Peltier cooling thermoelectric conversion module
The Peltier-cooled thermoelectric conversion module addresses cooling performance limitations by using thin, low-resistance thermoelectric chips, enhancing heat absorption and thermal efficiency.
Patent Information
- Application Number
- JP2023056105
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing π-type thermoelectric conversion modules lack improvements in cooling performance, particularly in thinning and heat absorption efficiency, despite advancements in thermoelectric performance.
The Peltier-cooled thermoelectric conversion module is designed with thermoelectric conversion material chips thinner than 200 μm, suppressing electrical resistance to 30 mΩ or less for P-type and 20 mΩ or less for N-type chips, enhancing current flow and heat absorption.
This configuration results in a module with improved cooling performance and increased heat absorption, achieving higher thermal efficiency and reduced electrical resistance.
Smart Images

Figure 2024143431000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a Peltier-cooled thermoelectric conversion module. [Background technology]
[0002] 2. Description of the Related Art Conventionally, as one of the means for effectively utilizing energy, there has been a device that directly converts thermal energy into electrical energy and vice versa using a thermoelectric conversion module having a thermoelectric effect such as the Seebeck effect or the Peltier effect. As a thermoelectric conversion module, a configuration of a so-called π-type thermoelectric conversion element is known. The π-type thermoelectric conversion element is configured by providing a pair of electrodes spaced apart from each other on a substrate, for example, providing a P-type thermoelectric element on one electrode and an N-type thermoelectric element on the other electrode, also spaced apart from each other, and connecting the upper surfaces of both thermoelectric elements to a common electrode on the opposing substrate. Also, a configuration of a so-called IP (in-plane) type thermoelectric conversion element is known. From the viewpoint of thermoelectric performance, the IP type thermoelectric conversion element is usually configured by alternately providing P-type thermoelectric elements and N-type thermoelectric elements in the in-plane direction of the substrate, and for example, by connecting the lower parts of the junctions between adjacent P-type thermoelectric elements and N-type thermoelectric elements in series via electrodes. In this situation, various demands remain for thermoelectric conversion modules, such as improved thermoelectric performance, thinner modules, higher integration, and improved mass productivity, etc. In particular, in the case of π-type thermoelectric conversion modules, there is a demand for further improvement in cooling performance from the viewpoint of thinner modules. Patent Document 1 discloses a π-type thermoelectric conversion module with improved thermoelectric performance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2021-150403 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, although Patent Document 1 improves the thermoelectric performance from the viewpoint of improving the ability to conform to heat source surfaces including curved shapes, there is no description or suggestion of further improving the cooling performance of the π-type thermoelectric conversion module itself.
[0005] In view of the above, an object of the present invention is to provide a Peltier-cooled thermoelectric conversion module having excellent cooling performance and in which the electrical resistance value of the thermoelectric conversion material chip is suppressed. [Means for solving the problem]
[0006] As a result of extensive research aimed at solving the above problems, the inventors discovered that the total heat absorption amount of a Peltier-cooled thermoelectric conversion module can be increased by setting the film thickness of the thermoelectric conversion material chip within a specific range, suppressing the electrical resistance value low, and increasing the value of the current flowing through the thermoelectric conversion material chip, and thus completed the present invention. That is, the present invention provides the following [1] to [4]. [1] A Peltier-cooled thermoelectric conversion module in which the thickness of the thermoelectric conversion material chip is less than 200 μm. [2] The Peltier-cooled thermoelectric conversion module according to [1] above, wherein the chips of thermoelectric conversion material include chips of P-type thermoelectric conversion material and chips of N-type thermoelectric conversion material. [3] The Peltier-cooled thermoelectric conversion module according to [2] above, wherein the electrical resistance value per chip of the P-type thermoelectric conversion material is 30 mΩ or less, and the electrical resistance value per chip of the N-type thermoelectric conversion material is 20 mΩ or less. [4] The Peltier cooling thermoelectric conversion module according to the above [1], wherein the Peltier cooling thermoelectric conversion module has a total thickness of 300 to 1000 μm. Effect of the Invention
[0007] According to the present invention, it is possible to provide a Peltier-cooled thermoelectric conversion module having excellent cooling performance and in which the electrical resistance value of the thermoelectric conversion material chip is suppressed. [Brief description of the drawings]
[0008] [Figure 1] 1 is a cross-sectional view showing an example of the configuration of a Peltier cooling thermoelectric conversion module of the present invention. [Diagram 2] FIG. 2 is a cross-sectional configuration diagram showing an example of a unit for evaluating the cooling characteristics of the Peltier cooling thermoelectric conversion module of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Peltier-cooled thermoelectric conversion module] The Peltier cooling thermoelectric conversion module of the present invention is characterized in that the thickness of the chip of the thermoelectric conversion material is less than 200 μm. By setting the film thickness of the thermoelectric conversion material chip used in the present invention to less than 200 μm, thereby suppressing the electrical resistance value low, and increasing the value of the current flowing through the thermoelectric conversion material chip, the amount of heat generated in the electrodes, solder material layers, etc. that constitute the thermoelectric conversion module increases, but the increase in the amount of heat absorbed by the thermoelectric conversion material chip of the thermoelectric conversion module becomes significant, and as a result, the total amount of heat absorbed by the thermoelectric conversion module increases.
[0010] In this specification, a dried film made of a thermoelectric semiconductor composition may be simply referred to as a "coated film". A film obtained by subjecting a coated film to a hot press (heating and pressurizing) treatment may be simply referred to as a "thermoelectric conversion material layer precursor". A film obtained by subjecting a thermoelectric conversion material layer precursor to a heat treatment (the "firing (annealing) treatment" described below) may be simply referred to as a "thermoelectric conversion material layer". Furthermore, chips obtained by singulating a thermoelectric conversion material layer may be simply referred to as "chips of thermoelectric conversion material" or "chips". In addition, a "chip of P-type thermoelectric conversion material and a chip of N-type thermoelectric conversion material" may be simply referred to as a "chip of thermoelectric conversion material" or "chip".
[0011] In this specification, preferred definitions may be selected arbitrarily, and combinations of preferred definitions may be considered more preferred. In this specification, the expression "XX to YY" means "at least XX and at most YY." In this specification, the lower limit and upper limit described in stages for the preferred numerical range (e.g., the range of the content, etc.) can be independently combined. For example, the description "preferably 10 to 90, more preferably 30 to 60" can be combined with the "preferable lower limit (10)" and the "more preferable upper limit (60)" to form "10 to 60."
[0012] Hereinafter, the Peltier cooling thermoelectric conversion module of the present invention will be described with reference to the drawings.
