% aqueous sodium carbonate solution) to form a pattern of the cured product. In the case of a dry film, after exposure, the first film is peeled off from the dry film and development is performed to form a patterned cured product on the substrate. In addition, in the case of a dry film form, the first film may be peeled off from the dry film before exposure, and the exposed resin layer may be exposed and developed, as long as the characteristics are not impaired. Furthermore, a cured product excellent in various properties such as adhesion and hardness can be formed by irradiating the cured product with active energy rays and then heat curing (e.g., 100 to 220°C), or irradiating active energy rays after heat curing, or by heat curing only to perform final finishing curing (main curing).

[0025] The exposure machine used for the above-mentioned active energy ray irradiation may be a machine equipped with a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, or the like, and capable of irradiating ultraviolet rays in the range of 350 to 450 nm. Furthermore, a direct imaging machine (for example, a laser direct imaging machine that directly draws an image with a laser based on CAD data from a computer) may also be used. The lamp light source or laser light source of the direct imaging machine may have a maximum wavelength in the range of 350 to 450 nm. The exposure dose for forming an image varies depending on the film thickness, etc., but is generally 10 to 1000 mJ / cm. 2 , preferably 20 to 800 mJ / cm 2 The range may be:

[0026] The developing method can be a dipping method, a shower method, a spray method, a brush method, or the like, and the developing solution can be an aqueous alkali solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, or the like.

[0027] <Photosensitive resin composition> The cured product of the present embodiment is a cured product of a photosensitive resin composition. The photosensitive resin composition contains a carboxyl group-containing resin, a photopolymerizable monomer, a photopolymerization initiator, an inorganic filler, and a colorant, and further contains other components as necessary.

[0028] <<Carboxyl group-containing resin>> The carboxyl group-containing resin is a resin having a carboxyl group in the molecule, and various conventionally known resins can be used. The photosensitive resin composition contains a carboxyl group-containing resin, which can impart developability (alkali developability) to the photosensitive resin composition. In particular, a carboxyl group-containing resin having an ethylenically unsaturated double bond in the molecule (carboxyl group-containing photosensitive resin) is preferred in terms of photocurability and development resistance. The ethylenically unsaturated double bond is preferably derived from acrylic acid or methacrylic acid, or a derivative thereof.

[0029] Specific examples of the carboxyl group-containing resin include the following compounds (which may be either oligomers or polymers): These may be used alone or in combination of two or more.

[0030] (1) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, isobutylene, etc.

[0031] (2) Carboxylic acid-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.

[0032] (3) Carboxylic acid-containing photosensitive urethane resins obtained by polyaddition reaction of diisocyanates with partially acid anhydride-modified products of reaction products of bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins and biphenol type epoxy resins with monocarboxylic acid compounds having ethylenically unsaturated double bonds such as (meth)acrylic acid, carboxyl group-containing dialcohol compounds and diol compounds.

[0033] (4) A photosensitive urethane resin containing a carboxyl group, which is terminated with (meth)acrylation by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (3).

[0034] (5) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acrylation formed by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (3).

[0035] (6) A carboxyl group-containing photosensitive resin obtained by reacting a difunctional or more polyfunctional (solid) epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride to the hydroxyl groups present in the side chains.

[0036] (7) A carboxyl group-containing photosensitive resin obtained by reacting a multifunctional epoxy resin with the hydroxyl groups of a bifunctional (solid) epoxy resin further epoxidized with epichlorohydrin, with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups.

[0037] (8) Carboxyl group-containing polyester resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.

[0038] (9) A carboxyl group-containing photosensitive resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl group of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, or the like.

[0039] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.

[0040] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.

[0041] (12) A carboxyl group-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to any one of the resins (1) to (11).

[0042] In this specification, (meth)acrylate is a term that collectively refers to acrylate, methacrylate, and mixtures thereof, and the same applies to other similar expressions.

