Epoxy resin composition

The novel epoxy resin composition, comprising specific epoxy resins A, B, and C, addresses handling and mechanical property challenges in fiber-reinforced composites by enhancing pot life and mechanical properties, especially glass transition temperature and flexural modulus.

JP2024143493AActive Publication Date: 2024-10-11TEIJIN LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023056209
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Conventional epoxy resin compositions used in fiber-reinforced composite materials face challenges in achieving good handling properties, pot life, and high mechanical properties, particularly in terms of glass transition temperature and flexural modulus.

Method used

A novel epoxy resin composition comprising specific combinations of epoxy resins A, B, and C, along with a hardening agent, optimized in terms of chemical structure and content ratios, to enhance handling, pot life, and mechanical properties.

Benefits of technology

The composition exhibits improved handling properties, extended pot life, and superior mechanical properties, including high glass transition temperature and flexural modulus, particularly when using biomass-derived epoxy resins B and C.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143493000001
    Figure 2024143493000001
  • Figure 2024143493000002
    Figure 2024143493000002
  • Figure 2024143493000003
    Figure 2024143493000003
Patent Text Reader

Abstract

To provide an epoxy resin composition which has good handleability and pot life and exhibits a relatively good flexural modulus when cured.SOLUTION: The epoxy resin composition contains an epoxy resin A represented by the following chemical formula 1, an epoxy resin B represented by a specific formula, an epoxy resin C represented by a specific formula, and a curing agent. (In the formula, R1-R4 each independently represent one selected from the group consisting of a hydrogen atom, an aliphatic hydrocarbon group, an alicyclic hydrocarbon group and a halogen atom; and X represents one selected from -CH2-, -O-, -S-, -CO-, -C(=O)O-, -O-C(=O)-, -NHCO-, -CONH- and -SO2-). The content of the epoxy resin A is preferably 50-90 mass% based on the total mass of epoxy resins contained in the epoxy resin composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an epoxy resin composition, and in particular to an epoxy resin composition for use in a fiber-reinforced composite material comprising a fiber-reinforced substrate. [Background technology]

[0002] Fiber-reinforced resin composite materials (also called fiber-reinforced composite materials or composites) are lightweight, strong, and rigid, and are therefore used in a wide range of fields, including sports and leisure applications such as fishing rods and golf shafts, and industrial applications such as automobiles and aircraft.

[0003] Fiber-reinforced resin composite materials can be obtained, for example, by a method in which a fiber-reinforced substrate is impregnated with resin in advance and formed into a sheet-like prepreg (intermediate substrate), which is then molded.Fiber-reinforced composite materials can also be obtained by a method in which a fiber-reinforced substrate placed in a mold is impregnated with liquid resin (i.e., uncured curable resin or molten thermoplastic resin, for example), and then cured or solidified to obtain a fiber-reinforced resin composite material (resin transfer molding method, RTM method).

[0004] Epoxy resin compositions are preferably used as a constituent component of fiber-reinforced composite materials.

[0005] Patent Document 1 describes an epoxy resin composition containing an aliphatic epoxy resin having a specific chemical structure and an epoxy resin different from the epoxy resin. This document also describes a prepreg containing the epoxy resin composition and a reinforcing material.

[0006] Patent Document 2 describes an epoxy resin composition having specific physical properties, which is obtained by blending a di- or higher functional aromatic epoxy resin with an aromatic amine compound and / or an alicyclic amine compound. This document describes the prepreg method, RTM method, etc. as methods for producing fiber-reinforced composite materials.

[0007] Patent Document 3 describes a liquid resin composition for compression molding that contains an aliphatic epoxy compound, an epoxy compound having an aromatic ring in the molecule, a nitrogen-containing heterocyclic compound, and an inorganic filler. This document claims to provide a liquid resin composition for compression molding that can suppress the occurrence of warping of semiconductor wafers, and an electronic component device using the same.

[0008] Patent Document 4 describes a crosslinker composition for resins, which contains an epoxy resin having a chain polyhydric alcohol skeleton having a specific chemical structure and an epoxy resin having a glycerin skeleton or polyglycerin skeleton having a specific chemical structure.

[0009] Patent Document 5 describes a curable resin composition containing an epoxy resin having a specific structure and / or an epoxy (meth)acrylate having a specific structure. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2006-83216 A [Patent Document 2] WO 00 / 53654 [Patent Document 3] International Publication No. 2018 / 221682 [Patent Document 4] JP 2017-66343 A [Patent Document 5] JP 2023-19448 A Summary of the Invention [Problem to be solved by the invention]

[0011] When an epoxy resin composition is used for a fiber-reinforced composite material, good handling properties and pot life are required, and the molded product obtained by curing the epoxy resin composition is also required to have high physical properties (especially high mechanical properties). In addition, it is preferable that the epoxy resin composition used for the fiber-reinforced composite material has a relatively high glass transition temperature.

[0012] With conventional epoxy resin compositions, it has not been easy to satisfy these requirements.

[0013] It is an object of the present invention to provide an epoxy resin composition which has good handleability and pot life, and which gives molded articles having excellent mechanical properties upon curing. It is a further object of the present invention to provide an epoxy resin composition which has good handleability and pot life, which exhibits a relatively high glass transition temperature, and which gives molded articles having excellent mechanical properties upon curing. [Means for solving the problem]

