Manufacturing method for electrode mixture and manufacturing method for conductive aid agent
A dry mixing method using oxidized carbon and conductive carbon composites effectively disperses carbon nanotubes in electrode active material particles, enhancing electrode density and conductivity while reducing environmental waste.
Patent Information
- Application Number
- JP2023056114
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for dispersing low-dispersity carbon such as carbon nanotubes in electrode active material particles face challenges in maintaining uniform dispersion and preventing agglomeration, particularly in dry mixing processes which lack the effectiveness of ultrasonic irradiation used in wet mixing, leading to environmental waste issues.
A dry mixing method involving the use of partially pasty oxidized carbon with hydrophilic parts and conductive carbon to form a composite, which is mixed with electrode active material particles and fibrous carbon under dry conditions, enhancing dispersion and preventing agglomeration.
The method achieves high dispersion and maintains the dispersed state of low-dispersity carbon, improving electrode density and conductivity while reducing environmental impact by minimizing waste generation.
Smart Images

Figure 2024143435000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an electrode mixture that forms an electrode active material layer of an electricity storage device, and a method for producing a conductive assistant contained in the electrode mixture.
[0002] There are various types of power storage devices, including secondary batteries, electric double layer capacitors, redox capacitors, and hybrid capacitors. These power storage devices are being considered for a wide range of applications, including power sources for information devices such as mobile phones and notebook computers, motor drive power sources for low-pollution vehicles such as electric vehicles and hybrid vehicles, and energy regeneration systems. In order to apply these devices to a wide range of applications, the power storage devices must meet the demand for further improvement in performance and miniaturization. In other words, there is a demand for further improvements in energy density and cycle life of power storage devices.
[0003] In general, an electricity storage device is composed of an electrolyte sandwiched between a pair of electrodes. The electrodes have an active material layer for storing energy. The electrode active material particles in the active material layer exhibit a capacitance by a faradaic reaction involving the transfer of electrons with ions in the electrolyte, or by a non-faradaic reaction such as polarization that does not involve the transfer of electrons. However, electrode active material particles generally have low electrical conductivity. Therefore, it has been considered to combine the electrode active material particles with conductive carbon and use the composite as a constituent of the active material layer.
[0004] Conductive carbon improves the conductivity of the electrode. That is, conductive carbon contributes to lowering the direct current internal resistance (DCIR) and equivalent series resistance (ESR) of the power storage device. However, conductive carbon does not contribute to the energy density of the power storage device. Therefore, it is better to minimize the amount of conductive carbon in the composite. In other words, it is better to maximize the amount of electrode active material particles per unit volume while maintaining good conductivity. Therefore, carbon nanotubes, which exhibit high conductivity even in small amounts, have attracted attention. A composite of carbon nanotubes and electrode active material particles can increase the electrode density. Furthermore, this composite can achieve low DCIR and ESR even when the electrode density is increased (see, for example, Patent Document 1).
[0005] Carbon nanotubes tend to aggregate due to van der Waals forces and form a bundle structure. In other words, carbon nanotubes are a type of low-dispersibility carbon that is difficult to disperse. Therefore, it is necessary to dissolve the bundle structure and disperse the carbon nanotubes uniformly before compounding them with the electrode active material particles.
[0006] A wet mixing method is known as a method for dispersing low-dispersibility carbon such as carbon nanotubes, in which the low-dispersibility carbon is added to a mixed solution of concentrated sulfuric acid or concentrated nitric acid, and high-output ultrasonic waves are irradiated. In order to maintain the dispersion of the low-dispersibility carbon, a substance that stabilizes the dispersion, such as a dispersant, is mixed into the dispersion liquid. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2004-2156 A Summary of the Invention [Problem to be solved by the invention]
[0008] In recent years, environmental considerations have become important. A method of mixing electrode active material particles and carbon nanotubes in a wet state generates waste liquid, etc. Therefore, a method of mixing electrode active material particles and carbon nanotubes in a dry state has been studied.
[0009] However, in the dry mixing method, it is not possible to employ a dispersion method using ultrasonic irradiation, and it is also not possible to make the dispersant exist uniformly and finely in the solid. Therefore, in the dry mixing method, it is difficult to highly disperse low-dispersibility carbon such as carbon nanotubes and to suppress aggregation.
[0010] The object of the present invention has been proposed to solve the above-mentioned problems, and its object is to provide a method for producing an electrode mixture in which low-dispersibility carbon is well dispersed, and a method for producing a conductive assistant contained in this electrode mixture. [Means for solving the problem]
[0011] In order to solve the above problems, the manufacturing method of the electrode mixture of the present embodiment includes a carbon mixing step of mixing conductive carbon, some of whose particles are in a paste form, and low-dispersibility carbon under dry conditions.
[0012] The method may include an oxidation step of forming a paste-like oxidized carbon containing hydrophilic parts at 10% by mass or more of the total by oxidation treatment, and a conductive carbon preparation step of mixing the oxidized carbon with another particulate carbon having a hydrophilic particulate content of less than 10% by mass of the total, thereby combining the particulate carbon and the oxidized carbon to obtain the conductive carbon.
[0013] The method may further include an active material mixing step of mixing the conductive assistant obtained in the carbon mixing step with an electrode active material under dry conditions.
[0014] The conductive carbon may have a primary particle diameter of 12 nm or more and 34 nm or less.
[0015] The low-dispersion carbon may be vapor-grown carbon fiber, single-walled carbon nanotubes, or multi-walled carbon nanotubes.
[0016] The method may include an electrolyte mixing step of mixing a solid electrolyte.
[0017] The electrolyte mixing step may be performed after the carbon mixing step and before the active material mixing step, and the electrolyte mixing step may be further performed after the active material mixing step.
[0018] The method may further include a binder mixing step of mixing a binder.
[0019] In order to solve the above problems, the method for producing a conductive additive of the present embodiment includes a carbon mixing step of mixing conductive carbon, some of whose particles are in a paste form, and low-dispersibility carbon under dry conditions.
[0020] The method may include an oxidation step of forming a paste-like oxidized carbon containing hydrophilic parts at 10% by mass or more of the total by oxidation treatment, and a conductive carbon preparation step of mixing the oxidized carbon with another particulate carbon having a hydrophilic particulate content of less than 10% by mass of the total, thereby combining the particulate carbon and the oxidized carbon to obtain the conductive carbon.
[0021] The conductive carbon may have a primary particle diameter of 12 nm or more and 34 nm or less.
