Biaxially stretched polypropylene film

The biaxially stretched polypropylene film addresses the challenge of balancing smoothness and handling properties by controlling surface parameters and layer composition, resulting in a film with enhanced performance for industrial applications.

JP2024144095APending Publication Date: 2024-10-11TORAY INDUSTRIES INC

Patent Information

Application Number
JP2023220403
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2023-12-27
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing biaxially oriented polypropylene films face challenges in achieving both high smoothness and handling properties, with methods to improve smoothness often leading to poor handling, and vice versa, while also facing issues with blocking, opacity, and mechanical strength degradation.

Method used

The biaxially stretched polypropylene film is characterized by specific surface parameters such as valley volume (Vvv) and peak density (Spd) ranges, along with controlled thickness, tensile strength, and static friction coefficient, ensuring optimal smoothness and handling properties, and includes a layered structure with polypropylene and olefin elastomer resins to enhance mechanical properties.

Benefits of technology

The film achieves excellent smoothness and handling properties, reducing the risk of dent transfer and deformation, improving storage stability, and maintaining mechanical strength, making it suitable for applications like cover films and laminates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144095000005
    Figure 2024144095000005
  • Figure 2024144095000001
    Figure 2024144095000001
  • Figure 2024144095000002
    Figure 2024144095000002
Patent Text Reader

Abstract

To provide a biaxially stretched polypropylene film that offers superior smoothness and handleability to address the issues detailed in the specifications.SOLUTION: In a biaxially stretched polypropylene film, when a surface with the lower valley volume (Vvv) is defined as the A surface, the Vvv of the A surface is defined as VvvA, and the summit density (Spd) of the A surface is defined as SpdA, the VvvA is within the range of 1.0 μL / m2≤VvvA≤20 μL / m2, and the SpdA is within the range of 1.0 / mm2≤SpdA≤100 / mm2.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a biaxially oriented polypropylene film which is excellent in smoothness and handleability and can be suitably used as an industrial material film. [Background technology]

[0002] Biaxially oriented polypropylene films have excellent surface releasability and mechanical properties, and are therefore suitable for use as protective films and process films for a variety of components, including plastic products, building materials, and optical components.

[0003] When used as a protective film or cover film, biaxially oriented polypropylene film is required to be smooth in order to suppress the transfer of dents to the adherend. In particular, when used as a cover film for UV-curable resins such as dry film resists, if there are localized irregularities on the surface of the biaxially oriented polypropylene film, the irregularities will be transferred to the resist surface, causing uneven UV curing and impairing the quality. In particular, in recent years, semiconductor circuits have become increasingly finer, and the requirements for the smoothness of cover films are increasing year by year. In addition, from the viewpoint of productivity, it is expected that handling properties such as mechanical strength and slipperiness will become more important than ever before.

[0004] Generally, industrial films are often required to be thick in order to maintain their handling properties. However, in biaxially oriented polypropylene films, the thickening of the film tends to lead to the formation of β-crystals that are the source of local unevenness during crystallization, and as a result, the formation of coarse unevenness tends to occur. In order to increase the smoothness of biaxially oriented polypropylene films, there are methods such as reducing the crystallinity of the polypropylene resin itself that is contained, but in exchange, the film tends to become less smooth and the handling properties tend to deteriorate, making it difficult to achieve both smoothness and handling properties.

[0005] For these reasons, films that meet the required characteristics for future cover films must have both good handling properties and high smoothness. In addition, there is a growing need for improved blocking resistance to improve storage properties, and high transparency to improve inspection efficiency.

[0006] As films aiming for high smoothness, for example, Patent Documents 1 and 2 disclose examples of blending a propylene resin with a butene-ethylene copolymer, and blending a polypropylene resin with a low crystallinity / low melting point resin such as a rubber domain resin. Patent Document 3 discloses an example in which particles with an average particle size of 0.7 μm or less are added to the polypropylene resin of the surface layer in order to make the film smoother and improve handling. Patent Document 4 discloses an example in which smoothness is achieved by thinning the film. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2015-107612 A [Patent Document 2] International Publication No. 2022 / 075101 [Patent Document 3] JP 2017-35884 A [Patent Document 4] JP 2020-100800 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, in the method of adding a raw material having a lower melting point and lower crystallinity than the main raw material described in the above-mentioned Patent Documents 1 and 2, there was a concern that the low melting point component in the film melts or deforms during long-term storage or transportation through a heating furnace, resulting in blocking, non-smoothness, and opacity. The film described in Patent Document 3 had a high surface roughness and insufficient smoothness. In addition, there was a concern that the mechanical strength of the film in Patent Document 4 was reduced and handleability was deteriorated. Therefore, the object of the present invention is to solve the above problems and provide a biaxially oriented polypropylene film with excellent smoothness and handleability. [Means for solving the problem]

[0009] In order to solve the above problems and achieve the object, the biaxially oriented polypropylene film of the present invention has the following configuration. That is, the surface with the lower valley volume Vvv is surface A, and the Vvv of surface A is Vvv A , the peak density Spd of the A surface is Spd A When Vvv A is 1.0μL / m 2 ≦Vvv A ≦20μL / m 2 and Spd A 1.0 pcs / mm 2 ≦Spd A ≦100 pieces / mm 2 It is characterized in that:

[0010] The biaxially stretched polypropylene film of the present invention can be configured as follows and can be used as a release film, a cover film for a photocurable resin, a cover film for a dry film resist, a process film, etc. Furthermore, a laminate, a current collector, and a storage battery can be obtained using the biaxially stretched polypropylene film of the present invention. (1) The lower surface of the valley volume Vvv is surface A, and Vvv on surface A is Vvv A , the peak density Spd of the A surface is Spd A When Vvv A is 1.0μL / m 2 ≦Vvv A ≦20μL / m 2and Spd A 1.0 pcs / mm 2 ≦Spd A ≦100 pieces / mm 2 A biaxially oriented polypropylene film, (2) When the surface opposite to the surface A is surface B, the difference of 1 mm 2 The number of large dents exceeding 150 μm in major axis per unit area was 0 / mm 2 More than 10 pieces / mm 2 The biaxially oriented polypropylene film according to (1), which is as follows: (3) The surface opposite to the surface A is surface B, and Vvv of the surface B is Vvv B When set at 5.0μL / m 2 ≦Vvv A +Vvv B ≦25μL / m 2 , and 0.10≦Vvv A / Vvv B The biaxially oriented polypropylene film according to (1) or (2), wherein the elastic modulus is ≦0.70. (4) The biaxially oriented polypropylene film according to any one of (1) to (3), having an Ft, which is the product of the initial tensile strength and the film thickness in the direction perpendicular to the main orientation direction of the film, of 300 Pa·m or more and 3000 Pa·m or less. (5) The biaxially oriented polypropylene film according to any one of (1) to (4), having a thickness of 10 μm or more and 100 μm or less. (6) The biaxially oriented polypropylene film according to any one of (1) to (5), having a haze of 0.1% or more and 5.0% or less. (7) The biaxially oriented polypropylene film according to any one of (1) to (6), wherein the static friction coefficient μs between the A side and the B side is 0.1 or more and less than 1.3. (8) The biaxially stretched polypropylene film according to any one of (1) to (7), having a peak temperature of 165°C or more and 180°C or less in a melting curve obtained when the film is heated from 30°C to 260°C using a differential scanning calorimeter DSC. (9) The biaxially stretched polypropylene film according to any one of (1) to (8), in which the heat of fusion at 160°C or less is 5% to 50% of the total heat of fusion when heated from 30°C to 260°C using a differential scanning calorimeter DSC. (10) The biaxially oriented polypropylene film according to any one of (1) to (9), which is composed of at least two layers. (11) A biaxially oriented polypropylene film according to any one of (1) to (10), in which a layer containing 50% by mass or more and 90% by mass or less of polypropylene having a melting point of 160°C or more and 10% by mass or more and 50% by mass or less of an olefin-based elastomer having a melting point of 140°C or more is located on at least one outermost surface. (12) A release film obtained by using the biaxially oriented polypropylene film according to any one of (1) to (11). (13) A cover film for photocurable resin, comprising the biaxially oriented polypropylene film according to any one of (1) to (11). (14) A cover film for a dry film resist, comprising the biaxially oriented polypropylene film according to any one of (1) to (11). (15) A casting film comprising the biaxially oriented polypropylene film according to any one of (1) to (11). (16) A laminate comprising the biaxially oriented polypropylene film according to any one of (1) to (11) and a metal film in contact with at least one surface of the biaxially oriented polypropylene film. (17) The laminate according to (16), wherein the metal film contains a metal belonging to Group 1 or 2 of the periodic table. (18) A laminate comprising the biaxially oriented polypropylene film according to any one of (1) to (11) and a transparent conductive film in contact with at least one surface of the biaxially oriented polypropylene film. (19) A laminate comprising an electrolyte membrane in contact with at least one surface of the biaxially oriented polypropylene film according to any one of (1) to (11). (20) The laminate according to (19), wherein the electrolyte membrane is for a fuel cell, a semi-solid battery, or an all-solid battery. (21) A current collector using the biaxially oriented polypropylene film according to any one of (1) to (11). (22) A storage battery using the biaxially stretched polypropylene film according to any one of (1) to (11). Effect of the Invention

[0011] According to the present invention, it is possible to provide a biaxially oriented polypropylene film having excellent smoothness and handleability. [Brief description of the drawings]

[0012] [Figure 1] FIG. 13 is a conceptual diagram showing a valley volume Vvv. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In the biaxially oriented polypropylene film of the present invention, the surface with the lower valley volume Vvv is surface A, and the Vvv of surface A is Vvv A , the peak density Spd of the A surface is Spd A When Vvv A is 1.0μL / m 2 ≦Vvv A ≦20μL / m 2 and Spd A 1.0 pcs / mm 2 ≦Spd A ≦100 pieces / mm 2 The biaxially oriented polypropylene film of the present invention is described in detail below.

[0014] The valley volume Vvv (hereinafter, sometimes simply referred to as Vvv) is one of the surface parameters obtained from a scanning white light interference microscope. More specifically, as shown in FIG. 1, the valley volume Vvv (symbol 2) is the area surrounded by a load curve (symbol 1) drawn with the vertical axis representing height and the horizontal axis representing the areal load ratio, an equivalent line (symbol 3) at an areal load ratio of 80%, and a position line (symbol 4) at an areal load ratio of 100%. Vvv represents the volume of the space of the protruding valley on the surface, and a small Vvv means that the surface of the biaxially oriented polypropylene film tends to have fewer coarse recessed structures.

