Method for precipitating polyvinyl alcohol-based resin
By mixing PVA resin with alcohols having 1 to 6 carbon atoms at a 71% ratio, the method addresses the rigidity issue of PVA resin precipitates, enabling efficient and cost-effective recovery without cutting devices.
Patent Information
- Application Number
- JP2023056155
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing methods for recovering polyvinyl alcohol (PVA) resin from waste liquids result in rigid precipitates that require cutting devices for handling, leading to inefficiencies and increased costs.
A method involving mixing a PVA resin aqueous solution with a precipitating liquid composed mainly of alcohols with 1 to 6 carbon atoms, maintaining an alcohol ratio of 71% or more, to achieve flexible and easy-to-handle PVA resin precipitation.
The method enables high recovery rates of flexible PVA resin without the need for cutting devices, reducing handling costs and improving recovery efficiency.
Smart Images

Figure 2024143459000001 
Figure 2024143459000002 
Figure 2024143459000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for precipitating a polyvinyl alcohol-based resin, and more particularly to a method for precipitating a polyvinyl alcohol-based resin from an aqueous solution of the polyvinyl alcohol-based resin. [Background technology]
[0002] Polyvinyl alcohol resins (hereinafter, also referred to as PVA resins) have been widely used industrially as water-soluble synthetic polymers, and are widely utilized as raw materials for synthetic fibers or films, fiber processing agents, paper processing agents, adhesives, inorganic binders, polymerization stabilizers for polyvinyl chloride resins, etc.
[0003] Among these applications, PVA resins are preferably used as support materials when producing molded bodies using 3D printers, as cores when producing molded bodies with hollow parts, as dispersants when producing water-insoluble resin microparticles, etc. This is because by using PVA resins to produce support materials and cores and dispersing microparticles, it is possible to finally separate the molded body and microparticles from the support materials, cores, and dispersants by contacting them with water.
[0004] On the other hand, when the PVA resin is finally separated by contacting with water, a PVA resin waste liquid is generated. From the viewpoint of reducing the burden on the environment, it is required to remove the PVA resin from the waste liquid. In addition, if it becomes possible to recover the PVA resin from the waste liquid, the recovered PVA resin can be reused, which is also preferable in terms of cost.
[0005] As a method for recovering a PVA-based resin from an aqueous solution containing the PVA-based resin, for example, Patent Document 1 proposes a method in which a polyvinyl alcohol-based resin molded body containing an inorganic filler is dissolved in water, and then brought into contact with a precipitating liquid containing an alcohol having 3 to 6 carbon atoms as a main component to precipitate a polyvinyl alcohol-based resin containing an inorganic filler, and the precipitate is separated and recovered. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2014-218642 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, although the technology described in Patent Document 1 provides a high recovery rate of the PVA-based resin, the precipitated PVA-based resin is rigid, and therefore needs to be cut using a device having a cutting function, such as a cutter pump, when transporting the precipitated PVA-based resin, leaving room for improvement in terms of ease of recovery and cost.
[0008] Therefore, an object of the present invention is to provide a method for precipitating a PVA-based resin which has an excellent recovery rate and is flexible and easy to recover. [Means for solving the problem]
[0009] As a result of intensive research, the inventors have found that the above-mentioned problems can be solved by mixing an aqueous PVA-based resin solution with a precipitating liquid mainly composed of an alcohol having a specific carbon number, and by setting the alcohol ratio in the mixed solution within a predetermined range, thereby arriving at the present invention.
[0010] That is, the present invention has the following aspects 1 to 6.
[0011] A first aspect of the present invention is a method for precipitating a polyvinyl alcohol-based resin, comprising the steps of: This is a method for precipitating a polyvinyl alcohol-based resin, which comprises mixing an aqueous solution of a polyvinyl alcohol-based resin with a precipitating liquid mainly composed of at least one alcohol having 1, 2, or 4 to 6 carbon atoms, and adjusting the alcohol ratio in the mixed solution to 71% or more by mass, thereby precipitating a polyvinyl alcohol-based resin.
