Carbamate compound

A flexible carbamate ester compound with a novel oxyalkylene spacer structure addresses the moldability issues of conventional carbamate esters, enabling the production of soft polyurethane with improved moldability into complex shapes.

JP2024144017APending Publication Date: 2024-10-11MITSUBISHI CHEM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023160735
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2023-09-25
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional carbamate ester compounds used in polyurethane synthesis lack flexibility due to their spacer structures, resulting in high hardness and limited moldability into irregular and complex shapes.

Method used

A novel carbamate ester compound with a flexible oxyalkylene spacer structure, synthesized by reacting specific carbonates with diamines, providing a soft polyurethane with improved moldability.

Benefits of technology

The novel carbamate ester compound enables the production of soft polyurethane with excellent moldability into complex and irregular shapes, enhancing its applicability in various forms.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144017000001
    Figure 2024144017000001
  • Figure 2024144017000002
    Figure 2024144017000002
  • Figure 2024144017000003
    Figure 2024144017000003
Patent Text Reader

Abstract

To provide a novel carbamate compound with a chemical structure distinct from traditional carbamate compounds, capable of producing flexible polyurethane through its polycondensation properties.SOLUTION: The present invention provides a carbamate compound represented by the formula (1). The carbamate compound is obtained by reacting (A) a carbonate selected from the group consisting of ethylene carbonate, propylene carbonate, and trimethylene carbonate and a diamine (B). (In the formula (1), R1 and R2 independently represent a C2-10 linear or branched hydrocarbon group. m, n, and p independently represent an integer of 2-4, and o represents an integer of 1-4).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a carbamate compound. [Background technology]

[0002] Polyurethane has excellent moldability and can be formed into a variety of shapes, and is used in a wide range of industrial applications, including containers, fixtures, display components, electrical appliances, automotive components, elastic fibers, and more.

[0003] Polyaddition reactions between diisocyanates and diols have been widely used as a method for synthesizing polyurethanes. However, isocyanate compounds generally have problems such as being highly irritating to the human body, being highly harmful to the environment, and being easily deactivated by moisture absorption, making them difficult to handle.

[0004] Thus, as a polymerization method for synthesizing polyurethane without using isocyanate, a method of polycondensing a carbamic acid ester compound is known. For example, Patent Document 1 discloses a method for polycondensing a di(β-hydroxyalkyl)carbamic acid ester compound alone or together with a diol. Furthermore, Patent Documents 2 to 4 disclose methods of polycondensing a di(alkyl)carbamic acid ester compound or a di(phenyl)carbamic acid ester with a diol. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 02-127428 [Patent Document 2] JP 2012-140473 A [Patent Document 3] Japanese Patent Application Publication No. 60-084257 [Patent Document 4] Special Publication No. 2009-518494 Summary of the Invention [Problem to be solved by the invention]

[0006] Patent Documents 1 to 4 disclose carbamic acid ester compounds having various spacer structures, such as aliphatic, alicyclic, and aromatic, between carbamic acid ester groups in the molecule as carbamic acid ester compounds used in the production of polyurethane. However, the carbamic acid ester compounds disclosed in all of these patent documents lack flexibility due to the spacer structure, and polyurethanes obtained using these carbamic acid ester compounds are considered to have high hardness and poor moldability and formability into molded articles with irregular and complex shapes.

[0007] The present invention has been made in view of the above problems, and an object of the present invention is to provide a novel carbamic acid ester compound which has a chemical structure different from that of conventional carbamic acid ester compounds and is capable of polycondensation to give a soft polyurethane. [Means for solving the problem]

[0008] As a result of intensive research, the present inventors have discovered that a carbamic acid ester compound having a specific structural unit is polycondensed to produce a polyurethane which is soft and exhibits good moldability and formability into molded articles of irregular and complex shapes. The present invention has been achieved based on these findings, and has the following gist.

[0009] [1] A carbamic acid ester compound represented by the following formula (1):

[0010] [ka]

[0011] (In formula (1), R1 and R2 each independently represent a linear or branched hydrocarbon group having 2 to 10 carbon atoms. m, n, and p each independently represent an integer of 2 to 4. o represents an integer of 1 to 4.)

[0012] [2] The carbamic acid ester compound according to [1], having a hydroxyl value of 130 mg-KOH / g or more and 400 mg-KOH / g or less.