[0013] 1 is a cross-sectional diagram showing an example of the configuration of a Peltier cooling thermoelectric conversion module of the present invention, in which a first electrode 3a on a first substrate 2a is joined to the lower surfaces of the chips 4 of P-type thermoelectric conversion material and the chips 5 of N-type thermoelectric conversion material via a solder material layer 6 and a solder receiving layer 7, and further, a second electrode 3b on a second substrate 2b is joined to the upper surfaces of the chips 4 of P-type thermoelectric conversion material and the chips 5 of N-type thermoelectric conversion material via the solder material layer 6 and the solder receiving layer 7. The chips 4 of P-type thermoelectric conversion material and the chips 5 of N-type thermoelectric conversion material are alternately adjacent to each other, electrically connected in series via the first electrode 3a or the second electrode 3b, and thermally connected in parallel via the first film substrate 2a and the second film substrate 2b.
[0014] The thickness of the thermoelectric conversion material chip is less than 200 μm. By having a thickness of less than 200 μm, the electrical resistance of the thermoelectric conversion material chip is kept low, which makes it easier for the current flowing through the thermoelectric conversion material chip to increase, leading to an increase in the amount of heat absorbed by the thermoelectric conversion module. On the other hand, when the thickness of the chip is reduced, various problems such as a decrease in the amount of heat absorbed due to a reduction in the temperature difference between the two substrates were of concern, but the inventors' various studies have made it clear that reducing the thickness of the chip is the most effective way to increase the amount of heat absorbed. The thickness of the thermoelectric conversion material chip is preferably 10 μm or more and less than 200 μm, more preferably 30 to 180 μm, further preferably 60 to 160 μm, and particularly preferably 80 to 120 μm. By making the thickness of the thermoelectric conversion material chip equal to or more than the lower limit, it is possible to suppress an increase in the amount of heat generated in the electrodes and solder material layers constituting the Peltier cooling thermoelectric conversion module, and to increase the amount of heat absorbed by the thermoelectric conversion module. On the other hand, when the thickness of the chip is reduced, various problems such as insufficient heat absorption due to insufficient thermal gradient between both substrates due to thermal convection, etc. are concerned. However, various studies by the present inventors have made it clear that reducing the thickness of the chip is the most effective way to increase the amount of heat absorbed.
[0015] From the viewpoint of thermoelectric performance, the chips of thermoelectric conversion material preferably include chips of P-type thermoelectric conversion material and chips of N-type thermoelectric conversion material.
[0016] The number of thermoelectric conversion material chips per unit area is preferably 20 to 300 (chips / cm 2 ), more preferably 30 to 150 (pieces / cm 2 ), and more preferably 40 to 100 (pieces / cm 2 ), and particularly preferably 50 to 90 (pieces / cm 2 ). When the number of chips of thermoelectric conversion material per unit area is within this range, the amount of heat absorption increases and the heat absorption surface becomes more uniform.
[0017] The electrical resistance value per chip of the P-type thermoelectric conversion material is preferably 30 (mΩ) or less. By having the electrical resistance value be 30 (mΩ) or less, the current value per unit area of the chip can be increased, and the amount of heat absorption can be easily increased to a desired range. The lower limit of the electrical resistance value is not particularly restricted, but is about 0.01 (mΩ) from the viewpoint of ease of manufacture. From this viewpoint, the electrical resistance value is preferably 0.01 to 30 (mΩ), more preferably 0.1 to 20 (mΩ), even more preferably 1.0 to 13 (mΩ), and particularly preferably 3 to 8 (mΩ). The electrical resistance value per chip of the N-type thermoelectric conversion material is preferably 20 (mΩ) or less. By having the electrical resistance value be 20 (mΩ) or less, the current value per unit area of the chip can be increased, and the amount of heat absorption can be easily increased to a desired range. The lower limit of the electrical resistance value is not particularly restricted, but is about 0.01 (mΩ) from the viewpoint of ease of manufacture. From this viewpoint, the electrical resistance value is preferably 0.01 to 20 (mΩ), more preferably 0.1 to 10 (mΩ), even more preferably 1.0 to 5 (mΩ), and particularly preferably 1.5 to 3 (mΩ).
[0018] The areas of the upper and lower surfaces of the thermoelectric conversion material chip are preferably 0.04 mm 2 ~0.90mm 2 , more preferably 0.06 mm 2 ~0.85mm 2 , and more preferably 0.09 mm 2 ~0.81mm 2 , particularly preferably 0.10 mm 2 ~0.60mm 2 It is. The ratio of the area of the upper surface to the area of the lower surface of the thermoelectric conversion material chip is preferably 0.80 to 1.20, more preferably 0.90 to 1.10, and even more preferably 0.99 to 1.01. When the areas of the top and bottom surfaces of the thermoelectric conversion material chip and the ratio of the area of the top surface to the area of the bottom surface of the thermoelectric conversion material chip are within this range, the electrical resistance is kept low, making it easier to increase the amount of heat absorption.
[0019] When the chip of the thermoelectric conversion material is rectangular, the length of one side is preferably 0.01 mm to 10 mm, more preferably 0.1 mm to 2 mm, and even more preferably 0.2 to 0.8 mm. By being in the above range, it is possible to manufacture a Peltier cooling thermoelectric conversion module with a high heat absorption capacity with good accuracy.
[0020] The distance between the chips of the thermoelectric conversion material is preferably 0.01 mm to 5 mm, more preferably 0.04 mm to 1 mm, and even more preferably 0.08 mm to 0.20 mm. By having the distance between the chips of the thermoelectric conversion material within the above range, it is possible to manufacture a Peltier cooling thermoelectric conversion module with high heat absorption capacity with good precision.
[0021] The current value that provides the maximum amount of heat absorption in the chip of the thermoelectric conversion material of the thermoelectric conversion module of the present invention (sometimes referred to as the "maximum current value") is preferably 1.0 (A) to 20.0 (A), more preferably 3.0 (A) to 10.0 (A), and even more preferably 3.0 (A) to 8.0 (A). If the maximum current value is within this range, the maximum amount of heat absorption can be easily increased.
[0022] [Amount of heat absorbed] By using a thermoelectric conversion material chip having a thickness of less than 200 μm, the electrical resistance of the thermoelectric conversion material chip is suppressed, and the current value flowing through the thermoelectric conversion material chip increases within the above-mentioned range of electrical resistance of the thermoelectric conversion material chip. This results in a significant increase in the amount of heat absorbed by the thermoelectric conversion material chip of the Peltier cooling thermoelectric conversion module, and as a result, the total amount of heat absorbed by the Peltier cooling thermoelectric conversion module increases. In other words, the electrical resistance per chip decreases due to the reduction in the thickness of the thermoelectric conversion material chip constituting the Peltier cooling thermoelectric conversion module, and therefore the electrical resistance of the Peltier cooling thermoelectric conversion module also decreases. Therefore, when the electrical resistance of the Peltier cooling thermoelectric conversion module is the same, it is possible to increase the number of pairs of chips, and the amount of heat absorbed increases. The endothermic amount can usually be calculated from the following formula (1). Qc=nST c I-1 / 2RI 2 -KΔT (1) Qc: Endothermic amount (W) n: logarithm of thermoelectric elements, S: Seebeck coefficient (V / K) T c : Temperature of the cooling surface of the Peltier-cooled thermoelectric conversion module (K), I: Current value of the Peltier-cooled thermoelectric conversion module (A) R: Electrical resistance of the Peltier cooling thermoelectric conversion module (Ω), K: Thermal conductance (reciprocal of thermal resistance) of the thermoelectric conversion material chip (W / K) ΔT: Temperature difference (K) The maximum heat absorption Q CMAX (W) can be calculated by setting the current value (A) of the Peltier cooling thermoelectric conversion module to the maximum current value (A) and setting ΔT to 0 in the above formula (1).