[0015] In general biaxially oriented polypropylene films for industrial use, methods for controlling convex portions are often used, but intentional control of concave portions is rare. On the other hand, in the manufacturing process of biaxially oriented polypropylene films, coarse spherulite structures such as β crystals formed during the crystallization process are stretched, and coarse concave portions with major diameters exceeding several hundred μm are easily formed. When a biaxially oriented polypropylene film having such concave portions is used as a cover film and laminated to a mating member such as a resist resin, air pockets may be generated and the surface of the mating member may be deformed. Therefore, it is important that the biaxially oriented polypropylene film of the present invention has a valley volume Vvv controlled within an appropriate range to solve the problems of smoothness and handleability. In addition, the surface with a low valley volume Vvv refers to the surface with a relatively low valley volume Vvv of the two surfaces of the biaxially oriented polypropylene film, and the Vvv on that surface is Vvv A It becomes.

[0016] In the biaxially oriented polypropylene film of the present invention, from the viewpoint of achieving both smoothness and handleability, Vvv A is 1.0μL / m 2 ≦Vvv A ≦20μL / m 2 From the above viewpoint, Vvv A The lower limit is preferably 2.5 μL / m 2 , more preferably 3.0 μL / m 2 , and more preferably 3.5 μL / m 2 It is. A is 1.0μL / m 2 If the Vvv is smaller than 100%, the biaxially oriented polypropylene film may not be slippery when used as an industrial material film, and the handling properties may be deteriorated. A The upper limit is preferably 15 μL / m 2 , more preferably 10 μL / m 2 and more preferably 7.5 μL / m 2 and particularly preferably 5.0 μL / m 2 It is. A is 20μL / m 2If it is larger, for example, when a biaxially oriented polypropylene film is used as a cover film for a UV-curable resin, the rough recessed structure on the surface may cause the flatness and curing non-uniformity of the cured resin to occur, resulting in a decrease in quality. Note that Vvv can be measured using a scanning white light interference microscope and an associated analysis system, and the details of the measurement method are shown in the Examples.

[0017] Vvv A In order to make the above range, for example, the raw material composition of the biaxially stretched polypropylene film can be set to the range described later, and the film-forming conditions can be set to the range described later. In particular, it is effective to use a polypropylene resin having a crystallization rate in an appropriate range as the main component, control the crystallization rate of the resin constituting the outermost layer of the film, and make the spherulite size formed during casting fine. In addition, in terms of the film-forming process, it is effective to lower the casting drum temperature and make the spherulite size fine. Furthermore, in order to promote the transition from β crystals to α crystals in the preheating step of the longitudinal stretching step, it is effective to set the preheating temperature to a proper temperature range below the melting point of the polypropylene resin to be added. These methods can be used in combination as appropriate as long as they do not impair the effects of the present invention.

[0018] Peak density Spd (hereinafter sometimes simply referred to as Spd) is one of the surface parameters obtained from a scanning white light interference microscope. Spd represents the number of surface peaks per unit area, and a large Spd means that a fine protrusion structure tends to be formed on the surface of the biaxially oriented polypropylene film. There are few examples of intentionally controlling Spd in general biaxially oriented polypropylene for industrial use, but for the biaxially oriented polypropylene film of the present invention, it is important to control the peak density Spd within an appropriate range as described below.

[0019] In the biaxially oriented polypropylene film of the present invention, from the viewpoint of improving the handling property, the peak density Spd of the A side is set to Spd A When Spd A 1.0 pcs / mm 2 ≦Spd A ≦100 pieces / mm2 From the above perspective, Spd A The lower limit is preferably 2.0 pieces / mm 2 , more preferably 3.0 pieces / mm 2 It is. A 1.0 pcs / mm 2 If the content is less than 100%, the surface becomes excessively smooth, and when the biaxially oriented polypropylene film is used as an industrial material film, the surface becomes less smooth and the handling properties may deteriorate. A The upper limit is preferably 60 pieces / mm 2 , more preferably 40 pieces / mm 2 and more preferably 20 pieces / mm 2 It is. A 100 pieces / mm 2 If it is larger, the height difference of the protrusion structure on the surface of the biaxially oriented polypropylene film tends to be small, and when used as an industrial material film, it may become difficult to slip and have poor handling properties. Spd can be measured using a scanning white light interference microscope and an associated analysis system, and the details of the measurement method are shown in the Examples.

[0020] Spd A In order to make the above range, for example, a method can be used in which the raw material composition of the biaxially oriented polypropylene film is within the range described later, and the film-forming conditions are within the range described later. In particular, it is effective to add a highly dispersible olefin-based elastomer resin to the polypropylene resin, which is the main component of the surface layer, at an appropriate ratio, to finely disperse the elastomer resin in the polypropylene resin matrix during casting, thereby forming a dense domain structure in the surface layer. In terms of the film-forming process, it is effective to set the casting drum temperature and cast sheet thickness to an appropriate range described later, and to set the temperature range in the preheating and stretching steps during longitudinal stretching and transverse stretching to a proper temperature range higher than the softening temperature of the elastomer resin to be added and lower than the melting point of the polypropylene resin to be added, thereby finely refining the dense domain structure formed during casting within an appropriate range and forming a moderately fine protrusion structure. These methods can also be used in combination as appropriate.

[0021] In the biaxially oriented polypropylene film of the present invention, when the film is used as a cover film for a photocurable resin, the occurrence of transfer marks on the cured resin surface is reduced, and the efficiency of foreign matter inspection is increased. In this respect, when the surface opposite to the surface A is surface B, the film is provided with a 1 mm 2 The number of large dents exceeding 150 μm in major axis per unit area was 0 / mm 2 More than 10 pieces / mm 2 From the above viewpoint, it is preferable that the thickness of the surface of the substrate is 1 mm or less on both sides of the A and B. 2 The number of large dents exceeding 150 μm in major axis per unit area is 10 / mm 2 Preferably less than 7.0 pieces / mm 2 Less than 5.0 pieces / mm, more preferably 5.0 pieces / mm 2 Less than 4.0 pieces / mm 2 The following is the result.

[0022] 1mm on both sides A and B 2 The number of large dents per unit area is 10 / mm 2 By being less than 1 mm on both sides A and B, when the biaxially oriented polypropylene film is used as a cover film for photocurable resin, the possibility of leaving a transfer mark on the cured resin surface is reduced, and in addition, the deterioration of the appearance and the influence on foreign body inspection can be reduced. 2 The fewer the number of the coarse recesses per mm, the better. The lower limit is 0 recesses per mm. 2 The "large dent" defined in the present invention is a shape having a large dent with a major axis of 150 μm or more, and is defined in the description of the examples described later. 2 The number of the coarse dents per unit area can be measured using a scanning white light interference microscope and an associated analysis system, and the details of the measurement method will be shown in the Examples.

[0023] 1mm on both sides A and B 2In order to make the number of the coarse recesses per unit area within the above range, for example, a method can be used in which the raw material composition of the biaxially oriented polypropylene film is within the range described below, and the film-forming conditions are within the range described below. In particular, it is effective to add a propylene-based elastomer resin having a higher dispersibility in propylene resin to a polypropylene resin having a crystallization rate within an appropriate range in an appropriate ratio, thereby controlling the crystallization rate of the resin constituting each layer as a whole to an optimal range and suppressing the formation of coarse β crystal spherulites. In addition, in terms of the film-forming process, it is effective to make the thickness of the cast sheet within an appropriate range and optimize the air temperature of the air knife to refine the α crystal and β crystal spherulites formed during casting to an appropriate range, from the viewpoint of efficiently cooling both sides of the sheet on the cast drum. Note that these methods can also be used in combination as appropriate.

[0024] In the biaxially oriented polypropylene film of the present invention, from the viewpoint of achieving both quality and ease of handling, the side opposite to side A is side B, and the Vvv of side B is Vvv B When set at 5.0μL / m 2 ≦Vvv A +Vvv B ≦25μL / m 2 , and 0.10≦Vvv A / Vvv B It is preferable that Vvv is ≦0.70. A +Vvv B The lower limit is more preferably 9.0 μL / m 2 , and more preferably 10 μL / m 2 It is. A +Vvv B is 5.0μL / m 2 By virtue of the above, when the biaxially oriented polypropylene film is used as an industrial material film, the film maintains its slipperiness and has good handleability. A +Vvv B The upper limit is more preferably 20 μL / mm 2 , and more preferably 18 μL / mm 2 It is. A is 25μL / mm 2By satisfying the above condition, when the biaxially oriented polypropylene film is used as an industrial material film, deterioration of the roll shape caused by surface unevenness can be suppressed, and when the film is used as a cover film for photocurable resin, deterioration of quality can be reduced. A +Vvv B can be measured by a scanning white light interference microscope and an associated analysis system, and the details of the measurement method will be shown in the Examples.

[0025] In the biaxially oriented polypropylene film of the present invention, Vvv A / Vvv B From the above viewpoint, the upper limit of Vvv is more preferably 0.60, and even more preferably 0.50. A / Vvv B By making Vvv less than 0.70, the biaxially oriented polypropylene film has a difference in smoothness between the front and back. Therefore, when the biaxially oriented polypropylene film is used as an industrial material film, even if the film has high smoothness, the static friction coefficient μs between the front and back of the film is kept low, resulting in good handling properties. A / Vvv B The lower limit of Vvv is more preferably 0.20, and even more preferably 0.30. A / Vvv B By making Vvv 0.10 or more, the smoothness of both sides of the biaxially oriented polypropylene film is maintained, so that when it is used as an industrial material film, the occurrence of dent transfer is suppressed, and the quality of the mating member to be laminated is improved. A / Vvv B can be measured by a scanning white light interference microscope and an associated analysis system, and the details of the measurement method will be shown in the Examples.

[0026] Vvv A +Vvv B and Vvv A / Vvv BIn order to keep within the above range, for example, a method can be used in which the raw material composition of the biaxially oriented polypropylene film is set within the range described below, and the film-forming conditions are set within the range described below. In particular, in order to form an appropriate structural difference between the front and back of the sheet at the time of casting, it is effective to control the influence on the crystallization of the main component polypropylene within an appropriate range by setting the melting point and MFR of the resin added other than the main component polypropylene within an appropriate range. In addition, in terms of the film-forming process, in addition to optimizing the air temperature and air speed of the air knife, it is effective to increase the thickness of the cast sheet (preferably 1.0 mm or more and 1.5 mm or less, more preferably 1.1 mm or more and 1.5 mm or less) and control the difference in the uneven structure between the front and back of the film within an appropriate range. These methods can also be used in combination as appropriate.

