High strength steel sheet with superior delayed fracture resistance
A surface treatment with organic compounds and resins on high-strength steel sheets addresses hydrogen embrittlement, enhancing delayed fracture resistance and adhesion without additional processing, suitable for automotive and building materials.
Patent Information
- Application Number
- JP2023209631
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2023-12-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-12
AI Technical Summary
High-strength steel sheets with tensile strength of 1180 MPa or more are prone to delayed fracture due to hydrogen embrittlement, and existing methods to prevent this, such as Ni plating or conductive polymer films, either fail to adequately suppress fracture or require additional processing steps like pickling.
A surface treatment involving specific organic compounds like azole, pyridine, thiocarbonyl, mercapto, and sulfide compounds combined with an organic resin forms a film on the steel sheet, enhancing adhesion and acting as a barrier to hydrogen intrusion, thereby preventing delayed fracture without additional processing steps.
The treated steel sheets exhibit excellent delayed fracture resistance, improved film adhesion, and reduced hydrogen intrusion, making them suitable for automotive and building applications while maintaining weldability and corrosion resistance.
Smart Images

Figure 2024144074000003 
Figure 2024144074000004 
Figure 2024144074000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a high-strength steel plate suitable for strength members for automobiles and building materials, and relates to a high-strength steel plate having excellent delayed fracture resistance and a tensile strength of 1180 MPa or more. [Background technology]
[0002] In recent years, the steel sheets used in automobiles have become more difficult to manufacture due to the CO2 emissions from automobiles. 2 From the viewpoint of reducing emissions and ensuring safety, efforts are being made to increase the strength of steel, and the use of high-strength steel plates with a tensile strength of 1180 MPa or more is also being promoted. However, it is known that increasing the strength of steel makes it more susceptible to a phenomenon called delayed fracture. Delayed fracture is a phenomenon in which brittle fracture occurs suddenly without plastic deformation after a certain period of time has passed when high-strength steel is subjected to a static load stress (load stress less than the tensile strength). Delayed fracture becomes more likely to occur as the strength of the steel increases, and is particularly noticeable in high-strength steel with a tensile strength of 1180 MPa or more.
[0003] It is known that delayed fracture of steel sheets occurs due to residual stress when formed into a predetermined shape by press working and hydrogen embrittlement of steel at stress concentration points. Non-Patent Document 1 reports that hydrogen embrittlement sensitivity increases with increasing steel strength, and is prominent in high-strength steels with tensile strengths of 1200 MPa or more, regardless of whether the amount of added alloy elements is increased or decreased. Non-Patent Document 2 also reports that hydrogen cracking occurs in high-strength cold-rolled steel sheets with tensile strengths of 1180 MPa class. In most cases, hydrogen that causes this hydrogen embrittlement is thought to be hydrogen that has penetrated and diffused into the steel from the external environment, and typically hydrogen that is generated during corrosion of the steel sheet penetrates and diffuses into the steel.
[0004] In order to prevent such delayed fracture in high-strength steel sheets, for example, Patent Document 1 considers weakening the delayed fracture susceptibility by adjusting the structure and components of the steel sheet. Patent Document 2 discloses a technique for suppressing delayed fracture by plating the steel sheet with Ni or Ni alloy to reduce hydrogen penetration into the steel sheet. Patent Document 3 discloses a technique for improving delayed fracture resistance by forming a conductive polymer film on the steel sheet to reduce hydrogen penetration into the steel sheet. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2004-231992 A [Patent Document 2] Japanese Patent Application Publication No. 7-54194 [Patent Document 3] JP 2018-44240 A [Non-patent literature]
[0006] [Non-Patent Document 1] "Delayed Fracture" by Shinsaku Matsuyama, Nikkan Kogyo Shimbun, 1989 [Non-Patent Document 2] Yuki Taji and 4 others, "Evaluation Method of Hydrogen Embrittlement Resistance of High Strength Thin Steel Plates," Iron and Steel Institute of Japan, Vol. 95, No. 12, pp. 887-894, 2009 Summary of the Invention [Problem to be solved by the invention]
[0007] However, the method of Patent Document 1 does not change the amount of hydrogen that penetrates into the steel sheet from the external environment, so although it is possible to delay the occurrence of delayed fracture, it is not effective enough in suppressing delayed fracture. In addition, the method of Patent Document 2 may cause damage to the plating when the steel sheet is processed, and it is considered that it may not be possible to reduce hydrogen penetration from this damaged area. Furthermore, the method of Patent Document 3 has an issue with the adhesion between the film and the steel sheet (hereinafter referred to as "film adhesion"), and in order to achieve both film adhesion and delayed fracture resistance, a process of pickling the steel sheet before the film application process is required.
