Trans fer device, and image formation device
The use of a resin-based endless belt with conductive carbon particles and specific silicone oil in image forming devices addresses the ghost phenomenon by minimizing charge conduction and toner scattering, improving the transfer process.
Patent Information
- Application Number
- JP2024020409
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-02-14
- Publication Date
- 2024-10-11
AI Technical Summary
In image forming devices using electrophotography, the transfer of toner images from an image carrier to a recording medium is hindered by the ghost phenomenon, where toner images shift due to creeping conduction of charges on the outer circumferential surface of an endless belt, caused by the use of a metal primary transfer roll with high conductivity, leading to diagonal electric fields and toner scattering.
The use of an endless belt with a resin containing conductive carbon particles and specific silicone oil, where the spatial distribution of carbon particles is finely dispersed, reducing creeping conduction and maintaining a non-electrostatic adhesion force, thereby suppressing the ghost phenomenon.
The proposed solution effectively suppresses the ghost phenomenon by ensuring that the integral value of the statistic L(r) in the spatial distribution of conductive carbon particles is within a specific range, enhancing the transfer process and reducing toner scattering.
Smart Images

Figure 2024144141000016 
Figure 2024144141000001 
Figure 2024144141000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a transfer device and an image forming apparatus. [Background technology]
[0002] In an image forming apparatus (such as a copier, a facsimile, or a printer) using an electrophotographic method, a toner image formed on the surface of an image carrier is transferred to the surface of a recording medium and fixed on the recording medium to form an image. Note that, for example, a transfer device equipped with a conductive endless belt such as an intermediate transfer belt is used to transfer such a toner image to the recording medium.
[0003] For example, Patent Document 1 discloses a printer that includes an image carrier, a developing device, an intermediate transfer body, and a secondary transfer device, and the intermediate transfer body is made of a multi-layer structure having a base material and a surface layer. The base material is made of a resin material having a conductive agent dispersed therein, and the surface layer is made of a resin material having a conductive agent and a hydrophobic inorganic material having an average particle diameter of 1 μm or less dispersed therein, and the volume resistivity of the surface layer is 10 9.5 Ωcm to 10 13 Imaging devices are disclosed that are characterized by a resistivity in the Ωcm range.
[0004] Patent Document 2 discloses an image forming apparatus comprising an image carrier, an intermediate transfer belt, and a secondary transfer roll, in which the secondary transfer roll and the intermediate transfer belt are arranged in pressure-contact with each other, and the outer peripheral surface of the intermediate transfer belt is in contact with the secondary transfer roll along the outer shape thereof. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 11-202648 [Patent Document 2] JP 2006-243031 A Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, due to the demand for low costs, there has been a demand to use a metallic primary transfer roll that contacts the inner surface of an endless belt to apply an electric field to the endless belt as a primary transfer member for primarily transferring a toner image formed on the surface of an image carrier to an intermediate transfer body consisting of an endless belt. However, in a transfer device having an intermediate transfer body made of an endless belt and a primary transfer device and a secondary transfer device having a metallic primary transfer roll, the metallic primary transfer roll is a rigid body and has high conductivity, so that electric charges are easily conducted along the axial direction of the primary transfer roll on the outer peripheral surface of the endless belt, and an electric field is applied obliquely between the endless belt and the image carrier, and the toner image is displaced from the transfer position, causing toner scattering, which tends to cause a phenomenon in which an afterimage appears in an area where an image is not supposed to be formed (hereinafter also referred to as a "ghost phenomenon").
[0007] The object of the present invention is to provide a transfer device having an intermediate transfer body consisting of an endless belt and a primary transfer device and a secondary transfer device having a metallic primary transfer roll, wherein the endless belt is made of a layer containing resin and conductive carbon particles or has said layer as the outermost layer, in which the ghost phenomenon caused by the surface conduction of charge on the outer peripheral surface of the endless belt is suppressed compared to when the layer does not contain silicone oil, when the layer contains only fluorine-modified silicone oil as the silicone oil, or when the integral value of the statistic L(r) expressed by the following formula (1) when the inter-particle distance r is 0.05 μm or more and 0.30 μm or less in the spatial distribution of the conductive carbon particles present in an evaluation area of 6.3 μm × 4.2 μm on the outer peripheral surface of the endless belt exceeds 0.1. [Means for solving the problem]
[0008] The above problems are solved by the following means. <1> an endless belt comprising a layer containing at least one resin selected from the group consisting of polyimide resin, polyamideimide resin, aromatic polyetheretherketone resin, polyphenylene sulfide resin, and polyetherimide resin, conductive carbon particles, and a silicone oil containing at least one resin selected from the group consisting of dimethylpolysiloxane and an organic group-substituted product of dimethylpolysiloxane, or having said layer as an outermost layer, said endless belt having said layer as an outermost layer, wherein in a spatial distribution of the conductive carbon particles present in an evaluation area of 6.3 μm×4.2 μm on the outer circumferential surface of said endless belt, an integral value of a statistic L(r) expressed by the following formula (1) when the inter-particle distance r is 0.05 μm or more and 0.30 μm or less is 0 or more and 0.1 or less; a primary transfer device having a metallic primary transfer roll that is in contact with an inner peripheral surface of the intermediate transfer body and applies an electric field to the intermediate transfer body, and that performs primary transfer of a toner image formed on a surface of an image carrier onto an outer peripheral surface of the intermediate transfer body; a secondary transfer device that secondarily transfers the toner image transferred onto the outer peripheral surface of the intermediate transfer body onto a surface of a recording medium; A transfer device comprising:
[0009]
number
[0010] [In the formula (1), r represents the interparticle distance, and K(r) represents Ripley's K function K(r) represented by the following formula (2)]
[0011]
number
[0012] [In the above formula (2), 1(|X i -X j |≦r) indicates the indicator function, and X i and X j indicate the coordinates of point i and point j, respectively, and |X i -X j | is the coordinate X i and coordinate Xj represents the Euclidean distance between the particles, r represents the interparticle distance, and s(|X i -X j |) indicates the edge correction coefficient s(x) of the evaluation area expressed by the following formula (3), and x = |X i -X j |, where N indicates the total number of particles in the evaluation area, and λ indicates the number density of particles in the evaluation area.
[0013]
number
[0014] [In the formula (3), L x and L y are the lengths (μm) of the sides of the evaluation area in the x-axis and y-axis directions, respectively, and x = |X i -X j | and X i and X j indicate the coordinates of point i and point j, respectively, and |X i -X j | is the coordinate X i and coordinate X j This shows the Euclidean distance between
[0015] <2> The silicone oil includes a modified silicone oil having, as an organic group substitutent of the dimethylpolysiloxane, at least one selected from the group consisting of an organic group having a polyether structure and an aralkyl group. <1> The transfer device according to claim 1 . <3> The silicone oil contains at least one selected from the group consisting of polyether-modified silicone oils and aralkyl-modified silicone oils as an organic group substitute of the dimethylpolysiloxane. <1> or <2> The transfer device according to claim 1 . <4> The silicone oil contains a polyether-modified silicone oil as an organic group substitute of the dimethylpolysiloxane. <1> ~ <3> 13. A transfer device according to any one of claims 1 to 12. <5> The silicone oil contains an aralkyl-modified silicone oil as an organic group substitute of the dimethylpolysiloxane. <1> ~ <3> 13. A transfer device according to any one of claims 1 to 12. <6> The content of the silicone oil is 0.5% by mass or more and 7% by mass or less with respect to the entire layer. <1> ~ <5> 13. A transfer device according to any one of claims 1 to 12. <7> The content of the silicone oil is 0.5% by mass or more and 6% by mass or less with respect to the entire layer. <1> ~ <6> 13. A transfer device according to any one of claims 1 to 12. <8> The content of the silicone oil is 1% by mass or more and 3% by mass or less with respect to the entire layer. <1> ~ <7> 13. A transfer device according to any one of claims 1 to 12. <9> The resin includes an imide resin. <1> ~ <8> 13. A transfer device according to any one of claims 1 to 12. <10> The imide-based resin includes a polyimide resin. <9> The transfer device according to claim 1 .
[0016] <11> the silicone oil contains at least one selected from the group consisting of polyether-modified silicone oil and aralkyl-modified silicone oil as an organic group substitute of the dimethylpolysiloxane, and the resin contains an imide-based resin; <1> The transfer device according to claim 1 . <12> The imide-based resin includes a polyimide resin. <11> The transfer device according to claim 1 .
[0017] <13> An image carrier; a charging device for charging the surface of the image carrier; an electrostatic latent image forming device for forming an electrostatic latent image on a charged surface of the image carrier; a developing device that contains a developer containing a toner and develops an electrostatic latent image formed on the surface of the image carrier with the developer to form a toner image; The toner image is transferred onto a surface of a recording medium. <1> ~ <12> A transfer device according to any one of the above items, An image forming apparatus comprising: Effect of the Invention
[0018] <1> According to the invention, there is provided a transfer device having an intermediate transfer body consisting of an endless belt and a primary transfer device and a secondary transfer device having a metallic primary transfer roll, wherein the endless belt is made of a layer containing resin and conductive carbon particles or has said layer as the outermost layer, in which the ghost phenomenon caused by the surface conduction of charge on the outer peripheral surface of the endless belt is suppressed compared to when the layer does not contain silicone oil, when the layer contains only fluorine-modified silicone oil as the silicone oil, or when the integral value of the statistic L(r) expressed by the following formula (1) when the inter-particle distance r is 0.05 μm or more and 0.30 μm or less exceeds 0.1 in the spatial distribution of the conductive carbon particles present in an evaluation area of 6.3 μm × 4.2 μm on the outer peripheral surface of the endless belt is greater than 0.1.
[0019] <2> , <3> , <4> or <5> According to the present invention, a transfer device is provided in which the ghost phenomenon is kept suppressed as compared to when the silicone oil is made of dimethylpolysiloxane. <6> or <7> According to the present invention, a transfer device is provided in which the ghost phenomenon is suppressed compared to when the silicone oil content is less than 0.5 mass %. <8> According to the invention, a transfer device is provided in which the ghost phenomenon is suppressed compared to when the silicone oil content is less than 1 mass %. <9> or <10> According to the present invention, a transfer device is provided in which the ghost phenomenon is kept suppressed as compared to when the resin is made of an aromatic polyether ether ketone resin.
[0020] <11> or <12> According to the present invention, a transfer device is provided in which the ghost phenomenon is maintained in a suppressed state compared to when the silicone oil is made of dimethylpolysiloxane or when the resin is made of aromatic polyether ether ketone resin.
[0021] <13> According to the invention, there is provided an image forming apparatus having a primary transfer device and a secondary transfer device having an intermediate transfer body made of an endless belt and a primary transfer roll made of metal, and the transfer device is made of a layer containing resin and conductive carbon particles or has said layer as the outermost layer, in which the ghost phenomenon caused by the surface conduction of charge on the outer peripheral surface of the endless belt is suppressed compared to a transfer device in which the layer does not contain silicone oil, a transfer device in which the layer contains only fluorine-modified silicone oil as the silicone oil, or a transfer device in which the integral value of the statistic L(r) expressed by the following formula (1) when the inter-particle distance r is 0.05 μm or more and 0.30 μm or less exceeds 0.1 in the spatial distribution of the conductive carbon particles present in an evaluation area of 6.3 μm × 4.2 μm on the outer peripheral surface of the endless belt is greater than 0.1. [Brief description of the drawings]
[0022] [Figure 1] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The present embodiment will be described below. The description and examples are merely illustrative of the embodiment, and are not intended to limit the scope of the embodiment.
[0024] In the numerical ranges described in the present embodiment, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range described in the present embodiment. In addition, in the numerical ranges described in the present embodiment, the upper or lower limit of the numerical range may be replaced with a value shown in the examples. In this embodiment, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved. When the embodiment is described with reference to the drawings, the configuration of the embodiment is not limited to the configuration shown in the drawings. Furthermore, the size of the members in each drawing is conceptual, and the relative relationship between the sizes of the members is not limited to this. In this embodiment, each component may contain multiple types of corresponding substances. When referring to the amount of each component in the composition in this embodiment, if multiple substances corresponding to each component are present in the composition, the amount refers to the total amount of the multiple substances present in the composition, unless otherwise specified.
[0025] [Transfer device] The transfer device according to the present embodiment is an endless belt that is made of a layer containing at least one resin selected from the group consisting of polyimide resin, polyamideimide resin, aromatic polyetheretherketone resin, polyphenylene sulfide resin, and polyetherimide resin, conductive carbon particles, and a silicone oil containing at least one selected from the group consisting of dimethylpolysiloxane and an organic group-substituted product of dimethylpolysiloxane, or has the layer as the outermost layer, and the outermost layer is a 6.3 μm×4.2 μm evaluation area on the outer circumferential surface of the endless belt. the conductive carbon particles existing in a valence region have an integral value of a statistic L(r) expressed by the following formula (1) that is 0 or more and 0.1 or less when the interparticle distance r is 0.05 μm or more and 0.30 μm or less; a primary transfer device that has a metallic primary transfer roll in contact with the inner peripheral surface of the intermediate transfer body and applies an electric field to the intermediate transfer body, and that performs primary transfer of a toner image formed on the surface of an image carrier onto the outer peripheral surface of the intermediate transfer body; and a secondary transfer device that performs secondary transfer of the toner image transferred to the outer peripheral surface of the intermediate transfer body onto a surface of a recording medium.
[0026]
number
[0027] [In the formula (1), r represents the interparticle distance, and K(r) represents Ripley's K function K(r) represented by the following formula (2)]
[0028]
number
[0029] [In the above formula (2), 1(|X i -X j |≦r) indicates the indicator function, and X i and X j indicate the coordinates of point i and point j, respectively, and |X i -X j | is the coordinate X i and coordinate X j represents the Euclidean distance between the particles, r represents the interparticle distance, and s(|X i -X j |) indicates the edge correction coefficient s(x) of the evaluation area expressed by the following formula (3), and x = |X i -X j |, where N indicates the total number of particles in the evaluation area, and λ indicates the number density of particles in the evaluation area.
[0030]
number
[0031] [In the formula (3), L x and L y are the lengths (μm) of the sides of the evaluation area in the x-axis and y-axis directions, respectively, and x = |X i -X j | and X i and X j indicate the coordinates of point i and point j, respectively, and |X i -X j | is the coordinate X i and coordinate X j This shows the Euclidean distance between
[0032] Hereinafter, a resin including at least one selected from the group consisting of polyimide resin, polyamideimide resin, aromatic polyether ether ketone resin, polyphenylene sulfide resin, and polyetherimide resin will also be referred to as a "first resin". In addition, at least one selected from the group consisting of dimethylpolysiloxane and organic group-substituted dimethylpolysiloxane is also referred to as a "specific silicone oil". The layer that constitutes the outer peripheral surface of the endless belt is also called the "outer peripheral layer." In addition, in the spatial distribution of conductive carbon particles present in an evaluation area of 6.3 μm × 4.2 μm on the outer peripheral surface of the endless belt, the integral value of the statistic L(r) expressed by equation (1) when the inter-particle distance r is 0.05 μm or more and 0.30 μm or less is also referred to as the "L(r) integral value." In addition, "electrical conductivity" means that the volume resistivity at 20℃ is 1×10 13 This means that the resistance is less than Ωcm.
