Device for manufacturing polyethylene terephthalate melt blown fiber web, and manufacturing method for polyethylene terephthalate melt blown fiber web using the same
The PET melt-blown fiber manufacturing apparatus addresses non-uniform crystallization and thickness issues by using a pressure belt and hot air system for uniform crystallization and adjustable thickness control, improving productivity and dimensional stability.
Patent Information
- Application Number
- JP2023147882
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2023-09-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-09-12
AI Technical Summary
Conventional PET melt-blown fiber webs face issues with non-uniform crystallization rates and thickness variation due to uneven heat treatment, leading to dimensional instability and production challenges.
A PET melt-blown fiber manufacturing apparatus and method that utilizes a perforated pressure belt and hot air supply chamber to uniformly crystallize PET melt-blown fibers under pressure, allowing for adjustable thickness control through a height-adjustable mechanism.
The apparatus achieves uniform crystallization and high-speed production of PET melt-blown fibers with consistent thickness, enhancing productivity and flexibility in manufacturing.
Smart Images

Figure 2024144009000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an apparatus for producing a PET meltblown fiber web and a method for producing a PET meltblown fiber web using the same. [Background technology]
[0002] Here, background art related to the present invention is provided, which does not necessarily mean that it is a known art. The meltblown method generally uses polypropylene (PP) as a raw material to produce a fiber web, and the PP meltblown fiber web is widely used as various high-performance filters, oil-absorbing cloths, heat insulating materials, sound absorbing materials, etc.
[0003] However, polypropylene (PP) has a characteristic that its melting point is about 160°C, making it difficult to apply in industrial fields that require high heat resistance of 150°C or more. To solve this problem, polyethylene terephthalate (PET) meltblown fiber webs, which have excellent heat resistance, physical properties, and recyclability, and have a melting point of about 255°C, are widely used.
[0004] However, PET meltblown fiber webs have a slower crystallization rate than other crystalline polymeric materials, and shrinkage occurs at around 70℃ (near the glass transition temperature, Tg), making it difficult to immediately use in products without post-processing such as heat treatment.The reason shrinkage occurs is that polymeric materials have crystalline and non-crystalline regions, and in the glass transition temperature range, the non-crystalline regions become mushy, losing their existing shape and causing shrinkage.
[0005] Conventionally, the heat treatment of PET meltblown fiber webs is carried out by applying hot air at a temperature of 100° C. to 200° C. on a foaming table where the fiber web is collected.
[0006] However, when the conventional PET meltblown fiber web is heat-treated, hot air is not uniformly transferred at a uniform temperature to the PET meltblown fiber web collected on the forming table, resulting in differences in crystallization speed, which not only results in differences in size and thickness of the produced PET meltblown fiber web, but also in the formation of an uneven fiber web. In addition, when the conventional PET meltblown fiber web is heat-treated, there is another problem in that the thickness of the produced fiber web cannot be controlled. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Korean Patent No. 10-0393869 [Patent Document 2] Korean Patent No. 10-0714340 [Patent Document 3] Korean Patent Publication No. 10-1988-0005308 [Patent Document 4] Korean Patent No. 10-0466556 Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a PET meltblown fiber manufacturing apparatus that crystallizes a PET meltblown fiber web at a high speed to improve dimensional stability and productivity, and a method for manufacturing a PET meltblown fiber web using the same.An object of the present invention is to provide a PET meltblown fiber manufacturing apparatus that makes it possible to adjust the thickness of the manufactured PET meltblown fiber web, and a method for manufacturing a PET meltblown fiber web using the same.In addition, the problems to be solved by the present invention are not limited to the technical problems mentioned above, and other technical problems not mentioned will be clearly understood by those skilled in the art to which the present invention pertains from the following description. [Means for solving the problem]
[0009] A general summary of the invention is provided herein, which should not be construed as limiting the scope of the invention.
[0010] The present invention provides a PET meltblown fiber web manufacturing apparatus, which includes an extruder for melt-extrusion of PET resin, a die for receiving the molten resin extruded by the extruder and emitting extremely thin PET meltblown fibers in the direction of its own weight, a forming table installed below the die and collecting and consolidating the PET meltblown fibers to form a PET meltblown fiber web, a winder for winding up the PET meltblown fiber web, and a blending nozzle for blending PET short fibers with the PET meltblown fibers emitted toward the forming table. The web manufacturing apparatus includes a heat treatment machine that pressurizes and heat-treats a PET meltblown fiber web formed on a forming table, and the heat treatment machine includes a porous pressure belt that presses the PET meltblown fiber web toward the forming table and transfers the PET meltblown fiber web toward a winder together with the porous circulation belt of the forming table, a hot air supply chamber that supplies high-temperature hot air to the PET meltblown fiber web so that the PET meltblown fiber web transferred under pressure by the porous pressure belt is crystallized, and a height adjustment means that adjusts the height of the porous pressure belt that presses the PET meltblown fiber web.