[0014] The object of the present invention can be achieved by the following aspects of the present invention. <Aspect 1> Epoxy resin A represented by the following chemical formula 1, Epoxy resin B represented by the following chemical formula 2, Epoxy resin C represented by the following chemical formula 3, and Hardener Epoxy resin composition comprising: [ka] (In formula 1, R1 to R4 each independently represent one selected from the group consisting of a hydrogen atom, an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, and a halogen atom, and X represents one selected from -CH2-, -O-, -S-, -CO-, -C(=O)O-, -OC(=O)-, -NHCO-, -CONH-, and -SO2-.) [ka] (In formula 2, R5 and R6 each independently represent an aliphatic hydrocarbon group having 4 to 12 carbon atoms.) [ka] (In formula 3, m is an integer of 0 to 20, R 10are each independently a hydrogen atom or a glycidyl group represented by the following chemical formula 4, and R 10 At least two of the above are glycidyl groups represented by the following chemical formula 4. [ka] <Aspect 2> The epoxy resin composition according to aspect 1, wherein the epoxy resin A is 50 to 90 mass% and / or the total of the epoxy resins B and C is 10 to 50 mass%, based on the total mass of the epoxy resins contained in the epoxy resin composition. <Aspect 3> 3. The epoxy resin composition according to aspect 1 or 2, wherein a ratio Mb / Mc of a content Mb(g) of the epoxy resin B in the epoxy resin composition to a content Mc(g) of the epoxy resin C in the epoxy resin composition is 0.80 to 3.5. <Aspect 4> The epoxy resin composition according to any one of Aspects 1 to 3, wherein at least one of the epoxy resin B and the epoxy resin C is a biomass-derived epoxy resin. <Aspect 5> The epoxy resin composition according to any one of Aspects 1 to 4, wherein the epoxy resin A is one or a combination of two or more selected from the group consisting of tetraglycidyl-4,4'-diaminodiphenyl ether, tetraglycidyl-4,4'-diaminodiphenylmethane, tetraglycidyl-3,4'-diaminodiphenyl ether, and tetraglycidyl-3,3'-diaminodiphenylmethane. <Aspect 6> The epoxy resin composition according to any one of aspects 1 to 5, wherein the epoxy resin B is an epoxy resin represented by the following chemical formula 2-1: [ka] <Aspect 7> The epoxy resin composition according to any one of aspects 1 to 6, wherein the epoxy resin C is an epoxy resin represented by the following chemical formula 3-1: [ka] <Aspect 8> A cured resin product obtained by curing the epoxy resin composition according to any one of aspects 1 to 7. <Aspect 9> A fiber-reinforced composite material comprising a cured resin obtained by curing the epoxy resin composition according to any one of aspects 1 to 7, and a fiber-reinforced substrate. <Aspect 10> 10. The fiber-reinforced composite material of embodiment 9, wherein the fiber-reinforced substrate is a carbon fiber-reinforced substrate. <Aspect 11> forming an intermediate composite comprising a fiber-reinforced substrate and the epoxy resin composition according to any one of aspects 1 to 7; and curing the intermediate composite to form a fiber reinforced composite material; A method for producing a fiber-reinforced composite material, comprising: <Aspect 12> Impregnating a fiber-reinforced substrate placed in a mold with the epoxy resin composition according to any one of aspects 1 to 7; and curing the fiber-reinforced substrate impregnated with the epoxy resin composition under heating to form a fiber-reinforced composite material; 12. A method for producing the fiber-reinforced composite material of claim 11, comprising: Effect of the Invention

[0015] According to the present invention, there is provided an epoxy resin composition which has good handleability and pot life, and which gives molded articles which are excellent in mechanical properties upon curing.

[0016] Furthermore, according to the present invention, there can be provided an epoxy resin composition which has good handleability and pot life, exhibits a relatively high glass transition temperature, and gives molded articles which are excellent in mechanical properties upon curing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] <<Epoxy resin composition>> The epoxy resin composition according to the present invention comprises: Epoxy resin A represented by the following chemical formula 1, Epoxy resin B represented by the following chemical formula 2, Epoxy resin C represented by the following chemical formula 3, and Hardener Contains:

[0018] As a result of extensive investigations, the present inventors have found that an epoxy resin composition containing three types of epoxy resins having the following specific chemical structures can provide desired excellent properties. More specifically, the epoxy resin composition according to the present invention has a relatively low viscosity at 100°C and is therefore easy to handle, and has a relatively high curing initiation temperature and is therefore excellent in pot life. Furthermore, the epoxy resin composition according to the present invention provides molded products obtained by curing with excellent mechanical properties, and in particular, exhibits a relatively good flexural modulus. Furthermore, the epoxy resin composition according to the present invention can exhibit a relatively high glass transition temperature.

[0019] Without intending to be limited by theory, it is believed that the present invention uses three specific types of epoxy resin compositions which differ from each other in terms of the number of epoxy groups in the molecule, the presence or absence of aromatic rings, the length of the carbon chain, the number of oxygen atoms, etc., so that the epoxy resin composition can have good physical properties in terms of viscosity, curing initiation temperature, and glass transition temperature, and also can have a relatively high flexural modulus for the molded product obtained by curing.

[0020] <Epoxy resin A> Epoxy resin A is represented by the following chemical formula 1. [ka] (In formula 1, R1 to R4 each independently represent one selected from the group consisting of a hydrogen atom, an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, and a halogen atom, and X represents one selected from -CH2-, -O-, -S-, -CO-, -C(=O)O-, -OC(=O)-, -NHCO-, -CONH-, and -SO2-.)

[0021] The epoxy resin composition according to the present disclosure may contain, as the epoxy resin A, a plurality of types of compounds corresponding to the above formula 1.

[0022] In the above formula 1, R1 to R4 preferably each independently represent one selected from the group consisting of a hydrogen atom and an aliphatic hydrocarbon group, and particularly preferably all are a hydrogen atom.

[0023] When at least one of R1 to R4 is an aliphatic hydrocarbon group, the aliphatic hydrocarbon group may be an alkyl group having 1 to 6 carbon atoms. When at least one of R1 to R4 is an aliphatic hydrocarbon group, it is preferably an alkyl group having 1 to 4 carbon atoms, and more preferably a methyl group or an ethyl group. When at least one of R1 to R4 is an alicyclic hydrocarbon group, this alicyclic hydrocarbon group may have 3 to 12 carbon atoms, and more preferably 6 to 10 carbon atoms.

[0024] In the above formula 1, X is preferably -CH2- or -O-.

[0025] The content of the epoxy resin A in the epoxy resin composition may be 35 to 90 mass % based on the total mass of the epoxy resins contained in the epoxy resin composition.

[0026] The epoxy resin A is preferably 40 to 90 mass%, 40 to 85 mass%, 50 to 90 mass%, 50 to 85 mass%, more than 50 mass% and 85 mass% or less, or even 60 to 82 mass%, based on the total mass of the epoxy resins contained in the epoxy resin composition.