[0033] In a transfer device having an intermediate transfer body consisting of an endless belt, a primary transfer device having a metallic primary transfer roll, and a secondary transfer device, as described above, the metallic primary transfer roll is rigid and highly conductive, making the ghost phenomenon prone to occur. Specifically, since the metal primary transfer roll is a rigid body, the circumferential width of the region where the intermediate transfer body is sandwiched between the image carrier and the primary transfer roll (hereinafter also referred to as the "nip region") is narrowed. Then, the endless belt comes into contact with the highly conductive primary transfer roll in the narrow circumferential nip region, so that the electric charge is easily conducted along the surface of the outer circumferential surface of the endless belt in the axial direction of the primary transfer roll. When the electric charge is conducted along the surface, the electric field between the endless belt and the image carrier is applied obliquely, and the toner image may be shifted from the transfer position. At this time, if the circumferential width of the nip region is narrow, the time for the endless belt to pass through the nip region is shortened, so that the toner is easily scattered, and the ghost phenomenon caused by the toner scattering is easily generated. In particular, when a second toner image formed on a second image carrier is superimposed on a first toner image that has been primarily transferred onto the outer peripheral surface of the endless belt, the electric field between the endless belt and the second image carrier is more likely to be applied at an angle due to the influence of the charge held by the first toner image on the endless belt, which can result in a noticeable ghost phenomenon.
[0034] In contrast, in the present embodiment, the outer peripheral layer contains a specific silicone oil, and the L(r) integral value in the outer peripheral layer is 0 or more and 0.1 or less, thereby suppressing the ghost phenomenon. The reason for this is unclear, but is presumed to be as follows. The L(r) integral value in the outer layer is 0 or more and 0.1 or less, which means that conductive carbon particles are finely dispersed on the outer peripheral surface of the endless belt. Therefore, the conductive carbon particles finely dispersed on the outer peripheral surface of the endless belt disperse the electric current, so that even if the metal primary transfer roll contacts the inner peripheral surface of the endless belt, the creeping conduction in the axial direction of the primary transfer roll is suppressed. In addition, it is presumed that the specific silicone oil is contained in the outer peripheral layer of the endless belt, so that the non-electrostatic adhesion force on the outer peripheral surface is reduced, and even if the toner scatters and adheres to the area where the image is not originally formed, it is easy to peel off, and the ghost phenomenon is suppressed.
[0035] [Intermediate Transfer Body] The intermediate transfer member is an endless belt. The endless belt may be a single layer body or a laminate body. When the endless belt is a single-layer body, the single-layer body is an outer peripheral layer that contains a first resin, conductive carbon particles, and a specific silicone oil, and has an L(r) integral value of 0 or more and 0.1 or less. Hereinafter, the conductive carbon particles contained in the outer peripheral layer are also referred to as "first conductive carbon particles," and the single-layer body that is the outer peripheral layer is also referred to as "single layer." When the endless belt is a laminate, the laminate has, for example, a base layer and a surface layer that is provided on the base layer and is the outermost layer. The laminate may have another layer between the base layer and the surface layer. When the endless belt is a laminate having a base layer and a surface layer, the surface layer is an outer peripheral layer that contains a first resin, first conductive carbon particles, and a specific silicone oil, and has an L(r) integral value of 0 or more and 0.1 or less. Hereinafter, the surface layer that is the outer peripheral layer is also referred to as the "first layer". In addition, when the endless belt is a laminate having a base layer and a surface layer, the base layer is not particularly limited, and may be, for example, a layer containing a second resin described later and second conductive carbon particles described later. Hereinafter, the base layer is also referred to as the "second layer."
[0036] <Resin> The first resin contained in the outer peripheral layer includes at least one selected from the group consisting of polyimide resin (PI resin), polyamideimide resin (PAI resin), aromatic polyetheretherketone resin (PEEK resin), polyphenylene sulfide resin (PPS resin), and polyetherimide resin (PEI resin). The first resin may be composed of one type of resin or a mixture of two or more types of resin. The first resin may contain other resins. The total content of polyimide resin, polyamideimide resin, aromatic polyetheretherketone resin, polyphenylene sulfide resin, and polyetherimide resin in the entire first resin is preferably 80 mass% or more, more preferably 90 mass% or more, and even more preferably 95 mass% or more. Examples of other resins include aromatic polyetherketone resins other than PEEK resins, polyester resins, polyamide resins, polycarbonate resins, and the like.
[0037] From the viewpoint of maintaining a state in which the ghost phenomenon is suppressed, the first resin preferably contains an imide-based resin. Although the reason why the ghost phenomenon is suppressed by the first resin containing an imide-based resin is not clear, it is presumed that the imide-based resin is rigid, which makes it easier to maintain the state in which the specific silicone oil is present in the region close to the outer peripheral surface of the endless belt. When the first resin contains an imide-based resin, the total content of the imide-based resin in the entire first resin is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more. Examples of the imide resin include polyimide resin, polyamideimide resin, polyetherimide resin, etc. From the viewpoint of maintaining a state in which the ghost phenomenon is suppressed, the first resin more preferably contains at least one selected from the group consisting of polyimide resin and polyamideimide resin among imide resins, and further preferably contains a polyimide resin.
[0038] Examples of the second resin contained in the base layer include polyimide resin, polyamideimide resin, aromatic polyetherketone resin, polyphenylene sulfide resin, polyetherimide resin, polyester resin, polyamide resin, polycarbonate resin, etc. The second resin may be composed of one type of resin or a mixture of two or more types of resins. In addition, when the endless belt has a first layer and a second layer, the first resin and the second resin may be the same resin or different resins, and are preferably the same type of resin (for example, the first resin and the second resin are both polyimide resins).
[0039] (Polyimide resin) Examples of polyimide resins include imidized products of polyamic acids (precursors of polyimide resins), which are polymers of tetracarboxylic dianhydrides and diamine compounds. An example of the polyimide resin is a resin having a structural unit represented by the following general formula (I).
[0040] [ka]
[0041] In general formula (I), R 1 represents a tetravalent organic group, R 2 represents a divalent organic group. R 1Examples of the tetravalent organic group represented by the formula (1) include an aromatic group, an aliphatic group, a cyclic aliphatic group, a group in which an aromatic group and an aliphatic group are combined, and groups in which these groups are substituted. Specific examples of the tetravalent organic group include residues of tetracarboxylic dianhydrides, which will be described later. R 2 Examples of the divalent organic group represented by the formula (1) include an aromatic group, an aliphatic group, a cyclic aliphatic group, a group in which an aromatic group and an aliphatic group are combined, and a group in which these groups are substituted. Specific examples of the divalent organic group include residues of diamine compounds described below.
[0042] Specific examples of tetracarboxylic dianhydrides used as raw materials for polyimide resins include pyromellitic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4-biphenyltetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxyphenyl)sulfonic dianhydride, perylene-3,4,9,10-tetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, and ethylenetetracarboxylic dianhydride.
[0043] Specific examples of diamine compounds used as raw materials for polyimide resins include 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,3'-dichlorobenzidine, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 1,5-diaminonaphthalene, m-phenylenediamine, p-phenylenediamine, 3,3'-dimethyl 4,4'-biphenyldiamine, benzidine, and 3,3'-dimethyl Benzidine, 3,3'-dimethoxybenzidine, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenylpropane, 2,4-bis(β-amino tert-butyl)toluene, bis(p-β-amino-tert-butylphenyl)ether, bis(p-β-methyl-δ-aminophenyl)benzene, bis-p-(1,1-dimethyl-5-amino-pentyl)benzene, 1-isopropyl-2,4-m-phenylenediamine, m-xylylenediamine, p-xylylenediamine, di(p -aminocyclohexyl)methane, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, diaminopropyltetradiamine, 3-methylheptamethylenediamine, 4,4-dimethylheptamethylenediamine, 2,11-diaminododecane, 1,2-bis-3-aminopropoxyethane, 2,2-dimethylpropylenediamine, 3-methoxyhexamethylenediamine, 2,5-dimethylheptamethylenediamine, Examples include 3-methylheptamethylenediamine, 5-methylnonamethylenediamine, 2,17-diaminoeicosadecane, 1,4-diaminocyclohexane, 1,10-diamino-1,10-dimethyldecane, 12-diaminooctadecane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, piperazine, H2N(CH2)3O(CH2)2O(CH2)NH2, H2N(CH2)3S(CH2)3NH2, and H2N(CH2)3N(CH3)2(CH2)3NH2.
[0044] (Polyamide-imide resin) The polyamide-imide resin includes a resin having an imide bond and an amide bond in the repeating unit. More specifically, the polyamide-imide resin may be a polymer of a trivalent carboxylic acid compound (also called tricarboxylic acid) having an acid anhydride group, and a diisocyanate compound or a diamine compound.
[0045] As the tricarboxylic acid, trimellitic anhydride and its derivatives are preferable. In addition to the tricarboxylic acid, tetracarboxylic dianhydride, aliphatic dicarboxylic acid, aromatic dicarboxylic acid, etc. may be used in combination.
[0046] Examples of the diisocyanate compound include 3,3'-dimethylbiphenyl-4,4'-diisocyanate, 2,2'-dimethylbiphenyl-4,4'-diisocyanate, biphenyl-4,4'-diisocyanate, biphenyl-3,3'-diisocyanate, biphenyl-3,4'-diisocyanate, 3,3'-diethylbiphenyl-4,4'-diisocyanate, 2,2'-diethylbiphenyl-4,4'-diisocyanate, 3,3'-dimethoxybiphenyl-4,4'-diisocyanate, 2,2'-dimethoxybiphenyl-4,4'-diisocyanate, naphthalene-1,5-diisocyanate, and naphthalene-2,6-diisocyanate. The diamine compound may be a compound having a structure similar to that of the above-mentioned isocyanate, but having an amino group instead of the isocyanato group.
[0047] (Aromatic polyether ether ketone resin) Examples of aromatic polyether ether ketone resins include resins in which aromatic rings such as benzene rings are linearly bonded by ether bonds and ketone bonds, and in which the bonds are arranged in the following order: ether bond, ether bond, ketone bond.
[0048] (Polyphenylene sulfide resin) An example of the polyphenylene sulfide resin is a resin in which groups having benzene rings and sulfur atoms are alternately bonded. Examples of the group having a benzene ring include p-phenylene, m-phenylene, o-phenylene, alkyl-substituted phenylene, phenyl-substituted phenylene, halogen-substituted phenylene, amino-substituted phenylene, and amido-substituted phenylene.
[0049] (Polyetherimide resin) An example of the polyetherimide resin is a polymer of an aromatic bis(etherdicarboxylic acid) and a diamine. Examples of aromatic bis(ether dicarboxylic acids include 2,2-bis[4-(2,3-dicarboxyphenoxy)phenyl]propane and 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane. The diamine includes 4,4'-diaminodiphenylmethane, metaphenylenediamine, and the like.
[0050] In the endless belt which is a single layer body, the content of the first resin in the entire single layer which is the outer peripheral layer is preferably from 48% by mass to 91% by mass, more preferably from 55% by mass to 89% by mass, and further preferably from 65% by mass to 84% by mass, from the viewpoints of mechanical strength, volume resistivity adjustment, and the like. In the endless belt which is a laminate, the content of the first resin in the entire first layer which is the outer peripheral layer is preferably from 48% by mass to 91% by mass, more preferably from 55% by mass to 89% by mass, and further preferably from 65% by mass to 84% by mass, from the viewpoints of mechanical strength, volume resistivity adjustment, and the like. In the endless belt which is a laminate, the content of the second resin in the entire second layer is preferably from 60% by mass to 95% by mass, more preferably from 70% by mass to 90% by mass, and further preferably from 70% by mass to 80% by mass, from the viewpoints of mechanical strength, volume resistivity adjustment, and the like.
[0051] <Conductive carbon particles> The first conductive carbon particles contained in the outer peripheral layer include, for example, carbon black. Examples of carbon black include ketjen black, oil furnace black, channel black, acetylene black, etc. As the carbon black, surface-treated carbon black (hereinafter also referred to as "surface-treated carbon black") may be used. Surface-treated carbon black can be obtained by imparting, for example, a carboxy group, a quinone group, a lactone group, a hydroxy group, etc. to its surface. Examples of the surface treatment method include an air oxidation method in which the carbon black is reacted by contacting with air in a high-temperature atmosphere, a method in which the carbon black is reacted with nitrogen oxides or ozone at room temperature (e.g., 22°C), and a method in which the carbon black is oxidized with air in a high-temperature atmosphere and then oxidized with ozone at a low temperature.
[0052] The number-average primary particle size of the first conductive carbon particles is, for example, in the range of 20 nm or less, and from the viewpoint of adjusting the L(r) integral value within the above range, is preferably in the range of 18 nm or less, more preferably in the range of 15 nm or less, and even more preferably in the range of 13 nm or less. The number-average primary particle size of the first conductive carbon particles is, for example, in the range of 2 nm or more, and from the viewpoint of adjusting the L(r) integral value within the above range, is preferably in the range of 5 nm or more, and more preferably in the range of 10 nm or more.
[0053] The number average primary particle size of the conductive carbon particles is measured by the following method. First, a measurement sample having a thickness of 100 nm is taken from each layer of the obtained belt using a microtome, and the measurement sample is observed using a TEM (transmission electron microscope).Then, the diameter of a circle equal to the projected area of each of 50 conductive carbon particles (i.e., the equivalent circle diameter) is taken as the particle diameter, and the average value is taken as the number-average primary particle diameter.
[0054] When the first resin contains at least one selected from the group consisting of polyimide resins and polyamideimide resins, and the peripheral layer is formed using the first coating liquid described below, the first conductive carbon particles are preferably channel black, and surface-treated channel black is more preferable, from the viewpoint of adjusting the L(r) integral value within the above range. When the outer peripheral layer is formed using the first coating liquid, the pH of the first conductive carbon particles is, for example, in the range of 1.0 or more and 5.5 or less, and from the viewpoint of adjusting the L(r) integral value within the above range, the pH is preferably in the range of 1.0 or more and 3.0 or less.