[0043] The acid value of the carboxyl group-containing resin is preferably 40 mgKOH / g to 150 mgKOH / g. By making the acid value of the carboxyl group-containing resin 40 mgKOH / g or more, alkaline development becomes good. Furthermore, when the photosensitive resin composition is used as a solder resist, it is possible to easily draw a good resist pattern by setting the acid value to 150 mgKOH / g or less, and more preferably 50 mgKOH / g to 130 mgKOH / g.

[0044] The weight average molecular weight of the carboxyl group-containing resin varies depending on the resin skeleton, but is generally preferably 2,000 to 150,000. By making the weight average molecular weight 2,000 or more, tack-free performance and resolution can be improved. Also, by making the weight average molecular weight 150,000 or less, developability and storage stability can be improved. More preferably, it is 5,000 to 100,000.

[0045] The amount of the carboxyl group-containing resin in the photosensitive resin composition is preferably 20% by mass or more and 60% by mass or less, calculated as solid content. By making it 20% by mass or more, the strength of the cured coating film can be improved. Also, by making it 60% by mass or less, the viscosity becomes appropriate and the printability is improved. More preferably, it is 25% by mass or more and 50% by mass or less.

[0046] <<Photopolymerizable monomer>> The photopolymerizable monomer is a monomer having an ethylenically unsaturated double bond. Examples of such photopolymerizable monomers include commonly known polyester (meth)acrylates, polyether (meth)acrylates, urethane (meth)acrylates, carbonate (meth)acrylates, and epoxy (meth)acrylates. Specifically, alkyl acrylates such as 2-ethylhexyl acrylate and cyclohexyl acrylate; hydroxyalkyl acrylates such as 2-hydroxyethyl acrylate and 2-hydroxypropyl acrylate; mono- or diacrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol and dipropylene glycol; acrylamides such as N,N-dimethylacrylamide, N-methylolacrylamide and N,N-dimethylaminopropylacrylamide; aminoalkyl acrylates such as N,N-dimethylaminoethyl acrylate and N,N-dimethylaminopropyl acrylate; hexanediol, trimethylolpropane, pentaerythritol, ditrimethylolpropane, dipentaerythritol, trishydroxyethyl Examples of the acrylates include polyhydric alcohols such as polyisocyanurate, or their alkylene oxide adducts or ε-caprolactone adducts; phenols such as phenoxy acrylate and bisphenol A diacrylate, or their alkylene oxide adducts; acrylates of glycidyl ethers such as glycerin diglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; and, without being limited to the above, acrylates and melamine acrylates obtained by directly acridating polyols such as polyether polyols, polycarbonate diols, hydroxyl-terminated polybutadienes, and polyester polyols, or by urethane acridating them via diisocyanates, and methacrylates corresponding to the above acrylates. These may be used alone or in combination of two or more. The photopolymerizable monomer can also be used as a reactive diluent.

[0047] The content of the photopolymerizable monomer is preferably 5 to 100 parts by mass relative to 100 parts by mass of the carboxyl group-containing resin. When the blending amount is 5 parts by mass or more, the photocurability is good, and pattern formation is easy in alkaline development after irradiation with active energy rays. On the other hand, when it is 100 parts by mass or less, halation is unlikely to occur and good resolution can be obtained.

[0048] <<Photopolymerization initiator>> The photopolymerization initiator is for reacting the above-mentioned carboxyl group-containing photosensitive resin or photopolymerizable monomer by exposure. Any known photopolymerization initiator can be used. The photopolymerization initiator may be used alone or in combination of two or more.