[0027] When the epoxy resin A is 40% by mass or more, or even more than 50% by mass, particularly 60% by mass or more, based on the total mass of the epoxy resins contained in the epoxy resin composition, a higher glass transition temperature can be obtained.

[0028] When the epoxy resin A is 85 mass % or less, particularly 82 mass % or less, based on the total mass of the epoxy resins contained in the epoxy resin composition, the curing initiation temperature does not become excessively high, and therefore the curing efficiency during the curing treatment of the epoxy resin composition can be improved.

[0029] In a particularly preferred embodiment of the present disclosure, the epoxy resin A is one or a combination of two or more selected from the group consisting of tetraglycidyl-4,4'-diaminodiphenyl ether, tetraglycidyl-4,4'-diaminodiphenylmethane, tetraglycidyl-3,4'-diaminodiphenyl ether, and tetraglycidyl-3,3'-diaminodiphenylmethane.

[0030] Specific examples of the epoxy resin A include compounds represented by the following formula 1-1 or 1-2.

[0031] [ka]

[0032] In one preferred embodiment, the epoxy resin composition contains, as the epoxy resin A, both of the compound represented by the above formula 1-1 and the compound represented by the formula 1-2.

[0033] When the epoxy resin composition contains both the compound represented by Formula 1-1 and the compound represented by Formula 1-2, the content of the compound represented by Formula 1-1 may be 60 to 90 mass %, and preferably 65 to 80 mass %, based on the total mass of the epoxy resin A.

[0034] When the epoxy resin composition contains both the compound represented by Formula 1-1 and the compound represented by Formula 1-2, the content of the compound represented by Formula 1-2 may be 10 to 40 mass %, and preferably 20 to 35 mass %, based on the total mass of the epoxy resin A.

[0035] <Epoxy resin B> Epoxy resin B is represented by the following chemical formula 2. [ka] (In formula 2, R5 and R6 each independently represent an aliphatic hydrocarbon group having 4 to 12 carbon atoms.)

[0036] R5 and R6 are each independently preferably an aliphatic hydrocarbon group having 5 to 10 carbon atoms, and more preferably an aliphatic hydrocarbon group having 6 to 8 carbon atoms. R5 may be an alkylene group, and R6 may be an alkyl group.

[0037] A specific example of a preferable epoxy resin B is an epoxy resin represented by the following chemical formula 2-1. [ka]

[0038] The content of epoxy resin B in the epoxy resin composition is preferably 2 to 35 mass%, more preferably 6 to 28 mass%, and particularly preferably 8 to 22 mass%, or even 12 to 22 mass%, based on the total mass of the epoxy resins contained in the epoxy resin composition.

[0039] <Epoxy resin C> Epoxy resin C is represented by the following chemical formula 3. [ka] (In formula 3, m is an integer of 0 to 20, R 10 are each independently a hydrogen atom or a glycidyl group represented by the following chemical formula 4, and R 10 At least two of the above are glycidyl groups represented by the following chemical formula 4. [ka]

[0040] m is preferably an integer from 1 to 10, more preferably an integer from 2 to 6 or even more preferably an integer from 2 to 4, and particularly preferably, m = 3.

[0041] Particularly preferably, 4 of R7 to R 10 are glycidyl groups represented by the above formula 4. That is, it is particularly preferable that the compound represented by formula 3 is a compound containing four glycidyl groups.

[0042] Epoxy resin C is particularly preferably an epoxy resin represented by the following chemical formula 3-1. [Chemical formula]

[0043] The content of epoxy resin C in the epoxy resin composition is preferably 2 to 35% by mass, more preferably 6 to 28% by mass, particularly preferably 8 to 18% by mass or even more preferably 10 to 18% by mass, based on the total mass of the epoxy resins contained in the epoxy resin composition.

[0044] [Regarding Component B and Component C]

[0045] The total of epoxy resins B and C may be 5 to 65% by mass based on the total mass of the epoxy resins contained in the epoxy resin composition.

[0046] The total of epoxy resins B and C is preferably 10 to 50% by mass, more preferably 15 to 45% by mass or even more preferably 16 to 45% by mass, particularly preferably 18 to 42% by mass or even more preferably 20 to 40% by mass, based on the total mass of the epoxy resins contained in the epoxy resin composition. Since both epoxy resin B and epoxy resin C can be provided as biomass-derived components, from the viewpoint of obtaining a composition with even better environmental compatibility, it is preferable that the contents of epoxy resin B and C are relatively high.

[0047] The ratio Mb / Mc of the content Mb(g) of the epoxy resin B in the epoxy resin composition to the content Mc(g) of the epoxy resin C in the epoxy resin composition may be 0.2 to 5.0.

[0048] This ratio Mb / Mc is preferably from 0.4 to 4.5, more preferably from 0.6 to 4.0, and particularly preferably from 0.8 to 3.5.

[0049] <Biomass-derived ingredients> In one embodiment according to the present disclosure, at least one of epoxy resin B and epoxy resin C is a biomass-derived epoxy resin.

[0050] Both epoxy resin B and epoxy resin C can be provided as biomass-derived components. Specifically, for example, component B can be produced from cashew nut shell oil, and component C can be produced from palm oil. Commercially available biomass-derived products include Cardolite (trademark) NC-514S (manufactured by Cardolite Corporation) for component B, and Denacol EX-512 (manufactured by Nagase ChemteX Corporation) for component C.

[0051] According to the present invention, by using epoxy resin B and epoxy resin C in combination, relatively good properties can be obtained for the same amount, compared with the case where either epoxy resin B or epoxy resin C is contained alone. Therefore, according to the present invention, the proportion of the biomass-derived component in the epoxy resin composition can be increased while maintaining the good performance of the epoxy resin composition. By relatively increasing the amount of the biomass-derived component contained in the epoxy resin composition, it is possible to provide an epoxy resin composition and a product using the same that are more compatible with the environment.

[0052] <Hardening agent> The epoxy resin composition according to the present disclosure contains a curing agent. As the curing agent, a known curing agent can be used. In particular, it is preferable to use an amine-based curing agent as the curing agent from the viewpoint of mechanical properties of the cured product.