[0011] In an apparatus for producing PET meltblown fiber according to one aspect of the present invention, the porous pressure belt is provided as a mesh belt, and is rotatably installed on a carrier roller rotatably installed between a pair of belt frames and a drive roller of a belt drive motor. The porous pressure belt passing through the lower end side of the belt frame is installed lower than the lower end of the belt frame and horizontally passes through carrier rollers installed on both sides of the lower end of the belt frame, and can transfer the PET meltblown fiber web to the winder side together with the porous circulation belt while pressing the surface of the PET meltblown fiber web against the porous circulation belt.
[0012] In an apparatus for producing PET meltblown fiber according to an aspect of the present invention, the hot air supply chamber is installed between the belt frames so as not to interfere with the perforated pressure belt, and is filled with hot air blown from a hot air passage installed outside the heat treatment machine. A number of hot air injection nozzles may be formed at the bottom of the hot air supply chamber to inject hot air toward the PET meltblown fiber web.
[0013] In the PET meltblown fiber manufacturing apparatus according to one aspect of the present invention, the height adjustment means is installed on a height adjustment frame fixedly installed at a distance from the upper side of the perforated pressure belt, and the height adjustment means may include a height adjustment servomotor installed in a gear box installed on the upper surface of the height adjustment frame, and a lifting bar that lifts and lowers the perforated pressure belt in cooperation with the height adjustment servomotor.
[0014] In an apparatus for producing PET meltblown fiber according to one aspect of the present invention, a pinion gear is installed on an output shaft that rotates by the operation of a height-adjusting servomotor, and a lifting bar is installed in a gear box so as to be movable up and down. A lower end of the lifting bar passes through the height-adjusting frame and is connected to an outer surface of the belt frame. A rack gear that meshes with the pinion gear may be formed on the lifting bar by extending along the length of the lifting bar.
[0015] The method for producing PET meltblown fiber according to the present invention includes a PET meltblown fiber emitting step of melting and emitting PET raw material in a meltblown manner to form PET meltblown fiber, a PET meltblown fiber web forming step of collecting and consolidating the PET meltblown fiber seated on a perforated circulation belt to form a PET meltblown fiber web, and a pressurized heat treatment step of applying high-temperature hot air to the PET meltblown fiber web to crystallize the PET meltblown fiber web.
[0016] In the PET meltblown fiber radiation step of the PET meltblown fiber manufacturing method according to another aspect of the present invention, the PET meltblown fiber is spun at a temperature of 270 to 330°C for 25 to 60 m. 3 / min and can be emitted to have a diameter of 2 to 5 μm.
[0017] In the PET meltblown fiber emitting step of the PET meltblown fiber producing method according to another aspect of the present invention, the PET meltblown fiber emitting is mixed with PET short fibers having a diameter of 15 to 40 μm, and the PET short fibers may be mixed with the PET meltblown fiber in a ratio of 3:7.
[0018] In the process for producing the PET meltblown fiber according to another aspect of the present invention, in the step of forming the PET meltblown fiber web, the perforated circulating belt is moved at a speed of 1 to 10 m / min, and the perforated circulating belt is provided with a density of 100 to 700 g / m 2 A PET meltblown fibrous web having a weight of
[0019] In the step of pressurizing and heat-treating the PET meltblown fiber web in the method for producing the PET meltblown fiber according to another aspect of the present invention, the perforated pressurizing belt rotates at a speed of 1 to 10 m / min along the transport direction of the PET meltblown fiber web, and the hot air supply chamber blows hot air of 80 to 200° C. through a hot air injection nozzle at a speed of 1 to 10 m. 3 It can be sprayed at a speed of / min.