[0012] A second aspect of the present invention is the method for precipitating a polyvinyl alcohol-based resin according to the first aspect, In the method for precipitating a polyvinyl alcohol-based resin, the alcohol is at least one selected from the group consisting of methanol, ethanol, and tert-butyl alcohol.
[0013] A third aspect of the present invention is the method for precipitating a polyvinyl alcohol-based resin according to the first or second aspect, The polyvinyl alcohol-based resin is a polyvinyl alcohol-based resin containing a 1,2-diol structural unit in a side chain.
[0014] A fourth aspect of the present invention is a method for precipitating a polyvinyl alcohol-based resin according to any one of the first to third aspects, The method for precipitating a polyvinyl alcohol-based resin includes precipitating a polyvinyl alcohol-based resin having a hardness of 100 N or less or in a gel state.
[0015] A fifth aspect of the present invention is a method for precipitating a polyvinyl alcohol-based resin according to any one of the first to fourth aspects, The method for precipitating a polyvinyl alcohol-based resin is such that the alcohol ratio is 75% or more.
[0016] A sixth aspect of the present invention is The present invention is a method for recycling a polyvinyl alcohol-based resin, which comprises recovering a polyvinyl alcohol-based resin precipitated by the method for precipitating a polyvinyl alcohol-based resin according to any one of the first to fifth aspects. Effect of the Invention
[0017] According to the precipitation method of the present invention, the precipitated PVA-based resin is flexible, and therefore can be easily recovered without cutting using a device having a cutting function such as a cutter pump, and the PVA-based resin can be precipitated with a high recovery rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following embodiments of the present invention will be described in detail. The following description is merely an example of the present invention, and the present invention is not limited thereto. In this specification, the notation "~" indicates a numerical value including the numbers before and after it.
[0019] <Polyvinyl alcohol resin> First, the PVA resin used in this embodiment will be described. PVA resins are resins mainly composed of vinyl alcohol structural units, obtained by saponifying polyvinyl ester resins obtained by copolymerizing vinyl ester monomers, and are composed of vinyl alcohol structural units and vinyl ester structural units with a degree of saponification corresponding to the degree of saponification.
[0020] Examples of the vinyl ester monomer include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, and vinyl versatate. From an economical standpoint, vinyl acetate is preferably used.
[0021] The average degree of polymerization of the PVA resin used in this embodiment (measured in accordance with JIS K6726:1994) is preferably 350-1,000, more preferably 400-800, and even more preferably 450-600. If the average degree of polymerization is 350 or more, the resin has sufficient strength, and if the average degree of polymerization is 1000 or less, decomposition of the resin due to generation of shear heat during injection molding can be suppressed.
[0022] The saponification degree (average saponification degree measured in accordance with JIS K6726:1994) of the PVA resin used in the present embodiment is preferably 60 to 99.9 mol %, more preferably 80 to 99.5 mol %, and even more preferably 90 to 99.5 mol %. If the saponification degree is 60 mol % or more, the water solubility is improved, and if it is 99.9 mol % or less, melt molding becomes easy.
[0023] In addition to unmodified PVA resins, the PVA resins of this embodiment may be modified PVA resins obtained by copolymerizing various monomers during the production of polyvinyl ester resins and saponifying the copolymerized PVA resins, or various post-modified PVA resins obtained by introducing various functional groups into unmodified PVA resins through post-modification. Such modification may be performed within a range in which the water solubility of the PVA resin is not lost. In some cases, the modified PVA resin may be further post-modified.