[0013] [3] The carbamate compound according to [1] or [2], wherein in the formula (1), R1 and R2 each independently represent a linear or branched hydrocarbon group having 2 to 4 carbon atoms.

[0014] [4] The carbamic acid ester compound according to any one of [1] to [3], obtained by reacting a carbonate (A) selected from the group consisting of ethylene carbonate, propylene carbonate, and trimethylene carbonate with a diamine (B). Effect of the Invention

[0015] According to the present invention, there is provided a novel carbamic acid ester compound which has a specific chemical structure and is capable of polycondensation to give a soft polyurethane. The polyurethane using the carbamic acid ester compound of the present invention is soft and has excellent moldability and processability, and can be molded into molded articles of irregular and complex shapes, and therefore can be widely used in various forms. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The following describes in detail the embodiments of the present invention; however, the present invention is not limited to the following description, and can be modified in any manner without departing from the gist of the present invention. In this specification, when "~" is used with a numerical value or a physical property value enclosed therein, the values ​​before and after the "~" are included in the expression.

[0017] The carbamic acid ester compound of the present invention is represented by the following formula (1).

[0018] [ka]

[0019] (In formula (1), R1 and R2 each independently represent a linear or branched hydrocarbon group having 2 to 10 carbon atoms. m, n, and p each independently represent an integer of 2 to 4. o represents an integer of 1 to 4.)

[0020] Conventional carbamic acid ester compounds have a spacer structure sandwiched between two carbamic acid ester groups, which is an aliphatic, alicyclic or aromatic linking group and has a rigid structure. Therefore, the carbamic acid ester compound itself is hard. Therefore, polyurethanes obtained by polycondensing such carbamic acid ester compounds have high hardness and poor moldability and formability into molded articles with irregular and complex shapes. In contrast, the carbamate compound of the present invention has a spacer structure sandwiched between two carbamate groups that has low crystallinity and is a flexible oxyalkylene structure, such as ethylene glycol, propylene glycol, or tetramethylene glycol, and therefore has excellent flexibility itself. Using this carbamate compound, a polyurethane can be obtained that is flexible and has excellent moldability and formability into molded articles of irregular and complex shapes.

[0021] In the above formula (1), R1 and R2 are each independently a straight-chain or branched hydrocarbon group having 2 to 10 carbon atoms. If the hydrocarbon group has only one carbon atom, the chemical structure is unstable and the desired carbamic acid ester compound cannot be obtained, whereas if the hydrocarbon group has 11 or more carbon atoms, it becomes difficult to remove the alcohol that is eliminated when polyurethane is synthesized by polycondensation. The number of carbon atoms in the hydrocarbon group is preferably 2 to 6, more preferably 2 to 4, and particularly preferably 2 or 3.

[0022] The hydrocarbon group may be a saturated or unsaturated hydrocarbon group, but is preferably a saturated hydrocarbon group from the viewpoint of preventing reactions and denaturation during the polyurethane synthesis process by polycondensation, and is preferably a straight-chain hydrocarbon group from the viewpoint of easy availability as a raw material for synthesizing the target carbamic acid ester compound. The saturated hydrocarbon group may be a straight-chain or branched alkylene group, and is preferably a straight-chain alkylene group.

[0023] In addition, R1 and R2 may be the same or different, but from the viewpoint of ease of synthesis, it is preferable that they are the same.

[0024] In formula (1), m, n, and p are each independently an integer of 2 to 4. From the viewpoint of obtaining a carbamic acid ester compound having low crystallinity and constituting a flexible oxyalkylene structure, m, n, and p are each preferably independently an integer of 2 to 3. In addition, m, n, and p may be the same or different, but from the viewpoint of ease of synthesis, it is preferable that they are the same.

[0025] In formula (1), o represents an integer of 1 to 4. From the viewpoint of obtaining a carbamic acid ester compound having low crystallinity and constituting a flexible oxyalkylene structure, o is preferably 1 to 3, and more preferably 1 or 2.