[0020] In the pressurized heat treatment step of the PET meltblown fiber web in the method for producing the PET meltblown fiber according to another aspect of the present invention, the porous pressurizing belt has a gap of 1 to 150 mm from the porous circulating belt, so that the PET meltblown fiber web can be pressurized and transferred. Effect of the Invention
[0021] According to the present invention, since the collected fiber web is heat-treated while being pressurized, the fiber web can be crystallized uniformly and at a high speed, and the productivity of the PET meltblown fiber web can be improved by shortening the heat treatment time. According to the present invention, since the collected fiber web is heat-treated while being pressurized, a PET meltblown fiber web having a uniform thickness can be produced. According to the present invention, since the pressure height of the collected fiber web can be adjusted, a PET meltblown fiber web having various thicknesses can be produced. [Brief description of the drawings]
[0022] [Figure 1] 1 is a schematic diagram of a manufacturing apparatus for a PET meltblown fiber web according to the present invention. [Diagram 2] 2 is a diagram illustrating the heat treatment machine of FIG. 1. [Diagram 3] 1 is a flow chart that illustrates a schematic method for producing a PET meltblown fibrous web according to the present invention. [Figure 4] 4 is a flow chart that generally illustrates the emission stage of the PET meltblown fiber of FIG. 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an embodiment of a PET meltblown fiber web manufacturing apparatus and a PET meltblown fiber web manufacturing method using the same according to the present invention will be described in detail with reference to the drawings.
[0024] It is clear that the essential technical idea of the present invention does not limit its possible implementation by the embodiments described below, but includes a range that can be easily proposed by a person skilled in the art by replacing or modifying the embodiments described below based on the essential technical idea of the present invention. Furthermore, since the terms used below are selected for the convenience of explanation, they should not be limited to their dictionary meanings when grasping the essential technical idea of the present invention, but should be appropriately interpreted in a meaning that corresponds to the technical idea of the present invention.
[0025] Fig. 1 is a schematic diagram of a manufacturing apparatus for a PET meltblown fiber web according to the present invention. Referring to Fig. 1, the manufacturing apparatus 100 for a PET meltblown fiber web according to the present invention has a similar configuration to that of a conventional meltblown fiber web manufacturing apparatus (equipment). In other words, the manufacturing apparatus 100 for a PET meltblown fiber web according to the present invention includes an extruder 10 for melt-extrusion of a PET (polyethylene terephthalate) resin, a die 20 for receiving the molten resin extruded by the extruder 10 and emitting PET meltblown fibers F that are extremely thin in the direction of its own weight, a forming table 30 that is installed below the die 20 and collects and gathers the PET meltblown fibers F to form a PET meltblown fiber web W, and a winder 40 for winding up the PET meltblown fiber web W.
[0026] In addition, the PET meltblown fiber web manufacturing apparatus 100 according to the present invention further includes a two-fluid nozzle 50 for spraying fine liquid droplets onto the PET meltblown fibers F emitted toward the forming table 30, and a blending nozzle 60 for air-blending (mixing) the PET short fibers S into the PET meltblown fibers F emitted toward the forming table 30, similar to conventional meltblown fiber web manufacturing apparatuses.
[0027] Here, the configurations of the extruder 10, die 20, forming table 30, winder 40, two-fluid nozzle 50 and blending nozzle 60 and their operational relationships are well known in the art, so detailed explanations will be omitted.
[0028] Meanwhile, the PET meltblown fiber web manufacturing apparatus 100 according to the present invention, unlike conventional meltblown fiber web manufacturing apparatuses, further includes a heat treatment device 110 for pressurizing and heat-treating the PET meltblown fiber web W collected and gathered on the forming table 30.
[0029] Figure 2 is a schematic diagram of the heat treatment machine shown in Figure 1. Referring to Figure 2, the heat treatment machine 110 of the PET meltblown fiber web manufacturing apparatus 100 according to the present invention includes a perforated pressure belt 120, a hot air supply chamber 130 and a height adjustment means 140.
[0030] First, the porous pressure belt 120 presses the PET meltblown fiber web W formed on the forming table 30 toward the forming table 30, and transfers the PET meltblown fiber web W toward the winder 40 together with the porous circulation belt 32 of the forming table 30. The porous pressure belt 120 is provided as a mesh belt, and is provided in a closed loop shape with one end and the other end connected in an endless manner.
[0031] In the present invention, the porous pressure belt 120 is not particularly limited, but is provided as a normal mesh belt as an example. The porous pressure belt 120 is rotatably mounted on a carrier roller 124 rotatably mounted between a pair of belt frames 122 and a drive roller 128 of a belt drive motor 126.