[0055] When the first resin contains at least one selected from the group consisting of polyetherimide resin, aromatic polyether ether ketone resin, and polyphenylene sulfide resin, and the outer peripheral layer is formed by melt extrusion as described below, the first conductive carbon particles are preferably channel black and furnace black from the viewpoint of adjusting the L(r) integral value within the above range, and more preferably, the first conductive carbon particles are not surface-treated.
[0056] The first conductive carbon particles may consist of one type of conductive carbon particles, or may be a mixture of two or more types of conductive carbon particles.
[0057] In the endless belt which is a single layer body, the content of the first conductive carbon particles in the entire single layer which is the outer peripheral layer is preferably from 8 mass % to 45 mass %, more preferably from 10 mass % to 38 mass %, and further preferably from 13 mass % to 30 mass %, from the viewpoint of reducing the L(r) integral value and ensuring strength. In the endless belt which is a laminate, the content of the first conductive carbon particles in the entire first layer which is the outer peripheral layer is preferably from 8 mass % to 45 mass %, more preferably from 10 mass % to 38 mass %, and even more preferably from 13 mass % to 30 mass %, from the viewpoint of reducing the L(r) integral value and ensuring strength.
[0058] In the endless belt which is a laminate, specific examples of the second conductive carbon particles contained in the second layer include the same as the specific examples of the first conductive carbon particles. The number average primary particle size of the second conductive carbon particles is, for example, in the range of 2 nm or more and 40 nm or less. From the viewpoints of dispersibility, mechanical strength, volume resistivity, film-forming properties, etc., the range of 20 nm or more and 40 nm or less is preferable, the range of 20 nm or more and 35 nm or less is more preferable, and the range of 20 nm or more and 28 nm or less is even more preferable.
[0059] When the endless belt has a first layer and a second layer, the number average primary particle size of the first conductive carbon particles is preferably smaller than the number average primary particle size of the second conductive carbon particles. The number average primary particle size of the first conductive carbon particles is preferably 0.5 to less than 1.0 times the number average primary particle size of the second conductive carbon particles, more preferably 0.5 to 0.8 times, and even more preferably 0.5 to 0.7 times.
[0060] In the case of forming a base layer in an endless belt which is a laminate using a second coating liquid described later, the pH of the second conductive carbon particles is, for example, in the range of 1.0 or more and 5.5 or less, and from the viewpoint of adjusting the L(r) integral value within the above range, the pH is preferably in the range of 1.0 or more and 3.0 or less. In addition, when the endless belt has a first layer formed using a first coating liquid and a second layer formed using a second coating liquid, it is preferable that the pH of the first conductive carbon particles is lower than the pH of the second conductive carbon particles.
[0061] In the endless belt which is a laminate, the content of the second conductive carbon particles relative to the entire base layer is preferably from 5 mass % to 40 mass %, more preferably from 10 mass % to 30 mass %, and even more preferably from 20 mass % to 30 mass %, from the viewpoints of dispersibility, mechanical strength, and volume resistivity adjustment.
[0062] <Silicone oil> The silicone oil contained in the outer peripheral layer includes at least one specific silicone oil selected from the group consisting of dimethylpolysiloxane and organic group-substituted dimethylpolysiloxane. Here, the term "organic group-substituted dimethylpolysiloxane" refers to a compound in which at least a portion of the methyl groups in dimethylpolysiloxane has been substituted with an organic group.
[0063] The organic group is not particularly limited as long as it is a group having carbon atoms. Examples of the organic group include a group having one or more carbon atoms, which is selected from the group consisting of an alkyl group, an amino group, an epoxy group, an alicyclic epoxy group, a hydroxyl group, a carboxyl group, a mercapto group, a phenyl group, a vinyl group, an alkylene group, a carbonyl group, an ether bond, a thioether bond, an ester bond, an amide bond, and a combination thereof.
[0064] The organic group-substituted dimethylpolysiloxane may be a side-chain modified silicone oil in which an organic group is bonded as a side chain of dimethylpolysiloxane, a single-end modified silicone oil in which an organic group is bonded to one end of dimethylpolysiloxane, a double-end modified silicone oil in which an organic group is bonded to each of both ends of dimethylpolysiloxane, or a side-chain double-end modified silicone oil in which an organic group is bonded to each of the side chain and both ends of dimethylpolysiloxane. From the viewpoint of suppressing the ghost phenomenon, the organic group-substituted dimethylpolysiloxane is preferably a side-chain modified silicone oil, a double-end modified silicone oil, or a side-chain double-end silicone oil, and more preferably a double-end modified silicone oil.
[0065] The organic group-substituted dimethylpolysiloxane may be silicone oil having at least one organic group selected from the group consisting of a group having a polyether structure, an aralkyl group, a fluoroalkyl group, a long-chain alkyl group, a phenyl group, a group containing an ester bond, a group containing an amide bond, a group containing an epoxy group, a group containing an amino group, a group containing a carboxyl group, a group containing a hydroxyl group, and a group containing a mercapto group.The organic group-substituted dimethylpolysiloxane may have only one type of the above organic group, or may have two or more types. From the viewpoint of maintaining a state in which the ghost phenomenon is suppressed, the organic group-substituted dimethylpolysiloxane is preferably a silicone oil having, as an organic group, at least one selected from the group consisting of a group having a polyether structure, an aralkyl group, a fluoroalkyl group, a long-chain alkyl group, a phenyl group, a group containing an ester bond, and a group containing an amide bond, more preferably a silicone oil having at least one selected from the group consisting of a group having a polyether bond, an aralkyl group, and a long-chain alkyl group, and even more preferably a silicone oil having at least one selected from the group consisting of a group having a polyether bond and an aralkyl group.
[0066] Examples of organic group substitution products of dimethylpolysiloxane include polyether-modified silicone oil, long-chain alkyl-modified silicone oil, epoxy-modified silicone oil, amino-modified silicone oil, carbinol-modified silicone oil, mercapto-modified silicone oil, carboxyl-modified silicone oil, methacrylic-modified silicone oil, acrylic-modified silicone oil, carboxylic anhydride-modified silicone oil, aralkyl-modified silicone oil, fluoroalkyl-modified silicone oil, higher fatty acid ester-modified silicone oil, higher fatty acid amide-modified silicone oil, phenyl-modified silicone oil, polyether-long-chain alkyl-aralkyl-modified silicone oil, long-chain alkyl-aralkyl-modified silicone oil, amino-polyether-modified silicone oil, epoxy-polyether-modified silicone oil, epoxy-aralkyl-modified silicone oil, and the like.
[0067] From the viewpoint of maintaining a state in which the ghost phenomenon is suppressed, the organic group substitution product of dimethylpolysiloxane is preferably polyether-modified silicone oil (silicone oil in which the organic group is a group having a polyether structure), aralkyl-modified silicone oil (silicone oil in which the organic group is an aralkyl group), polyether-long-chain alkyl-aralkyl-modified silicone oil (silicone oil in which the organic group is a group having a polyether structure, a long-chain alkyl group, and an aralkyl group), and long-chain alkyl-aralkyl-modified silicone oil (silicone oil in which the organic group is a long-chain alkyl group and an aralkyl group), more preferably polyether-modified silicone oil and aralkyl-modified silicone oil, and even more preferably aralkyl-modified silicone oil. The reason why the ghost phenomenon is suppressed by using polyether-modified silicone oil as the organic group substitute of dimethylpolysiloxane is not clear, but it is assumed that the presence of polyether group makes it easier to maintain the silicone oil oriented on the outer peripheral surface side of the endless belt. Also, the reason why the ghost phenomenon is suppressed by using aralkyl-modified silicone oil as the organic group substitute of dimethylpolysiloxane is not clear, but it is assumed that the stability is excellent because of the presence of benzene ring.
[0068] From the viewpoint of further suppressing the ghost phenomenon, the organic group substitute of dimethylpolysiloxane is preferably a compound having no cyclic siloxane structure. It is considered that the cyclic siloxane structure affects the orientation state of the compound on the outer peripheral surface side of the endless belt. Therefore, it is presumed that the ghost phenomenon is further suppressed by using a compound having no cyclic siloxane structure as the organic group substitute of dimethylpolysiloxane, compared to the case of using a compound having a cyclic siloxane structure.
[0069] The combination of the resin and silicone oil contained in the outer peripheral layer is preferably the combination of the first resin containing imide resin and the silicone oil containing at least one selected from the group consisting of polyether modified silicone oil and aralkyl modified silicone oil, among which, the combination of the first resin containing polyimide resin and the silicone oil containing at least one selected from the group consisting of polyether modified silicone oil and aralkyl modified silicone oil is more preferable, and the combination of the first resin containing polyimide resin and the silicone oil containing at least one selected from the group consisting of polyether modified silicone oil not having cyclic siloxane structure and aralkyl modified silicone oil not having cyclic siloxane structure is even more preferable.The reason why the state of suppressing the ghost phenomenon is maintained by combining imide resin and polyether modified silicone oil is not clear, but it is speculated that it is because the steric hindrance between the polyether group of silicone oil and imide resin makes it easier to maintain the state of silicone oil oriented on the outer peripheral surface side of the endless belt. In addition, the reason why the ghost phenomenon is suppressed by combining an imide resin with an aralkyl-modified silicone oil is not clear, but it is speculated that this is because the imide resin has a benzene ring, which makes steric hindrance more likely to occur.
[0070] The number average molecular weight of the specific silicone oil is not particularly limited, and may be, for example, from 50 to 2,000. From the viewpoint of suppressing the ghost phenomenon, the number average molecular weight is preferably from 100 to 1,500, and more preferably from 200 to 1,200. The number average molecular weight of silicone oil is measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120GPC as the measuring device, a Tosoh TSKgel SuperHM-M (15 cm) column, and tetrahydrofuran (THF) as the solvent. The number average molecular weight is calculated from the measurement results using a molecular weight calibration curve created with monodisperse polystyrene standard samples. The viscosity of the specific silicone oil at 20°C is not particularly limited and can be, for example, 0.1 mPa·s or more and 100 mPa·s or less. From the viewpoint of suppressing the ghost phenomenon, the viscosity is preferably 0.1 mPa·s or more and 50 mPa·s or less, and more preferably 0.1 mPa·s or more and 20 mPa·s or less. The viscosity of the silicone oil is measured using a B-8L type viscometer manufactured by Tokyo Keiki.
[0071] The silicone oil contains at least the specific silicone oil, and may or may not contain a silicone oil other than the specific silicone oil. The ratio of the specific silicone oil to the total silicone oil is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more. Examples of silicone oils other than the specific silicone oil include fluorine-modified silicone oil, methyl hydrogen silicone oil, and silanol-modified silicone oil.
[0072] In the endless belt which is a single layer, the content of silicone oil in the entire single layer which is the outer peripheral layer is preferably from 0.5% by mass to 7% by mass, more preferably from 0.5% by mass to 6% by mass, and even more preferably from 1% by mass to 3% by mass, from the viewpoint of suppressing the ghost phenomenon. In the endless belt which is a laminate, the content of silicone oil in the entire first layer which is the outer peripheral layer is preferably from 0.5% by mass to 7% by mass, more preferably from 0.5% by mass to 6% by mass, and even more preferably from 1% by mass to 3% by mass, from the viewpoint of suppressing the ghost phenomenon. By the content of silicone oil in the entire outer peripheral layer being within the above range, compared with the case where it is lower than the above range, the effect of reducing the non-electrostatic adhesion of the outer peripheral surface of the endless belt by silicone oil is easily obtained, and the ghost phenomenon is more suppressed.In addition, by the content of silicone oil in the entire outer peripheral layer being within the above range, compared with the case where it is higher than the above range, the reduction in the effect of reducing the non-electrostatic adhesion caused by the aggregation of silicone oil is less likely to occur, and the ghost phenomenon is more suppressed.
[0073] <Other ingredients> The outer peripheral layer may contain other components in addition to the first resin, the first conductive carbon particles, and the silicone oil, and the second layer in the endless belt which is a laminate may contain other components in addition to the second resin and the second conductive carbon particles. In the endless belt which is a single layer, the total content of the first resin, the first conductive carbon particles, and the silicone oil in the entire single layer which is the outer peripheral layer is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more. In the endless belt which is a laminate, the total content of the first resin, the first conductive carbon particles, and the silicone oil in the entire first layer which is the outer peripheral layer is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more. In the endless belt which is a laminate, the total content of the second resin and the second conductive carbon particles in the entire second layer is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more. Examples of other components include conductive agents other than conductive carbon particles, fillers for improving the strength of the belt, antioxidants for preventing thermal deterioration of the belt, surfactants for improving fluidity, and heat-resistant anti-aging agents.
[0074] <Characteristics of endless belts> (L(r) integral value) The integral value of L(r) on the outer circumferential surface of the endless belt is 0 or more and 0.1 or less, and from the viewpoint of suppressing the ghost phenomenon, is preferably 0 or more and 0.08 or less, and more preferably 0 or more and 0.06 or less.
[0075] Here, the spatial distribution of the conductive carbon particles is obtained by observing the outer peripheral surface of the endless belt with a scanning electron microscope (e.g., Hitachi High-Technologies Corporation, model number: SU8010) at a magnification of 20,000 times, and binarizing the obtained 256-level image at a threshold value of 128 using analysis software (e.g., free software "ImageJ") as necessary. Then, the statistical quantity L(r) value when the interparticle distance r is 0.05 μm or more and 0.30 μm or less is calculated every 0.05 μm based on the above formula, and the integral value in the range of 0.05 μm or more and 0.30 μm or less is obtained, and this value is called the "L(r) integral value."
[0076] The method for setting the L(r) integral value within the above range is not particularly limited, and examples thereof include a method of using conductive carbon particles having a small number average primary particle size, a method of selecting the type of conductive carbon particles used, and a method of adjusting the conditions (e.g., drying conditions) in the manufacturing process of the endless belt.
[0077] (Endless belt thickness) In the endless belt which is a single layer, the thickness of the single layer is preferably 60 μm or more and 120 μm or less, and more preferably 80 μm or more and 120 μm or less, from the viewpoint of the mechanical strength of the belt. In the endless belt which is a laminate, the thickness of the first layer is preferably 1 μm or more and 60 μm or less, and more preferably 3 μm or more and 60 μm or less, from the viewpoints of manufacturability and suppression of the ghost phenomenon. In the endless belt which is a laminate, the thickness of the second layer is preferably 10 μm or more and 80 μm or less, and more preferably 20 μm or more and 40 μm or less, from the viewpoint of the mechanical strength of the belt. When the endless belt has a first layer and a second layer, the ratio of the outer peripheral layer to the total thickness is preferably 3% or more and 90% or less, and more preferably 5% or more and 80% or less, from the viewpoint of suppressing the ghost phenomenon. The thickness of each layer is measured as follows. That is, the cross section of the endless belt in the thickness direction is observed with an optical microscope or a scanning electron microscope, the thickness of the layer to be measured is measured at 10 points, and the average value is regarded as the thickness.