[0053] Amine-based hardeners include ethylenediamine, 4,4'-diamino-3,3'-diisopropyl-5,5'-dimethyldiphenylmethane, 1,2-diaminopropane, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, diethylenetriamine, dipropylenetriamine, triethylenetetramine, tripropylenetetramine, tetraethylenepentamine, hexamethylenediamine, iminobispropylamine, bis(hexamethylene)triamine, 1,3,6-trisaminomethylhexane, trimethylhexamethylenediamine, polyetherdiamine, diethylaminopropylamine, dimeric acid ester of polyethyleneimine, dicyandiamide, tetramethylguanidine, adipic acid hydrazide, menthenediamine, 1,4-cyclohexanediamine, isophoronediamine, bis(aminomethyl)norbornane, bis(4-aminocyclohexyl)methane , N-aminoethylpiperazine, diaminodicyclohexylmethane, bisaminomethylcyclohexane, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro(5.5)undecane, norbornene diamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, diaminodiethyldiphenylmethane, and other amine compounds having a primary amine in the molecule; chain polyamine compounds such as 1,2-propanediamine and 1,3-butanediamine; and amine compounds having a secondary amine in the molecule such as N-methylpiperazine, morpholine, piperidine, N-methylaniline, N-ethylaniline, N-ethyltoluidine, diphenylamine, hydroxyphenylglycine, and N-methylaminophenol sulfate. These may be used alone or in combination of two or more.

[0054] The curing agent is preferably 4,4'-diamino-3,3'-diisopropyl-5,5'-dimethyldiphenylmethane (M-MIPA).

[0055] The content of the curing agent may be 40 to 80 parts by weight, or even 45 to 70 parts by weight, based on 100 parts by weight of the total epoxy resin in the epoxy resin composition.

[0056] The total amount of curing agent contained in the epoxy resin composition that can be used in the present invention is particularly an amount suitable for curing all of the epoxy resins blended in the composition, and can be appropriately adjusted depending on the types of epoxy resins and curing agents used, etc.

[0057] Specifically, for example, the ratio of the number of epoxy groups derived from the epoxy resin in the composition to the number of active hydrogens derived from the curing agent is preferably 0.7 to 1.3.

[0058] <Other ingredients> The epoxy resin composition according to the present disclosure may contain other components in addition to the above-mentioned epoxy resin and curing agent, such as a curing accelerator, other epoxy resins, colorants, fillers, various additives, etc. In addition, in order to improve the impact resistance of the matrix resin, the epoxy resin composition may contain a thermoplastic resin component or resin particles (e.g., core-shell rubber particles) as other components. These other components are preferably present in a total amount of 20% by mass or less, 10% by mass or less, 5% by mass or less, or 1% by mass or less, based on the total mass of the epoxy resin composition.

[0059] (Cure accelerator) The epoxy resin composition may also contain an accelerator (curing accelerator).

[0060] The curing accelerator includes urea compounds, particularly aromatic urea compounds (aromatic urea compounds). Specific examples thereof include 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 1,1'-(4-methyl-1,3-phenylene)bis(3,3-dimethylurea), N-phenyl-N',N'-dimethylurea, N-(4-chlorophenyl)-N',N'-dimethylurea, N-(3,4-dichlorophenyl)-N',N'-dimethylurea, N-(3-chloro-4-methylphenyl)-N',N'-dimethylurea, N-(3-chloro-4-ethylphenyl)-N',N'-dimethylurea, N-(3-chloro-4-methoxyphenyl)-N',N'-dimethylurea, N-(4-methyl-3-nitrophenyl)-N',N'-dimethylurea, 2,4-bis(N',N'-dimethylureido)toluene, and methylene-bis(p-N',N'-dimethylureidophenyl). Among these, 3-(3,4-dichlorophenyl)-1,1-dimethylurea and 1,1'-(4-methyl-1,3-phenylene)bis(3,3-dimethylurea) are preferred. These may be used alone or in combination of two or more.

[0061] When a curing accelerator is contained, the content thereof may be 1 to 10 parts by weight, or even 2 to 6 parts by weight, based on 100 parts by weight of the total epoxy resin in the epoxy resin composition.

[0062] (core-shell rubber particles) The epoxy resin composition according to the present disclosure may contain core-shell rubber particles (CSR) for additional toughness.

[0063] Such core-shell rubber particles include particles having a polybutadiene core and a tetraglycidyl-4,4'-diaminodiphenylmethane shell. Specific commercially available products include Kane Ace (registered trademark) MX series products from Kaneka Corporation.

[0064] When the core-shell rubber particles are contained, the content thereof may be 1 to 15 parts by mass, 1 to 10 parts by mass, or even 2 to 6 parts by mass, based on 100 parts by mass of the total epoxy resin in the epoxy resin composition.

[0065] (Other epoxy resins) The epoxy resin composition according to the present disclosure may contain other epoxy resins other than the above-mentioned epoxy resins A to C, so long as the effects of the present invention are not impaired. The other epoxy resins are preferably contained in an amount of 10 mass % or less, 5 mass % or less, or 3 mass % or less, based on the total mass of the epoxy resin composition. Examples of the other epoxy resins include DGEBA and GOT. [ka]

[0066] When an epoxy resin other than the epoxy resins A to C is contained, the content thereof may be 0.5 to 8 parts by weight, or even 1 to 4 parts by weight, based on 100 parts by weight of the total epoxy resins in the epoxy resin composition.

[0067] <Composition> In one embodiment according to the present disclosure, the epoxy resin composition comprises the following components in the following amounts per 100 parts by weight of the total epoxy resin in the epoxy resin composition: 35 parts by weight to 90 parts by weight of epoxy resin A 2 parts by weight to 35 parts by weight of epoxy resin B 2 to 35 parts by weight of epoxy resin C 0 to 10 parts by weight of other epoxy resin 0 to 10 parts by weight of core-shell rubber particles 40 parts by weight to 80 parts by weight of hardener.