[0032] At this time, the porous pressure belt 120 passing along the lower end side of the belt frame 122 is installed so as to pass horizontally over carrier rollers 124 installed on both sides of the lower end of the belt frame 122, lower than the lower end of the belt frame 122. In this manner, the face surface of the porous pressure belt 120 passing horizontally along the lower end side of the belt frame 122 presses the surface of the PET meltblown fiber web W, which is transferred to the winder 40 side by the operation of the porous circulating belt 32 of the forming table 30, toward the porous circulating belt 32 of the forming table 30, and transfers the PET meltblown fiber web W to the winder 40 side together with the porous circulating belt 32.
[0033] For this reason, the porous pressure belt 120 is circulated along the transport direction of the PET meltblown fiber web W by the operation of the belt drive motor 126, and the belt drive motor 126 circulates and rotates the porous pressure belt 120 at the same speed as the transport speed of the porous circulation belt 32 of the forming table 30, preferably at a speed of 1 to 10 m / min. The face surface of the porous pressure belt 120 horizontally passing through the lower end side of the belt frame 122 has a pressure position for pressing the PET meltblown fiber web W adjusted by the operation of the height adjustment means 140, so that the PET meltblown fiber web W can be manufactured to have various thicknesses.
[0034] The hot air supply chamber 130 supplies high-temperature hot air to the PET meltblown fiber web W, which is pressurized and transported by the porous pressure belt 120, so that the PET meltblown fiber web W is crystallized. The hot air supply chamber 130 is installed between a pair of belt frames 122 so as not to interfere with the rotating porous pressure belt 120, and is connected to a hot air duct (not shown) installed outside the heat treatment machine 110. At this time, the inside of the hot air supply chamber 130 is filled with hot air blown from the hot air duct. A number of hot air injection nozzles 132 are formed in a number of rows and columns at the bottom of the hot air supply chamber 130, which inject the hot air from inside the hot air supply chamber 130 toward the PET meltblown fiber web W.
[0035] The hot air supply chamber 130 thus installed blows hot air of 80 to 200° C. through a number of hot air injection nozzles 132 at a depth of 1 to 10 m. 3 The hot air is sprayed onto the PET meltblown fiber web W at a speed of 1000 / min. Since the PET meltblown fiber web W is pressurized by the perforated pressure belt 120, the hot air sprayed through the multiple hot air spray nozzles 132 can be delivered to the front and back sides of the PET meltblown fiber web W at a uniform temperature, so that the PET meltblown fiber web W is uniformly crystallized (heat-treated).
[0036] The height adjusting means 140 adjusts the height of the perforated pressure belt 120 which presses the PET meltblown fiber web W, thereby manufacturing the PET meltblown fiber web W with various thicknesses. One or more height adjusting means 140 is installed on a height adjusting frame 142 which is fixedly installed at a distance from the upper side of the perforated pressure belt 120. FIG. 2 shows a state in which two height adjusting means 140 are installed on the height adjusting frame 142. The height adjusting means 140 includes a height adjusting servo motor 146 and a lifting bar 150 which lifts and lowers the perforated pressure belt 120 in cooperation with the height adjusting servo motor 146.
[0037] The height adjustment servomotor 146 is installed in a gear box 144 installed on the upper surface of the height adjustment frame 142 as shown in the figure. At this time, a pinion gear 148 that meshes with a lifting bar 150 via the gear box 144 is installed on an output shaft (not shown) that rotates by the operation of the height adjustment servomotor 146.
[0038] The lifting bar 150 is provided in the form of a vertically extending bar and is installed in the gear box 144 so as to be movable up and down. At this time, the lower end of the lifting bar 150 passes through the height adjustment frame 142, and the lower end of the lifting bar 150 passing through the height adjustment frame 142 is connected to the outer surface of the belt frame 122 so as not to interfere with the perforated pressure belt 120. In addition, the lifting bar 150 is formed with a rack gear 152 that meshes with the pinion gear 148 and extends along the length of the lifting bar 150.
[0039] That is, when the height adjustment servo motor 146 rotates the output shaft to one side or the other, the pinion gear 148 also rotates to one side or the other along the output shaft, and as the pinion gear 148 rotates to one side or the other, the lifting bar 150, which has a rack gear 152 with which the pinion gear 148 meshes, moves up and down. As a result, the belt frame 122 and the perforated pressure belt 120 move up and down along the lifting bar 150, and their heights are adjusted.