[0008] Therefore, an object of the present invention is to solve the above-mentioned problems of the conventional art and to provide a high-strength steel sheet having a tensile strength of 1180 MPa or more suitable for strength members for automobiles and building materials, which has excellent delayed fracture resistance and excellent coating adhesion, and which can be produced without carrying out a special process such as pickling before the coating process. [Means for solving the problem]
[0009] The present inventors have conducted extensive research and studies into means for reducing the amount of hydrogen penetrating into the interior of a steel sheet in order to prevent delayed fracture of the steel sheet in a usage environment. As a result, they have found that by incorporating a specific organic compound, such as an azole compound or a pyridine compound, into an organic resin film formed on the surface of the steel sheet, it is possible to suppress hydrogen penetration into the interior of the steel sheet and delayed fracture of the steel sheet while ensuring good film adhesion. The present invention has been made based on the above findings, and the gist of the present invention is as follows.
[0010] [1] A coating (A) is provided on the surface of a steel sheet having a tensile strength of 1180 MPa or more, the coating (A) including at least one organic compound (x) selected from an azole compound, a pyridine compound, a thiocarbonyl compound, a mercapto compound, and a sulfide compound, and an organic resin (y); The coating (A) has an adhesion amount [x] of the organic compound (x) of 100 to 2000 mg / m 2 The amount of organic resin (y) attached [y] is 200 to 3800 mg / m 2a ratio [x] / ([x]+[y]) of the amount of adhesion [x] of the organic compound (x) to the total amount of adhesion [x]+[y] of the organic compound (x) and the organic resin (y) is 0.05 to 0.5, and a film thickness is 0.3 to 4.0 μm.
[0011] [2] The high-strength steel plate according to the above [1], wherein the organic resin (y) is at least one selected from the group consisting of urethane-based resins, epoxy-based resins, acrylic-based resins, and ethylene-based resins. [3] A surface treatment solution for forming a coating on the surface of a steel plate to suppress delayed fracture of a steel plate having a tensile strength of 1180 MPa or more, A surface treatment solution comprising an organic compound (x) consisting of at least one selected from an azole compound, a pyridine compound, a thiocarbonyl compound, a mercapto compound, and a sulfide compound, and an organic resin (y). Effect of the Invention
[0012] The high-strength steel sheet of the present invention has excellent delayed fracture resistance because hydrogen penetration into the steel sheet is suppressed, and also has excellent coating adhesion, and can be manufactured without carrying out a special process such as pickling before the coating process. Therefore, the high-strength steel sheet of the present invention is particularly suitable for strength members for automobiles and building materials, and enables weight reduction of strength members applied in the fields of automobiles and building materials. [Brief description of the drawings]
[0013] [Figure 1] Schematic diagram of a test piece for evaluating delayed fracture used in the examples. [Diagram 2] FIG. 1 is an explanatory diagram showing the steps of a complex cycle corrosion test performed in the examples. [Diagram 3] Schematic diagram of the hydrogen permeability measuring device used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The steel plate serving as the base material (substrate) of the steel plate having excellent delayed fracture resistance of the present invention is a high-strength steel plate having a tensile strength of 1180 MPa or more, and more preferably a high-strength steel plate having a tensile strength of 1470 MPa or more. A steel plate having a low tensile strength is less likely to cause delayed fracture. The effect of the present invention is also exhibited in a steel plate having a low tensile strength, but is exhibited significantly in a steel plate having a tensile strength of 1180 MPa or more, and is more exhibited significantly in a steel plate having a tensile strength of 1470 MPa or more. The chemical composition and steel structure are not particularly limited. However, among these, a high-strength steel plate having a tensile strength of 1180 MPa or more, which is used in the automotive field and building material field, and is particularly often used in the automotive field, is preferred, and a high-strength steel plate having a tensile strength of 1470 MPa or more is more preferred.
[0015] The high-strength steel sheet preferably used in the present invention may have any composition and structure as long as it has the desired tensile strength. Therefore, in order to improve various properties such as mechanical properties, for example, the following structural or textural modifications may be performed alone or in combination. Solid solution strengthening by adding interstitial solid solution elements such as C and N, and substitutional solid solution elements such as Si, Mn, P, and Cr Precipitation strengthening by carbonitrides such as Ti, Nb, V, and Al Chemical composition modification, such as the addition of strengthening elements such as W, Zr, Hf, Co, B, Cu, and rare earth elements - Strengthening by recovery annealing at a temperature where recrystallization does not occur, or by partially recrystallizing the material without completely recrystallizing it, leaving unrecrystallized areas. Strengthening due to transformation structures such as single phase bainite or martensite, or a combination of ferrite and these transformed structures Hall-Petch equation when ferrite grain size is d: σ=σ 0 +kd -1 / 2 (In the formula, σ: stress, σ 0 , k: material constant) - Strengthening processing through rolling, etc.