[0023] The Seebeck coefficient of the P-type thermoelectric conversion material chip is preferably 10×10 -6 (V / K)~1000×10 -6 (V / K). The Seebeck coefficient of the N-type thermoelectric conversion material chip is preferably -10×10 -6 (V / K)~-1000×10 -6 (V / K). When the Seebeck coefficient of the chip of P-type thermoelectric conversion material and the Seebeck coefficient of the chip of N-type thermoelectric conversion material are within this range, it becomes easier to maintain a high amount of heat absorption.
[0024] <Thermoelectric conversion material chip> The chip of the thermoelectric conversion material used in the present invention is preferably formed by dividing a thermoelectric conversion material layer made of a thermoelectric semiconductor composition containing a thermoelectric semiconductor material (hereinafter sometimes referred to as "thermoelectric semiconductor particles"), a binder resin, and an ionic compound (ionic liquid, inorganic ionic compound).
[0025] (Thermoelectric semiconductor materials) The thermoelectric semiconductor material is preferably pulverized to a predetermined size using, for example, a fine grinding device, and then used as thermoelectric semiconductor particles. The particle size of the thermoelectric semiconductor particles is preferably 10 nm to 100 μm, more preferably 50 nm to 50 μm, and further preferably 1 μm to 30 μm. The average particle size of the thermoelectric semiconductor particles was obtained by measurement using a laser diffraction particle size analyzer (Malvern, Mastersizer 3000) and was taken as the median value of the particle size distribution.
[0026] The thermoelectric semiconductor material used in the present invention is not particularly limited. For example, bismuth-tellurium-based thermoelectric semiconductor materials such as P-type bismuth telluride and N-type bismuth telluride; telluride-based thermoelectric semiconductor materials such as GeTe and PbTe; antimony-tellurium-based thermoelectric semiconductor materials; zinc-antimony-based thermoelectric semiconductor materials such as ZnSb and Zn3Sb 2、 Zn4Sb3; silicon-germanium-based thermoelectric semiconductor materials such as SiGe; bismuth selenide-based thermoelectric semiconductor materials such as Bi2Se3; silicide-based thermoelectric semiconductor materials such as β-FeSi2, CrSi2, and MnSi 1.73 , Mg2Si; oxide-based thermoelectric semiconductor materials; Heusler materials such as FeVAl, FeVAlSi, and FeVTiAl; sulfide-based thermoelectric semiconductor materials such as TiS2, etc. are used.
[0027] Among these, the thermoelectric semiconductor material used in the present invention is preferably a bismuth-tellurium-based thermoelectric semiconductor material such as P-type bismuth telluride or N-type bismuth telluride. In the P-type bismuth telluride, the carrier is a hole and the Seebeck coefficient is a positive value. For example, Bi X Te3Sb 2-X represented by is preferably used. In this case, X is preferably 0 < X ≦ 0.8, more preferably 0.4 ≦ X ≦ 0.6. When X is greater than 0 and less than or equal to 0.8, the Seebeck coefficient and electrical conductivity increase, and the characteristics as a P-type thermoelectric conversion material are maintained, which is preferable. In addition, in the N-type bismuth telluride, the carrier is an electron and the Seebeck coefficient is a negative value. For example, Bi2Te 3-Y Se Y represented by is preferably used. In this case, Y is preferably 0 ≦ Y ≦ 3 (when Y = 0: Bi2Te3), more preferably 0.1 < Y ≦ 2.7. When Y is 0 or more and 3 or less, the Seebeck coefficient and electrical conductivity increase, and the characteristics as an N-type thermoelectric conversion material are maintained, which is preferable.
[0028] The content of the thermoelectric semiconductor particles in the thermoelectric semiconductor composition is preferably 30 to 99% by mass. More preferably, it is 50 to 96% by mass, and further preferably, it is 70 to 95% by mass. If the content of the thermoelectric semiconductor particles is within the above range, the Seebeck coefficient (absolute value of the Peltier coefficient) is large, and the decrease in electrical conductivity is suppressed, and only the thermal conductivity decreases, so that a film exhibiting high thermoelectric performance and having sufficient film strength and flexibility is preferably obtained. Note that, in calculating the content in the thermoelectric semiconductor composition, the value is calculated assuming that the solvent is not included (hereinafter, the same applies).
[0029] The thermoelectric semiconductor particles are preferably annealed. By performing annealing, the crystallinity of the thermoelectric semiconductor particles is improved and the surface oxide film of the thermoelectric semiconductor particles is removed, so that the Seebeck coefficient (absolute value of the Peltier coefficient) of the thermoelectric conversion material is increased, and the thermoelectric figure of merit can be further improved.
[0030] (binder resin) The binder resin used in the present invention has the effect of physically binding the thermoelectric semiconductor material (thermoelectric semiconductor particles) together, and can increase the flexibility of the thermoelectric conversion module while facilitating the formation of a thin film by coating or the like.
[0031] The binder resin is appropriately selected depending on the temperature of the heat treatment of the thermoelectric semiconductor material and the baking (annealing) temperature. It is preferable to heat the material at a temperature higher than the decomposition temperature of the binder resin. Furthermore, it is more preferable to use a resin that maintains various physical properties such as mechanical strength and thermal conductivity without being impaired when the coating film made of the thermoelectric semiconductor composition is subjected to a heat treatment or the like to cause crystal growth of the thermoelectric semiconductor particles. In this specification, the term "decomposition temperature" refers to the temperature at which the mass reduction rate by thermogravimetry (TG) is 100% (the mass after decomposition is less than 1% of the mass before decomposition). The decomposition temperature of the binder resin is preferably 150 to 400° C., and it is preferable that 90% by mass or more of the binder resin is decomposed and vaporized.