[0022] The low-dispersion carbon may be vapor-grown carbon fiber, single-walled carbon nanotubes, or multi-walled carbon nanotubes. Effect of the Invention
[0023] According to the present invention, the low-dispersibility carbon is highly dispersed in the dry mixing method, and the highly dispersed state is maintained. [Brief description of the drawings]
[0024] [Figure 1] 1A to 1C are schematic diagrams showing a method for producing a conductive assistant. [Diagram 2] 1 is a first flowchart showing a method for producing an electrode mixture. [Diagram 3] FIG. 2 is a schematic diagram showing an electrode active material particle. [Figure 4] 4 is a second flowchart showing the method for producing an electrode mixture. [Diagram 5] 13 is a third flowchart showing the method for producing an electrode mixture. [Figure 6] 1A is the particle size distribution of the conductive assistant of Comparative Example 1, and FIG. 1B is the particle size distribution of the conductive assistant of Example 1. [Figure 7] 1A is the particle size distribution of the conductive assistant of Comparative Example 1, and FIG. 1B is the particle size distribution of the conductive assistant of Example 2. [Figure 8] 1A is the particle size distribution of the conductive assistant of Comparative Example 1, and FIG. 1B is the particle size distribution of the conductive assistant of Example 3. [Figure 9] 1A is the particle size distribution of the conductive assistant of Comparative Example 1, and FIG. 1B is the particle size distribution of the conductive assistant of Example 4. [Figure 10] 1A is an SEM photograph of the surface of an electrode mixture, (a) is Example 1, (b) is Example 2, and (c) is Comparative Example 1. [Figure 11] 1A is an SEM photograph of the surface of an electrode mixture, (a) is an example 3, (b) is an example 4, and (c) is a comparative example 1. [Figure 12] 1 shows SEM photographs of the surface of an electrode mixture, where (a) is Example 1, (b) is Example 2, (c) is Example 3, and (d) is Comparative Example 1. [Figure 13] 1 is a graph showing pellet density in each example in each manufacturing method of an electrode mixture. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] Hereinafter, embodiments of the method for producing an electrode mixture according to the present invention and the method for producing a conductive assistant contained therein will be described in detail. Note that the present invention is not limited to the embodiments described below.
[0026] (Electrode mixture) The electrode mixture according to the present embodiment is a mixture that forms an active material layer of an electrode, and is used to manufacture an electrode for an electricity storage device. An electricity storage device is a passive element that charges and discharges electric energy, and examples of the device include a secondary battery, an electric double layer capacitor, a redox capacitor, and a hybrid capacitor.
[0027] The power storage device is roughly classified as comprising a pair of electrodes and an electrolyte interposed between the electrodes. The electrode mixture is applied to the active material layer of one or both of the positive electrode or the negative electrode of the pair of electrodes.
[0028] The active material layer is formed by applying an electrode mixture to a current collector and drying it. The current collector is an electrical conductor and also serves as a support substrate for the active material layer. The active material layer is formed on one or both sides of the current collector. That is, the electrode mixture is applied to one or both sides of the current collector. The active material layer formed by this electrode mixture becomes an energy storage layer.
[0029] The current collector is made of a conductive material such as platinum, gold, nickel, aluminum, titanium, steel, carbon, etc. The current collector may have any shape such as a film, foil, plate, mesh, expanded metal, or cylinder.
[0030] The electrode mixture includes an electrode active material and a conductive assistant. The electrode mixture may further include a solid electrolyte and a binder. The electrode active material exhibits a capacity by a Faraday reaction involving the transfer of electrons with ions in the electrolyte, or by a non-Faraday reaction such as polarization not involving the transfer of electrons. The conductive assistant is conductive carbon, which is composited with the electrode active material. The solid electrolyte may be a pseudo-solid electrolyte, that is, an electrolyte that is pseudo-solid powder or gel-like by adjusting the component ratio of the ionic liquid and the oxide nanoparticles.
[0031] Pressure is applied to the electrode mixture by pressing, and the electrode is pressure-molded to obtain a pellet-shaped electrode. The electrode is obtained by pressing the electrode mixture and the current collector together. The electrode may be obtained by pressing both the electrode mixture and the current collector. Alternatively, the electrode mixture is stretched by rolling to form a sheet. The electrode mixture is integrated with the current collector by applying pressure onto the current collector or by using an adhesive, etc. to obtain an electrode. Note that the electrode may be obtained by applying pressure to the electrode mixture on the current collector.
[0032] The pressure applied to the active material layer by the rolling process is generally 50,000 to 1,000,000 N / cm 2 The rolling temperature is not particularly limited, and the rolling may be performed at room temperature or under heated conditions.
[0033] The electrode mixture refers to a method for producing an electrode mixture by mixing a conductive assistant and an electrode active material under dry conditions, but is not limited thereto. The electrode mixture may be produced by adding a conductive assistant, an electrode active material, a solvent, and a diluent, and further adding a binder and a solid electrolyte as necessary, and mixing them under wet conditions. In this case, the electrode mixture is in a slurry state, and may be applied to a current collector and dried, and the formed active material layer may be subjected to pressure by rolling to obtain an electrode. However, a dry manufacturing method such as powder compaction or sheet molding can reduce the environmental load by suppressing the amount of waste liquid during the production process.
[0034] (electrode active material particles) Specifically, examples of electrode active materials used in the positive electrode of secondary batteries include layered rock salt LiMO2, layered Li2MnO3-LiMO2 solid solution, and spinel LiM2O4 (wherein M is Mn, Fe, Co, Ni, or a combination thereof). Specific examples of these include LiCoO2, LiNiO2, LiNi 4 / 5 Co 1 / 5 O2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 1 / 2 Mn 1 / 2 O2, LiFeO2, LiMnO2, Li2MnO3-LiCoO2, Li2MnO3-LiNiO2, Li2MnO3-LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, Li2MnO3-LiNi 1 / 2 Mn 1 / 2 O2, Li2MnO3-LiNi 1 / 2 Mn 1 / 2 O2-LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiMn2O4, LiMn 3 / 2 Ni 1 / 2 O4. Sulfur and Li2S, TiS2, MoS2, FeS2, VS2, Cr 1 / 2 V 1 / 2 Sulfides such as S2, selenides such as NbSe3, VSe2, NbSe3, oxides such as Cr2O5, Cr3O8, VO2, V3O8, V2O5, V6O13, LiNi 0.8 Co 0.15 Al 0.05 O2, LiVOPO4, LiV3O5, LiV3O8, MoV2O8, Li2FeSiO4, Li2MnSiO4, LiFePO4, LiFe 1 / 2 Mn 1 / 2 Examples include complex oxides such as PO4, LiMnPO4, and Li3V2(PO4)3.
[0035] Examples of electrode active materials used in the negative electrodes of secondary batteries include oxides such as Fe2O3, MnO, MnO2, Mn2O3, Mn3O4, CoO, Co3O4, NiO, Ni2O3, TiO, TiO2, SnO, SnO2, SiO, SiO2, RuO2, WO, WO2, and ZnO; metals such as Sn, Si, Al, and Zn; and LiVO2, Li3VO4, Li4Ti5O. 12 Complex oxides such as Li 2.6 Co 0.4 Nitrides such as N, Ge3N4, Zn3N2, and Cu3N.
[0036] Examples of electrode active materials in the polarizable electrodes of electric double layer capacitors include carbon materials with large specific surface areas, such as activated carbon, graphene, carbon nanofibers, carbon nanotubes, phenolic resin carbide, polyvinylidene chloride carbide, and microcrystalline carbon. In hybrid capacitors, the active materials used for the positive electrode exemplified for the secondary battery can be used for the positive electrode, and in this case, the negative electrode is composed of a polarizable electrode using activated carbon or the like. In addition, the negative electrode active materials exemplified for the secondary battery can be used for the negative electrode, and in this case, the positive electrode is composed of a polarizable electrode using activated carbon or the like.
[0037] Examples of the electrode active material in the positive electrode of the redox capacitor include metal oxides such as RuO2, MnO2, and NiO, and the electrode active material particles in the negative electrode are composed of an active material such as RuO2 and a polarizable material such as activated carbon.
[0038] In addition, Si-based compounds are also suitable as the electrode active material on the negative electrode side of a lithium ion secondary battery, and the electrode active material on the negative electrode side of a hybrid capacitor combined with a positive electrode that exhibits an electric double layer action. The Si-based compound is a compound represented by SiOx (0≦x<2), such as Si or SiO, and may be doped with a different element such as Ti or P, and may further have a surface coated with carbon. In particular, SiO particles are suitable as the electrode active material.