[0016] Examples of the composition of such high-strength steel plate include C: 0.1-0.4 mass%, Si: 0-2.5 mass%, Mn: 1-3.5 mass%, P: 0-0.05 mass%, S: 0-0.01 mass%, and the balance being Fe and unavoidable impurities. The alloy may further contain one or more selected from the group consisting of Cu: 1.0 mass% or less, Ti: 0.2 mass% or less, V: 0.5 mass% or less, Al: 0.1 mass% or less, Cr: 1.0 mass% or less, Nb: 0.2 mass% or less, W: 0.5 mass% or less, Zr: 0.1 mass% or less, B: 0.005 mass% or less, N: 0.0005 to 0.0100 mass%, Ni: 0.01 to 2.00 mass%, Mo: 0.005 to 2.000 mass%, Ca: 0.0002 to 0.0050 mass%, Mg: 0.0001 to 0.0020%, REM: 0.0002 to 0.0050 mass%, Sb: 0.002 to 0.200 mass%, and Sn: 0.002 to 0.200 mass%. In general, it is preferable that the total amount of these elements other than C, Si, Mn, P, and S is not more than about 4 mass%. The lower limit of the content of each element is preferably about 0.01 mass% for Si, Al, and Cr, about 0.005 mass% for Cu, Ti, V, Nb, W, and Zr, about 0.001 mass% for P, and about 0.0001 mass% for B and S.
[0017] In addition, examples of commercially available high-strength steel sheets include, but are not limited to, JFE-CA1180, JFE-CA1320, JFE-CA1470, JFE-CA1180SF, JFE-CA1180Y1, JFE-CA1180Y2 (all manufactured by JFE Steel Corporation), SAFC1180D (manufactured by Nippon Steel & Sumitomo Metal Corporation), etc. In addition, the high-strength steel sheet may be either a cold-rolled steel sheet or a hot-rolled steel sheet. The high-strength steel sheet may be a zinc-based plated steel sheet that has been subjected to zinc-based plating such as hot-dip galvanization, electrolytic galvanization, etc. In the case of hot-dip galvanization, an alloying treatment may be performed. The thickness of the high-strength steel plate that is the substrate is not particularly limited, but is generally about 0.8 to 5 mm, and more preferably about 1.0 to 2.0 mm.
[0018] According to the results of the research and examination by the present inventors, it is believed that the salt attached to the steel sheet surface from the environment in an atmospheric corrosion environment where drying and wetting are repeated contributes greatly to the penetration of hydrogen into the steel sheet during the corrosion process. Examples of salt that is applied to the steel sheet in an atmospheric environment include salt that comes from seawater and snow-melting salt applied as an anti-icing agent on road surfaces. This salt absorbs water due to an increase in humidity or adhesion of road surface water, forming a water film and corroding the steel sheet. In the water film formed on the steel sheet surface, a reduction reaction of oxygen and an oxidation reaction of iron occur. In the reduction reaction of oxygen, hydroxide ions are generated, so the pH increases, but if the chloride ion concentration is high, the iron ions eluted by the oxidation reaction further undergo hydrolysis, generating iron oxyhydroxide and hydrogen ions, so the pH decreases. As the humidity decreases, the water film decreases, and as the chloride concentration increases, the hydrolysis reaction of iron ions is promoted, so the pH decreases and the amount of hydrogen that penetrates into the steel sheet increases. In other words, in order to suppress the penetration of hydrogen, it is important to block the adhesion of salt to the steel sheet, which causes a decrease in pH during the corrosion process.
[0019] For this reason, in the present invention, an organic resin film (A) (hereinafter sometimes referred to as "organic resin film (A)") is formed on the surface of a steel sheet having a tensile strength of 1180 MPa or more, thereby blocking chloride ions that adhere in the atmosphere, and the organic resin film (A) contains an organic compound (x) consisting of at least one selected from azole compounds, pyridine compounds, thiocarbonyl compounds, mercapto compounds, and sulfide compounds, thereby suppressing corrosion at paint defects, thereby providing the property of being able to suppress delayed fracture. Furthermore, high film adhesion can be obtained by retaining the organic compound (x) in the organic resin film (A).
[0020] Here, it is believed that the organic compound (x) in the coating (A) is dissolved into the water film formed on the steel sheet surface at the paint defect area, and is then adsorbed onto the steel sheet. The nitrogen and sulfur contained in the organic compound (x) form polar groups in the organic compound and have unshared electron pairs. This unshared electron pair enters the vacant orbital of the iron atom in the steel sheet, forming a coordinate bond in which both the metal and the polar group have an electron pair, causing the organic compound to be adsorbed onto the metal surface and form a molecular film, which is believed to act as a barrier layer that blocks chloride ions. It is believed that in an aqueous film with a high chloride concentration, the pH level drops due to hydrolysis of iron ions, making the aqueous film weakly acidic. Examples of azole compounds, pyridine compounds, thiocarbonyl compounds, mercapto compounds, and sulfide compounds that adsorb to the steel sheet and form a molecular film in this weakly acidic aqueous solution (pH 5 or less) include the following: Among these, pyridine compounds are particularly preferred because they dissolve into the water film, increase the pH of the water film, and have the effect of inhibiting corrosion. The reason why pyridine compounds have the corrosion inhibition effect is considered to be as follows. That is, since the lone pair on the nitrogen atom contained in the pyridine compound is not delocalized, even if the iron ions in the water film are hydrolyzed, the pyridine compound increases the pH, and the water film is kept neutral to weakly alkaline. As a result, it is considered that the cathodic reaction that generates hydroxide ions is less likely to occur.