[0027] From the viewpoint of improving the handling property, the biaxially oriented polypropylene film of the present invention preferably has Ft, which is the product of the initial tensile strength and the film thickness in the direction perpendicular to the main orientation direction of the film and the film plane, of 300 Pa·m or more and 3000 Pa·m or less. From the above viewpoint, the lower limit of Ft, which is the product of the initial tensile strength and the film thickness in the direction perpendicular to the main orientation direction of the film and the film plane, is more preferably 500 Pa·m, even more preferably 700 Pa·m, particularly preferably 900 Pa·m, and most preferably 950 Pa·m. By having Ft of 300 Pa·m or more, when used as an industrial material film, deformation is suppressed even when a load is applied to the film, and wrinkles and sagging are unlikely to occur during transportation, so that the handling property is good. Also, from the above viewpoint, the upper limit of Ft is more preferably 2000 Pa·m, and even more preferably 1500 Pa·m. By having Ft of 3000 Pa·m or less, the rigidity of the biaxially oriented polypropylene film is suppressed, and the occurrence of winding defects and the like is reduced, so that the handling property is improved.

[0028] The main orientation direction is the direction that gives the highest initial tensile strength when an arbitrary direction is set as 0° in the film plane and the initial tensile strength is measured in each direction that forms an angle of 0° to 165° with respect to the arbitrary direction at 15° intervals. The details of the measurement method of the initial tensile strength and Ft are shown in the Examples.

[0029] In order to set the Ft value within the above range, for example, a method can be used in which the raw material composition of the biaxially oriented polypropylene film is set within the range described below, and the film forming conditions are set within the range described below. In particular, it is effective to set the film thickness within an appropriate range in addition to setting the molecular weight and melting point of the polypropylene resin used within an appropriate range.

[0030] The biaxially oriented polypropylene film of the present invention preferably has a thickness of 10 μm or more and 100 μm or less from the viewpoint of achieving both smoothness and handleability. From the above viewpoint, the lower limit of the thickness is more preferably 15 μm, and even more preferably 21 μm. When the biaxially oriented polypropylene film is used as an industrial material film, the mechanical strength is ensured by having a thickness of 10 μm or more, and thus the handleability is improved. From the above viewpoint, the upper limit of the thickness is more preferably 50 μm, and even more preferably 40 μm. When the thickness is 100 μm or less, the handleability of the biaxially oriented polypropylene film is improved, and the smoothness is improved because the film is efficiently cooled during casting. The thickness of the biaxially oriented polypropylene film can be adjusted by the screw rotation speed of the extruder, the slit gap of the die, the thickness and width of the cast sheet, the film production speed, the stretching ratio, and the like. The thickness of the biaxially oriented polypropylene film can be measured by a micro thickness meter, and the detailed measurement method will be described later.

[0031] From the viewpoint of improving the handleability, the biaxially oriented polypropylene film of the present invention preferably has a static friction coefficient μs between the A side and the B side (hereinafter, simply referred to as μs) of 0.1 or more and less than 1.3. From the above viewpoint, μs is more preferably less than 1.2, even more preferably less than 1.0, and particularly preferably less than 0.8. By having μs less than 1.3, the handleability of the biaxially oriented polypropylene film is improved, and the transport and winding properties are improved. In addition, the lower limit of μs is 0.1 from the viewpoint of feasibility such as compatibility with smoothness. The static friction coefficient μs can be measured in accordance with JIS K 7125 (1999), and the details thereof will be described later.

[0032] In order to set the μs of the biaxially stretched polypropylene film in the above-mentioned preferred range, for example, a method can be used in which the raw material composition of the film is set in the range described below and the film-forming conditions are set in the range described below. A In addition to controlling the surface roughness within the above range to form an appropriate fine projection structure on the surface, it is effective to use polypropylene resin or elastomer resin with high softening and melting points to reduce low melting point or low crystalline components that may become adhesive parts. These methods can be used in combination as appropriate.

[0033] From the viewpoint of transparency, the biaxially oriented polypropylene film of the present invention preferably has a haze of 0.1% or more and 5.0% or less. The haze is more preferably 3.0% or less, further preferably 1.5% or less, and particularly preferably 1.0% or less. By having a haze of 5.0% or less, for example, when used as a protective film, the transparency of the protective film is maintained even after passing through the above-mentioned conveying process in which high temperatures are applied, and defects occurring when inspecting with a defect inspection machine in a state where the film is laminated to an adherend are reduced. The lower limit of the haze is better, but from the viewpoint of feasibility, it is substantially about 0.1%.

[0034] In order to set the haze of the biaxially oriented polypropylene film within the above range, it is effective to set the raw material composition and film-making conditions of the film within the ranges described below. A In addition to controlling the number of small and large recesses within the above range to form a fine uneven surface structure within an appropriate range, it is effective to set the melting point of the added resin within an appropriate range, reduce the difference in melting point between the main component polypropylene resin and other additives, and suppress the collapse of the uneven structure during the stretching process. In terms of the film-making process, it is effective to set the stretching temperature in the longitudinal stretching and transverse stretching processes below the melting point of each resin constituting the film. The haze can be measured by the method specified in JIS K 7136 (2000), and the details will be described later.

[0035] From the viewpoint of improving the handleability, the biaxially stretched polypropylene film of the present invention preferably has a peak temperature of 165°C or more and 180°C or less in the melting curve obtained when the temperature is raised from 30°C to 260°C by a differential scanning calorimeter DSC. From the above viewpoint, the peak temperature of the melting curve obtained by DSC (differential scanning calorimeter) is more preferably 167°C or more, and even more preferably 168°C or more. When the peak temperature of the melting curve is 165°C or more, the crystal orientation proceeds sufficiently, and the mechanical strength and the associated handleability are improved. From the above viewpoint, the peak temperature of the melting curve is more preferably 175°C or less. When the peak temperature of the melting curve is 180°C or less, excessive crystal orientation in the biaxially stretched polypropylene film is suppressed, and the deterioration of the handleability, such as an excessive increase in stiffness and the associated poor winding, is reduced.

[0036] In order to set the peak temperature of the melting curve within the above range in consideration of the above points, for example, it is effective to set the raw material composition of the biaxially stretched polypropylene film within the range described below, and to set the film-forming conditions within the range described below. In particular, it is effective to add a polypropylene resin or elastomer resin with a high melting point to suppress the reduction in crystallinity and orientation of the film. In addition, in terms of the film-forming process, by setting the preheating temperature and stretching temperature during transverse stretching to be equal to or lower than the melting point of the polypropylene resin contained, transverse stretching is possible without significantly relaxing the oriented structure of the uniaxially stretched film after longitudinal stretching, which is effective in forming a film with a more stable crystal structure. These methods can also be used in combination as appropriate.

[0037] From the viewpoint of improving blocking resistance, the biaxially oriented polypropylene film of the present invention is preferably such that the heat of fusion of 160°C or less is 5% to 50% of the total heat of fusion when heated from 30°C to 260°C by a differential scanning calorimeter DSC. From the above viewpoint, the ratio of the heat of fusion of 160°C or less is more preferably 45% or less, and even more preferably 40% or less. By making the ratio of the heat of fusion of 160°C or less 50% or less, the amount of low-melting point components that are likely to cause deformation or fusion when stored for a long period of time in an oven or in a wound state during heating is suppressed, thereby reducing the occurrence of slippage and blocking. In addition, the lower the ratio of the heat of fusion of 160°C or less, the better, but due to the characteristics of polypropylene resin, the substantial lower limit is 5%.

[0038] In consideration of the above, in order to set the heat of fusion of 160°C or less within the above range, for example, the raw material composition of the film is set to the range described later, and the film-forming conditions are set to the range described later. In consideration of the above, in order to set the peak temperature of the melting curve within the above range, for example, the raw material composition of the biaxially stretched polypropylene film is set to the range described later, and the film-forming conditions are set to the range described later. In particular, it is effective to add a polypropylene resin or elastomer resin with a high melting point to suppress the reduction in crystallinity and orientation of the film. In addition, in terms of the film-forming process, by setting the preheating temperature and stretching temperature during transverse stretching to the melting point of the polypropylene resin contained or lower, transverse stretching is possible without significantly relaxing the orientation structure of the uniaxially stretched film after longitudinal stretching, and it is effective to form a film with a more stable crystal structure. In addition, these methods can be used in combination as appropriate.

[0039] Next, the raw materials for the biaxially oriented polypropylene film of the present invention will be described, but the raw materials are not necessarily limited thereto.

[0040] The biaxially stretched polypropylene film of the present invention is mainly composed of a polypropylene resin. In the present invention, the "main component" means a component that accounts for more than 50% by mass and not more than 100% by mass of the total components of the film, more preferably 90% by mass or more and not more than 100% by mass, even more preferably 95% by mass or more and not more than 100% by mass, still more preferably 96% by mass or more and not more than 100% by mass, particularly preferably 97% by mass or more and not more than 100% by mass, and most preferably 98% by mass or more and not more than 100% by mass.

[0041] The biaxially stretched polypropylene film of the present invention may contain only one type of polypropylene resin, but preferably contains two or more types of polyolefin resins including polypropylene resin. When the film contains two or more components equivalent to polypropylene resin, the film is deemed to be "mainly composed of polypropylene resin" if the total amount of these components is more than 50% by mass and not more than 100% by mass.

[0042] The polypropylene resin refers to a polyolefin resin that contains more than 50 mol % and not more than 100 mol % of propylene units, when all structural units constituting the molecular chain of the resin are taken as 100 mol %.

[0043] The biaxially oriented polypropylene film of the present invention is not particularly limited in terms of its layer structure, and may have either a single layer or a laminate structure, but from the viewpoint of satisfying different properties such as smoothness and handleability, it is preferably composed of at least two layers, more preferably has a surface layer (I) and a base layer (II), and further preferably has a surface layer (I) on both sides of the base layer (II). When there are multiple surface layers (I), the compositions of the surface layers (I) may be the same or different.

[0044] The polypropylene resin A, which is the most suitable component contained in the biaxially oriented polypropylene film of the present invention, will be described below.

[0045] In the biaxially oriented polypropylene film of the present invention, the Mw of the polypropylene resin A is 20×104 More than 60×10 4 From the viewpoint of crystallization behavior and film strength, it is preferable that the lower limit of Mw is 30×10 4 is more preferable, with an upper limit of 50×10 4 In order to set the Mw of the polypropylene resin A of the present invention to the above value, a method of adjusting the hydrogen gas concentration during polymerization, or appropriately selecting a catalyst and / or a co-catalyst and a composition are preferably adopted.

[0046] In the biaxially oriented polypropylene film of the present invention, the lower limit of the melting point of polypropylene resin A is preferably 155 ° C, more preferably 160 ° C. When the melting point of polypropylene resin A is 155 ° C or higher, the obtained biaxially oriented polypropylene film has excellent heat resistance, and when used as a release film, for example, it maintains its shape even when passing through a heat-applied process after being laminated with an adherend, and the adherend can be prevented from being deformed. From the above viewpoint, the upper limit of the melting point of polypropylene resin A is preferably 167 ° C, more preferably 165 ° C. By having the melting point of polypropylene resin A of the present invention be 167 ° C or lower, the crystal formation rate is appropriately suppressed, so that the formation of a coarse uneven structure during crystallization by casting is suppressed, and the smoothness of the biaxially oriented polypropylene film is good.