[0068] In a preferred embodiment of the present disclosure, the epoxy resin composition comprises the following components in the following amounts relative to the total mass of the epoxy resin composition: Epoxy resin A: more than 50 parts by mass and not more than 82 parts by mass 6 parts by weight to 28 parts by weight of epoxy resin B 6 parts by weight to 28 parts by weight of epoxy resin C 0 to 6 parts by weight of other epoxy resin 0 to 5 parts by weight of core-shell rubber particles 45 parts by weight to 80 parts by weight of hardener.

[0069] In one preferred embodiment of the present disclosure, the epoxy resin composition comprises the following components in the following amounts relative to the total weight of the epoxy resin composition: 60 parts by weight to 82 parts by weight of epoxy resin A 8 parts by weight to 22 parts by weight of epoxy resin B 8 parts by weight to 18 parts by weight of epoxy resin C 0 to 3 parts by weight of other epoxy resin 0 to 6 parts by weight of core-shell rubber particles 45 parts by weight to 70 parts by weight of hardener.

[0070] <Cured resin> The present disclosure includes a cured resin product obtained by curing the epoxy resin composition according to the present disclosure.

[0071] The method for producing a resin cured product by curing the epoxy resin composition is not particularly limited. For example, the epoxy resin composition according to the present disclosure can be heat-treated at 130 to 180° C. for 0.5 to 2 hours to produce a resin cured product.

[0072] <Fiber-reinforced composite materials> The present disclosure also includes a fiber-reinforced composite material. The fiber-reinforced composite material includes a cured resin obtained by curing the epoxy resin composition according to the present disclosure, and a fiber-reinforced substrate.

[0073] The fiber-reinforced composite material according to the present disclosure can be obtained, for example, by impregnating a fiber-reinforced substrate with a liquid resin (i.e., for example, an uncured epoxy resin composition) and curing or solidifying the resin.

[0074] The method for producing the fiber-reinforced composite material is not particularly limited, and a prepreg in which a fiber-reinforced substrate is previously impregnated with a matrix resin may be molded, or the fiber-reinforced substrate and the matrix resin may be composited at the same time as molding by a resin transfer molding method (RTM method), a resin film infusion molding method (RFI method), etc. Specific production methods for obtaining a fiber-reinforced composite material will be described later.

[0075] <Fiber reinforced base material> The fiber-reinforced substrate comprises reinforcing fibers, and is preferably a carbon fiber-reinforced substrate.

[0076] (Reinforced fiber sheet) The fiber reinforced substrate may comprise one or more reinforcing fiber sheets comprising the reinforcing fibers.

[0077] The reinforcing fiber sheet may be a fabric in which reinforcing fibers as warp and weft are woven in a plain weave, satin weave, etc. In such a fabric, for example, the reinforcing fibers as warp and the reinforcing fibers as weft extend perpendicularly to each other.

[0078] In contrast, a unidirectional (UD) reinforcing fiber sheet in which reinforcing fibers are aligned in one direction can be used. An example of such a unidirectional reinforcing fiber sheet is a unidirectional woven fabric. The unidirectional fabric is a fabric composed of reinforcing fibers aligned in one direction as warp threads and auxiliary threads as weft threads, and is a so-called blind fabric.

[0079] A non-crimp fabric can also be used for the fiber reinforced substrate. In a non-crimp fabric, a plurality of reinforcing fiber sheets made of reinforcing fibers aligned in one direction are laminated, and these laminated reinforcing fiber sheets are sewn together with a stitch thread as an auxiliary thread. In other words, in a non-crimp fabric, a laminate of reinforcing fiber sheets made of reinforcing fibers aligned in one direction is integrated by being sewn together with an auxiliary thread (particularly called a stitch thread) that penetrates the laminate in the thickness direction.

[0080] (Reinforced Fiber) Examples of the reinforcing fibers constituting the fiber-reinforced substrate include carbon fibers, glass fibers, aramid fibers, boron fibers, metal fibers, etc. The reinforcing fibers are preferably carbon fibers.

[0081] The average length of the reinforcing fibers is not particularly limited, but may be, for example, 5 cm to 100 m.

[0082] The fiber-reinforced substrate according to the present disclosure preferably has a fiber density of 100 to 2000 g / m 2 , more preferably 150 to 1500 g / m 2 The thickness of the fiber-reinforced substrate according to the present disclosure can be appropriately selected depending on the application of the molded product, and may be 0.1 to 2 mm, or 0.5 to 1.5 mm.

[0083] (auxiliary thread) In the fiber-reinforced substrate, the auxiliary yarns have the role of connecting the reinforcing fibers and / or the reinforcing fiber sheets to each other, thereby maintaining the integrity of the reinforcing fiber sheet and / or the fiber-reinforced substrate. The auxiliary yarns may include polyolefin fibers, polyamide resins, polyester resins, cellulose fibers, polyethersulfone (PES) resins, or polyetherimide (PEI) resin fibers, or a mixture thereof. Alternatively, the auxiliary yarns may be made of at least one of these.

[0084] (Resin material layer) The fiber reinforced substrate according to the present disclosure may include one or more reinforcing fiber sheets and one or more resin material layers. The resin material layer may be a sheet containing thermoplastic resin fibers, particularly a nonwoven fabric containing thermoplastic resin fibers. In one embodiment according to the present disclosure, the resin material layer is a nonwoven fabric produced by a melt-blowing method. By using the melt-blowing method, a nonwoven fabric containing thermoplastic resin fibers with a smaller fiber diameter can be produced compared to the case of using the spunbonding method.

[0085] The resin material layer can be laminated, for example, together with a reinforcing fiber sheet to form a laminate. The resin material layer may be disposed between the reinforcing fiber sheets in such a laminate. Preferably, the resin material layer is adjacent to the reinforcing fiber sheet, and in particular, disposed on the surface of the reinforcing fiber sheet. By having the resin material layer in the fiber-reinforced substrate, the impact resistance of the fiber-reinforced resin composite material produced from the fiber-reinforced substrate can be improved.

[0086] <Method of manufacturing fiber-reinforced composite materials> The present disclosure also includes a method of making a fiber reinforced composite material, the method comprising: forming an intermediate composite comprising a fiber reinforced substrate and an epoxy resin composition according to the present disclosure; and curing the intermediate composite to form a fiber reinforced composite material; Includes.