[0021] Examples of the azole compound include 2-N,N-diethylthiobenzothiazole, 2-N-mercaptobenzothiazole, pyrazole, 3,5-dimethylpyrazole, 3-methyl-5-pyrazolone, 3-amino-5-methylpyrazole, 1,2,4-triazole, 3-amino-1,2,4-triazole, 3-mercapto-1,2,4-triazole, 5-amino-3-mercapto-1,2,4-triazole, 2,3-dihydro-3-oxo-1,2,4-triazole, 5-amino-2-mercapto-1,3,4-thiadiazole, 2,5-dimercapto-1,3,4-thiadiazole, 5-phenyl-1,2,3,4-tetrazole, 5-mercapto-1-phenyl-1,2,3,4-tetrazole, 1H-benzotriazole, 1,2,3-benzotriazole, and 1-hydroxybenzotriazole (monohydrate).
[0022] Examples of the pyridine compound include pyridine, 4-methylpyridine, 4-ethylpyridine, 4-propylpyridine, 4-butylpyridine, 4-pentylpyridine, quinoline, isoquinoline, 4-methoxypyridine, and 2,3,5,6-tetrachloro-4-(methylsulfonyl)pyridine. Examples of the thiocarbonyl compound include thiourea, thiosemicarbazide, phenylthiourea, tolylthiourea, N-methylthiourea, dimethylthiourea, diethylthiourea, diphenylthiourea, and 2-mercaptobenzimidazole. Examples of the mercapto compound include isobutyl mercaptan, butyl mercaptan, octyl mercaptan, and 2-mercaptoimidazoline. Examples of the sulfide compound include mercaptobenzothiazyl sulfide, tetramethylthiuram monosulfide, tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, and dipentamethylenethiuram tetrasulfide.
[0023] By incorporating the organic compound (x) in the organic resin film (A), the organic compound (x) can be retained on the steel sheet surface, improving the film adhesion, because chemical interactions occur between the steel sheet surface and various groups of the molecules contained in the organic resin film (A). In the case of steel sheets for automobiles, after they are pressed into a desired shape, the steel sheets are joined together by spot welding, and finally painted. At this time, if the coating (A) is too thick, the current during welding may not flow, resulting in poor welding, so the thickness of the coating (A) is set to 4.0 μm or less. On the other hand, if the coating (A) is too thin, it will not function as a barrier layer to block the corrosive environment, so the thickness is set to 0.3 μm or more. In addition, hydrogen, which causes delayed fracture, is generated by corrosion, so the thickness must be 0.3 μm or more from the perspective of preventing delayed fracture.
[0024] In order to fully exert the effect of suppressing the occurrence of delayed fracture in an atmospheric corrosive environment, the adhesion amount [x] of the organic compound (x) in the coating (A) is 100 mg / m 2 On the other hand, from the viewpoint of suppressing delayed fracture, there is no problem even if the coating weight is large, but if the coating weight is too large, the adhesion between the coating (A) and the steel sheet decreases, which is not preferable especially for steel sheets for automobiles, so the coating weight [x] of the organic compound (x) is set to 2000 mg / m 2 The amount of organic resin (y) attached in the coating (A) [y] is set to 200 mg / m2 from the viewpoint of providing a barrier against corrosion factors, i.e., from the viewpoint of suppressing delayed fracture. 2 More than 3800mg / m 2 In addition, the amount of organic resin (y) attached [y] is set to 3800 mg / m2 from the viewpoint of weldability. 2 It is preferable that: In addition, the ratio [x] / ([x]+[y]) of the amount of adhesion of the organic compound (x) to the total amount of adhesion of the organic compound (x) and the organic resin (y) [x]+[y] is 0.05 to 0.5. If [x] / ([x]+[y]) is less than 0.05, the effect of suppressing the occurrence of delayed fracture may decrease. From the viewpoint of suppressing delayed fracture, it is preferable that [x] / ([x]+[y]) is 0.3 or more. On the other hand, if [x] / ([x]+[y]) exceeds 0.5, the coating adhesion may decrease.
[0025] There is no particular limitation on the type of organic resin used in the organic resin film (A), and examples thereof include epoxy resins, modified epoxy resins, urethane resins, alkyd resins, acrylic resins, ethylene resins (polyolefin resins), polyester resins, polybutadiene resins, amino resins, phenolic resins, fluororesins, silicone resins, etc., and one or more of these can be used. Among these, urethane resins, epoxy resins, acrylic resins, and ethylene resins are particularly preferred because of their high barrier effect against moisture and chlorides, which are corrosion factors.