[0039] In particular, SiO has a theoretical specific capacity per weight of approximately 2000 mAhg-1 , and the operating potential is about 0.5 V (vs. Li / Li + ) In other words, the specific capacitance is much larger than that of graphite, and the operating potential is low like that of graphite, but the operating potential is about 0.05 V (vs. Li / Li + ) is not as extremely low as that of graphite. SiO is also easily available and has a low environmental impact.
[0040] There is no limitation on the shape or particle size of the electrode active material. However, the average particle size of the electrode active material is preferably more than 2 μm and not more than 25 μm. An electrode active material having this relatively large average particle size improves the electrode density by itself. The average particle size of the electrode active material means the 50% diameter (median diameter) in the measurement of particle size distribution using a light scattering particle sizer.
[0041] (Conductive assistant) FIG. 1 is a schematic diagram showing a method for producing a conductive additive. The conductive additive is a carbon composite made by combining conductive carbon 1 and fibrous carbon 2. The fibrous carbon 2 is a type of low-dispersibility carbon, but the conductive carbon 1 adheres to its surroundings, preventing aggregation due to van der Waals forces and dispersing it. Some of the particles of the conductive carbon 1 are paste-like particles. This conductive carbon 1 is a composite of oxidized carbon 3 and particulate carbon 4.
[0042] More specifically, examples of the fibrous carbon 2 include fibrous carbon such as carbon nanotubes, carbon nanofibers (hereinafter, CNF), vapor-grown carbon fibers, etc. The carbon nanotubes may be single-walled carbon nanotubes (SWCNTs) having one graphene sheet, or multi-walled carbon nanotubes (MWCNTs) having two or more graphene sheets rolled coaxially to form multiple tube walls, or may be a mixture of these.
[0043] The outer diameter of the fibrous carbon 2 is in the range of 1 to 150 nm, preferably 1 to 70 nm, and more preferably 1 to 40 nm. The length of the fibrous carbon 2 is in the range of 1 to 500 μm, preferably 5 to 400 μm, and more preferably 5 to 200 μm. If it is smaller than these ranges, it becomes difficult to increase the electrode density.
[0044] In addition, since the fewer the number of graphene sheets in a carbon nanotube, the higher the capacity density of the carbon nanotube itself, carbon nanotubes having 50 or less layers, preferably 10 or less layers, are preferred in terms of capacity density. Note that the fibrous carbon 2 may also be subjected to an opening treatment or activation treatment in which holes are made at the tip or wall of the fibrous carbon 2.
[0045] In the conductive carbon 1 constituting the conductive assistant, the oxidation-treated carbon 3 is made from porous carbon powder, Ketjen black, furnace black having voids, carbon nanofibers, carbon nanotubes, and other carbon materials having voids, and has hydrophilic portions on the particle surface. The content of the hydrophilic portions is preferably 10% by mass or more of the entire oxidation-treated carbon 3. It is particularly preferable that the content of the hydrophilic portions is 12% by mass or more and 30% by mass or less of the entire amount.
[0046] The hydrophilic parts are the parts where hydroxyl groups, carboxyl groups, or ether bonds have been introduced to the carbon by the oxidation process, parts where the conjugated double bonds of the carbon have been oxidized to generate single carbon bonds, and parts where the carbon-carbon bonds have been partially broken. 0.1 g of carbon is added to 20 mL of an aqueous ammonia solution at pH 11, and ultrasonic waves are irradiated for 1 minute. The resulting solution is left for 5 hours to precipitate the solid phase. The parts that do not precipitate and are dispersed in the aqueous ammonia solution at pH 11 are called hydrophilic parts.
[0047] After leaving it for 5 hours to allow the solid phase to settle, the supernatant liquid is removed and the remaining part is dried and the weight of the dried solid is measured. The weight of the dried solid is subtracted from the initial weight of carbon (0.1 g) to determine the weight of the hydrophilic part dispersed in the ammonia aqueous solution at pH 11. The weight ratio of the weight of the hydrophilic part to the initial weight of carbon (0.1 g) is the content of the hydrophilic part in the carbon.
[0048] Since the oxidation treated carbon 3 has hydrophilic portions at this ratio, it easily spreads out like a paste. Therefore, the oxidation treated carbon 3 easily extends along the surface of the particulate carbon 4 and is easily combined, and the conductive carbon 1 easily extends along the surface of the fibrous carbon 2 and is easily combined. Therefore, the conductive carbon 1 suppresses the aggregation of the fibrous carbon 2 and promotes dispersion.
[0049] The term "paste-like" means that in an SEM photograph taken at a magnification of 25,000 times, no grain boundaries are observed in the primary particles of the oxidation-treated carbon 3, and non-particulate, amorphous carbon is connected together.
[0050] The voids in the oxidized carbon 3 are determined by the BET method, and the specific surface area is 300 m 2 / g or more is preferable. If the material has such voids, it is easy to give the material a property of changing into a paste by oxidation treatment. Among them, spherical particles such as Ketjen Black and furnace black having voids are preferable as raw materials.
[0051] The particulate carbon 4 is distinguished from the oxidized carbon 3 that has spread into a paste-like form, and has a hydrophilic portion content of less than 10% by mass of the entire conductive carbon, and is less likely to turn into a paste-like form than the oxidized carbon 3. If the content is less than 10% by mass, the particulate carbon 4 may be oxidized or unoxidized.
[0052] As the particulate carbon 4, carbon black such as ketjen black, acetylene black, furnace black, channel black, etc., which are used for electrodes of conventional electricity storage devices, fullerene, graphene, amorphous carbon, natural graphite, artificial graphite, graphitized ketjen black, mesoporous carbon, etc., can be used.
[0053] The particulate carbon 4 preferably has a spherical particle shape, and examples of the particulate carbon 4 include carbon black such as ketjen black, acetylene black, furnace black, and channel black, fullerene, mesoporous carbon, and artificial graphite. The particulate carbon 4 is preferably made of conductive carbon having a higher conductivity than the oxidation-treated carbon 3, and furnace black is particularly preferred.
[0054] A method for producing such a conductive assistant will be described. The oxidized carbon 3 is produced by oxidizing a carbon raw material. Any known oxidation method can be used without particular limitation. For example, the oxidized carbon 3 can be obtained by treating the carbon raw material in an acid or hydrogen peroxide solution. Examples of acids that can be used include nitric acid, a nitric acid-sulfuric acid mixture, and an aqueous hypochlorous acid solution. The oxidized carbon 3 can also be obtained by heating the carbon raw material in an oxygen-containing atmosphere, water vapor, or carbon dioxide. Furthermore, the oxidized carbon 3 can be obtained by subjecting the carbon raw material to plasma treatment, ultraviolet irradiation, corona discharge treatment, or glow discharge treatment in an oxygen-containing atmosphere. As the intensity of the oxidation treatment is increased, the proportion of hydrophilic parts increases.