[0087] The "intermediate composite" may be, for example, a fiber-reinforced substrate impregnated with an epoxy resin composition. Details of the manufacturing method are described below with reference to exemplary embodiments.

[0088] One exemplary embodiment of a method for producing a fiber reinforced composite material according to the present disclosure includes: Impregnating a fiber reinforced substrate disposed in a mold with an epoxy resin composition according to the present disclosure; and curing the fiber-reinforced substrate impregnated with the epoxy resin composition according to the present disclosure under heating to form a fiber-reinforced composite material; Includes.

[0089] When impregnating with the epoxy resin composition, for example, a fiber-reinforced substrate placed in a mold is impregnated with a liquid epoxy resin composition before curing as a matrix resin.

[0090] The mold may be a closed mold made of a rigid material, or an open mold made of a rigid material and a flexible film (bag). In the latter case, a fiber-reinforced substrate can be placed between the open mold made of a rigid material and the flexible film. As rigid materials, various existing materials such as metals such as steel and aluminum, fiber-reinforced plastics (FRP), wood, and gypsum are used. As materials for the flexible film, polyamide, polyimide, polyester, fluororesin, silicone resin, etc. are used.

[0091] When a closed mold of a rigid material is used, the mold is usually clamped under pressure, and the resin composition is injected under pressure. At this time, a suction port can be provided in addition to the injection port, and connected to a vacuum pump for suction. It is also possible to inject the resin composition under atmospheric pressure without using a special pressurizing means by suction. This method is suitable for use because it allows the manufacture of large components by providing multiple suction ports.

[0092] When using an open mold of a rigid material and a flexible film, suction may be performed and the resin composition may be injected only at atmospheric pressure without using a special pressurizing means. In order to achieve good impregnation by injection only at atmospheric pressure, it is effective to use a resin diffusion medium. Furthermore, it is preferable to apply a gel coat to the surface of the rigid material prior to the installation of the fiber-reinforced substrate.

[0093] The impregnation pressure when the epoxy resin composition is impregnated into the fiber-reinforced substrate can be appropriately determined taking into consideration the viscosity and resin flow of the resin. A specific impregnation pressure is 0.001 to 10 MPa, and preferably 0.01 to 1 MPa. The viscosity of the epoxy resin when producing the fiber-reinforced composite material is preferably less than 5000 mPa·s at 100°C, and more preferably 1 to 1000 mPa·s.

[0094] In the above manufacturing method, the viscosity of the resin composition at the injection temperature is preferably 0.01 to 1 Pa·s. It is preferable to adjust the viscosity at the time of injection to within the above range by treating the resin to be injected in advance by a method such as heating.

[0095] In the manufacturing method according to the present disclosure, the fiber-reinforced substrate impregnated with the epoxy resin composition is cured under heating. The mold temperature during heat curing is usually selected to be higher than the mold temperature during injection of the thermosetting resin. The mold temperature during heat curing is preferably 80 to 200°C. The heat curing time is preferably 1 minute to 20 hours. After completion of heat curing, the fiber-reinforced composite material is removed from the mold. Thereafter, the obtained fiber-reinforced composite material may be post-cured by heating at a higher temperature. The post-curing temperature is preferably 150 to 200°C, and the post-curing time is preferably 1 minute to 4 hours.

[0096] The amount of the epoxy resin composition may be 20 to 60 parts by mass based on 100 parts by mass of the fiber-reinforced substrate.

[0097] <Preform material> When a fiber-reinforced composite material is molded using a fiber-reinforced base material, the fiber-reinforced base material can be used as is, but from the viewpoint of handleability and workability, it is preferable to use a preform material in which the fiber-reinforced base material is stacked and preformed.

[0098] The preform material can be manufactured by a method including a step of heating a composite containing a fiber-reinforced substrate and a binder resin under pressure (particularly a composite composed of these). For example, the preform material is manufactured by stacking the fiber-reinforced substrate on one side of a preform production mold to a desired thickness, scattering a powder of a resin (binder resin) that serves as a binder or laminating a resin sheet as necessary, and heating under pressure by a press using a heating plate or the like to perform preforming. The resin melts by heating, and the fiber-reinforced substrates are molded according to the mold, resulting in a preform material that retains the shape of the mold.

[0099] The resin material used as the binder resin is not particularly limited, and can be a thermosetting resin such as an epoxy resin or a vinyl ester resin, a thermoplastic resin such as a polyamide or a polyethersulfone, or a mixture thereof. These resins can be used by scattering powder, or can be formed into a sheet or nonwoven fabric and laminated on the fiber-reinforced substrate of the present invention. Alternatively, they can be attached in advance to each thread constituting the fiber-reinforced substrate of the present invention.

[0100] The amount of binder resin constituting the preform material is preferably 1 to 20 parts by mass, more preferably 5 to 10 parts by mass, per 100 parts by mass of the fiber-reinforced substrate of the present invention. The thickness of the preform material differs depending on the purpose of use, but is preferably 1 to 40 mm.

[0101] <Application> The applications of the epoxy resin composition according to the present disclosure and the fiber-reinforced resin composite material produced from the epoxy resin composition according to the present disclosure are not particularly limited, and can be used, for example, as structural materials for aircraft, automobiles, railway vehicles, and ships. EXAMPLES

[0102] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Each component and measurement method used in the examples and comparative examples are described below.