[0026] The hydrogen penetration suppression effect of the coating on high-strength steel plate is the maximum hydrogen permeability coefficient H t and the maximum hydrogen permeability coefficient H 0 Ratio to (H t / H 0 ) can be evaluated using this H t / H 0 represents the degree of hydrogen penetration suppression effect of the coating. 0 H measured on a steel plate with a coating t If is less than half, i.e., H t / H 0 If the following formula (1) is satisfied, the coating can be evaluated as being capable of effectively suppressing hydrogen penetration into steel. As will be shown in the examples described later, the high-strength steel sheet of the present invention has excellent properties that satisfy the following formula (1). H t / H 0 ≦0.50 …(1)
[0027] Here, the maximum hydrogen permeability coefficient H t is calculated as follows. The surface of the steel plate having the coating (one side of the steel plate) of the test piece is used as the hydrogen entry surface, and the other side of the steel plate is plated with palladium to use as the hydrogen detection surface. The hydrogen entry surface is corroded in a corrosion test simulating an atmospheric corrosion environment, and an electrochemical cell placed on the hydrogen detection surface detects the current generated due to hydrogen entering the steel from the hydrogen entry surface, to calculate the hydrogen permeation current (J). This hydrogen permeation current is multiplied by the plate thickness (L) of the test piece to calculate the hydrogen permeation coefficient (JL), and the maximum value of this hydrogen permeation coefficient during the measurement is called the maximum hydrogen permeation coefficient H t In addition, the maximum hydrogen permeability coefficient H 0 is calculated as follows. The surface of the steel plate that does not have a coating (one side of the steel plate) of the test piece is used as the hydrogen entry surface, and the other side of the steel plate is plated with palladium to use as the hydrogen detection surface. This test piece is then subjected to the same corrosion test as above, and the hydrogen permeability coefficient (JL) is calculated using the same method as above. The maximum value of this hydrogen permeability coefficient during the measurement is called the maximum hydrogen permeability coefficient H 0 Let us assume that.
[0028] The high-strength steel sheet of the present invention may have a multi-layer coating in which another coating is provided under or over the coating (A).The coating (A) may have a multi-layer structure consisting of two or more layers. The thickness of the coating (A) is determined by observing the cross section of the coating, measuring the thickness of the coating (from the surface of the base steel sheet to the surface of the coating (A)) at multiple points (e.g., three points) in an arbitrary field of view, and averaging these values. The method of processing the cross section is not particularly limited, but examples include FIB processing. The amount of the organic compound (x) attached in the coating (A) can be measured, for example, by fluorescent X-ray analysis. Specifically, the coating surface is irradiated with X-rays, the intensity of the fluorescent X-rays of the elements (e.g., nitrogen and sulfur) contained in the organic compound (x) is measured, and the amount of attachment can be calculated by comparing with a calibration curve. Furthermore, the amount of organic resin (y) attached in the coating (A) can be calculated, for example, by measuring the weight of the steel sheet with and without the coating attached, dividing the difference between the measured weights by the area of the steel sheet, and then subtracting the amount of organic compound (x) attached from the resultant value.
[0029] The coating (A) is formed on the surface of a steel sheet by a method in which an organic compound (x) is added to a treatment liquid (resin solution) prepared by dissolving and / or dispersing an organic resin (y) in a solvent (water and / or an organic solvent), and the treatment liquid is then coated on the surface of the steel sheet and subsequently dried by heating. The method of coating the treatment liquid (resin solution) on the steel sheet surface is not particularly limited, and may be any of the known methods, for example, coating, dipping, and spraying. In the coating method, any coating means such as a roll coater (three-roll type, two-roll type, etc.), a bar coater, a squeeze coater, and a die coater may be used. In addition, after coating treatment using a squeeze coater or the like, dipping treatment, and spraying treatment, it is also possible to adjust the coating amount, uniformize the appearance, and uniformize the film thickness by an air knife method or a roll squeezing method. The method of heating and drying the coated treatment liquid is arbitrary, and for example, means such as a dryer, a hot air oven, a high-frequency induction heating oven, and an infrared oven can be used.
[0030] The manufacturing method of the steel sheet used as the substrate in the present invention is not particularly limited. In order to facilitate understanding of the present invention, a series of processes from steelmaking will be briefly described using an example. However, the manufacturing process of the steel sheet as the substrate is not limited to the following example. Steel having a predetermined composition is melted and made into a slab by continuous casting according to a conventional method. The obtained slab is then heated in a heating furnace at a temperature of 1100 to 1300 ° C, hot rolled at a finishing temperature of 750 to 950 ° C, and coiled at 500 to 650 ° C. Following this, pickling is performed, followed by cold rolling at a rolling reduction of 30 to 70%. Thereafter, if necessary, cleaning treatment is performed according to a conventional method (i.e., cleaning with an alkali or a mixed solution of an alkali and a surfactant and an organic compound containing nitrogen or sulfur that is adsorbed on the steel sheet to form a molecular film, electrolytic cleaning, hot water cleaning, and drying), followed by heating treatment at 650 to 900 ° C, rapid cooling, and adjustment of the tensile strength of the steel sheet. Furthermore, if necessary, temper rolling of about 0.01 to 0.5% is performed according to a conventional method to obtain a cold-rolled steel sheet having a desired tensile strength.