[0032] As such a binder resin, a thermoplastic resin or a curable resin can be used. Examples of the thermoplastic resin include polyolefin resins such as polyethylene, polypropylene, polyisobutylene, and polymethylpentene; polycarbonate; thermoplastic polyester resins such as polyethylene terephthalate and polyethylene naphthalate; polyvinyl polymers such as polystyrene, acrylonitrile-styrene copolymer, polyvinyl acetate, ethylene-vinyl acetate copolymer, vinyl chloride, polyvinylpyridine, polyvinyl alcohol, and polyvinylpyrrolidone; polyurethane; and cellulose derivatives such as ethyl cellulose. Examples of the curable resin include thermosetting resins and photocurable resins. Examples of the thermosetting resin include epoxy resins and phenolic resins. Examples of the photocurable resin include photocurable acrylic resins, photocurable urethane resins, and photocurable epoxy resins. These may be used alone or in combination of two or more. Among these, thermoplastic resins are preferred, polycarbonate and cellulose derivatives such as ethyl cellulose are more preferred, and polycarbonate is particularly preferred.
[0033] The content of the binder resin in the thermoelectric semiconductor composition is preferably 0.1 to 20 mass %, more preferably 0.5 to 15 mass %, and further preferably 1.0 to 10 mass %.
[0034] (ionic compounds) (Ionic Liquid) The ionic liquid that can be contained in the thermoelectric semiconductor composition is a molten salt formed by combining a cation and an anion, and refers to a salt that can exist in a liquid state in any temperature range of -50°C or more and less than 400°C. In other words, the ionic liquid is an ionic compound whose melting point is in the range of -50°C or more and less than 400°C. The melting point of the ionic liquid is preferably -25°C or more and 200°C or less, more preferably 0°C or more and 150°C or less. The ionic liquid has characteristics such as extremely low vapor pressure and non-volatility, excellent thermal stability and electrochemical stability, low viscosity, and high ionic conductivity, and therefore can effectively suppress the reduction in electrical conductivity between thermoelectric semiconductor materials as a conductive auxiliary. In addition, the ionic liquid exhibits high polarity based on an aprotic ionic structure and has excellent compatibility with binder resins, so that the electrical conductivity of the thermoelectric element layer can be made uniform.
[0035] The ionic liquid may be a known or commercially available one. For example, a mixture of a cationic component such as a pyridinium, pyrimidinium, pyrazolium, pyrrolidinium, piperidinium, imidazolium, etc., and a derivative thereof; a tetraalkylammonium-based amine-based cation and a derivative thereof; a phosphine-based cation such as a phosphonium, trialkylsulfonium, tetraalkylphosphonium, etc., and a derivative thereof; a lithium cation and a derivative thereof; and a mixture of a Cl cation and ... - , Br - , I - , AlCl4 - , Al2Cl7 - , BF4 - , PF6 - , ClO4 - , NO3 - , CH3COO - , CF3COO - , CH3SO3 - , CF3SO3 - , (FSO2)2N - , (CF3SO2)2N - , (CF3SO2)3C - , AsF6 - , SbF6 - , NbF6 - , TaF6- , F(HF) n - , (CN)2N - , C4F9SO3 - , (C2F5SO2)2N - , C3F7COO - , (CF3SO2)(CF3CO)N - and an anion component such as the above.
[0036] Of the above ionic liquids, from the viewpoints of high-temperature stability, compatibility with thermoelectric semiconductor materials and resins, suppression of a decrease in the electrical conductivity in the gaps between thermoelectric semiconductor materials, and the like, it is preferable that the cationic component of the ionic liquid contains at least one selected from pyridinium cations and derivatives thereof, and imidazolium cations and derivatives thereof.
[0037] As the ionic liquid in which the cationic component contains a pyridinium cation or a derivative thereof, 1-butyl-4-methylpyridinium bromide, 1-butylpyridinium bromide, N-octylpyridinium bromide, and 1-butyl-4-methylpyridinium hexafluorophosphate are preferred.
[0038] As the ionic liquid in which the cationic component contains an imidazolium cation or a derivative thereof, [1-butyl-3-(2-hydroxyethyl)imidazolium bromide] or [1-butyl-3-(2-hydroxyethyl)imidazolium tetrafluoroborate] is preferred.
[0039] The ionic liquid preferably has a decomposition temperature of 300° C. or higher. If the decomposition temperature is within the above range, the effect as a conductive auxiliary agent can be maintained even when a coating film made of the thermoelectric semiconductor composition is annealed, as described below.
[0040] The content of the ionic liquid in the thermoelectric semiconductor composition is preferably 0.01 to 50 mass%, more preferably 0.5 to 30 mass%, and further preferably 1.0 to 20 mass%. When the content of the ionic liquid is within the above range, the decrease in electrical conductivity is effectively suppressed, and a film having high thermoelectric performance is obtained.
[0041] (Inorganic ionic compounds) The inorganic ionic compound that can be contained in the thermoelectric semiconductor composition is a compound composed of at least a cation and an anion. The inorganic ionic compound exists in a solid state in a wide temperature range of 400 to 900°C and has characteristics such as high ionic conductivity, so that it can suppress the decrease in electrical conductivity between thermoelectric semiconductor materials as a conductive auxiliary.
[0042] The content of the inorganic ionic compound in the thermoelectric semiconductor composition is preferably 0.01 to 50 mass%, more preferably 0.5 to 30 mass%, and further preferably 1.0 to 10 mass%. If the content of the inorganic ionic compound is within the above range, the decrease in electrical conductivity can be effectively suppressed, and as a result, a film with improved thermoelectric performance can be obtained. In addition, when an inorganic ionic compound and an ionic liquid are used in combination as the ionic compound, the total content of the inorganic ionic compound and the ionic liquid in the thermoelectric semiconductor composition is preferably 0.01 to 50 mass%, more preferably 0.4 to 20 mass%, and even more preferably 0.8 to 10 mass%.
[0043] (Other additives) The thermoelectric semiconductor composition used in the present invention may further contain, as necessary, other additives other than those mentioned above, such as dispersants, film-forming assistants, light stabilizers, antioxidants, tackifiers, plasticizers, colorants, resin stabilizers, fillers, pigments, conductive fillers, conductive polymers, curing agents, etc. These additives may be used alone or in combination of two or more.
[0044] (Method for preparing thermoelectric semiconductor composition) The method for preparing the thermoelectric semiconductor composition is not particularly limited, and the thermoelectric semiconductor composition may be prepared by, for example, mixing and dispersing the thermoelectric semiconductor particles, the binder resin, and the ionic compound, as well as the other additives as necessary and a solvent, using a known method such as an ultrasonic homogenizer, a spiral mixer, a planetary mixer, a disperser, or a hybrid mixer. Examples of the solvent include toluene, ethyl acetate, methyl ethyl ketone, alcohol, tetrahydrofuran, methylpyrrolidone, ethyl cellosolve, and the like. These solvents may be used alone or in combination of two or more. The solid content concentration of the thermoelectric semiconductor composition is not particularly limited as long as the composition has a viscosity suitable for coating.