[0040] Preferably, the height adjusting means 140 enables the porous pressure belt 120 to pressurize and transfer the PET meltblown fiber web W so that the gap between the porous circulation belt 32 of the forming table 30 and the porous pressure belt 120 is adjusted to a distance of 1 to 150 mm.
[0041] The following describes a method for manufacturing a PET meltblown fiber web using a manufacturing apparatus for a PET meltblown fiber web. Among the accompanying drawings, Figures 3 and 4 are flow charts that show a schematic diagram of a method for manufacturing a PET meltblown fiber web according to the present invention, and the method for manufacturing a PET meltblown fiber web according to the present invention includes a step of emitting PET meltblown fibers (S10), a step of forming a PET meltblown fiber web (S20), and a step of pressurizing and heat-treating the PET meltblown fiber web (S30).
[0042] Radiation stage of PET meltblown fiber (S10) The PET meltblown fiber emission step (S10) is a step of forming PET meltblown fiber F by melt-blowing PET (polyethylene terephthalate) polymer resin (S10).
[0043] The PET meltblown fibers F formed in the PET meltblown fiber emission step (S10) are melted and emitted vertically toward the perforated circulation belt 32 side through the die 20 that faces the perforated circulation belt 32 of the forming table 30 in a vertical direction. Here, the forming table 30 collects and gathers the PET meltblown fibers F to manufacture a PET meltblown fiber web W in the subsequent PET meltblown fiber web formation step (S20).
[0044] Meanwhile, the PET meltblown fiber radiation step (S10) will be described. The PET meltblown fiber radiation step (S10) includes a PET raw material charging step (S10-1), a PET raw material extrusion step (S10-2), and a PET raw material radiation step (S10-3). The PET raw material charging step (S10-1) is a step (S10-1) of charging the prepared PET raw material into a dry hopper (not shown) connected to the extruder 10, and in the PET raw material charging step (S10-1), the PET raw material can be charged into the dry hopper through a normal spring conveyor.
[0045] The PET raw material loaded into the dry hopper is transferred to the extruder 10 installed at the lower side of the dry hopper, and in the process of being transferred from the dry hopper to the extruder 10, the PET raw material can be dried by hot air to have a moisture content of about 0.01 to 1.0%. The PET raw material extrusion step (S10-2) is a step of receiving the PET raw material from the dry hopper, melting the PET raw material while transferring it, and extruding the molten PET raw material (S10-2), and in the PET raw material extrusion step (S10-2), the PET raw material can be extruded at a speed of 1,250 g / min while maintaining a temperature of 280 to 300°C.
[0046] Here, if the PET raw material is extruded at a temperature below 280°C, not only will the flowability be reduced, causing stress, but the molecular weight will also increase, which may cause changes in physical properties. On the other hand, if the PET raw material is extruded at a temperature above 300°C, thermal decomposition may cause a decrease in molecular weight, which may cause physical properties to deteriorate and lead to yellowing.
[0047] In addition, the extrusion speed of the PET raw material can be set differently depending on the melting temperature, but if the extrusion speed of the PET raw material is too slow, the residence time in the extruder becomes long, causing a decrease in molecular weight due to thermal decomposition, and if the extrusion speed is too fast, there is a risk of the raw material not being melted. Therefore, the extrusion speed of the PET raw material is preferably 1,250 g / min. The molten PET raw material extruded from the extruder can be supplied to the PET raw material ejection step (S10-3) via a conventional screen changer (not shown) and gear pump (not shown).
[0048] The PET raw material ejection step (S10-3) is a step (S10-3) in which the molten PET raw material supplied in the PET raw material extrusion step (S10-2) is ejected in the form of ultra-thin fibers, PET melt-blown fibers, using high-temperature, high-pressure gas. The molten PET raw material supplied in the PET raw material ejection step (S10-3) flows in the direction of its own weight through the ejection nozzle installed at the bottom of the die 20 via the die 20, and the molten PET raw material flowing through the ejection nozzle is elongated in the direction of its own weight and its diameter is reduced by the high-temperature, high-pressure gas sprayed from the side of the ejection nozzle, so that it can be ejected in the form of ultra-thin PET melt-blown fibers F.
[0049] Here, the high-temperature, high-pressure gas may be at 310 to 330°C, and the 3 The high-temperature, high-pressure gas may be sprayed at a speed of 1000 / min. However, if the temperature of the high-temperature, high-pressure gas is less than 310°C, the sprayed PET meltblown fiber F will cool quickly and become a hard fiber instead of a soft fiber, and if the temperature of the high-temperature, high-pressure gas exceeds 330°C, thermal decomposition will occur and the fiber will turn yellow.