[0047] In the biaxially oriented polypropylene film of the present invention, the lower limit of the half crystallization time of polypropylene resin A is preferably 50 seconds, more preferably 100 seconds, even more preferably 200 seconds, and particularly preferably 300 seconds. By having the half crystallization time of polypropylene resin A be 50 seconds or more, the crystal formation is not excessively fast, so that the formation of coarse spherulites during crystallization by casting is suppressed, and the smoothness of the biaxially oriented polypropylene film is good. In addition, the upper limit of the half crystallization time of polypropylene resin A is preferably less than 1500 seconds, more preferably 1000 seconds or less. By having the half crystallization time be 1500 seconds or less, the crystal formation is sufficient, and fine unevenness is easily formed on the film surface. Therefore, the biaxially oriented polypropylene film becomes easy to slip and has good handleability.

[0048] The half-crystallization time of polypropylene resin A in the biaxially stretched polypropylene film of the present invention is an index showing the crystallization rate, which is obtained by isothermal crystallization measurement at 130°C using DSC. The crystallization rate is determined by a combination of factors such as stereoregularity, crystallinity, and molecular weight. The detailed method and device for measuring the half-crystallization time of polypropylene resin A will be described in the Examples below.

[0049] In particular, the polypropylene resin A used in the outermost layer of the biaxially oriented polypropylene film of the present invention has a melting point of preferably 165° C., more preferably 163° C., in order to form fine irregularities on the surface. The melting point of the polypropylene resin A is preferably equal to or higher than the melting point of the elastomer resin added to the layer, and is preferably higher than the melting point of the elastomer resin added to the layer. Furthermore, the semi-crystallization time of the polypropylene resin A is preferably 300 seconds or more, and more preferably 1500 seconds or less.

[0050] The polypropylene resin A is not particularly limited as long as it satisfies the above-mentioned preferred conditions. Examples of polypropylene resins that can be used in the biaxially oriented polypropylene film of the present invention and are commercially available include polypropylene resins E-203GP and F113G manufactured by Prime Polymer Co., Ltd., polypropylene resins D101, FS2011DG3, and FSX20L8 manufactured by Sumitomo Chemical Co., Ltd., and polypropylene resins FY6H and FL4 manufactured by Japan Polypropylene Corporation.

[0051] The biaxially stretched polypropylene film of the present invention preferably contains an elastomer resin, which is a polyolefin resin different from the above-mentioned polypropylene resin A. By adding and dispersing the elastomer resin in the above-mentioned polypropylene resin, it becomes easier to promote the refinement of the structure during casting or stretching.

[0052] As the type of elastomer resin, from the viewpoint of dispersibility in polypropylene resin A and the effect of refining the structure formed by the polypropylene resin, an olefin-based elastomer is preferred, and a propylene-based elastomer is more preferred. Examples of commercially available elastomer resins that can be used in the biaxially stretched polypropylene film of the present invention include "Toughmer" (registered trademark) PN2060, PN2070, and BL3450 manufactured by Mitsui Chemicals, Inc., "Dynaron" (registered trademark) 2324P manufactured by JSR Corporation, and "Milastomer" (registered trademark) 8030NHS manufactured by Mitsui Chemicals, Inc.

[0053] From the viewpoint of dispersibility in polypropylene resin, the MFR of the elastomer resin is 5.0 g / 10 min to 50 g / 10 min, preferably 5.0 g / 10 min to 10 g / 10 min. The MFR of the elastomer resin is a value measured at a temperature of 230°C and a load of 21.2 N based on JIS K 7210 (2014).

[0054] From the viewpoint of handling property and blocking resistance, it is preferable that the elastomer resin has a melting point. The melting point of the elastomer resin can be measured by DSC (differential thermal scanning calorimeter), and each peak of the melting curve is taken as the melting point. The lower limit of the melting point of the elastomer resin is preferably 100°C, more preferably 140°C, further preferably 155°C, and particularly preferably 160°C, in order to suppress melting and deformation during heating and blocking during long-term storage. In addition, from the viewpoint of film-forming property, the upper limit of the melting point is preferably 250°C, more preferably 200°C, and further preferably 165°C.

[0055] In order to obtain an appropriate difference in extensibility between the elastomer resin and the polypropylene resin, the lower limit of the softening temperature of the elastomer resin is preferably 100° C., more preferably 110° C., and further preferably 120° C. From the above viewpoints, the upper limit of the softening temperature of the elastomer resin is preferably 150° C., more preferably 140° C. The softening temperature of the elastomer resin can be measured by the method specified in JIS K 7196 (1991), the details of which will be described later.

[0056] In the biaxially stretched polypropylene film of the present invention, the proportions of the polypropylene resin and the elastomer resin relative to the total amount of resin components are preferably as follows. The polypropylene resin is preferably 90% by mass or more from the viewpoints of the mechanical strength, handleability, etc. of the film. The lower limit of the proportion of the polypropylene resin is more preferably 95% by mass, and even more preferably 98% by mass. The proportion of the elastomer resin is preferably 0.10% by mass or more and 5.0% by mass or less of the total amount of resin components. The lower limit of the proportion of the elastomer resin is more preferably 0.50% by mass. The upper limit of the proportion of the elastomer resin is more preferably 4.5% by mass, and even more preferably 2.0% by mass.

[0057] The proportions of polypropylene resin and elastomer resin in the total amount of resin components in the outermost layer of the biaxially oriented polypropylene film of the present invention are preferably as follows: The lower limit of the proportion of polypropylene resin in the outermost layer is preferably 60% by mass, more preferably 70% by mass, The upper limit of the proportion of polypropylene resin in the outermost layer is preferably 99% by mass, more preferably 95% by mass, even more preferably 90% by mass, and particularly preferably 85% by mass.

[0058] The preferred range of the proportion of the elastomer resin in the outermost layer differs between the propylene-based elastomer resin and the other elastomer resin in terms of dispersibility in polypropylene. The lower limit of the proportion of the propylene-based elastomer resin in the outermost layer is preferably 1% by mass, more preferably 10% by mass, and even more preferably 20% by mass. The upper limit of the proportion of the elastomer resin in the outermost layer is preferably 40% by mass, more preferably 35% by mass, and even more preferably 30% by mass. The lower limit of the proportion of the elastomer resin other than the propylene-based resin in the outermost layer is preferably 0.1% by mass or more, and more preferably 1.0% by mass or more. The upper limit of the proportion of the elastomer resin other than the propylene-based resin in the outermost layer is preferably 20% by mass, more preferably 10% by mass, and even more preferably 5.0% by mass. When the proportion of polypropylene resin and elastomer resin is within the above range, adverse effects such as adhesion caused by the elastomer resin are suppressed, while the surface irregularities of the biaxially oriented polypropylene film are easily refined and the surface is easily smoothed.

[0059] The polypropylene resin and elastomer resin used in the biaxially oriented polypropylene film of the present invention may contain various additives, such as a crystal nucleating agent, an antioxidant, a heat stabilizer, a slipping agent, an antistatic agent, an antiblocking agent, a filler, a viscosity modifier, a color inhibitor, etc., within the scope of not impairing the object of the present invention. These additives may be added to any layer, and multiple types may be used in combination, as long as they do not impair the effects of the present invention.

[0060] Among these, the selection of the type and amount of antioxidant is important from the viewpoint of antioxidant bleed-out. That is, such antioxidants are sterically hindered phenol-based, and at least one of them is preferably a high molecular weight type with a molecular weight of 500 or more. Specific examples include various types, but it is preferable to use 2,6-di-t-butyl-p-cresol (BHT: molecular weight 220.4), 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene (e.g., BASF's "Irganox" (registered trademark) 1330: molecular weight 775.2), tetrakis[methylene-3(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane (e.g., BASF's "Irganox" (registered trademark) 1010: molecular weight 1177.7), etc., alone or in combination.

[0061] In particular, phosphorus-based antioxidants may easily bleed out onto the surface of the biaxially oriented polypropylene film. Such bleed-out may induce various problems. For example, when a resin film is formed on the surface of the biaxially oriented polypropylene film, curing may be inhibited if the uncured or semi-cured resin film is subjected to a curing treatment. In addition, when an electrolyte membrane or a metal membrane is formed on the surface of the biaxially oriented polypropylene film, the properties of the electrolyte membrane and the quality of the metal layer may be reduced. From the above viewpoint, the content of the phosphorus-based antioxidant in the biaxially oriented polypropylene film is preferably 100 ppm or less, more preferably 50 ppm or less, and even more preferably 10 ppm or less. From the above viewpoint, it is preferable that the phosphorus-based antioxidant is not contained in the biaxially oriented polypropylene film, and the lower limit of the content is 0 ppm. Examples of phosphorus-based antioxidants include tris(2,4-di-t-butylphenyl)phosphite (e.g., BASF's "Irgafos" (registered trademark) 168: molecular weight 647).

[0062] In the biaxially oriented polypropylene film, the total content of these antioxidants is preferably in the range of 0.03 to 1.0 parts by mass relative to the total amount of resin. If the amount of antioxidant is too small, the polymer may deteriorate during the extrusion process, causing the film to become discolored, or the film may have poor long-term heat resistance. If the amount of antioxidant is too large, the transparency may decrease due to the bleed-out of these antioxidants. From the above viewpoints, the content of the antioxidant is more preferably 0.05 to 0.9 parts by mass, particularly preferably 0.1 to 0.8 parts by mass, relative to the total amount of resin.

[0063] A crystal nucleating agent can be added to the biaxially stretched polypropylene film of the present invention within a range that does not interfere with the purpose. Specific examples of crystal nucleating agents include α crystal nucleating agents (dibenzylidene sorbitols, sodium benzoate, etc.), β crystal nucleating agents (potassium 1,2-hydroxystearate, magnesium benzoate, amide-based compounds such as N,N'-dicyclohexyl-2,6-naphthalenedicarboxamide, quinacridone-based compounds, etc.). However, since excessive addition of the above-mentioned other types of nucleating agents may cause a decrease in stretchability or a decrease in transparency and strength due to void formation, etc., the amount added is 0.5 parts by mass or less, preferably 0.1 parts by mass or less, and more preferably 0.05 parts by mass or less, based on the total amount of resin.

[0064] The biaxially oriented polypropylene film of the present invention preferably does not contain organic particles and inorganic particles. The polypropylene resin that can be preferably used as the main component of the biaxially oriented polypropylene film of the present invention has low affinity with organic particles and inorganic particles, so if these particles are included, the particles may fall off during the film-forming process and contaminate the process or product. In addition, if coarse protrusions are formed on the surface of the biaxially oriented polypropylene film by particles with high hardness, when the film is used as a release film for an optical member, the unevenness may be transferred to the resin layer of the optical member. Therefore, when the film is used as a protective film or a manufacturing base film for products that require high quality, such as display members, it may cause a decrease in quality. From the above viewpoint, the polypropylene film of the present invention preferably does not contain organic particles, inorganic particles, etc.