[0078] (Volume resistivity of endless belt) From the viewpoint of improving transferability, the common logarithm of the volume resistivity when a voltage of 500 V is applied to the endless belt for 10 seconds is preferably 9.0 (log Ω·cm) or more and 13.5 (log Ω·cm) or less, more preferably 9.5 (log Ω·cm) or more and 13.2 (log Ω·cm) or less, and particularly preferably 10.0 (log Ω·cm) or more and 12.5 (log Ω·cm) or less. The volume resistivity of the endless belt when a voltage of 500 V is applied for 10 seconds is measured by the following method. A microammeter (Advantest R8430A) is used as the resistance measuring device, and a UR probe (Mitsubishi Chemical Analytech Co., Ltd.) is used as the probe to measure the volume resistivity (log Ω cm) at 6 equally spaced points in the circumferential direction of the endless belt, and 3 points in the center and both ends in the width direction, for a total of 18 points, at a voltage of 500 V, application time of 10 seconds, and pressure of 1 kgf, and the average value is calculated. The measurements are also performed in an environment with a temperature of 22°C and a humidity of 55% RH.
[0079] (surface resistivity of endless belt) From the viewpoint of improving transferability, the common logarithm of the surface resistivity when a voltage of 500 V is applied to the outer peripheral surface of the endless belt for 10 seconds is preferably 9.5 (log Ω / suq.) or more and 15.0 (log Ω / suq.) or less, more preferably 10.0 (log Ω / suq.) or more and 14.0 (log Ω / suq.) or less, and particularly preferably 11.0 (log Ω / suq.) or more and 13.5 (log Ω / suq.) or less. The unit of surface resistivity, logΩ / suq., is a logarithmic value of the resistance per unit area, and is also expressed as log(Ω / suq.), logΩ / suquare, logΩ / □, etc. The surface resistivity when a voltage of 500 V is applied to the outer peripheral surface of the endless belt for 10 seconds is measured by the following method. A microammeter (R8430A manufactured by Advantest) is used as the resistance measuring device, and a UR probe (manufactured by Mitsubishi Chemical Analytech Co., Ltd.) is used as the probe to measure the surface resistivity (logΩ / suq.) of the outer peripheral surface of the endless belt at 6 equally spaced points in the circumferential direction, and 3 points at the center and both ends in the width direction, for a total of 18 points, at a voltage of 500V, application time of 10 seconds, and pressure of 1kgf, and the average value is calculated. The measurements are also performed in an environment with a temperature of 22°C and a humidity of 55%RH.
[0080] <Manufacturing method of endless belt> The method for producing the endless belt according to the present embodiment is not particularly limited. In one example of the method for manufacturing an endless belt, for example, a first coating liquid preparation step is performed to prepare a first coating liquid containing a first resin or a precursor thereof, a first conductive carbon particle, a specific silicone oil, and a first solvent, a first coating film formation step is performed to apply the first coating liquid onto the outer circumference of a substrate to form a first coating film, and a first drying step is performed to dry the first coating film while increasing the temperature of the substrate. The method for manufacturing the endless belt may include other steps in addition to the first coating liquid preparation step, the first coating film formation step, and the first drying step. For example, when a precursor of the first resin is used, a first baking step is performed to bake the first coating film dried by the first drying step.
[0081] In the case of manufacturing an endless belt that is a single layer body, a single layer that is a peripheral layer containing the first resin, the first conductive carbon particles, and the specific silicone oil is formed on the peripheral surface of the coated material through the above-mentioned first coating solution preparation process, the first coating film formation process, and the first drying process. Note that the single layer may be formed, for example, by preparing pellets containing the first resin, the first conductive carbon particles, and the specific silicone oil, and melt-extruding the pellets.
[0082] When manufacturing an endless belt which is a laminate, for example, a first layer which is an outer peripheral layer containing a first resin, first conductive carbon particles, and a specific silicone oil is formed on the outer peripheral surface of a second layer formed on a substrate through the first coating liquid preparation process, the first coating film formation process, and the first drying process. In the case of manufacturing an endless belt which is a laminate, the second layer is formed on the outer peripheral surface of the material to be coated, for example, through a second coating liquid preparation step of preparing a second coating liquid containing a second resin or a precursor thereof, second conductive carbon particles, and a second solvent, a second coating film formation step of applying the second coating liquid onto the outer peripheral surface of the material to be coated to form a second coating film, and a second drying step of drying the second coating film. Note that the second layer may be formed, for example, by preparing pellets containing the second resin and the second conductive carbon particles, and melt-extruding the pellets.
[0083] (Coating solution preparation process) In the first coating liquid preparation step, a first coating liquid containing a first resin or its precursor, a first conductive carbon particle, a specific silicone oil, and a first solvent is prepared. For example, when the first resin is a polyimide resin and the first conductive carbon particle is carbon black, the first coating liquid is prepared as a solution in which, for example, carbon black is dispersed and polyamic acid, which is a precursor of the polyimide resin, and a specific silicone oil are dissolved in the first solvent. Also, for example, when the first resin is a polyamideimide resin and the first conductive carbon particle is carbon black, the first coating liquid is prepared as a solution in which, for example, carbon black is dispersed and polyamideimide resin and a specific silicone oil are dissolved in the first solvent.
[0084] As a method for preparing the first coating liquid, from the viewpoint of pulverizing aggregates of the first conductive carbon particles and from the viewpoint of increasing the dispersibility of the first conductive carbon particles, it is preferable to carry out a dispersion treatment using a pulverizer such as a ball mill or a jet mill. In addition, in the first coating liquid preparation process, from the viewpoint of increasing the dispersibility of the first conductive carbon particles, it is preferable to add a specific silicone oil to the first solvent in which the first conductive carbon particles are dispersed after performing a dispersion treatment of the first conductive carbon particles. The first solvent is not particularly limited and may be appropriately selected depending on the type of resin used as the first resin, etc. For example, when the first resin is a polyimide resin or a polyamide-imide resin, a polar solvent described later is preferably used as the first solvent.
[0085] Examples of polar solvents include N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide (DEAc), dimethylsulfoxide (DMSO), hexamethylene phosphoramide (HMPA), N-methylcaprolactam, N-acetyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone (N,N-dimethylimidazolidinone, DMI), and the like. These may be used alone or in combination of two or more.
[0086] In the case where the second coating liquid preparation step is performed, a second coating liquid containing a second resin, second conductive carbon particles, and a second solvent is prepared in the second coating liquid preparation step. The second resin and the second conductive carbon particles are as described above, and the preparation method of the second coating liquid and the second solvent are the same as the preparation method of the first coating liquid and the first solvent, respectively.
[0087] (Coating film formation process) In the first coating film forming step, the first coating liquid is applied onto the outer periphery of the coating target material to form a first coating film. The material to be coated may be, for example, a cylindrical or columnar metal mold. The material to be coated may be the metal mold having an outer peripheral surface treated with a release agent. When an endless belt which is a single layer is manufactured, in the first coating film forming step, for example, the first coating liquid is directly applied to the outer peripheral surface of the material to be coated or the material to be coated which has been treated with a release agent. When an endless belt which is a laminate is manufactured, in the first coating film forming step, for example, the first coating liquid is applied to the outer peripheral surface of the material to be coated on which the second layer or the second coating film has been formed.
[0088] Examples of methods for applying the first coating liquid include known methods such as spray coating, spiral coating (flow coating), blade coating, wire bar coating, dip coating, bead coating, air knife coating, and curtain coating. In addition, when the second coating film forming process is performed, the second coating film is formed by applying the second coating liquid onto the outer periphery of the coated material in the second coating film forming process. The method of applying the second coating liquid is the same as the method of applying the first coating liquid.
[0089] (drying process) In the first drying step, the first coating film formed in the first coating film forming step is dried. The first drying step removes the first solvent contained in the first coating film, and a single layer or a first layer is obtained. Examples of a method for drying the first coating film include a method of supplying hot air to the first coating film and a method of heating the material to be coated.
[0090] In the first drying step, when the integral average value of the temperature of the coated material in the drying step is A°C and the time from the start of drying until the temperature of the coated material reaches the integral average value A°C is Bmin, it is preferable that the integral average heating rate A / B (°C / min) is 5.74°C / min or more. When the integral average heating rate A / B (°C / min) is 5.74°C / min or more, the first coating film dries quickly, and the first conductive carbon particles are fixed before they aggregate in the first coating film, thereby obtaining a layer in which the first conductive carbon particles are well dispersed. It is presumed that the first conductive carbon particles are finely dispersed in the obtained layer, which makes it easier for the L(r) integral value to be in the range of 0 to 0.1.
[0091] Here, the above-mentioned integral average heating rate A / B is measured by first measuring the time change in temperature of the material being coated during the drying process by connecting a thermometer (e.g., Graphtec K thermocouple, model number: JBS-7115-5M-K) to a Graphtec data recorder (model number: GL240).Then, the temperature at which the integral value (area) of the temperature of the material being coated from the start of drying becomes half the integral value (area) of the temperature of the material being coated from the start of drying to the end of drying is taken as the "integral average value (A°C)", and the time (Bmin) from the start of drying until the temperature of the material being coated reaches the integral average value A°C is found to calculate the integral average heating rate A / B (°C / min).
[0092] The integrated average heating rate A / B (° C. / min) is more preferably 5.74° C. / min or more, and even more preferably 8.0° C. / min or more. The method for controlling the integrated average heating rate A / B within the above range is not particularly limited, and examples thereof include, when drying the first coating film by supplying hot air to the surface of the first coating film, a method for adjusting the speed of the hot air at the surface of the first coating film, a method for adjusting the temperature of the hot air, and the like.
[0093] The speed of the hot air on the surface of the first coating film is, for example, in the range of 0.1 m / s to 50 m / s, preferably in the range of 1 m / s to 40 m / s, and more preferably in the range of 1 m / s to 20 m / s. Here, the speed of the hot air on the surface of the first coating film is measured as follows: Specifically, a probe is placed on the surface of the coating film using an anemometer (TM350, manufactured by TASCO Corporation) and the measurement is performed.
[0094] The temperature of the hot air on the surface of the first coating film is, for example, in the range of 100°C or more and 280°C or less, preferably in the range of 100°C or more and 250°C or less, and more preferably in the range of 110°C or more and 235°C or less. The temperature of the hot air on the surface of the first coating film is measured by a thermometer (for example, a Graphtec K thermocouple, model number: JBS-7115-5M-K) connected to a Graphtec data recorder, model number: GL240). The method of supplying hot air to the surface of the first coating film is not particularly limited, and examples thereof include a method of blowing hot air from a drying oven from a slit nozzle toward the surface of the first coating film, a method of directly supplying hot air from a drying oven to the first coating film, etc. Among these, the method using a slit nozzle is preferred from the viewpoint of making it easier to control the speed of the hot air on the surface of the first coating film.
[0095] In addition, when the second drying step is performed, the second coating film formed in the second coating film forming step is dried in the second drying step. The method for drying the second coating film is the same as the method for drying the first coating film. The second drying step may be completed before the first coating film forming step is performed, or the first coating film forming step may be performed before the second drying step is completed, and the first drying step may also serve as a part of the second drying step.
[0096] (Firing process) As described above, the method for producing an endless belt may include a first baking step. In the first baking step, the first coating film dried in the first drying step is heated and baked. For example, when the first resin is a polyimide resin, the polyamic acid contained in the first coating film is imidized in the first baking step to obtain a polyimide. The heating temperature in the first baking step is, for example, in the range of 150° C. to 450° C., and preferably in the range of 200° C. to 430° C. The heating time in the first baking step is, for example, in the range of 20 minutes to 180 minutes, and preferably in the range of 60 minutes to 150 minutes. In the case of manufacturing an endless belt which is a laminate, when the second layer is formed through the second coating solution preparation step, the second coating film formation step, and the second drying step, a second baking step may be performed to bake the second coating film dried in the second drying step. The second baking step may also serve as the first baking step.
[0097] [Primary transfer device] The primary transfer device has a metallic primary transfer roll that is in contact with the inner surface of the intermediate transfer body and applies an electric field to the intermediate transfer body, and performs primary transfer of a toner image formed on the surface of an image carrier onto the outer surface of the intermediate transfer body. The metallic primary transfer roll is disposed opposite to the image carrier with the intermediate transfer body, which is an endless belt, sandwiched therebetween. In the primary transfer device, the metallic primary transfer roll applies a voltage of the opposite polarity to the charge polarity of the toner to the intermediate transfer body, thereby performing primary transfer of the toner image onto the outer peripheral surface of the intermediate transfer body. Examples of the primary transfer roll include metal members such as iron, copper, brass, stainless steel (SUS), sulfur composite steel (SUM), aluminum, nickel, etc. The primary transfer roll may be a hollow metal roll or a solid metal roll. The outer diameter of the primary transfer roll is, for example, in the range of 4 mm or more and 28 mm or less. The circumferential width of the nip region where the intermediate transfer body is sandwiched between the primary transfer roll and the image carrier is, for example, in the range of 0.5 mm or more and 5 mm or less.
[0098] [Secondary Transfer Device] The secondary transfer device is a device that performs second transfer of the toner image transferred onto the outer peripheral surface of the intermediate transfer body onto the surface of a recording medium. The secondary transfer device includes, for example, a secondary transfer roll arranged on the outer peripheral surface side of the intermediate transfer body, i.e., the side on which the toner image is held, and a back roll arranged on the inner peripheral surface side of the intermediate transfer body, i.e., the side opposite the side on which the toner image is held. In the secondary transfer device, the intermediate transfer body and the recording medium are sandwiched between the secondary transfer roll and the back roll to form a transfer electric field, whereby the toner image on the intermediate transfer body is secondarily transferred to the recording medium.
[0099] [Image forming equipment] The image forming apparatus according to this embodiment includes an image holder, a charging device that charges the surface of the image holder, an electrostatic latent image forming device that forms an electrostatic latent image on the charged surface of the image holder, a developing device that contains a developer containing toner and uses the developer to develop the electrostatic latent image formed on the surface of the image holder to form a toner image, and a transfer device that transfers the toner image to the surface of a recording medium, and uses the transfer device described above as the transfer device.
[0100] The image forming apparatus according to the present embodiment may be any of known image forming apparatuses, such as an apparatus equipped with a fixing means for fixing a toner image transferred onto the surface of a recording medium; an apparatus equipped with a cleaning means for cleaning the surface of an image holder before charging after the toner image is transferred; an apparatus equipped with a discharging means for irradiating the surface of the image holder with discharging light to discharge the surface before charging after the toner image is transferred; and an apparatus equipped with an image holder heating member for increasing the temperature of the image holder and reducing the relative temperature.