[0026] The molecular weight of the carbamic acid ester compound of the present invention is preferably in the range of 280-850, and more preferably in the range of 310-560. The hydroxyl value of the carbamic acid ester compound of the present invention is preferably in the range of 130 to 400 mg-KOH / g, and more preferably in the range of 200 to 360 mg-KOH / g. When the molecular weight is equal to or more than the above-mentioned lower limit and the hydroxyl value is equal to or less than the above-mentioned upper limit, the resulting carbamic acid ester compound has a spacer structure of sufficient length to exhibit flexibility, whereas when the molecular weight is equal to or less than the above-mentioned upper limit and the hydroxyl value is equal to or more than the above-mentioned lower limit, the resulting carbamic acid ester compound has a number of hydroxyl groups that exhibits high polycondensation reactivity.

[0027] Here, the molecular weight of the carbamate compound can be calculated as the sum of the atomic weights of the atoms constituting the carbamate compound, and the hydroxyl value can be calculated based on the number of hydroxyl groups relative to the calculated molecular weight.

[0028] Such a carbamic acid ester compound of the present invention may be synthesized by adding a carbonate (A) and a diamine (B) in a molar ratio of 2:1, or may be synthesized by subjecting another carbamic acid ester compound to an ester exchange reaction with a diol compound. From the viewpoint of obtaining the target carbamic acid ester compound in high yield, it is preferable to add the carbonate (A) and the diamine (B) in a molar ratio of 2:1.

[0029] The carbonate (A) may be any carbonate (A) capable of forming the carbamate ester group R1 and R2 in formula (1), and examples of the carbonate (A) that can be used include ethylene carbonate (R1 and R2 are straight-chain alkylene groups having 2 carbon atoms), propylene carbonate (R1 and R2 are branched alkylene groups having 3 carbon atoms), trimethylene carbonate (R1 and R2 are straight-chain alkylene groups having 3 carbon atoms), etc. These may be used alone or in combination of two or more, but usually only one is used.

[0030] The diamine (B) may be any diamine capable of forming a spacer structure between the carbamate groups in formula (1), and examples of the diamine (B) include the diamine (B) represented by the following formula (2).

[0031] [ka]

[0032] (In formula (2), m, n, o, and p are defined as in formula (1).)

[0033] Examples of such diamines (B) include, but are not limited to, 1,2-bis(2-aminoethoxy)ethane, diethylene glycol bis(3-aminopropyl) ether, 1,4-butanediol bis(3-aminopropyl) ether, and the like. These may be used alone or in combination of two or more, but usually only one is used.

[0034] The reaction between carbonate (A) and diamine (B) can be carried out in a solvent such as tetrahydrofuran, toluene, acetone, N,N-dimethylacetamide, water, or the like, or without a solvent, at a reaction temperature of 25 to 200° C. The reaction time varies depending on the reaction temperature, but is usually about 3 to 30 hours.

[0035] Polyurethane can be produced by polycondensing such a carbamic acid ester compound of the present invention. Moreover, the carbamic acid ester compound of the present invention or a polymer obtained by polycondensation of the carbamic acid ester compound can be further reacted with another compound such as a diol to produce a polyurethane having a higher molecular weight.

[0036] As a method for polycondensing the carbamic acid ester compound of the present invention, a known polymerization method can be applied, for example, melt polymerization in which the carbamic acid ester compound alone or the compound to be copolymerized with the carbamic acid ester compound are reacted by heating to a melting point or higher and mixing and stirring, or solution polymerization in which the carbamic acid ester compound is dissolved in a solvent and reacted by mixing and stirring may be used. From the viewpoint of not requiring a purification step after polycondensation, melt polymerization is preferably used.

[0037] In the polycondensation of the carbamic acid ester compound, a tin compound such as tin dichloride, dibutyltin oxide, dibutyltin dilaurate, or a urethane catalyst such as tetrabutoxytitanium can be used.

[0038] When producing a polyurethane using the carbamic acid ester compound of the present invention, the carbamic acid ester compound of the present invention may be used alone as the carbamic acid ester compound, or the carbamic acid ester compound of the present invention may be used in combination with one or more conventional carbamic acid ester compounds other than the carbamic acid ester compound of the present invention. The carbamic acid ester compounds of the present invention may be used either alone or in combination of two or more. When the carbamic acid ester compound of the present invention is used in combination with a carbamic acid ester compound other than the carbamic acid ester compound of the present invention, from the viewpoint of effectively obtaining the flexibility effect of the carbamic acid ester compound of the present invention, it is preferable to use the carbamic acid ester compound of the present invention in such a manner that the content of the carbamic acid ester compound of the present invention in all the carbamic acid ester compounds is 10 mass % or more, particularly 50 to 100 mass %.

