Composite, composition, coating material, adsorbent, and method for producing composition

A composite of metal-organic frameworks, cellulose derivatives, and crosslinking agents addresses dispersibility and adhesion issues, ensuring uniform dispersion and strong coating films with improved adsorption performance.

JP2024143842APending Publication Date: 2024-10-11OSAKA GAS CO LTD

Patent Information

Application Number
JP2023056750
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing composites containing metal-organic structures face issues with dispersibility in water or organic solvents, leading to non-uniform dispersion, poor adhesion to structures, and inadequate viscosity, which affects the quality of the coating film and work efficiency.

Method used

Incorporating a metal-organic framework with a cellulose derivative and a crosslinking agent, such as epoxy resin or polyisocyanate, to enhance dispersibility, adhesion, and viscosity, while maintaining high water resistance.

Benefits of technology

The composite achieves uniform dispersion, excellent adhesion, and appropriate viscosity, enabling the formation of strong coating films with enhanced adsorption performance, even under high moisture conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143842000001
    Figure 2024143842000001
  • Figure 2024143842000002
    Figure 2024143842000002
  • Figure 2024143842000003
    Figure 2024143842000003
Patent Text Reader

Abstract

To provide a composite which achieves both maintenance of adsorption performance of a metal-organic structure and water resistance.SOLUTION: There is provided a composite which contains a metal-organic structure, a cellulose derivative, and a crosslinking agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite, composition, coating material, adsorbent, and method for producing the composition, each of which includes a metal-organic framework. [Background technology]

[0002] Metal-organic frameworks are materials consisting of a central metal and organic ligands that coordinate to the central metal, and are expected to be used in gas adsorption, molecular adsorption, separation technologies, solid catalysts, sensors, and more.

[0003] As an example of utilizing the properties of metal-organic frameworks, Patent Document 1 proposes a molded article capable of separating and collecting, or adsorbing and removing, moisture and malodorous components in the air.

[0004] This molded body contains a metal-organic framework and an organic binder having an ethylene-vinyl acetate-acrylic copolymer having a structural unit derived from ethylene. This molded body has sufficient adsorption performance for moisture and malodorous components due to the metal-organic framework, and also has excellent water resistance due to the inclusion of the organic binder. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6237059 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the molded body described in Patent Document 1 may have low dispersibility in water or organic solvents depending on the type of metal-organic framework used, which may limit the manner in which the molded body can be used.

[0007] In addition, for example, when preparing a coating material containing the molded body in order to apply the molded body to a structure, the molded body may not be uniformly dispersed in the solvent, resulting in the formation of aggregates, or the coating material may not have an appropriate viscosity, resulting in poor coating properties. This can lead to problems such as a decrease in the quality of the coating film and a decrease in work efficiency.

[0008] Furthermore, when a paint containing the molded body described in Patent Document 1 is applied to a structure, the molded body is difficult to adhere to the structure (low adhesion), and a good coating film cannot be obtained, or sufficient strength cannot be obtained.

[0009] Such problems can occur not only in the molded body described in Patent Document 1, but also in various composites including a metal organic framework, and a composite that fully exhibits the adsorption performance of a metal organic framework while solving these problems has not yet been developed. Therefore, there is a demand for the development of a molded body (composite) that has excellent dispersibility in water or organic solvents, adhesion to the structure, and viscosity while maintaining the adsorption performance of the metal organic framework.

[0010] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a composite that combines the adsorption performance of a metal-organic framework with the properties of imparting dispersibility, adhesiveness, and viscosity, and further has high water resistance even when used under conditions of high water concentration. [Means for solving the problem]

[0011] As a result of intensive research, the present inventors have found that when a composite contains a metal organic framework, a cellulose derivative, and a crosslinking agent, the composite maintains the excellent adsorption performance of the metal organic framework, while also imparting excellent dispersibility, adhesiveness, and viscosity, and further has high water resistance, and have completed the present invention.

[0012] That is, the characteristic configuration of the composite according to the present invention for achieving the above object is as follows: The metal-organic framework includes a cellulose derivative and a crosslinking agent.

[0013] The crosslinking agent has a function of crosslinking the cellulose derivative in the composite, and therefore, according to the above-mentioned characteristic configuration, the composite has high water resistance. In addition, the composite has excellent adsorption performance, dispersibility, adhesiveness, and viscosity.

[0014] In the composite according to the present invention, the cellulose derivative preferably has a hydrophilic group.

[0015] In the complex according to the present invention, the hydrophilic group is preferably any one of those represented by the following formulas (1) to (4). [ka] [ka] [ka] [ka] (In formula (4), R is any one of Na, K, NH4, and H.)

[0016] In the composite according to the present invention, the cellulose derivative is preferably nonionic.

[0017] Furthermore, the complex according to the present invention preferably contains, as the cellulose derivative, at least one selected from the group consisting of hydroxypropyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose, methyl cellulose and carboxymethyl cellulose.