[0045] The coating film made of the thermoelectric semiconductor composition is not particularly limited, but can be formed, for example, by applying the thermoelectric semiconductor composition to a substrate such as at least glass, alumina, silicon, or resin to obtain a coating film, and drying the coating film. Methods for applying the thermoelectric semiconductor composition to obtain a coating film include known methods such as screen printing, flexographic printing, gravure printing, spin coating, dip coating, die coating, spray coating, bar coating, doctor blade, etc., and are not particularly limited. When forming a coating film in a pattern, a screen printing method, a slot die coating method, etc., which can easily form a pattern using a screen plate having a desired pattern, are preferably used. The coating film is then dried to form a coating film, and the drying method may be a conventionally known drying method such as hot air drying, hot roll drying, infrared irradiation, etc. The heating temperature is usually 80 to 150° C., and the heating time varies depending on the heating method, but is usually several seconds to several tens of minutes. When a solvent is used in the preparation of the thermoelectric semiconductor composition, the heating temperature is not particularly limited as long as it is within a temperature range in which the solvent used can be dried. Furthermore, the dried coating film may be subjected to a hot press (heating and pressing) treatment to form a thermoelectric conversion material layer precursor for the purpose of suppressing voids in the chip of the thermoelectric conversion material, improving electrical conductivity, etc. The hot press (heating and pressing) treatment can be performed, for example, by using a device such as a hydraulic press to apply pressure to the entire upper surface of the coating film at a predetermined temperature and in an atmospheric atmosphere at a predetermined pressure for a predetermined time. The temperature for the hot press (heating and pressing) treatment is not particularly limited, but is usually 100 to 300°C, and preferably 200 to 300°C. The pressure for the hot pressing (heating and pressing) treatment is not particularly limited, but is usually 20 to 200 MPa, and preferably 50 to 150 MPa. The time for the hot press (heating and pressing) treatment is not particularly limited, but is usually from several seconds to several tens of minutes, preferably from several tens of seconds to several tens of minutes.
[0046] The obtained thermoelectric conversion material layer precursor is preferably subjected to a firing (annealing) treatment for the purposes of stabilizing the thermoelectric performance and causing crystal growth of the thermoelectric semiconductor particles in the thermoelectric semiconductor composition to form a thermoelectric conversion material layer. The firing (annealing) treatment is not particularly limited, but is usually carried out under an inert gas atmosphere such as nitrogen or argon, under a reducing gas atmosphere, or under vacuum conditions with the gas flow rate controlled. The temperature of the firing (annealing) treatment depends on the thermoelectric semiconductor particles, binder resin, ionic liquid, inorganic ionic compound, etc. used in the thermoelectric semiconductor composition and is appropriately adjusted, but is usually 260 to 600°C, preferably 280 to 550°C. The time for the firing (annealing) treatment is not particularly limited, but is usually from several minutes to several tens of hours, and preferably from several minutes to several hours.
[0047] The thermoelectric conversion material chips used in the present invention can be obtained by dicing the thermoelectric conversion material layer. There are no particular limitations on the method for dicing, but from the viewpoints of processing accuracy and process stability, it is preferable to use a dicing blade.
[0048] <Substrate> As the substrates of the thermoelectric conversion module of the present invention, for example, the first substrate 2a and the second substrate 2b are preferably made of plastic films that do not affect the decrease in electrical conductivity or the increase in thermal conductivity of the thermoelectric conversion material chip. Even when the thermoelectric conversion material layer is annealed, the substrate does not thermally deform, and the performance of the thermoelectric conversion module can be maintained. In view of high heat resistance and dimensional stability, the plastic films are preferably polyimide films, polyamide films, polyetherimide films, polyaramid films, polyamideimide films, and glass-epoxy sheets.
[0049] The thickness of the plastic film used for the substrate is preferably from 1 to 1000 μm, more preferably from 10 to 500 μm, and even more preferably from 20 to 100 μm, from the viewpoints of flexibility, heat resistance, and dimensional stability. The plastic film preferably has a 5% weight loss temperature of 300°C or higher, more preferably 400°C or higher, as measured by thermogravimetric analysis. The thermal dimensional change rate measured at 200°C in accordance with JIS K7133 (1999) is preferably 0.5% or lower, more preferably 0.3% or lower. The linear expansion coefficient in the planar direction measured in accordance with JIS K7197 (2012) is 0.1 ppm·°C or higher. -1 ~50ppm·℃ -1 and 0.1 ppm·℃ -1 ~30ppm·℃ -1 It is more preferable that:
[0050] <Electrode> There are no particular limitations on the metal material used as the electrodes of the thermoelectric conversion module of the present invention. For example, the metal material of the first electrode 3a and the second electrode 3b may be gold, nickel, aluminum, rhodium, platinum, chromium, palladium, stainless steel, molybdenum, or an alloy containing any of these metals. In addition to the metal material, a paste material containing a solvent or a resin component may be used. When using a paste material, it is preferable to remove the solvent or the resin component by firing, etc. As the paste material, silver paste and aluminum paste are preferable. The thickness of the electrode layer is preferably 10 nm to 200 μm, more preferably 30 nm to 150 μm, and further preferably 50 nm to 120 μm. When the thickness of the electrode layer is within the above range, the electrical conductivity is high and the resistance is low, and sufficient strength as an electrode is obtained.
[0051] Examples of methods for forming the electrodes include a method of processing into a predetermined pattern shape by known physical or chemical treatments mainly based on photolithography, or a combination of these, and a method of forming an electrode pattern by screen printing, stencil printing, inkjet printing, or the like. Methods for forming electrodes without a pattern include vacuum deposition methods such as PVD (physical vapor deposition) methods such as vacuum deposition, sputtering, and ion plating, or CVD (chemical vapor deposition) methods such as thermal CVD and atomic layer deposition (ALD), or various coating methods such as dip coating, spin coating, spray coating, gravure coating, die coating, and doctor blade methods, wet processes such as electrodeposition, silver halide methods, electrolytic plating, electroless plating, and lamination of metal foils, and are appropriately selected depending on the metal material. The electrodes used in the present invention are required to have high conductivity, and since electrodes formed by plating or vacuum film formation can easily achieve high conductivity, vacuum film formation methods such as vacuum deposition and sputtering, electrolytic plating, and electroless plating are preferred. Depending on the size and dimensional accuracy of the pattern to be formed, a pattern can also be easily formed through a hard mask such as a metal mask. In addition, when forming a film by the vacuum film formation method, the substrate to be used may be heated to a degree that does not impair the characteristics of the substrate in order to improve adhesion to the substrate to be used and remove moisture. When forming a film by the plating method, a film may be formed by electrolytic plating on a film formed by electroless plating.