[0024] Examples of monomers copolymerizable with vinyl ester monomers include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; hydroxyl-containing α-olefins such as 3-buten-1-ol, 4-penten-1-ol, 5-hexen-1-ol, and 3,4-dihydroxy-1-butene; acylated derivatives thereof; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, and itaconic acid; salts, monoesters, or dialkyl esters thereof; nitriles such as acrylonitrile and methacrylonitrile; and diacetone acrylate. amides such as ethylene sulfonic acid, allyl sulfonic acid, methallyl sulfonic acid, and other olefin sulfonic acids or their salts; alkyl vinyl ethers, dimethylallyl vinyl ketone, N-vinylpyrrolidone, vinyl chloride, vinyl ethylene carbonate, 2,2-dialkyl-4-vinyl-1,3-dioxolane, glycerin monoallyl ether, 3,4-diacetoxy-1-butene, and other vinyl compounds; substituted vinyl acetates such as isopropenyl acetate and 1-methoxyvinyl acetate; vinylidene chloride, 1,4-diacetoxy-2-butene, and vinylene carbonate.
[0025] In addition, examples of modified PVA-based resins into which functional groups have been introduced by a post-reaction include those having acetoacetyl groups by reaction with diketene, those having polyalkylene oxide groups by reaction with ethylene oxide, those having hydroxyalkyl groups by reaction with epoxy compounds, etc., and those obtained by reacting aldehyde compounds having various functional groups with PVA.
[0026] When the PVA-based resin is a modified PVA-based resin, the content (modification amount) of the modified species in the modified PVA-based resin, i.e., the constituent units derived from various monomers in the copolymer or the functional groups introduced by a post-reaction, cannot be generally determined because the characteristics vary greatly depending on the modified species, but is preferably in the range of 0.1 to 20 mol %, more preferably in the range of 0.5 to 12 mol %.
[0027] Among these various modified PVA resins, in the present embodiment, a PVA resin having a hydrophilic modified group is preferably used. Examples of the hydrophilic modified group include a hydroxyl group, a carboxyl group, and an amino group. In particular, from the viewpoint of water solubility, a PVA-based resin containing a structural unit having a 1,2-diol modifying group is preferred.
[0028] Among such PVA-based resins containing structural units having 1,2-diol modifying groups, it is preferable to use a PVA-based resin containing a 1,2-diol structural unit in the side chain, represented by the following general formula (1) (hereinafter, sometimes referred to as a "PVA-based resin containing a 1,2-diol structural unit in the side chain"). By using a PVA-based resin containing a 1,2-diol structural unit in the side chain, the melting point can be lowered, and the temperature range during melt molding can be expanded. The portions other than the 1,2-diol structural units are vinyl alcohol structural units and unsaponified vinyl ester structural units, like ordinary PVA resins.
[0029] [ka]
[0030] (In formula (1), R 1 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and X represents a single bond or a bonding chain.
[0031] In the above general formula (1), R 1 ~R 6 R each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. 1 ~R 6 are preferably all hydrogen atoms, but may be alkyl groups having 1 to 5 carbon atoms in an amount that does not significantly impair the resin properties. The alkyl group is not particularly limited, but examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, and pentyl groups, and the alkyl group may have a substituent such as a halogeno group, a hydroxyl group, an ester group, a carboxylic acid group, or a sulfonic acid group, as necessary.
[0032] Furthermore, X in the 1,2-diol structural unit represented by general formula (1) is most preferably a single bond in terms of thermal stability and stability under high temperature or acidic conditions, but may be a linking chain as long as it does not impair the effects of the present invention. Examples of such linking chains include hydrocarbons such as alkylene groups, alkenylene groups, alkynylene groups, phenylene groups, and naphthylene groups (these hydrocarbons may be substituted with halogen atoms such as fluorine atoms, chlorine atoms, and bromine atoms), as well as -O-, -(CH 2 O)m-, -(OCH 2 ) m -, -(CH 2 O) m CH 2 -, -CO-, -COCO-, -CO(CH 2 ) m CO-, -CO(C 6 H 4 )CO-, -S-, -CS-, -SO-, -SO 2 -, -NR-, -CONR-, -NRCO-, -CSNR-, -NRCS-, -NRNR-, -HPO 4 -, -Si(OR) 2-, -OSi (OR) 2 -, -OSi (OR) 2 O-, -Ti(OR) 2 -, -OTi(OR) 2 -, -OTi(OR) 2 Examples of such groups include -O-, -Al(OR)-, -OAl(OR)-, -OAl(OR)O-, and the like (each R is independently an arbitrary substituent, preferably a hydrogen atom or an alkyl group, and m is an integer of 1 to 5). Among these, from the viewpoint of stability during production or use, an alkylene group having 6 or less carbon atoms, particularly a methylene group, or -CH 2 OCH 2 - is preferred.