[0018] In the composite according to the present invention, the cellulose derivative preferably has a viscosity of 15 mPa·s or more in an aqueous solution having a solid content of 2.0 wt % at 20°C.

[0019] Moreover, the composite according to the present invention preferably contains the cellulose derivative in an amount of 1 part by mass or more and 100 parts by mass or less in terms of the solid content relative to 100 parts by mass of the solid content of the metal-organic framework.

[0020] In the composite according to the present invention, the metal organic framework preferably contains one type selected from Fe, Zn, Cr, Cu, and Al as a central metal.

[0021] In the complex according to the present invention, the crosslinking agent is preferably a hydrophilic substance. In the composite according to the present invention, the crosslinking agent more preferably contains at least one of an epoxy resin, a melamine resin, and a polyisocyanate, and is further preferably an isocyanate. In this case, the equivalent ratio of isocyanate to the hydroxyl groups of the cellulose derivative is preferably 0.10 or more and 1.0 or less.

[0022] According to the above characteristic configuration, the composite can exhibit high water resistance.

[0023] The composition according to the present invention for achieving the above object has the following characteristic features: The complex is contained in water or an organic solvent.

[0024] According to the above characteristic configuration, the composition has a uniform dispersion of the complex in water or an organic solvent, and has appropriate viscosity and high water resistance, and can be used for various applications that utilize the adsorption performance of the complex.

[0025] The characteristic configuration of the paint according to the present invention for achieving the above object is as follows: The complex is contained in water or an organic solvent such that the proportion of the water or the organic solvent is 50 wt % or more.

[0026] According to the above characteristic configuration, the coating material has a suitable viscosity and excellent coatability because the composite is uniformly dispersed in water or an organic solvent. In addition, since the composite has excellent adhesiveness, a coating film made of the composite with high strength can be formed by applying the coating material to a structure.

[0027] The characteristic configuration of the adsorbent according to the present invention for achieving the above object is as follows: The adsorbent is made of the above-mentioned complex and adsorbs at least one of water and carbon dioxide.

[0028] According to the above characteristic configuration, the adsorption performance of the metal-organic framework in the composite constituting the adsorbent is exhibited, making it possible to separate and capture, or adsorb and remove, water and carbon dioxide.

[0029] The characteristic configuration of the method for producing a composition according to the present invention for achieving the above object is as follows: A method for producing a composition containing a composite including a metal organic framework, a cellulose derivative, and a crosslinking agent, comprising: The method includes a step of mixing the dispersion of the metal organic framework, the dispersion of the cellulose derivative, and the dispersion of the crosslinking agent.

[0030] According to the above characteristic configuration, when the metal-organic framework, the cellulose derivative, and the dispersion of the crosslinking agent are mixed, each of them is in a dispersion state, so that aggregates of the metal-organic framework, the cellulose derivative, and the crosslinking agent are unlikely to occur, and a composition in which the composite is dispersed in the solvent can be produced.

[0031] Further, a further characteristic feature of the method for producing a composition according to the present invention is The dispersion liquid of the metal organic framework is characterized in that the metal organic framework is dispersed in water or an organic solvent at a solid content concentration of 5.0 wt % or more and 40 wt % or less.

[0032] According to the above characteristic configuration, the generation of aggregates of the metal organic framework in the manufacturing process can be further suppressed.

[0033] Further, a further characteristic feature of the method for producing a composition according to the present invention is The cellulose derivative dispersion is characterized in that the cellulose derivative is dispersed in water or an organic solvent at a solid content concentration of 0.50 wt % or more and 30 wt % or less.

[0034] According to the above characteristic configuration, the generation of aggregates of the cellulose derivative during the production process can be further suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] The composite, composition, paint, adsorbent, and method for producing the composition according to the present invention will be described below. Note that, although preferred examples are described below in order to more specifically illustrate the present invention, various modifications are possible without departing from the spirit of the present invention, and the present invention is not limited to the following descriptions.

[0036] [Complex] The composite according to the present invention includes a metal organic framework, a cellulose derivative, and a crosslinking agent. In the present invention, the ratio of the metal organic framework, the cellulose derivative, and the crosslinking agent based on mass is not particularly limited, but the cellulose derivative is preferably contained in an amount of 1 part by mass or more and 100 parts by mass or less in terms of solid content mass relative to 100 parts by mass of the solid content mass of the metal organic framework, more preferably 5 parts by mass or more and 50 parts by mass or less, even more preferably 10 parts by mass or more and 40 parts by mass or less, and even more preferably 10 parts by mass or more and 25 parts by mass or less. In addition, the equivalent ratio of the isocyanate of the crosslinking agent to the hydroxyl group of the cellulose derivative is preferably 0.10 to 1.0, more preferably 0.10 to 0.90, and even more preferably 0.10 to 0.75.

[0037] The metal organic framework is composed of a central metal and an organic ligand coordinated to the central metal. The metal organic framework may be a commercially available product or may be obtained by synthesis.