[0031] As described above, the treatment liquid (surface treatment liquid) of the present invention is a surface treatment liquid for forming a coating (A) on the surface of a steel sheet for suppressing delayed fracture of a steel sheet having a tensile strength of 1180 MPa or more, and contains at least one organic compound (x) selected from azole compounds, pyridine compounds, thiocarbonyl compounds, mercapto compounds, and sulfide compounds, and an organic resin (y). The functions, effects, and specific examples of the organic compound (x) and organic resin (y) are as described above. In addition, the concentrations of the organic compound (x) and the organic resin (y) are adjusted so that the treatment liquid can satisfy the above-mentioned coating structure (adhesion amounts [x], [y], and [x] / ([x]+[y])) when applied to the steel sheet surface to form the coating (A). EXAMPLES
[0032] The steel sheets used were cold-rolled steel sheets and galvannealed steel sheets (GA steel sheets). The cold-rolled steel sheets (as-cold-rolled steel sheets) had a composition of 0.19% by mass of C, 0.8% by mass of Si, 1.8% by mass of Mn, 0.011% by mass of P, 0.001% by mass of S, the balance being Fe and unavoidable impurities, and had a tensile strength of 1470 MPa and a thickness of 1.6 mm. The galvannealed steel sheets (GA steel sheets) had a composition of 0.22% by mass of C, 1.2% by mass of Si, 3.0% by mass of Mn, 0.007% by mass of P, 0.0005% by mass of S, the balance being Fe and unavoidable impurities, and had a tensile strength of 1580 MPa and a thickness of 1.4 mm. This alloyed hot-dip galvanized steel sheet (double-sided coated steel sheet) has a coating weight of 44 g / m per side. 2 The Fe content of the zinc plating film was 14 mass %. Each of the above steel sheets was immersed in toluene and ultrasonically cleaned for 5 minutes to remove the rust-preventive oil, and then an organic resin film was formed on the surface (however, in some comparative examples, no organic resin film was formed).
[0033] The following A1 to A5 were used as organic resins (y) for the organic resin coating. A treatment liquid containing any of the organic resins (y) and a specified organic compound (x) (in some comparative examples, the treatment liquid contains only an organic resin) was applied to the steel sheet surface by any of the coating methods (bar coating), spraying, and immersion (and roll squeezing), and then the steel sheet was heated with an induction heater so that the ultimate sheet temperature was 120°C, thereby forming an organic resin coating. A1: Acrylic resin (manufactured by DIC Corporation, product name: 40-418EF) A2: Epoxy resin (Japan Epoxy Resin Co., Ltd., product name: jER1009) A3: Urethane resin (manufactured by Dai Nippon Paint Co., Ltd., product name: V Top RC Clear) A4: Ethylene-based resin (manufactured by Dow Mitsui Polychemicals, product name: Hylamin) A5: Fluorine-based resin (manufactured by Asahi Glass Co., Ltd., product name: Lumiflon LF552)
[0034] The high-strength steel sheets of the invention and comparative examples on which the coating was formed as described above were evaluated for delayed fracture resistance, coating adhesion, and corrosion resistance after painting, and the maximum hydrogen permeability coefficient H t ,H 0 and H t / H 0 The results are shown in Tables 1 and 2 together with the production conditions. In measuring the thickness of the organic resin film, the cross section obtained by FIB processing was observed with an SEM, the thickness of the organic resin film (thickness from the base steel surface to the surface of the organic resin film) was measured at three points in an arbitrary field of view, and the average value of these was taken as the film thickness. The amount [x] of organic compound (x) attached in the organic resin film was calculated by measuring the amount of N and S before and after applying the film using fluorescent X-rays, and comparing the difference in the measured amounts with a calibration curve. The amount [y] of organic resin (y) attached was calculated by measuring the weight of the steel sheet with and without the film attached, and dividing the difference in the measured amounts by the steel sheet area, and subtracting the amount [x] of organic compound (x) attached from this value. In addition, the pH of the organic compound (x) was measured when 1 mol / L of the organic compound (x) was added to pure water, and this was regarded as the pH of the organic compound (x).
[0035] (1) Evaluation of delayed fracture resistance The steel plates of the invention and comparative examples, each having a thickness of 1.4 mm, were sheared to a width of 35 mm and a length of 100 mm, and then ground to a width of 30 mm to remove residual stress during shearing, to prepare test pieces. The prepared test pieces were bent 90° with a radius of curvature of 10 mmR to prepare bending test pieces, and as shown in Figure 1, the shape of this bending test piece 1 was restrained with a nut 2 (size: M8), a SUS jig 3, and a bolt 4 (size: M8) to fix the shape of the test piece, and a test piece for evaluating delayed fracture resistance was obtained. In preparing this test piece, the inner distance between the flange ends was narrowed by 14 mm after restraint (after the test piece shape was fixed by tightening with bolts and nuts, etc.) compared to before restraint (test piece 1a in Figure 1).