[0039] The carbamic acid ester compound of the present invention can be used together with polyurethane raw materials other than the carbamic acid ester compound. In either case, from the viewpoint of effectively obtaining the flexibility effect of the carbamic acid ester compound of the present invention, it is preferable to use the carbamic acid ester compound of the present invention so that the content ratio of the carbamic acid ester compound of the present invention in the total polyurethane raw materials is 5 mass % or more, particularly 20 to 100 mass %. EXAMPLES

[0040] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0041] [Synthesis of carbamic acid esters] <Synthesis Example 1: Synthesis of carbamic acid ester 1> In a 1L three-neck flask equipped with a condenser and a thermometer, 177.4 g of tetrahydrofuran (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 88.1 g of ethylene carbonate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added, and the ethylene carbonate was dissolved while stirring with a magnetic stirrer. 74.1 g of 1,2-bis(2-aminoethoxy)ethane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was further added, and the reaction was allowed to proceed by maintaining the internal temperature at 60°C for 8 hours while stirring the solution. The solution after the reaction was concentrated under reduced pressure using a rotary evaporator, and dried under reduced pressure at 0.1 MPa or less at 40°C until the weight became constant, thereby obtaining a liquid carbamic acid ester 1.

[0042] <Synthesis Example 2: Synthesis of carbamic acid ester 2> As shown in Table 1, tetrahydrofuran, ethylene carbonate, and diethylene glycol bis(3-aminopropyl)ether (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were used, and the procedure was the same as in Synthesis Example 1, except that heating was continued for 6 hours a day for 3 days at 70°C. A liquid carbamic acid ester 2 was obtained by the same procedure as in Synthesis Example 1.

[0043] <Synthesis Example 3: Synthesis of carbamic acid ester 3> As shown in Table 1, triethylene carbonate and 1,3-bis(aminomethyl)cyclohexane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were used and heated at 120° C. for 22 hours and at 130° C. for 5 hours to obtain solid carbamic acid ester 3.

[0044] <Synthesis Example 4: Synthesis of carbamic acid ester 4> As shown in Table 1, the reaction was carried out by using tetrahydrofuran, ethylene carbonate, and hexamethylenediamine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and maintaining at 70° C. for 6 hours. After the reaction, the solution was concentrated under reduced pressure using a rotary evaporator, and the precipitated solid was recovered by suction filtration and then washed by suspending in tetrahydrofuran to obtain a solid carbamic acid ester 4.

[0045] <Synthesis Example 5: Synthesis of carbamic acid ester 5> As shown in Table 1, tetrahydrofuran, ethylene carbonate, and 1,3-bis(aminomethyl)cyclohexane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were used and heating was continued for 3 days at 70° C. for 6 hours per day. After the reaction, the solution was concentrated under reduced pressure using a rotary evaporator, and the precipitated solid was collected by suction filtration and then suspended and washed in ethyl acetate to obtain a solid carbamic acid ester 5.

[0046] <Synthesis Example 6: Synthesis of carbamic acid ester 6> As shown in Table 1, tetrahydrofuran, ethylene carbonate, and 1,4-butanediol bis(3-aminopropyl)ether (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were used, and the mixture was first thoroughly mixed with tetrahydrofuran, and then concentrated under reduced pressure at room temperature. The mixture was concentrated while being heated stepwise from room temperature to 110°C, and after it was confirmed that no bubbles were generated, the reaction was continued for 3 hours at normal pressure and 110°C. The mixture was then heated under reduced pressure at 110°C for 5 hours to remove unreacted components, thereby obtaining solid carbamic acid ester 6.

[0047] [Table 1]

[0048] The structural formula of the carbamic acid ester obtained in each synthesis example, and the molecular weight and hydroxyl value calculated from the structural formula are shown below. Carbamic acid esters 4 and 5 are the carbamic acid esters described in Patent Document 1.