[0038] In the present invention, the central metal to be used is not particularly limited, and any known metal ion capable of forming a metal organic framework can be used. Examples of the central metal include K, Mg, Ca, Sr, Ba, Sc, Y, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Re, Fe, Ru, Os, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zn, Cd, Hg, Al, Ga, In, Tl, Si, Ge, Sn, Pb, As, Sb, and Bi, and preferably one selected from Fe, Zn, Cr, Cu, and Al.

[0039] In the present invention, the organic ligand used is not particularly limited as long as it is a compound having a functional group capable of coordinating to the central metal, and may be a commercially available product or may be obtained by synthesis. Examples of the organic ligand used include 1,4-butanedicarboxylic acid, 4-oxopyran-2,6-dicarboxylic acid, 1,6-hexanedicarboxylic acid, decanedicarboxylic acid, 1,8-heptadecanedicarboxylic acid, 1,9-heptadecanedicarboxylic acid, heptadecanedicarboxylic acid, 1,2-benzenedicarboxylic acid, 2,3-pyridinedicarboxylic acid, pyridine-2,3-dicarboxylic acid, 1,3-butadiene-1,4-dicarboxylic acid, terephthalic acid, isophthalic acid, imidazole-2,4-dicarboxylic acid, 2-methyl ... Quinoline-3,4-dicarboxylic acid, quinoline-2,4-dicarboxylic acid, quinoxaline-2,3-dicarboxylic acid, 6-chloroquinoxaline-2,3-dicarboxylic acid, 4,4'-diaminophenylmethane-3,3'-dicarboxylic acid, quinoline-3,4-dicarboxylic acid, 7-chloro-4-hydroxyquinoline-2,8-dicarboxylic acid, diimidedicarboxylic acid, 2-methylimidazole-4,5-dicarboxylic acid, thiophene-3,4-dicarboxylic acid, 2-isopropylimidazole-4,5-dicarboxylic acid, tetrahydrofuran-2,4 ... Lahydrofuran-4,4'-dicarboxylic acid, perylene-3,9-dicarboxylic acid, perylenedicarboxylic acid, Pluriol E200-dicarboxylic acid, 3,6-dioxaoctanedicarboxylic acid, 3,5-cyclohexadiene-1,2-dicarboxylic acid, sebacic acid, pentane-3,3'-dicarboxylic acid, 4,4'-diamino-1,1'-diphenyl-3,3'-dicarboxylic acid, 4,4'-diaminodiphenyl-3,3'-dicarboxylic acid, benzidine-3,3'-dicarboxylic acid, 1,4-bis-(phenylamino) -benzene-2,5-dicarboxylic acid, 1,1'-binaphthyl-8,8'-dicarboxylic acid, 7-chloro-8-methylquinoline-2,3-dicarboxylic acid, 1-anilinoanthraquinone-2,4'-dicarboxylic acid, polytetrahydrofuran-250-dicarboxylic acid, 1,4-bis-(carboxymethyl)-piperazine-2,3-dicarboxylic acid, 7-chloroquinoline-3,8-dicarboxylic acid, 1-(4-carboxy)phenyl-3-(4-chloro)phenylpyrazoline-4,5-dicarboxylic acid, 1,4,5,6,7,7-Hexachloro-5-norbornene-2,3-dicarboxylic acid, Phenylindanedicarboxylic acid, 1,3-dibenzyl-2-oxo-imidazoline-4,5-dicarboxylic acid, 2-benzoylbenzene-1,3-dicarboxylic acid, 1,3-dibenzyl-2-oxo-imidazoline-4,5-dicarboxylic acid, 2,2'-biquinoline-4,4'-dicarboxylic acid, Pyridine-3,4-dicarboxylic acid, 3,6,9-trioxaundecanedicarboxylic acid, O-hydroxybenzophenonedicarboxylic acid, Pluriol E300-dicarboxylic acid, Pluriol E400-dicarboxylic acid carboxylic acid, Pluriol E600-dicarboxylic acid, pyrazole-3,4-dicarboxylic acid, 5,6-dimethyl-2,3-pyrazinedicarboxylic acid, 4,4'-diamino(diphenyl ether)diimidedicarboxylic acid, 4,4'-diaminodiphenylmethanediimidedicarboxylic acid, 4,4'-diamino(diphenyl sulfone)diimidedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,3-adamantanedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 2,6-pyridinedicarboxylic acid, 8-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 1,7-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 1,7 ... -Methoxy-2,3-naphthalenedicarboxylic acid, 8-nitro-2,3-naphthalenedicarboxylic acid, 8-sulfo-2,3-naphthalenedicarboxylic acid, anthracene-2,3-dicarboxylic acid, 