[0033] A particularly preferred structure in the 1,2-diol structural unit represented by the above general formula (1) is R 1 ~R 6 are all hydrogen atoms and X is a single bond, and is a structural unit represented by the following formula (1a). [ka]
[0034] When the PVA resin is a PVA resin containing a 1,2-diol structural unit in a side chain, the content (modification amount) of the structural unit represented by general formula (1) contained in the PVA resin containing a 1,2-diol structural unit in a side chain is preferably 0.1 to 10 mol%, more preferably 0.5 to 9 mol%, and even more preferably 1 to 8 mol%. When the content is 0.1 mol% or more, the effect of the 1,2-diol structure in the side chain is sufficiently obtained. Also, when the content is 10 mol% or less, the melt moldability is improved.
[0035] The content (modification amount) of 1,2-diol structural units in the PVA resin is the same as that of the PVA resin that has been completely saponified. 1It can be obtained from the H-NMR spectrum (solvent: DMSO-d6, internal standard: tetramethylsilane). Specifically, it may be calculated from the peak areas derived from the hydroxyl group protons, methine protons, and methylene protons in the 1,2-diol structural unit, the methylene protons in the main chain, the protons of the hydroxyl groups linked to the main chain, etc.
[0036] When a PVA resin having a 1,2-diol structural unit in a side chain is used, the saponification degree is preferably 80 to 99.9 mol%, more preferably 98.5 to 99.5 mol%. If the saponification degree is 80 mol% or more, the resin is less likely to decompose and deformation at high temperatures can be suppressed.
[0037] The PVA resin having a 1,2-diol structural unit in the side chain can be produced by a known production method. For example, (i) a method of saponifying a copolymer of a vinyl ester monomer and a compound represented by the following general formula (2), (ii) a method of saponifying and decarbonating a copolymer of a vinyl ester monomer and a compound represented by the following general formula (3), or (iii) a method of saponifying and deketalizing a copolymer of a vinyl ester monomer and a compound represented by the following general formula (4) is preferably used.
[0038] [ka]
[0039] (In formula (2), R 1 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, X represents a single bond or a bonding chain, R 7 and R 8 are each independently a hydrogen atom or R 9 -CO-(wherein, R 9 represents an alkyl group having 1 to 6 carbon atoms.
[0040] [ka]
[0041] (In formula (3), R 1 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and X represents a single bond or a bonding chain.
[0042] [ka]
[0043] (In formula (4), R 1 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, X represents a single bond or a bonding chain, R 10 and R 11 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms.
[0044] R in the above general formulas (2) to (4) 1 ~R 6 Specific examples and preferred examples of X are the same as those in the above formula (1). 7 and R 8 are each independently a hydrogen atom or R 9 -CO-(wherein, R 9 R is an alkyl group having 1 to 6 carbon atoms. 10 and R 11 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and specific and preferred examples of the alkyl group having 1 to 5 carbon atoms are the same as those in formula (1).
[0045] As for the methods (i), (ii), and (iii), for example, the methods described in JP-A-2006-95825 can be used. Among the above methods, the method (i) is preferred from the viewpoint of excellent copolymerization reactivity and industrial handling properties. In particular, the method (i) is preferred in which R 1 ~R 6 is a hydrogen atom, X is a single bond, R 7 , R 8 R 9 -CO-, R 9It is preferable to use 3,4-diacyloxy-1-butene, in which R is an alkyl group having 1 to 4 carbon atoms. 9 In particular, 3,4-diacetoxy-1-butene, in which R is a methyl group, is preferably used.