[0050] Preferably, in the PET meltblown fiber emission step (S10), the PET meltblown fiber F is emitted to have a diameter of 2 to 10 μm. If the diameter of the PET meltblown fiber F is less than 2 μm, the ease of workability is poor and it is difficult to form stable process conditions, and if the diameter of the PET meltblown fiber F exceeds 10 μm, the sound absorption performance is reduced.
[0051] Meanwhile, in the PET meltblown fiber emission step (S10), a PET staple fiber air blending step (not shown) for mixing PET staple fibers S may be optionally added. The PET staple fiber air blending step is for imparting bulkiness to the PET meltblown fiber web W produced, and the PET staple fibers S may be air blended (mixed) with the PET meltblown fibers F emitted toward the forming table 30 through a blending nozzle 60.
[0052] Here, the PET short fibers S have a diameter of 15 to 40 μm. If the diameter of the PET short fibers S is 15 μm, it is difficult to impart bulkiness to the PET melt-blown fiber web W produced. If the diameter of the PET short fibers S exceeds 40 μm, the bulkiness is improved, but the cotton density of the PET melt-blown fiber web W produced is inferior, resulting in reduced sound absorption performance.
[0053] For example, to improve sound absorption performance in the low frequency range (1,000Hz or less), PET meltblown fiber F and PET staple fiber S are blended in a ratio of 3:7, and to improve sound absorption performance in the mid to high frequency range (1,000Hz or more), PET meltblown fiber F and PET staple fiber S are blended in a ratio of 7:3. In other words, the blending ratio of PET meltblown fiber F and PET staple fiber S may vary depending on the use of the manufactured PET meltblown fiber web, and generally, PET meltblown fiber F and PET staple fiber S are blended in a ratio of 5:5.
[0054] PET meltblown fiber web forming stage (S20) The PET meltblown fiber web forming step (S20) is a step of collecting and consolidating the PET meltblown fibers F seated on the perforated circulation belt 32 of the forming table 30 to form a PET meltblown fiber web W (S20).
[0055] In the step of forming the PET meltblown fiber web (S20), the PET meltblown fibers F are collected on the circulating porous circulating belt 32 and transported along the circulating porous circulating belt 32, and the PET meltblown fibers F transported along the circulating porous circulating belt 32 are bonded by a conventional suction means provided on the forming table 30 to form a PET meltblown fiber web W.
[0056] Here, the forming table 32 may be disposed 10 to 100 cm away from the emitting nozzle for melting and emitting the PET meltblown fiber F, and the perforated circulation belt 32 may be moved at a speed of 1 to 10 m / min. Thus, the perforated circulation belt 32 may have a melting point of 100 to 700 g / m. 2 However, if the distance between the forming table 32 and the radiating nozzle and the transport speed of the perforated circulating belt 32 are less than or greater than the critical value, the weight of the PET meltblown fiber web W may be 100 to 700 g / m. 2 Therefore, it becomes impossible to form a PET meltblown fiber web W having a weight of 100 g / m.
[0057] For example, in the step of forming the PET meltblown fiber web (S20), if the transport speed of the perforated circulating belt 32 is set at 5 m / min, the fiber web can have a weight of 400 g / m 2 A PET meltblown fiber web W having a weight of 1000 g may be formed. In addition, in the PET meltblown fiber web forming step (S20), the present invention does not particularly limit the suction pressure of the suction means, but it is set within a range in which the collected PET meltblown fiber web W is not excessively dense and the PET meltblown fiber web W does not scatter. In this way, the PET meltblown fiber web W formed in the PET meltblown fiber web forming step (S20) is transferred to the winder 40 side.
[0058] Pressurized heat treatment step (S30) of PET meltblown fiber web The pressurized heat treatment step (S30) of the PET meltblown fiber web is a step (S30) of crystallizing the PET meltblown fiber web W by applying pressure to the PET meltblown fiber web W while providing high-temperature hot air so as not to interfere with the transport of the PET meltblown fiber web W formed in the preceding PET meltblown fiber web formation step (S20).