2',3'-diphenyl-p-terphenyl-4,4''-dicarboxylic acid, (diphenyl ether)-4,4'-dicarboxylic acid, imidazole-4,5-dicarboxylic acid, 4(1H)-oxo-thiochromene-2,8-dicarboxylic acid, 5-t-butyl-1,3-benzenedicarboxylic acid, 7,8-quinolinedicarboxylic acid, 4,5-imidazoledicarboxylic acid, 4-cyclohexyl 1,2-hexenedicarboxylic acid, hexatriacontanedicarboxylic acid, tetradecanedicarboxylic acid, 1,7-heptanedicarboxylic acid, 5-hydroxy-1,3-benzenedicarboxylic acid, pyrazine-2,3-dicarboxylic acid, furan-2,5-dicarboxylic acid, 1-nonene-6,9-dicarboxylic acid, eicosenedicarboxylic acid, 4,4'-dihydroxydiphenylmethane-3,3'-dicarboxylic acid, 1-amino-4-methyl-9,10-dioxo-9,10-dihydroanthracene-2,3-dicarboxylic acid, 2,5-pyridinedicarboxylic acid, cyclohexene-2,3-dicarboxylic acid, 2,9-dichlorofluorine-4,11-dicarboxylic acid, 7-chloro-3-methylquinoline-6,8-dicarboxylic acid, 2,4-dichlorobenzophenone-2',5'-dicarboxylic acid, 1,3-benzenedicarboxylic acid, 1-methylpyrrole-3,4-dicarboxylic acid, 1-benzyl-1H-pyrrole-3,4-dicarboxylic acid, anthraquinone-1,5-dicarboxylic acid, 3,5-pyrazole dicarboxylic acid, 2-nitrobenzene-1,4-dicarboxylic acid, heptane-1,7-dicarboxylic acid, cyclobutane-1,1-dicarboxylic acid, 1,1 4-Tetradecanedicarboxylic acid, 5,6-dehydronorbornane-2,3-dicarboxylic acid, 5-ethyl-2,3-pyridinedicarboxylic acid, 2-hydroxy-1,2,3-propanetricarboxylic acid, 7-chloro-2,3,8-quinolinetricarboxylic acid, trimellitic acid, 1,2,4-butanetricarboxylic acid, 2-phosphono-1,2,4-butanedicarboxylic acid, trimesic acid, 1-hydroxy-1,2,3-propanetricarboxylic acid, 4,5-dihydro-4,5-dioxo-1H-pyrrolo[2,3-F]quinoline-2,7,9-tricarboxylic acid, 5-acetonitrile, 1,2,3-propanetricarboxylic acid, 1,2,3-propanetricarboxylic acid, 1,1-dioxidoperillo[1,12-BCD]thiophene-3,4,9,10-tetracarboxylic acid, perylene-3,4,9,10-tetracarboxylic acid, perylene-1,12-sulfone-3,4,9,10-tetracarboxylic acid, decane-2,4,6,8-tetracarboxylic acid, 1,4,7,10,13,16-hexaoxacyl Cyclooctadiene-2,3,11,12-tetracarboxylic acid, pyromellitic acid, 1,2,11,12-dodecanetetracarboxylic acid, 1,2,5,6-hexanetetracarboxylic acid, 1,2,7,8-octanetetracarboxylic acid, 1,4,5,8-naphthalenetetracarboxylic acid, 1,2,9,10-decanetetracarboxylic acid, benzophenonetetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, tetrahydrofurantetracarboxylic acid, cyclopentane-1,2,3,4-tetracarboxylic acid, 2,5-dihydroxyterephthalic acid, 4,4'-Biphenyldicarboxylic acid, 1,3,5-tris(4-carboxyphenyl)benzene, acetylenedicarboxylic acid, trans,trans-muconic acid, 1,4-cyclohexanedicarboxylic acid, trans-1,4-cyclohexanedicarboxylic acid, cis-1,2-cyclohexanedicarboxylic acid, trans-1,2-cyclohexanedicarboxylic acid, 5-hydroxyisophthalic acid, 5-nitroisophthalic acid, 3-nitrophthalic acid, 4-methylphthalic acid, 4-nitrophthalic acid Examples of suitable amines include phthalic acid, 2,2'-biphenyldicarboxylic acid, 1,4,5,8-naphthalenetetracarboxylic acid, pyridine-2-carboxylic acid, pyridine-3-carboxylic acid, pyridine-4-carboxylic acid, 2,6-pyridinedicarboxylic acid, triethylenediamine, hexamethylenetetramine, imidazole, 2-methylimidazole, pyrazine, 2,2'-bipyridyl, 4,4'-bipyridyl, 1,3-di(4-pyridyl)propane, 5-aminoisophthalic acid, and picolinic acid.

[0040] In the present invention, the cellulose derivative preferably has a hydrophilic group from the viewpoint of dispersibility of the complex in water or an organic solvent. Examples of the hydrophilic group include a hydroxyl group, a carboxyl group, an amino group, and a nitro group. Taking into consideration the affinity with the metal-organic framework, the hydrophilic group is preferably any one of the above chemical formulas (1) to (4).