[0052] <Solder material layer> The solder material layer is used to join the chip of thermoelectric conversion material and the electrodes. The solder material constituting the solder material layer may be appropriately selected taking into consideration the heat resistance temperature of the binder resin contained in the substrate and the thermoelectric conversion material chip, as well as the electrical conductivity and thermal conductivity, and examples of known materials include Sn, Sn / Pb alloy, Sn / Ag alloy, Sn / Cu alloy, Sn / Sb alloy, Sn / In alloy, Sn / Zn alloy, Sn / In / Bi alloy, Sn / In / Bi / Zn alloy, Sn / Bi / Pb / Cd alloy, Sn / Bi / Pb alloy, Sn / Bi / Cd alloy, Bi / Pb alloy, Sn / Bi / Zn alloy, Sn / Bi alloy, Sn / Bi / Pb alloy, Sn / Pb / Cd alloy, and Sn / Cd alloy. From the viewpoints of lead-free and / or cadmium-free, melting point, electrical conductivity, and thermal conductivity, alloys such as 43Sn / 57Bi alloy, 42Sn / 58Bi alloy, 40Sn / 56Bi / 4Zn alloy, 48Sn / 52In alloy, and 39.8Sn / 52In / 7Bi / 1.2Zn alloy are preferred. Commercially available solder materials include the following: 42Sn / 58Bi alloy (manufactured by Tamura Manufacturing Co., Ltd., product name: SAM10-401-27), 41Sn / 58Bi / Ag alloy (manufactured by Nihon Handa Co., Ltd., product name: PF141-LT7HO), 96.5Sn3Ag0.5Cu alloy (manufactured by Nihon Handa Co., Ltd., product name: PF305-207BTO), etc.
[0053] The thickness of the solder material layer (after heating and cooling) is preferably 10 to 200 μm, more preferably 20 to 150 μm, further preferably 30 to 130 μm, and particularly preferably 40 to 120 μm. When the thickness of the solder material layer is within this range, adhesion between the thermoelectric conversion material chip and the electrodes can be easily obtained.
[0054] Methods for applying solder material to a board include stencil printing, screen printing, and die printing. The heating temperature varies depending on the solder material, resin film, etc., used, but is usually performed at 150 to 280° C. for 3 to 20 minutes.
[0055] <Solder acceptance layer> The solder-receiving layer has the function of improving the bonding strength between the chip of thermoelectric conversion material containing resin and the solder material layer on the opposing electrode side that constitutes the thermoelectric conversion module, and is directly bonded to the chip of thermoelectric conversion material.
[0056] The solder-receiving layer preferably contains a metal material. The metal material is preferably at least one selected from gold, silver, nickel, aluminum, rhodium, platinum, chromium, palladium, tin, and an alloy containing any of these metal materials. Among these, a two-layer structure of gold, silver, nickel, aluminum, or tin and gold is preferable, and from the viewpoints of material cost, high thermal conductivity, and bonding stability, silver, nickel, and aluminum are more preferable.
[0057] The thickness of the solder-receiving layer is preferably 10 nm to 50 μm, more preferably 50 nm to 16 μm, further preferably 200 nm to 4 μm, and particularly preferably 500 nm to 3 μm. When the thickness of the solder-receiving layer is within this range, the adhesion to the surface of the thermoelectric conversion material chip and the adhesion to the surface of the solder material layer on the electrode side constituting the thermoelectric conversion module are excellent, and a highly reliable bond can be obtained. In addition, high thermal conductivity as well as electrical conductivity can be maintained, and as a result, the thermoelectric performance of the thermoelectric conversion module is maintained without deterioration. The solder-receiving layer may be a single layer formed by directly depositing a metal material, or may be a multilayer formed by laminating two or more metal materials.
[0058] The solder-receiving layer is preferably formed using the above-mentioned metal material. Since the solder-receiving layer is required to have high electrical conductivity and high thermal conductivity in order to maintain thermoelectric performance, it is preferable to use a solder-receiving layer formed by electrolytic plating, electroless plating, or vacuum film formation.
[0059] <Heat dissipation layer> In the Peltier cooling thermoelectric conversion module of the present invention, from the viewpoint of thermoelectric performance, it is preferable to further provide a heat dissipation layer on at least one surface of the substrate. The material used for the heat dissipation layer is not particularly limited, and any known material can be used, but is preferably selected from gold, silver, copper, nickel, tin, iron, chromium, platinum, palladium, rhodium, iridium, ruthenium, osmium, indium, zinc, molybdenum, manganese, titanium, aluminum, stainless steel, and brass.
[0060] The method for laminating the heat dissipation layer is not particularly limited, and examples thereof include dry processes such as PVD (physical vapor deposition) methods such as vacuum deposition, sputtering, and ion plating, or CVD (chemical vapor deposition) methods such as thermal CVD and atomic layer deposition (ALD), or various coating methods such as dip coating, spin coating, spray coating, gravure coating, die coating, and doctor blade methods, wet processes such as electrodeposition, silver halide methods, electrolytic plating, and electroless plating. The heat dissipation layer can be patterned by known physical or chemical treatments, mainly photolithography, or a combination of these. The thermal conductivity of each of the heat dissipation layers is independently preferably 5 to 500 W / (m·K), more preferably 8 to 500 W / (m·K), even more preferably 10 to 450 W / (m·K), particularly preferably 12 to 420 W / (m·K), and most preferably 15 to 400 W / (m·K).
[0061] The thickness of the heat dissipation layer is appropriately determined from the viewpoint of thermoelectric performance, but is preferably 1 to 550 μm, more preferably 10 to 400 μm, and further preferably 30 to 200 μm.
[0062] The total thickness of the Peltier cooling thermoelectric conversion module is preferably 300 to 1000 μm, more preferably 340 to 600 μm, and further preferably 360 to 480 μm. When the total thickness of the Peltier-cooled thermoelectric conversion module is within this range, the module resistance value of the thermoelectric conversion module is easily suppressed, and therefore a thin Peltier-cooled thermoelectric conversion module with high cooling performance can be obtained.
[0063] The Peltier cooling thermoelectric conversion module of the present invention includes a chip of a thermoelectric conversion material with a reduced electrical resistance value, and has an excellent heat absorption capacity. EXAMPLES
[0064] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.
[0065] The electrical resistance values of the chips of the thermoelectric conversion materials produced in the examples and comparative examples, and the cooling characteristics of the Peltier-cooled thermoelectric conversion modules were evaluated by the following methods.
[0066] (a) Electrical resistance evaluation of thermoelectric conversion material chips The electrical resistance values (mΩ) of the chips of the thermoelectric conversion materials obtained in the examples and comparative examples were measured in an environment of 25° C.×50% RH by the four-terminal method using a low resistance meter (RM3545, manufactured by Hioki E.E. Corporation).