[0046] The PVA-based resin used in the present embodiment may be one type or a mixture of two or more types. In this case, combinations such as the above-mentioned unmodified PVAs, an unmodified PVA and a PVA-based resin having a structural unit represented by general formula (1), PVA-based resins having structural units represented by general formula (1) that differ in degree of saponification, average degree of polymerization, amount of modification, etc., an unmodified PVA, or a PVA-based resin having a structural unit represented by general formula (1) and another modified PVA-based resin may be used.
[0047] [Other ingredients] The PVA-based resin may contain lubricants such as magnesium stearate and magnesium 12-hydroxystearate as additives to the extent that the effects of the present invention are not impaired. Furthermore, the PVA-based resin may contain plasticizers such as glycerin, diglycerin, polyglycerin, ethylene oxide adducts of glycerin, and glycerin fatty acids, as necessary.
[0048] 《Precipitation method》 Next, the method for precipitating a PVA-based resin according to the present invention will be described. The precipitation method according to the present embodiment is characterized in that an aqueous solution of a PVA-based resin is mixed with a precipitating liquid mainly composed of at least one alcohol having 1, 2, or 4 to 6 carbon atoms, and the alcohol ratio in the mixed solution is set to 71% or more by mass ratio, thereby precipitating a PVA-based resin.
[0049] Here, the PVA-based resin aqueous solution is an aqueous solution containing the above-mentioned PVA-based resin. The PVA-based resin aqueous solution is obtained by contacting the PVA-based resin with water to dissolve the PVA-based resin (dissolving step).
[0050] The method for contacting the PVA resin with water is not particularly limited and may be any known method, such as normal pressure hot water dissolution method or high pressure hot water dissolution method. The water temperature in such a high-pressure hot water dissolution method is preferably 50 to 150° C., more preferably 80 to 120° C. If the water temperature is 50° C. or higher, the solubility of the PVA resin is improved, and if the water temperature is 150° C. or lower, decomposition of the PVA resin can be suppressed. The dissolution time is preferably 0.5 to 50 hours, more preferably 1 to 25 hours, and further preferably 1.5 to 5 hours. If the dissolution time is 0.5 hours or more, it is possible to prevent undissolved matter from remaining, and if it is 50 hours or less, it is economically preferable.
[0051] The concentration of the PVA resin aqueous solution obtained by the dissolving step varies somewhat depending on the type and dissolving apparatus, but is preferably 1 to 40% by mass, more preferably 5 to 30% by mass, and even more preferably 10 to 20% by mass. When the concentration of the PVA-based resin aqueous solution is 1% by mass or more, the number of repetitions of the recovery step described below can be reduced, which is efficient. On the other hand, when the concentration is 40% by mass or less, the solubility is increased, and the efficiency of the dissolution step can be sufficiently increased.
[0052] Next, the PVA-based resin aqueous solution obtained above is mixed with a precipitating solution mainly composed of at least one alcohol having a carbon number of 1, 2, or 4 to 6, and the alcohol ratio in the mixed solution is adjusted to 71% or more to precipitate the PVA-based resin (precipitating step). The PVA-based resin precipitated in this step is flexible, so that it is not necessary to cut it using a cutter pump or the like when transporting it, and it is easy to recover it.
[0053] The deposition solution used in this embodiment is mainly composed of at least one alcohol having 1, 2, or 4 to 6 carbon atoms, and the content thereof is preferably 50 to 100% by mass, more preferably 80 to 100% by mass, and further preferably 100% by mass. If the content is 50% or more, a sufficient deposition effect can be obtained. The components other than the alcohol are not particularly limited so long as they do not inhibit the precipitability. Usually, methyl acetate, ethyl acetate or water can be used, with water being particularly preferred.