[0041] In the present invention, the cellulose derivative is preferably nonionic.

[0042] There are various compounds as nonionic cellulose derivatives having hydrophilic groups represented by the above chemical formulas (1) to (4), and the compounds are not particularly limited. However, in the present invention, it is preferable that the complex contains one selected from hydroxypropyl cellulose (HPC), hydroxyethyl cellulose (HEC), hydroxypropyl methylcellulose (HPMC), hydroxyethyl methylcellulose (HEMC), methylcellulose (MC), and carboxymethyl cellulose (CMC).

[0043] In the present invention, the cellulose derivative has a viscosity at 20°C of an aqueous solution having a solids concentration of 2.0 wt% (hereinafter simply referred to as "viscosity"), which is not particularly limited; however, it is preferably 15 mPa·s or more, more preferably from 15 to 100,000 mPa·s, and even more preferably from 1,000 to 100,000 mPa·s.

[0044] A composite having the above-mentioned structure has excellent adsorption performance, and also has excellent dispersibility in water or organic solvents, adhesiveness to structures, and properties of imparting viscosity.

[0045] [Crosslinking Agent] The crosslinking agent has the function of crosslinking the cellulose derivative in the composite. The composite is used by dispersing it in water or an organic solvent. In particular, when dispersing it in water, the crosslinking agent is preferably a hydrophilic substance, and more preferably is selected from at least one of epoxy resin, melamine resin, and polyisocyanate. Among these substances, isocyanate is more preferable. In this case, the equivalent ratio of isocyanate to the hydroxyl group of the cellulose derivative is preferably 0.10 or more and 1.0 or less. By having such a structure, the composite can exhibit high water resistance. Here, isocyanate refers to the available NCO in the polyisocyanate. Since the composite of the present invention contains a metal organic framework, when heating is required in the production and use of the composite, it is preferable that the crosslinker is a substance that is not decomposed even when heated and dried at or below 250° C. The above-mentioned crosslinkers are preferably used because they satisfy this condition.

[0046] [Compositions and paints] The composition according to the present invention contains the above-mentioned complex in water or an organic solvent. The ratio of water or organic solvent in the composition is not particularly limited, but compositions in which the ratio of water or organic solvent is 50 wt% or more (more preferably 60 wt% or more) can be suitably used as a paint.

[0047] The composition and paint may contain other than the complex and water or organic solvent. The solid content concentration of the complex in the composition and paint is not particularly limited, but the solid content concentration of the complex in the composition is preferably 0.50 wt% or more and 40 wt% or less, more preferably 2.0 wt% or more and 30 wt% or less, even more preferably 3.0 wt% or more and 20 wt% or less, and even more preferably 5.0 wt% or more and 15 wt% or less. The solid content concentration of the complex in the paint is preferably 0.50 wt% or more and 50 wt% or less, more preferably 2.0 wt% or more and 30 wt% or less, and even more preferably 3.0 wt% or more and 20 wt% or less.

[0048] In the composition and coating material of the present invention, the organic solvent is not particularly limited, but is preferably an alcohol such as methanol, ethanol, or isopropyl alcohol.

[0049] In the composition having the above-mentioned configuration, the complex is uniformly dispersed in water or an organic solvent, and has a suitable viscosity, and can be used in various applications that utilize the adsorption performance of the complex. In addition, in the paint having the above-mentioned configuration, the complex is uniformly dispersed in water or an organic solvent, and has a suitable viscosity and excellent coatability. In addition, since the paint contains a complex having excellent adhesive properties, a high-strength coating film made of the complex can be formed by applying the paint to a structure.

[0050] [Adsorbent] The adsorbent according to the present invention is made of the above-mentioned complex and adsorbs water and carbon dioxide. The adsorbent can be produced, for example, by removing water and an organic solvent from the above-mentioned composition. This adsorbent exhibits the adsorption performance of the metal-organic framework in the complex, and is capable of separating and recovering water and carbon dioxide, as well as adsorbing and removing them.

[0051] [Method of producing the composition] The method for producing a composition according to the present invention is a method for producing a composition containing a composite comprising a metal organic framework, a cellulose derivative, and a crosslinking agent, and includes a step of mixing the metal organic framework, the cellulose derivative, and the crosslinking agent, each of which is in the state of a dispersion.

[0052] In the present invention, water or an organic solvent such as alcohol can be used as the solvent for each dispersion when mixing the metal organic framework, the cellulose derivative, and the crosslinking agent.

[0053] The dispersion of the metal-organic framework is preferably a dispersion of the metal-organic framework in water or an organic solvent, and has a solid content of preferably 5.0 wt% to 40 wt%, more preferably 10 wt% to 35 wt%, and even more preferably 15 wt% to 30 wt%. The dispersion of the metal-organic framework does not necessarily have to be liquid, and may be clay-like or slurry-like depending on the solid content.