[0067] (b) Evaluation of the cooling characteristics of a Peltier-cooled thermoelectric conversion module The thermoelectric conversion modules obtained in the examples and comparative examples were placed at predetermined positions in a cooling characteristic evaluation unit 11 shown in FIG. 2, and a cooling characteristic evaluation was performed. Temperature controllers 14a and 14b (manufactured by Advance Riko Co., Ltd., model name: Peltier evaluation device) were placed on the upper and lower surfaces of the thermoelectric conversion module 12 via temperature measuring plates 13a and 13b into which a K thermocouple was inserted, and the surroundings were insulated by drawing a vacuum. Next, the temperature of the upper and lower surfaces of the thermoelectric conversion module 12 was adjusted to 85°C by the temperature controllers 14a and 14b, and then a current was passed through the thermoelectric conversion module 12 to measure the temperature difference between the upper and lower surfaces of the thermoelectric conversion module 12. The amount of heat absorbed on the heat absorption side at this time was Qc, the maximum value of the amount of heat absorbed when the temperatures of the heat generation side and the heat absorption side were equal (ΔT=0) was the maximum amount of heat absorption Qcmax (W), and the current value giving Qcmax was the maximum current value (A). Note that when electricity was passed through the thermoelectric conversion module 12, the temperature was controlled by the temperature controller so that the temperature of the heat generation side did not exceed 85°C. Qcmax was calculated from the maximum current value, the thermal resistance value and the electrical resistance value of the thermoelectric conversion module described below, according to the above-mentioned formula (1). Also, the amount of heat absorbed per effective area (W / cm 2 ) was calculated by dividing Qcmax by the effective area of the thermoelectric conversion material chip. The effective area of the thermoelectric conversion material chip was calculated by multiplying the area per chip of the thermoelectric conversion material by its logarithm and 2 (an integer).
[0068] (c) Thermal resistance evaluation of Peltier-cooled thermoelectric conversion module The thermal resistance Re of the chip of the thermoelectric conversion material was found from the following formula (2), and the thermal resistance value of the Peltier cooling thermoelectric conversion module was calculated by multiplying it by the number of chips. Re(K / W)=L(m) / [A(m 2 )×k(W / (m K))] (2) Re(K / W): Thermal resistance (one chip of thermoelectric conversion material) L(m): Film thickness of the thermoelectric conversion material chip A(m 2 ): Area of the top and bottom surfaces of the thermoelectric conversion material chip k (W / (m K)): Thermal conductivity of the thermoelectric conversion material chip The thermal conductivity of the P-type thermoelectric conversion material chip was set to 1.2 (W / (m K)), and the thermal conductivity of the N-type thermoelectric conversion material chip was set to 1.0 (W / (m K)).
[0069] (d) Evaluation of electrical resistance of Peltier-cooled thermoelectric conversion module The electrical resistance value between the output electrodes of the Peltier cooling thermoelectric conversion module was measured in an environment of 25° C.×50% RH using a low resistance measuring device (manufactured by HIOKI EE Corporation, model number: RM3545).
[0070] Example 1 <Fabrication of Peltier-cooled thermoelectric conversion module> (1) Preparation of thermoelectric semiconductor particles As a P-type thermoelectric semiconductor particle, P-type bismuth telluride Bi, a bismuth-tellurium-based thermoelectric semiconductor material, was used. 0.4 Te3Sb1.6 (manufactured by Kojundo Chemical Laboratory, average particle size: 16 μm) was used. As the N-type thermoelectric semiconductor particles, N-type bismuth telluride Bi2Te3 (manufactured by Kojundo Chemical Laboratory, particle size: 90 μm), a bismuth-tellurium based thermoelectric semiconductor material, was used, and was pulverized in a nitrogen gas atmosphere using a planetary ball mill (Fritsch Japan, Premium line P-7) to prepare thermoelectric semiconductor particles with an average particle size of 2.8 μm. The particle size distribution of each of the thermoelectric semiconductor particles used was measured using a laser diffraction particle size analyzer (Malvern, Mastersizer 3000).
[0071] (2) Preparation of coating solution of thermoelectric semiconductor composition Coating liquid (P) The P-type bismuth telluride Bi 0.4 Te3Sb 1.6 A coating liquid (P) was prepared, which was a thermoelectric semiconductor composition obtained by mixing and dispersing 78.5 parts by mass of particles, 5.2 parts by mass of polyethylene carbonate as a binder resin, 0.8 parts by mass of N-octylpyridinium bromide as an ionic liquid, and 15.5 parts by mass of N-methylpyrrolidone as a solvent. Coating fluid (N) A coating liquid (N) was prepared by mixing and dispersing 78.8 parts by mass of the obtained N-type bismuth telluride Bi2Te3 particles, 4.25 parts by mass of polyethylene carbonate as a binder resin, 4.2 parts by mass of N-octylpyridinium bromide as an ionic liquid, and 12.75 parts by mass of N-methylpyrrolidone as a solvent.
[0072] (3) Fabrication of thermoelectric conversion material chips The coating solution (P) prepared in (2) was applied onto a polyimide film (manufactured by Ube Industries, product name "Kapton 500H", 100 mm x 160 mm x thickness 125 μm) using a screen printer (manufactured by Newlong, model name: LS-34TVA), and the film was dried by heating at 110°C for 20 minutes to form a coating film having a thickness of 300 μm. Next, the coating film was subjected to a heat press at 250°C and 50 MPa for 10 minutes to obtain a P-type thermoelectric conversion material layer precursor having a thickness of 150 μm. The obtained P-type thermoelectric conversion material layer precursor was subjected to a baking (annealing) treatment at 430° C. for 30 minutes in an argon-hydrogen mixed gas atmosphere to obtain a P-type thermoelectric conversion material layer. Next, a solder-receiving layer [Ni (thickness: 4 μm) laminated with Au (thickness: 30 nm)] was formed on the entire surface of the P-type thermoelectric conversion material layer by electroless plating, and then the P-type thermoelectric conversion material layer was diced into chips using a dicing device (manufactured by DISCO, model name: DFD6362) to produce P-type thermoelectric conversion material chips measuring 0.9 mm x 0.9 mm. Similarly, the coating solution (N) prepared in (2) was applied onto a polyimide film (manufactured by Ube Industries, product name "Kapton 500H", 100 mm x 160 mm x thickness 125 μm) using a screen printer (manufactured by Newlong, product name: LS-34TVA), and the film was dried by heating at 110 ° C for 20 minutes to form a coating film having a thickness of 270 μm. Next, the coating film was subjected to a heat press at 250 ° C and 30 MPa for 20 minutes to obtain an N-type thermoelectric conversion material layer precursor having a thickness of 150 μm. The obtained N-type thermoelectric conversion material layer precursor was subjected to a baking (annealing) treatment at 370° C. for 30 minutes in an argon-hydrogen mixed gas atmosphere to obtain an N-type thermoelectric conversion material layer. Next, a solder-receiving layer [Ni (thickness: 4 μm) laminated with Au (thickness: 30 nm)] was formed on the entire surface of the N-type thermoelectric conversion material layer by electroless plating, and then the N-type thermoelectric conversion material layer was diced into chips using a dicing device (manufactured by DISCO, model name: DFD6362) to produce N-type thermoelectric conversion material chips measuring 0.9 mm x 0.9 mm.