[0049] Examples of the photopolymerization initiator include bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, and bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide. bisacylphosphine oxides such as bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide and bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphine acid methyl ester, 2-methylbenzoyldiphenylphosphine oxide, pivaloylphenylphosphine Isopropyl phosphinate, monoacylphosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide; ethyl phenyl(2,4,6-trimethylbenzoyl)phosphinate, 1-hydroxy-cyclohexyl phenyl ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, Hydroxyacetophenones such as 2-hydroxy-2-methyl-1-phenylpropan-1-one; benzoins such as benzoin, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, and benzoin n-butyl ether; benzoin alkyl ethers; benzophenones such as benzophenone, p-methylbenzophenone, Michler's ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, and 4,4'-bisdiethylaminobenzophenone;Acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl)-1-[4-(4-morpholinyl)phenyl]-1-butanone acetophenones such as acetophenone, N,N-dimethylaminoacetophenone; thioxanthones such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; anthraquinone, chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, Anthraquinones such as 2-aminoanthraquinone; ketals such as acetophenone dimethyl ketal and benzil dimethyl ketal; benzoic acid esters such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate, and p-dimethylbenzoic acid ethyl ester; 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyl oxime esters such as bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrol-1-yl)ethyl)phenyl]titanium, and other titanocenes; phenyl disulfide 2-nitrofluorene, butyroin, anisoin ethyl ether, azobisisobutyronitrile, tetramethylthiuram disulfide, and the like.

[0050] The content of the photopolymerization initiator is preferably 0.5 to 10 parts by mass, more preferably 3 to 8 parts by mass, based on 100 parts by mass of the carboxyl group-containing resin, calculated as solid content. When the content value is within this range, the hardness of the cured product of the photosensitive resin composition can be improved.

[0051] <<Inorganic filler>> The inorganic filler is also contained to form irregularities on the surface of the cured product, thereby decreasing the measurement value of the cured product by the SCI method. As the filler, any known filler can be used, with barium sulfate, amorphous silica, crystalline silica, fused silica, spherical silica, hydrotalcite and talc being particularly preferred. The amorphous silica may be any known or commonly used one, may be synthetic or natural, and may or may not be surface-treated.

[0052] The content of the filler is preferably 20 to 80 mass %, more preferably 25 to 75 mass %, and further preferably 30 to 50 mass %, calculated as solid content based on the total amount of the photosensitive resin composition. By having the amount of the filler in the above range, the strength of the cured product can be increased.

[0053] <<Coloring agent>> The colorant preferably contains a black colorant, and more preferably contains a colorant other than black as required.

[0054] <<<Black colorant>>> The black colorant is not particularly limited as long as it is black, and can be appropriately selected depending on the purpose, and examples thereof include carbon black, zirconium nitride, Pigment Black 1, 6, 7, 8, 9, 10, 11, 12, 13, 18, 20, 25, 26, 28, 29, 30, 31, 32, etc. These may be used alone or in combination of two or more kinds.

[0055] <<<Colorants other than black>>> The colorant other than black is not particularly limited as long as it does not impair the effect of the cured product of the present embodiment and can be appropriately selected depending on the purpose. For example, commonly used and known colorants such as red, blue, green, and yellow can be used, and any of pigments, dyes, and colorants can be used.

[0056] Specifically, the following color index (CI; published by The Society of Dyers and Colourists) numbers can be included.

[0057] Red colorants include monoazo, disazo, azo lake, benzimidazolone, perylene, diketopyrrolopyrrole, condensed azo, anthraquinone, and quinacridone. Blue colorants include phthalocyanine and anthraquinone, and pigments can be used as pigments. In addition to these, metal-substituted or unsubstituted phthalocyanine compounds can also be used. Green colorants include phthalocyanine, anthraquinone, and perylene. In addition to these, metal-substituted or unsubstituted phthalocyanine compounds can also be used. Yellow colorants include monoazo, disazo, condensed azo, benzimidazolone, isoindolinone, and anthraquinone.

[0058] The content of the colorant is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 10 parts by mass or less, and more preferably 0.1 to 7 parts by mass, relative to 100 parts by mass of the carboxyl group-containing resin. When the content of the colorant falls within this range, a cured product with a high black color is obtained.