[0055] The oxidized carbon 3 containing 10 mass % or more of a hydrophilic portion as a whole is (a) treating a porous carbon raw material with an acid; (b) mixing the acid-treated product with a transition metal compound; (c) grinding the resulting mixture to cause a mechanochemical reaction; (d) heating the product of the mechanochemical reaction in a non-oxidizing atmosphere; and (e) removing the transition metal compound and / or its reaction products from the product after heating; It can be suitably obtained by a production method including the steps of:
[0056] In step (a), a carbon raw material having voids, preferably Ketjen black, is immersed in acid and left to stand. During this immersion, ultrasonic irradiation may be used. The acid may be an acid normally used in the oxidation treatment of carbon, such as nitric acid, a mixture of nitric acid and sulfuric acid, or an aqueous solution of hypochlorous acid. The immersion time depends on the concentration of the acid and the amount of the carbon raw material to be treated, but is generally in the range of 5 minutes to 5 hours. After the acid treatment, the carbon is thoroughly washed with water and dried, and then mixed with a transition metal compound in step (b).
[0057] As the transition metal compound added to the carbon raw material in the step (b), inorganic metal salts such as transition metal halides, nitrates, sulfates, and carbonates, organic metal salts such as formates, acetates, oxalates, methoxides, ethoxides, and isopropoxides, or mixtures thereof can be used. These compounds may be used alone or in combination of two or more. Compounds containing different transition metals may be mixed and used in a predetermined amount. In addition, as long as they do not adversely affect the reaction, compounds other than the transition metal compound, such as alkali metal compounds, may be added together. Since the oxidation-treated carbon 3 is used by being mixed with electrode active material particles in the manufacture of electrodes for electricity storage devices, it is preferable to add compounds of elements constituting the active material to the carbon raw material, since this can prevent the inclusion of elements that may become impurities in the active material.
[0058] In step (c), the mixture obtained in step (b) is pulverized to cause a mechanochemical reaction. Examples of pulverizers for this reaction include a mortar mill, a stone mill, a ball mill, a bead mill, a rod mill, a roller mill, an agitator mill, a planetary mill, a vibration mill, a hybridizer, a mechanochemical composite device, and a jet mill. The pulverization time depends on the pulverizer used and the amount of carbon to be treated, and is not strictly limited, but is generally in the range of 5 minutes to 3 hours. Step (d) is performed in a non-oxidizing atmosphere such as a nitrogen atmosphere or an argon atmosphere. The heating temperature and heating time are appropriately selected depending on the transition metal compound used. In the subsequent step (e), the transition metal compound and / or the reaction product of the transition metal compound are removed from the product after heating by means of dissolving it in an acid, and then the product is thoroughly washed and dried to obtain an oxidized carbon containing hydrophilic parts of 10% by mass or more of the total.
[0059] In this manufacturing method, in step (c), the transition metal compound acts to promote the oxidation of the carbon raw material through a mechanochemical reaction, and the oxidation of the carbon raw material proceeds rapidly. By this oxidation, an oxidized carbon 3 containing hydrophilic portions of 10 mass% or more of the total is obtained.
[0060] The thus produced oxidation-treated carbon 3 is mixed with particulate carbon 4 to obtain conductive carbon 1. A dry mixing method is preferable, and a Raikai mill, a stone grinder, a ball mill, a bead mill, a rod mill, a roller mill, an agitator mill, a planetary mill, a vibration mill, a hybridizer, a mechanochemical composite device, or a jet mill can be used.
[0061] During this dry mixing process, the oxidation treated carbon 3 adheres to the surface of the particulate carbon 4, and the oxidation treated carbon 3 is partially gelatinized to obtain conductive carbon 1 at least partially converted into a paste. The ratio of the oxidation treated carbon 3 to the particulate carbon 4 is preferably in the range of 1:9 to 9:1, and more preferably 5:5, by mass ratio.
[0062] The primary particle diameter of the conductive carbon 1 is preferably 12 nm or more and 34 nm or less. When the primary particle diameter of the conductive carbon 1 is in this range, the aggregation of the fibrous carbon 2 can be effectively suppressed. Even if the primary particle diameter of the conductive carbon 1 is 44 nm or more, the aggregation suppression effect of the fibrous carbon 2 can be obtained, but in the range of 12 nm or more and 34 nm or less, the aggregation suppression effect is more remarkable than in the case of 44 nm.
[0063] Even when the conductive carbon 1 is 44 nm or more, the conductive carbon 1 adheres to the fibrous carbon 2 using the oxidation-treated carbon 3 and intervenes between the fibrous carbons 2 to separate the fibrous carbons 2. However, in some cases, the conductive carbons 1 adhere to each other via the oxidation-treated carbon 3. As a result, the fibrous carbons 2 come into close proximity to each other via the conductive carbon 1, which is thought to reduce the aggregation inhibition effect compared to when the conductive carbon is 12 nm or more and 34 nm or less.
[0064] The conductive carbon 1 is mixed with the fibrous carbon 2 in a dry state. In the dry mixing, for example, zirconia beads or the like are added and kneaded with a stirrer. By this kneading, the oxidized carbon 3 portion of the conductive carbon 1 adheres to the periphery of the fibrous carbon 2. The conductive carbon 1 penetrates between the fibrous carbon 2 that has been defibrated by the kneading, and the fibrous carbon 4 remains dispersed and aggregation is suppressed.
[0065] The method for producing an electrode mixture using the conductive carbon 1 produced in this manner is as follows. Fig. 2 is a first flow chart showing the method for producing an electrode mixture. As shown in Fig. 2, conductive carbon 1 and fibrous carbon 2 are dry-mixed to produce a conductive assistant (step S01). The conductive assistant is preferably adjusted so that it is contained in the electrode mixture at a ratio of 1 wt% to 5 wt% relative to the electrode active material particles.
[0066] In step S01, the mass ratio of the electrode active material to the conductive assistant is preferably in the range of 90:10 to 99.5:0.5, and more preferably in the range of 95:5 to 99:1. If the proportion of the conductive assistant is less than the above range, the conductivity of the active material layer is insufficient, and the coverage of the electrode active material by the conductive carbon 1 decreases, tending to degrade the cycle characteristics. If the proportion of the conductive assistant is more than the above range, the electrode density decreases, and the energy density of the electricity storage device tends to decrease.
[0067] Next, the solid electrolyte is added and mixed into the dry mixer containing the conductive assistant (step S02). In step S02, the amount of the solid electrolyte is preferably half of the total amount added and mixed during the manufacturing process of the electrode mixture. That is, in the final step of the manufacturing method of this electrode mixture, the remaining half of the solid electrolyte is added and mixed.
[0068] The solid electrolyte is not particularly limited, but in the case of a secondary battery, examples of the solid electrolyte include sulfide-based solid electrolytes and oxide-based solid electrolytes. As the sulfide-based solid electrolyte, for example, a LGPS-type solid electrolyte containing Li 10 GeP2S 12 , Argyrodite-type solid electrolytes Li3PS4, Li7P3S 11 , Li6PS5Cl, and glass-based solid electrolytes such as P2S5-Li2O, LiS-P2S5, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, LiI-Li2S-SiS2, LiCl-Li2S-SiS2, LiI-Si2S-P2S5, Li2S-P2S5-LiI-LiBr, LiI-Li2S-P2S5, Li2S-B2S3, LiI-Li2S-P2O5, Li2S-Li3PO4-SiS2, LiI-Li3PO4-P2S5, Li2S-GeS2, and Li2S-P2S5-GeS2.