[0059] In the pressurized heat treatment step (S30) of the PET meltblown fiber web, the PET meltblown fiber web W formed on the forming table 30 is pressed toward the porous circulation belt 32 of the forming table 30 by the porous pressure belt 120 of the heat treatment machine 110, and the PET meltblown fiber web W pressed by the porous pressure belt 120 is crystallized by high-temperature hot air sprayed through the hot air spray nozzle 132 formed in the hot air supply chamber 130 of the heat treatment machine 110.
[0060] At this time, the porous pressure belt 120 rotates at a speed of 1 to 10 m / min, which is the same as the moving speed of the porous circulation belt 32, and circulates along the moving direction of the PET meltblown fiber web W. Then, the hot air injection nozzle 132 blows high-temperature hot air of 80 to 200° C. at a speed of 1 to 10 m. 3 The hot air can be sprayed at a speed of 6 m / min. 3 / min.
[0061] Here, if the high-temperature hot air is less than 80°C, crystallization of the amorphous region does not occur even if stabilization heat treatment is performed at a temperature lower than the PET glass transition temperature and crystallization temperature, and shrinkage occurs at a temperature of 120°C or higher. If the high-temperature hot air exceeds 200°C, shrinkage occurs severely, and the produced PET meltblown fiber web becomes hard and yellowing may occur.
[0062] In addition, the high-temperature hot air is sprayed at a speed of 1 m 3 If the speed is less than 10m / min, the diameter of the produced PET meltblown fiber web will be too large and the fiber will not be formed. 3If the speed exceeds 1 / min, the diameter of the PET meltblown fiber web produced will be small, and the PET meltblown fiber web will not be collected on the forming table 30 but will fly away. In the pressurized heat treatment step (S30) of the PET meltblown fiber web, the porous pressurizing belt 120 forms a gap of 1 to 150 mm with the porous circulating belt 32 of the forming table 30 by the height adjusting means 140 of the heat treatment machine 110 to pressurize and transfer the PET meltblown fiber web W. As a result, the PET meltblown fiber web W can be produced to have various thicknesses corresponding to the gap between the porous pressurizing belt 120 and the porous circulating belt 32.
[0063] Meanwhile, nonwoven fabrics (not shown) may be heat-pressed onto the front and back surfaces of the PET meltblown fiber web W that has been subjected to the pressurized heat treatment step (S30). According to the present invention thus formed, since the PET meltblown fiber web W is heat-treated while being pressurized, the PET meltblown fiber web W can be crystallized uniformly and at a high speed, and the productivity of the PET meltblown fiber web W can be improved by shortening the heat treatment time.
[0064] According to the present invention, since the PET meltblown fiber web W is heat-treated while being pressurized, it is possible to manufacture a PET meltblown fiber web W having a uniform thickness. According to the present invention, since the pressurization height of the PET meltblown fiber web W can be adjusted, it is possible to manufacture a PET meltblown fiber web W having various thicknesses. [Explanation of symbols]
[0065] 10 Expressor 20 Die 30 Forming Table 32 Perforated Circulation Belt 40 Winder 50 Two-fluid nozzle 60 Blending Nozzle 100 PET meltblown fiber web production equipment 110 Heat treatment machine 120 Perforated pressure belt 122 Belt Frame 124 Carrier roller 126 Belt drive motor 128 Drive Roller 130 Hot air supply chamber 132 Hot air nozzle 140 Height adjustment means 142 Height adjustable frame 144 Gearbox 146 Height adjustment servo motor 148 Pinion Gear 150 Lifting bar 152 Rack Gear
Claims
1. An apparatus for producing a PET meltblown fiber web, comprising: an extruder for melt-extrusion of a PET resin; a die for receiving the molten resin extruded by the extruder and emitting PET meltblown fibers which are extremely thinned in the direction of their own weight; a forming table installed below the die and spaced apart to collect and gather the PET meltblown fibers to form a PET meltblown fiber web; a winder for winding up the PET meltblown fiber web; and a blending nozzle for blending PET short fibers with the PET meltblown fibers emitted toward the forming table, The PET meltblown fiber web manufacturing apparatus comprises: A heat treatment device is provided for pressing and heat-treating the PET meltblown fiber web formed on the forming table, The heat treatment machine is A perforated pressure belt that presses the PET meltblown fiber web against the forming table and transfers the PET meltblown fiber web to the winder together with the perforated circulation belt of the forming table; a hot air supply chamber for supplying high-temperature hot air to the PET meltblown fiber web so that the PET meltblown fiber web, which is pressurized and transferred by the perforated pressure belt, is crystallized; and a height adjusting means for adjusting the height of the perforated pressure belt that presses the PET meltblown fiber web.