[0059] <<Other ingredients>> The photosensitive resin composition of the present embodiment may further contain, as necessary, components such as a thermosetting component, a photoinitiator assistant, a cyanate compound, an elastomer, a mercapto compound, a urethanization catalyst, a thixotropic agent, an adhesion promoter, a block copolymer, a chain transfer agent, a polymerization inhibitor, a copper inhibitor, an antioxidant, an anti-rust agent, a thickener such as organic bentonite or montmorillonite, at least one of silicone-based, fluorine-based, or polymer-based defoamers and leveling agents, imidazole-based, thiazole-based, or triazole-based silane coupling agents, phosphinates, phosphate ester derivatives, phosphorus compounds such as phosphazene compounds, and other flame retardants. These may be known in the field of electronic materials.

[0060] <Method for producing photosensitive resin composition> The method for producing the photosensitive resin composition is not particularly limited, and the composition can be produced, for example, by blending the above-mentioned components in a predetermined ratio and then kneading or mixing at room temperature with a kneading means such as a three-roll mill, a ball mill, a bead mill, a sand mill, or a stirring means such as a super mixer, a planetary mixer, etc. Furthermore, prior to the kneading or mixing, pre-kneading or pre-mixing may be performed as necessary.

[0061] The photosensitive resin composition of the present embodiment may be used in the form of a dry film or in the form of a liquid. When used in the form of a liquid, the composition may be one-component or two or more-component.

[0062] (Dry film) The dry film of the present embodiment includes a first film and a resin layer. The first film in the dry film according to the present invention refers to a film that is at least adhered to the resin layer when the dry film is laminated by heating or the like so that the resin layer side made of the photosensitive resin composition formed on the dry film is in contact with a base material such as a substrate to be integrally molded. The first film may be peeled off from the resin layer in a step after lamination. In particular, in the present invention, it is preferable to peel off from the resin layer in a step after exposure.

[0063] <<Resin layer>> The resin layer is made of a photosensitive resin composition. The photosensitive resin composition may be the above-mentioned photosensitive resin composition, and the resin layer may be the above-mentioned resin layer. The resin layer is cured to become the above-mentioned cured product. That is, the cured product of the resin layer in a state in which it has been peeled off from the first film is the above-mentioned cured product.

[0064] <<First Film>> As the first film, any known film can be used without any particular limitation, and for example, a film made of a thermoplastic resin such as a polyester film such as polyethylene terephthalate or polyethylene naphthalate, a polyimide film, a polyamideimide film, a polypropylene film, or a polystyrene film can be suitably used. Among these, a polyester film is preferred from the viewpoints of heat resistance, mechanical strength, handling, etc. A laminate of these films can also be used as the first film.

[0065] From the viewpoint of improving mechanical strength, the above-mentioned thermoplastic resin film is preferably a film stretched in a uniaxial or biaxial direction.

[0066] When a thermoplastic resin film is used as the first film, a film having a specific surface morphology may be used by adding a filler to the resin when forming the film (kneading process), by matte coating (coating process), by subjecting the film surface to a blasting process such as sandblasting, or by hairline processing or chemical etching, etc.

[0067] The thickness of the first film is not particularly limited, but can be, for example, 10 μm to 150 μm.

[0068] <<Second film>> After forming a resin layer of the photosensitive resin composition of the present invention on the first film, it is preferable to further laminate a peelable second film on the surface of the resin layer for the purpose of preventing dust from adhering to the surface of the resin layer, etc. The second film in the dry film of the present invention refers to a film that is peeled off from the resin layer before lamination when the dry film is laminated by heating or the like so that the resin layer side of the dry film is in contact with a base material such as a substrate to be integrally molded.

[0069] The second film that can be peeled off from the resin layer may be, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, surface-treated paper, etc., as long as the adhesive strength between the resin layer and the second film is smaller than the adhesive strength between the resin layer and the first film when the second film is peeled off.

[0070] The thickness of the second film is not particularly limited, but can be, for example, 10 μm to 150 μm.