[0069] Examples of oxide-based solid electrolytes include phosphate compounds having a NASICON structure or compounds in which a part of the phosphate compound is replaced with another element. 1.3 Al0.3 Ti 1.7 (PO4)3, Na3Zr2Si2PO 12 , Na 3.2 Zr 1.3 S 2.2 P 0.8 O 10.5 , Na3Zr 1.6 Ti 0.4 SiPO 12 , Na3Hf2Si2PO 12 , Na 3.4 Zr 0.9 Hf 1.4 Al 0.6 S 1.2 P 1.8 O 12 , Na3Zr 1.7 Nb 0.24 SiPO 12 , Na 3.6 Ti 0.2 Y 0.8 S 2.8 O9, Na3Zr 1.88 Y 0.12 SiPO 12 , Na 3.12 Zr 1.88 Y 0.12 SiPO 12 , Na 3.6 Zr 0.13 Yb 1.67 S 0.11 P 2.9 O 12 Li7La3Zr2O 12 Examples of the lithium ion conductor include a lithium ion conductor having a garnet-type structure or a structure similar to the garnet-type structure, such as a lithium ion conductor having a basic composition of Li5La3Ta2O. In addition, an oxide-based solid electrolyte having a perovskite structure or a structure similar to the perovskite may also be used. For example, an oxide-based solid electrolyte is Li5La3Ta2O. 12 , Li7Zr2O 12 , Li7La3Zr2O 12 , LiTi(PO4)3, LiGe(PO4)3, LiLaTiO3, Li6BaLa2Ta2O 12 etc. may also be used.
[0070] In addition, as for the solid electrolyte, in the case of an electric double layer capacitor, there is no particular limitation. For example, La 2 / 3-x Li 3x A perovskite-type inorganic solid electrolyte represented by TiO3 (0 < x < 1.7) can be mentioned. Specific examples of this perovskite-type inorganic solid electrolyte include, for example, La 0.5 Li 0.5 TiO3. In addition, as the perovskite-type inorganic solid electrolyte, Li 1.3 Al 0.3 Ti 1.7 (PO4)3, Na 1.4 Al 0.4 Ti 1.6 (PO4)3, Li 1.3 Y 0.3 Ti 1.7 (PO4)3, Li 1.2 Ga 0.2 Ti 1.8 (PO4)3 may also be used.
[0071] In addition, as for the solid electrolyte, in the case of a redox capacitor, there is no particular limitation. For example, an amorphous semiconductor containing hydrogen as a proton conductor can be mentioned. Examples of the amorphous semiconductor containing hydrogen include amorphous silicon, amorphous silicon germanium, or amorphous germanium. Alternatively, examples of the amorphous semiconductor containing hydrogen include an oxide semiconductor containing hydrogen, and examples of the oxide semiconductor containing hydrogen include zinc oxide, titanium oxide, nickel oxide, vanadium oxide, tin oxide, or indium oxide.
[0072] After the solid electrolyte is introduced, the electrode active material is additionally introduced and mixed in a dry stirrer (step S03). In the dry mixing of the conductive assistant and the electrode active material, the oxidized carbon 3 adheres to the surface of the electrode active material, and the conductive carbon 1 covers the surface of the electrode active material particles, so the aggregation of the electrode active material is suppressed. Also, due to the pressure exerted on the oxidized carbon 3 during the mixing process, at least a part of the oxidized carbon 3 spreads in a paste form with respect to the fibrous carbon 2 and the electrode active material, thereby generating an active material composite. Note that when the average particle diameter of the electrode active material is larger than 2 μm and 25 μm or less, the pasty state of the oxidized carbon 3 is promoted by the pressing force.
[0073] Fig. 3 is a schematic diagram showing the composite produced in step 3. As shown in Fig. 3, the fibrous carbon 2 in the conductive assistant is attached to the electrode active material particles 6 (hereinafter referred to as electrode active material particles 6) via the conductive carbon 1 while maintaining dispersion due to the attachment of the conductive carbon 1.
[0074] For this reason, the electrode active material particles 6 are connected to each other by the fibrous carbon 2, which is an excellent electron path. And since both the fibrous carbon 2 and the conductive carbon 1 are mainly made of carbon, they fit well at the contact surface and are compatible for electron transfer. In addition, the conductive carbon 1 adheres closely to the electrode active material particles 6. Therefore, compared to the transfer of electrons between the fibrous carbon 2 and the electrode active material particles 6, it is easier to transfer electrons to the electrode active material particles 6. Therefore, this composite structure contributes to lowering the resistance of the electrode.
[0075] 2, after the electrode active material is added and mixed (step S03), the solid electrolyte is again added and mixed in the dry mixer (step S04). The electrode density is most improved by adding and mixing the solid electrolyte twice, with the electrode active material particles 6 and the conductive carbon 1 being mixed in between.
[0076] Here, by adding and mixing the solid electrolyte twice, the contact state of the conductivity between the electrode active material and the solid electrolyte becomes good. That is, a good conductive path is formed between the electrode active material and the solid electrolyte, and the resistance is reduced and the electrical conductivity is improved. Although it is a supposition and not limited thereto, the reason is as follows. That is, first, if the conductive assistant covers the entire surface of the electrode active material under dry conditions, the conductive assistant will be blocked and it will be difficult to form an ion path between the electrode active material and the solid electrolyte. Also, if the amount of solid electrolyte on the surface of the electrode active material is large and the coating thickness of the solid electrolyte is thick, it will be difficult for the conductive assistant to contact the electrode active material, and in this case, it will be difficult to form a conductive path between the conductive assistant and the electrode active material. Therefore, by adding and mixing the solid electrolyte in step S02, a part of the solid electrolyte is brought into contact with the surface of the electrode active material. Then, by mixing the conductive assistant, an ion path with the solid electrolyte is formed on the surface of the electrode active material, and a conductive path can also be formed by the conductive assistant on the active material surface and between the active material. Then, by adding the solid electrolyte in step S04, the solid electrolyte can be filled so as to fill the gaps between the electrode active material, the conductive assistant, and the solid electrolyte, and the electrical conductivity of the electrode mixture becomes good.
[0077] After preparing the electrode mixture in this manner, a binder, a solvent, and a diluent are added to the electrode mixture to form a slurry. The diluent is added last. The slurry is then applied onto a current collector and dried, and pressure is applied to the active material layer by rolling to obtain an electrode. The slurry may be formed into a sheet or pellet shape and dried, and then integrated with the current collector by a roll, a press, or the like.
[0078] As the binder, known binders such as polytetrafluoroethylene, polyvinylidene fluoride, tetrafluoroethylene-hexafluoropropylene copolymer, polyvinyl fluoride, and carboxymethyl cellulose are used. The content of the binder is preferably 1 to 30% by mass with respect to the total amount of the electrode mixture. If it is 1% by mass or less, the strength of the active material layer is insufficient, and if it is 30% by mass or more, inconveniences such as a decrease in the discharge capacity of the electrode and excessive internal resistance occur. As the solvent, a solvent that does not adversely affect other components in the electrode material, such as N-methylpyrrolidone, can be used without any particular limitation. As long as each component in the mixture is mixed uniformly, there is no particular limitation on the amount of the solvent.
[0079] In the rolling process, the active material layer is pressurized, so that the oxidation-treated carbon 3, at least a part of which has been changed into a paste-like state, spreads further and is pushed out into the gaps formed between the electrode active material particles 6 and into the insides of the pores present on the surfaces of the electrode active material particles 6, so that the amount of active material per unit volume in the electrode increases, and the electrode density increases. In addition, the densely packed paste-like oxidation-treated carbon 3 has sufficient conductivity to function as a conductive agent.