[0101] In the image forming apparatus according to the present embodiment, for example, the portion including the image carrier may have a cartridge structure (process cartridge) that is detachably attached to the image forming apparatus.
[0102] Hereinafter, an example of an image forming apparatus according to the present embodiment will be described with reference to the drawings. However, the image forming apparatus according to the present embodiment is not limited to this. Note that only the main parts shown in the drawings will be described, and the description of the rest will be omitted.
[0103] FIG. 1 is a schematic diagram showing the configuration of an image forming apparatus according to the present embodiment.
[0104] 1, the image forming apparatus 100 according to the present embodiment is, for example, an intermediate transfer type image forming apparatus generally called a tandem type, and includes a plurality of image forming units 1Y, 1M, 1C, and 1K in which toner images of each color component are formed by an electrophotographic method, a primary transfer section 10 (an example of a primary transfer device) that sequentially transfers (primary transfer) each of the color component toner images formed by each of the image forming units 1Y, 1M, 1C, and 1K to an intermediate transfer belt 15 (an example of an intermediate transfer body), a secondary transfer section 20 (an example of a secondary transfer device) that collectively transfers (secondary transfer) the superimposed toner images transferred onto the intermediate transfer belt 15 to a recording medium, paper K, and a fixing device 60 that fixes the secondarily transferred image onto the paper K (an example of a recording medium). The image forming apparatus 100 also includes a control section 40 that controls the operation of each device (each section).
[0105] Each of the image forming units 1Y, 1M, 1C, and 1K of the image forming apparatus 100 includes a photoconductor 11 that rotates in the direction of arrow A as an example of an image carrier that carries a toner image formed on its surface.
[0106] Around the photoconductor 11, there is provided a charger 12 as an example of a charging device that charges the photoconductor 11, and there is provided a laser exposure device 13 (the exposure beam is indicated by the symbol Bm in the figure) as an example of an electrostatic latent image forming device that writes an electrostatic latent image on the photoconductor 11.
[0107] In addition, around the photoconductor 11, there is provided a developing device 14, which is an example of a developing device, and which contains toner of each color component and makes the electrostatic latent image on the photoconductor 11 visible using the toner, and there is also provided a metallic primary transfer roll 16 which transfers the toner image of each color component formed on the photoconductor 11 to an intermediate transfer belt 15 at the primary transfer section 10. The toner may have a volume average particle diameter of, for example, 2 μm to 5 μm, and more preferably, 3.5 μm to 4.8 μm. The volume average particle size of the toner is measured using a Coulter Multisizer II (manufactured by Beckman Coulter) and an ISOTON-II (manufactured by Beckman Coulter). For the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5% aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant. This is added to 100 ml to 150 ml of electrolyte. The electrolyte in which the sample is suspended is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with a particle size range of 2 μm to 60 μm is measured using a Coulter Multisizer II with an aperture diameter of 100 μm. The number of particles sampled is 50,000. A cumulative distribution is drawn from the small diameter side for the particle size range (channel) divided based on the particle size distribution to be measured, and the particle size at which the cumulative 50% is reached is defined as the volume average particle size.
[0108] Furthermore, a photoreceptor cleaner 17 that removes residual toner on the photoreceptor 11 is provided around the photoreceptor 11, and electrophotographic devices including a charger 12, a laser exposure device 13, a developer 14, a primary transfer roll 16, and the photoreceptor cleaner 17 are sequentially arranged along the rotation direction of the photoreceptor 11. These image forming units 1Y, 1M, 1C, and 1K are arranged in a substantially linear fashion in the order of yellow (Y), magenta (M), cyan (C), and black (K) from the upstream side of the intermediate transfer belt 15.
[0109] The intermediate transfer belt 15 is driven (rotated) in a circular manner in the direction B shown in Fig. 1 at a speed suited to the purpose by various rolls. The various rolls include a drive roll 31 driven by a motor (not shown) excellent in constant speed performance to rotate the intermediate transfer belt 15, a support roll 32 supporting the intermediate transfer belt 15 extending in a substantially straight line along the arrangement direction of the photoconductors 11, a tensioning roll 33 that applies tension to the intermediate transfer belt 15 and functions as a correction roll to prevent the intermediate transfer belt 15 from meandering, a back roll 25 provided in the secondary transfer unit 20, and a cleaning back roll 34 provided in a cleaning unit that scrapes off residual toner on the intermediate transfer belt 15.
[0110] The primary transfer section 10 is composed of a primary transfer roll 16 arranged opposite the photoconductor 11 with the intermediate transfer belt 15 sandwiched therebetween. The primary transfer roll 16 is arranged in pressure contact with the photoconductor 11 with the intermediate transfer belt 15 sandwiched therebetween, and a voltage (primary transfer bias) of the opposite polarity to the charge polarity of the toner (negative polarity; the same applies below) is applied to the primary transfer roll 16. As a result, the toner images on the photoconductors 11 are electrostatically attracted to the intermediate transfer belt 15 in sequence, and superimposed toner images are formed on the intermediate transfer belt 15.
[0111] The secondary transfer unit 20 includes a back roll 25 and a secondary transfer roll 22 that is disposed on the toner image bearing surface side of the intermediate transfer belt 15 .
[0112] The back roll 25 has a surface resistivity of 1×10 7 Ω / □ or more 1×10 10 The hardness is set to, for example, 70° (Asker C: manufactured by Kobunshi Keiki Co., Ltd., the same applies below.) The back roll 25 is disposed on the back side of the intermediate transfer belt 15 to constitute an opposing electrode of the secondary transfer roll 22, and is in contact with a metallic power supply roll 26 to which a secondary transfer bias is stably applied.
[0113] On the other hand, the secondary transfer roll 22 has a volume resistivity of 10 7.5 Ωcm or more 108.5 The secondary transfer roll 22 is a cylindrical roll of Ωcm or less. The secondary transfer roll 22 is arranged in pressure contact with the back roll 25 with the intermediate transfer belt 15 sandwiched therebetween, and the secondary transfer roll 22 is further grounded to form a secondary transfer bias between the secondary transfer roll 22 and the back roll 25, and performs a second transfer of the toner image onto the paper K transported to the secondary transfer unit 20. The transport speed of the paper K in the secondary transfer unit 20 may be in the range of 50 mm / s to 600 mm / s, for example.
[0114] In addition, an intermediate transfer belt cleaner 35 is provided on the downstream side of the secondary transfer section 20 of the intermediate transfer belt 15 in a manner that allows it to be freely attached and detached, which removes residual toner and paper dust from the intermediate transfer belt 15 after the secondary transfer and cleans the surface of the intermediate transfer belt 15.
[0115] The intermediate transfer belt 15, the primary transfer section 10 (the primary transfer roll 16), and the secondary transfer section 20 (the secondary transfer roll 22) correspond to an example of a transfer device. Here, the image forming apparatus 100 may be configured to include a secondary transfer belt instead of the secondary transfer roll 22.
[0116] Meanwhile, a reference sensor (home position sensor) 42 is provided upstream of the yellow image forming unit 1Y to generate a reference signal that serves as a reference for timing image formation in each of the image forming units 1Y, 1M, 1C, and 1K. An image density sensor 43 for adjusting image quality is provided downstream of the black image forming unit 1K. This reference sensor 42 generates a reference signal by recognizing a mark provided on the back side of the intermediate transfer belt 15, and each of the image forming units 1Y, 1M, 1C, and 1K is configured to start image formation in response to an instruction from the control unit 40 based on the recognition of this reference signal.
[0117] Furthermore, in the image forming apparatus according to this embodiment, as transport means for transporting the paper K, there are provided a paper storage section 50 for storing the paper K, a paper feed roll 51 for taking out and transporting the paper K accumulated in the paper storage section 50 at a predetermined timing, a transport roll 52 for transporting the paper K fed by the paper feed roll 51, a transport guide 53 for sending the paper K transported by the transport roll 52 to the secondary transfer section 20, a transport belt 55 for transporting the paper K transported after secondary transfer by the secondary transfer roll 22 to the fixing device 60, and a fixing entrance guide 56 for guiding the paper K to the fixing device 60.
[0118] Next, a basic image forming process of the image forming apparatus according to this embodiment will be described.
[0119] In the image forming apparatus of this embodiment, image data output from an image reading device (not shown) or a personal computer (PC) (not shown), etc., is subjected to image processing by an image processing device (not shown), and then image formation work is performed by image forming units 1Y, 1M, 1C, and 1K.
[0120] The image processing device performs image processing on the input image data, such as shading correction, positional deviation correction, brightness / color space conversion, gamma correction, and various image editing such as frame erasure, color editing, and movement editing. The image data that has undergone image processing is converted into color material gradation data of four colors, Y, M, C, and K, and is output to the laser exposure device 13.
[0121] In the laser exposure device 13, an exposure beam Bm emitted from, for example, a semiconductor laser is irradiated onto the photoconductor 11 of each of the image forming units 1Y, 1M, 1C, and 1K in accordance with the input color material gradation data. In each of the photoconductors 11 of the image forming units 1Y, 1M, 1C, and 1K, the surface is charged by the charger 12, and then the surface is scanned and exposed by the laser exposure device 13 to form an electrostatic latent image. The formed electrostatic latent image is developed into a toner image of each color of Y, M, C, and K by each of the image forming units 1Y, 1M, 1C, and 1K.
[0122] The toner images formed on the photoconductors 11 of the image forming units 1Y, 1M, 1C, and 1K are transferred onto the intermediate transfer belt 15 in the primary transfer section 10 where each photoconductor 11 comes into contact with the intermediate transfer belt 15. More specifically, in the primary transfer section 10, a voltage (primary transfer bias) of the opposite polarity to the charging polarity (negative polarity) of the toner is applied to the base material of the intermediate transfer belt 15 by the primary transfer roll 16, and the toner images are sequentially superimposed on the surface of the intermediate transfer belt 15 to perform the primary transfer.
[0123] After the toner images are sequentially primarily transferred onto the surface of the intermediate transfer belt 15, the intermediate transfer belt 15 moves to transport the toner images to the secondary transfer unit 20. When the toner images are transported to the secondary transfer unit 20, the transport means rotates the paper feed roll 51 in accordance with the timing at which the toner images are transported to the secondary transfer unit 20, and paper K of the desired size is supplied from the paper storage unit 50. The paper K supplied by the paper feed roll 51 is transported by the transport roll 52 and reaches the secondary transfer unit 20 via the transport guide 53. Before reaching the secondary transfer unit 20, the paper K is temporarily stopped, and an alignment roll (not shown) rotates in accordance with the movement timing of the intermediate transfer belt 15 on which the toner images are held, thereby aligning the position of the paper K with the position of the toner image.
[0124] In the secondary transfer section 20, the secondary transfer roll 22 is pressed against the back roll 25 via the intermediate transfer belt 15. At this time, the paper K, which has been transported in time, is sandwiched between the intermediate transfer belt 15 and the secondary transfer roll 22. At this time, when a voltage (secondary transfer bias) of the same polarity as the charging polarity (negative polarity) of the toner is applied from the power supply roll 26, a transfer electric field is formed between the secondary transfer roll 22 and the back roll 25. Then, the unfixed toner images held on the intermediate transfer belt 15 are electrostatically transferred collectively onto the paper K in the secondary transfer section 20, which is pressed by the secondary transfer roll 22 and the back roll 25.
[0125] Thereafter, the paper K onto which the toner image has been electrostatically transferred is transported as it is after being peeled off from the intermediate transfer belt 15 by the secondary transfer roll 22, and is transported to a transport belt 55 provided downstream of the secondary transfer roll 22 in the paper transport direction. The transport belt 55 transports the paper K to the fixing device 60 at an optimal transport speed for the fixing device 60. The unfixed toner image on the paper K transported to the fixing device 60 is fixed onto the paper K by being subjected to a fixing process using heat and pressure by the fixing device 60. The paper K on which the fixed image has been formed is then transported to an ejected paper storage section (not shown) provided in the ejection section of the image forming apparatus.
[0126] On the other hand, after the transfer to the paper K is completed, the residual toner remaining on the intermediate transfer belt 15 is transported to the cleaning section as the intermediate transfer belt 15 rotates, and is removed from the intermediate transfer belt 15 by the cleaning back roll 34 and the intermediate transfer belt cleaner 35.
[0127] Although the present embodiment has been described above, the present invention is not limited to the above embodiment, and various modifications, changes, and improvements are possible. EXAMPLES
[0128] Hereinafter, examples of the present invention will be described, but the present invention is not limited to the following examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.
[0129] [Example A1] <Preparation of Coating Solution A1> 1000g of fully aromatic polyimide varnish (solid content: 18% by mass, Unitika, U-imide KX, solvent: NMP) was mixed with 39.6g (22phr) of oxidized gas black (Channel Black, Orion Engineered Carbons, FW200, number average primary particle size: 13nm) as the first conductive carbon particles, and the mixture was passed through a φ0.1mm orifice at a pressure of 200MPa using a high-pressure collision type disperser (Genus), and the slurry was collided into two parts 20 times to obtain a dispersion. 6.8g of polyether modified silicone oil (double-end type polyether modified silicone oil, Shin-Etsu Chemical Co., Ltd., product name: KF-600x, number of carbon atoms in organic groups: 6, number average molecular weight: 900, viscosity at 20℃: 2mPa·s) was added to the obtained dispersion and stirred to obtain coating solution A1, which is the first coating solution.
[0130] <Production of Belt A1> The obtained coating solution A1 was applied to the outer surface of a SUS pipe having a diameter of φ366 (outer diameter 366 mm) by a flow coating method so as to obtain a predetermined film thickness, and after 30 minutes of rotary drying at 150°C, the pipe was placed in an oven at 320°C for 4 hours and then removed to obtain a SUS pipe having an endless belt A1 formed on its outer surface. The total film thickness of the endless belt A1 (i.e., the film thickness of a single layer) was 80 μm. The integrated average temperature rise rate A / B in the drying process was 8.0°C / min.
[0131] The endless belt A1 with the coated outer surface was removed from the SUS pipe and cut to a width of 369 mm to obtain the belt-shaped intermediate transfer body, belt A1. The content of the conductive carbon particles in the entire belt A1 was 17.5% by mass, and the content of the silicone oil in the entire belt A1 was 3% by mass. In addition, when the volume resistivity and the surface resistivity of the outer peripheral surface of the belt A1 were measured by the above-mentioned method, the common logarithm value of the volume resistivity was 9.8 (log Ω·cm), and the common logarithm value of the surface resistivity was 9.6 (log Ω / suq.).