[0071] When producing a dry film, the photosensitive resin composition of the present embodiment is diluted with an organic solvent to adjust the viscosity to an appropriate level, and then coated on a first film to a uniform thickness using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, applicator, or the like, and typically dried for 1 to 30 minutes at a temperature of 50° C. to 130° C. to obtain a film. There are no particular limitations on the coating film thickness, but it is generally appropriately selected within the range of 1 μm to 150 μm, preferably 5 μm to 60 μm, in terms of the film thickness after drying.

[0072] (Printed Wiring Board) The printed wiring board of the present embodiment has the above-mentioned cured product. The size and type of the printed wiring board are not particularly limited and can be appropriately selected depending on the purpose. EXAMPLES

[0073] Next, tests carried out by the present inventors will be described, but the present invention is not limited to these.

[0074] (Preparation of Photosensitive Resin Composition) <Synthesis of carboxyl group-containing resin> 650 parts by mass of diethylene glycol monoethyl ether acetate was charged with 1,070g of orthocresol novolac epoxy resin (EPICLON N-695, manufactured by DIC Corporation, softening point 95°C, epoxy equivalent 214, average functional group number 7.6), 360g of acrylic acid, and 1.5g of hydroquinone, and the mixture was heated to 100°C and stirred to dissolve uniformly. Next, 4.3 parts by mass of triphenylphosphine was charged, and the mixture was heated to 110°C and reacted for 2 hours, after which 1.6 parts by mass of triphenylphosphine was added, and the mixture was heated to 120°C and reacted for another 12 hours. 525g of aromatic hydrocarbon (T-Sol 150, manufactured by Standard Oil Co., Ltd. Osaka Sales Office) and 608g (4.0 mol) of tetrahydrophthalic anhydride were charged into the resulting reaction liquid, and the reaction was carried out at 110°C for 4 hours. Further, 142.0 g of glycidyl methacrylate was added to the obtained reaction liquid, and the reaction was carried out for 4 hours at 115° C. In this manner, a solution of a carboxyl group-containing resin having a solid content of 65% and an acid value of the solid content of 77 mgKOH / g was obtained.

[0075] <Preparation of Photosensitive Resin Composition> The components shown in Table 1 below were mixed in the amounts shown in the table, pre-mixed with a mixer, and then kneaded with a three-roll mill to prepare photosensitive resin compositions A to D. The values ​​in Table 1 indicate parts by mass and are calculated as solid contents.

[0076] [Table 1]

[0077] The details of each component in Table 1 are as follows. Carboxyl group-containing resin: Carboxyl group-containing resin synthesized in the synthesis example Photopolymerizable monomer: Product name: Dipentaerythritol hexaacrylate (DPHA), (manufactured by Nippon Kayaku Co., Ltd.) Photopolymerization initiator: 2-benzyl-2-(dimethylamino)-4'morpholinobutyrophenone (Omnirad 369E, IGM Resins) Inorganic filler: Silica (ACE MATT OK412, manufactured by EVONIK DEGUSSA) Inorganic filler: Talc (LMP-100, manufactured by Fuji Talc Co., Ltd.) Inorganic filler: barium sulfate (B-30, Sakai Chemical Industry Co., Ltd.) Black colorant: Carbon black (MA-100, manufactured by Mitsubishi Chemical Corporation) Black colorant: Zirconium nitride (UB-2, manufactured by Mitsubishi Materials Denka-kasei Co., Ltd.) Blue colorant: Fastgen Blue 5380 / FA5380, manufactured by DIC Corporation Red colorant: Paliogen Red K3580, manufactured by BASF Japan Ltd. Other ingredients: Epoxy resin (EPICLON N-770, manufactured by DIC Corporation)