[0054] Furthermore, the dispersion of the cellulose derivative is preferably a dispersion of the cellulose derivative in water or an organic solvent, and the solid content concentration is preferably 0.5 wt% or more and 30 wt% or less, and more preferably 1.0 wt% or more and 10 wt% or less.

[0055] In addition, the dispersion of the crosslinking agent is preferably a dispersion of the crosslinking agent derivative in water or an organic solvent, and the equivalent ratio of the crosslinking agent to the cellulose derivative is preferably 0.10 or more and 1.0 or less, more preferably 0.10 or more and 0.90 or less, and even more preferably 0.10 or more and 0.75 or less.

[0056] In the method for producing a composition according to the present invention, when the metal organic framework, the cellulose derivative, and the crosslinking agent are mixed, each of them is in a state of a dispersion, so that aggregates of the metal organic framework, the cellulose derivative, and the crosslinking agent are unlikely to occur, and a composition in which the composite is dispersed in the solvent can be produced. EXAMPLES

[0057] The present invention will be described in more detail below with reference to examples, although it goes without saying that the present invention is not limited to the examples.

[0058] Table 1 shows the metal-organic framework (MOF), binder (cellulose derivative), solid content ratio (MOF:binder), crosslinking agent, and evaluation results used in the examples and comparative examples.

[0059] [Table 1]

[0060] 1. Preparation of the Composition The metal organic framework and / or the binder and / or the crosslinker were each dispersed in water to prepare a dispersion so that the concentration of the metal organic framework (MOF) was 20 wt% and the solid content ratio (MOF:binder) was the value shown in Table 1, and then the dispersion was mixed and stirred to prepare the compositions of Examples 1 to 5 and Comparative Examples 2 to 10. The metal organic framework dispersion used was one in which the solid content concentration was 20 wt% dispersed in water. The binder dispersion used was one in which the cellulose derivative was dispersed in water at a solid content concentration of 5.0 wt%. In the preparation of the compositions of Comparative Examples 3 to 9, the binder was used as it was in the form of an emulsion.

[0061] When using a crosslinking agent for a cellulose derivative, it is desirable that the weight ratio of the effective NCO content contained in the crosslinking agent to the hydroxyl value (OH) of the cellulose derivative is 0.1 to 1.0. The method for calculating the weight ratio of the effective NCO content contained in the crosslinking agent to the hydroxyl value of the cellulose derivative is as follows. NCO / OH=(parts by mass converted from solid content of polyisocyanate × amount of available NCO contained in polyisocyanate × 56.1) / (parts by mass converted from solid content of cellulose derivative × hydroxyl value contained in cellulose derivative × 42) The hydroxyl value is mg of potassium hydroxide equivalent to the hydroxyl groups per gram of sample, the molecular weight of potassium hydroxide was 56.1 g / mol, and the formula weight of NCO was 42 g / mol.

[0062] The metal organic frameworks, binders, and crosslinking agents used in each of the examples and comparative examples are as follows.

[0063] (Metal-organic structure) MIL-101(Cr) was used in Examples 1 to 5 and Comparative Examples 1 to 10. MIL-101(Cr) was synthesized by the method described in "Kunyue Leng et al., "Rapid Synthesis of Metal-Organic Frameworks MIL-101(Cr) Without the Addition of Solvent and Hydrofluoric Acid", Cryst. Growth Des. 2016, 16, 1168-1171." MIL-101(Cr) has a specific surface area of ​​3,229 m2 measured by the BET method. 2 / g and the pore volume is 1.55 cm 3 / g.

[0064] (binder) In Examples 1 to 5 and Comparative Examples 2 and 10, hydroxypropyl cellulose (HPC) (manufactured by Wako Pure Chemical Industries, Ltd.) was used, which had a solid content of 2.0 wt% and a viscosity of 150 to 400 (mPa s) at a temperature of 20° C. Here, the hydroxyl value of hydroxypropyl cellulose (HPC) was 350 (mgKOH / g). In Comparative Example 3, silicone (KR-400, manufactured by Shin-Etsu Chemical Co., Ltd.) was used. In Comparative Example 4, polyacrylic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., molecular weight 25,0000) was used. In Comparative Example 5, an ionomer (MYE25A, manufactured by Maruyoshi Chemical Co., Ltd.) was used. In Comparative Example 6, latex (Resitex S-500, manufactured by Resitex Co., Ltd.) was used. In Comparative Example 7, polyurethane (manufactured by Nagase ChemteX Corporation) was used. In Comparative Example 8, a styrene-acrylic copolymer (Saibinol EK-61, manufactured by Saiden Chemical Co., Ltd.) was used. In Comparative Example 9, an ethylene-vinyl acetate copolymer (Sumikaflex 355HQ, manufactured by Sumitomo Chemical Co., Ltd.) was used.