[0132] [Example A2] Coating liquid A2 was obtained in the same manner as coating liquid A1, except that the amount of oxidized gas black added as the first conductive carbon particles was changed from 39.6 g to 32.9 g (18.3 phr). Belt A2 was obtained in the same manner as Belt A1, except that Coating Liquid A2 was used instead of Coating Liquid A1. The total thickness of belt A2 (ie, the thickness of a single layer) is 80 μm, the content of conductive carbon particles in the entire belt A2 is 15.0 mass %, and the content of silicone oil in the entire belt A2 is 3 mass %. In addition, when the volume resistivity and surface resistivity of the outer peripheral surface of belt A2 were measured using the method described above, the common logarithm value of the volume resistivity was 11.0 (log Ω·cm), and the common logarithm value of the surface resistivity was 10.8 (log Ω / suq.).
[0133] [Example A3] Coating liquid A3 was obtained in the same manner as Coating liquid A1, except that the amount of polyether-modified silicone oil added was changed from 6.8 g to 11.6 g. Belt A3 was obtained in the same manner as Belt A1, except that Coating Liquid A3 was used instead of Coating Liquid A1. The total thickness of belt A3 (that is, the thickness of a single layer) is 80 μm, the content of conductive carbon particles in the entire belt A3 is 17.1 mass %, and the content of silicone oil in the entire belt A3 is 5 mass %. In addition, when the volume resistivity and the surface resistivity of the outer surface of the belt A3 were measured by the above-mentioned method, the common logarithm value of the volume resistivity was 9.8 (log Ω·cm), and the common logarithm value of the surface resistivity was 9.8 (log Ω / suq.).
[0134] [Example A4] Coating liquid A4 was obtained in the same manner as Coating liquid A1, except that the amount of polyether-modified silicone oil added was changed from 6.8 g to 16.6 g. Belt A4 was obtained in the same manner as Belt A1, except that Coating Liquid A4 was used instead of Coating Liquid A1. The total thickness of the belt A4 (ie, the thickness of a single layer) is 80 μm, the content of conductive carbon particles in the entire belt A4 is 16.8 mass %, and the content of silicone oil in the entire belt A4 is 7 mass %. In addition, when the volume resistivity and surface resistivity of the outer surface of the belt A4 were measured by the method described above, the common logarithm value of the volume resistivity was 9.8 (log Ω·cm), and the common logarithm value of the surface resistivity was 9.5 (log Ω / suq.).
[0135] [Example A5] Coating liquid A5 was obtained in the same manner as Coating liquid A1, except that the amount of polyether-modified silicone oil added was changed from 6.8 g to 55 g. Belt A5 was obtained in the same manner as Belt A1, except that Coating Liquid A5 was used instead of Coating Liquid A1. The total thickness of belt A5 (ie, the thickness of a single layer) is 80 μm, the content of conductive carbon particles in the entire belt A5 is 14.4 mass %, and the content of silicone oil in the entire belt A5 is 20 mass %. In addition, when the volume resistivity and the surface resistivity of the outer surface of the belt A5 were measured by the above-mentioned method, the common logarithm value of the volume resistivity was 12.0 (log Ω·cm), and the common logarithm value of the surface resistivity was 11.6 (log Ω / suq.).
[0136] [Example A6] Coating liquid A6 was obtained in the same manner as in Coating liquid A1, except that the amount of polyether-modified silicone oil added was changed from 6.8 g to 2.3 g. Belt A6 was obtained in the same manner as Belt A1, except that Coating Liquid A6 was used instead of Coating Liquid A1. The total thickness of the belt A6 (ie, the thickness of a single layer) is 80 μm, the content of conductive carbon particles in the entire belt A6 is 17.9 mass %, and the content of silicone oil in the entire belt A6 is 1 mass %. In addition, when the volume resistivity and the surface resistivity of the outer peripheral surface of Belt A6 were measured by the above-mentioned method, the common logarithm value of the volume resistivity was 10.0 (log Ω·cm), and the common logarithm value of the surface resistivity was 11.2 (log Ω / suq.).
[0137] [Example A7] Coating Solution A7 was obtained in the same manner as Coating Solution A1, except that long-chain alkyl-modified silicone oil (side-chain type long-chain alkyl-modified silicone oil, manufactured by Shin-Etsu Chemical Co., Ltd., product name: KF-41x, number of carbon atoms in organic group: 10, number average molecular weight: 1100, viscosity at 20°C: 4 mPa s) was used instead of polyether-modified silicone oil. Belt A7 was obtained in the same manner as Belt A1, except that Coating Liquid A7 was used instead of Coating Liquid A1. The total thickness of belt A7 (that is, the thickness of a single layer) is 80 μm, the content of conductive carbon particles in the entire belt A7 is 17.5 mass %, and the content of silicone oil in the entire belt A7 is 3 mass %. In addition, when the volume resistivity and the surface resistivity of the outer peripheral surface of Belt A7 were measured by the above-mentioned method, the common logarithm value of the volume resistivity was 9.8 (log Ω·cm), and the common logarithm value of the surface resistivity was 9.6 (log Ω / suq.).
[0138] [Example A8] Coating Solution A8 was obtained in the same manner as Coating Solution A1, except that epoxy-modified silicone oil (side chain both end type epoxy-modified silicone oil, manufactured by Shin-Etsu Chemical Co., Ltd., product name: X-22-900x, number of carbon atoms in organic group: 9, number average molecular weight: 1100, viscosity at 20°C: 4 mPa s) was used instead of polyether-modified silicone oil. Belt A8 was obtained in the same manner as Belt A1, except that Coating Liquid A8 was used instead of Coating Liquid A1. The total thickness of the belt A8 (that is, the thickness of a single layer) is 80 μm, the content of conductive carbon particles in the entire belt A8 is 17.5 mass %, and the content of silicone oil in the entire belt A8 is 3 mass %. In addition, when the volume resistivity and the surface resistivity of the outer peripheral surface of Belt A8 were measured by the above-mentioned method, the common logarithm value of the volume resistivity was 9.8 (log Ω·cm), and the common logarithm value of the surface resistivity was 9.6 (log Ω / suq.).
[0139] [Example A9] Coating solution A9 was obtained in the same manner as coating solution A1, except that dimethyl silicone oil (dimethylpolysiloxane, manufactured by Kyoei Chemical Industry Co., Ltd., product name: KL400, number average molecular weight: 200, viscosity at 20°C: 0.5 mPa·s) was used instead of polyether-modified silicone oil. Belt A9 was obtained in the same manner as Belt A1, except that Coating Liquid A9 was used instead of Coating Liquid A1. The total thickness of belt A9 (that is, the thickness of a single layer) is 80 μm, the content of conductive carbon particles in the entire belt A9 is 17.5 mass %, and the content of silicone oil in the entire belt A9 is 3 mass %. In addition, when the volume resistivity and the surface resistivity of the outer peripheral surface of Belt A9 were measured by the above-mentioned method, the common logarithm value of the volume resistivity was 9.8 (log Ω·cm), and the common logarithm value of the surface resistivity was 11.0 (log Ω / suq.).
[0140] [Example A10] Coating solution A10 was obtained in the same manner as Coating solution A1, except that 43.2 g (24 phr) of oxidized gas black (Channel Black, manufactured by Orion Engineered Carbons, SB6, number average primary particle size: 17 nm) was used as the first conductive carbon particles. Belt A10 was obtained in the same manner as Belt A1, except that Coating Liquid A10 was used instead of Coating Liquid A1. The total thickness of the belt A10 (that is, the thickness of a single layer) is 80 μm, the content of conductive carbon particles in the entire belt A10 is 18.8 mass %, and the content of silicone oil in the entire belt A10 is 3 mass %. In addition, when the volume resistivity and the surface resistivity of the outer peripheral surface of the belt A10 were measured by the above-mentioned method, the common logarithm value of the volume resistivity was 9.5 (log Ω·cm), and the common logarithm value of the surface resistivity was 9.5 (log Ω / suq.).
[0141] [Example A11] Instead of polyether-modified silicone oil, aralkyl-modified silicone oil (side-chain type aralkyl-modified silicone oil, Shin-Etsu Chemical Co., Ltd., product name: KF-410, viscosity at 20°C: 1000mm 2 Coating solution A11 was obtained in the same manner as in Coating solution A1, except that Coating solution A11 was used instead of Coating solution A1. Belt A11 was obtained in the same manner as Belt A1, except that Coating Liquid A11 was used instead of Coating Liquid A1. The total thickness of the belt A11 (that is, the thickness of a single layer) is 80 μm, the content of conductive carbon particles in the entire belt A11 is 18.5 mass %, and the content of silicone oil in the entire belt A11 is 1.5 mass %. In addition, when the volume resistivity and the surface resistivity of the outer peripheral surface of the belt A11 were measured by the above-mentioned method, the common logarithm value of the volume resistivity was 9.7 (log Ω·cm), and the common logarithm value of the surface resistivity was 9.7 (log Ω / suq.).
[0142] [Example B1] <Preparation of Coating Solution B1> 1000g of aromatic polyamideimide varnish (solid content 18% by mass, HPC-9000 made by Resonac, solvent: NMP) was mixed with 37.8g (22phr) of oxidized gas black (channel black, made by Orion Engineered Carbons, FW200, number average primary particle size: 13nm) as the first conductive carbon particles, and the mixture was passed through a φ0.1mm orifice at a pressure of 200MPa using a high-pressure collision type disperser (made by Genus), and the slurry was collided into two parts 10 times to obtain a dispersion. 6.8g of polyether-modified silicone oil (double-end type polyether-modified silicone oil, made by Shin-Etsu Chemical Co., Ltd., product name: KF-600x, number of carbon atoms in organic groups: 6, number average molecular weight: 900, viscosity at 20℃: 2mPa·s) was added to the obtained dispersion and stirred to obtain coating solution B1, the first coating solution.
[0143] <Preparation of Belt B1> -Release agent treatment for coated materials- A cylindrical mold made of stainless steel with an outer diameter of 366 mm and a length of 400 mm was prepared as the material to be coated. A silicone-based mold release agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name: Sepacoat SP) was applied to its outer surface and a drying process (mold release agent treatment) was performed.
[0144] - Formation of the first coating film - While rotating a cylindrical mold treated with a mold release agent in the circumferential direction at a speed of 10 rpm, the above-mentioned coating liquid B1 was discharged from a dispenser with a diameter of 1.0 mm from the end of the cylindrical mold, and applied by pressing with a uniform pressure using a metal blade installed on the mold. The dispenser unit was moved in the axial direction of the cylindrical mold at a speed of 100 mm / min, so that the coating liquid B1 was applied in a spiral shape onto the cylindrical mold, forming a first coating film.
[0145] - Drying of the first coating film - Thereafter, the mold and the first coating film were dried in a drying oven for 15 minutes while rotating at 10 rpm in an air atmosphere at 150° C. The integrated average temperature rise rate A / B in the drying process of the first coating film was 6.0° C. / min.
[0146] - Firing - Next, the endless belt B1 was obtained by placing the endless belt B1 in an oven for 4 hours at a temperature of 290° C. The total thickness of the endless belt B1 (that is, the thickness of a single layer) was 80 μm. The endless belt B1 was removed from the mold, stretched around a holder, and cut with a cutter whose insertion angle was adjusted to obtain a ring-shaped belt having a diameter of 366 mm and a width of 369.5 mm. The intermediate transfer belt thus produced was designated as belt B1. The conductive carbon particle content in the entire belt B1 is 16.8% by mass, and the silicone oil content in the entire belt B1 is 3% by mass. In addition, when the volume resistivity and surface resistivity of the outer peripheral surface of belt B1 were measured using the method described above, the common logarithm value of the volume resistivity was 9.9 (log Ω·cm), and the common logarithm value of the surface resistivity was 9.5 (log Ω / suq.).
[0147] [Example C1] <Preparation of Belt C1> PEEK resin (450G manufactured by Victrex) pellets and furnace black (first conductive carbon particles, manufactured by Orion Engineered Carbons, FW171, number average primary particle size: 11 nm) were charged into a Henschel mixer (FM10C manufactured by Nippon Coke) so that the ratio was 180 g of PEEK resin and 27 g (15 phr) of furnace black, and mixed. 6.6 g of polyether-modified silicone oil (double-end type polyether-modified silicone oil, manufactured by Shin-Etsu Chemical Co., Ltd., product name: KF-600x, number of carbon atoms in organic group: 6, number average molecular weight: 900, viscosity at 20 °C: 2 mPa s) was added to the mixed composition and stirred. The mixture to which silicone oil had been added was melt-kneaded in a twin-screw extrusion melt kneader (L / D60, manufactured by Parker Corporation), and then extruded into a string-like shape from a hole of φ5 (inner diameter 5 mm). The extruded material was placed in a water tank to cool and solidify, and then cut to obtain mixed resin pellets containing furnace black.
[0148] The resulting mixed resin pellets were fed into a single-screw melt extruder (L / D24, melt extrusion device (manufactured by Mitsuba Manufacturing Co., Ltd.)) set at a predetermined temperature (380°C), and extruded into a cylindrical shape from the gap between the annular die and the nipple while melting. In order to fix the cylindrical shape and diameter of the film while pulling up the extruded cylindrical film, the inner surface of the cylindrical film was brought into contact with a sizing die (cooling mold) set at a predetermined temperature (50°C) and cooled to obtain an endless belt C1. The endless belt C1 was removed from the cooling mold, stretched over a holder, and cut with a cutter whose insertion angle was adjusted to obtain a ring-shaped body with a diameter of 366 mm and a width of 369 mm. The intermediate transfer belt thus produced was the belt C1. The overall thickness of the belt C1 (i.e., the thickness of a single layer) was 80 μm. The conductive carbon particles were contained in the entire belt C1 at a content of 12.6% by mass, and the silicone oil was contained in the entire belt C1 at a content of 3% by mass. In addition, when the volume resistivity and surface resistivity of the outer surface of belt C1 were measured using the method described above, the common logarithm value of the volume resistivity was 11.1 (log Ω·cm), and the common logarithm value of the surface resistivity was 10.5 (log Ω / suq.).
[0149] [Example D1] <Preparation of Belt D1> PPS resin (Toray Torelina T1881) powder and gas black (first conductive carbon particles, channel black, Orion Engineered Carbons, FW1, number average primary particle size: 13 nm) were charged into a Henschel mixer (Nippon Coke FM10C) to a ratio of 180 g PPS resin and 27 g (15 phr) gas black (i.e., channel black), and mixed. 6.6 g of polyether-modified silicone oil (double-end type polyether-modified silicone oil, Shin-Etsu Chemical Co., Ltd., product name: KF-600x, number of carbon atoms in organic group: 6, number average molecular weight: 900, viscosity at 20°C: 2 mPa·s) was added to the mixed composition and stirred. The mixture to which silicone oil had been added was melt-kneaded in a twin-screw extrusion melt kneader (L / D60, manufactured by Parker Corporation), and then extruded into a string-like shape from a hole of φ5 (inner diameter 5 mm). The extruded material was placed in a water tank to cool and solidify, and then cut to obtain mixed resin pellets containing gas black (i.e., channel black).