[0078] (Preparation of the first film) <Preparation of Matte PETα> An iso-butylated melamine resin (Amidair L-125-60, solid content 60%, manufactured by DIC Corporation) and an acrylic resin for melamine baking (Acrydic A-405, solid content 50%, manufactured by DIC Corporation) were mixed in a mass ratio of 25:75 (solid content equivalent), and the mixture was pre-mixed with a mixer to obtain an acrylic melamine resin. Next, the obtained acrylic melamine resin was diluted with methyl ethyl ketone to prepare a resin solution with a solid content concentration of 35% by mass. Methyl ethyl ketone was further added to this resin solution to obtain an appropriate solid content concentration according to the thickness of the coating film, and then a silicone-based resin (Simac US-270, manufactured by Toa Gosei Co., Ltd.) and a filler (J-4P, acrylic beads, manufactured by Negami Chemical Industries Co., Ltd.) adjusted to have a maximum particle size of 2 μm were added so that the blending ratio of the acrylic melamine resin, the silicone-based resin, and the filler was 59.7:0.3:108 (solid content equivalent) by mass, and the mixture was thoroughly stirred at room temperature to obtain a uniform coating liquid. The obtained coating liquid was applied to a polyethylene terephthalate film (Lumirror T60, manufactured by Toray Industries, Inc.) having a thickness of 38 μm and dried at 130° C. for 20 seconds to prepare a first film 1 including a matte coating layer. The first film 1 had a total thickness of 40 μm. In addition, the arithmetic surface roughness Ra of the side on which the matte coating layer was provided was measured in shape measurement mode using a laser microscope (VX-100, manufactured by Keyence Corporation) in accordance with JIS B 0601:2001. Specifically, in the shape measurement mode of the laser microscope, an observation application (VK-H1XV) was started, the sample to be measured was placed on the XY stage, and the focus was adjusted by autofocus using a 50x objective lens in the shape measurement mode. The Z axis was controlled as necessary to adjust the focus to an optimal position. The observation image was captured in the automatic measurement mode or manual measurement mode. Next, an analysis application (VK-H1XA) was started, and measurement of Ra was started. As a result of the measurement, the arithmetic surface roughness Ra of the surface on which the matte coating layer was provided of the first film 1 was 0.180 μm.

[0079] <Matting PETβ> In the method for producing matte PETα, the filler was changed to fumed silica (AEROSIL200, manufactured by Nippon Aerosil Co., Ltd.), the mixing ratio of acrylic melamine resin, silicone resin and filler was changed to 59.7:0.3:80.0 (solid content equivalent) by mass, and dispersion was performed using a bead mill. Except for this, matte PETβ including a matte coating layer was produced in the same manner as the manufacturing method of matte PETα. The total thickness of this film was 40 μm, and the arithmetic surface roughness Ra of the surface on which the matte coating layer was provided was 1.43 μm.

[0080] <Production of Matte PETγ> Matte PETγ including a matte coating layer was produced in the same manner as in the production method of matte PETα, except that in the production method of matte PETα, the filler was changed to spherical silica (SO-C2, manufactured by Admatechs Co., Ltd.) and the blending ratio of acrylic melamine resin, silicone resin and filler was changed to 59.7:0.3:12.0 (solids content equivalent) by mass. The total thickness of this film was 43 μm, and the arithmetic surface roughness Ra of the surface on which the matte coating layer was provided was 0.196 μm.

[0081] The glossy PET used was a commercially available product (DIAFOIL T100-25, manufactured by Mitsubishi Chemical Corporation).

[0082] (Example 1 and Comparative Example 2: Cured product of photosensitive resin composition) Each photosensitive resin composition was applied to a Cu solid substrate (150 mm x 95 mm x 0.89 mmt) by screen printing in the combinations shown in Table 2 so that the thickness of the coating film after drying was 25 μm, and the substrate was dried in a heat circulation box furnace at 80° C. for 30 minutes to obtain a structure having a resin layer made of the photosensitive resin composition. The Cu solid substrate used was chemically polished with an etching agent (CZ8101, manufactured by MEC Co., Ltd.).