[0103] <<Ingredients>> <Epoxy resin> Epoxy Resin A Tetraglycidyl-3,4'-diaminodiphenyl ether (a compound synthesized by the method of Synthesis Example 1 and represented by the following chemical formula 1-1. Hereinafter abbreviated as "3,4'-TGDDE") [ka] Tetraglycidyl-4,4'-diaminodiphenylmethane (Araldite MY721 manufactured by Huntsman. A compound represented by the following chemical formula 1-2. Hereinafter abbreviated as "TGDDM") [ka]

[0104] Epoxy Resin B Epoxy resin having the structure of the following chemical formula 2-1 (NC-514S manufactured by Cardlite Co., Ltd.) [ka]

[0105] Epoxy Resin C Polyglycerol polyglycidyl ether (EX-512, manufactured by Nagase ChemteX Corporation) having the chemical structure shown in Chemical Formula 3-1 below [ka]

[0106] Other epoxy resins Bisphenol A diglycidyl ether (Mitsubishi Chemical Corporation jER825, hereafter abbreviated as "DGEBA") N,N-diglycidyl-o-toluidine (GOT manufactured by Nippon Kayaku Co., Ltd., hereafter abbreviated as "GOT") Sorbitol polyglycidyl ether represented by the following chemical formula 5 (EX-612, manufactured by Nagase ChemteX Corporation) [ka]

[0107] (Amine-based hardener) 4,4'-Diamino-3,3'-diisopropyl-5,5'-dimethyldiphenylmethane (Lonzacure M-MIPA manufactured by Lonza, hereafter abbreviated as "M-MIPA") [ka]

[0108] (Additives) MX-416 (MX-416 manufactured by Kaneka Corporation, a master batch in which particulate butadiene rubber component (CSR) is dispersed in glycidylamine-type tetrafunctional epoxy resin to a concentration of 25 mass %) (The glycidylamine-type tetrafunctional epoxy resin in the product is tetraglycidyl-4,4'-diaminodiphenylmethane, which corresponds to the epoxy resin A of the present invention.)

[0109] <Synthesis Example 1> Synthesis of 3,4'-TGDDE In a four-neck flask equipped with a thermometer, a dropping funnel, a cooling tube and a stirrer, 1110.2g (12.0mol) of epichlorohydrin was charged, and the temperature was raised to 70°C while purging with nitrogen, and 200.2g (1.0mol) of 3,4'-diaminodiphenyl ether dissolved in 1000g of ethanol was dropped into it over 4 hours. The mixture was stirred for another 6 hours to complete the addition reaction, and N,N,N',N'-tetrakis(2-hydroxy-3-chloropropyl)-3,4'-diaminodiphenyl ether was obtained. The temperature in the flask was then lowered to 25°C, and 500.0g (6.0mol) of 48% NaOH aqueous solution was dropped into it over 2 hours and stirred for another hour. After the cyclization reaction was completed, the ethanol was distilled off, and the mixture was extracted with 400g of toluene and washed twice with 5% saline. Toluene and epichlorohydrin were removed from the organic layer under reduced pressure to obtain 361.7 g (yield 85.2%) of a brown viscous liquid. The purity of the main product, 3,4'-TGDDE, was 84% ​​(HPLC area %).

[0110] <<Evaluation method>> (1) Physical properties of resin composition (1-1) Preparation of epoxy resin composition Epoxy resin compositions were prepared by mixing epoxy resin heated to 80°C and additives in the ratios shown in Tables 1 and 2 below using a stirrer, then adding a curing agent and mixing for 30 minutes. Note that in the compositions shown in Tables 1 and 2, the glycidyl groups of the epoxy resin and the amino groups of the curing agent are equivalent.

[0111] (1-2)100℃ viscosity The viscosity of the epoxy resin composition obtained in (1-1) above was measured at 100° C. using a B-type viscometer TVB-15M manufactured by Toki Sangyo Co., Ltd.

[0112] (1-3) Curing start temperature 2.5 to 3.5 mg of the epoxy resin composition obtained in (1-1) above was weighed out and subjected to DSC measurement. The intersection point between the baseline and the tangent line at the inflection point on the low temperature side at the exothermic peak accompanying curing in the obtained chart was taken as the curing initiation temperature. The DSC measurement was performed under the following conditions. ·Measurement temperature range: 30~350℃ Heating rate: 10℃ / min

[0113] (2) Physical properties of cured resin (2-1) Preparation of cured resin The epoxy resin composition prepared in (1-1) above was degassed in a vacuum, and then poured into a silicone resin mold set to a thickness of 4 mm using a 4 mm silicone resin spacer. It was cured at 180°C for 2 hours to obtain a 4 mm thick cured resin product.

[0114] (2-2) Glass transition temperature after water absorption (DMA-wet-Tg) The glass transition temperature was measured according to the SACMA 18R-94 method. The resin cured product obtained in (2-1) above was cut and polished to prepare a test piece with dimensions of 50 mm x 6 mm x 2 mm. The prepared resin test piece was subjected to water absorption treatment at 121°C for 24 hours using a pressure cooker (HASTEST PC-422R8, manufactured by Espec Corporation). The storage modulus E' of the water-absorbed resin test piece was measured from 50°C to the rubber elasticity region using a dynamic viscoelasticity measuring device Rheogel-E400 manufactured by UBM under the conditions of a measurement frequency of 1 Hz, a heating rate of 5°C / min, and a strain of 0.0167%, with the distance between the chucks set to 30 mm. logE' was plotted against temperature, and the temperature obtained from the intersection of the approximation line of the flat region of logE' and the approximation line of the region where E' transitions was recorded as the glass transition temperature (wet-Tg).

[0115] (2-3) Bending modulus of resin The test was carried out according to JIS K7171. The resin test piece was prepared with dimensions of 80mm x 10mm x h4mm. The bending test was carried out with a support distance L of 16 x h (thickness) and a test speed of 2m / min to measure the bending modulus.

[0116] <<Examples 1 to 9>> In Examples 1 to 9, the components shown in Table 1 below were mixed using a stirrer to obtain an epoxy resin composition. The physical properties of the obtained epoxy resin composition and the cured resin product are shown in Table 1. The amount of MX-416 added was adjusted so that the CSR was the mass percentage shown in Table 1 relative to the weight of the total resin composition.

[0117] [Table 1]

[0118] <<Comparative Examples 1 to 9>> In Comparative Examples 1 to 9, the components shown in Table 2 were mixed using a stirrer to obtain epoxy resin compositions. The physical properties of the obtained epoxy resin compositions and the cured resin products are shown in Table 2. The amount of MX-416 added was adjusted so that the CSR was the mass percentage shown in Table 2 relative to the weight of the total resin composition.