[0150] The obtained mixed resin pellets were fed into a single-screw melt extruder (L / D24, melt extrusion device (manufactured by Mitsuba Manufacturing Co., Ltd.)) set at a predetermined temperature (350°C), and extruded into a cylindrical shape from the gap between the annular die and the nipple while melting. In order to fix the cylindrical shape and diameter of the film while pulling up the extruded cylindrical film, the inner peripheral surface of the cylindrical film was brought into contact with a sizing die (cooling mold) set at a predetermined temperature (50°C) and cooled to obtain an endless belt D1. The endless belt D1 was removed from the cooling mold, and the removed endless belt D1 was stretched around a holder and cut with a cutter whose insertion angle was adjusted to obtain a ring-shaped body with a diameter of 366 mm and a width of 369 mm. The intermediate transfer belt thus produced was belt D1. The total thickness of belt D1 (i.e., the thickness of a single layer) was 80 μm. The conductive carbon particles were contained in the entire belt D1 at a content of 12.6% by mass, and the silicone oil was contained in the entire belt D1 at a content of 3% by mass. In addition, when the volume resistivity and the surface resistivity of the outer peripheral surface of belt D1 were measured by the above-mentioned method, the common logarithm value of the volume resistivity was 11.1 (log Ω·cm), and the common logarithm value of the surface resistivity was 10.5 (log Ω / suq.).
[0151] [Example E1] <Preparation of Belt E1> PEI resin (made by Sabic, product name: ULTEM) powder and gas black (first conductive carbon particles, channel black, made by Orion Engineered Carbons, FW1, number average primary particle size: 13 nm) were charged into a Henschel mixer (made by Nippon Coke, FM10C) so that the ratio was 180 g of PPS resin and 27 g (15 phr) of gas black (i.e., channel black), and mixed. 6.6 g of polyether-modified silicone oil (both end-type polyether-modified silicone oil, made by Shin-Etsu Chemical, product name: KF-600x, number of carbon atoms in organic group: 6, number average molecular weight: 900, viscosity at 20 °C: 2 mPa s) was added to the mixed composition and stirred. The mixture to which silicone oil had been added was melt-kneaded in a twin-screw extrusion melt kneader (L / D60, manufactured by Parker Corporation), and then extruded into a string-like shape from a hole of φ5 (inner diameter 5 mm). The extruded material was placed in a water tank to cool and solidify, and then cut to obtain mixed resin pellets containing gas black (i.e., channel black).
[0152] The resulting mixed resin pellets were fed into a single-screw melt extruder (L / D24, melt extrusion device (manufactured by Mitsuba Manufacturing Co., Ltd.)) set at a predetermined temperature (350°C), and extruded into a cylindrical shape from the gap between the annular die and the nipple while melting. In order to fix the cylindrical shape and diameter of the film while pulling up the extruded cylindrical film, the inner peripheral surface of the cylindrical film was brought into contact with a sizing die (cooling mold) set at a predetermined temperature (50°C) and cooled, to obtain an endless belt E1. The endless belt E1 was removed from the cooling mold, and the removed endless belt E1 was stretched on a holder and cut with a cutter with an adjusted insertion angle to obtain a ring-shaped body with a diameter of 366 mm and a width of 369 mm. The intermediate transfer belt thus produced was belt E1. The total thickness of belt E1 (i.e., the thickness of a single layer) was 80 μm. The conductive carbon particles were contained in the entire belt E1 at a content of 12.6% by mass, and the silicone oil was contained in the entire belt E1 at a content of 3% by mass. In addition, when the volume resistivity and surface resistivity of the outer peripheral surface of belt E1 were measured using the method described above, the common logarithm value of the volume resistivity was 11.1 (log Ω·cm), and the common logarithm value of the surface resistivity was 10.0 (log Ω / suq.).
[0153] [Example F1] <Synthesis of polyamic acid> Polyamic acid DA-A1, which is a polyamic acid having amino groups at both ends of the molecular chain, and polyamic acid DC-A1, which is a polyamic acid having carboxy groups at both ends of the molecular chain, were synthesized by the following method.
[0154] -Preparation of polyamic acid solution DA-A1- To 800 g of N-methyl-2-pyrrolidone (hereinafter abbreviated as "NMP"), 83.48 g (416.9 mmol) of 4,4'-diaminodiphenyl ether (hereinafter abbreviated as "ODA") was added as a diamine compound, and dissolved with stirring at room temperature (25°C). Next, 116.52 g (396.0 mmol) of 3,3',4,4'-biphenyltetracarboxylic dianhydride (hereinafter abbreviated as "BPDA") was gradually added as a tetracarboxylic dianhydride. After the tetracarboxylic dianhydride was added and dissolved, the temperature of the reaction solution was heated to 60°C, and then the polymerization reaction was carried out for 20 hours while maintaining the reaction solution temperature, thereby obtaining a reaction solution containing polyamic acid DA-A1 and NMP.
[0155] The resulting reaction solution was filtered using a #800 stainless steel mesh and cooled to room temperature (25°C) to obtain a polyamic acid solution DA-A1 having a solution viscosity of 2.0 Pa·s at 25°C. The solution viscosity of the polyamic acid solution was measured using a Toki Sangyo Co., Ltd. E-type rotational viscometer, TV-20H, with a standard rotor (1°34" x R24) at a measurement temperature of 25°C and a rotation speed of 0.5 rpm (100 Pa s or more) and 1 rpm (less than 100 Pa s). The solution viscosities of the polyamic acid solutions obtained in the following synthesis examples were also measured in the same manner.
[0156] -Preparation of polyamic acid solution DC-A1- A polyamic acid solution DC-A1 containing polyamic acid DC-A1 and NMP and having a solution viscosity of 6.0 Pa s was obtained in the same manner as in Synthesis Example 1, except that the amount of ODA was 79.57 g (397.4 mmol) and the amount of BPDA was 120.43 g (409.3 mmol).
[0157] <Preparation of coating solution> -Preparation of Coating Solution F2 (Second Coating Solution)- Polyamic acid solution DA-A1 (solid content: 45% by weight) 70 parts by weight Polyamic acid solution DC-A1 (solid content: 15% by weight) 30 parts by weight Acidic carbon black (dry; conductive carbon particles) [SPECIAL BLACK4: Orion Engineered Carbons, pH 4.5, volatile content: 18.0%, gas black (i.e., channel black), number-average primary particle size: 25 nm (hereinafter abbreviated as "SB-4")] 26 parts by mass The polyamic acid solutions DA-A1 and DC-A1 having the above compositions were mixed, and SB-4 was added and dispersed in the polyamic acid solution mixture by dispersing in a ball mill at 30° C. for 12 hours. The mixture in which SB-4 was dispersed was then filtered through a #400 stainless steel mesh to obtain coating solution F2, which was the second coating solution.
[0158] - Preparation of Coating Solution F1 (First Coating Solution) - Polyamic acid solution DA-A1 (solid content: 45% by weight) 70 parts by weight Polyamic acid solution DC-A1 (solid content: 15% by weight) 30 parts by weight Acidic carbon black (dry; conductive carbon particles) [Color Black FW200, manufactured by Orion Engineered Carbons, gas black (i.e., channel black), number-average primary particle size: 13 nm, pH: 3.0 (hereinafter abbreviated as "FW200")] 18 parts by mass Polyether-modified silicone oil (double-terminated polyether-modified silicone oil, manufactured by Shin-Etsu Chemical Co., Ltd., product name: KF-600x, number of carbon atoms in organic group: 6, number average molecular weight: 900, viscosity at 20°C: 2 mPa s) 6.8 parts by mass The polyamic acid solution DA-A1 and the polyamic acid solution DC-A1 of the above composition were mixed, and FW200 was added and dispersed in a ball mill at 30°C for 12 hours to obtain a polyamic acid solution mixture. The obtained dispersion was added with polyether-modified silicone oil and stirred for 10 minutes to obtain a mixture. The mixture to which the silicone oil was added was then filtered with a #800 stainless steel mesh to obtain coating solution F1, which is the first coating solution.
[0159] <Production of Belt F1> -Release agent treatment for coated materials- A cylindrical mold made of stainless steel with an outer diameter of 366 mm and a length of 400 mm was prepared as the material to be coated. A silicone-based mold release agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name: Sepacoat SP) was applied to its outer surface and a drying process (mold release agent treatment) was performed.
[0160] - Formation of the second coating film - While rotating the cylindrical mold treated with a mold release agent in the circumferential direction at a speed of 10 rpm, the above coating solution F2 was discharged from a dispenser with a diameter of 1.0 mm from the end of the cylindrical mold, and applied by pressing with a uniform pressure using a metal blade installed on the mold. The dispenser unit was moved in the axial direction of the cylindrical mold at a speed of 100 mm / min, so that the coating solution F2 was applied in a spiral shape onto the cylindrical mold, forming a second coating film.
[0161] - Drying of the second coating - Thereafter, the mold and the second coating film were subjected to a drying treatment in a drying oven at 140° C. in an air atmosphere for 15 minutes while rotating at 10 rpm. After drying, the solvent volatilized from the second coating film, and the second coating film changed into a polyamic acid resin molded article (substrate 1) having self-supporting properties.
[0162] - Formation and drying of the first coating film - The coating solution F1 was applied to the outer peripheral surface of the substrate 1 by the same spin coating method as that for coating the coating solution F2 to form a first coating film, and then the first coating film was dried in a drying oven for 15 minutes at 140° C. in an air atmosphere while rotating at 10 rpm. The integrated average heating rate A / B in the drying process of the first coating film was 6.00° C. / min.
[0163] - Firing - Next, the endless belt F1 was obtained by placing the endless belt F1 in an oven for 4 hours at a temperature of 320° C. The total thickness of the endless belt F1 (total thickness of the base layer and the surface layer) was 80 μm, of which the base layer thickness was 26.7 μm and the surface layer thickness was 53.3 μm. The endless belt F1 was removed from the mold, stretched around a holder, and cut with a cutter whose insertion angle was adjusted to obtain a ring-shaped body having a diameter of 366 mm and a width of 369 mm. The intermediate transfer belt thus produced was designated as belt F1. In addition, the content of conductive carbon particles in the entire base layer of belt F1 is 22 mass %, the content of conductive carbon particles in the entire surface layer is 29 mass %, and the content of silicone oil in the entire surface layer is 3 mass %. In addition, when the volume resistivity and surface resistivity of the outer surface of belt F1 were measured using the method described above, the common logarithm value of the volume resistivity was 11.0 (log Ω·cm), and the common logarithm value of the surface resistivity was 9.5 (log Ω / suq.).
[0164] [Comparative Example G1] The intermediate transfer belt of DocuCentre C2000 (manufactured by Fujifilm Business Innovation Co., Ltd.) was used as it was as belt G1. The total thickness of the belt G1 (that is, the thickness of a single layer) is 75 μm, the content of conductive carbon particles in the entire belt G1 is 13 mass %, and the belt G1 does not contain silicone oil. In addition, when the volume resistivity and surface resistivity of the outer peripheral surface of belt G1 were measured using the method described above, the common logarithm value of the volume resistivity was 10.0 (log Ω·cm), and the common logarithm value of the surface resistivity was 9.8 (log Ω / suq.).
[0165] [Comparative example G2] An intermediate transfer belt of Apeos C8180 (manufactured by Fujifilm Business Innovation Co., Ltd.) was cut to a desired size (i.e., a width of 369 mm) and used as belt G2. The total thickness of the belt G2 (that is, the thickness of a single layer) is 80 μm, the content of the conductive carbon particles in the entire belt G2 is 16 mass %, and the belt G2 does not contain silicone oil. In addition, when the volume resistivity and surface resistivity of the outer peripheral surface of belt G2 were measured using the method described above, the common logarithm value of the volume resistivity was 11.0 (log Ω·cm), and the common logarithm value of the surface resistivity was 10.8 (log Ω / suq.).
[0166] [Comparative example G3] Coating solution G3 was obtained in the same manner as coating solution A1, except that 16 mass % of oxidized gas black (manufactured by Degussa, Special Black SB4, number average primary particle size: 25 nm) was used as the first conductive carbon particles. Belt G3 was obtained in the same manner as Belt A1, except that Coating Liquid G3 was used instead of Coating Liquid A1. The total thickness of belt G3 (ie, the thickness of a single layer) is 80 μm, the content of conductive carbon particles in the entire belt G3 is 16 mass %, and the content of silicone oil in the entire belt G3 is 3 mass %. In addition, when the volume resistivity and surface resistivity of the outer surface of the belt G3 were measured using the method described above, the common logarithm value of the volume resistivity was 10.5 (log Ω·cm), and the common logarithm value of the surface resistivity was 9.5 (log Ω / suq.).
[0167] [Comparative Example G4] Coating liquid G4 was obtained in the same manner as Coating liquid A1, except that fluorine-modified silicone oil (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KF400) was used instead of polyether-modified silicone oil. Belt G4 was obtained in the same manner as Belt A1, except that Coating Liquid G4 was used instead of Coating Liquid A1. The total thickness of the belt G4 (ie, the thickness of a single layer) is 80 μm, the content of conductive carbon particles in the entire belt G4 is 17.5 mass %, and the content of silicone oil in the entire belt G4 is 3 mass %. In addition, when the volume resistivity and surface resistivity of the outer peripheral surface of belt G4 were measured using the method described above, the common logarithm value of the volume resistivity was 9.8 (log Ω·cm), and the common logarithm value of the surface resistivity was 9.6 (log Ω / suq.).
[0168] [Comparative Example G5] Coating solution G5 was obtained in the same manner as coating solution A1, except that a surfactant (oligomer having a silicone structure with a methyl group, siloxane repeat number of 500, manufactured by Shin-Etsu Chemical Co., Ltd., product name: KP126) was used instead of polyether-modified silicone oil. Belt G5 was obtained in the same manner as Belt A1, except that Coating Liquid G5 was used instead of Coating Liquid A1. The total thickness of belt G5 (i.e., the thickness of a single layer) is 80 μm, the content of conductive carbon particles in the entire belt G5 is 17.5 mass%, the content of surfactant in the entire belt G5 is 3 mass%, and belt G5 does not contain any specific silicone oil. In addition, when the volume resistivity and surface resistivity of the outer surface of the belt G5 were measured using the method described above, the common logarithm value of the volume resistivity was 9.8 (log Ω·cm), and the common logarithm value of the surface resistivity was 9.6 (log Ω / suq.).