[0083] The obtained structure was exposed to light using an ultra-high pressure mercury lamp DI exposure machine (DXP-3580, manufactured by Oak Manufacturing Co., Ltd.) with a Stouffer 41-step step tablet so that the number of hardening steps was 15. Development was performed with a 1% by mass sodium carbonate aqueous solution at 30°C for a development time twice the break point (shortest development time). Then, a UV conveyor (manufactured by Oak Manufacturing Co., Ltd., metal halide lamp) was used to expose the structure to 1000 mJ / cm. 2 The photosensitive resin composition was exposed to light at 400° C. and cured in a heat circulation box furnace at 150° C. for 60 minutes to obtain a test substrate having a cured product of the photosensitive resin composition (solder resist layer) on the substrate.

[0084] (Examples 2 to 5, Comparative Examples 1 and 3: Dry Film) In the combinations shown in Table 2, each photosensitive resin composition was applied by applicator onto a first film (matte PET α-γ, glossy PET) so that the thickness of the coating film after drying was 25 μm, and then dried in a heat circulation box furnace at 80° C. for 15 minutes to obtain a dry film. The surface of the dry film on which the photosensitive resin composition was formed was laminated onto a Cu solid substrate (150 mm×95 mm×0.89 mmt) using a vacuum laminator CVP-300 (manufactured by Nikko Materials Co., Ltd.) to obtain a structure. The Cu solid substrate used was chemically polished using an etching agent (CZ8101, manufactured by MEC Co., Ltd.).

[0085] The obtained structure was exposed to light using an ultra-high pressure mercury lamp DI exposure machine (DXP-3580, manufactured by Oak Manufacturing Co., Ltd.) so that the number of hardening steps was 15 using a Stouffer 41-step step tablet. After 10 minutes from the end of exposure, the first film was peeled off, and development was performed with a 1% by mass aqueous solution of sodium carbonate at 30°C for a development time twice the break point (shortest development time). Then, a UV conveyor (manufactured by Oak Manufacturing Co., Ltd., metal halide lamp) was used to expose the structure to 1000 mJ / cm. 2 and curing it at 150° C. for 60 minutes in a heat circulation box furnace to obtain a test substrate having a cured product (solder resist layer) of the photosensitive resin composition formed from the dry film on the substrate.

[0086] [Table 2]

[0087] The 60° glossiness, reflectance, Rv (maximum valley depth) value, and L value of the test substrate of the obtained cured product were measured, and the light-receiving property to the sensor was evaluated. The evaluation results are shown in Table 3. * The value was measured, and the light-receiving property to the sensor was evaluated. The evaluation results are shown in Table 3.

[0088] <60° Glossiness> For glossiness measurement, a digital variable-angle glossmeter (BYK-micro-TRI-gloss) was used. After calibration with a standard plate, the glossiness of Gs(60°) on the uneven surface of the cured product was measured.

[0089] <Measurement by SCI method (total reflectance) · SCE method (diffuse reflectance)> The reflectance (total reflectance) of the SCI method was measured using a color difference meter (CM-2600d, manufactured by Konica Minolta Inc.). The surface of the obtained cured product was irradiated with light having a wavelength of 360 nm to 730 nm, and the reflectance of the reflected light including the specularly reflected light from the surface of the cured product was measured. The measurement was performed at 10 nm intervals. The maximum value in this measurement was taken as the measurement value of the cured product by the SCI method. Also, the reflectance (diffuse reflectance) of the SCE method was measured using a color difference meter (CM-2600d, manufactured by Konica Minolta Inc.). The surface of the obtained cured product was irradiated with light having a wavelength of 360 nm to 730 nm, and the reflectance of the reflected light excluding the specularly reflected light from the surface of the cured product was measured. The measurement was performed at 10 nm intervals. The maximum value in this measurement was taken as the measurement value of the cured product by the SCE method. From the measured values of the obtained SCI method and SCE method, the reflectance (SCI method - SCE method) in the specular reflection method was calculated.