[0080] Furthermore, when pressure is applied to the active material layer, the oxidized carbon 3 on the electrode active material particles 6 spreads into a paste-like shape by rolling, and in the process, some of the carbon reaches the fibrous carbon 4. This promotes a reduction in the resistance of the active material layer.
[0081] The active material layer can be dried by removing the solvent under reduced pressure and heating as necessary. The pressure applied to the active material layer by the rolling treatment is generally 50,000 to 1,000,000 N / cm. 2 , preferably 100,000 to 500,000 N / cm 2 The rolling temperature is not particularly limited, and the rolling may be performed at room temperature or under heating.
[0082] FIG. 4 is a second flow chart showing a method for producing an electrode mixture. As shown in FIG. 4, the solid electrolyte may be added once. That is, conductive carbon 1 and fibrous carbon 2 are dry-mixed to produce a conductive assistant (step S11). The entire amount of solid electrolyte to be included in the active material layer is added and mixed in the dry mixer in which the conductive assistant has been added (step S12). After the solid electrolyte is added, the electrode active material is added and mixed in the dry mixer (step S13). In this way, an electrode mixture can also be produced.
[0083] Fig. 5 is a third flow chart showing a method for producing an electrode mixture. As shown in Fig. 5, a solid electrolyte is not essential in the active material layer. After preparing a conductive assistant by dry mixing conductive carbon 1 and fibrous carbon 2 (step S101), the electrode active material may be additionally charged and mixed in a dry mixer (step S102) to complete the production of the electrode mixture.
[0084] In this way, the carbon mixing step in which the conductive carbon 1, some of whose particles are in a paste form, and the fibrous carbon 2 are mixed under dry conditions keeps the fibrous carbon 2 dispersed and inhibits aggregation. Therefore, even if the electrode active material particles 6 and the conductive assistant are mixed in a dry manner, the amount of aggregates generated can be inhibited. Therefore, the electrode density of the active material layer can be increased while being environmentally friendly in a dry manner.
[0085] In addition, other types of low-dispersion carbon may be added to the conductive assistant instead of the fibrous carbon 2. The aggregation of various types of low-dispersion carbon can be suppressed by the conductive carbon 1, and the electrode density of the active material layer can be increased while being dry and environmentally friendly. Examples of low-dispersion carbon include graphene, single-layer graphene, multi-layer graphene, reduced graphene oxide, graphene nanoribbons, and graphene nanoplatelets. Further examples of low-dispersion carbon include fullerene, C 60 Fullerene, C 70 Examples of the fullerene include fullerene, fullerene derivatives having functional groups such as ester groups modified on some carbon atoms, flake graphite, and scaly graphite.
[0086] The conductive carbon 1 preferably has a primary particle diameter of 12 nm or more and 34 nm or less. When the primary particle diameter of the conductive carbon 1 is within this range, the amount of aggregates generated in the electrode mixture can be effectively suppressed. EXAMPLES
[0087] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0088] Example 1 10 g of Ketjen Black with a particle size of about 40 nm was added to 300 mL of 60% nitric acid, and the resulting solution was irradiated with ultrasonic waves for 10 minutes, and then filtered to recover the Ketjen Black. The recovered Ketjen Black was washed with water three times and dried to obtain acid-treated Ketjen Black.
[0089] 3 g of this acid-treated Ketjen Black was mixed with 21.98 g of Fe(CH3COO), 0.77 g of Li(CH3COO), 1.10 g of C6H8O7·H2O, 1.32 g of CH3COOH, 1.31 g of H3PO4, and 120 mL of distilled water. The resulting mixture was stirred with a stirrer for 1 hour, then evaporated to dryness at 100°C in air and the mixture was collected. The resulting mixture was then introduced into a vibrating ball mill and ground for 30 minutes at 20 Hz. The ground powder was heated in nitrogen at 700°C for 3 minutes to obtain a composite of LiFePO4 supported on the oxidized Ketjen Black.
[0090] 1 g of the resulting composite was added to 100 mL of a 30% aqueous hydrochloric acid solution, and the resulting solution was irradiated with ultrasonic waves for 15 minutes to dissolve the LiFePO4 in the composite, and the remaining solid was filtered, washed with water, and dried. A part of the dried solid was heated to 900°C in air by TG analysis to measure the weight loss. The above-mentioned steps of dissolving LiFePO4 in an aqueous hydrochloric acid solution, filtering, washing with water, and drying were repeated until it was confirmed that the weight loss was 100%, that is, no LiFePO4 remained, to obtain an oxidation-treated carbon 3 from which LiFePO4 had been removed.
[0091] Next, 0.1 g of the obtained oxidized carbon 3 was added to 20 mL of an aqueous ammonia solution of pH 11, and ultrasonic irradiation was performed for 1 minute. The obtained liquid was left for 5 hours to precipitate the solid phase. After the precipitation of the solid phase, the supernatant liquid was removed and the remaining part was dried, and the weight of the dried solid was measured. The weight ratio of the weight of the dried solid to the weight of the initial oxidized carbon 3 (0.1 g) was taken as the content of the "hydrophilic portion" in the oxidized carbon 3. As a result, the weight ratio of the hydrophilic portion in the oxidized carbon was 15 mass%.
[0092] Next, the obtained oxidation-treated carbon 3 was dry-mixed with furnace black, which is particulate carbon 4. The oxidation-treated carbon 3 and particulate carbon 4 were introduced into a ball mill in a mass ratio of 1:9. The average particle size of the primary particles of the particulate carbon 4 was 12 nm. Ketjen black, which had an initial particle size of about 40 nm, was processed into oxidation-treated carbon 3 and kneaded together with the particulate carbon 4, whereby it was finely broken down and combined with the particulate carbon 4. As a result, conductive carbon 1 with an average primary particle size of 12 nm was obtained.
[0093] The primary particle diameter of the conductive carbon 1 was measured using a transmission electron microscope (TEM). The diameter of each unit particle was measured from a TEM image of the conductive carbon 1, and the average diameter of a certain number of the unit particles was taken as the primary particle diameter. In practice, the primary particle diameter of the conductive carbon 1 was obtained by measuring 1,000 unit particles and calculating the average particle diameter of the primary particles. In other words, the primary particle diameter of the conductive carbon 1 shown in Example 1 was 12 nm.
[0094] The conductive carbon 1 and fibrous carbon 2 were dry mixed. Vapor-phase grown carbon fiber VGCF (Showa Denko K.K.) was used as the fibrous carbon 2. 0.1 g of the conductive carbon 1 and 0.1 g of the fibrous carbon 2 were put into a 50 cc vial, and 6 g of zirconium balls with a diameter of 1φ were further added, and the materials were dry mixed in a dry kneading device (model ARE-310, manufactured by Thinky Corporation). As a result, a conductive assistant of Example 1 was obtained in which the conductive carbon 1 was attached to the fibrous carbon 2.
[0095] Next, the electrode active material particles 6 and the conductive assistant were dry-mixed. The electrode active material particles 6 were LiNi 0.5 Mn 0.3 Co 0.2 O2 particles. 98 parts by mass of electrode active material particles 6 were mixed with 2 parts by mass of conductive assistant. In the dry mixing, both were placed in a mortar and kneaded with a pestle for about 10 to 15 minutes. In this way, the electrode mixture of Example 1 was completed.