[0036] The test pieces for evaluating delayed fracture resistance prepared in this way were subjected to a complex cyclic corrosion test shown in Figure 2, up to a maximum of 40 cycles. In this cyclic test, the test temperature was constant (50°C), and one humidity cycle consisted of a total of four steps: a dry step at a relative humidity of 30%, a wet step at a relative humidity of 90%, and a humidity increase / decrease step (transition period). Each step was switched every 2 hours, and the test was repeated for one cycle of 8 hours. In addition, twice a week at the start of the dry step, the test pieces for evaluating delayed fracture resistance were washed with pure water, and then sprayed with salt water with a salt concentration of 8.1 mass% to add chloride (amount of salt attached: 3,000 mg / m per side). 2 ). Here, "twice a week" refers to a 3 or 4 day gap between the first treatment and the next treatment. For example, if the first treatment is performed on Monday, the second treatment will be performed on Thursday or Friday. This process is repeated thereafter. At the start of the dry step of each cycle, the presence or absence of cracks in the bent parts of the test pieces for evaluating delayed fracture resistance was visually confirmed, and the number of cycles until cracks occurred was determined. In addition, the number of days until cracks occurred ("Days to crack" in Tables 1 and 2) was determined based on the results (presence or absence of cracks) every three cycles (every day).
[0037] This test was carried out on three specimens of each steel plate, and the average value was used for evaluation. Evaluation was based on the number of cycles and was based on the following criteria. In Tables 1 and 2, the number of cycles to crack occurrence exceeding 40 indicates that no cracks occurred in the results of this example. ◎: More than 40 cycles 〇: 30 cycles or more, 40 cycles or less △: 10 or more cycles, less than 30 cycles ×: Less than 10 cycles
[0038] (2) Maximum hydrogen permeability coefficient H t ,H 0 and H t / H 0 Calculation of hydrogen absorption amount (evaluation of hydrogen absorption amount) Maximum hydrogen permeability coefficient H twas calculated as follows. The backsides of the steel sheets of the invention and comparative examples (test pieces with an organic resin film formed only on one side (front side) of the steel sheet) with a thickness of 1.4 mm were ground and then chemically polished to a thickness of 0.5 mm. Furthermore, metal Pd was formed on the backsides by electroplating. That is, the front side of the steel sheet with the organic resin film formed thereon was the hydrogen entry surface (surface subject to corrosion test), and the backside of the steel sheet with the Pb plating was the hydrogen detection surface (surface for detecting the current generated due to hydrogen that penetrates into the steel due to corrosion). As shown in FIG. 3, the sample 5 (test piece) was fixed so that the Pd-plated surface was in contact with the current detection cells 6 (6a to 6d), and a 0.1 mol / L aqueous solution of sodium hydroxide deaerated with nitrogen gas was poured into each cell 6. A part of the sample 5 was covered with a protective film 9 to protect the sample on the reference cell 6a from corrosion. Each cell 6 was subjected to the corrosion test shown in Figure 2 while being polarized at a constant potential so as to be +0.2 V with respect to the reference electrode, and the surface of the sample 5 was corroded for up to 40 cycles to detect the current generated due to hydrogen penetrating into the steel. At this time, the net hydrogen permeation current (J) was calculated by finding the difference between the current value measured in each cell and the current value measured in the reference cell. Furthermore, the hydrogen permeation coefficient (JL) was calculated by multiplying the hydrogen permeation current by the plate thickness (L) of the test piece. The maximum value of this hydrogen permeation coefficient during the measurement was called the maximum hydrogen permeation coefficient H t In addition, the maximum hydrogen permeability coefficient H 0 was calculated as follows. A 1.4 mm thick steel plate (test piece) not having an organic resin film was processed and Pb plated in the same manner as above, and a test piece was prepared in which the front surface of the steel plate not having an organic resin film was used as the hydrogen entry surface and the back surface of the steel plate plated with Pb was used as the hydrogen detection surface. This test piece was subjected to the same corrosion test as above, and the hydrogen permeability coefficient (JL) was calculated in the same manner as above, and the maximum value of this hydrogen permeability coefficient during measurement was taken as the maximum hydrogen permeability coefficient H 0 The maximum hydrogen permeability coefficient H t The maximum hydrogen permeability coefficient H 0 By dividing by H t / H 0 Calculate H t / H 0 The case of ≦0.50 was evaluated as passing. In addition, for some comparative examples in which an organic resin film was not formed on the steel sheet surface, the maximum hydrogen permeability coefficient H 0 Only was calculated.