[0065] (Crosslinking agent) In Examples 1 to 5 and Comparative Example 10, a polyisocyanate (Burnoc DNW-5500, manufactured by DIC Corporation) was used as a crosslinking agent. The effective NCO content of the polyisocyanate used here was 13.3 (mgNCO / g), and the mass equivalent to the solid content was 79.6%. In Examples 1 to 5, the crosslinking agent was added so that the NCO / OH ratio was 0.1 to 1.0, and in Comparative Example 10, the crosslinking agent was added so that the NCO / OH ratio was 0.050.

[0066] 2. Dispersibility evaluation The appearance of the prepared compositions was visually observed to evaluate dispersibility. In Table 1, compositions that were uniform in appearance were marked with "○", and compositions that were non-uniform due to the occurrence of unevenness or lumps (aggregates) were marked with "×".

[0067] 3. Coatability evaluation Both ends of a stainless steel test piece were protected with mending tape, and the liquid composition was dropped onto the surface of the test piece, and then spread evenly with a glass rod. After confirming that the composition had become uniform by appearance, the mending tape was peeled off, and the behavior of the composition was observed and evaluated. In Table 1, the composition was marked as "○" when it was maintained without spreading on the test piece, "△" when the composition was not seen to spread on the test piece when the mending tape was peeled off, but spread when the test piece was moved, and "×" when the composition spread on the test piece when the mending tape was peeled off. In addition, the composition was marked as "-" when the coatability was not evaluated because the dispersibility was extremely poor.

[0068] 4. Coating condition evaluation In the above coating property evaluation, each composition was applied onto a test piece, dried at 50°C for at least 1 hour to remove most of the moisture, and then heated at 80°C for at least 1 hour. The appearance of the dried coating film was visually observed and evaluated. In Table 1, coating films with no cracks on the surface were marked with "○", those with minute cracks were marked with "△", and those that formed a coating film but did not adhere to the test piece were marked with "×". Those that were not evaluated were marked with "-".

[0069] 5. Strength evaluation Among the above coating film condition evaluations, for those in which the coating film was adhered to the test piece at room temperature, a peeling tape (manufactured by Nichiban Co., Ltd., product name "Cellotape (registered trademark)" (CT405-AP24)) was applied on top of the coating film to adhere it, and the strength of the coating film was evaluated based on whether or not the coating film peeled off from the test piece when it was peeled off in the vertical direction. In Table 1, those that did not peel off are marked with "○", and those that peeled off are marked with "×". Also, those that were not evaluated are marked with "-". Furthermore, for samples that showed good peel strength at room temperature (evaluated as ○), they were immersed in boiling water for one hour or more and then similar evaluation was performed immediately after removal. The evaluation criteria were the same as above.

[0070] 6. Measurement of water vapor adsorption amount The water vapor adsorption amount was measured for the composite obtained by vacuum drying the composition prepared in "1. Preparation of composition" at 150°C overnight or more. BERSORP Aqua (manufactured by Microtrack Bell Co., Ltd.) was used for the measurement. Table 1 shows the water vapor adsorption amount when the water vapor partial pressure was about 0.90 under the condition of an adsorption temperature of 25°C. The water vapor adsorption amount value in Table 1 is a numerical value for the composite per unit mass. Since Comparative Example 1 does not contain a binder, the numerical value in Table 1 is the water vapor adsorption amount by the metal organic framework as it is. For the purposes of comparison, Examples 1 to 5 and Comparative Examples 2, 8, and 9 are values ​​that are divided back so that the mass of the metal organic framework contained in the composite is the same as that of Comparative Example 1. In addition, "-" is used for those for which the water vapor adsorption amount was not measured.

[0071] 7. Moisture absorption performance evaluation The moisture absorption performance of Examples 1 to 5 and Comparative Examples 1 to 3 and 8 to 10 was evaluated based on Comparative Example 1, which did not contain a binder. In Table 1, samples that showed a water vapor adsorption amount of 60% or more of the standard were evaluated as "◎", samples that showed a water vapor adsorption amount of 50% or more of the standard were evaluated as "◯", and samples that showed a water vapor adsorption amount of less than 50% of the standard were evaluated as "△".

[0072] As shown in Table 1, Examples 1 to 5, which used a cellulose derivative and a crosslinking agent as a binder, received favorable evaluations in terms of dispersibility, coatability, coating film condition, strength, water vapor adsorption amount, moisture absorption performance, and adhesive strength after immersion in hot water.

[0073] On the other hand, Comparative Example 1, which had good dispersibility, did not receive a good evaluation for coatability. In Comparative Examples 3 to 9 in which no cellulose derivative was used as a binder, Comparative Examples 4 to 7 had problems with dispersibility. In Comparative Example 3 in which dispersibility was good, good evaluations were not obtained for the coatability, state of the coating film, and strength of the coating film. In Comparative Examples 8 and 9, although the coatability was good, good evaluations were not obtained for the state of the coating film and strength of the coating film. That is, in Comparative Examples 3, 8, and 9, unlike Examples 1 to 5, none of them obtained good evaluations for all evaluation items. Comparative Examples 2 and 10 were evaluated as being good in terms of dispersibility, coatability, coating film condition, strength, water vapor adsorption amount, and moisture absorption performance, but the adhesive strength after immersion in warm water was significantly reduced.