[0096] Example 2 Furthermore, a conductive assistant and an electrode mixture of Example 2 were prepared. Example 2 differs from Example 1 in that the average particle size of the primary particles of the conductive carbon 1 is 17 nm. The rest of the conductive assistant and electrode mixture were prepared by the same manufacturing method and manufacturing conditions as Example 1. Unlike Example 1, Example 2 used particulate carbon 4 having an average primary particle size of 13 nm, and mixed oxidized carbon 3 and particulate carbon 4 at a mass ratio of 3:7 to obtain conductive carbon 1 having an average primary particle size of 17 nm.
[0097] Example 3 Furthermore, a conductive assistant and an electrode mixture of Example 3 were prepared. Example 3 differs from Example 1 in that the average particle diameter of the primary particles of the conductive carbon 1 is 34 nm. The rest was prepared by the same manufacturing method and manufacturing conditions as Example 1. Unlike Example 1, Example 3 used particulate carbon 4 having an average particle diameter of the primary particles of 34 nm, and mixed oxidized carbon 3 and particulate carbon 4 at a mass ratio of 1:9 to obtain conductive carbon 1 having an average particle diameter of the primary particles of 34 nm.
[0098] Example 4 Furthermore, a conductive assistant and an electrode mixture of Example 4 were prepared. Example 4 differs from Example 1 in that the average particle size of the primary particles of the conductive carbon 1 is 44 nm. The rest of the conductive assistant and electrode mixture were prepared by the same manufacturing method and manufacturing conditions as Example 1. Unlike Example 1, Example 4 used particulate carbon 4 having an average primary particle size of 42 nm, and mixed oxidized carbon 3 and particulate carbon 4 at a mass ratio of 1:1 to obtain conductive carbon 1 having an average primary particle size of 44 nm.
[0099] Comparative Example 1 A conductive assistant and an electrode mixture of Comparative Example 1 were prepared as a comparison control for Examples 1 to 4. The conductive assistant of Comparative Example 1 differs from Example 1 in that the oxidized carbon 3 is omitted. That is, Ketjen black, which is particulate carbon 4, and single-walled carbon nanotubes, which are fibrous carbon 2, were mixed in a dry manner, and the mixture was used as the conductive assistant of Comparative Example 1. 0.1 g of Ketjen black and 0.1 g of single-walled carbon nanotubes were kneaded in a mortar with a pestle for about 10 to 15 minutes to prepare the conductive assistant of Comparative Example 1. The manufacturing method and manufacturing conditions of the electrode mixture of Comparative Example 1 using this conductive assistant are the same as those of Example 1.
[0100] (Observation results of conductive additive) The particle size distribution of the conductive assistant of Examples 1 to 4 and Comparative Example 1 was measured. The particle size distribution was measured using a particle size distribution meter (manufactured by Microtrackbell Co., Ltd., model number MT3300EXII). The measurement environment was room temperature of 20°C to 25°C, and a 1 wt% sodium hexametaphosphate aqueous solution was used as the measurement solvent. First, 10.00±3.00 mg of the conductive assistant was placed in a 50 cc sample bottle, and 10 mL of the measurement solvent weighed with a 5 mL pipette was dropped into the sample bottle. After the measurement solvent was dropped, the measurement sample in the sample bottle was dispersed by ultrasonic treatment for 10 minutes using an ultrasonic device (ASU CLEAER, model number ASU-06). Then, after the ultrasonic treatment, the obtained measurement sample was measured with a particle size distribution meter.
[0101] The results of measuring the particle size distribution of the conductive assistant of Examples 1 to 4 and Comparative Example 1 are shown in Figs. 6 to 9. Fig. 6(a) shows the particle size distribution of Comparative Example 1, and (b) shows the particle size distribution of Example 1. Fig. 7(a) shows the particle size distribution of Comparative Example 1, and (b) shows the particle size distribution of Example 2. Fig. 8(a) shows the particle size distribution of Comparative Example 1, and (b) shows the particle size distribution of Example 3. Fig. 9(a) shows the particle size distribution of Comparative Example 1, and (b) shows the particle size distribution of Example 4.
[0102] 6 to 8, in Examples 1 to 3 in which the average primary particle diameter of the conductive carbon 1 is 34 nm or less, the particle size distribution is composed of a single peak. On the other hand, in Comparative Example 1 in which the conductive assistant is a composite of particulate carbon 4 and fibrous carbon 2 instead of conductive carbon 1, the particle size distribution has peaks at particle sizes of 8 μm and 60 μm, as shown in FIG.
[0103] 6 to 8, it can be seen that no agglomerates were generated in the conductive additive in Examples 1 to 4. On the other hand, it can be seen that agglomerates with a particle size of about 60 μm were generated in Comparative Example 1.
[0104] 9, in Example 4 in which the average primary particle diameter of the conductive carbon 1 is 44 nm, the particle size distribution has a peak at a particle diameter of 8 μm and a peak at a particle diameter of 15 μm. That is, it can be confirmed that when the average primary particle diameter of the conductive carbon 1 is 44 nm, the generation of small aggregates can be kept as compared with Comparative Example 1. In other words, it was confirmed that when the average primary particle diameter of the conductive carbon 1 is 34 nm or less, no aggregates are generated in the conductive assistant, and the aggregation suppression effect is significant.
[0105] 10 and 11 are SEM photographs taken at 25k magnification using a scanning electron microscope of the surfaces of the conductive assistants of Examples 1 to 4 and Comparative Example 1. (a) in Fig. 10 is Example 1, (b) is Example 2, and (c) is Comparative Example 1. (a) in Fig. 11 is Example 3, (b) is Example 4, and (c) is Comparative Example 1.
[0106] In the SEM images of Comparative Example 1 in FIG. 10 and FIG. 11(c), there are many aggregates of Ketjen Black, and the Ketjen Black aggregates are in contact with the fibrous carbon 2 such that a part of the fibrous carbon 2 is stuck into them, or the Ketjen Black aggregates are in contact with the fibrous carbon 2 such that a part of the fibrous carbon 2 is entangled with them. Therefore, there are parts on the surface of the fibrous carbon 2 in Comparative Example 1 where Ketjen Black is not attached. In other words, the Ketjen Black and the fibrous carbon 2 in Comparative Example 1 are simply mixed and in contact with each other, and the Ketjen Black and the fibrous carbon 2 are not composited and exist independently. Therefore, there is no Ketjen Black between some of the fibrous carbon 2, and some of the fibrous carbon 2 are close to each other, so the dispersibility of the entire fibrous carbon 2 is poor.
[0107] On the other hand, in the SEM images of Example 1 in (a) and Example 2 in (b) of FIG. 10, the amount of aggregation of the conductive carbon 1 is less than that of Comparative Example 1 in (c), and the conductive carbon 1 is attached to the surface of the fibrous carbon 2. The conductive carbon 1 and the fibrous carbon 2 are composited. Even when the primary particle size of the conductive carbon 1 is large as in Examples 3 and 4 in (a) and (b) of FIG. 11, the amount of aggregation is less than that of Comparative Example 1 in (c) of FIG. 11, and the conductive carbon 1 is attached around the fibrous carbon 2, and the conductive carbon 1 and the fibrous carbon are composited. Therefore, the conductive carbon 1 is firmly inserted between many pieces of fibrous carbon 2, and many pieces of fibrous carbon 2 are kept apart, and the dispersibility of the entire fibrous carbon 2 is high.
[0108] (Observation results of electrode mixture) Next, the surfaces of the electrode mixtures of Examples 1 to 3 and Comparative Example 1 were observed at a magnification of 1.50k using a scanning electron microscope. Fig. 12 shows SEM images showing the results of this SEM observation, where (a) is Example 1, (b) is Example 2, (c) is Example 3, and (d) is Comparative Example 4.