[0065] The biaxially oriented polypropylene film of the present invention is preferably obtained by biaxially stretching an unstretched sheet obtained by using the above-mentioned resin. As the method of biaxial stretching, any of the inflation simultaneous biaxial stretching method, the tenter simultaneous biaxial stretching method, and the successive biaxial stretching method using a roll-type stretching machine and a tenter can be used. Among them, the successive biaxial stretching method using a roll-type stretching machine and a tenter is preferably adopted from the viewpoints of controlling the film formation stability, the thickness uniformity, the high rigidity and the dimensional stability of the film.

[0066] Next, one embodiment of the manufacturing method for the biaxially oriented polypropylene film of the present invention will be described mainly using a two-type three-layer biaxially oriented polypropylene film having a structure of surface layer (I) / base layer (II) / surface layer (I) as an example, but the biaxially oriented polypropylene film of the present invention is not necessarily limited to this.

[0067] First, a polypropylene resin and an elastomer resin (or a different type of polypropylene resin) are dry-blended in an arbitrary ratio to obtain a resin composition. Thereafter, in order to increase the dispersibility of the elastomer resin or the different type of polypropylene resin, it is preferable to melt-mix the resin composition as described below and use it as pellets. As an example, the obtained dry blend of the resin composition is charged from a hopper in a twin-screw extruder and melt-mixed at a maximum temperature of 250 to 270°C. Next, resin strands are generated, and after continuous water cooling, pellets are made using a strand cutter to obtain pellets of the melt-blended (melt-mixed) resin composition.

[0068] The pellets of the resin composition obtained above are fed to a single screw extruder for the surface layer (I), and the polypropylene resin is fed to a single screw extruder for the base layer (II). Then, melt extrusion is performed at 200 to 280°C, more preferably 220 to 280°C, even more preferably 240 to 270°C, and particularly preferably 240°C to 255°C, respectively. Then, after removing foreign matter and modified polymers with a filter installed in the middle of the polymer tube, the layers are laminated in a layer structure of surface layer (I) / base layer (II) / surface layer (I) with a multi-manifold type composite T-die, and discharged onto a casting drum and cooled and solidified to obtain a laminated unstretched sheet having a layer structure of surface layer (I) / base layer (II) / surface layer (I). At this time, the lamination thickness ratio is preferably in the range of 1 / 10 / 1 to 1 / 60 / 1. By setting the thickness within the above range, the surface layer (I) containing the elastomer resin is formed thinly and uniformly on the film surface, thereby increasing the uniformity of the height of the irregularities formed during stretching and suppressing the formation of a coarse irregular structure.

[0069] As long as the effects of the invention are not impaired, the layer structure may be a two-layer laminate structure of surface layer (I) / base layer (II), or a three-layer laminate structure of surface layer (I) / base layer (II) / surface layer (III) by using a resin composition or polypropylene resin different from the surface layer (I) and base layer (II) as the surface layer (III).

[0070] In addition, in order to suppress the formation of β-crystal spherulites during crystallization, the surface temperature of the casting drum is 10 to 45°C, preferably 10 to 40°C, more preferably 15 to 30°C, and even more preferably 15 to 25°C. As a method for adhering to the casting drum, any method may be used from among an electrostatic application method, an adhering method using the surface tension of water, an air knife method, a press roll method, and an underwater casting method, but the air knife method, which has good flatness and allows control of surface roughness, is preferred. From the viewpoint of cooling the non-cooled drum surface of the sheet on the casting drum, it is preferable to lower the air temperature of the air knife. The air temperature of the air knife is 10 to 45°C, preferably 10 to 35°C, more preferably 10 to 25°C, and even more preferably 15 to 20°C, and the blowing air speed is preferably 130 to 150 m / s. In addition, it is also preferable to appropriately adjust the position of the air knife so that air flows downstream of the film production in order to prevent vibration of the film. In the case of a two-kind, two-layer laminate structure of surface layer (I) / base layer (II), it is preferable that the surface layer (I) side faces the casting drum.

[0071] At this time, the thickness of the cast sheet is preferably 0.4 mm or more and 1.5 mm or less. By having a thickness of 0.4 mm or more, it is possible to maintain the thickness in a suitable range even when stretched under the preferred stretching conditions described later, and in addition, excessive refinement of spherulites formed during casting is suppressed, and it becomes easy to maintain the surface unevenness structure expressed by Spd and the like in a suitable range. As a result, the handleability of the obtained biaxially stretched polypropylene film is improved. On the other hand, by having a thickness of 1.5 mm or less, the entire sheet is efficiently cooled in the casting process, so that the spherulites formed during casting can be refined. The thickness of the cast sheet can be adjusted by the screw rotation speed of the extruder, the slit gap of the die, the film production speed (the rotation speed of the casting drum), etc. The lower limit of the thickness of the cast sheet is preferably 1.0 mm, more preferably 1.1 mm.

[0072] The obtained laminated unstretched sheet is introduced into the longitudinal stretching step, in which the laminated unstretched sheet is first heated by contacting it with one or more metal rolls kept at a temperature of 80° C. to 130° C., preferably 90° C. to 130° C., and more preferably 100° C. to 130° C.

[0073] Then, in order to form a surface having fine irregularities while suppressing the formation of coarse irregularities, a stepwise preheating is performed with a metal roll immediately before the stretching section as described below. First, in the first preheating step, in order to form a more uniform structure, the film is brought into contact with a metal roll having a temperature of -20°C or more and -8°C or less from the melting point of the polypropylene resin used in the surface layer (I), preferably a temperature of -15°C or more and -10°C or less from the melting point of the polypropylene resin, to further promote the transition from β crystals to α crystals of the polypropylene resin. Furthermore, in the second preheating step, the film is brought into contact with a metal roll having a temperature of -15°C to -5°C in the first preheating step, more preferably a temperature of -10°C to -5°C in the first preheating step, to stabilize the transitioned crystal structure.

[0074] Next, in the stretching step, the laminated unstretched sheet is stretched in the longitudinal direction by 2.0 to 6.0 times, preferably 3.0 to 5.0 times, between rolls with a difference in peripheral speed, and cooled to room temperature to obtain a uniaxially stretched film (stretching in the longitudinal direction is sometimes called longitudinal stretching). In order to more uniformly stretch the polypropylene resin portion and the elastomer resin portion and form a fine protrusion structure, the longitudinal stretching temperature is equal to or higher than the softening temperature of the added elastomer, equal to or lower than the melting point of the polypropylene resin, and is from -10°C (temperature of the metal roll in the first preheating step) to -1°C (temperature of the metal roll in the first preheating step), and preferably equal to or lower than the melting point of the added elastomer, and is from -8°C (temperature of the metal roll in the first preheating step) to -3°C (temperature of the metal roll in the first preheating step).

[0075] Next, the uniaxially stretched film is guided to a tenter with both ends in the width direction held by clips, preheated, and then transversely stretched 7.0 to 12 times in the width direction. The preheating and stretching temperature is equal to or higher than the softening temperature of the elastomer resin to be added and equal to or lower than the melting point of the polypropylene resin to be added, from the viewpoint of uniformly stretching the film, forming a fine protrusion structure, and optimizing the crystallinity and orientation of the film. The lower limit of the preheating and stretching temperature is preferably the softening temperature of the elastomer resin to be added + 20°C, more preferably the softening temperature of the elastomer resin to be added + 30°C. The upper limit of the preheating and stretching temperature is preferably equal to or lower than the melting point of the polypropylene resin to be added and the melting point of the elastomer resin to be added, more preferably equal to or lower than the lower melting point of the polypropylene resin to be added and the elastomer resin to be added - 3°C. In this case, by making the difference between the preheating temperature and the stretching temperature within 6°C, preferably within 4°C, more preferably within 2°C, the stretching section is less susceptible to extreme temperature changes such as conveying flow. This enables uniform high-orientation stretching across the entire width of the film, improving the smoothness of the resulting biaxially oriented polypropylene film.

[0076] In the subsequent heat treatment and relaxation treatment steps, both widthwise ends of the biaxially stretched film are held taut with clips while being relaxed in the widthwise direction at a relaxation rate of 5.0 to 20%, more preferably 7.5 to 15%, and the film is heat-fixed at 140°C to 180°C, more preferably 150°C to 170°C, and while still held taut in the widthwise direction with clips, the film is passed through a cooling step at 80 to 100°C and then led to the outside of the tenter, the clips at the film ends are released, and the film edges are slit in the winding step, and the biaxially stretched polypropylene film product roll is wound up.

[0077] The biaxially oriented polypropylene film obtained in the above manner can be used for various industrial applications such as packaging films, cover films, processing films, sanitary products, agricultural products, construction products, and medical products. However, since it has excellent surface smoothness, handling properties, and blocking resistance, it is preferably used as a cover film, processing film, or release film.

[0078] Since the biaxially oriented polypropylene film of the present invention has excellent transparency, it can be particularly preferably used as a cover film for photocurable resins and dry photoresists. Here, the cover film refers to a film that is attached to an object such as a molded body or film and has the function of protecting the object from scratches, contamination, etc. that occur during processing or transportation.

[0079] A process film refers to a film used in the manufacturing process of an object such as a molded body or film. Examples of such films include those that are attached to an object during the manufacturing process to protect it from scratches and contamination, and those that function as a support when it is difficult to form a film from the object itself because it is thin or fragile.

[0080] A release film is a film that has high releasability and can be attached to objects such as molded bodies and films to protect them from scratches and contamination that occur during processing and transportation, and can be easily peeled off and discarded when used as a final product.

[0081] The laminate of the present invention will now be described.

[0082] The biaxially oriented polypropylene film of the present invention is excellent in smoothness and handleability, and therefore can be preferably used when forming a laminate with a metal film by subjecting the biaxially oriented polypropylene film of the present invention to sputtering or vapor deposition processing. That is, one embodiment of the laminate of the present invention is one in which a metal film or an electrolyte membrane is in contact with at least one surface of the biaxially oriented polypropylene film.

[0083] In sputtering and deposition, polyethylene terephthalate (PET) films, which have excellent surface smoothness, mechanical strength, heat resistance, and other properties, have often been used. However, PET has high hydrophilicity due to the presence of ester bonds, and PET films contain a small amount of moisture. Such a small amount of moisture can have an adverse effect during sputtering and deposition, and is particularly noticeable when metals belonging to Group 1 or 2 of the periodic table, which are easily reactive with moisture, or compounds containing these metals are deposited. In this context, the laminate of the present invention preferably contains a metal belonging to Group 1 or 2 of the periodic table, since a laminate can be obtained suitably even when the presence of a small amount of moisture makes it difficult to use a PET film. Here, the metal belonging to Group 1 or 2 refers to lithium, sodium, potassium, rubidium, cesium, francium, beryllium, magnesium, calcium, strontium, barium, and radium.