[0090] <Maximum valley depth (Rv value)> The maximum depth (Rv value) was measured using a shape measurement laser microscope (VX-100, manufactured by Keyence Corporation) in shape measurement mode. The specific measurement method was to start the observation application (VK-H1XV), place the sample (cured material) to be measured on the xy stage, and adjust the focus with autofocus using a 50x objective lens in shape measurement mode. If necessary, the z-axis was controlled to adjust the focus to the optimal position. The observation image was captured in either automatic measurement mode or manual measurement mode. Next, the analysis application (VK-H1XA) was started and measurement began. The measurement conditions were: observation measurement range (area) 55,965 μm 2 The evaluation points were measured for Rv at 10 points spaced equally from the center of the sample toward the outside, and the average of the values ​​was taken as the maximum depth (Rv value) of the cured surface.

[0091] <L * Value> L in the Lab color space of the cured product * The value was measured on the cured product using a color difference meter (CM-2600d, manufactured by Konica Minolta, Inc.).

[0092] <Light reception by the sensor> The light reception of the cured product by the sensor was evaluated using a digital lux meter (BT-881D, manufactured by BTMETER). The test substrate (cured product) was placed in a room (dark room) where the digital lux meter reading was 0.00 Lux. Using a laser pointer (Sashi-41N), the test substrate was irradiated with laser light from a fixed position 0.3 m high and 1.3 m away horizontally. The light receiving part of the digital lux meter was placed 3 cm horizontally from the laser irradiation point, and the reading was read and evaluated based on the following evaluation criteria. -Evaluation criteria- ◎: Display value is between 0 Lux and 0.5 Lux ○: Display value is between 0.5 Lux and 5 Lux ×: Display value is 5 Lux or more

[0093] [Table 3]

[0094] As is clear from Table 3, in Examples 1 to 5, in which the value of the SCI method minus the value of the SCE method (regular reflectance) was 2.5% or less at 360 nm to 730 nm on the surface of the cured product, and the value of the SCI method (total reflectance) was 6.3% or less, the evaluation result of the light receptivity of the cured product to the sensor was "◎" or "◯". In contrast, in Comparative Examples 1 and 2, in which the values ​​of the regular reflectance were 4.2% and 4.4%, the evaluation result of the light receptivity of the sensor was "×". In addition, in Comparative Example 3, in which the total reflectance was 7.5%, the evaluation result of the light receptivity of the sensor was "×". From the results of Comparative Examples 1 to 3, it was made clear that the evaluation of the light receptivity to the sensor cannot be made good simply by having a low regular reflectance or a low total reflectance. From the above, it was made clear that a cured product having a regular reflectance of 2.5% or less and a total reflectance of 6.3% or less is a cured product capable of suppressing light reflection.

[0095] Although the embodiment of the present invention has been specifically described above, the present invention is not limited to this embodiment, and various modifications are possible without departing from the spirit and scope of the present invention.

Claims

1. A cured product of a photosensitive resin composition, The cured product is characterized in that, when the surface of the cured product is measured by the SCI method and the SCE method at a measurement wavelength of 360 nm to 730 nm, the SCI method-SCE method (regular reflectance) value is 2.5% or less and the SCI method (total reflectance) value is 6.3% or less over the entire range of measurement wavelengths.

2. The cured product according to claim 1 , wherein the photosensitive resin composition contains a carboxyl group-containing resin, a photopolymerizable monomer, a photopolymerization initiator, an inorganic filler, and a colorant.

3. A dry film comprising a first film and a resin layer made of the photosensitive resin composition, A dry film, characterized in that the cured product of the resin layer in a state peeled off from the first film is the cured product according to claim 1 or 2.

4. A printed wiring board comprising the cured product according to claim 1 or 2.

Citation Information

Patent Citations

  • Curable composition, dry film, cured product, printed wiring board, and method for manufacturing printed wiring board

    JP2016065942A