[0109] As shown in Fig. 12, no aggregates were generated in the electrode mixture when the conductive carbon 1 was included in the conductive assistant of Examples 1 to 3. On the other hand, as shown in (d) of Fig. 12, when the conductive carbon 1 and the fibrous carbon 2 were not combined, aggregates were found in the electrode mixture.
[0110] Example 5 The electrode mixture of Example 5 was prepared by the following manufacturing method. This manufacturing method is different from Example 1 in that the solid electrolyte is added to the electrode mixture in two separate batches. In Example 5, the electrode active material particles 6, the conductive assistant, and the solid electrolyte are added in a ratio of 67:3:30, respectively.
[0111] That is, after preparing a conductive additive using the same manufacturing method and conditions as in Example 1, this conductive additive was mixed with a solid electrolyte in a dry state. The solid electrolyte used was 75mol%Li2S·25mol%P2S5. 75mol%Li2S·25mol%P2S5 was added in a ratio of 5 times the conductive additive, in other words, half of the total amount of solid electrolyte added. In the dry mixing, both were placed in a mortar and kneaded with a pestle for about 10 to 15 minutes.
[0112] After the solid electrolyte was added first, the same type of electrode active material particles 6 as in Example 1 were added, and the mixture was dry-mixed with a pestle in a mortar for about 10 to 15 minutes. After the electrode active material particles 6 were added, the solid electrolyte was further added. For the second solid electrolyte, the same 75 mol% Li2S·25 mol% P2S5 as in the first solid electrolyte was used. For the second solid electrolyte, the same amount of conductive assistant as in the first solid electrolyte was added at a ratio of 5 times that of the first solid electrolyte, that is, the remaining half of the total amount of solid electrolyte added. In the dry mixing, both were placed in a mortar and kneaded with a pestle for about 10 to 15 minutes.
[0113] Example 6 In addition, the electrode mixture of Example 6 was prepared by the following manufacturing method. This manufacturing method is different from Example 5 in that all the solid electrolyte is included in the electrode mixture at one time. That is, after preparing the conductive assistant by the same manufacturing method and conditions as Example 1, this conductive assistant and the solid electrolyte were mixed in a dry state. The solid electrolyte used was 75 mol% Li2S·25 mol% P2S5. 75 mol% Li2S·25 mol% P2S5 was added at a ratio of 10 times the conductive assistant. In the dry mixing, both were placed in a mortar and kneaded with a pestle for about 10 to 15 minutes. After adding the solid electrolyte, the same type and amount of electrode active material particles 6 as those in Example 1 and Example 5 were added, and the mixture was kneaded in a dry state with a pestle in the mortar for about 10 to 15 minutes.
[0114] Example 7 In addition, the electrode mixture of Example 7 was prepared by the following manufacturing method. This manufacturing method is different from Examples 5 and 6 in that the solid electrolyte is added to the electrode mixture at once, and the solid electrolyte and the electrode active material particles 6 are added to the electrode mixture at the same time. That is, after preparing the conductive assistant by the same manufacturing method and conditions as in Example 1, this conductive assistant, the solid electrolyte, and the same type and amount of the electrode active material particles 6 as in Example 1 and Example 5 were mixed in a dry manner. The solid electrolyte used was 75 mol% Li2S·25 mol% P2S5. 75 mol% Li2S·25 mol% P2S5 was added at a ratio of 10 times the conductive assistant. In the dry mixing, both were placed in a mortar and kneaded with a pestle for about 10 to 15 minutes.
[0115] (Pellet density measurement) The electrode mixtures of Examples 5 to 7 were pelletized. 2.0 g of the electrode mixture was weighed out and pelletized by applying a load of 20 kN. The pellets were then observed with a scanning electron microscope to measure the pellet volume, and the density (g / cc) was calculated from the measurement results.
[0116] The electrode density of the pellets of Examples 5 to 7 is shown in Fig. 13. Fig. 13 is a graph showing the pellet density of each Example in each manufacturing method of the electrode mixture. As shown in Fig. 13, it was confirmed that Example 5, which is a manufacturing method in which the solid electrolyte is added in two separate batches, had the highest pellet density.
[0117] In addition to using 75mol%Li2S·25mol%P2S5 as a solid electrolyte, sodium sulfate may also be used. Although sodium sulfate does not have electrical conductivity, its particle shape, size, and hardness are similar to those of 75mol%Li2S·25mol%P2S5, which is known as a solid electrolyte. Therefore, by using it as a substitute for a solid electrolyte, the contact state between the active material, conductive additive, and binder can be confirmed. [Explanation of symbols]
[0118] 1. Conductive carbon 2. Fibrous carbon 3. Oxidized carbon 4. Particulate carbon 6 Electrode active material particles
Claims
1. a carbon mixing step of mixing conductive carbon, some of whose particles are in a paste form, with low-dispersion carbon under dry conditions; A method for producing an electrode mixture, comprising the steps of:
2. an oxidation process for forming a paste-like oxidized carbon having a hydrophilic portion in an amount of 10 mass% or more by oxidation; a conductive carbon preparation step of mixing the oxidation-treated carbon with particulate carbon having a hydrophilic portion content of less than 10 mass% of the total carbon, thereby compounding the particulate carbon with the oxidation-treated carbon to obtain the conductive carbon; The method for producing an electrode mixture according to claim 1,
3. an active material mixing step of mixing the conductive assistant obtained in the carbon mixing step with an electrode active material under dry conditions; containing, The method for producing an electrode mixture according to claim 1 or 2,
4. The conductive carbon has a primary particle size of 12 nm or more and 34 nm or less; The method for producing an electrode mixture according to claim 1 or 2,
5. The low-dispersion carbon is a vapor-grown carbon fiber, a single-walled carbon nanotube, or a multi-walled carbon nanotube; The method for producing an electrode mixture according to claim 1 or 2,
6. Including an electrolyte mixing step of mixing a solid electrolyte; The method for producing an electrode mixture according to claim 3,
7. The electrolyte mixing step is carried out after the carbon mixing step and before the active material mixing step; After the active material mixing step, the electrolyte mixing step is further performed; The method for producing an electrode mixture according to claim 6,
8. Further comprising a binder mixing step of mixing a binder; The method for producing the electrode mixture according to claim 6.
9. a carbon mixing step of mixing conductive carbon, some of whose particles are in a paste form, with low-dispersion carbon under dry conditions; A method for producing a conductive assistant, comprising the steps of:
10. an oxidation process for forming a paste-like oxidized carbon having a hydrophilic portion in an amount of 10 mass% or more by oxidation; a conductive carbon preparation step of mixing the oxidation-treated carbon with particulate carbon having a hydrophilic portion content of less than 10 mass% of the total carbon, thereby compounding the particulate carbon with the oxidation-treated carbon to obtain the conductive carbon; The method for producing the conductive assistant according to claim 9,
11. The conductive carbon has a primary particle size of 12 nm or more and 34 nm or less; The method for producing the conductive assistant according to claim 9 or 10,
12. The low-dispersion carbon is a vapor-grown carbon fiber, a single-walled carbon nanotube, or a multi-walled carbon nanotube; The method for producing the conductive assistant according to claim 9 or 10,
Citation Information
Patent Citations
Working method of carbon nanotube
JP2004002156A
Cited By
Carbon nanotube conductive additive composite, electrode composition or electrode for battery comprising the same