2. The perforated pressure belt is provided as a mesh belt, The perforated pressure belt is rotatably mounted on a carrier roller rotatably mounted between a pair of belt frames and a drive roller of a belt drive motor, The porous pressure belt passing through the lower end side of the belt frame is installed lower than the lower end of the belt frame so as to pass horizontally through the carrier rollers installed on both sides of the lower end of the belt frame, and the PET meltblown fiber web is transferred to the winder side together with the porous circulation belt while pressing the surface of the PET meltblown fiber web against the porous circulation belt.
3. The hot air supply chamber is installed between the belt frames so as not to interfere with the perforated pressure belt, and is filled with hot air blown from a hot air passage installed outside the heat treatment machine, 3. The apparatus for manufacturing a PET meltblown fiber web according to claim 2, wherein a number of hot air injection nozzles for injecting hot air toward the PET meltblown fiber web are formed in a lower portion of the hot air supply chamber.
4. The height adjusting means is installed on a height adjusting frame fixedly installed at a distance from the upper side of the perforated pressure belt, The height adjustment means is a height adjustment servomotor installed in a gear box installed on an upper surface of the height adjustment frame; 3. The apparatus for producing a PET meltblown fiber web according to claim 2, further comprising a lifting bar for lifting and lowering the perforated pressure belt in cooperation with the height adjusting servo motor.
5. A pinion gear is installed on the output shaft that rotates by the operation of the height adjustment servomotor, the lifting bar is installed in the gear box so as to be liftable, and a lower end of the lifting bar is connected to an outer surface of the belt frame through the height adjustment frame, The apparatus for manufacturing a PET meltblown fiber web according to claim 4, wherein the lift bar is provided with a rack gear, which engages with the pinion gear, extending along a length direction of the lift bar.
6. In the method for producing a PET meltblown fiber web using the PET meltblown fiber web production apparatus of claim 1, A PET meltblown fiber emission step (S10) of melting and emitting a PET raw material in a meltblown manner to form the PET meltblown fiber; (S20) forming a PET meltblown fiber web by collecting and consolidating the PET meltblown fibers seated on the perforated circulation belt to form the PET meltblown fiber web; and (S30) applying high-temperature hot air to the PET meltblown fiber web while applying pressure to the PET meltblown fiber web to crystallize the PET meltblown fiber web.
7. In the PET meltblown fiber emission step (S10), The PET meltblown fiber is spun at a temperature of 270 to 330°C for a length of 25 to 60 m. 3 7. The method for producing a PET meltblown fiber web according to claim 6, wherein the PET meltblown fiber web is emitted at a speed of 1000 rpm / min and has a diameter of 2 to 10 μm.
8. In the PET meltblown fiber emission step (S10), The PET meltblown fibers are mixed with PET short fibers having a diameter of 15 to 40 μm, The method for producing a PET meltblown fiber web according to claim 6, wherein the PET staple fiber is mixed with the PET meltblown fiber in a ratio of 3:
7.
9. In the step of forming the PET meltblown fiber web (S20), The perforated circulating belt is moved at a speed of 1 to 10 m / min, The perforated circulating belt has a thickness of 100 to 700 g / m 27. The method of claim 6, wherein the PET meltblown fibrous web is formed having a weight of about 1000 g / m.
10. In the pressurized heat treatment step (S30) of the PET meltblown fiber web, The perforated pressure belt rotates at a speed of 1 to 10 m / min along the transport direction of the PET meltblown fiber web, The hot air supply chamber blows hot air at a temperature of 80 to 200°C through a hot air nozzle at a depth of 1 to 10 m. 3 The method for producing a PET meltblown fiber web according to claim 6, characterized in that the spraying is performed at a speed of 1000 rpm / min.
11. In the pressurized heat treatment step (S30) of the PET meltblown fiber web, The method for producing a PET meltblown fiber web according to claim 10, wherein the perforated pressure belt is spaced from the perforated circulation belt by 1 to 150 mm to pressurize and transfer the PET meltblown fiber web.
Citation Information
Patent Citations
Heating and molding apparatus for producing nonwoven fabric
JP1983018463A
Special nonwoven fabric
JP1994093550A
Specific nonwoven fabric
JP1994116854A
Formation of non-woven fabric and device for forming the same
JP1997132851A
Thermostable nonwoven web containing meltblown blended polymer fibers