[0119] [Table 2]

[0120] As can be seen from Table 1, good results were obtained for all physical properties in the epoxy resin compositions according to Examples 1 to 9, which contained all of the epoxy resins A to C. Specifically, the composition properties of viscosity at 100°C and curing initiation temperature were all good, and the cured product properties of glass transition temperature after water absorption (wet-Tg) and flexural modulus were also good.

[0121] On the other hand, as can be seen from Table 2, in Comparative Examples 1 to 9 which did not contain at least any one of the epoxy resins A to C, one or more of the physical properties was relatively poor.

[0122] Specifically, Comparative Examples 1 and 5 contained epoxy resin B but did not contain epoxy resin C, and the flexural modulus of the cured product was relatively poor. In addition, when Comparative Example 1 (B component only) was compared with Examples 1 and 2 (B component + C component), the glass transition temperature was relatively low in Comparative Example 1. The same was true when Comparative Example 5 (B component only) was compared with Examples 3 and 4 (B component + C component).

[0123] Comparative Examples 2, 6 and 7 showed excessively high viscosities because they contained epoxy resin C but did not contain epoxy resin B. If the viscosity is too high, the handleability of the epoxy resin composition is poor.

[0124] Comparative Example 3 is an example in which the compound represented by the above chemical formula 5 was used instead of the compound represented by the above chemical formula 3-1 as epoxy resin C. The compound represented by the above chemical formula 5 does not correspond to the above chemical formula 3, which is a requirement for epoxy resin C. As can be seen from Table 2, Comparative Example 3 exhibited an excessively high viscosity.

[0125] In Comparative Example 4, epoxy resin A was not used, and GOT was used instead, resulting in a significant decrease in wet-Tg.

[0126] Comparative Examples 8 and 9 showed excessively high viscosity and excessively high curing initiation temperature as a result of not using epoxy resin B and epoxy resin C. When the curing initiation temperature is excessively high, the curing efficiency during the curing treatment of the epoxy resin composition may be insufficient.

[0127] In particular, the above results show that the combined use of epoxy resins B and C provides better physical properties than the use of epoxy resin B or epoxy resin C alone. As epoxy resins B and C, biomass-derived resins can be used, and in fact, NC514S and Ex-512, which were used as epoxy resins B and C in the examples, are both biomass-derived epoxy resins. Therefore, by using epoxy resins B and C in combination according to the present invention, a relatively large amount of biomass-derived components can be used in the epoxy resin composition while ensuring the desired excellent physical properties.

Claims

1. Epoxy resin A represented by the following chemical formula 1, Epoxy resin B represented by the following chemical formula 2, Epoxy resin C represented by the following chemical formula 3, and Hardener Epoxy resin composition comprising: 【Chemistry 1】 (In formula 1, R 1 ~R 4 each independently represents one selected from the group consisting of a hydrogen atom, an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, and a halogen atom; X is -CH 2 -, -O-, -S-, -CO-, -C(=O)O-, -OC(=O)-, -NHCO-, -CONH-, -SO 2 - represents one selected from. 【Chemistry 2】 (In formula 2, R 5 , R 6 are each independently an aliphatic hydrocarbon group having 4 to 12 carbon atoms. 【Chemistry 3】 (In formula 3, m is an integer from 0 to 20, R 7 ~R 10 are each independently a hydrogen atom or a glycidyl group represented by the following chemical formula 4, R 7 ~R 10 At least two of the above are glycidyl groups represented by the following chemical formula 4. 【Chemistry 4】

2. 2. The epoxy resin composition according to claim 1, wherein the epoxy resin A is 50 to 90 mass% and / or the total of the epoxy resins B and C is 10 to 50 mass%, based on the total mass of the epoxy resins contained in the epoxy resin composition.

3. 3. The epoxy resin composition according to claim 1, wherein a ratio Mb / Mc of a content Mb (g) of the epoxy resin B in the epoxy resin composition to a content Mc (g) of the epoxy resin C in the epoxy resin composition is 0.8 to 3.

5.

4. 3. The epoxy resin composition according to claim 1, wherein at least one of the epoxy resin B and the epoxy resin C is a biomass-derived epoxy resin.

5. The epoxy resin composition according to claim 1 or 2, wherein the epoxy resin A is one or a combination of two or more selected from the group consisting of tetraglycidyl-4,4'-diaminodiphenyl ether, tetraglycidyl-4,4'-diaminodiphenylmethane, tetraglycidyl-3,4'-diaminodiphenyl ether, and tetraglycidyl-3,3'-diaminodiphenylmethane.

6. The epoxy resin composition according to claim 1 or 2, wherein the epoxy resin B is an epoxy resin represented by the following chemical formula 2-1. 【Chemistry 5】

7. The epoxy resin composition according to claim 1 or 2, wherein the epoxy resin C is an epoxy resin represented by the following chemical formula 3-1. 【Chemistry 6】

8. A cured resin product obtained by curing the epoxy resin composition according to claim 1 or 2.

9. A fiber-reinforced composite material comprising a cured resin obtained by curing the epoxy resin composition according to claim 1 or 2, and a fiber-reinforced substrate.

10. The fiber-reinforced composite material according to claim 9 , wherein the fiber-reinforced substrate is a carbon fiber-reinforced substrate.

11. forming an intermediate composite comprising a fiber-reinforced substrate and the epoxy resin composition of claim 1 or 2; and curing the intermediate composite to form a fiber reinforced composite material; A method for producing a fiber-reinforced composite material, comprising:

12. Impregnating a fiber-reinforced substrate placed in a mold with the epoxy resin composition according to claim 1 or 2; and curing the fiber-reinforced substrate impregnated with the epoxy resin composition under heating to form a fiber-reinforced composite material; A method for producing a fiber-reinforced composite material, comprising:

Citation Information

Patent Citations

  • Epoxy resin composition, fiber reinforced composite material, and method for producing them

    JP2013159618A

  • Epoxy resin composition, molding material and fiber-reinforced composite material

    JP2014145018A

  • Organic aerogels based on amine and cyclic ether polymer networks

    JP2020516710A

  • Two-component (2K) compositions based on modified epoxy resins

    JP2022537623A

  • Molding material, sheet molding compound, and molded article

    WO2020241180A1