[0054] By using a precipitating solution mainly composed of one or more alcohols with carbon numbers of 1, 2, and 4 to 6, the precipitated PVA resin becomes flexible, making it easy to recover without the need for a cutting device such as a cutter pump. This is thought to be because, influenced by the affinity between alcohol and water, the precipitated PVA resin contains a larger amount of water when using alcohols with carbon numbers of 1, 2, and 4 to 6, while when using alcohol with carbon number 3, a larger amount of water is expelled from the precipitated PVA resin. Examples of the alcohol having 1, 2, or 4 to 6 carbon atoms include methanol, ethanol, tert-butyl alcohol, n-butyl alcohol, and sec-butyl alcohol. Among these, from the viewpoint of low adhesion of the precipitated PVA-based resin, one or more selected from the group consisting of methanol, ethanol, and tert-butyl alcohol are preferred. The alcohol may be used alone or in combination of two or more.
[0055] The method for mixing the above-mentioned precipitating solution and the aqueous PVA resin solution is not particularly limited, and can be carried out by a known method. For example, there may be mentioned a method of adding a precipitating liquid to an aqueous PVA-based resin solution, a method of adding a PVA-based resin to a precipitating liquid, a method of mixing an aqueous PVA-based resin solution and a precipitating liquid all at once, and from the viewpoint of efficiently precipitating the PVA-based resin, a method of gradually adding an aqueous PVA-based resin solution to a precipitating liquid is preferred.
[0056] A typical mixing method is to fill the precipitation liquid in a tank and add the PVA-based resin aqueous solution to the circulating precipitation liquid little by little. The amount of the PVA-based resin aqueous solution added is preferably 0.1 to 3.0 kg / min, more preferably 0.3 to 1.5 kg / min. The PVA-based resin precipitates from the PVA-based resin aqueous solution added to the precipitation liquid, and a mixed solution and precipitated PVA-based resin are obtained.
[0057] The liquid temperature when mixing the PVA-based resin aqueous solution and the precipitation liquid is preferably adjusted to 10 to 30° C., more preferably 20 to 25° C. By keeping the temperature during mixing within the above range, volatilization of alcohol can be suppressed.
[0058] In the precipitation method according to the present embodiment, the PVA-based resin aqueous solution and the precipitation liquid are mixed to make the alcohol ratio of the mixed solution (mass of alcohol / mass of mixed solution) 71% or more. By making the alcohol ratio (mass ratio) in the mixed solution 71% or more, the recovery rate is improved. The alcohol ratio in the mixed solution is preferably 75% or more, more preferably 80% or more, and even more preferably 85% or more. From the viewpoint of the amount recovered relative to the amount charged, the alcohol ratio in the mixed solution is preferably 98% or less, more preferably 95% or less, and particularly preferably 90% or less.
[0059] The PVA-based resin precipitated by the precipitation method according to the present embodiment has low hardness and is flexible. Specifically, the PVA-based resin precipitated by the precipitation method according to the present embodiment preferably has a hardness of 100N or less, or is in a gel state. By using a PVA-based resin having a hardness of 100N or less, or in a gel state, there is no need to cut the precipitated PVA-based resin using a cutter pump or the like when transporting it, and recovery is easy. In addition, since equipment such as a cutter pump is not required, costs can be reduced. The hardness of the PVA resin is more preferably 80N or less, and further preferably 50N or less. Here, the hardness of the precipitated PVA-based resin can be measured by the following procedure. The PVA-based resin precipitated by the above-mentioned precipitation method is filtered through a mesh, and three samples of 2 cm x 2 cm in size are selected. The hardness at which the PVA-based resin cracks is measured using a tablet hardness tester (e.g., PORTABLE CHECKER PC-30, manufactured by Okada Seiko Co., Ltd.), and the average value is calculated. In this specification, the term "gel-like" refers to an elastic semi-solid substance.