[0074] Furthermore, even when the test pieces for the composition of Example 4 were changed to copper, aluminum, or glass, the evaluation results obtained in terms of coatability, coating condition, and coating strength were comparable to those obtained when stainless steel test pieces were used.

[0075] In this way, by including a cellulose derivative as a binder in the composite, the composite is uniformly dispersed in the composition, the composition has good coating properties that allow it to be used as a paint, a high-quality coating film with high strength is formed, and the moisture absorption performance of the coating film is also excellent. Furthermore, it was confirmed that by adding a crosslinking agent, the composite containing the metal-organic framework and the cellulose derivative has water resistance even in water and hot water and can maintain adhesive strength, and it was confirmed that the composite has the excellent adsorption performance of the metal-organic framework, as well as the properties of imparting dispersibility, adhesiveness, water resistance, and viscosity.

[0076] In addition, the configurations disclosed in the above-mentioned embodiments (including other embodiments, the same applies below) can be applied in combination with configurations disclosed in other embodiments, provided that no contradiction arises. Furthermore, the embodiments disclosed in this specification are illustrative, and the embodiments of the present invention are not limited thereto, and can be appropriately modified within the scope that does not deviate from the purpose of the present invention. [Industrial Applicability]

[0077] The composite, composition, coating material, adsorbent, and method for producing a composition according to the present invention can be used in applications that utilize the properties of the metal-organic framework.

Claims

1. A composite comprising a metal-organic framework, a cellulose derivative, and a crosslinking agent.

2. The composite according to claim 1 , wherein the cellulose derivative has a hydrophilic group.

3. The complex according to claim 2 , wherein the hydrophilic group is represented by any one of the following formulas (1) to (4): 【Chemistry 1】 【Chemistry 2】 【Chemistry 3】 【Chemistry 4】 (In formula (4), R is Na, K, NH 4 or H)

4. The composite of claim 1 , wherein the cellulose derivative is non-ionic.

5. 2. The complex according to claim 1, wherein the cellulose derivative comprises at least one selected from the group consisting of hydroxypropyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose, methyl cellulose, and carboxymethyl cellulose.

6. 2. The composite according to claim 1, wherein the cellulose derivative has a viscosity of 15 (mPa·s) or more at 20° C. in an aqueous solution having a solid content of 2.0 wt %.

7. The composite according to claim 1 , wherein the cellulose derivative is contained in an amount of 1 part by mass or more and 100 parts by mass or less in terms of solid content relative to 100 parts by mass of the solid content of the metal-organic framework.

8. The composite according to claim 1 , wherein the metal organic framework contains one selected from the group consisting of Fe, Zn, Cr, Cu, and Al as a central metal.

9. The complex according to claim 1 , wherein the crosslinking agent is a substance having a hydrophilic group.

10. The composite of claim 9 , wherein the crosslinking agent comprises at least one of an epoxy resin, a melamine resin, and a polyisocyanate.

11. The composite according to claim 10, wherein an equivalent ratio of isocyanate to hydroxyl groups of the cellulose derivative is 0.10 or more and 1.0 or less.

12. A composition comprising the complex according to any one of claims 1 to 11 in water or an organic solvent.

13. A paint comprising the complex according to any one of claims 1 to 11 in water or an organic solvent such that the proportion of the water or the organic solvent is 50 wt % or more.

14. An adsorbent comprising the composite according to any one of claims 1 to 11, which adsorbs at least one of water and carbon dioxide.

15. A method for producing a composition containing a composite including a metal organic framework, a cellulose derivative, and a crosslinking agent, comprising: A method for producing a composition, comprising: mixing a dispersion of the metal organic framework, a dispersion of the cellulose derivative, and a dispersion of the crosslinking agent.

16. The method for producing a composition according to claim 15, wherein the dispersion liquid of the metal organic framework is a dispersion liquid in which the metal organic framework is dispersed in water or an organic solvent at a solid content concentration of 5.0 wt % or more and 40 wt % or less.

17. The method for producing a composition according to claim 15 or 16, wherein the dispersion of the cellulose derivative is a dispersion in which the cellulose derivative is dispersed in water or an organic solvent at a solid content concentration of 0.50 wt % or more and 30 wt % or less.

Citation Information

Patent Citations

  • Water dispersion of organic polyisocyanate compound

    JP1989006037A

  • Water-base coating composition

    JP1995053907A

  • Film-like composition, manufacturing method thereof, and coating slip

    JP2019171259A

  • Aqueous dispersion for forming gas barrier film-like body, gas barrier film-like body, gas barrier laminate and manufacturing method of gas barrier film-like body

    JP2020143247A

  • Molded sheet containing porous metal complex

    JP2022164183A

Cited By

  • Composite, composition, paint, adsorbent, and method for producing the composition

    JP2026161914A