[0049] [ka]

[0050] [Example 1] <Synthesis of carbamic acid ester polymer 1> To a reaction vessel equipped with a stirrer, a nitrogen inlet, a heater, a thermometer, and a pressure reduction port, 16.6 g of the carbamic acid ester 1 obtained in Synthesis Example 1 and 0.030 g of tin dichloride dihydrate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) were added as raw materials, and a nitrogen atmosphere was created by repeatedly introducing nitrogen gas and reducing the pressure. Next, the reaction vessel was placed in an oil bath at 170°C and kept at 170°C for 2 hours. After that, the pressure in the reaction vessel was reduced to 30 mmHg over 45 minutes, and then kept at 30 mmHg until the outflow of liquid stopped. Next, the pressure in the reaction vessel was reduced to an ultimate reduced pressure of 1.5 mmHg, and when the viscosity increased and the resin began to cling to the stirring blade, the heating was stopped and the pressure was returned to atmospheric pressure to stop the polymerization, thereby obtaining carbamic acid ester polymer 1. Table 2 shows the amounts of raw materials and catalysts charged and the ultimate vacuum level.

[0051] <Calculation of the average polymerization degree of carbamic acid ester polymer 1> The obtained carbamic acid ester polymer 1 was dissolved in dimethylsulfoxide-d6, and the average degree of polymerization of the carbamic acid ester polymer 1 was calculated as follows using an NMR measurement device (Ascend400, manufactured by Bruker). The peak area intensity Ip at around 4.7 ppm chemical shift due to the terminal hydroxyl group was obtained under normalized conditions with the peak intensity due to the methylene group adjacent to the nitrogen atom in the polymer set at 4.0. The peak area intensity Im at the chemical shift of 4.7 ppm due to the terminal hydroxyl group was obtained under similar normalized conditions for carbamic acid ester 1. The average degree of polymerization was determined from Ip and Im using the following formula. Average degree of polymerization=Im / Ip The average degree of polymerization of the resulting carbamic acid ester polymer 1 is shown in Table 2.

[0052] <Evaluation of Flexibility of Carbamic Acid Ester Polymer 1> 0.5 g of the carbamic acid ester polymer 1 obtained by polymerization was weighed out, and a press film was obtained by holding a pressure of 2 MPa at 20° C. for 3 minutes using a hand press machine (Mini Test Press, model MP-WNH, manufactured by Toyo Seiki Co., Ltd.) The flexibility of the film was evaluated by repeating the operation of holding an edge of the obtained film and folding it at an angle of 90 degrees or more and then returning it to its original state twice. The film that did not crack after being returned was evaluated as ◯, and the film that cracked was evaluated as ×. The results are shown in Table 2.

[0053] [Examples 2 to 5, Comparative Examples 1 to 2] Carbamic acid ester polymers 2 to 7 were obtained in the same manner as in Example 1, except that the raw material charges and pressing conditions were changed as shown in Table 2, and were similarly evaluated. Table 2 shows the evaluation results for the raw material charge, ultimate vacuum level, average degree of polymerization, and flexibility.

[0054] [Table 2]

[0055] As shown in Table 2, the carbamic acid ester polymers shown in Examples 1 to 5 were excellent in flexibility and could be deformed without cracking when bent during film formation, whereas the carbamic acid ester polymers shown in Comparative Examples 1 and 2 were cracked when bent. These results show that the carbamic acid ester compound of the present invention has excellent flexibility, and that this carbamic acid ester compound can be used to obtain a soft polyurethane that has excellent moldability and processability and can be molded into molded articles of irregular and complex shapes.

Claims

1. A carbamic acid ester compound represented by the following formula (1): 【Chemistry 1】 (In formula (1), R 1 , R 2 each independently represents a linear or branched hydrocarbon group having 2 to 10 carbon atoms; m, n, and p each independently represent an integer of 2 to 4; and o represents an integer of 1 to 4.

2. The carbamic acid ester compound according to claim 1, having a hydroxyl value of 130 mg-KOH / g or more and 400 mg-KOH / g or less.

3. In the formula (1), R 1 , R 2 each independently represents a linear or branched hydrocarbon group having 2 to 4 carbon atoms.

4. The carbamic acid ester compound according to any one of claims 1 to 3, which is obtained by reacting a carbonate (A) selected from the group consisting of ethylene carbonate, propylene carbonate, and trimethylene carbonate with a diamine (B).

Citation Information

Patent Citations

  • Manufacture of n,o-substituted mono- and / or polyurethane

    JP1985084257A

  • Production of linear polyurethane resin

    JP1990127428A

  • Melt-transfer polyurethane process for manufacturing polyurethane

    JP2009518494A

  • Method for producing polyurethane

    JP2012140473A