[0084] In addition, in a high-temperature environment, the moisture in the film evaporates as outgassing, and the effect is particularly noticeable under high vacuum conditions such as in a metal deposition process. When outgassing from the film, the degree of vacuum in the system deteriorates, and the quality of the metal film formed by deposition and the yield of deposition processing may decrease. From this perspective, the biaxially oriented polypropylene film of the present invention, which has a lower moisture content than PET film, can be suitably used in applications where a metal film is formed, and the laminate of the present invention can maintain good film quality of the metal film.

[0085] In addition, electrolyte membranes used in fuel cells, semi-solid batteries, all-solid batteries, etc. are usually produced in an environment where temperature and humidity are strictly controlled. In particular, since a sulfide-type electrolyte membrane reacts with moisture to generate hydrogen sulfide, the processing film used in its production is also required to have an extremely low moisture content. Therefore, the biaxially oriented polypropylene film of the present invention is preferably used as the processing film in the production of such electrolyte membranes. That is, a preferred embodiment of the laminate of the present invention includes one in which an electrolyte membrane is in contact with at least one side of a biaxially oriented polypropylene film, and further, it is particularly preferred that the electrolyte membrane is for a fuel cell, a semi-solid battery, or an all-solid battery.

[0086] From the above viewpoint, the upper limit of the moisture content of the biaxially stretched polypropylene film of the present invention is preferably 2000 ppm, more preferably 1000 ppm, further preferably 500 ppm, particularly preferably 200 ppm, and most preferably 100 ppm. The lower limit of the moisture content is not particularly limited, but is substantially 1 ppm. The moisture content of the biaxially stretched polypropylene film can be measured by the Karl Fischer method, the details of which will be described later.

[0087] In order to set the moisture content of the biaxially oriented polypropylene film of the present invention within the above range, it is preferable to minimize the content of hydrophilic resin in the biaxially oriented polypropylene film and to limit the amount of additives to the minimum necessary. Specifically, among all the components of the biaxially oriented polypropylene film of the present invention, the lower limit of the content of polyolefin resin such as polypropylene resin or propylene-based elastomer resin is preferably 90 mass%, more preferably 95 mass%, and even more preferably 97 mass%. The upper limit of the content of these resins is substantially 100%.

[0088] From the above viewpoint, the content of the antioxidant in all the components of the biaxially stretched polypropylene film of the present invention is preferably 500 to 9000 ppm, more preferably 1000 to 8000 ppm. In particular, since the phosphorus-based antioxidant that bleeds out to the surface may deteriorate the properties and quality of the metal film formed on the surface, it is preferable to control the content. More specifically, the content of the phosphorus-based antioxidant in all the components of the biaxially stretched polypropylene film of the present invention is preferably 100 ppm or less, more preferably 50 ppm or less, and even more preferably 10 ppm or less. There is no particular restriction on the lower limit of the content of the phosphorus-based antioxidant, and it is theoretically 0 ppm (same as not containing a phosphorus-based antioxidant). It is preferable that the content of the antioxidant including the phosphorus-based antioxidant is the same even when the film formed on the surface is not a metal film, from the viewpoint of properties, quality, and reduction of effect inhibition.

[0089] In order to reduce defects caused by bleed-out in the biaxially stretched polypropylene film of the present invention, the total content of additives other than the antioxidant (e.g., antistatic agent, viscosity modifier, color inhibitor, slip agent, etc.) is preferably 0 to 500 ppm or less.

[0090] The antioxidant preferably used in the biaxially stretched polypropylene film of the present invention is a sterically hindered phenol-based antioxidant, and at least one of them is preferably a high molecular weight type having a molecular weight of 500 or more. Specific examples include various types, and it is preferable to use 2,6-di-t-butyl-p-cresol (BHT: molecular weight 220.4) in combination with 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene (e.g., BASF's "Irganox" (registered trademark) 1330: molecular weight 775.2) or tetrakis[methylene-3(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane (e.g., BASF's "Irganox" (registered trademark) 1010: molecular weight 1177.7), etc.

[0091] As described above, the biaxially oriented polypropylene film of the present invention has an extremely low moisture content, generates very little outgassing, and is superior in smoothness and handling to existing olefin-based films, and is therefore preferably used when forming transparent conductive films that require stricter vacuum conditions or high quality. That is, a preferred embodiment of the laminate of the present invention includes a laminate in which a transparent conductive film is in contact with at least one side of the biaxially oriented polypropylene film of the present invention. The transparent conductive film here refers to a thin film formed of a material that is conductive and transmits visible light, and specific examples include indium-tin composite oxide (ITO), zinc oxide (ZnO), and palladium film.

[0092] Next, the current collector of the present invention will be described. The current collector of the present invention is made of the biaxially oriented polypropylene film of the present invention. The biaxially oriented polypropylene film of the present invention is preferably used as a current collector because of its excellent handling properties. The current collector is a foil-shaped laminate used for electrodes of storage batteries such as lithium ion batteries. Usually, metal foil is used as the current collector, but a laminate in which a metal film is laminated on a resin film as a base material is also used for the purpose of improving safety and reducing weight. This metal film is laminated by processing such as vapor deposition, sputtering, plating, and electroless plating. In addition, from the viewpoint of increasing the energy density of the battery, the film as the base material of the current collector is required to have a small thickness, but as the film becomes thinner, its stiffness decreases, and therefore the handling properties during processing are greatly reduced. In particular, in the process of laminating the metal film, high heat such as radiant heat is applied during processing, and tension is also applied in the conveying direction, so the film is required to have good handling properties. The biaxially oriented polypropylene film of the present invention is preferably used as a current collector because it can be made thin and has good handling properties.

[0093] Next, the storage battery of the present invention will be described. The storage battery of the present invention is made by using the biaxially oriented polypropylene film of the present invention. The biaxially oriented polypropylene film of the present invention is preferably used as a current collector because of its excellent handling properties, and is generally used in storage batteries in which the current collector is an electrode. A storage battery is a device that stores electrical energy and converts it back to electrical energy when needed. Specific examples include lead acid batteries, nickel-metal hydride batteries, lithium ion batteries, NAS batteries, and redox flow batteries. EXAMPLES

[0094] The present invention will be described in detail below with reference to examples. The properties were measured and evaluated by the following methods.

[0095] (1) Film thickness The thickness was measured using a micro thickness gauge (manufactured by MITUTOYO Co., Ltd.) A biaxially oriented polypropylene film was sampled in a 10 cm square area, and measurements were taken at any five points to calculate the average value.

[0096] (2) Cast sheet thickness The thickness was measured using a micro thickness gauge (manufactured by MITUTOYO Co., Ltd.) A 10 cm square sample was taken from the center of the cast sheet in the width direction, and measurements were taken at any five points to calculate the average value.

[0097] (3) Valley volume (Vvv), peak density (Spd) The measurements were performed using a scanning white light interference microscope "VS1540" (manufactured by Hitachi High-Tech Science Corporation; the measurement conditions and device configuration are described below), and measurements of 561.1 μm × 561.5 per field were performed by measuring multiple fields of view of 5 × 5 fields. Then, all images were stitched with a 20% overlap to obtain surface shape data of 2356.716 μm × 2358.294 μm. The captured image was complemented (fully complemented) using the attached analysis software, surface correction was performed using a polynomial 4th order approximation, and the surface shape was obtained by processing with a median filter (3 × 3 pixels). The measurements were performed on both the front and back surfaces of the biaxially oriented polypropylene film, and the intersection of the diagonals of the biaxially oriented polypropylene film cut into a 5 cm × 5 cm square shape was used as the starting point. A total of nine measurement positions were determined according to the following procedure, and measurements were performed at each measurement position. Vvv and Spd were obtained at each measurement position according to the above procedure, and the average values ​​were adopted as Vvv and Spd.

[0098] <How to determine the measurement position> Measurement 1: Starting point position Measurement 2: 5.0 mm to the right of the starting point Measurement 3: 10.0 mm to the right of the starting point Measurement 4: 5.0 mm below the starting point Measurement 5: 5.0mm below and 5.0mm to the right of the starting point Measurement 6: 5.0 mm below and 10.0 mm to the right of the starting point Measurement 7: 10.0 mm below the starting point Measurement 8: 10.0 mm below and 5.0 mm to the right of the starting point Measurement 9: 10.0 mm below and 10.0 mm to the right of the starting point <Measurement conditions and equipment configuration> Objective lens: 10x Optical tube: 1x Zoom lens: 1x Wavelength filter: 530nm white Measurement mode: Wave Measurement software: VS-Measure 10.0.4.0 Analysis software: VS-Viewer 10.0.3.0 Measurement area: 561.1μm×561.5μm Number of pixels: 1,024 x 1,024.

[0099] (4) Number of large dents with a major axis of 150 μm or more The measurements were performed using a scanning white light interference microscope "VS1540" (Hitachi High-Tech Science Corporation, measurement conditions and device configuration are described later), with measurements of 561.1 μm × 561.5 per field of view, and multiple field measurements of 5 × 5 fields of view were performed. All images were then stitched with a 20% overlap to obtain surface shape data of 2356.716 μm × 2358.294 μm. In the pore analysis of the particle analysis mode of the attached analysis software "VS-Viewer10.0.3.0", the height threshold was set to -0.1 μm to extract the dents, and the number of dents with a major axis of 150 nm or more was counted as large dents. Measurements were performed on both the front and back surfaces of the biaxially oriented polypropylene film. The intersection of the diagonal lines of the biaxially oriented polypropylene film cut into a 5 cm x 5 cm square was used as the starting point. A total of nine measurement positions were determined according to the following procedure, measurements were taken at each measurement position, and the number of measurements at each measurement position was calculated according to the above procedure. The average value was calculated for both sides A and B, and this value was divided by the measurement field area (2356.716 μm x 2358.294 μm) for 1 mm2 for both sides A and B. 2 The number of large dents with major diameters of 150 μm or more per unit area (pieces / mm 2 The method for determining the measurement position and the measurement conditions and device configuration are the same as those in the previous section (2).

[0100] (5) Melting point of resin 5 mg of the resin was collected as a sample in an aluminum pan and measured under a nitrogen atmosphere using a differential scanning calorimeter (Seiko Denshi Kogyo RDC220). First, the temperature was raised from 30°C to 260°C at 20°C / min, and then held at 260°C for 5 minutes. Then, the temperature was lowered from 260°C to 30°C at 20°C / min, and then the temperature was raised again from 30°C to 260°C at 20°C / min. The maximum peak temperature of the melting curve observed when the temperature was raised again from 30°C to 260°C at 20°C / min was taken as the melting point Tm (°C) of the resin.