[0169] [Measurement of endless belts] The L(r) integral value of each of the obtained endless belts was determined by the above-mentioned method. The results are shown in Table 1. Table 1 also shows the layer structure of the endless belt and the type of resin contained in the single layer or the first layer.
[0170] [Manufacture of transfer devices and image forming devices] As the metallic primary transfer roll, a metal roll made of SUS304 having a diameter of φ12 (outer diameter 12 mm) and an axial length of 334 mm was used. The obtained belt and the above-mentioned primary transfer roll were attached to Apeos C2360 (FUJIFILM Business Innovation Co., Ltd.) to obtain an image forming apparatus equipped with a transfer device. The circumferential width of the nip region where the intermediate transfer member was sandwiched between the primary transfer roll and the image carrier was 4 mm.
[0171] [evaluation] Using toner with a volume average particle size of 5.8 μm, the obtained image forming device was used to print 100,000 full-color images on A3-sized coated paper in an ambient environment of 10°C and 15% RH in full-speed mode (transport speed: 308 mm / s) and half-speed mode (transport speed: 154 mm / s). The images were printed on 100,000 sheets of a 50 mm square grid tilted at 45 degrees over a full-surface halftone density of 20% process black, and the change in image density outside the grid was defined as a ghost. The occurrence of ghosting in the second image (initial image) was confirmed, and the initial ghost phenomenon suppression was evaluated according to the following criteria. In addition, the 2000th image (image after continuous use) was checked for the presence or absence of ghosting, and the maintenance of the suppression of the ghosting phenomenon was evaluated according to the following criteria ("Maintenance 1" in the table). Furthermore, the presence or absence of ghosting in the 100,000th image (image after continuous use) was confirmed, and the maintenance of the suppression of the ghosting phenomenon was evaluated according to the following criteria ("Maintenance 2" in the table).
[0172] -Initial and maintenance 1 criteria- A: No ghosting occurred in either full speed or half speed mode. B: No ghosting in full speed mode. C: Ghosting occurs in both full speed and half speed modes. - Standard for sustainability 2 - A: No ghosting occurred in either full speed or half speed mode. B+: No ghosting in full speed mode. Ghosting in half speed mode is equivalent to the 2000th card. B-: No ghosting in full speed mode. Ghosting in half speed mode worsens from the 2000th shot. C: Ghosting occurs in both full speed and half speed modes.
[0173] [Table 1]
[0174] From the results shown in Table 1, it can be seen that in the transfer device of this embodiment, even though a metal primary transfer roll is used, the ghost phenomenon is suppressed compared to the transfer device of the comparative example.
[0175] The present disclosure includes the following aspects.
[0176] (((1))) an endless belt comprising a layer containing at least one resin selected from the group consisting of polyimide resin, polyamideimide resin, aromatic polyetheretherketone resin, polyphenylene sulfide resin, and polyetherimide resin, conductive carbon particles, and a silicone oil containing at least one resin selected from the group consisting of dimethylpolysiloxane and an organic group-substituted product of dimethylpolysiloxane, or having said layer as an outermost layer, said endless belt having said layer as an outermost layer, wherein in a spatial distribution of the conductive carbon particles present in an evaluation area of 6.3 μm×4.2 μm on the outer circumferential surface of said endless belt, an integral value of a statistic L(r) expressed by the following formula (1) when the inter-particle distance r is 0.05 μm or more and 0.30 μm or less is 0 or more and 0.1 or less; a primary transfer device having a metallic primary transfer roll that is in contact with an inner peripheral surface of the intermediate transfer body and applies an electric field to the intermediate transfer body, and that performs primary transfer of a toner image formed on a surface of an image carrier onto an outer peripheral surface of the intermediate transfer body; a secondary transfer device that secondarily transfers the toner image transferred onto the outer peripheral surface of the intermediate transfer body onto a surface of a recording medium; A transfer device comprising:
[0177]
number
[0178] [In the formula (1), r represents the interparticle distance, and K(r) represents Ripley's K function K(r) represented by the following formula (2)]
[0179]
number
[0180] [In the above formula (2), 1(|X i -X j |≦r) indicates the indicator function, and X i and X j indicate the coordinates of point i and point j, respectively, and |X i -X j | is the coordinate X i and coordinate Xj represents the Euclidean distance between the particles, r represents the interparticle distance, and s(|X i -X j |) indicates the edge correction coefficient s(x) of the evaluation area expressed by the following formula (3), and x = |X i -X j |, where N indicates the total number of particles in the evaluation area, and λ indicates the number density of particles in the evaluation area.
[0181]
number
[0182] [In the formula (3), L x and L y are the lengths (μm) of the sides of the evaluation area in the x-axis and y-axis directions, respectively, and x = |X i -X j | and X i and X j indicate the coordinates of point i and point j, respectively, and |X i -X j | is the coordinate X i and coordinate X j This shows the Euclidean distance between
[0183] (((2))) The transfer device described in (((1))), wherein the silicone oil includes a modified silicone oil having at least one selected from the group consisting of an organic group having a polyether structure and an aralkyl group as an organic group substitute of the dimethylpolysiloxane. (((3))) The transfer device according to (((1))) or (((2))), wherein the silicone oil contains at least one selected from the group consisting of polyether-modified silicone oils and aralkyl-modified silicone oils as an organic group substitute of the dimethylpolysiloxane. (((4))) The transfer device according to any one of (((1))) to (((3))), wherein the silicone oil contains a polyether-modified silicone oil as an organic group substitute of the dimethylpolysiloxane. (((5))) The transfer device according to any one of (((1))) to (((3))), wherein the silicone oil contains an aralkyl-modified silicone oil as an organic group substitute of the dimethylpolysiloxane. (((6))) The transfer device according to any one of (((1))) to (((5))), wherein the content of the silicone oil is 0.5% by mass or more and 7% by mass or less with respect to the entire layer. (((7))) The transfer device according to any one of (((1))) to (((6))), wherein the content of the silicone oil is 0.5% by mass or more and 6% by mass or less with respect to the entire layer. (((8))) The transfer device according to any one of (((1))) to (((7))), wherein the content of the silicone oil is 1% by mass or more and 3% by mass or less with respect to the entire layer. (((9))) The transfer device according to any one of (((1))) to (((8))), wherein the resin includes an imide-based resin. (((10))) The transfer device according to (((9))), wherein the imide-based resin includes a polyimide resin.
[0184] (((11))) The transfer device described in (((1))), wherein the silicone oil contains at least one selected from the group consisting of polyether-modified silicone oil and aralkyl-modified silicone oil as an organic group substitute of the dimethylpolysiloxane, and the resin contains an imide-based resin. (((12))) The transfer device according to (((11))), wherein the imide-based resin includes a polyimide resin.
[0185] (((13))) An image carrier; a charging device for charging the surface of the image carrier; an electrostatic latent image forming device for forming an electrostatic latent image on a charged surface of the image carrier; a developing device that contains a developer containing a toner and develops an electrostatic latent image formed on the surface of the image carrier with the developer to form a toner image; A transfer device according to any one of (((1))) to (((12))) that transfers the toner image onto a surface of a recording medium; An image forming apparatus comprising:
[0186] According to the invention pertaining to (((1))), there is provided a transfer device which has an intermediate transfer body consisting of an endless belt, a primary transfer device having a metallic primary transfer roll, and a secondary transfer device, and in which the endless belt is composed of a layer containing resin and conductive carbon particles or has said layer as the outermost layer, in which the ghost phenomenon caused by the surface conduction of charge on the outer peripheral surface of the endless belt is suppressed compared to when the layer does not contain silicone oil, when the layer contains only fluorine-modified silicone oil as the silicone oil, or when the integral value of the statistic L(r) expressed by the following formula (1) when the inter-particle distance r is 0.05 μm or more and 0.30 μm or less exceeds 0.1 in the spatial distribution of the conductive carbon particles present in an evaluation area of 6.3 μm × 4.2 μm on the outer peripheral surface of the endless belt is greater than 0.1.
[0187] According to the invention related to (((2))), (((3))), (((4))), or (((5))), a transfer device is provided in which a state in which the ghost phenomenon is suppressed is maintained, as compared to when the silicone oil is made of dimethylpolysiloxane. According to the invention related to (((6))) or (((7))), a transfer device is provided in which the ghost phenomenon is suppressed compared to when the silicone oil content is less than 0.5 mass %. According to the invention related to (((8))), a transfer device is provided in which the ghost phenomenon is suppressed compared to when the silicone oil content is less than 1 mass %. According to the invention related to (((9))) or (((10))), a transfer device is provided in which the ghost phenomenon is maintained in a suppressed state compared to when the resin is made of an aromatic polyether ether ketone resin.
[0188] According to the invention relating to (((11))) or (((12))), a transfer device is provided in which a state in which the ghost phenomenon is suppressed is maintained, as compared to when the silicone oil is made of dimethylpolysiloxane or when the resin is made of aromatic polyether ether ketone resin.
[0189] According to the invention pertaining to (((13))), there is provided an image forming apparatus which has an intermediate transfer body consisting of an endless belt, a primary transfer device having a metallic primary transfer roll, and a secondary transfer device, and in which the endless belt is composed of a layer containing resin and conductive carbon particles or has said layer as the outermost layer, in which the ghost phenomenon caused by creeping conduction of charge on the outer peripheral surface of the endless belt is suppressed compared to a transfer device in which the layer does not contain silicone oil, a transfer device in which the layer contains only fluorine-modified silicone oil as the silicone oil, or a transfer device in which, in the spatial distribution of the conductive carbon particles present in an evaluation area of 6.3 μm × 4.2 μm on the outer peripheral surface of the endless belt, the integral value of the statistic L(r) expressed by the following formula (1) when the inter-particle distance r is 0.05 μm or more and 0.30 μm or less exceeds 0.1. [Explanation of symbols]
[0190] 1Y, 1M, 1C, 1K Image forming unit 10 Primary transfer section 11 Photoreceptor 12 Charger 13 Laser exposure device 14 Developer 15 Intermediate transfer belt 16 Primary transfer roll 17 Photoconductor cleaner 20 Secondary transfer section 22 Secondary transfer roll 25 Back roll 26 Power supply roll 31 Driving Roll 32 Support roll 33 Tensioning roll 34 Cleaning back roll 35 Intermediate transfer belt cleaner 40 Control section 42 Reference Sensor 43 Image density sensor 50 Paper storage section 51 Paper feed roll 52 Transport roll 53 Transport guide 55 Conveyor belt 56 Fixing entrance guide 60 Fixing device 100 Image forming device K Paper
Claims
1. an endless belt comprising a layer containing at least one resin selected from the group consisting of polyimide resin, polyamideimide resin, aromatic polyetheretherketone resin, polyphenylene sulfide resin, and polyetherimide resin, conductive carbon particles, and a silicone oil containing at least one resin selected from the group consisting of dimethylpolysiloxane and an organic group-substituted product of dimethylpolysiloxane, or having said layer as an outermost layer, wherein in a spatial distribution of the conductive carbon particles present in an evaluation area of 6.3 μm×4.2 μm on the outer circumferential surface of the endless belt, an integral value of a statistic L(r) expressed by the following formula (1) when the inter-particle distance r is 0.05 μm or more and 0.30 μm or less is 0 or more and 0.1 or less; a primary transfer device having a metallic primary transfer roll that is in contact with an inner peripheral surface of the intermediate transfer body and applies an electric field to the intermediate transfer body, and that performs primary transfer of a toner image formed on a surface of an image carrier onto an outer peripheral surface of the intermediate transfer body; a secondary transfer device that secondarily transfers the toner image transferred onto the outer peripheral surface of the intermediate transfer body onto a surface of a recording medium; A transfer device comprising: [0010] [In the formula (1), r represents the interparticle distance, and K(r) represents Ripley's K function K(r) represented by the following formula (2).] [0025] [In the formula (2), 1(|X i -X j |≦r) indicates the indicator function, and X i and X j indicate the coordinates of point i and point j, respectively, and |X i -X j | is the coordinate X i and coordinate X j represents the Euclidean distance between the particles, r represents the interparticle distance, and s(|X i -X j |) indicates the edge correction coefficient s(x) of the evaluation area expressed by the following formula (3), and x = |X i -X j|, N indicates the total number of particles in the evaluation area, and λ indicates the number density of particles in the evaluation area. [0030] [In the formula (3), L x and L y indicate the lengths (μm) of the sides of the evaluation area in the x-axis and y-axis directions, respectively, and x = |X i -X j | and X i and X j indicate the coordinates of point i and point j, respectively, and |X i -X j | is the coordinate X i and coordinate X j This shows the Euclidean distance between
2. 2. The transfer device according to claim 1, wherein the silicone oil includes a modified silicone oil having, as an organic group substitutent of the dimethylpolysiloxane, at least one selected from the group consisting of an organic group having a polyether structure and an aralkyl group.
3. 2. The transfer device according to claim 1, wherein the silicone oil contains at least one type selected from the group consisting of polyether-modified silicone oil and aralkyl-modified silicone oil as the organic group substitutent of the dimethylpolysiloxane.
4. 2. The transfer device according to claim 1, wherein the silicone oil contains a polyether-modified silicone oil as an organic group substitute of the dimethylpolysiloxane.
5. 2. The transfer device according to claim 1, wherein the silicone oil contains an aralkyl-modified silicone oil as an organic group substitute of the dimethylpolysiloxane.
6. The transfer device according to claim 1 , wherein the silicone oil content is from 0.5% by mass to 7% by mass with respect to the entire layer.
7. The transfer device according to claim 6 , wherein the content of the silicone oil is 0.5% by mass or more and 6% by mass or less with respect to the entire layer.
8. The transfer device according to claim 6 , wherein the content of the silicone oil is from 1% by mass to 3% by mass with respect to the entire layer.
9. The transfer device according to claim 1 , wherein the resin includes an imide resin.
10. The transfer device according to claim 9 , wherein the imide resin includes a polyimide resin.
11. 2. The transfer device according to claim 1, wherein the silicone oil contains at least one selected from the group consisting of polyether-modified silicone oil and aralkyl-modified silicone oil as the organic group substitute of the dimethylpolysiloxane, and the resin contains an imide-based resin.
12. The transfer device according to claim 11 , wherein the imide resin includes a polyimide resin.
13. An image carrier; a charging device for charging the surface of the image carrier; an electrostatic latent image forming device for forming an electrostatic latent image on a charged surface of the image carrier; a developing device that contains a developer containing a toner and develops an electrostatic latent image formed on the surface of the image carrier with the developer to form a toner image; A transfer device according to any one of claims 1 to 12, which transfers the toner image onto a surface of a recording medium; An image forming apparatus comprising:
Citation Information
Patent Citations
Image forming device
JP1999202648A
Image forming apparatus
JP2006243031A