[0073] (4) Preparation of electrode substrate First, a substrate was prepared by attaching copper foil of 35 μm thickness to both sides of a 60 μm thick glass-epoxy sheet. A nickel layer (thickness: 3 μm) and a gold layer (thickness: 40 nm) were laminated in this order on the copper foil of the substrate by electroless plating, and then an electrode pattern (0.9 × 0.9 mm, 126 pieces, distance between adjacent electrodes: 0.1 mm, 6 columns, 21 rows) was formed only on one side to produce a substrate with an electrode on one side and a heat sink on the other side (first substrate with first electrode, hereinafter sometimes referred to as "first electrode substrate"). Similarly, a substrate with electrodes arranged in a pattern was produced so that a π-type thermoelectric conversion module would be obtained when it was bonded to the first electrode substrate (a second substrate having a second electrode, hereinafter sometimes referred to as the "second electrode substrate"). Note that the materials of the substrate and electrodes, and the dimensions including the thickness, were the same as those of the first electrode substrate.
[0074] (Fabrication of a π-type Peltier-cooled thermoelectric conversion module) Using the P-type thermoelectric material chips with solder acceptance layers only on the top and bottom surfaces and the N-type thermoelectric material chips produced in (3), a π-type Peltier-cooled thermoelectric conversion module consisting of 63 pairs of P-type and N-type thermoelectric material chips was produced as follows.
[0075] A solder material layer with a thickness of 50 μm was formed on the first electrode substrate prepared in (4) by stencil printing using solder paste (manufactured by Kokisha, product name: T4AB58-M742) as the solder material. Next, one side of the solder acceptance layer of each of the P-type and N-type thermoelectric conversion material chips prepared in (3) was placed on the solder material layer, heated at 190°C for 1 minute, and then cooled, thereby placing the P-type and N-type thermoelectric conversion material chips on the first electrode substrate, respectively. Furthermore, a solder material layer with a thickness of 50 μm was formed on the other side of the solder acceptance layer of each of the P-type and N-type thermoelectric conversion material chips using the solder paste in the same manner as described above, and the second electrode substrate prepared in (4) was attached to the layer. Heating was performed at 190° C. for 2 minutes to produce a π-type Peltier-cooled thermoelectric conversion module consisting of 63 pairs each of P-type and N-type thermoelectric conversion material chips.
[0076] Example 2 A π-type Peltier-cooled thermoelectric conversion module was produced in the same manner as in Example 1, except that in Example 1, the P-type and N-type thermoelectric conversion material layers were each diced into individual pieces of 0.64 mm × 0.64 mm, and these were used as P-type and N-type thermoelectric conversion material chips.
[0077] Example 3 A π-type Peltier-cooled thermoelectric conversion module was produced in the same manner as in Example 1, except that in Example 1, the thickness of the coating film formed from the coating liquid (P) was 200 μm, the thickness of the coating film formed from the coating liquid (N) was 190 μm, and the thicknesses of the P-type and N-type thermoelectric conversion material layer precursors formed by hot pressing were each 100 μm.
[0078] Comparative Example 1 A π-type Peltier-cooled thermoelectric conversion module was produced in the same manner as in Example 1, except that in Example 1, the thickness of the coating film formed from the coating liquid (P) was set to 600 μm, and hot pressing was performed to set the thickness of the P-type thermoelectric conversion material layer precursor to 285 μm, and the thickness of the coating film formed from the coating liquid (N) was set to 540 μm, and hot pressing was performed to set the thickness of the N-type thermoelectric conversion material layer precursor to 285 μm.
[0079] Comparative Example 2 A π-type Peltier-cooled thermoelectric conversion module was produced in the same manner as in Example 1, except that in Example 1, the thickness of the coating film formed from the coating liquid (P) was set to 1200 μm, heat pressing was performed to set the thickness of the P-type thermoelectric conversion material layer precursor to 600 μm, and the thickness of the coating film formed from the coating liquid (N) was set to 1140 μm, heat pressing was performed to set the thickness of the N-type thermoelectric conversion material layer precursor to 600 μm.
[0080] The electrical resistance values of the chips of the thermoelectric conversion materials obtained in Examples 1 to 3 and Comparative Examples 1 and 2, and the evaluation results of the thermal resistance value, electrical resistance value, maximum current value, maximum heat absorption amount, and heat absorption amount per effective area of the Peltier cooling thermoelectric conversion modules are shown in Table 1.
[0081] [Table 1]
[0082] According to Table 1, it can be seen that the heat absorption amount per effective area of the Peltier-cooled thermoelectric conversion modules of Examples 1 to 3, in which the range of film thickness of the thermoelectric conversion material chip satisfies the provisions of the present invention, is significantly larger than the heat absorption amount per effective area of the Peltier-cooled thermoelectric conversion modules of Comparative Examples 1 and 2, which do not satisfy the provisions of the range of film thickness of the thermoelectric conversion material chip of the present invention. [Industrial Applicability]
[0083] The Peltier cooling thermoelectric conversion module of the present invention has a large amount of heat absorption per effective area of the thermoelectric conversion module, and therefore can be used, for example, in cooling applications in the field of electronic devices, such as CPUs (Central Processing Units) used in smartphones and various computers, image sensors such as CMOS (Complementary Metal Oxide Semiconductors) and CCD (Charge Coupled Devices), and further, for temperature control of various sensors such as MEMS (Micro Electro Mechanical Systems) and light receiving elements. [Explanation of symbols]
[0084] 1: Thermoelectric conversion module 2a: 1st board 2b: 2nd board 3a: 1st electrode 3b: 2nd electrode 4: P-type thermoelectric conversion material chip 5: N-type thermoelectric conversion material chip 6: Solder material layer 7: Solder acceptance layer 11: Cooling characteristic evaluation unit 12: Peltier-cooled thermoelectric conversion module 13a, 13b: Temperature measurement board 14a, 14b: Temperature controller
Claims
1. A Peltier-cooled thermoelectric conversion module, in which the thickness of the chip of thermoelectric conversion material is less than 200 μm.
2. 2. The Peltier cooling thermoelectric conversion module according to claim 1, wherein the chips of thermoelectric conversion material include chips of P-type thermoelectric conversion material and chips of N-type thermoelectric conversion material.
3. 3. The Peltier cooling thermoelectric conversion module according to claim 2, wherein the electrical resistance value per chip of the P-type thermoelectric conversion material is 30 (mΩ) or less, and the electrical resistance value per chip of the N-type thermoelectric conversion material is 20 (mΩ) or less.
4. 2. The Peltier cooling thermoelectric conversion module according to claim 1, wherein the total thickness of the Peltier cooling thermoelectric conversion module is 300 to 1000 μm.