[0101] (6) Crystallization half time Using a differential scanning calorimeter (Seiko Instruments EXSTAR DSC6220), 3 mg of biaxially stretched polypropylene film was heated from 25°C to 250°C at 20°C / min in a nitrogen atmosphere and held for 5 minutes. The temperature was then lowered from 250°C to 130°C at 20°C / min and held at 130°C for 30 minutes. The time when the sample temperature reached 130 was defined as 0 seconds, and the elapsed time from the peak appearing after 60 seconds for the endothermic curve obtained during isothermal holding at 130 was defined as the half crystallization time (seconds).

[0102] (7) Weight average molecular weight Mw The polypropylene resin pellets were dissolved in 1,2,4-trichlorobenzene by stirring at 165°C for 30 minutes. The mixture was then filtered using a 0.5μm filter, and the molecular weight distribution of the filtrate was measured. The weight average molecular weight Mw of the sample was calculated using a molecular weight calibration curve prepared using the following standard sample. Equipment: Agilent high temperature GPC PL-GPC220 Detector: Agilent refractive index detector (RI detector) Column: Agilent PL1110-6200 (20μm MIXED-A) x 2 ·Flow rate: 1.0mL / min Column temperature: 145℃ ·Injection volume: 0.500mL Sample concentration: 0.1wt% Standard samples: Monodisperse polystyrene manufactured by Tosoh, dibenzyl manufactured by Tokyo Kasei.

[0103] (8) Softening temperature The softening temperature of the elastomer resin was determined based on JIS K 7196 (1991) using the following equipment and conditions. Using a hydraulic hot press molding machine set at 190°C, the sample was preheated for 5 minutes, molded for 2 minutes under a pressure of 10 MPa, and then cooled at 20°C under a pressure of 10 MPa for 4 minutes to produce a sheet of a specified thickness, thereby obtaining a sheet sample. After leaving the sample at room temperature for 72 hours after molding, the sample was subjected to a thermomechanical analysis using a TMASS6100 thermomechanical analyzer (Hitachi High-Tech Science Corporation) at a pressure of 2 kg / cm on a 1 mm diameter probe. 2 The displacement (penetration depth) was measured when the specimen was heated at a temperature increase rate of 5°C / min while applying a pressure of 100 MPa. The temperature at which the displacement reached 500 µm was used as the softening temperature.

[0104] (9) Static friction coefficient μs Two samples were cut out into a rectangular shape with a width of 75 mm and a length of 100 mm, with the main orientation direction of the biaxially oriented polypropylene film as the long side, and then the two samples were conditioned for 24 hours under an atmosphere of 25°C and 65% RH. After conditioning, the two samples were arranged so that the outer surface and the inner surface of the roll were in contact with each other, and the resistance value when the sample started to slip was measured using a slip tester TR-2 manufactured by Toyo Seiki Co., Ltd. The resistance value when the sample started to slip was measured using a slip tester manufactured by Toyo Seiki Co., Ltd. in accordance with JIS K 7125 (1999). The measurement was performed in the main orientation orthogonal directions and with different surfaces overlapping each other, that is, with the surface of one film overlapping the back surface of the other film in contact with each other. The measurement was performed three times under the following conditions, and the static friction coefficient (μs) was calculated from the average value using the following formula, which was used as the static friction coefficient (μs). Sliding speed: 100mm / min Load: 200g Measurement environment: 25℃±2℃ 65RH%±5RH% Static friction coefficient (μs) = resistance value when the sample begins to slide / load.

[0105] (10)Ft The biaxially oriented polypropylene was cut into rectangular pieces of 150 mm long (measurement direction) × 10 mm wide, and five pieces were cut out to prepare samples (the measurement direction was selected arbitrarily, and the selected measurement direction was defined as the 0° direction). Then, using a tensile tester (Orientec's "Tensilon" (registered trademark) UCT-100), the samples were subjected to a tensile test at an initial tensile chuck distance of 50 mm and a tensile speed of 300 mm / min in an atmosphere of room temperature 23°C and relative humidity 65%. The load applied to the film when the sample was stretched by 5% (when the chuck distance became 52.5 mm) was read, and the value divided by the cross-sectional area (film thickness × width 10 mm) before the test was taken as the initial tensile strength. Then, the initial tensile strength was measured in each direction at an angle of 0° to 175° at 5° intervals with respect to the measurement direction in the film plane, and the direction showing the highest value was taken as the main orientation direction of the film. Furthermore, the product of the initial tensile strength and the film thickness in the direction perpendicular to the main orientation direction of the film was calculated. The test was performed five times, and the arithmetic average value of the product of the initial tensile strength and the film thickness in the direction perpendicular to the main orientation direction of the film was calculated and designated as Ft.

[0106] (11) Melting point and heat of fusion ratio below 160°C 5 mg of biaxially oriented polypropylene film was placed in an aluminum pan as a sample and measured using a differential scanning calorimeter (Seiko Denshi Kogyo RDC220). For the melting curve observed when the temperature was raised from 30°C to 260°C at 20°C / min (first run) under a nitrogen atmosphere, the peak temperature was taken as the melting point Tm (°C) of the biaxially oriented polypropylene film, the heat flow rate at each temperature was corrected with a straight line that was the baseline from 60°C to 250°C, and the heat of fusion ratio below 150°C was calculated by subtracting the heat of fusion from 60°C to 250°C from the heat of fusion from 60°C to 150°C.

[0107] (12) Hayes The haze value (%) of the biaxially stretched polypropylene film was measured three times at 23° C. using a haze meter (NDH-5000, manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K 7136 (2000), and the average value was used.

[0108] (13) Blocking resistance The biaxially oriented polypropylene film was cut to a size of 60 mm x 210 mm, and 5 sheets were stacked so that the A and B sides of the film were in contact with each other, and a load of 1 kg was applied and heated in an oven set at 120°C for 15 minutes. After removing from the oven, it was left to stand and gradually cooled to room temperature. The laminated biaxially oriented polypropylene film was then peeled off and evaluated according to the following criteria. A and B were considered to be acceptable, and C was considered to be unacceptable. A: The films did not adhere to each other. B: The films were in close contact with each other, but could be peeled off without rupturing. C: Impossible to peel off, or the film broke during peeling.

[0109] (14) Handling Based on the results of Ft and the static friction coefficient μs described above, the following scores were assigned and applied to the following formula to evaluate the handling properties. In the evaluation, A to C were considered to be pass, and D was considered to be fail. (Ft score) 2 points: 700 Pa m or more and less than 2000 Pa m 1 point: 300 Pa·m or more but less than 700 Pa·m, 2000 Pa·m or more but less than 3000 Pa·m 0 points: less than 300 Pa·m, more than 3000 Pa·m (Static friction coefficient μs score) 3 points: less than 0.8 2 points: 0.8 or more and less than 1.0 1 point: 1.0 or more and less than 1.3 0 points: 1.3 or higher (Handling (Ft score x static friction coefficient score)) 6 points: A 3~4 points:B 1~2 points:C 0 points:D.

[0110] (15) Quality evaluation as a cover film On the A side of the film cut to 21 cm x 30 cm, a coating agent consisting of a resin composition obtained by mixing 50 parts by mass of commercially available urethane acrylate (viscosity at 25 ° C: 600,000 mPa s, weight average molecular weight Mw: 1600, glass transition temperature 10 ° C), 50 parts by mass of commercially available methyl ethyl ketone, and 3 parts by mass of commercially available 1-hydroxycyclohexyl phenyl ketone was applied to a film thickness of 45 μm. This was introduced into a hot air dryer and heated at 80 ° C to remove the solvent. Next, ultraviolet rays were irradiated using a UV lamp under a nitrogen atmosphere to harden the coating agent on the film, and then the film was left to stand at room temperature for 24 h. Thereafter, the appearance was confirmed, and the resin composition layer was peeled off to obtain a resin composition film consisting of polyurethane acrylate. Thereafter, using a surface roughness measuring instrument (MITUTOYO: SJ-210), the Ra of the peeled surface of the resin composition film was measured in the same direction as the direction perpendicular to the main orientation axis of the film in the film plane based on JIS B 0601 (2001). The same measurement was performed a total of five times, and the average value of the obtained values ​​was taken as the Ra of the resin composition film. The appearance and roughness were evaluated according to the following criteria. Appearance: Before peeling, the specimen was visually inspected and the appearance was evaluated according to the following criteria, with A to C being acceptable and D being unacceptable. A: 1 visible uneven defect / cm 2 The results were below the expected level and transparent. B: 1 visible defect / cm 2 More than 5 pieces / cm 2 Although the surface was less than 100% clear or slightly cloudy, it was easy to visually distinguish uneven defects. C: 5 visible defects / cm 2 More than 10 pieces / cm 2 Although the defect was less than 10 mm or cloudy, it was possible to visually distinguish the unevenness defects. D: 10 visually noticeable defects / cm 2 Or, since strong white turbidity was observed, it was difficult to visually distinguish uneven defects. Roughness: Using a simple roughness meter, Ra was measured five times and the average value was used as Ra. The roughness quality was evaluated according to the following criteria, with A to C being acceptable and D being unacceptable. A:Ra≦50nm B: 50 nm <Ra≦75nm C: 75 nm <Ra≦100nm D:100 <Ra。

[0111] (16) Yield evaluation during metal film formation Using a vacuum deposition device, the pressure is reduced from atmospheric pressure to 1×10 -5 The pressure was reduced to 100 MPa, and a magnesium film with a thickness of 200 Å was formed on one side of a biaxially oriented polypropylene film or a PET film by vacuum deposition using magnesium as a deposition source. -5 The time it took to reduce the pressure to the full was measured, and the unevenness of the metal film surface was visually observed to evaluate the yield according to the following criteria, where A was considered pass and B was considered fail. A: 1×10 above atmospheric pressure -5 The time to reduce pressure to the bottom was less than 50 minutes, and the metal film surface did not appear smooth. B: 1×10 above atmospheric pressure -5 The time to reduce the pressure to the bottom was longer than 50 minutes, or irregularities were observed on the metal film surface.

[0112] (17) Moisture content A biaxially oriented polypropylene film or PET film sample was left in a room conditioned at 23°C and 20% relative humidity for at least 4 hours, and then immersed in distilled water at 23°C for 24 hours. After that, the moisture on the sample surface was wiped off, and the moisture in the sample was dried and evaporated at a temperature of 150°C using a trace moisture meter (Mitsubishi Chemical Corporation, CA-20 model), and the moisture amount was quantified by the Karl Fischer method to calculate the moisture content.