[0060] In this embodiment, the ratio (recovery rate) of the mass of the PVA-based resin precipitated by the above-mentioned precipitation method to the mass of the PVA-based resin in the aqueous PVA-based resin solution is preferably 50% or more. If the recovery rate is 50% or more, the PVA-based resin in the solution can be sufficiently recovered. The higher the recovery rate, the more preferable it is, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 85% or more, with the upper limit being 100%. Here, the recovery rate can be calculated by the following method. The PVA-based resin precipitated by the above precipitation method is dried for 3 hours at 140° C. using a dryer (e.g., SPH-102 manufactured by ESPEC Co., Ltd.). The mass of the dried PVA-based resin is measured, and the recovery rate is calculated based on the following formula. Recovery rate (%) = mass of PVA-based resin after drying (g) / mass of PVA-based resin (g) × 100
[0061] How to recycle The recycling method according to this embodiment includes recovering the PVA-based resin precipitated by the precipitation method according to this embodiment (recovery step).
[0062] The method for recovering the PVA-based resin precipitated by the precipitation method according to the present embodiment is not particularly limited and can be performed by a known method. Specifically, for example, the precipitated PVA-based resin can be filtered from the mixed solution, centrifuged, and then dried by a vibration fluidized dryer or a vacuum dryer to obtain the PVA-based resin. The drying time is preferably 2 to 24 hours, more preferably 3 to 15 hours, and the drying temperature is not particularly limited, but is preferably 150° C. or lower. EXAMPLES
[0063] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention. In the examples, "parts" and "%" are by weight unless otherwise specified.
[0064] (Example 1) <Production of PVA-based resin> A PVA-based resin (a) having a 1,2-diol structural unit represented by the general formula (1a) (saponification degree: 99.2 mol%, degree of polymerization: 350, content of 1,2-diol structural unit: 6 mol%) was pelletized by melt extrusion using a twin-screw extruder. Such pellets are cylindrical with a total length of 3 mm and an outer diameter of 2 mm.
[0065] (A) Dissolution step Water was put into a reaction vessel equipped with a stirring blade, and the above-mentioned pellets were added while stirring at 500 rpm. After raising the temperature to 85°C, the above-mentioned pellets were completely dissolved in water to obtain an aqueous solution of PVA-based resin (a) of about 27% by mass. Next, the solid content was calculated by the volatile matter method (mass of solid after drying / mass of aqueous solution × 100), and a 25% aqueous solution of PVA-based resin (a) was adjusted by adding water.
[0066] (B) Precipitation step To 100 g of a precipitation solution composed of methanol, 20 g of a 25% by mass aqueous solution of PVA-based resin (a) obtained in the above dissolution step was gradually added, and the mixture was stirred for 10 minutes to prepare a mixed solution. Precipitation of PVA-based resin (a') was confirmed in the mixed solution.
[0067] <<Evaluation method>> <Measurement of hardness of precipitated PVA-based resin> The PVA-based resin (a') precipitated in the above precipitation step was filtered with a mesh. Next, a sample with a size of 2 cm × 2 cm was selected, and the hardness at which the PVA-based resin (a') cracked was measured using a tablet hardness tester (PORTABLE CHECKER PC-30, manufactured by Okada Seiko Co., Ltd.). The average value of three-point measurements was calculated, and the results are shown in Table 1.
[0068] <Recovery rate> The PVA-based resin (a') obtained in the above precipitation step was dried at 140°C for 3 hours using an explosion-proof dryer (SPH-102, manufactured by ESPEC). The mass of the dried PVA-based resin (a') was measured, and the recovery rate was calculated based on the following formula. The results are shown in Table 1. Recovery rate (%) = mass (g) of PVA resin (a') after drying / mass (g) of PVA resin (a) before use × 100
[0069] (Examples 2 to 5) Evaluation was performed in the same manner as in Example 1, except that the type of alcohol in Example 1 was changed to one shown in Table 1. The results are shown in Table 1. In addition, in the case where the precipitated PVA-based resin (a') was in a gel state, the hardness was not measured.