[0039] (3) Evaluation of film adhesion A test piece was prepared by bending in the same manner as in the evaluation test of delayed fracture resistance, and the coating on the inside of the bend after bending was cut into a grid pattern with an area of 35 mm wide x 20 mm long according to a method conforming to JIS K5600, and a tape peeling test was performed. The coating peeling area rate in this test was calculated by the following formula (coating area before peeling: 35 mm x 20 mm). Film peeling area rate=(C x / C о ) x 100 where C x : Area of film that has been peeled off and adhered to the tape C о : Film area before peeling From this peeled area rate, the coating adhesion was evaluated according to the following criteria, with ◯ being good and × being bad. ○: Peeling area rate is less than 5% ×: Film peeling area rate 5% or more
[0040] (4) Evaluation of corrosion resistance after painting The galvanized steel sheets of the invention and comparative examples were each sheared to a size of 150 mm x 70 mm to obtain flat test pieces, which were used as test pieces for corrosion resistance tests. The test pieces for corrosion resistance tests were subjected to chemical conversion treatment by immersion under standard conditions (35°C, 120 seconds) using "Palbond" manufactured by Nippon Parkerizing Co., Ltd. Next, electrodeposition coating and baking treatment were performed using electrodeposition paint "GT-150T" manufactured by Kansai Paint Co., Ltd. The coating thickness of the electrodeposition coating was 15 μm, and the coating thickness was measured using a commercially available electromagnetic coating thickness meter. After painting, the test pieces were cut with a cutter knife to make an X-cut (crossing angle 60° to 90°) that reached the base material, and a salt spray test specified in JIS Z2371 was performed for 840 hours. The maximum rust width from the cross cut of the test pieces after the test was measured, and the corrosion resistance was evaluated based on this maximum rust width as follows. That is, the maximum rust width A of each test piece was calculated assuming that the maximum rust width of the as-is steel plate was 1, and the test pieces were evaluated according to the following criteria, with ⊚ and ◯ being deemed to be pass. ◎:A≦0.8 ○:0.8 <A≦0.95 △:0.95 <A≦1.2 ×:1.2
[0041] In Tables 1 and 2, No. 1 is a comparative example of a cold-rolled steel sheet without an organic resin film formed, and the maximum hydrogen permeability coefficient H 0 The maximum hydrogen permeability coefficient during corrosion, H, is relatively high at 30μA / cm, and delayed fracture occurs early, indicating that delayed fracture resistance is low. 0 The current density was 300μA / cm, which is significantly higher than that of the comparative example of cold-rolled steel sheet No. 1, and it is clear that the delayed fracture resistance is poor. This is because, while zinc exhibits excellent sacrificial corrosion protection during the corrosion process of zinc-based coating, it generates more hydrogen than the cold-rolled steel sheet during the corrosion process.
[0042] No. 3 is a comparative example in which a film containing only organic resin (y) was formed on a cold-rolled steel sheet. The maximum hydrogen permeability coefficient during corrosion H t Although the number of cycles to cracking is improved compared to No. 1, cracking occurs in less than 30 cycles. Nos. 4 to 6 and 13 to 15 are comparative examples in which a film not satisfying the conditions of the present invention is formed on a cold-rolled steel sheet. Among them, Nos. 4 to 6, 13 and 14 crack in less than 30 cycles, like No. 3. No. 15 has poor film adhesion due to an excessive amount of organic compound (x) attached. On the other hand, Nos. 7 to 12 and 16 to 37 are invention examples in which a film satisfying the conditions of the present invention is formed on a cold-rolled steel sheet or a galvannealed steel sheet, and the number of cycles to cracking is 30 or more, high delayed fracture resistance is obtained, and the film adhesion and corrosion resistance after painting are also good. Among them, Nos. 7 to 12, 16 to 20 and 25 to 37, which use a pyridine compound as the organic compound (x), have particularly excellent corrosion resistance after painting.
[0043] [Table 1]
[0044] [Table 2] [Explanation of symbols]
[0045] 1 Test piece 1a Test piece (before stress loading) 2 Nuts 3 SUS jig 4 Volts 5 Sample (steel plate) 6a~6d Cells 7 Reference electrode 8. Opposite 9 Protective film
Claims
1. A coating (A) is provided on a surface of a steel sheet having a tensile strength of 1180 MPa or more, the coating (A) including at least one organic compound (x) selected from an azole compound, a pyridine compound, a thiocarbonyl compound, a mercapto compound, and a sulfide compound, and an organic resin (y); The coating (A) has an adhesion amount [x] of the organic compound (x) of 100 to 2000 mg / m 2 , the amount [y] of the organic resin (y) attached is 200 to 3800 mg / m 2 a ratio [x] / ([x]+[y]) of an adhesion amount [x] of an organic compound (x) to a total adhesion amount [x]+[y] of the organic compound (x) and the organic resin (y) is 0.05 to 0.5, and a film thickness is 0.3 to 4.0 μm.
2. 2. The high-strength steel plate according to claim 1, wherein the organic resin (y) is at least one selected from the group consisting of urethane-based resins, epoxy-based resins, acrylic-based resins, and ethylene-based resins.
3. A surface treatment solution for forming a coating on a surface of a steel sheet to suppress delayed fracture of a steel sheet having a tensile strength of 1180 MPa or more, A surface treatment solution comprising an organic compound (x) consisting of at least one selected from an azole compound, a pyridine compound, a thiocarbonyl compound, a mercapto compound, and a sulfide compound, and an organic resin (y).
Citation Information
Patent Citations
Galvanized steel sheet with non-chromium type treatment
JP2000248367A
Chromium-free surface treated galvanized steel
JP2000248377A
Water-based coating composition and coated article coated with the coating composition
JP2002121470A
STEEL PLATE OF 1,180 MPa IN TENSILE STRENGTH WITH SUPERIOR DELAYED FRACTURE RESISTANCE
JP2018188707A
High tensile strength cold rolled steel sheet excellent in delayed fracture resistance
JP1995054194A