[0113] (Polypropylene resin, etc.) The raw materials used for the biaxially oriented polypropylene in the examples and comparative examples and their properties are shown in Tables 1 to 3 below. These property values ​​are values ​​evaluated in the form of resin pellets. Six types of polypropylene raw materials (PP1 to PP6) and four types of elastomer resins (ELA1 to ELA4) were prepared. In addition, three types of polypropylene resin pellets (PP7 to PP9) were prepared by pre-kneading with the composition in Table 2. All of PP1 to PP9 contain BASF's "Irganox" (registered trademark) 1010 as an antioxidant in the range of 1000 ppm to 5000 ppm, and only PP8 further contains BASF's "Irgafos" (registered trademark) 168 at 3000 ppm. Polypropylene resin 1 (PP1): Prime Polymer Polypropylene resin 2 (PP2): Borealis Polypropylene resin 3 (PP3): Prime Polymer Branched chain polypropylene resin 4 (PP4): Japan Polypropylene Corporation Polypropylene resin 5 (PP5): Idemitsu Kosan Co., Ltd. Polypropylene resin 6 (PP6): Prime Polymer

[0114] [Table 1]

[0115] Elastomer resin 1 (ELA1): "Toughmer" (registered trademark) "PN2060" (propylene-based elastomer), manufactured by Mitsui Chemicals, Inc. Elastomer resin 2 (ELA2): Mitsui Chemicals, Inc., "Toughmer" (registered trademark) "BL3450" (butene-based elastomer) Elastomer resin 3 (ELA3): "Toughmer" (registered trademark) "PN2070" (propylene-based elastomer), manufactured by Mitsui Chemicals, Inc. Elastomer resin 4 (ELA4): Mitsubishi Chemical Corporation, "Wellnex" (registered trademark) "RFX4V" (propylene-based elastomer)

[0116] [Table 2]

[0117] Polypropylene resin 7 (PP7): Mixed polypropylene resin pellets made by mixing PP1 and PP4 in the mass ratio shown in Table 3 Polypropylene resin 8 (PP8): Mixed polypropylene resin pellets made by mixing PP1 and PP5 in the mass ratio shown in Table 3 Polypropylene resin 9 (PP9): Mixed polypropylene resin pellets made by mixing PP6, PP5, PP4, and ELA4 in the mass ratios shown in Table 3.

[0118] [Table 3]

[0119] Example 1 Polypropylene resin 1 (PP1) and elastomer resin 1 (ELA1) were dry blended at a ratio of 70:30 (mass ratio) to obtain a resin composition. The obtained dry blend of the resin composition was fed from a hopper into a twin-screw extruder and melt-mixed at a maximum temperature of 250°C. Resin strands were then generated, and pellets were continuously produced using a strand cutter after water cooling to obtain pellets of the melt-blended resin composition. As a raw material for the surface layer (I), this resin composition was fed to a single-screw extruder with a single screw for the surface layer (I). As a raw material for the base layer (II), PP1 was fed to a single-screw extruder with a single screw for the base layer (II). The resin or resin mixture for each layer was melt-extruded at 245°C, and after removing foreign matter with a sintered filter with a cut of 20μm, the layers were laminated in a feed block type A / B / A composite T die so that the thickness ratio of the surface layer (I) / base layer (II) / surface layer (I) was 1 / 30 / 1, and the layers were discharged onto a casting drum with a surface temperature controlled at 20°C and adhered to the casting drum by an air knife. Thereafter, compressed air at 15°C was blown out by an air knife onto the non-cooled drum surface of the sheet on the casting drum at an air speed of 140m / s to cool the sheet, thereby obtaining an unstretched sheet. The unstretched sheet was then brought into contact with a metal roll heated to 125°C. The unstretched sheet was then preheated by contacting it with a metal roll heated to 148°C as a preheating 1 step, and then by contacting it with a metal roll heated to 140°C as a preheating 2 step. Then, in the stretching step, the film was brought into contact with a metal roll heated to 144 ° C., and stretched 4.5 times in the longitudinal direction between the next metal rolls with a difference in peripheral speed. Next, the obtained uniaxially stretched film was introduced into a tenter-type stretching machine with both ends in the width direction held by clips, preheated at 158 ​​° C. for 1 second, stretched 8.5 times in the width direction at 156 ° C., and heat-treated at 155 ° C. while giving 7.5% relaxation in the width direction. After that, it was guided to the outside of the tenter through a cooling step at 100 ° C., the clips at both ends in the width direction of the film were released, and it was wound around a core to obtain a biaxially stretched polypropylene film with a thickness of 25 μm. The physical properties and evaluation results of the obtained film are shown in Table 4.

[0120] (Examples 2 to 6, Comparative Examples 1 to 5) A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that the raw material composition of each layer and the film-forming conditions were as shown in Table 4. At this time, the thickness was adjusted by adjusting the discharge amount during extrusion and the speed of the casting drum. The physical properties and evaluation results of the obtained biaxially oriented polypropylene film are shown in Table 4.

[0121] Comparative Example 6 The raw material composition and film-forming conditions of each layer are as shown in Table 4. In the longitudinal stretching step, the unstretched sheet was preheated to 90°C with a ceramic roll, and the initial stretching was performed in the longitudinal direction between rolls at 90°C with a peripheral speed difference of 1.3 times. Then, the film after the initial stretching was preheated to 140°C, and the second stage of longitudinal stretching was performed at a ratio of 3.5 times. Except for this, a biaxially stretched polypropylene film was obtained in the same manner as in Example 1. At this time, the thickness was adjusted by adjusting the discharge amount during extrusion and the speed of the casting drum. The physical properties and evaluation results of the obtained biaxially stretched polypropylene film are shown in Table 4.

[0122] Comparative Example 7 Instead of the biaxially oriented polypropylene film, a PET film "Lumirror" (registered trademark) S10 (manufactured by Toray Industries, Inc.) was used to evaluate the quality and the yield during metal film formation, and the moisture content was measured. The evaluation results are shown in Table 4.

[0123] [Table 4]

[0124] In Table 4, the stretching ratio in the longitudinal direction is shown multiplied by two stretchings (the temperature in the first stretching is 90° C., and the temperature in the second stretching is 140° C.). Note that the moisture content and the yield in the production of the metal film were evaluated only for Example 1 and Comparative Examples 3 and 7. [Industrial Applicability]

[0125] As described above, the biaxially oriented polypropylene film of the present invention can be used for various industrial applications such as packaging films, surface protection films, process films, sanitary products, agricultural products, construction products, and medical products. In particular, since it has excellent surface smoothness and transparency, it can be preferably used as a cover film for photocurable resins and a cover film for dry film resists. [Explanation of symbols]

[0126] 1: Load curve with height on the vertical axis and load area ratio on the horizontal axis 2: Valley volume Vvv 3: Equivalent line at area load ratio of 80% 4: Linear position of 100% areal load ratio

Claims

1. The lower surface of the valley volume Vvv is surface A, and Vvv of surface A is Vvv A , the peak density Spd of the A side is Spd A When the above Vvv A is 1.0 μL / m 2 ≦Vvv A ≦20 μL / m 2 and the Spd A 1.0 pieces / mm 2 ≦Spd A ≦100 pieces / mm 2 A biaxially oriented polypropylene film,

2. When the surface opposite to the surface A is surface B, the surface A and the surface B are 2 The number of large dents exceeding 150 μm in major axis per mm 2 More than 10 pieces / mm 2 2. The biaxially oriented polypropylene film according to claim 1, wherein:

3. The surface opposite to the surface A is surface B, and the Vvv of the surface B is Vvv B When set at 5.0 μL / m 2 ≦Vvv A +Vvv B ≦25 μL / m 2 , and 0.10≦Vvv A / Vvv B 3. The biaxially oriented polypropylene film according to claim 1, wherein the elastic modulus is ≦0.

70.

4. 3. The biaxially oriented polypropylene film according to claim 1, wherein Ft, which is the product of the initial tensile strength and the film thickness in the direction perpendicular to the main orientation direction of the film, is 300 Pa·m or more and 3000 Pa·m or less.

5. The biaxially oriented polypropylene film according to claim 1 or 2, having a thickness of 10 μm or more and 100 μm or less.

6. 3. The biaxially oriented polypropylene film according to claim 1 or 2, having a haze of 0.1% or more and 5.0% or less.

7. The biaxially oriented polypropylene film according to claim 1 or 2, wherein the static friction coefficient μs between the A side and the B side is 0.1 or more and less than 1.

3.

8. 3. The biaxially oriented polypropylene film according to claim 1 or 2, which has a peak temperature of 165°C or more and 180°C or less in a melting curve obtained when the film is heated from 30°C to 260°C using a differential scanning calorimeter (DSC).

9. 3. The biaxially oriented polypropylene film according to claim 1 or 2, wherein the heat of fusion at 160°C or less is 5% to 50% of the total heat of fusion when heated from 30°C to 260°C using a differential scanning calorimeter DSC.

10. The biaxially oriented polypropylene film according to claim 1 or 2, which is composed of at least two layers.

11. 3. The biaxially oriented polypropylene film according to claim 1 or 2, wherein a layer containing 50% by mass or more and 90% by mass or less of polypropylene having a melting point of 160°C or more and 10% by mass or more and 50% by mass or less of an olefin-based elastomer having a melting point of 140°C or more is located on at least one outermost surface.

12. A release film comprising the biaxially oriented polypropylene film according to claim 1 or 2.

13. A cover film for photocurable resin, comprising the biaxially oriented polypropylene film according to claim 1 or 2.

14. A cover film for a dry film resist, comprising the biaxially oriented polypropylene film according to claim 1 or 2.

15. A processing film comprising the biaxially oriented polypropylene film according to claim 1 or 2.

16. A laminate comprising the biaxially oriented polypropylene film according to claim 1 or 2 and a metal film in contact with at least one surface of the film.

17. 17. The laminate of claim 16, wherein the metal film comprises a metal from Group 1 or 2 of the periodic table.

18. A laminate comprising the biaxially oriented polypropylene film according to claim 1 or 2 and a transparent conductive film in contact with at least one surface of the biaxially oriented polypropylene film.

19. A laminate comprising the biaxially oriented polypropylene film according to claim 1 or 2 and an electrolyte membrane in contact with at least one surface of the film.

20. 20. The laminate according to claim 19, wherein the electrolyte membrane is for a fuel cell, a semi-solid battery, or an all-solid battery.

21. A current collector comprising the biaxially oriented polypropylene film according to claim 1 or 2.

22. A storage battery comprising the biaxially oriented polypropylene film according to claim 1 or 2.

Citation Information

Patent Citations

  • Biaxially oriented polypropylene film

    JP2015107612A

  • Biaxially oriented polypropylene film

    JP2017035884A

  • Polypropylene film, metal layer-integrated polypropylene film, film capacitor and film roll

    JP2020100800A

  • Film, layered product, and method for producing resin composition film

    WO2022075101A1

Cited By

  • Easy-to-peel tape, wound body, and packaging bag for heating