[0070] Example 6 The evaluation was carried out in the same manner as in Example 1, except that the amount of alcohol in Example 1 was changed to 50 g. The results are shown in Table 1.
[0071] Example 7 The evaluation was carried out in the same manner as in Example 1, except that the alcohol in Example 1 was changed to ethanol and the amount of alcohol was changed to 50 g. The results are shown in Table 1.
[0072] (Comparative Examples 1 and 2) Evaluation was performed in the same manner as in Example 1, except that the type of alcohol in Example 1 was changed to one shown in Table 1. The results are shown in Table 1.
[0073] Comparative Example 3 The evaluation was carried out in the same manner as in Example 1, except that the amount of alcohol in Example 1 was changed to 30 g. The results are shown in Table 1.
[0074] Comparative Example 4 In Example 2, the alcohol was changed to ethanol, and the amount of alcohol was changed to 20 g, but the same procedures as in Example 1 were followed and evaluation was performed. The results are shown in Table 1.
[0075] [Table 1]
[0076] In Examples 1 to 7, in which an alcohol having 1, 2 or 4 carbon atoms was used as the precipitating solution and the alcohol ratio in the mixed solution was 71% or more, the hardness of the precipitate was 55N or less, and the recovery rate was high at 61% or more. It is presumed that the same effect can be obtained with alcohol having 5 or 6 carbon atoms. This is because, while alcohol having 3 carbon atoms is likely to expel water from the precipitated PVA-based resin due to its affinity with water, and the hardness is likely to increase, alcohol having a carbon number greater than that contains a moderate amount of moisture in the precipitated PVA-based resin, and therefore the hardness is thought to be lower. On the other hand, in Comparative Examples 1 and 2, in which IPA or nPA was used as the precipitation solution, the hardness of the precipitate was higher than that of the Examples. Also, in Comparative Examples 3 and 4, in which the alcohol ratio in the mixed solution was less than 70%, the recovery rate was lower than that of the Examples. [Industrial Applicability]
[0077] The PVA-based precipitation method of the present invention has a high recovery rate and, since the precipitated PVA-based resin has low hardness, a cutter pump or the like is not required during recovery, and recovery can be easily performed.
Claims
1. A method for precipitating a polyvinyl alcohol-based resin, comprising the steps of: The method for precipitating a polyvinyl alcohol-based resin comprises mixing an aqueous solution of a polyvinyl alcohol-based resin with a precipitating liquid mainly composed of one or more alcohols having 1, 2, or 4 to 6 carbon atoms, and adjusting the alcohol ratio in the mixed solution to 71% or more by mass ratio, thereby precipitating a polyvinyl alcohol-based resin.
2. 2. The method for precipitating a polyvinyl alcohol-based resin according to claim 1, wherein the alcohol is at least one selected from the group consisting of methanol, ethanol, and tert-butyl alcohol.
3. 2. The method for precipitating a polyvinyl alcohol-based resin according to claim 1, wherein the polyvinyl alcohol-based resin contains a 1,2-diol structural unit in a side chain.
4. 2. The method for precipitating a polyvinyl alcohol-based resin according to claim 1, wherein the polyvinyl alcohol-based resin is precipitated having a hardness of 100 N or less or in a gel state.
5. 2. The method for precipitating a polyvinyl alcohol-based resin according to claim 1, wherein the alcohol ratio is 75% or more.
6. A method for recycling a polyvinyl alcohol-based resin, comprising recovering the polyvinyl alcohol-based resin precipitated by the method for precipitating a polyvinyl alcohol-based resin according to any one of claims 1 to 5.
Citation Information
Patent Citations
Method of manufacturing recycled raw material from polyvinyl alcohol resin molded product
JP2014218642A